Electrolyte-sealed structure
The electrolyte encapsulation structure using multiple layers of low moisture permeability materials addresses the issue of H2S gas release from sulfide solid electrolytes, ensuring stability and performance during storage and transportation by maintaining the electrolyte's shape and particle size.
Patent Information
- Application Number
- JP2023057792
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Sulfide solid electrolytes in powder form react with moisture, leading to the release of H2S gas, which can corrode equipment and alter the shape and particle size of the electrolyte, compromising the integrity and performance of the battery during storage and transportation.
An electrolyte encapsulation structure using multiple layers of packaging materials with low moisture permeability, including organic resins and aluminum, to maintain a concentration of H2S gas below 50 ppm, ensuring the sulfide solid electrolyte remains stable and functional.
The proposed structure effectively prevents the release of H2S gas, maintaining the shape and particle size of the sulfide solid electrolyte, thereby ensuring the stability and performance of the battery during storage and transportation.
Smart Images

Figure 2024145442000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte containment structure. [Background technology]
[0002] In recent years, secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2. As such secondary batteries, solid-state batteries using a sulfide solid electrolyte are known. As sulfide solid electrolytes, for example, materials having an argyrodite crystal structure are known from the viewpoint of further improving lithium ion conductivity. Here, the argyrodite crystal structure is a crystal structure possessed by a group of compounds derived from a mineral represented by the chemical formula: Ag8GeS6. The sulfide solid electrolyte used as an electrolyte for solid-state batteries is usually in a powder form. The powdered sulfide solid electrolyte is usually sealed in a package after production, and then stored and transported. Hereinafter, a structure in which a sulfide solid electrolyte is sealed in a package is also referred to as an "electrolyte-encapsulated structure".
[0003] However, sulfide solid electrolytes easily react with moisture in the air to generate H2S gas. If H2S gas is released when the electrolyte encapsulation structure is opened, it may corrode metal parts of surrounding devices and machines. For this reason, it is preferable that the electrolyte encapsulation structure has a structure that is less likely to release H2S gas generated by the reaction between the sulfide solid electrolyte and moisture in the air during storage and transportation.
[0004] Moreover, the sulfide solid electrolyte is usually in the form of a powder whose shape and particle size are controlled within a predetermined range. When a large external force is applied to the sulfide solid electrolyte powder, the particles may be damaged, and the desired characteristics may not be exhibited. For this reason, it is preferable that the shape and particle size of the sulfide solid electrolyte are unlikely to change during storage and transportation.
[0005] As a conventional example of an electrolyte encapsulation structure, Patent Document 1 discloses a water-absorbent sulfur-based gas absorbing packaging material for a sulfide-based inorganic solid electrolyte type all-solid-state lithium ion battery that absorbs gaseous water and / or liquid water and sulfur-based gas. This water-absorbent sulfur-based gas absorbing packaging material includes a base layer made of nylon film or the like, a gas barrier layer made of aluminum foil or the like, and a heat-sealable sealant layer made of a water-absorbent sulfur-based gas absorbing sealant film, and the sealant layer is said to include a sulfur-based gas absorbent, an inorganic water absorbent, and a heat-sealable resin. When a sulfide solid electrolyte is encapsulated in a package with the sealant layer of the water-absorbent sulfur-based gas absorbing packaging material of Patent Document 1 on the inside, an electrolyte encapsulation structure is formed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2021-57232 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the water-absorbent sulfur-based gas absorbing packaging material shown in the examples of Patent Document 1 has a high relative humidity of up to 45% in a relative humidity test using a gas absorbing film that is part of the layer structure, and the base layer is made of nylon film or the like that is generally known to have high moisture permeability. Therefore, if an electrolyte encapsulation structure in which a sulfide solid electrolyte is encapsulated is used in this water-absorbent sulfur-based gas absorbing packaging material, there is a risk that H2S gas will be released when the package is opened due to a reaction between the sulfide solid electrolyte and moisture in the air during storage and transportation.
[0008] The present invention has been made in consideration of the above problems, and has an object to provide an electrolyte encapsulation structure that is less likely to release H2S gas when opened. [Means for solving the problem]
[0009] The inventors have discovered that by using an electrolyte encapsulation structure having a first packaging body that encapsulates a sulfide-based solid electrolyte, in which the concentration of H2S gas in the filled gas present in a first space partitioned by the inner surface of the first packaging body that encapsulates the sulfide solid electrolyte is 50 ppm or less, an electrolyte encapsulation structure that is less likely to release H2S gas when opened can be obtained, and have completed the present invention.
[0010] That is, the gist of the present invention is as follows. (1) The electrolyte encapsulation structure of the present invention comprises a sulfide-based solid electrolyte and a packaging body encapsulating the sulfide-based solid electrolyte, wherein the packaging body is a first packaging body in which n is 1 encapsulates the sulfide-based solid electrolyte, and when an nth packaging body encapsulating the first packaging body is present, the nth packaging body encapsulating the first packaging body has n increasing sequentially toward the outer surface side of the first packaging body, and when the space packaged by the first packaging body is defined as a first space and the space partitioned by the nth packaging body and the n-1th packaging body is defined as an nth space, the concentration of H2S gas in the filled gas present in each of the spaces from the first space to the nth space is 50 ppm or less after 7 days.
[0011] (2) It is preferable that the dew point temperature of the fill gas present in the first space is −20° C. or lower.
[0012] (3) The filling gas is preferably Ar, air, N2 or CO2.
[0013] (4) It is preferable that the packaging material constituting the first package has a layer made of an organic material on at least a portion of the inner surface.
[0014] (5) It is preferable that the first package is sealed by welding the layer made of the organic material.
[0015] (6) The organic material is preferably one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol.
[0016] (7) It is preferable that the packaging material constituting the first packaging body has an inner welded portion made of a weldable organic material and an outer non-welded portion which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion.
[0017] (8) It is preferable that the device further has a second packaging body that contains and encloses the first packaging body, and that the concentration of H2S gas in the filling gas present in a second space partitioned by the outer surface of the first packaging body and the inner surface of the second packaging body is 50 ppm or less.
[0018] (9) It is preferable that the device further has a third packaging body that contains and encloses the second packaging body, and that the concentration of H2S gas in the filling gas present in a third space partitioned by the outer surface of the second packaging body and the inner surface of the third packaging body is 50 ppm or less.
[0019] (10) A method for manufacturing an electrolyte encapsulation structure according to the present invention includes a sulfide-based solid electrolyte and a packaging body that encapsulates the sulfide-based solid electrolyte, the packaging body being made of packaging material arranged in an nth layer (n is an integer of 1 or more) from the sulfide-based solid electrolyte side, a first packaging body in which n is 1 encapsulates the sulfide-based solid electrolyte, and when a packaging body that encapsulates the first packaging body is present, an nth packaging body that packages the first packaging body is a manufacturing method for an electrolyte encapsulation structure in which n increases sequentially toward an outer surface side of the first packaging body, the method including an encapsulation step of filling the filled gas such that the concentration of H2S gas in the filled gas present in each space from the first space to the nth space becomes 50 ppm or less after 7 days, where a space packed with the first packaging body is a first space, and a space partitioned by the nth packaging body and the n-1th packaging body is an nth space. (11) The dew point temperature of the filled gas is preferably −20° C. or lower. (12) It is preferable that the method further includes a drying step of drying the first package at 50° C. or higher before the sealing step. Effect of the Invention
[0020] According to the present invention, it is possible to provide an electrolyte containment structure that is less likely to release H2S gas when opened. [Brief description of the drawings]
[0021] [Figure 1] 1 is a plan view showing an electrolyte containment structure according to a first embodiment of the present invention; [Diagram 2] FIG. 2 is a diagram showing the internal state of the electrolyte containment structure of FIG. 1 so as to be clearly understood. [Diagram 3] FIG. 8 is a perspective view of a package constituting the electrolyte containment structure of FIGS. 1, 5 and 7, with the opening open; [Figure 4] 4 is a cross-sectional view of a packaging material that constitutes the package of FIG. 3. [Diagram 5] FIG. 2 is a plan view showing an electrolyte containment structure according to a first modified example of the first embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing the internal state of the electrolyte containment structure of FIG. 5 so as to be clearly understood. [Figure 7] FIG. 4 is a plan view showing an electrolyte containment structure according to a second modified example of the first embodiment of the present invention. [Figure 8] FIG. 8 is a diagram showing the internal state of the electrolyte containment structure of FIG. 7 so as to be clearly understood. [Figure 9] FIG. 4 is a perspective view showing an electrolyte containment structure according to a second embodiment of the present invention. [Figure 10] FIG. 10 is a diagram showing the internal state of the electrolyte containment structure of FIG. 9 so as to be clearly understood. [Figure 11] FIG. 17 is a perspective view of a package constituting the electrolyte containment structure of FIGS. 9, 14 and 16, with the opening in a closed state. [Figure 12] 10 is an exploded perspective view of a package constituting the electrolyte containment structure of FIG. 9. [Figure 13] 12 is a cross-sectional view of a packaging material that constitutes the package of FIG. 11. [Figure 14] FIG. 11 is a perspective view showing an electrolyte containment structure according to a first modified example of the second embodiment of the present invention. [Figure 15]FIG. 15 is a diagram showing the internal state of the electrolyte containment structure of FIG. 14 so as to be clearly understood. [Figure 16] 1 is a perspective view showing an electrolyte containment structure according to a second modified example of the second embodiment of the present invention, and FIG. 2 is a schematic view showing an electrolyte containment structure according to a second modified example of the second embodiment of the present invention. [Figure 17] FIG. 17 is a diagram showing the internal state of the electrolyte containment structure of FIG. 16 so as to be clearly understood. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The electrolyte containment structure 1 according to the present invention includes a sulfide-based solid electrolyte 3 and a packaging body that contains the sulfide-based solid electrolyte 3. In the electrolyte containment structure 1 according to the present invention, the packaging body is made of a packaging material arranged in an n-th layer (n is an integer of 1 or more) from the sulfide-based solid electrolyte 3 side, and when a first packaging body in which n is 1 contains the sulfide-based solid electrolyte 3 and a packaging body that contains the first packaging body is present, the n-th packaging body that contains the first packaging body has n increasing in order toward the outer surface side of the first packaging body. In the electrolyte containment structure 1 according to the present invention, when the space contained by the first packaging body is defined as the first space and the space partitioned by the n-1 packaging body is defined as the n-th space, the concentration of H2S gas in the filled gas present in each space from the first space to the n-th space is 50 ppm or less 7 days after filling.
[0023] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the shape and size of the drawings are appropriately changed for convenience of explanation. Therefore, the present invention is not limited to the shape of the drawings.
[0024] [Electrolyte Encapsulation Structure] <First embodiment> Fig. 1 is a plan view showing an electrolyte containment structure according to a first embodiment of the present invention, Fig. 2 is a diagram showing the internal state of the electrolyte containment structure of Fig. 1, Fig. 3 is a perspective view of a package constituting the electrolyte containment structure of Fig. 1, Fig. 5 and Fig. 7, with the opening open. Fig. 4 is a cross-sectional view of the package constituting the package of Fig. 3.
[0025] 1 includes a sulfide-based solid electrolyte 3 and a first packaging body 100A (100) that encloses the sulfide-based solid electrolyte 3. In the electrolyte containment structure 1AA, the first packaging body 100A is made of a packaging material 110 arranged in the first layer from the sulfide-based solid electrolyte 3 side.
[0026] In the electrolyte containment structure 1AA, the first packaging body 100A, in which n is 1, contains the sulfide-based solid electrolyte 3, and there is no packaging body that contains the first packaging body 100A. In the electrolyte containment structure 1AA, when the space contained in the first packaging body 100A is partitioned by the first space 109 and referred to as the n-th space (first space 109), the concentration of H2S gas in the filling gas FG present in the first space 109 is 50 ppm or less 7 days after filling.
[0027] The first packaging body 100A(100), for example a heat-sealed bag 120, constituting the electrolyte encapsulation structure 1AA(1) according to the first embodiment shown in FIG. 1 has a thickness in the direction perpendicular to the plane of the paper in FIG. 1 because the sulfide solid electrolyte 3 is encapsulated inside the bag body 121 constituting the first packaging body 100A(100).
[0028] 1 and 2, the electrolyte containment structure 1AA(1) according to the first embodiment includes a sulfide solid electrolyte 3 and a first packaging body 100A(100) that contains the sulfide solid electrolyte 3. In addition, in FIG. 2, the thickness of the bag body 121 is exaggerated compared to the actual thickness.
[0029] 3, the first packaging body 100A is formed into a heat-sealed bag 120 capable of encapsulating the sulfide solid electrolyte 3 by forming a heat-sealed portion 123 by welding at least a portion of the sealing portion 122. The first packaging body 100A is formed into the heat-sealed bag 120 with an opening 127 welded.
[0030] (Sulfide solid electrolyte) The sulfide solid electrolyte 3 typically contains lithium (Li), phosphorus (P) and sulfur (S). When the sulfide solid electrolyte 3 has an argyrodite-type crystal structure, it has high lithium ion conductivity and is electrochemically stable, and therefore exhibits favorable characteristics as an all-solid-state battery, which is preferable. Here, the argyrodite-type crystal structure is a crystal structure possessed by a group of compounds derived from a mineral represented by the chemical formula: Ag8GeS6. Specific composition formulas of the sulfide solid electrolyte 3 include Li6PS5Cl, Li6PS5Br, Li 5.5 P.S. 4.5 Cl 1.5 , Li 5.4 P.S. 4.4 Cl 0.8 Br 0.8 , Li6PS5I, etc.
