Purifier for chromium plating solution and purification method

A portable chromium plating solution purification device with on-site resin regeneration and gas bubbling addresses the inefficiencies of conventional methods, enabling efficient and waste-reducing purification of chromium plating solutions in various factory locations.

JP2024145546AActive Publication Date: 2024-10-15FUKUOKA PREFECTURAL GOVERNMENT +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023057943
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional chromium plating solution purification methods require large-scale installation space, piping, and are costly, with ion exchange resins being oxidized by high-concentration chromic acid, leading to inefficient and time-consuming processes.

Method used

A portable chromium plating solution purification device that combines an ion exchange resin column with on-site resin regeneration, using gas bubbling for efficient purification and regeneration, reducing the need for large-scale installations and minimizing waste through batch processing.

Benefits of technology

The device enables efficient purification of large volumes of chromium plating solution without extensive space or piping, effectively removing impurities and regenerating resins with minimal waste, suitable for small and medium-sized factories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145546000001_ABST
    Figure 2024145546000001_ABST
Patent Text Reader

Abstract

To provide a portable purifier for chromium plating solution that does not require a large-scale installation space or piping work and can process a large amount of chromium plating solution.SOLUTION: A portable purifier 1 for purifying chromium plating solution containing an impure metal ion has: an ion exchange resin tower 110 having a resin packed layer filled with cation exchange resin; a tank 40 for storing acid; a plating solution feed route for supplying chromium plating solution to the ion exchange resin tower 110; a water feed route for providing water to the ion exchange resin tower 110; a gas blowing route for supplying gas to the ion exchange resin tower 110; an acid feed route for supplying acid to the ion exchange resin tower 110; a discharge route for discharging chromium plating solution, water, gas, and acid from the ion exchange resin tower 110; and dollies 120a and 120b.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an apparatus and method for refining a chrome plating solution. [Background technology]

[0002] As plating is repeated, impurity metal ions such as iron ions and copper ions that have eluted from the base material being plated accumulate in the chrome plating solution. If the impurity metal ions accumulate above the control value, it will have an adverse effect on the plating quality, such as narrowing the gloss range of the plating, so it is necessary to remove the impurity metal ions from the chrome plating solution.

[0003] The diaphragm electrolysis method and the ion exchange resin method are mainly known as methods for refining chrome plating solutions and treating chrome wastewater. The diaphragm electrolysis method is a method in which impurity metal ions collected in a cathode tank by diaphragm electrolysis are precipitated and removed as hydroxides by increasing the pH of the cathode, but it requires an electrolytic membrane that can withstand high-concentration chromic acid, and has problems such as a long purification time due to low current efficiency.

[0004] The ion exchange resin method is a method for removing impurity metal ions by adsorption using ion exchange resins, and is an effective method in that it has a higher treatment efficiency than the diaphragm electrolysis method. As ion exchange devices for carrying out this ion exchange resin method, plant type and cylinder (cartridge) type are known.

[0005] A plant-type ion exchange device is an ion exchange device installed in a factory for the treatment of large amounts of wastewater in a large-scale factory. The plant-type ion exchange device can adsorb and remove impurity metal ions by passing chrome plating solution from a plating tank to an ion exchange resin tower through piping also installed in the factory. In addition, it can regenerate the resin by passing acid through saturated resin through piping also installed in the factory.

[0006] As an example of a plant-type ion exchange apparatus, Patent Document 1 discloses an apparatus for purifying a deteriorated chromium plating solution or a deteriorated chromate solution containing Cr(III) and impurity cations in a chromium plating bath or a chromate bath, the apparatus comprising: a circulation tank for storing the chromium plating solution or the chromate solution in a circulable manner; a circulation means for circulating the chromium plating solution or the chromate solution; a cation exchange resin tower through which the circulated chromium plating solution or chromate solution is passed in a drained state; and a recovery means for recovering the chromium plating solution or chromate solution remaining in the cation exchange resin tower outside the tower.

[0007] Cylinder-type (cartridge-type) ion exchange devices are primarily used for low-concentration chromium wastewater, and involve passing water containing heavy metals through an ion exchange resin cartridge to adsorb and remove impurity ions.

[0008] As for the treatment of chrome plating solution equipped with a cylinder-type ion exchange device, Patent Document 2 discloses a purification and reuse device for waste chrome solution, comprising: a plurality of ion exchange devices installed on a transport vehicle; a storage tank for waste chrome solution installed on the ground; a flexible hose connecting the ion exchange devices on the vehicle to the waste solution storage tank on the ground; a flexible hose connecting the plurality of ion exchange devices on the vehicle; a storage tank on the ground for storing chrome solution purified by passing the waste chrome solution through the plurality of ion exchange devices; and a regeneration specialized factory for regenerating the ion exchange device on the vehicle in which the ion exchange resin is saturated by purifying the waste solution. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 9-228069 [Patent Document 2] Patent No. 3816547 Summary of the Invention [Problem to be solved by the invention]

[0010] The plant-type ion exchange device requires a large-scale ion exchange device and piping equipment, and therefore the conditions for its implementation are limited in terms of securing the installation space for the device within the factory, piping work, and equipment costs.

[0011] Cylinder-type ion exchange devices are regenerated by transporting the saturated ion exchange devices to a regeneration factory. This creates problems in terms of transportation and processing costs. In addition, cylinder-type ion exchange devices are small, with a resin capacity of about 50 L, so one cylinder is insufficient to remove impurities from chrome plating solution. Furthermore, ion exchange resins are also easily oxidized by high-concentration chromic acid, and the exchange capacity gradually decreases. Therefore, when treating chrome plating solution, it is common to dilute the chrome plating solution, remove heavy metals, and then concentrate it, which creates problems in terms of time and cost.