[0031] The contents of Li, P and S in the sulfide solid electrolyte 3 can be appropriately adjusted.
[0032] The sulfide solid electrolyte 3 has a Li element content of preferably 41 mol% or more, more preferably 41 mol% or more, even more preferably 42 mol% or more, and even more preferably 43 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The above content is preferably 50 mol% or less, more preferably 48 mol% or less, even more preferably 47 mol% or less, and even more preferably 45 mol% or less. When the lithium (Li) element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0033] The sulfide solid electrolyte 3 has a P element content of preferably 7.0 mol % or more, more preferably 7.2 mol % or more, even more preferably 7.5 mol % or more, and even more preferably 7.7 mol % or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol %. The above content is preferably 20 mol % or less, more preferably 18 mol % or less, even more preferably 16 mol % or less, and even more preferably 12 mol % or less. When the P element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0034] The sulfide solid electrolyte 3 has an S element content of preferably 31 mol% or more, more preferably 32 mol% or more, even more preferably 33 mol% or more, and even more preferably 34 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The above content is preferably 43 mol% or less, more preferably 42 mol% or less, even more preferably 40 mol% or less, and even more preferably 38 mol% or less. When the S element content is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0035] The sulfide solid electrolyte 3 has a molar ratio of the Li element content to the P element content (Li element content / P element content) of preferably 4.8 or more, more preferably 5.0 or more, and even more preferably 5.2 or more. The molar ratio is preferably 7.0 or less, more preferably 6.4 or less, and even more preferably 5.8 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0036] The sulfide solid electrolyte 3 has a molar ratio of the S element content to the P element content (S element content / P element content) of preferably 3.6 or more, more preferably 4.0 or more, and even more preferably 4.2 or more. The molar ratio is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.6 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0037] The sulfide solid electrolyte 3 preferably further contains at least one halogen (X) element selected from fluorine (F), chlorine (Cl), bromine (Br) and iodine (I), and more preferably further contains at least one X element selected from Cl and Br. When the sulfide solid electrolyte 3 further contains the above-mentioned elements, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0038] The sulfide solid electrolyte 3 has an X element content of preferably 3.7 mol% or more, more preferably 4.0 mol% or more, even more preferably 8.0 mol% or more, and even more preferably 10 mol% or more, where the total molar amount of the constituent elements of the sulfide solid electrolyte 3 is taken as 100 mol%. The content is preferably 19 mol% or less, more preferably 17 mol% or less, even more preferably 15 mol% or less, and even more preferably 14 mol% or less. When the sulfide solid electrolyte 3 contains two or more X elements, the "content of the X element" means the total content of the two or more X elements. When the content of the X element is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is easily improved.
[0039] In the sulfide solid electrolyte 3, the molar ratio of the content of X element to the content of P element (content of X element / content of P element) is preferably 0.50 or more, more preferably 0.80 or more, and even more preferably 1.2 or more. Moreover, the molar ratio is preferably 2.1 or less, more preferably 2.0 or less, and even more preferably 1.8 or less. When the molar ratio is within the above range, the lithium ion conductivity of the sulfide solid electrolyte 3 is likely to be improved.
[0040] The sulfide solid electrolyte 3 may contain one or more elements (hereinafter referred to as "other elements") other than Li, P, S, and X. Examples of other elements include silicon (Si), germanium (Ge), tin (Sn), lead (Pb), boron (B), aluminum (Al), gallium (Ga), arsenic (As), antimony (Sb), and bismuth (Bi).
[0041] Sulfide solid electrolyte 3 is D 50 is preferably 0.10 μm or more, more preferably 0.20 μm or more, further preferably 0.3 μm or more, and particularly preferably 0.5 μm or more. 50 However, it is preferably 100 μm or less, more preferably 50 μm or less, further preferably 30 μm or less, and particularly preferably 10 μm or less. 50When D is within the above range, the sulfide solid electrolyte 3 is uniformly distributed inside the positive and negative electrodes, and good battery characteristics are easily obtained. 50 is the particle size at which the cumulative volume is 50% in the volume-based particle size distribution of the powder measured by a laser diffraction / scattering particle size distribution measurement method.
[0042] (First package) The first packaging body 100A is a structure in which the sulfide solid electrolyte 3 is enclosed.
[0043] In the electrolyte containment structure 1AA, the concentration of H2S gas in the filling gas FG present in the first space 109 partitioned by the inner surface 107, which is the surface of the first packaging body 100A that contains the sulfide solid electrolyte 3, and in each space in the packaging space 959, which is the entire space in the outermost packaging body 900, which is the packaging body that contains the first packaging body 100A and is the outermost packaging body of the electrolyte containment structure 1AA, is within a specific range. Specifically, in the electrolyte containment structure 1AA, the concentration of H2S gas in the filling gas FG (first space gas 119) present in the first space 109 is 50 ppm or less 7 days after filling.
[0044] In the electrolyte containment structure 1AA, the outermost packing body 900 is the first packing body 100A itself. In the electrolyte containment structure 1AA, since the outermost packing body 900 is the first packing body 100A itself, the packing space 959 is the same as the first space 109. The gas present in the packing space 959 is referred to as a packing space gas 969. In the electrolyte containment structure 1AA, the packing space gas 969 is only the first space gas 119 described below, which is the filling gas FG present in the first space 109. That is, in the electrolyte containment structure 1AA, the filling gas FG is only the first space gas 119.
[0045] The first packaging body 100A has a function (hereinafter also referred to as a "first sealing function") of sealing the sulfide solid electrolyte 3. If the first packaging body 100A further has a function of low moisture permeability (hereinafter also referred to as a "first low moisture permeability function"), this is preferable because it suppresses the generation of H2S due to the reaction between the sulfide solid electrolyte 3 and moisture, making it difficult to release H2S gas when opened.
[0046] As shown in FIGS. 2 and 3, the first packaging body 100A is made by using a sheet-like packaging material 110 to form a heat-sealed bag 120 in which the sulfide solid electrolyte 3 can be sealed.
[0047] 3, the heat-sealed bag 120 constituting the first packaging body 100A includes a bag body 121 and a sealing portion 122 which is a strip-shaped member formed continuously with the bag body 121 and which forms an opening 127 at an end. At least a portion of the sealing portion 122 is welded to form a heat-sealed portion 123, which makes it possible to enclose the sulfide solid electrolyte 3 in the first packaging body 100A.
[0048] 2, in first packaging body 100A, the sulfide solid electrolyte 3 is enclosed in a first space 109 defined by inner surface 107, which is the surface of first packaging body 100A that encloses sulfide solid electrolyte 3. First packaging body 100A made of heat-sealed bag 120 has a relatively flat shape, and therefore has high storage space efficiency.
[0049] Filling gas FG is sealed in the first space 109. As the filling gas FG, Ar, air, N2, CO2, or the like is used. Among these, Ar is preferable because of its low reactivity with the sulfide solid electrolyte 3. The filling gas FG present in the first space 109 is hereinafter also referred to as a first space gas 119. Note that the composition of the first space gas 119 may change due to a reaction with the sulfide solid electrolyte 3, or the like.
[0050] In the electrolyte containment structure 1AA, the concentration of H2S gas in the filling gas FG (first space gas 119, packing space gas 969) present in the first space 109 partitioned by the inner surface 107 of the first packaging body 100A, which is the surface on the side where the sulfide solid electrolyte 3 is enclosed, and in each space in the packing space 959, which is the entire space within the outermost packaging body 900, which is the packaging body that contains the first packaging body 100A and is the outermost packaging body of the electrolyte containment structure 1AA, is 50 ppm or less 7 days after filling. If the concentration of H2S gas in the filling gas FG is within the above range, it is preferable because H2S gas is less likely to be released when opening the package.
[0051] The concentration of H2S gas in the filled gas FG present in the first space 109 is preferably 30 ppm or less, more preferably 20 ppm or less, and further preferably 10 ppm or less. The concentration of H2S gas in the filled gas FG within the latter range is preferable because it is less likely to release H2S gas when opened.
[0052] The dew point temperature of the filled gas FG present in the first space 109 is preferably −20° C. or lower, more preferably −40° C. or lower, and even more preferably −60° C. or lower. The closer the dew point temperature of the filled gas FG is to the latter range, the less likely it is to release H2S gas when opened, which is preferable.
[0053] In the first packaging body 100A in which the sulfide solid electrolyte 3 is sealed, the volume V1 (cm 3 ) the volume V of the sulfide solid electrolyte 3 itself SE (cm 3 ) ratio (V SE The first packing ratio (V1) is, for example, more than 0%, preferably 10% or more, and more preferably 20% or more. The packing ratio is, for example, 50% or less, preferably 40% or less, and more preferably 30% or less. When the first packing ratio is more than 0%, the storage space efficiency tends to be high. When the first packing ratio is 50% or less, aggregation and changes in particle shape due to crushing of the particles of the sulfide solid electrolyte 3 tend to be suppressed.
[0054] The packaging material 110 constituting the first packaging body 100A is made of a material and has a structure capable of keeping the concentration of H2S gas in the filling gas FG present in the first space 109 partitioned by the inner surface 107, which is the surface on the side that encloses the sulfide solid electrolyte 3, within a specific range.
[0055] The first packing ratio (%) is, for example, the true density Dt (g / cm 3 ) of the sulfide solid electrolyte 3 obtained by a pycnometer method (gas replacement method). 3 ) multiplied by the mass M (g) of the sulfide solid electrolyte 3 to obtain the internal volume V1 (cm 3 ) and then multiplying this value by 100, (1 / Dt)M / V1×100.
[0056] The packaging material 110 constituting the first packaging body 100A, the entire heat-sealed bag 120 including the sealing portion 122, has a multi-layer structure having an inner welding portion 117 made of a weldable organic material and an outer non-welded portion 118 which is a layer made of aluminum and is laminated on the outer surface of the inner welding portion 117, as shown in Figure 4.
[0057] When the packaging material 110 has such a multi-layer structure, the moisture permeability is, for example, 10 (g / m 2 When using outer non-welded parts 118 made of a material with a low moisture permeability as follows (hereinafter also referred to as "low moisture permeability material"), it is possible to impart to first packaging body 100A a first sealing function of sealing in sulfide solid electrolyte 3 by welding inner welded parts 117, and a first low moisture permeability function by outer non-welded parts 118. When outer non-welded parts 118 are imparted with the first low moisture permeability function, it becomes easier to suppress the generation of H2S gas from sulfide solid electrolyte 3.
[0058] Here, the inner welding portion 117 refers to a member that includes the inner surface 107, which is the surface of the packaging material 110 that is located on the sulfide solid electrolyte 3 side when the sulfide solid electrolyte 3 is enclosed, and contributes to welding. The inner surface 107 and the surface are shown in FIG.
[0059] The inner welded portion 117 may be a single layer structure made of one or more types of weldable organic material, or may be a multi-layer structure (not shown) in which two or more types of weldable organic material are formed into two or more layers. When the inner welded portion 117 has a multi-layer structure, the inner welded portion 117 has an innermost layer including the inner surface 107, and one or more adjacent inner layers laminated on the outer non-welded portion 118 side as viewed from the innermost layer.
[0060] For example, the inner welded portion 117 can have a two-layer structure including an innermost layer made of a weldable organic material W1 and including the inner surface 107, and a first adjacent inner layer made of a weldable organic material W2 and laminated on the outer non-welded portion 118 side as viewed from the innermost layer.
[0061] In addition, the inner welded portion 117 can have a three-layer structure including an innermost layer made of a weldable organic material W1 and including the inner surface 107, a first adjacent inner layer made of a weldable organic material W2 and laminated on the outer non-welded portion 118 side as viewed from the innermost layer, and a second adjacent inner layer made of a weldable organic material W3 and laminated on the outer non-welded portion 118 side as viewed from the first adjacent inner layer.
[0062] The outer non-welded portion 118 refers to a member that includes the outer surface 108, which is the surface opposite to the inner surface 107 when the sulfide solid electrolyte 3 is enclosed, among the surfaces of the packaging material 110 and does not contribute to welding. The outer surface 108 and the surface are shown in FIG. 2.
[0063] The outer non-welded portion 118 may have a single layer structure made of one or more materials, or may have a multi-layer structure (not shown) made of two or more materials. When the outer non-welded portion 118 has a multi-layer structure, the outer non-welded portion 118 has an outermost layer including the outer surface 108, and one or more auxiliary outer layers laminated on the inner welded portion 117 side as viewed from the outermost layer.
[0064] For example, the outer non-welded portion 118 can have a two-layer structure including an outermost layer made of material N1 and including the outer surface 108, and a first adjacent outer layer made of material N2 and laminated on the inner welded portion 117 side as viewed from the outermost layer.
[0065] In addition, the outer non-welded portion 118 can have a three-layer structure including an outermost layer made of material N1 and including the outer surface 108, a first adjacent outer layer made of material N2 and laminated on the inner welded portion 117 side as viewed from the outermost layer, and a second adjacent outer layer made of material N3 and laminated on the inner welded portion 117 side as viewed from the first adjacent outer layer.
[0066] As the weldable organic material constituting the inner weld portion 117, for example, one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol are used. Among these, polyethylene (PE) is preferred because of its high versatility and excellent recyclability.
[0067] Each of the one or more layers constituting the inner weld portion 117 may be made of one or more organic resins that are weldable organic materials. For example, the inner weld portion 117 may include a layer made of one organic resin and a layer made of two or more organic resins. The layer made of two or more organic resins may be, for example, a layer made of a mixture of two or more organic resins.
[0068] It is preferable that the outer unwelded portion 118 is made of a low moisture permeable material, since this can impart a first low moisture permeability function to the first packaging body 100A.
[0069] The low moisture permeable material used for the outer non-welded portion 118 may be, for example, metals such as aluminum, stainless steel, and iron, or organic materials such as one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol. Among these, aluminum is preferable because it is easy to reduce the moisture permeability of the packaging material 110 constituting the first packaging body 100A.
[0070] For this reason, it is preferable that the packaging material 110 includes an aluminum layer 118 as the outer non-welded portion 118, since this makes it easier to reduce the moisture permeability of the packaging material 110.
[0071] Each of the one or more layers constituting the outer non-welded portion 118 may be made of one or more materials. For example, the outer non-welded portion 118 may include a layer made of one material and a layer made of two or more materials. The layer made of two or more materials may be, for example, a layer made of a mixture of two or more organic resins.
[0072] As the multi-layered packaging material 110, for example, a three-layered packaging material can be used in which, from the inner surface 107 side, an innermost layer of an inner welded portion 117 made of polyethylene PE, a first adjacent inner layer of the inner welded portion 117 made of chlorinated polyethylene SPE, and an outer non-welded portion 118 made of aluminum are laminated in this order.
[0073] In addition, as the multi-layered packaging material 110, for example, a five-layered packaging material can be used in which, from the inner surface 107 side, the innermost layer of the inner welded portion 117 made of polyethylene PE, a first adjacent inner layer of the inner welded portion 117 made of chlorinated polyethylene SPE, a second adjacent outer layer of the outer non-welded portion 118 made of aluminum, a first adjacent outer layer of the outer non-welded portion 118 made of chlorinated polyethylene SPE, and the outermost layer of the outer non-welded portion 118 made of polyethylene PE are laminated in this order.
[0074] Thus, in the electrolyte containment structure 1AA, the packaging material 110 constituting the first packaging body 100A has a layer made of an organic material, so-called an inner welded portion 117, on at least a part of the inner surface 107 side. When the inner welded portion 117 is made of a weldable organic material, the first packaging body 100A of the electrolyte containment structure 1AA is sealed by welding of the layer made of an organic material, so-called the inner welded portion 117, at the heat seal portion 123.
[0075] The thickness of the packaging material 110 constituting the first packaging body 100A is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100A. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because it is easy to reduce the moisture permeability. It is also preferable because it increases the mechanical strength and suppresses the occurrence of pinholes and the intrusion of air when an impact is applied from the outside.
[0076] The packaging material 110 of the first packaging body 100A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 110 has a first enclosing function, the packaging material 110 of the first packaging body 100A may have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single-layer structure as shown in Fig. 13.
[0077] When the outer non-welded portion 118 is made of a low moisture permeable material, in the first packaging body 100A consisting of a heat-sealed bag 120, the material of the packaging material 110 mainly contributes to the first sealing function and the first low moisture permeability function, and the structure of the first packaging body 100A consisting of the heat-sealed bag 120 mainly contributes to the first sealing function.
[0078] For example, when the outer non-welded portion 118 of the packaging material 110 is made of a low moisture permeable material, the first sealing function is mainly realized by welding the inner welded portion 117 of the packaging material 110 of the first packaging body 100A, and the first low moisture permeability function is also mainly realized by the outer non-welded portion 118 of the packaging material 110. In addition, the first sealing function is mainly realized by the heat-sealed portion 123 of the first packaging body 100A made of the heat-sealed bag 120.
[0079] (effect) According to the electrolyte containment structure 1AA, it is possible to provide an electrolyte containment structure that is less likely to release H2S gas when opened.
[0080] Moreover, according to the electrolyte containment structure 1AA, since the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to provide an electrolyte containment structure with high storage space efficiency.
[0081] The concentration of H2S gas in the filled gas FG present in the first space 109 of the electrolyte containment structure 1AA can be measured by a known method.
[0082] <First Modification of the First Embodiment> FIG. 5 is a plan view showing an electrolyte containment structure according to a first modified example of the first embodiment of the present invention, and FIG. 6 is a diagram showing the internal state of the electrolyte containment structure of FIG. 5.
[0083] 5 and 6, an electrolyte containment structure 1AB(1) according to a first modified example of the first embodiment includes a sulfide-based solid electrolyte 3, a first package 100A(100) that contains the sulfide-based solid electrolyte 3, and a second package 200A(200) that contains the first package 100A. In the electrolyte containment structure 1AB, the first package 100A and the second package 200A are made of packaging materials 110 and 210 arranged in the first and second layers from the sulfide-based solid electrolyte 3 side.
[0084] The electrolyte containment structure 1AB has a first space 109 defined between an inner surface 107 of the packaging material 110 of the first packaging body 100A and the sulfide-based solid electrolyte 3 contained in the first packaging body 100A. The electrolyte containment structure 1AB also has a second space 209 defined between an inner surface 207 of the packaging material 210 of the second packaging body 200A and the first packaging body 100A. In the electrolyte containment structure 1AB, the first packaging body 100A, in which n is 1, contains the sulfide-based solid electrolyte 3, and there is a packaging body that contains the first packaging body 100A, and the n-th packaging body (second packaging body 200A) that contains the first packaging body 100A is provided such that n increases in sequence toward the outer surface side of the first packaging body 100A. In the electrolyte encapsulation structure 1AB, when the space packaged in the first packaging body 100A is defined as the first space 109, and the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100A) is defined as the nth space (second space 209), the concentration of H2S gas in the filled gas FG present in each space (first space 109, second space 209) from the first space 109 to the nth space (second space 209) is 50 ppm or less 7 days after filling.
[0085] As shown in Fig. 5 and Fig. 6, an electrolyte containment structure 1AB(1) according to a first modification of the first embodiment includes a first packaging body 100A(100) that contains a sulfide solid electrolyte 3, and a second packaging body 200A(200) that houses and contains the first packaging body 100A. A bag body 221 of the second packaging body 200A that houses and contains the first packaging body 100A has a thickness in the direction perpendicular to the plane of Fig. 5. Note that in Fig. 6, the thicknesses of the bag bodies 121, 221 are exaggerated compared to their actual thickness.
[0086] An electrolyte containment structure 1AB according to a first modified example of the first embodiment is an electrolyte containment structure 1AA according to the first embodiment, which further includes a second packaging body 200A that accommodates and encloses the first packaging body 100A.
[0087] 3, the second packaging body 200A is made into a heat-sealed bag 220 capable of enclosing the first packaging body 100A by welding at least a part of the sealing portion 222 to form a heat-sealed portion 223. The first packaging body 100A is made into a heat-sealed bag 220 with an opening 227 welded.
[0088] The electrolyte containment structure 1AB according to the first modification of the first embodiment is the same as the electrolyte containment structure 1AA according to the first embodiment except that it further includes a second package 200A. Therefore, the same components in the electrolyte containment structure 1AB according to the first modification of the first embodiment and the electrolyte containment structure 1AA according to the first embodiment are denoted by the same reference numerals, and the description of the components and functions is omitted or simplified. The following mainly describes the second package 200A.
[0089] (Second packaging) The second packaging body 200A is a structure that contains and encloses the first packaging body 100A.
[0090] In the electrolyte containment structure 1AB, the concentration of H2S gas in the filling gas FG present in the second space 209 partitioned by the outer surface 108 of the first package 100A and the inner surface 207 of the second package 200A, and in each space in the packaging space 959 which is the entire space in the outermost packaging body 900 which is the packaging body containing the first package 100A and is the outermost packaging body of the electrolyte containment structure 1AA, is within a specific range. Specifically, in the electrolyte containment structure 1AB, the concentration of H2S gas in the filling gas FG (first space gas 119 and second space gas 219) present in each space of the first space 109 and the second space 209 is 50 ppm or less 7 days after filling.
[0091] In the electrolyte containment structure 1AB, the outermost packaging body 900 is the second packaging body 200A. In the electrolyte containment structure 1AB, the packaging space 959 is the first space 109 and the second space 209. In the electrolyte containment structure 1AB, the packaging space gas 969 is the first space gas 119 and the second space gas 219 described below, which is the filler gas FG present in the second space 209. That is, in the electrolyte containment structure 1AB, the filler gas FG is the first space gas 119 and the second space gas 219.
[0092] The second packaging body 200A has a function of enclosing the electrolyte enclosing structure 1AA, which is the first packaging body 100A enclosing the sulfide solid electrolyte 3. Such a function of enclosing the first packaging body 100 is hereinafter also referred to as a "second enclosing function." Note that it is preferable that the second packaging body 200A further has a function of low moisture permeability (hereinafter also referred to as a "second low moisture permeability function"), since this suppresses the generation of H2S due to the reaction between the sulfide solid electrolyte 3 and moisture, making it difficult to release H2S gas when opened.
[0093] As shown in FIG. 6 and FIG. 3, the second package 200A is made by using a sheet-like package material 210 to form a heat-sealed bag 220 capable of containing and sealing the first package 100A.
[0094] As shown in Fig. 3, the heat seal bag 220 constituting the second packaging body 200A has the same structure as the heat seal bag 120 constituting the first packaging body 100A. That is, as shown in Fig. 3, the heat seal bag 220 constituting the second packaging body 200A includes a bag body 221 and a sealing portion 222 which is a strip-shaped member formed continuously with the bag body 221 and which forms an opening 227 at an end. At least a part of the sealing portion 222 of the second packaging body 200A is welded to form a heat seal portion 223, which makes it possible to contain and enclose the first packaging body 100A in the second packaging body 200A.
[0095] 3, in the second packaging body 200A, the first packaging body 100A is enclosed in a second space 209 defined by an inner surface 207, which is the surface of the second packaging body 200A that encloses the first packaging body 100A. The second packaging body 200A made of a heat-sealed bag 220 has a relatively flat shape, and therefore has high storage space efficiency.
[0096] The second space 209 is filled with a filling gas FG. The filling gas FG filled in the second space 209 is Ar, air, N2, CO2, or the like, which is the same as the filling gas FG used in the filling gas FG filled in the first space 109. Among these, Ar is preferable because it has low reactivity with the sulfide solid electrolyte 3 even if the first packaging body 100A is damaged and the sulfide solid electrolyte 3 is exposed to the atmosphere in the second space 209. The filling gas FG filled in the second space 209 and the filling gas FG filled in the first space 109 may have the same components and concentrations or may be different. The filling gas FG present in the second space 209 is also referred to as a second space gas 219 below. The components of the second space gas 219 may change due to a reaction with the sulfide solid electrolyte 3, etc.
[0097] In the electrolyte containment structure 1AB, the concentration of H2S gas in the filling gas FG (second space gas 219) present in the second space 209 is 50 ppm or less 7 days after filling. If the concentration of H2S gas in the filling gas FG is within the above range, it is preferable because the H2S gas is unlikely to be released when the package is opened.
[0098] The preferred range of the concentration of H2S gas in the filling gas FG (second space gas 219) filled in the second space 209 and the reasons therefor are similar to those for the filling gas FG (first space gas 119) filled in the first space 109.
[0099] The preferred numerical range of the dew point temperature of the filler gas FG present in the second space 209 and the reasons therefor are similar to those of the filler gas FG sealed in the first space 109 .
[0100] The packaging material 210 constituting the second packaging body 200A is made of a material and has a structure that makes it possible to keep the concentration of H2S gas in the filling gas FG present in the second space 209 partitioned by the inner surface 207, which is the surface that encloses the first packaging body 100A, within a specific range.
[0101] The packaging material 210 constituting the second packaging body 200A has a multilayer structure in which the entire heat-sealed bag 220, including the sealing portion 222, has an inner welded portion 217 made of a weldable organic material and an outer non-welded portion 218 which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion 217, as shown in Figure 4.
[0102] When the packaging material 210 has such a multi-layer structure, when an outer non-welded portion 218 made of a low moisture permeable material is used, the second packaging body 200A can be provided with a second encapsulation function of enclosing the first packaging body 100A by welding the inner welded portion 217, and a second low moisture permeability function by the outer non-welded portion 218.
[0103] The inner welded portion 217 and the outer non-welded portion 218 of the second packaging body 200A are conceptually similar to the inner welded portion 117 and the outer non-welded portion 118 of the first packaging body 100A, and therefore a description thereof will be omitted.
[0104] The weldable organic material constituting the inner weld portion 217 is the same as the organic material used for the inner weld portion 117 of the first packaging body 100A for the same reasons. Note that the weldable organic material constituting the inner weld portion 217 and the weldable organic material constituting the inner weld portion 117 of the first packaging body 100A may have the same components or concentrations as or different from each other.
[0105] It is preferable that the outer unwelded portion 218 is made of a low moisture permeable material, since this can impart a second low moisture permeability function to the second package 200A.