[0012] In Patent Document 2, the waste chromium solution in the waste solution storage tank is purified by passing it through multiple ion exchange devices mounted on a transport vehicle, and there is no need to install an ion exchange device in the factory. However, since multiple ion exchange resin towers are used, the device is large and requires space.

[0013] As described above, conventional devices require a large installation space or are large-scale devices equipped with multiple ion devices, and there has been no small-sized device that does not require installation and can treat plating baths in various locations within a factory.

[0014] The present invention has been made in view of the above circumstances, and has an object to provide a portable apparatus for purifying a chromium plating solution that does not require a large installation space or piping work, and is capable of treating a large amount of chromium plating solution. Another object of the present invention is to provide a method for purifying a chromium plating solution. [Means for solving the problem]

[0015] In order to solve the above problems, the inventors came up with the idea of ​​freely moving a small device near chrome plating baths in various locations in a factory for processing. Furthermore, they came up with the idea of ​​combining an ion exchange device for purifying chrome plating solutions with a unit for regenerating ion exchange resins so that a large amount of chrome plating solutions can be processed. In the course of their investigation, they found that when a small device is used, the conventional method of passing acid through a saturated ion exchange resin to regenerate the resin tends to result in insufficient removal of impurities adsorbed on the resin. In order to solve this problem, they investigated a method for efficiently removing impurities adsorbed on the ion exchange resin. As a result, they found that the following invention meets the above object, and arrived at the present invention.

[0016] The refining apparatus of the present invention comprises: A portable chrome plating solution purification device for purifying a chrome plating solution containing impurity metal ions, The chrome plating solution refining apparatus comprises: an ion exchange resin tower provided with a resin packed bed packed with a cation exchange resin for removing impurity metal ions; A tank containing an acid for regenerating the resin-filled bed; a plating solution delivery path for supplying the chromium plating solution in the chromium plating bath to the ion exchange resin tower; A water supply path for supplying water to the ion exchange resin tower; a gas blowing path for blowing a gas into the ion exchange resin tower; an acid supply path for supplying the acid contained in the tank to the ion exchange resin tower; a discharge path for discharging the chromium plating solution, the water, the gas, and the acid from the ion exchange resin tower; A cart for moving the refining apparatus; has.

[0017] In this way, by making the refining device portable, it can be moved close to chrome plating baths in various locations within a factory to treat chrome plating solution.

[0018] In addition, the purification of the chromium plating solution with the ion exchange resin, washing of the ion exchange resin with water, and regeneration of the ion exchange resin with acid can be repeated on the spot, and even with a portable size, the ion exchange resin can be efficiently regenerated and a large amount of chromium plating solution can be purified.

[0019] In the purification apparatus of the present invention, the gas injection path preferably has a first gas injection path for injecting gas from within or below the resin packed bed, and a second gas injection path for injecting gas from above the resin packed bed, and the exhaust path preferably has a path for discharging the gas injected from the first gas injection path to the outside of the ion exchange resin tower through above the resin packed bed, and a path for discharging the gas injected from the second gas injection path to the outside of the ion exchange resin tower through the resin packed bed.

[0020] With this configuration, by blowing gas through the first gas blowing path, stirring by bubbling can be performed during resin regeneration, so that the cation exchange resin can be efficiently cleaned and regenerated. In addition, by blowing gas through the second gas blowing path, the chromium plating solution remaining in the resin-filled layer can be pushed out by the gas, so that deterioration of the resin can be suppressed. Therefore, even with a portable device, a larger amount of chromium plating solution can be treated by repeating the plating solution purification process and the resin regeneration process. In addition, since the cation exchange resin can be regenerated with a small amount of water or acid, the amount of waste liquid is reduced, the environmental load can be reduced, and even in small and medium-sized factories, the waste liquid can be easily treated within the factory.

[0021] The purification apparatus of the present invention is preferably movable by human power. Therefore, the amount of the cation exchange resin packed is preferably 45 to 200 L. If the amount of the cation exchange resin packed is too small, the amount of the chromium plating solution that can be treated is small, resulting in inefficiency, whereas if the amount of the cation exchange resin packed is too large, it is difficult to move the apparatus by human power.

[0022] The refining apparatus of the present invention is preferably provided with valves in the plating solution delivery path, the water delivery path, the gas injection path, the acid delivery path and the discharge path, and has a control unit for automatically controlling the opening and closing of one or more of the valves. By automatically opening and closing the valves in this manner, it is possible to easily switch between the operation of the refining process of the chrome plating solution and the operation of the resin regeneration process.

[0023] The volume of the tank is preferably at least twice as large as the volume of the resin-filled layer. With this configuration, the regeneration treatment with acid can be continuously repeated multiple times, improving the regeneration rate of the resin.

[0024] The purification method of the present invention comprises the steps of: A method for purifying a chrome plating solution containing impurity metal ions, comprising: The plating solution purification process includes passing the chromium plating solution through an ion exchange resin tower having a resin packed layer packed with a cation exchange resin to obtain a purified chromium plating solution, and regenerating the cation exchange resin after the plating solution purification process. The resin regeneration treatment comprises: a batch-type water washing step of supplying water to the ion exchange resin tower and then stirring the water to wash the cation exchange resin; and a batch-type regeneration step of supplying an acid to the ion exchange resin tower after the water-washing step and then stirring the acid to regenerate the cation exchange resin.

[0025] In this way, by carrying out the purification process of the chrome plating solution and the resin regeneration process, and by carrying out the water washing step and the regeneration step in a batchwise manner, the cation exchange resin can be efficiently regenerated after the purification of the chrome plating solution. This allows the cation exchange resin to be regenerated with a small amount of water or acid, and the amount of waste liquid is reduced, thereby reducing the environmental load. Furthermore, by alternately repeating the purification process of the chrome plating solution and the resin regeneration process, a large amount of chrome plating solution can be purified even when a small amount of cation exchange resin is used. According to the purification method of the present invention, the amount of waste liquid can be reduced even when the purification process of the chrome plating solution and the resin regeneration process are alternately repeated, so that even small and medium-sized factories can easily treat the waste liquid within the factory.