[0106] The low moisture permeable material used for the outer unwelded portion 218 is the same as the low moisture permeable material used for the outer unwelded portion 118 of the first packaging body 100A for the same reason.
[0107] For this reason, it is preferable that the packaging material 210 includes an aluminum layer 218 as the outer non-welded portion 218, since this makes it easier to reduce the moisture permeability of the packaging material 210.
[0108] The thickness of the packaging material 210 constituting the second packaging body 200A, at its thinnest portion, is within the same numerical range as the thickness of the packaging material 110 constituting the first packaging body 100 for the same reasons.
[0109] The thickness of the inner welded portion 217 at the thinnest portion of the second package 200A is within the same numerical range as the thickness of the inner welded portion 117 constituting the first package 100 for the same reasons.
[0110] The thickness of the outer non-welded portion 218 at the thinnest portion of the second package 200A is within the same numerical range as the thickness of the outer non-welded portion 118 constituting the first package 100 for the same reasons.
[0111] The packaging material 210 of the second packaging body 200A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 210 has a second enclosing function, the packaging material 210 of the second packaging body 200A may have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single-layer structure as shown in Fig. 13.
[0112] When the outer non-welded portion 218 is made of a low moisture permeable material, in the second packaging body 200A consisting of the heat-sealed bag 220, the material of the packaging material 210 mainly contributes to the second sealing function and the second low moisture permeability function, and the structure of the second packaging body 200A consisting of the heat-sealed bag 220 mainly contributes to the second sealing function.
[0113] For example, when the outer non-welded portion 218 of the packaging material 210 is made of a low moisture permeable material, the second sealing function is mainly realized by welding the inner welded portion 217 of the packaging material 210 of the second packaging body 200A, and the second low moisture permeability function is also mainly realized by the outer non-welded portion 218 of the packaging material 210. In addition, the second sealing function is mainly realized by the heat-sealed portion 223 of the second packaging body 200A made of the heat-sealed bag 220.
[0114] (effect) According to the electrolyte containment structure 1AB, it is possible to provide an electrolyte containment structure which is less likely to release H2S gas when opened, as compared with the electrolyte containment structure 1AA.
[0115] Furthermore, according to the electrolyte containment structure 1AB, since the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to provide an electrolyte containment structure with high storage space efficiency.
[0116] The concentration of H2S gas in the filled gas FG present in the first space 109 and the second space 209 of the electrolyte containment structure 1AB can be measured by a known method.
[0117] <Second Modification of the First Embodiment> FIG. 7 is a plan view showing an electrolyte containment structure according to a second modified example of the first embodiment of the present invention, and FIG. 8 is a diagram showing the internal state of the electrolyte containment structure of FIG. 7.
[0118] 7 and 8, an electrolyte containment structure 1AC(1) according to the second modification of the first embodiment includes a sulfide-based solid electrolyte 3, a first packaging body 100A(100) that contains the sulfide-based solid electrolyte 3, a second packaging body 200A(200) that contains the first packaging body 100A, and a third packaging body 300A(300) that contains the second packaging body 200A. In the electrolyte containment structure 1AC, the first packaging body 100A, the second packaging body 200A, and the third packaging body 300A are made of packaging materials 110, 210, and 310 arranged in the first, second, and third layers from the sulfide-based solid electrolyte 3 side.
[0119] The electrolyte containment structure 1AC has a first space 109 defined between an inner surface 107 of the packaging material 110 of the first packaging body 100A and the sulfide-based solid electrolyte 3 contained in the first packaging body 100A. The electrolyte containment structure 1AC also has a second space 209 defined between an inner surface 207 of the packaging material 210 of the second packaging body 200A and the first packaging body 100A. The electrolyte containment structure 1AC also has a third space 309 defined between an inner surface 307 of the packaging material 310 of the third packaging body 300A and the second packaging body 200A. In the electrolyte containment structure 1AC, the first packaging body 100A, in which n is 1, contains a sulfide-based solid electrolyte 3, and there is a packaging body that contains the first packaging body 100A, and the nth packaging body (second packaging body 200A) that contains the first packaging body 100A is arranged so that n increases sequentially toward the outer surface side of the first packaging body 100A. In the electrolyte encapsulation structure 1AC, when the space packaged by the first packaging body 100A is defined as the first space 109, the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100A) is defined as the nth space (second space 209), and the space partitioned by the nth packaging body (third packaging body 300A) and the n-1th packaging body (second packaging body 200A) is defined as the nth space (third space 309), the concentration of H2S gas in the filled gas FG present in each space (first space 109, second space 209, third space 309) from the first space 109 to the nth space (third space 309) is 50 ppm or less 7 days after filling.
[0120] As shown in Fig. 7 and Fig. 8, the electrolyte containment structure 1AC (1) according to the second modification of the first embodiment includes a first package 100A (100) that contains a sulfide solid electrolyte 3, a second package 200A (200) that contains and contains the first package 100A, and a third package 300A (300) that contains and contains the second package 200A. The electrolyte containment structure 1AC has a thickness in the direction perpendicular to the paper surface of Fig. 7 because it includes the electrolyte containment structure 1AB. In Fig. 8, the thicknesses of the bag bodies 121, 221, and 321 are exaggerated compared to their actual thicknesses.
[0121] The electrolyte containment structure 1AC according to the second modified example of the first embodiment is the electrolyte containment structure 1AB according to the first modified example of the first embodiment, further including a third packaging body 300A that accommodates and encloses the second packaging body 200A.
[0122] 3, the third packaging body 300A is made into a heat-sealed bag 320 capable of enclosing the second packaging body 200A by welding at least a part of the sealing portion 322 to form a heat-sealed portion 323. The second packaging body 200A is made into a heat-sealed bag 320 with an opening portion 327 welded.
[0123] The electrolyte containment structure 1AC according to the second modification of the first embodiment is the same as the electrolyte containment structure 1AB according to the first modification of the first embodiment, except that it further includes a third packaging body 300A. Therefore, the same components in the electrolyte containment structure 1AC according to the second modification of the first embodiment and the electrolyte containment structure 1AB according to the first modification of the first embodiment are denoted by the same reference numerals, and the description of the components and functions is omitted or simplified. The following mainly describes the third packaging body 300A.
[0124] (Third packaging) The third package 300A is a structure that contains and encloses the second package 200A.
[0125] In the electrolyte containment structure 1AC, the first packaging body 100A, in which n is 1, contains a sulfide-based solid electrolyte 3, and there are packaging bodies that contain the first packaging body 100A, and the nth packaging body (second packaging body 200A, third packaging body 300A) that contains the first packaging body 100A is arranged so that n increases in sequence toward the outer surface side of the first packaging body 100A. In the electrolyte containment structure 1AC, the concentration of H2S gas in the filled gas FG present in the third space 309 partitioned by the outer surface 208 of the second packaging body 200A and the inner surface 307 of the third packaging body 300A, and in each space within the packaging space 959, which is the entire space within the outermost packaging body 900, which is the first packaging body 100A itself or a packaging body that contains the first packaging body 100A and is the outermost packaging body of the electrolyte containment structure 1AA, is within a specific range. Specifically, in the electrolyte encapsulation structure 1AC, when the space packaged by the first packaging body 100A is defined as the first space 109, the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100A) is defined as the nth space (second space 209), and the space partitioned by the nth packaging body (third packaging body 300A) and the n-1th packaging body (second packaging body 200A) is defined as the nth space (third space 309), the concentration of H2S gas in the filled gas FG (first space gas 119, second space gas 219, and third space gas 319) present in each space (first space 109, second space 209, third space 309) from the first space 109 to the nth space (second space 209) is 50 ppm or less 7 days after filling.
[0126] In the electrolyte containment structure 1AC, the outermost packaging body 900 is the third packaging body 300A. In the electrolyte containment structure 1AC, the packaging space 959 is the first space 109, the second space 209, and the third space 309. In the electrolyte containment structure 1AC, the packaging space gas 969 is the first space gas 119, the second space gas 219, and the third space gas 319 described below, which is the filler gas FG present in the third space 309. That is, in the electrolyte containment structure 1AC, the filler gas FG is the first space gas 119, the second space gas 219, and the third space gas 319.
[0127] The third packaging body 300A has a function of enclosing the second packaging body 200A constituting the outermost layer of the electrolyte containment structure 1AB. Such a function of enclosing the second packaging body 200 is hereinafter also referred to as a "third enclosing function." It is preferable that the third packaging body 300A further has a function of low moisture permeability (hereinafter also referred to as a "third low moisture permeability function"), because this suppresses the generation of H2S due to the reaction between the sulfide solid electrolyte 3 and moisture, and thus makes it difficult to release H2S gas when opened.
[0128] As shown in FIG. 8 and FIG. 3, the third package 300A is made by using a sheet-like packaging material 310 to form a heat-sealed bag 320 capable of containing and sealing the second package 200A.
[0129] As shown in Fig. 8, the heat-sealed bag 320 constituting the third packaging body 300A has the same structure as the heat-sealed bag 120 constituting the first packaging body 100A. That is, as shown in Fig. 3, the heat-sealed bag 320 constituting the third packaging body 300A includes a bag body 321 and a sealing portion 322 which is a strip-shaped member formed continuously with the bag body 321 and which forms an opening 327 at an end. At least a part of the sealing portion 322 of the third packaging body 300A is welded to form a heat-sealed portion 323, which makes it possible to accommodate and enclose the second packaging body 200A in the third packaging body 300A.
[0130] 8, in the third packaging 300A, the second packaging 200A is enclosed in a third space 309 defined by an inner surface 307, which is the surface of the third packaging 300A that encloses the second packaging 200A. The third packaging 300A made of a heat-sealed bag 320 has a relatively flat shape, and therefore has high storage space efficiency.
[0131] The third space 309 is filled with a filling gas FG. The filling gas FG filled in the third space 309 is Ar, air, N2, CO2, or the like, which is the same as the filling gas FG used in the filling gas FG filled in the first space 109. Among these, Ar is preferable because it has low reactivity with the sulfide solid electrolyte 3 even if the first packaging body 100A and the second packaging body 200A are damaged and the sulfide solid electrolyte 3 is exposed to the atmosphere in the third space 309. The filling gas FG filled in the third space 309 and the filling gas FG filled in the first space 109 may have the same components and concentrations or may be different. The filling gas FG present in the third space 309 is also referred to as a third space gas 319 below. The components of the third space gas 319 may change due to a reaction with the sulfide solid electrolyte 3, etc.
[0132] In the electrolyte containment structure 1AC, the concentration of H2S gas in the filling gas FG (third space gas 319) present in the third space 309 is 50 ppm or less 7 days after filling. If the concentration of H2S gas in the filling gas FG is within the above range, it is preferable because the H2S gas is unlikely to be released when the package is opened.
[0133] The preferred range of the concentration of H2S gas in the filling gas FG (third space gas 319) filled in the third space 309 and the reasons for it are the same as those for the filling gas FG (first space gas 119) filled in the first space 109.
[0134] The preferred numerical range of the dew point temperature of the filler gas FG filled in the third space 309 and the reasons therefor are similar to those of the filler gas FG filled in the first space 109.
[0135] The packaging material 310 constituting the third packaging body 300A is made of a material and has a structure that enables the concentration of H2S gas in the filling gas FG present in the third space 309 partitioned by the inner surface 307, which is the surface that encloses the second packaging body 200A, to be within a specific range.
[0136] The packaging material 310 constituting the third packaging body 300A has a multilayer structure in which the entire heat-sealed bag 320, including the sealing portion 322, has an inner welded portion 317 made of a weldable organic material and an outer non-welded portion 318, which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion 317, as shown in Figure 4.
[0137] When the packaging material 310 has such a multi-layer structure, when an outer non-welded portion 318 made of a low moisture permeable material is used, the third packaging body 300A can be provided with a third encapsulation function of enclosing the second packaging body 200A by welding the inner welded portion 317, and a third low moisture permeability function by the outer non-welded portion 318.
[0138] The inner welded portion 317 and the outer non-welded portion 318 of the third packaging body 300A are conceptually similar to the inner welded portion 117 and the outer non-welded portion 118 of the first packaging body 100A, and therefore a description thereof will be omitted.
[0139] The weldable organic material constituting the inner weld portion 317 is the same as the organic material used for the inner weld portion 117 of the first packaging body 100A for the same reasons. Note that the weldable organic material constituting the inner weld portion 317 and the weldable organic material constituting the inner weld portion 117 of the first packaging body 100A may have the same components or concentrations as or different from each other.
[0140] It is preferable that the outer unwelded portion 318 is made of a low moisture permeable material, since this can impart a third low moisture permeability function to the third package 300A.
[0141] The low moisture permeable material used for the outer unwelded portion 318 is the same as the low moisture permeable material used for the outer unwelded portion 118 of the first package 100A for the same reason.
[0142] For this reason, it is preferable that the packaging material 310 includes an aluminum layer 318 as the outer non-welded portion 318, since this makes it easier to reduce the moisture permeability of the packaging material 310.
[0143] The thickness of the packaging material 310 constituting the third packaging body 300A, at its thinnest portion, is within the same numerical range as the thickness of the packaging material 110 constituting the first packaging body 100 for the same reasons.
[0144] The thickness of the inner welded portion 317 at the thinnest portion of the third package 300A is within the same numerical range as the thickness of the inner welded portion 117 constituting the first package 100 for the same reasons.