[0026] The purification method of the present invention can be carried out even in an apparatus equipped with a portable amount of ion exchange resin, and therefore the purification apparatus of the present invention is a suitable apparatus for carrying out the purification method of the present invention.

[0027] In the purification method of the present invention, the stirring in the water washing step and the stirring in the regeneration step are preferably performed by bubbling a gas. By performing stirring by bubbling a gas, it is easy to reduce the size of the purification device.

[0028] In the purification method of the present invention, the washing time in the regeneration step is preferably 5 to 60 minutes per cycle. By setting the washing time in this range, the efficiency of regeneration of the ion exchange resin is further improved, and the efficiency of removing impurities from the chromium plating solution during the purification of the plating solution is further improved.

[0029] In the purification method of the present invention, it is preferable that each of the water washing step and the regeneration step is performed consecutively two or more times. By performing washing consecutively multiple times, the efficiency of regeneration of the ion exchange resin is further improved, and the efficiency of removing impurities from the chromium plating solution during the purification of the plating solution is further improved.

[0030] In the purification method of the present invention, it is preferable that the water washing step is performed two or more times in succession, and the waste liquid discharged in the first water washing step is returned to the chrome plating bath containing the chrome plating solution. The waste liquid discharged in the first water washing step often has a high chromium concentration. By returning this waste liquid with a high chromium concentration to the plating bath, resources can be reused, wastewater can be reduced, and the environmental load can be reduced. Effect of the Invention

[0031] According to the present invention, there is provided a portable chrome plating solution purification device that does not require a large installation space or piping work, and is capable of treating a large amount of chrome plating solution. Also, according to the present invention, there is provided a chrome plating solution purification method. [Brief description of the drawings]

[0032] [Figure 1] 1 is a photograph showing the appearance of a refining apparatus 1 which is an example of the refining apparatus of the present invention. [Diagram 2] FIG. 1 is a schematic diagram for explaining a refining device 1. [Diagram 3] FIG. 2 is a schematic diagram for explaining an ion-exchange resin tower 110 of the refining device 1. [Figure 4] 1 shows a flow diagram of the purification method of the present invention. [Diagram 5] FIG. 2 is a schematic diagram for explaining a plating solution purification process P1 using the purification device 1. [Figure 6] FIG. 13 is a schematic diagram for explaining a plating solution removing step S10. [Figure 7] 1A and 1B are schematic diagrams for explaining the water washing step S20 of the resin regeneration process P2 using the purification apparatus 1, in which (A) is a schematic diagram for explaining the flow of water W in the water supply step S21, (B) is a schematic diagram for explaining the flow of gas G in the water agitation step S22, and (C) is a schematic diagram for explaining the flow of gas G in the water removal step S23. [Figure 8]Schematic diagrams for explaining the regeneration step S30 of the resin regeneration process P2 using the purification device 1, where (A) is a schematic diagram for explaining the flow of acid A in the acid supply step S31, (B) is a schematic diagram for explaining the flow of gas G in the acid stirring step S32, and (C) is a schematic diagram for explaining the flow of gas G in the acid removal step S23. [Figure 9] 1 is a photograph showing the appearance of a refining apparatus 2 which is another embodiment of the refining apparatus of the present invention. [Figure 10] FIG. 2 is a schematic diagram for explaining the refining device 2. [Figure 11] FIG. 2 is a schematic diagram of an experimental device in Reference Example 1. [Figure 12] 1 is a photograph showing the state of the cleaning liquid during the water washing process of Reference Example 1. [Figure 13] FIG. 1 is a graph showing the relationship between the chromium concentration in the cleaning solution of Reference Example 1 and the number of cleaning cycles. [Figure 14] FIG. 13 is a plot of the chromium concentration in the cleaning water for each cleaning number in Use Example 2. [Figure 15] FIG. 13 is a plot of the chromium concentration in acid versus the number of washings in Use Example 3. [Figure 16] FIG. 13 is a plot of the relationship between the acid cleaning time per one pickling and the chromium concentration in the acid in Use Example 4. [Figure 17] FIG. 1 is a plot of the concentrations of Fe(III) ions and Cr(III) ions in the treatment liquid versus liquid passing time in Reference Example 2. [Figure 18] FIG. 1 is a plot of the concentrations of Fe(III) ions and Cr(III) ions in the treatment liquid versus the liquid passing time in Reference Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical value or physical property value before and after it.

[0034] The refining apparatus of the present invention will be described in detail below with reference to FIGS.

[0035] [Embodiment 1] <Chrome plating solution purification equipment> FIG. 1 is an external view of the refining apparatus 1, FIG. 2 is a schematic diagram for explaining the refining apparatus 1, and FIG. 3 is a schematic diagram for explaining an ion exchange resin tower 110 of the refining apparatus 1. The refining apparatus 1 shown in FIG. 1 and FIG. 2 has a first unit 100a provided on a first carriage 120a and a second unit 100b provided on a second carriage 120b. As shown in FIG. 2, the first unit 100a has an ion exchange resin tower 110 for refining the chromium plating solution S, a plating solution delivery path R1, a water delivery path R2, gas blowing paths R3a and R3b, an acid delivery path R4a, and discharge paths R5a to R5e. The second unit 100b has a tank 40 that contains an acid A for regenerating the cation exchange resin after the chromium plating solution S has been passed through it, and an acid delivery path R4b.