[0145] The thickness of the outer non-welded portion 318 at the thinnest portion of the third package 300A is within the same numerical range as the thickness of the outer non-welded portion 118 constituting the first package 100 for the same reasons.
[0146] The packaging material 310 of the third packaging body 300A has a multi-layer structure as shown in Fig. 4. However, as long as the packaging material 310 has the third enclosing function, the packaging material 310 of the third packaging body 300A may have a layer structure other than the multi-layer structure shown in Fig. 4, for example, a single layer structure as shown in Fig. 13.
[0147] When the outer non-welded portion 318 is made of a low moisture permeability material, in the third packaging body 300A consisting of the heat-sealed bag 320, the material of the packaging material 310 mainly contributes to the third sealing function and the third low moisture permeability function, and the structure of the third packaging body 300A consisting of the heat-sealed bag 320 mainly contributes to the third sealing function.
[0148] For example, when the outer non-welded portion 318 of the packaging material 310 is made of a low moisture permeable material, the third sealing function is mainly realized by welding the inner welded portion 317 of the packaging material 310 of the third packaging body 300A, and the third low moisture permeability function is also mainly realized by the outer non-welded portion 318 of the packaging material 310. In addition, the third sealing function is mainly realized by the heat-sealed portion 323 of the third packaging body 300A made of the heat-sealed bag 320.
[0149] (effect) According to the electrolyte containment structure 1AC, it is possible to provide an electrolyte containment structure which is less likely to release H2S gas when opened, as compared with the electrolyte containment structure 1AB.
[0150] Moreover, according to the electrolyte containment structure 1AC, since the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to provide an electrolyte containment structure with high storage space efficiency.
[0151] The concentration of H2S gas in the filled gas FG present in the first space 109, the second space 209, and the third space 309 of the electrolyte containment structure 1AC can be measured by a known method.
[0152] <Second embodiment> Figure 9 is an oblique view showing an electrolyte containment structure according to a second embodiment of the present invention, Figure 10 is a diagram showing the internal state of the electrolyte containment structure of Figure 9, Figure 11 is an oblique view of a packaging body constituting the electrolyte containment structure of Figures 9, 14 and 16, shown with the opening closed, Figure 12 is an exploded oblique view of the packaging body constituting the electrolyte containment structure of Figure 9, and Figure 13 is a cross-sectional view of the packaging material constituting the packaging body of Figure 11.
[0153] 9 and 10, an electrolyte containment structure 1BA(1) according to the second embodiment includes a sulfide-based solid electrolyte 3 and a first packaging body 100B(100) that contains the sulfide-based solid electrolyte 3. In the electrolyte containment structure 1BA, the first packaging body 100B is made of a packaging material 110 arranged in the first layer from the sulfide-based solid electrolyte 3 side.
[0154] The electrolyte containment structure 1BA has a first space 109 partitioned between an inner surface 107 of the packaging material 110 of the first packaging body 100B and the sulfide-based solid electrolyte 3 sealed in the first packaging body 100B. In the electrolyte containment structure 1BA, when the space packed by the first packaging body 100B is partitioned by the first space 109 as the n-th space (first space 109), the concentration of H2S gas in the filling gas FG present in the first space 109 is 50 ppm or less 7 days after filling.
[0155] 9 and 10, an electrolyte containment structure 1BA(1) according to the second embodiment has a sulfide solid electrolyte 3 and a packaging body 100B(100) that contains the sulfide solid electrolyte 3. The first packaging body 100B is a bottle 130 with a lid.
[0156] 9 and 10, the first packaging body 100B is a lidded bottle 130 capable of sealing the sulfide solid electrolyte 3 in the first packaging body 100B by screwing together a male threaded portion, which is a first connecting portion 133 provided on the outer surface of a bottle body 131, and a female threaded portion, which is a second connecting portion 134 provided on the inner surface of a screw cap 132. The first packaging body 100B is a lidded bottle 130 equipped with a screw cap 132.
[0157] The electrolyte containment structure 1BA according to the second embodiment is the same as the electrolyte containment structure 1AA according to the first embodiment, except that the first packaging body 100A is replaced with a first packaging body 100B. For this reason, the same components in the electrolyte containment structure 1BA according to the second embodiment and the electrolyte containment structure 1AA according to the first embodiment are denoted by the same reference numerals, and explanations of the components and functions will be omitted or simplified.
[0158] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, the same sulfide solid electrolyte 3 as that used in the electrolyte containment structure 1AA according to the first embodiment can be used.
[0159] The first package 100B consisting of the covered bottle 130 of the electrolyte containment structure 1BA according to the second embodiment is generally less susceptible to deformation due to external forces than the package 100A consisting of the heat-sealed bag 120 of the electrolyte containment structure 1AA according to the first embodiment. Therefore, in the electrolyte containment structure 1BA according to the second embodiment, the sulfide solid electrolyte 3 is generally less susceptible to deformation due to external forces and the associated deterioration of the sulfide solid electrolyte 3 compared to the electrolyte containment structure 1AA according to the first embodiment.
[0160] Therefore, in the electrolyte containment structure 1BA of the second embodiment, the ionic conductivity of the sulfide solid electrolyte 3 is less likely to decrease over time compared to the electrolyte containment structure 1AA of the first embodiment, and it is possible to contain the sulfide solid electrolyte 3 that is easily deformed by external forces.
[0161] (First package) The first packaging body 100B is a structure in which the sulfide solid electrolyte 3 is enclosed.
[0162] In the electrolyte containment structure 1BA, the concentration of H2S gas in the filling gas FG present in the first space 109 partitioned by the inner surface 107, which is the surface of the first packaging body 100B that contains the sulfide solid electrolyte 3, and in each space in the packaging space 959, which is the entire space in the outermost packaging body 900, which is the packaging body that contains the first packaging body 100B and is the outermost packaging body of the electrolyte containment structure 1BA, is within a specific range. Specifically, in the electrolyte containment structure 1BA, the concentration of H2S gas in the filling gas FG (first space gas 119) present in the first space 109 is 50 ppm or less 7 days after filling.
[0163] In the electrolyte containment structure 1BA, the outermost packing body 900 is the first packing body 100B itself, so that the packing space 959 is the same as the first space 109. In the electrolyte containment structure 1BA, the packing space gas 969 is only the first space gas 119. That is, in the electrolyte containment structure 1BA, the filling gas FG is only the first space gas 119.
[0164] The first packaging body 100B has a function (first sealing function) of sealing the sulfide solid electrolyte 3. If the first packaging body 100B further has a first low moisture permeability function, the generation of H2S due to a reaction between the sulfide solid electrolyte 3 and moisture is suppressed, and thus H2S gas is less likely to be released when the packaging body 100B is opened, which is preferable.
[0165] As shown in FIGS. 9 to 12, the first packaging body 100B is formed by using a packaging material 110 into a bottle 130 with a lid in which the sulfide solid electrolyte 3 can be sealed.
[0166] 11 and 12, the lidded bottle 130 constituting the first packaging body 100B includes a bottle body 131 having a first connecting portion (male thread portion) 133, and a screw cap 132 having a second connecting portion (female thread portion) 134. The lidded bottle 130 is configured to be capable of sealing the sulfide solid electrolyte 3 in the first packaging body 100B by screwing the bottle body 131 and the screw cap 132 together.
[0167] 10, in first packaging body 100B, the sulfide solid electrolyte 3 is enclosed in first space 109 defined by inner surface 107, which is the surface of first packaging body 100B that encloses sulfide solid electrolyte 3. First packaging body 100B made of lidded bottle 130 generally has high mechanical strength and is resistant to deformation due to its shape, so damage to particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.
[0168] Filling gas FG is sealed in the first space 109. As the filling gas FG, Ar, air, N2, CO2, etc. are used. Among these, Ar is preferable because it has low reactivity with the sulfide solid electrolyte 3.
[0169] In the electrolyte containment structure 1BA, the concentration of H2S gas in the filling gas FG (first space gas 119, packing space gas 969) present in the first space 109 partitioned by the inner surface 107 of the first packaging body 100B, which is the surface on the side where the sulfide solid electrolyte 3 is enclosed, and in each space in the packing space 959, which is the entire space within the outermost packaging body 900, which is the packaging body that contains the first packaging body 100B and is the outermost packaging body of the electrolyte containment structure 1BA, is 50 ppm or less 7 days after filling. If the concentration of H2S gas in the filling gas FG is within the above range, it is preferable because H2S gas is less likely to be released when opening the package.
[0170] The concentration of H2S gas in the filled gas FG present in the first space 109 is preferably 30 ppm or less, more preferably 20 ppm or less, and further preferably 10 ppm or less. The concentration of H2S gas in the filled gas FG within the latter range is preferable because it is less likely to release H2S gas when opened.
[0171] The dew point temperature of the filled gas FG present in the first space 109 is preferably −20° C. or lower, more preferably −40° C. or lower, and even more preferably −60° C. or lower. The closer the dew point temperature of the filled gas FG is to the latter range, the less likely it is to release H2S gas when opened, which is preferable.
[0172] In the first packaging body 100B in which the sulfide solid electrolyte 3 is sealed, the volume V1 (cm 3 ) the volume V of the sulfide solid electrolyte 3 itself SE (cm 3 ) ratio (V SE The first packing ratio (V1) is, for example, more than 0%, preferably 10% or more, and more preferably 20% or more. The packing ratio is, for example, 50% or less, preferably 40% or less, and more preferably 30% or less. When the first packing ratio is more than 0%, the storage space efficiency tends to be high. When the first packing ratio is 50% or less, aggregation and changes in particle shape due to crushing of the particles of the sulfide solid electrolyte 3 tend to be suppressed.
[0173] The packaging material 110 constituting the first packaging body 100B is made of a material and has a structure capable of keeping the concentration of H2S gas in the filling gas FG present in the first space 109 partitioned by the inner surface 107, which is the surface on the side that encloses the sulfide solid electrolyte 3, within a specific range.
[0174] As shown in Fig. 9, the packaging material 110 constituting the first package 100B is a single-layer structure in which the entire capped bottle 130, including the bottle body 131 and the screw cap 132, is made of a single layer 116. Note that the bottle body 131 and the screw cap 132 constituting the capped bottle 130 have different shapes depending on the location, but have one thing in common in that the packaging material 110 is made of a single layer 116.
[0175] The packaging material 110 consisting of a single layer 116 constituting the first packaging body 100B is preferably made of a material having low moisture permeability.
[0176] When the single layer 116 is made of a low moisture permeable material, it is possible to impart a low moisture permeability function to the first packaging body 100B.
[0177] The low moisture permeable material used in the single layer 116 is the same as the low moisture permeable material used in the outer non-welded portion 118 of the first packaging body 100A of the electrolyte encapsulation structure 1AA according to the first embodiment. Specifically, the low moisture permeable material used in the single layer 116 is, for example, metals such as aluminum, stainless steel, and iron; and organic substances such as one or more organic resins selected from polyethylene terephthalate (PET), polyethylene PE, chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol. Among these, it is preferable that the first packaging body 100B is made of aluminum, since it is easy to reduce the moisture permeability of the packaging material 110 constituting the first packaging body 100B and it is lightweight.
[0178] When the low moisture permeable material used in the single layer 116 of the first package 100B is aluminum, the first package 100B becomes a lidded bottle 130 made of aluminum. When the low moisture permeable material used in the single layer 116 of the first package 100B is high density polyethylene, the first package 100B becomes a lidded bottle 130 made of high density polyethylene.
[0179] The thickness of the packaging material 110 constituting the first packaging body 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because the moisture permeability is easily reduced.
[0180] When the first packaging body 100B is a lidded bottle 130 made of aluminum, the thickness of the packaging material 110 constituting the first packaging body 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first packaging body 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because the moisture permeability is easily reduced.
[0181] When the first package 100B is a lidded bottle 130 made of high density polyethylene, the thickness of the packaging material 110 constituting the first package 100B is, for example, 50 μm or more, preferably 100 μm or more, at the thinnest part of the first package 100B. The thickness of the thinnest part is preferably 10,000 μm or less. If the thickness of the packaging material 110 is within the above range, it is preferable because it is easy to reduce the moisture permeability.
[0182] When the single layer 116 is made of a low moisture permeable material, in the first packaging body 100B consisting of a capped bottle 130, the material of the packaging material 110 mainly contributes to the low moisture permeability function, and the structure of the first packaging body 100B consisting of the capped bottle 130 mainly contributes to the sealing function.
[0183] For example, when the single layer 116 of the packaging material 110 of the first packaging body 100B is made of a low moisture permeable material, the low moisture permeability function is also mainly exhibited. Also, the sealing function is mainly exhibited by the screwing of the bottle body 131 and the screw cap 132 of the first packaging body 100B made of the lidded bottle 130.
[0184] (effect) According to the electrolyte containment structure 1BA, it is possible to provide an electrolyte containment structure that is less likely to release H2S gas when opened.
[0185] Furthermore, according to the electrolyte containment structure 1BA, the first packaging body 100B consisting of the lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so that damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.
[0186] The concentration of H2S gas in the filled gas FG present in the first space 109 of the first packaging body 100A of the electrolyte containment structure 1BA can be measured by a known method.