[0036] (Ion exchange resin tower) The ion exchange resin tower 110 has a resin-filled layer 111 filled with a cation exchange resin for removing impurity metal ions in the chrome plating solution S. As shown in FIG. 3, the ion exchange resin tower 110 has a housing 112 having a cylindrical section 112a. A support plate 113 is provided on the bottom surface of the cylindrical section 112a, and the support plate 113 is filled with a cation exchange resin to form a resin-filled layer 111. In addition, there is a space 114 above the resin-filled layer 111 in the cylindrical section 112a, and gas G can be bubbled by blowing it into the resin-filled layer 111. A level sensor 115 for detecting the liquid levels of the chrome plating solution S, water W, and acid A is attached to the upper space 114. In addition, a pressure gauge (not shown) can be attached to adjust the pressure inside the cylindrical section 112a.

[0037] (cation exchange resin) Cation exchange resins are used to exchange cations and H +The cation exchange resin is a resin that can be exchanged with cations of 1 to 3. Examples of the cation exchange resin include styrene-based, acrylic-based, and hydrogel-based strongly acidic cation exchange resins. The cation exchange resin may be of a gel type or a porous type, but it is preferable to use a gel type cation exchange resin because it can increase the removal rate of Fe(III) ions in the chrome plating solution. The crosslinking degree of the cation exchange resin is not particularly limited, but is preferably one with a high crosslinking degree, for example, 8 to 20%, 10 to 16%, or 14 to 16%, etc. The particle size of the cation exchange resin is not particularly limited, but is preferably 300 to 800 μm, and more preferably 300 to 500 μm.

[0038] The amount of the cation exchange resin packed (the volume of the resin packed layer 111) is preferably 45 to 200 L, and more preferably 50 to 100 L. If the amount packed is too large, the ion exchange resin tower becomes large, making it difficult to reduce the size and portability.

[0039] (tank) The tank 40 is a container in which acid A for regenerating the resin-filled layer 111 (cation exchange resin) is stored. As shown in FIG. 2, in the purification device 1, the tank 40 is mounted on a second carriage 120b different from the first carriage 120a on which the ion exchange resin tower 110 is mounted. The acid used is sulfuric acid or hydrochloric acid. Usually, the acid A is used as an aqueous solution, and the concentration thereof can be 5 to 25 vol. %, 10 to 20 vol. %, or the like.

[0040] If the size of the tank 40 is too small, frequent replenishment is required during the resin regeneration process, which is inefficient. As described later in the examples, the exchange capacity recovery rate is high by repeating the batch-type regeneration process using acid A multiple times. Since the batch-type regeneration process using acid A can be repeated multiple times without additionally supplying acid A to the tank 40, the volume of the tank 40 is preferably at least twice the volume of the resin-filled layer 111, and more preferably at least three times. The upper limit of the size of the tank 40 may be within a range that allows it to be transported, but if the tank 40 is too large, it becomes difficult to move it by hand. Therefore, the volume ratio of the tank 40 to the resin-filled layer 111 is preferably 2 to 6, and more preferably 3 to 5.

[0041] (Plumbing) As shown in FIG. 2, the refining device 1 has a plurality of pipes, which constitute a plating solution delivery path R1, a water delivery path R2, gas blowing paths R3a and R3b, acid delivery paths R4a and R4b, and discharge paths R5a to R5e. As shown in FIG. 3, the pipes L50, L51, and L52 attached to the ion exchange resin tower 110 are provided so as to penetrate from the outside to the inside of the housing 112. The pipe L50 is a pipe for supplying liquid or gas, and functions as a part of the plating solution delivery path R1, the water delivery path R2, the gas blowing path R3a, and the acid delivery path R4a. The pipe L51 is a pipe for supplying gas, discharging gas, or discharging liquid, and functions as a part of the gas blowing path R3b and the discharge path R5a. The pipe L52 is a pipe for discharging liquid or gas, and functions as the discharge path R5b.

[0042] The downstream end 50a of the pipe L50 is disposed at a lower position in the resin-filled layer 111, and a nozzle is attached to it. As shown in FIG. 2, the upstream side of the pipe L50 (outside the housing 112) is connected to the pipe L15 through which the liquid flows and the pipe L32 through which the gas flows. The upstream side of the pipe L15 is connected to the pipe L14 through which the chrome plating solution S or the water W flows and the pipe L46 through which the acid A flows, and the upstream side of the pipe L14 is connected to the pipe L13 through which the chrome plating solution S flows and the pipe L21 through which the water W flows, and the pipe L13 is connected to the pipe L12 via the pump P1 on the upstream side. The upstream side of the pipe L46 is detachable from the hose H44, and is connected to the pipe L42 of the second unit 100b via the hose H44. The pipe L42 is connected to the pipe L41 connected to the tank 40 via the pump P2.

[0043] As shown in Fig. 3, the pipe L51 attached to the upper part of the ion-exchange resin tower 110 branches into three inside the housing 112, and nozzles are attached to the respective ends 51a, 51b, and 51c. The ends 51a, 51b, and 51c are disposed above and spaced apart from the resin-filled layer 111. As shown in Fig. 2, the end of the pipe L51 on the outer side of the housing 112 is connected to a pipe L33 for supplying gas and a pipe L53 for discharging liquid or gas. The upstream side of the pipe L33 merges with the upstream side of the pipe L32 through which gas passes, and is connected to the pipe L31.

[0044] As shown in Fig. 3, the upstream side of the pipe L52 attached to the lower part of the ion-exchange resin tower 110 is branched into three, and the respective ends 52a, 52b, and 52c are arranged below in the resin-filled layer 111. As shown in Fig. 2, the downstream side of the pipe L52 is connected to the downstream side of the pipe L53 for discharging liquid or gas, and to the upstream sides of the pipes L54 and L61. The downstream side of the pipe L54 is connected to the pipes L71 and L81.

[0045] (Plating solution delivery path) The plating solution delivery path is a path for supplying the chromium plating solution in the plating bath to the ion exchange resin tower. In the refining device 1, the plating solution delivery path R1 is composed of a pipe L12, a pump P1, a pipe L13, a pipe L14, a pipe L15, and a pipe L50. The pipe L12 has a connection part 11 at the upstream end, so that a hose H10a can be connected. The end of the hose H10a not connected to the connection part 11 is placed in the chromium plating solution S, and the chromium plating solution S can be delivered by driving the pump P1. The pipe L13 is provided with a valve V1, and the delivery of the chromium plating solution S can be controlled by opening and closing the valve V1.

[0046] (Water supply route) The water supply path is a path for supplying water to the ion exchange resin tower. In the purification device 1, the water supply path R2 is composed of a pipe L21, a pipe L14, a pipe L15, and a pipe L50. The pipe L21 has a connection part 20 at the upstream end, and connects the pipe L21 to a water supply facility (not shown) such as a waterworks in the facility via a hose H22. Water W flows through the path by supplying the water W from the water supply facility (not shown). In addition, a valve V2 is provided in the path of the pipe L21, and the water supply can be controlled by opening and closing the valve V2.

[0047] (Gas injection route) The gas injection path is a path for supplying gas to the ion-exchange resin tower. The gas may be air and / or nitrogen. The refining device 1 has a gas injection path R3a (first gas injection path) composed of the pipes L31, L32, and L50, and a gas injection path R3b (second gas injection path) composed of the pipes L31, L33, and L51. The gas injection path R3a is a path for injecting gas G into the resin-filled layer 111 from below, and the gas injection path R3b is a path for injecting gas G from above the resin-filled layer 111. The gas injection paths R3a and R3b are composed of the same pipe L31 on the upstream side. This pipe L31 has a connection part 30 at the upstream end, and is connected to a gas supply facility (not shown) such as a cylinder via a hose H32, and gas G flows through the path by sending gas G from the gas supply facility (not shown). Pipes L32 and L33 are provided with valves V3a and V3b, respectively, and the blowing of gas G can be controlled by opening and closing these valves.

[0048] (Acid delivery path) The acid liquid supply path is a path for supplying acid to the ion exchange resin tower. The purification device 1 has an acid liquid supply path R4a (downstream acid liquid supply path) composed of the pipe L46, the pipe L15, and the pipe L50, and an acid liquid supply path R4b (upstream acid liquid supply path) composed of the pipe L41, the pump P2, and the pipe L42. The pipe L46 has a connection part 45 at the upstream end, and the pipe L42 has a connection part 43 at the downstream end. The acid liquid supply path R4a and the acid liquid supply path R4b are connected via a hose H44, and the pump P2 is driven to supply the acid A. In addition, the supply of the acid A can be controlled by opening and closing the valve V4 provided in the pipe L46.

[0049] (Excretion route) The discharge path is a path for discharging liquid and gas from the ion exchange resin tower. That is, the discharge path is a path for discharging chrome plating solution, water, acid, and gas from the ion exchange resin tower. In the refining device 1, the discharge path includes a discharge path R5a (upper discharge path) for discharging from above the resin filled layer 111, a discharge path R5b (lower discharge path) for discharging from below the resin filled layer 111, a discharge path R5c for discharging to the plating bath 10, a discharge path R5d for discharging to the waste water tank 70, and a discharge path R5e for discharging to the acid waste liquid tank 80. The discharge path R5a is composed of the pipe L51 and the pipe L53, the discharge path R5b is composed of the pipe L52, the discharge path R5c is composed of the pipe L61, the discharge path R5d is composed of the pipe L54 and the pipe L71, and the discharge path R5e is composed of the pipe L54 and the pipe L81. The downstream sides of the discharge paths R5a and R5b are connected to the discharge paths R5c to R5e. The pipes L52, L53, L61, L71, and L81 are each provided with a valve. By controlling these valves according to the flow in the supply side paths (i.e., the plating solution delivery path R1, the water delivery path R2, the gas blowing paths R3a and R3b, and the acid delivery paths R4a and R4b), the liquid and gas can be discharged.

[0050] [Method of refining chrome plating solution] Hereinafter, a method for purifying a chromium plating solution containing impurity metal ions using the refining apparatus 1 will be described.

[0051] First, the carts 120a and 120b are pushed to move the first unit 100a and the second unit 100b close to the plating bath 10 containing the chromium plating solution S. Next, the first unit 100a is connected to the plating bath 10, the water supply means, and the gas supply means using hoses or the like, and the first unit 100a and the second unit 100b are connected to the plating bath 10, the waste water tank 70, and the acid waste liquid tank 80, respectively (see FIG. 1). Then, the plating solution purification process and the resin regeneration process are alternately and repeatedly performed.

[0052] The amount of chrome plating solution S to be treated depends on the amount of the cation exchange resin filled, but with a typical chrome plating solution S, it is possible to treat an amount (L) of chrome plating solution S that is 1 to 200 times the amount of the cation exchange resin filled.

[0053] A flow diagram of the purification method of the present invention is shown in Figure 4. The purification method shown in Figure 4 involves alternately and repeatedly carrying out a plating solution purification treatment P1 and a resin regeneration treatment P2.

[0054] (Plating solution purification process P1) The plating solution purification process P1 is a step in which the chromium plating solution S is passed through an ion exchange resin tower 110 having a resin-packed layer 111 packed with a cation exchange resin to obtain a purified chromium plating solution.

[0055] The chromium plating solution S to be subjected to the plating solution purification process P1 is a plating solution containing impurity metal ions and mainly composed of chromic anhydride. The impurity metal ions are Fe(III) ions, Cr(III) ions, etc. The concentrations of these impurity metal ions are not particularly limited. The control values ​​of the concentrations of Fe(III) ions and Cr(III) ions in the chromium plating solution are 10 g / L, respectively, and the purification method of the present invention may be used to make the Fe(III) ion concentration and the Cr(III) ion concentration in the chromium plating solution below the control values, or may be used to maintain the Fe(III) ion concentration and the Cr(III) ion concentration in the chromium plating solution below the control values. For example, the chromium plating solution S may be a deteriorated chromium plating solution in which the Fe(III) ion and the Cr(III) ion are at or above the control values, or may be a chromium plating solution in which the Fe(III) ion and the Cr(III) ion are at or above the control values ​​(for example, 1 g / L or more and less than 10 g / L, respectively). In addition, the concentration of chromic anhydride in the chromium plating solution is 100 to 400 g / L or 150 g / L to 300 g / L. In the purification method of the present invention, such a chromium plating solution having a high concentration of chromic anhydride can be used as it is as the chromium plating solution S without diluting it.