[0187] <First Modification of the Second Embodiment> FIG. 14 is a perspective view showing an electrolyte containment structure according to a first modified example of the second embodiment of the present invention, and FIG. 15 is a diagram showing the internal state of the electrolyte containment structure of FIG. 14.
[0188] 14 and 15, an electrolyte containment structure 1BB(1) according to a first modified example of the second embodiment includes a sulfide-based solid electrolyte 3, a first package 100B(100) that contains the sulfide-based solid electrolyte 3, and a second package 200A(200) that contains the first package 100B. In the electrolyte containment structure 1BB, the first package 100B and the second package 200A are made of packaging materials 110, 210 arranged in the first and second layers from the sulfide-based solid electrolyte 3 side.
[0189] The electrolyte containment structure 1BB has a first space 109 defined between an inner surface 107 of the packaging material 110 of the first packaging body 100B and the sulfide-based solid electrolyte 3 contained in the first packaging body 100B. The electrolyte containment structure 1BB also has a second space 209 defined between an inner surface 207 of the packaging material 210 of the second packaging body 200A and the first packaging body 100B. In the electrolyte containment structure 1BB, the first packaging body 100B, in which n is 1, contains the sulfide-based solid electrolyte 3, and there is a packaging body that contains the first packaging body 100B, and the n-th packaging body (second packaging body 200A) that contains the first packaging body 100B is provided such that n increases in sequence toward the outer surface side of the first packaging body 100B. In the electrolyte encapsulation structure 1BB, when the space packaged in the first packaging body 100B is defined as the first space 109, and the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100B) is defined as the nth space (second space 209), the concentration of H2S gas in the filled gas FG present in each space (first space 109, second space 209) from the first space 109 to the nth space (second space 209) is 50 ppm or less 7 days after filling.
[0190] As shown in Fig. 14 and Fig. 15, the electrolyte containment structure 1BB (1) according to the first modification of the second embodiment includes a first package 100B (100) that contains a sulfide solid electrolyte 3, and a second package 200A (200) that contains and contains the first package 100B. The first package 100B is made of a bottle 130 with a lid, and is usually contained and contained in the second package 200A of the electrolyte containment structure 1BB with a thickness equal to the diameter of the bottle. Therefore, the bag body 221 of the second package 200A that contains and contains the first package 100B and the electrolyte containment structure 1BB have a thickness in the direction perpendicular to the plane of Fig. 14.
[0191] The electrolyte containment structure 1BB according to the first modified example of the second embodiment is an electrolyte containment structure 1BA according to the second embodiment further including a second packaging body 200A that accommodates and encloses the first packaging body 100B.
[0192] As shown in FIG. 3, the second packaging body 200A is turned into a heat-sealed bag 220 capable of enclosing the first packaging body 100B by forming a heat-sealed portion 223 by welding at least a portion of the sealing portion 222.
[0193] The electrolyte containment structure 1BB according to the first modification of the second embodiment is the same as the electrolyte containment structure 1BA according to the second embodiment except that it further includes a second packaging body 200A. Therefore, the same components in the electrolyte containment structure 1BB according to the first modification of the second embodiment and the electrolyte containment structure 1BA according to the second embodiment are denoted by the same reference numerals, and the description of the components and functions is omitted or simplified. The following mainly describes the second packaging body 200A.
[0194] (Second packaging) The second packaging body 200A is a structure that houses and encloses the first packaging body 100B. The second packaging body 200A constituting the electrolyte containment structure 1BB according to the first modification of the second embodiment is similar to the second packaging body 200A constituting the electrolyte containment structure 1AB according to the first modification of the first embodiment. Therefore, the description of the configuration and function of the second packaging body 200A will be omitted. In the electrolyte containment structure 1BB, the concentration of H2S gas in the filling gas FG (first space gas 119 and second space gas 219) present in each space of the first space 109 and the second space 209 is 50 ppm or less 7 days after filling.
[0195] In the electrolyte containment structure 1BB, the outermost packaging body 900 is the second packaging body 200A. In the electrolyte containment structure 1BB, the packaging space 959 becomes the first space 109 and the second space 209. In the electrolyte containment structure 1BB, the packaging space gas 969 becomes the first space gas 119 and the second space gas 219. That is, in the electrolyte containment structure 1BB, the filling gas FG becomes the first space gas 119 and the second space gas 219.
[0196] (effect) According to the electrolyte containment structure 1BB, it is possible to provide an electrolyte containment structure that is less likely to release H2S gas when opened.
[0197] Furthermore, according to the electrolyte containment structure 1BB, the first packaging body 100B consisting of the lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so that damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.
[0198] The concentration of H2S gas in the filled gas FG present in the first space 109 and the second space 209 of the electrolyte containment structure 1BB can be measured by a known method.
[0199] <Second Modification of the Second Embodiment> FIG. 16 is a plan view showing an electrolyte containment structure according to a second modified example of the second embodiment of the present invention, and FIG. 17 is a diagram showing the internal state of the electrolyte containment structure of FIG. 16.
[0200] 16 and 17, an electrolyte containment structure 1BC (1) according to a second modification of the second embodiment includes a sulfide-based solid electrolyte 3, a first package 100B (100) that contains the sulfide-based solid electrolyte 3, a second package 200A (200) that contains the first package 100B, and a third package 300A (300) that contains the second package 200A. In the electrolyte containment structure 1BC, the first package 100B, the second package 200A, and the third package 300A are made of packaging materials 110, 210, and 310 arranged in the first, second, and third layers from the sulfide-based solid electrolyte 3 side.
[0201] The electrolyte containment structure 1BC has a first space 109 defined between an inner surface 107 of the packaging material 110 of the first packaging body 100B and the sulfide-based solid electrolyte 3 contained in the first packaging body 100B. The electrolyte containment structure 1BC also has a second space 209 defined between an inner surface 207 of the packaging material 210 of the second packaging body 200A and the first packaging body 100B. The electrolyte containment structure 1BC also has a third space 309 defined between an inner surface 307 of the packaging material 310 of the third packaging body 300A and the second packaging body 200A. In the electrolyte containment structure 1BC, the first packaging body 100B, in which n is 1, contains a sulfide-based solid electrolyte 3, and there are packaging bodies that contain the first packaging body 100B, and the nth packaging body (second packaging body 200A, third packaging body 300A) that contains the first packaging body 100B is arranged so that n increases in sequence toward the outer surface side of the first packaging body 100B. In the electrolyte encapsulation structure 1BC, when the space packaged by the first packaging body 100B is defined as the first space 109, the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100B) is defined as the nth space (second space 209), and the space partitioned by the nth packaging body (third packaging body 300A) and the n-1th packaging body (second packaging body 200A) is defined as the nth space (third space 309), the concentration of H2S gas in the filled gas FG present in each space (first space 109, second space 209, third space 309) from the first space 109 to the nth space (second space 209) is 50 ppm or less 7 days after filling.
[0202] 16 and 17, an electrolyte containment structure 1BC(1) according to the second modification of the second embodiment includes a first package 100B(100) that contains a sulfide solid electrolyte 3, a second package 200A(200) that contains and contains the first package 100B, and a third package 300A(300) that contains and contains the second package 200A. The electrolyte containment structure 1BC includes an electrolyte containment structure 1BB, and therefore has a thickness in the direction perpendicular to the plane of FIG.
[0203] The electrolyte containment structure 1BC according to the second variant of the second embodiment is an electrolyte containment structure 1BB according to the first variant of the second embodiment, further including a third packaging body 300A that accommodates and encloses the second packaging body 200A.
[0204] As shown in FIG. 3, the third packaging body 300A is formed into a heat-sealed bag 320 capable of enclosing the second packaging body 200A by forming a heat-sealed portion 323 by welding at least a portion of the sealing portion 322.
[0205] The electrolyte containment structure 1BC according to the second modification of the second embodiment is the same as the electrolyte containment structure 1BB according to the first modification of the second embodiment, except that it further includes a third packaging body 300A. Therefore, the same components in the electrolyte containment structure 1BC according to the second modification of the second embodiment and the electrolyte containment structure 1BB according to the first modification of the second embodiment are denoted by the same reference numerals, and the description of the components and functions is omitted or simplified. The following mainly describes the third packaging body 300A.
[0206] (Third packaging) The third packaging body 300A is a structure that contains and encloses the second packaging body 200A. The third packaging body 300A constituting the electrolyte containment structure 1BC according to the second modified example of the second embodiment is similar to the third packaging body 300A constituting the electrolyte containment structure 1AC according to the second modified example of the first embodiment. Therefore, a description of the configuration and function of the third packaging body 300A will be omitted. Note that, in the electrolyte containment structure 1BC, When the space packed with the first packaging body 100B is defined as the first space 109, the space partitioned by the nth packaging body (second packaging body 200A) and the n-1th packaging body (first packaging body 100B) is defined as the nth space (second space 209), and the space partitioned by the nth packaging body (third packaging body 300A) and the n-1th packaging body (second packaging body 200A) is defined as the nth space (third space 309), the concentration of H2S gas in the filled gas FG (first space gas 119, second space gas 219, and third space gas 319) present in each space (first space 109, second space 209, third space 309) from the first space 109 to the nth space (third space 309) is 50 ppm or less 7 days after filling.
[0207] In the electrolyte containment structure 1BC, the outermost packaging body 900 is the third packaging body 300A. In the electrolyte containment structure 1BC, the packaging space 959 is the first space 109, the second space 209, and the third space 309. In the electrolyte containment structure 1BC, the packaging space gas 969 is the first space gas 119, the second space gas 219, and the third space gas 319. That is, in the electrolyte containment structure 1BC, the filling gas FG is the first space gas 119, the second space gas 219, and the third space gas 319.
[0208] (effect) According to the electrolyte containment structure 1BC, it is possible to provide an electrolyte containment structure that is less likely to release H2S gas when opened.
[0209] In addition, according to the electrolyte containment structure 1BC, the first packaging body 100B consisting of the lidded bottle 130 generally has high mechanical strength and is not easily deformed due to its shape, so damage to the particles of the enclosed sulfide solid electrolyte 3 is strongly suppressed.
[0210] The concentration of H2S gas in the filled gas FG present in the first space 109, the second space 209, and the third space 309 of the electrolyte containment structure 1BC can be measured by a known method.
[0211] In the above-mentioned electrolyte containment structures 1AA, 1AB, 1AC, 1BA, 1BB, and 1BC, examples have been shown in which the heat-sealed bag 120 (220, 320) and the lidded bottle 130 are used as the first package 100, the second package 200, and the third package 300. However, the shape and structure of each package of the electrolyte containment structure 1 according to the present invention are not particularly limited as long as they can contain the contents. As each package of the electrolyte containment structure 1 according to the present invention, in addition to the heat-sealed bag and the lidded bottle, for example, a container, a drum can, etc. can be used.
[0212] Further, in the above-mentioned electrolyte containment structures 1AA, 1AB, 1AC, 1BA, 1BB, and 1BC, examples have been shown that include the first package 100, the second package 200, and the third package 300. However, the electrolyte containment structure 1 according to the present invention may include further packages such as a fourth package (not shown) that encloses the third package 300.
[0213] [Method of manufacturing electrolyte encapsulation structure] Next, a method for manufacturing the electrolyte encapsulation structure 1 according to the present invention will be described. The method for manufacturing the electrolyte encapsulation structure 1 according to the present invention is a method for manufacturing an electrolyte encapsulation structure having a sulfide-based solid electrolyte 3 and a packaging body that encapsulates the sulfide-based solid electrolyte 3, the packaging body being made of packaging materials arranged in an n-th layer (n is an integer of 1 or more) from the sulfide-based solid electrolyte 3 side, a first packaging body in which n is 1 encapsulates the sulfide-based solid electrolyte 3, and when a packaging body that encapsulates the first packaging body exists, the packaging body that packages the first packaging body has n that increases in sequence toward the outer surface side of the first packaging body. The method for manufacturing the electrolyte encapsulation structure 1 according to the present invention includes a sealing step of filling the filled gas so that the concentration of H2S gas in the filled gas present in each space from the first space to the nth space becomes 50 ppm or less 7 days after filling, when the space packed by the first packaging body is defined as the first space and the space partitioned by the nth packaging body and the n-1th packaging body is defined as the nth space.
[0214] The manufacturing method of the electrolyte containment structure 1 of the present invention includes a filling step of filling a filled gas so that the concentration of H2S gas in each space from the first space to the nth space of the electrolyte containment structure 1 is 50 ppm or less 7 days after filling.
[0215] (Encapsulation process) The filling step is a step of filling the filling gas FG so that the concentration of H2S gas in the filling gas FG present in each space from the first space to the nth space of the electrolyte containment structure becomes 50 ppm or less 7 days after filling. In other words, the filling step is a step of filling the filling gas FG so that the concentration of H2S gas in the filling gas FG filled in each space of the first packaging body 100 itself or each space in the packaging space 959, which is the entire space in the outermost packaging body 900 that is a packaging body that contains the first packaging body 100 and is the outermost packaging body of the electrolyte containment structure 1, becomes 50 ppm or less 7 days after filling.
[0216] For example, when manufacturing an electrolyte containment structure 1AA, the outermost packaging body 900 is the first packaging body 100A itself, the packaging space 959 is only the first space 109, and the packaging space gas 969 is only the first space gas 119. In the electrolyte containment structure 1AA, the concentration of H2S gas in the filling gas FG filled in the first space 109 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119 is set to 50 ppm or less 7 days after filling.