[0056] Fig. 5 is a schematic diagram for explaining a plating solution purification process P1 using the purification apparatus 1. Note that in Fig. 5, the water supply path R2, the gas blowing paths R3a and R3b, the acid supply path R4a, the discharge paths R5b, R5d and R5e, the cart 120a and the second unit 100b of the purification apparatus 1 are omitted.

[0057] 5, in the plating solution purification process P1, a hose H10a is connected to a connection part 11 of a pipe L12 of a plating solution delivery path R1 of the purification device 1, and the end of the hose H10a not connected to the connection part 11 is disposed in the chromium plating solution S in the chromium plating bath 10. In addition, a hose H10b is connected to a connection part 62 at the downstream end of a pipe L61 of the purification device 1, and the end of the hose H10b not connected to the connection part 62 is disposed in the chromium plating solution S in the chromium plating bath 10.

[0058] In the plating solution purification process P1, as shown in Fig. 5, the valves V1, V5a, and V6 are opened, the other valves are closed, and the pump P1 is driven to circulate the chromium plating solution S. The chromium plating solution S is supplied to the ion exchange resin tower 110 via the hose H10a and the plating solution delivery path R1, and after contacting with the resin filled layer 111 (cation exchange resin) in the ion exchange resin tower 110, it is returned to the chromium plating bath 10 via the discharge paths R5a and R5c and the hose H10b. By circulating the chromium plating solution S in this way, when the chromium plating solution S comes into contact with the resin filled layer 111, impurities such as Fe(III) ions and Cr(III) ions in the chromium plating solution S are adsorbed and removed by the cation exchange resin, and a purified chromium plating solution with reduced concentrations of Fe(III) ions and Cr(III) ions is returned to the chromium plating bath 10.

[0059] The treatment time of one plating solution purification process P1 (the time for circulating the chromium plating solution S) depends on the capacity and the liquid sending speed of the liquid sending means such as a pump, but is preferably 0.5 to 3 hours, more preferably 0.75 to 1.5 hours. If the treatment time of one process is too long, the cation exchange resin becomes saturated, and impurities cannot be removed even if the treatment time is extended. On the other hand, if the treatment time of one process is too short, it is inefficient. In addition, it is preferable to perform the resin regeneration process P2 at the stage where the adsorption amount reaches 80 to 85% of the adsorption capacity of the cation exchange resin. By performing the resin regeneration process P2 before the adsorption capacity of the cation exchange resin reaches the saturation point, the final adsorption amount can be increased.

[0060] The liquid sending speed may be appropriately adjusted according to the concentration of impurity ions, particularly Fe(III) ions, in the chrome plating solution S, and is preferably 100 to 1000 L / h. If the liquid sending speed is too fast, it is not preferable because impurities are not easily adsorbed by the cation exchange resin and the load on the device increases. Also, if the liquid sending speed is too slow, it is inefficient.

[0061] (Resin Regeneration Treatment P2) The resin regeneration process P2 is a process for regenerating the cation exchange resin after the plating solution purification process P1. The resin regeneration process P2 shown in Fig. 4 includes a plating solution removal process S10, a water washing process S20, and a regeneration process S30.

[0062] (Plating solution removal step S10) The plating solution removal step S10 is a step of pushing out the chromium plating solution S remaining in the resin filled layer 111 by gas G after the plating solution purification process P1. Fig. 6 is a schematic diagram for explaining the plating solution removal step S10. Note that Fig. 6 omits the plating solution delivery path R1, the water delivery path R2, the gas blowing path R3a, the acid delivery path R4a, the discharge paths R5a, R5d, and R5e, the cart 120a, and the second unit 100b of the refining device 1.

[0063] In the plating solution removal step S10, as shown in Fig. 6, the pipe L31 of the gas blowing path is connected to a gas supply facility (not shown) via a hose H32. Valves V3b, V5b, and V6 are opened, and the other valves are closed to send gas G. As a result, gas G is blown from above the ion-exchange resin tower 110 via the gas blowing path R3b, and the chromium plating solution S remaining in the resin-filled layer 111 after the plating solution purification process P1 can be pushed out from below the resin-filled layer 111 into the chromium plating bath 10 via discharge paths R5b and R5c.

[0064] (Water washing process S20) The water washing step S20 is a batch-type washing step in which water W is supplied to the ion exchange resin tower 110 and then stirred to wash the cation exchange resin, and includes a water supplying step S21, a water stirring step S22, and a water removing step S23.

[0065] 7 is a schematic diagram for explaining the water washing step S20 of the resin regeneration treatment P2 using the refining apparatus 1, where (A) is a schematic diagram for explaining the flow of water W in the water supplying step S21, (B) is a schematic diagram for explaining the flow of gas G in the water stirring step S22, and (C) is a schematic diagram for explaining the flow of gas G in the water removing step S23. Note that in FIG. 7, the plating solution sending path R1, the acid sending path R4a, the discharge paths R5c, R5e, the cart 120a, and the second unit 100b of the first unit 100a of the refining apparatus 1 are omitted.

[0066] 7, in the water-washing step S20, the water supply path R2 of the refining device 1 is connected to a water supply facility (not shown) such as a waterworks in the facility via a hose H22. A hose H70b is connected to a connection part 72 at the downstream end of a pipe L71 of the refining device 1, and the end of the hose H70b not connected to the connection part 72 is disposed in a wastewater tank 70. A pipe L31 of the gas injection path is connected to a gas supply facility (not shown) via a hose H32.

[0067] (Water supply process W21) The water supply step S21 is a step of supplying water W to the ion exchange resin tower 110. In the water supply step S21, as shown in FIG. 7(A), valves V2, V5a, and V7 are opened, and the other valves are closed, and water W is sent from a water supply means (not shown). The water W is supplied to the ion exchange resin tower 110 from a water supply path R2. It is preferable to supply water W in an amount equal to or more than one time the volume of the resin-filled layer 111, and the water level is detected by a level sensor 115 (see FIG. 2). When the water surface reaches a predetermined height above the upper surface of the resin-filled layer 111, the supply of water W is stopped.

[0068] The supply of the water W may be performed for a predetermined period of time by determining the time in advance.

[0069] (Water agitation process S22) The water agitation step S22 is a step of agitating the supplied water W and the cation exchange resin to wash the cation exchange resin. In the water agitation step S22, as shown in FIG. 7(B), valves V3a, V5a, and V7 are opened, and the other valves are closed to send gas G. Gas G is injected from below into the resin-filled layer 111 of the ion exchange resin tower 110 via the gas injection path R3a, and bubbling is performed, whereby the resin-filled layer 111 (cation exchange resin) and water W are agitated and washed. The injected gas G is discharged from discharge paths R5a and R5d to the waste water tank 70.

[0070] The stirring time in the water stirring step S22 (the time for blowing and bubbling gas G) is preferably 0.5 to 60 minutes, more preferably 1 to 20 minutes. If the stirring time in the water stirring step S22 is too short, the cleaning tends to be insufficient, and if it is too long, the effect tends to be saturated.

[0071] (Water removal process S23) The water removal step S23 is a step of extracting the post-wash water W from the resin-filled bed 111 by using gas G. In the water removal step S23, as shown in Fig. 7(C), valves V3b, V5b, and V7 are opened, and the other valves are closed to send gas G. As a result, gas G is blown in from above the ion-exchange resin tower 110 via the gas blowing path R3b, and the post-wash water W can be pushed out from below the resin-filled bed 111 to the wastewater tank 70 via the discharge paths R5b and R5d.

[0072] (Number of times of water washing step S20) The water washing step S20 may be performed once, but is preferably repeated multiple times. That is, after performing the water supplying step S21, the water stirring step S22, and the water removing step S23, it is preferable to repeat the water supplying step S21, the water stirring step S22, and the water removing step S23 again. On the other hand, if the number of steps is too many, the effect becomes saturated, so the water washing step S20 is preferably repeated 2 to 5 times, and more preferably repeated 3 to 4 times.

[0073] Furthermore, when the water washing step S20 is performed multiple times, the same discharge route may be used each time, but it is preferable to switch the discharge route depending on the number of times.

[0074] In particular, since the chromium concentration in the water W removed in the water removing step S23 tends to be high in the first water rinsing step S20, it is preferable to discharge the water W after washing into the chrome plating bath 10 in the first water rinsing step S20, and to discharge the water W after washing into the waste water tank 70 in the second and subsequent water rinsing steps S20. In this way, resources can be used effectively and the amount of waste water is reduced, thereby reducing the environmental burden.

[0075] 7 shows the water W after washing being pushed out into the waste water tank 70, but when the water W after washing is pushed out into the chrome plating bath 10, the valve V6 is opened (the valve V7 is closed) instead of the valve V7 in the water supply step S21, the water stirring step S22, and the water removal step S23. As a result, the gas G and the water W are discharged into the chrome plating bath 10 via the discharge paths R5a, R5c and the discharge paths R5b, R5c. In order to discharge the water W after washing into the chrome plating bath 10 in the first water washing step S20 and to discharge the water W after washing into the waste water tank 70 in the second or subsequent water washing steps S20, the discharge path in the first water washing step S20 should be a path through R5c with the valve V6 opened, and the discharge path in the second or subsequent water washing steps S20 should be a path through R5d with the valve V7 opened.

[0076] (Regeneration process S30) The regeneration step S30 is a batch-type regeneration step in which acid A is supplied to the ion exchange resin tower 110 and then stirred to regenerate the cation exchange resin, and includes an acid supplying step S31, an acid stirring step S32, and an acid removing step S33.

[0077] 8 is a schematic diagram for explaining the regeneration step S30 of the resin regeneration treatment P2 using the refining apparatus 1, where (A) is a schematic diagram for explaining the flow of acid A in the acid supplying step S31, (B) is a schematic diagram for explaining the flow of gas G in the acid stirring step S32, and (C) is a schematic diagram for explaining the flow of gas G in the acid removing step S33. Note that in FIG. 8, the plating solution sending path R1, the water sending path R2, the discharge paths R5c and R5d, the cart 120a of the first unit 100a of the refining apparatus 1, and the cart 120b of the second unit 100b are omitted.

[0078] 8, in the regeneration step S30, the acid liquid supply path R4b and the acid liquid supply path R4a of the refining device 1 are connected via a hose H44. A hose H80b is connected to a connection part 82 at the downstream end of a pipe L81 of the refining device 1, and the end of the hose H80b not connected to the connection part 82 is disposed in an acid waste liquid tank 80. The pipe L31 of the gas blowing path is connected to a gas supply facility (not shown) via a hose H32.

[0079] (Acid supply step S31) In the acid supply step S31, as shown in Fig. 8(A), the valves V4, V5a, and V8 are opened, the other valves are closed, P2 is started, and acid A stored in the tank 40 is sent. Acid A is supplied to the ion exchange resin tower 110 via the acid supply path R4b, the hose H44, and the acid supply path R4a. It is preferable to supply acid A in an amount equal to or more than one time the volume of the resin-filled layer 111, and the liquid level is detected by the level sensor 115 (see Fig. 2). When the liquid level reaches a predetermined height above the upper surface of the resin-filled layer 111, the supply of acid A is stopped.