[0217] When manufacturing the electrolyte containment structure 1AB, the outermost packaging body 900 is the second packaging body 200A, the packaging space 959 becomes the first space 109 and the second space 209, and the packaging space gas 969 becomes the first space gas 119 and the second space gas 219. In the electrolyte containment structure 1AB, the concentration of H2S gas in the filling gas FG filled in each of the first space 109 and the second space 209 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119 and the second space gas 219 is set to 50 ppm or less 7 days after filling.
[0218] When manufacturing the electrolyte containment structure 1AC, the outermost packaging body 900 is the third packaging body 300A, the packaging space 959 is the first space 109, the second space 209, and the third space 309, and the packaging space gas 969 is the first space gas 119, the second space gas 219, and the third space gas 319. In the electrolyte containment structure 1AC, the concentration of H2S gas in the filling gas FG filled in each of the first space 109, the second space 209, and the third space 309 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119, the second space gas 219, and the third space gas 319 is set to 50 ppm or less 7 days after filling.
[0219] When manufacturing the electrolyte containment structure 1BA, the outermost packaging body 900 is the first packaging body 100B itself, the packaging space 959 is only the first space 109, and the packaging space gas 969 is only the first space gas 119. In the electrolyte containment structure 1BA, the concentration of H2S gas in the filling gas FG filled in the first space 109 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119 is set to 50 ppm or less 7 days after filling.
[0220] When manufacturing an electrolyte containment structure 1BB, the outermost packaging body 900 is the second packaging body 200A, the packaging space 959 becomes the first space 109 and the second space 209, and the packaging space gas 969 becomes the first space gas 119 and the second space gas 219. In the electrolyte containment structure 1BB, the concentration of H2S gas in the filling gas FG filled in each of the first space 109 and the second space 209 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119 and the second space gas 219 is set to 50 ppm or less 7 days after filling.
[0221] When manufacturing an electrolyte containment structure 1BC, the outermost packaging body 900 is the third packaging body 300A, the packaging space 959 is the first space 109, the second space 209, and the third space 309, and the packaging space gas 969 is the first space gas 119, the second space gas 219, and the third space gas 319. In the electrolyte containment structure 1BC, the concentration of H2S gas in the filling gas FG filled in each of the first space 109, the second space 209, and the third space 309 is set to 50 ppm or less, so that the concentration of H2S gas in the first space gas 119, the second space gas 219, and the third space gas 319 is set to 50 ppm or less 7 days after filling.
[0222] If the concentration of H2S gas in the filling gas FG sealed in each of the n-th spaces is within the above range, it is preferable because the H2S gas is unlikely to be released when the electrolyte containment structure 1 is opened.
[0223] The concentration of H2S gas in the filled gas FG sealed in each of the n-th spaces is preferably 30 ppm or less, more preferably 20 ppm or less, and further preferably 10 ppm or less. The concentration of H2S gas in the filled gas FG sealed in the latter range is preferable because it is less likely to release H2S gas when opened.
[0224] The dew point temperature of the filled gas FG is preferably −20° C. or lower, more preferably −40° C. or lower, and further preferably −60° C. or lower. The closer the dew point temperature of the filled gas FG is to the latter range, the less likely it is to release H2S gas when opened, which is preferable.
[0225] (drying process) The manufacturing method of the electrolyte encapsulation structure 1 according to the present invention preferably further includes a drying step of drying the first packaging body 100 at 50° C. or higher before the encapsulation step. If the manufacturing method of the electrolyte encapsulation structure 1 according to the present invention further includes a drying step, the sulfide solid electrolyte 3 encapsulated in the first packaging body 100A reacts with moisture attached to the first packaging body 100A, which is preferable because generation of H2S gas is suppressed.
[0226] The drying temperature in the drying step is preferably 60°C or higher, more preferably 70°C or higher. The drying temperature is preferably 200°C or lower, more preferably 150°C or lower. If the drying temperature has the above lower limit, the moisture adhering to the inside of the first packaging body 100A is reduced, and therefore the reaction between the sulfide solid electrolyte 3 enclosed in the first packaging body 100A and the moisture is suppressed, and as a result, the generation of H2S gas is suppressed, which is preferable. If the drying temperature has the above upper limit, the change in the material and shape of the packaging body is easily suppressed.
[0227] The drying time in the drying step is preferably 30 minutes or more, more preferably 1 hour or more, and further preferably 5 hours or more. If the drying time is within the above range, the sulfide solid electrolyte 3 sealed in the first packaging body 100A reacts with the moisture attached to the first packaging body 100A, and generation of H2S gas is suppressed, which is preferable.
[0228] The drying process may include, in addition to the above-mentioned drying treatment of the first package 100, a step of drying the second package 200 at 50°C or higher and a step of drying the third package 300 at 50°C or higher.
[0229] (effect) According to the manufacturing method of the electrolyte containment structure of the present invention, it is possible to manufacture an electrolyte containment structure 1 that is less likely to release H2S gas when opened.
[0230] Furthermore, according to the manufacturing method of the electrolyte containment structure of the present invention, since the first package 100A made of the heat-sealed bag 120 has a relatively flat shape, it is possible to manufacture an electrolyte containment structure 1 that has high storage space efficiency.
[0231] The concentration of H2S gas in the filled gas FG present in each of the n-th spaces of the electrolyte containment structure 1 can be measured by a known method. EXAMPLES
[0232] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0233] [Example 1] The electrolyte containment structure 1BC shown in Fig. 16 was produced as follows. The conditions for producing the electrolyte containment structure 1BC are shown in Table 1.
[0234] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, a sulfide solid electrolyte having an argyrodite-type crystal structure containing Li, P, S, Cl, and Br (D 50 A 0.7 μm thick film was prepared.
[0235] (First package) As the raw material for the first package 100B, a capped bottle 130 shown in Figures 11 and 12 was prepared. The packaging material 110 for the capped bottle 130 was a single layer 116 made of high-density polyethylene. The minimum thickness of the packaging material 110 for the first package 100B was 950 μm.
[0236] (Second packaging) As the raw material of the second packaging body 200A, a heat-sealed bag 220 shown in Fig. 3 was prepared. The packaging material 210 of the heat-sealed bag 220 had a multi-layer structure in which an inner welded portion 217 made of chlorinated polyethylene SPE and polyethylene PE and an outer non-welded portion 218 made of aluminum Al, chlorinated polyethylene SPE, and polyethylene PE were laminated, and the minimum thickness of the entire packaging material 210 of the second packaging body 200A was 110 µm. The inner welded portion 217 had an innermost layer made of polyethylene PE and including the inner surface 207, and a first adjacent inner layer made of chlorinated polyethylene SPE laminated on the outer non-welded portion 218 side as viewed from the innermost layer. The outer non-welded portion 218 comprised an outermost layer made of polyethylene PE and including the outer surface 208, a first adjacent outer layer made of chlorinated polyethylene SPE and laminated to the inner welded portion 217 side as viewed from the outermost layer, and a second adjacent outer layer made of aluminum and laminated to the inner welded portion 217 side as viewed from the first adjacent outer layer. Packaging material 210 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 207 to outer surface 208.
[0237] (Third packaging) As the raw material of the third packaging body 300A, a heat-sealed bag 320 shown in Fig. 3 was prepared. The packaging material 310 of the heat-sealed bag 320 had a multi-layer structure in which an inner welded portion 317 made of chlorinated polyethylene SPE and polyethylene PE and an outer non-welded portion 318 made of aluminum Al, chlorinated polyethylene SPE, and polyethylene PE were laminated, and the minimum thickness of the entire packaging material 310 of the third packaging body 300A was 110 µm. The inner welded portion 317 had an innermost layer made of polyethylene PE and including the inner surface 307, and a first adjacent inner layer made of chlorinated polyethylene SPE laminated on the outer non-welded portion 318 side as viewed from the innermost layer. The outer non-welded portion 318 comprised an outermost layer made of polyethylene PE and including the outer surface 308, a first adjacent outer layer made of chlorinated polyethylene SPE and laminated to the inner welded portion 317 side as viewed from the outermost layer, and a second adjacent outer layer made of aluminum and laminated to the inner welded portion 317 side as viewed from the first adjacent outer layer. Packaging material 310 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 307 to outer surface 308.
[0238] (packing) 11 and 12 were heated and dried at 80° C. for 10 hours, and then allowed to cool to 25° C. Thereafter, at room temperature in an Ar gas atmosphere, the sulfide solid electrolyte 3 was charged into the bottle body 131 through the opening 137, and the screw cap 132 was screwed onto the bottle body 131, thereby sealing the sulfide solid electrolyte 3 in the first package 100B.
[0239] Next, the heat-sealed bag 220 shown in Fig. 3 was heated and dried at 80°C for 10 hours, and then allowed to cool to 25°C. Thereafter, at room temperature and in an Ar gas atmosphere, the first packaging body 100B was inserted into the heat-sealed bag 220 through the opening 227, and a part of the sealed portion 222 was welded to form the heat-sealed portion 223, thereby sealing the first packaging body 100B in the second packaging body 200A.
[0240] Furthermore, the heat-sealed bag 320 shown in FIG. 3 was heated at 80° C. for 10 hours, dried, and then cooled to 25° C. Thereafter, at room temperature and in an Ar gas atmosphere, the second packaging body 200A in which the first packaging body 100B was sealed was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing portion 322 was welded to form a heat-sealed portion 323, thereby sealing the second packaging body 200A in the third packaging body 300A. In this way, the electrolyte encapsulation structure 1BC shown in FIG. 12 was produced. In this way, the electrolyte encapsulation structure 1BC shown in FIG. 16 was produced.
[0241] [Table 1]
[0242] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1BC was stored in the atmosphere at 25° C. for 7 days. When the electrolyte containment structure 1BC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0243] [Example 2] The electrolyte containment structure 1AB shown in Fig. 5 was produced as follows. The conditions for producing the electrolyte containment structure 1AB are shown in Table 1.
[0244] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, a sulfide solid electrolyte having an argyrodite-type crystal structure containing Li, P, S, Cl, and Br, the same as in Example 1, was prepared.
[0245] (First package) As the raw material of the first packaging body 100A, a heat-sealed bag 120 shown in Fig. 3 was prepared. The packaging material 110 of the heat-sealed bag 120 had a multi-layer structure in which an inner welded portion 117 made of chlorinated polyethylene SPE and polyethylene PE and an outer non-welded portion 118 made of aluminum Al {chlorinated polyethylene SPE and polyethylene PE} were laminated, and the minimum thickness of the entire packaging material 110 of the first packaging body 100A was 110 μm. The inner welded portion 117 had an innermost layer made of polyethylene PE and including the inner surface 107, and a first adjacent inner layer made of chlorinated polyethylene SPE laminated on the outer non-welded portion 118 side as viewed from the innermost layer. The outer non-welded portion 118 comprised an outermost layer made of polyethylene PE and including the outer surface 108, a first adjacent outer layer made of chlorinated polyethylene SPE and laminated to the inner welded portion 117 side as viewed from the outermost layer, and a second adjacent outer layer made of aluminum and laminated to the inner welded portion 117 side as viewed from the first adjacent outer layer. Packaging material 110 had a PE layer, an SPE layer, an Al layer, an SPE layer, and a PE layer laminated in this order from inner surface 107 to outer surface .
[0246] (Second packaging) As the raw material of the second package 200A, the same heat seal bag 220 as in Example 1 was prepared. The minimum thickness of the entire package material 210 of the second package 200A was 110 μm.
[0247] (packing) 3 was heated and dried at 80° C. for 10 hours, and then allowed to cool to 25° C. Thereafter, at room temperature and in an Ar gas atmosphere, the sulfide solid electrolyte 3 was placed in the heat-sealed bag 120 through the opening 127, and a part of the sealed portion 122 was welded to form the heat-sealed portion 123, thereby sealing the sulfide solid electrolyte 3 in the first package 100A.
[0248] Next, the heat-sealed bag 220 shown in Fig. 3 was heated at 80°C for 10 hours to dry, and then allowed to cool to 25°C. Thereafter, at room temperature and in an Ar gas atmosphere, the first packaging body 100A containing the sulfide solid electrolyte 3 was inserted into the heat-sealed bag 220 through the opening 227, and a part of the sealing portion 222 was welded to form a heat-sealed portion 223, thereby sealing the first packaging body 100A in the second packaging body 200A. In this way, the electrolyte encapsulation structure 1AB shown in Fig. 5 was produced.
[0249] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1AB was stored in air at 25° C. for 7 days. When the electrolyte containment structure 1AB was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119 and the second space gas 219 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0250] [Example 3] The electrolyte encapsulation structure 1BC shown in Fig. 16 was produced in the same manner as in Example 1, except that the first packaging body 100B had a volume of 500 ml as shown below, the first filling rate was changed, and the heat-sealed bag 320 used in the third packaging body 300A was not dried. The conditions for the electrolyte encapsulation structure 1BC are shown in Table 1. The specific packaging procedure is as follows.
[0251] (First package) As the raw material for the first package 100B, a capped bottle 130 shown in Figures 11 and 12 was prepared. The packaging material 110 for the capped bottle 130 was a single layer 116 made of high density polyethylene.
[0252] Next, in the same manner as in Example 1, the first package 100B was enclosed in the second package 200A.
[0253] The second packaging body 200A was enclosed in the third packaging body 300A in the same manner as in Example 1. In this manner, the electrolyte containment structure 1BC shown in Fig. 12 was produced. In this manner, the electrolyte containment structure 1BC shown in Fig. 16 was produced.
[0254] (evaluation) <Storage test in air> In the same manner as in Example 1, when the electrolyte containment structure 1BC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0255] [Example 4] An electrolyte encapsulation structure 1BC shown in Fig. 16 was produced in the same manner as in Example 1, except that the first packaging body 100B, the second packaging body 200A, and the third packaging body 300A were not heated and dried during packaging. The conditions for the electrolyte encapsulation structure 1BC are shown in Table 1. The specific packaging procedure is described below.
[0256] (packing) 11 and 12 were prepared. At room temperature in an Ar gas atmosphere, the sulfide solid electrolyte 3 was charged into the bottle body 131 from the opening 137, and the screw cap 132 was screwed onto the bottle body 131 to enclose the sulfide solid electrolyte 3 in the first packaging body 100B.
[0257] Next, the heat seal bag 220 shown in Fig. 3 was prepared. At room temperature and in an Ar gas atmosphere, the first package 100B was inserted into the heat seal bag 220 through the opening 227, and a part of the sealing portion 222 was welded to form the heat seal portion 223, thereby sealing the first package 100B in the second package 200A.
[0258] Further, a heat-sealed bag 320 shown in Fig. 3 was prepared. At room temperature and in an Ar gas atmosphere, the second packaging body 200A enclosing the first packaging body 100B was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing part 322 was welded to form a heat-sealed part 323, thereby enclosing the second packaging body 200A in the third packaging body 300A. In this way, an electrolyte encapsulation structure 1BC shown in Fig. 16 was produced.
[0259] (evaluation) <Storage test in air> In the same manner as in Example 1, when the electrolyte containment structure 1BC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0260] [Example 5] The electrolyte containment structure 1AC shown in Fig. 7 was produced as follows. The conditions for producing the electrolyte containment structure 1AC are shown in Table 1.
[0261] (Sulfide solid electrolyte) As the sulfide solid electrolyte 3, a sulfide solid electrolyte having an argyrodite-type crystal structure containing Li, P, S, Cl, and Br, the same as in Example 1, was prepared.
[0262] (First package) As the raw material of the first package 100A, the same heat seal bag 120 as in Example 2 was prepared. The minimum thickness of the entire package material 110 of the first package 100A was 110 μm.
[0263] (Second packaging) As the raw material of the second package 200A, the same heat seal bag 220 as in Example 1 was prepared. The minimum thickness of the entire package material 210 of the second package 200A was 110 μm.
[0264] (Third packaging) As the raw material of the third package 300A, the same heat seal bag 320 as in Example 1 was prepared. The minimum thickness of the entire package material 310 of the third package 300A was 110 μm.
[0265] (packing) A heat-sealed bag 120 shown in Fig. 3 was prepared. At room temperature and in an Ar gas atmosphere, the sulfide solid electrolyte 3 was charged into the heat-sealed bag 120 from the opening 127, and a part of the sealed portion 122 was welded to form the heat-sealed portion 123, thereby sealing the sulfide solid electrolyte 3 in the first package 100A.
[0266] Next, the heat seal bag 220 shown in Fig. 3 was prepared. At room temperature and in an Ar gas atmosphere, the first package 100A was inserted into the heat seal bag 220 through the opening 227, and a part of the sealing portion 222 was welded to form the heat seal portion 223, thereby sealing the first package 100A in the second package 200A.
[0267] Further, a heat-sealed bag 320 shown in Fig. 3 was prepared. At room temperature and in an Ar gas atmosphere, the second packaging body 200A enclosing the first packaging body 100A was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing part 322 was welded to form a heat-sealed part 323, thereby enclosing the second packaging body 200A in the third packaging body 300A. In this way, an electrolyte encapsulation structure 1AC shown in Fig. 7 was produced.
[0268] (evaluation) <Storage test in air> The electrolyte encapsulation structure 1AC was stored in air at 25° C. for 7 days. When the electrolyte containment structure 1AC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0269] [Example 6] The electrolyte encapsulation structure 1BC shown in Fig. 16 was produced in the same manner as in Example 3, except that the first packaging body 100B had a volume of 500 ml as shown below, and the packaging atmosphere was changed from Ar gas to dry air (dew point temperature -48°C) in a dry room. The conditions for the electrolyte encapsulation structure 1BC are shown in Table 1. The specific packaging procedure is as follows.
[0270] (First package) As the first package 100B, a bottle 130 with a lid as shown in Figures 11 and 12 was prepared. The packaging material 110 of the bottle 130 with a lid was a single layer 116 made of high-density polyethylene. The minimum thickness of the packaging material 110 of the first package 100B was 950 μm.
[0271] (packing) 11 and 12 were prepared. In dry air (dew point temperature -48°C) in a dry room, the sulfide solid electrolyte 3 was charged into the bottle body 131 from the opening 137, and the screw cap 132 was screwed onto the bottle body 131 to enclose the sulfide solid electrolyte 3 in the first package 100B.
[0272] Next, a heat seal bag 220 shown in Fig. 3 was prepared. In dry air (dew point temperature -48°C) in a dry room, the first package 100B was inserted into the heat seal bag 220 through the opening 227, and a part of the sealing part 222 was welded to form a heat seal part 223, thereby sealing the first package 100B in the second package 200A.
[0273] Further, a heat-sealed bag 320 shown in Fig. 3 was prepared. In dry air (dew point temperature -48°C) in a dry room, the second package 200A enclosing the first package 100B was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing portion 322 was welded to form a heat-sealed portion 323, thereby enclosing the second package 200A in the third package 300A. In this way, an electrolyte encapsulation structure 1BC shown in Fig. 16 was produced.
[0274] (evaluation) <Storage test in air> In the same manner as in Example 1, when the electrolyte containment structure 1BC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0275] [Comparative Example 1] An electrolyte encapsulation structure 1BC shown in Fig. 16 was produced in the same manner as in Example 6, except that the atmosphere during packaging was changed from dry air (dew point temperature -48°C) in a dry room to air with a dew point temperature of 10°C. The conditions for the electrolyte encapsulation structure 1BC are shown in Table 1. The specific packaging procedure is as follows.
[0276] (packing) 11 and 12 were prepared. The sulfide solid electrolyte 3 was charged into the bottle body 131 from the opening 137 in the atmosphere with a dew point temperature of 10° C., and the screw cap 132 was screwed onto the bottle body 131 to enclose the sulfide solid electrolyte 3 in the first packaging body 100B.
[0277] Next, a heat seal bag 220 shown in Fig. 3 was prepared. In the atmosphere with a dew point temperature of 10°C, the first package 100B was inserted into the heat seal bag 220 through the opening 227, and a part of the sealing part 222 was welded to form a heat seal part 223, thereby sealing the first package 100B in the second package 200A.
[0278] Further, a heat-sealed bag 320 shown in Fig. 3 was prepared. In the atmosphere with a dew point temperature of 10°C, the second packaging body 200A enclosing the first packaging body 100B was inserted into the heat-sealed bag 320 through the opening 327, and a part of the sealing part 322 was welded to form a heat-sealed part 323, thereby enclosing the second packaging body 200A in the third packaging body 300A. In this way, an electrolyte encapsulation structure 1BC shown in Fig. 16 was produced.
[0279] (evaluation) <Storage test in air> In the same manner as in Example 1, when the electrolyte containment structure 1BC was opened after 7 days of storage, the H2S concentration (ppm) in each of the first space gas 119, the second space gas 219, and the third space gas 319 was measured. The results are shown in Table 1. The H2S concentration (ppm) was measured using a hydrogen sulfide detector tube (4LL) manufactured by Gastec Corporation.
[0280] From the examples and comparative examples, it was found that in the electrolyte containment structure 1 of the examples, the concentration of H2S gas in the filled gas present in the first space 109 was 50 ppm or less. [Explanation of symbols]
[0281] 1, 1AA, 1AB, 1AC, 1BA, 1BB, 1BC Electrolyte Encapsulation Structure 3 Sulfide solid electrolyte 100, 100A, 100B 1st package 107 Inside 108 Exterior 109 1st space 110 Packaging materials 116 Single Layer 117 Inner weld 118 Outside non-welded part 119 First Space Gas 120 Heat seal bag 121 Bag body 122 Sealing part 123 Heat seal section 127 Opening 130 Bottle with lid 131 Bottle body 132 Screw Cap 133 1st connection part 134 2nd connection part 137 Opening 140 Ziplock bag 141 Bag body 142 Sealing part 143 Chuck part 147 Opening 200, 200A 2nd package 207 Inside 208 Exterior 209 2nd space 210 Packaging materials 216 Single Layer 217 Inner weld 218 Outside non-welded part 219 Second Space Gas 220 Heat seal bag 221 Bag body 222 Sealing part 223 Heat seal section 227 Opening 300, 300A 3rd package 307 Inside 308 Exterior 309 Third space 310 Packaging materials 316 Single Layer 317 Inner weld 318 Outside non-welded part 319 Third Space Gas 320 Heat seal bag 321 Bag body 322 Sealing part 323 Heat seal section 327 Opening 900 Outer packaging 959 Packing Space 969 Packaging Space Gas FG Filling gas
Claims
1. A sulfide-based solid electrolyte; A packaging body that encapsulates the sulfide-based solid electrolyte, the packaging body is made of a packaging material arranged in an n-th layer (n is an integer of 1 or more) from the sulfide-based solid electrolyte side, When a first packaging body in which n is 1 encloses the sulfide-based solid electrolyte, and a packaging body enclosing the first packaging body is present, the nth packaging body that encloses the first packaging body has n increasing in sequence toward the outer surface side of the first packaging body, When the space packed by the first packaging body is defined as a first space, and the space partitioned by the nth packaging body and the n-1th packaging body is defined as an nth space, H in the filled gas present in each space from the first space to the nth space is 2 An electrolyte encapsulation structure having an S gas concentration of 50 ppm or less after 7 days.
2. 2. The electrolyte containment structure according to claim 1, wherein the dew point temperature of the fill gas present in said first space is -20° C. or lower.
3. The filling gas is Ar, air, N 2 Or CO 2 3. The electrolyte containment structure of claim 2, wherein
4. 3. The electrolyte containment structure according to claim 1, wherein the packaging material constituting the first packaging body has a layer made of an organic material on at least a part of the inner surface side.
5. 5. The electrolyte containment structure according to claim 4, wherein the first package is sealed by welding the layer made of the organic material.
6. 5. The electrolyte containment structure according to claim 4, wherein the organic material is one or more organic resins selected from polyethylene terephthalate (PET), polyethylene (PE), chlorinated polyethylene (SPE), high density polyethylene, nylon, and polyvinyl alcohol.
7. The electrolyte containment structure described in claim 4, wherein the packaging material constituting the first packaging body comprises an inner welded portion made of a weldable organic material and an outer non-welded portion which is a layer made of aluminum and is laminated on the outer surface of the inner welded portion.
8. Further comprising a second package that receives and encloses the first package, H in the filling gas present in the second space defined by the outer surface of the first packaging body and the inner surface of the second packaging body. 2 3. The electrolyte encapsulation structure according to claim 1, wherein the concentration of S gas is 50 ppm or less.
9. Further comprising a third package that receives and encloses the second package, H in the filling gas present in a third space defined by the outer surface of the second packaging body and the inner surface of the third packaging body. 2 9. The electrolyte containment structure of claim 8, wherein the concentration of S gas is 50 ppm or less.
10. A sulfide-based solid electrolyte; A packaging body that encapsulates the sulfide-based solid electrolyte, the packaging body is made of a packaging material arranged in an n-th layer (n is an integer of 1 or more) from the sulfide-based solid electrolyte side, A method for manufacturing an electrolyte encapsulation structure, in which a first packaging body in which n is 1 encapsulates the sulfide-based solid electrolyte, and when a packaging body encapsulating the first packaging body is present, an nth packaging body encapsulating the first packaging body is an nth packaging body in which n increases sequentially toward an outer surface side of the first packaging body, When the space packed by the first packaging body is defined as a first space, and the space partitioned by the nth packaging body and the n-1th packaging body is defined as an nth space, H in the filled gas present in each space from the first space to the nth space is 2 A method for manufacturing an electrolyte encapsulation structure, comprising: an encapsulation step of encapsulating the electrolyte with the encapsulating gas so that the concentration of S gas is 50 ppm or less after 7 days.
11. The method for producing an electrolyte containment structure according to claim 10, wherein the dew point temperature of the filling gas is -20°C or lower.
12. The method for manufacturing an electrolyte encapsulation structure according to claim 10 or 11, further comprising a drying step of drying the first package at 50° C. or higher before the encapsulating step.
Citation Information
Patent Citations
Sulfide-based fully solid battery laminated sheet and laminated pack using same
CN113784835A
The invention relates to a container for examining solid electrolytes
DE102019102589A1
Material storage and dispensing package and method
JP2008539145A
Production method of sulfide compound storage container
JP2014234212A
Packaging material and packaging body for all-solid lithium ion battery
JP2021057231A