[0080] The supply time of acid A may be determined in advance, and acid A may be supplied for a predetermined period of time.

[0081] (Acid stirring step S32) 8(B), in the acid mixing step S32, valves V3a, V5a, and V8 are opened and the other valves are closed to send gas G. Gas G is blown into the resin-filled layer 111 of the ion-exchange resin tower 110 from below via gas blowing path R3a, and bubbling is performed to mix the resin-filled layer 111 and acid A, thereby regenerating the cation exchange resin. The blown gas G is discharged from discharge paths R5a and R5e to the acid waste liquid tank 80.

[0082] The mixing time in the acid mixing step S32 (the time for blowing and bubbling gas G) is preferably 5 to 60 minutes, more preferably 10 to 45 minutes. If the mixing time in the acid mixing step S32 is too short, the recovery of the resin tends to be insufficient, and if it is too long, the effect tends to be saturated.

[0083] (Acid removal step S33) The acid removal step S33 is a step of extracting the acid A from the resin-filled layer 111 by using a gas G. In the acid removal step S33, as shown in FIG. 8(C), the valves V3b, V5b, and V8 are opened, and the other valves are closed to send the gas G. As a result, the gas G is blown in from above the ion-exchange resin tower 110 via the gas blowing path R3b, and the acid A can be pushed out from below the resin-filled layer 111 to the acid waste liquid tank 80 via the discharge paths R5b and R5e. If the discharged acid A is used as a pH adjuster for wastewater treatment, the amount of waste liquid can be reduced, and the environmental load can be reduced.

[0084] (Number of times of regeneration process S30) The regeneration step S30 may be performed once, but is preferably repeated multiple times. That is, after performing the acid supplying step S31, the acid stirring and washing step S32, and the acid removing step S33, it is preferable to repeat the operations of the acid supplying step S31, the acid stirring and washing step S32, and the acid removing step S33 again. On the other hand, if the number of times is too many, the effect becomes saturated, so the regeneration step S30 is preferably repeated 2 to 5 times, and more preferably repeated 3 to 4 times.

[0085] In addition, when the regeneration step S30 is performed multiple times, the same discharge route may be used for each regeneration step, but it is preferable to switch the discharge route depending on the number of times. For example, the opening and closing of the valves V7 and V8 may be controlled so that the first regeneration step S30 discharges the acid A into the waste water tank 70, and the second and subsequent regeneration steps S30 discharge the acid A into the acid waste liquid tank 80.

[0086] 4, the plating solution purification process P1 and the resin regeneration process P2 constitute one cycle, and the plating solution purification process P1 and the resin regeneration process P2 are performed multiple times. The number of repetitions is appropriately set depending on the amount of the chromium plating solution S to be treated and the concentration of the impurity metal ions, and the plating solution purification process P1 and the resin regeneration process P2 are alternately repeated until the impurity metal ions in the chromium plating solution S reach a target concentration.

[0087] [Embodiment 2] Fig. 9 is a photograph showing the appearance of a refining device 2 which is another embodiment of the refining device of the present invention, and Fig. 10 is a schematic diagram for explaining the refining device 2. In Figs. 9 and 10, the same components as those in Figs. 1 to 8 are given the same reference numerals as those in Figs. 1 to 8, and explanations thereof will be omitted.

[0088] 9 and 10 includes an ion exchange resin tower 110, a tank 40, a plating solution delivery path R1, a water delivery path R2, gas blowing paths R3a and R3b, an acid delivery path R4, discharge paths R5a to R5e, a control unit 130, and a cart 120. In the refinery 1, the tank 40 is mounted on a cart 120b different from the cart 120a on which the ion exchange resin tower 110 is mounted, whereas in the refinery 2, the tank 40 is mounted on the same cart 120 as the ion exchange resin tower 110, and further includes a control unit 130.

[0089] In the refining device 2, the ion exchange resin tower 110 and the tank 40 are mounted on the same cart 120. The ion exchange resin tower 110 and the tank 40 are connected via a pipe L42b provided with a valve V4, a pump P2, and a pipe L41, and the pipe L42b, the pump P2, and the pipe L41 constitute an acid liquid supply path R4. The other paths (R1, R2, R3a, R3b, R5a to R5e) are the same as those in the refining device 1, and the plating solution supply path R1, the water supply path R2, and the acid liquid supply path R4 join together on the downstream side and then join together with the downstream side of the gas blowing path R3a. The upstream side of the discharge path R5a can also become the downstream side of the gas blowing path R3b by switching the valve or the like.

[0090] The control unit 130 is a unit for controlling the valves (V1, V2, V3a, V3b, V4, V5a, V5b, V6, V7, V8) provided in each path (R1, R2, R3a, R3b, R4, and R5a to R5e), and has an input unit 131 and a control unit 132. The valves in each path are connected to the control unit 132. The input unit 131 is a touch panel or the like, and when information on opening and closing of the valves is input using the input unit 131, the information is input to the control unit 132. The control unit 132 controls the opening and closing of the valves in the paths based on the input information.

[0091] The method of purifying the chromium plating solution S using the refining device 2 is the same as the method of purifying the chromium plating solution S using the refining device 1. For example, the input unit 131 is used to input valve operations for the plating solution refining process P1 and the resin regenerating process P2 according to the flow diagram shown in Fig. 4, and the control unit 132 controls the opening and closing of the valves in accordance with the input valve operations, thereby automatically purifying the chromium plating solution S.

[0092] The refining apparatus of the present invention has been described above using the refining apparatus 1 and the refining apparatus 2 as examples, but the refining apparatus of the present invention is not limited to these. For example, the valve of the refining apparatus 1 may be automatically controlled by a control unit, as in the refining apparatus 2. The chromium plating solution S, the water W, and the acid A are not limited to being supplied to the lower part of the resin-filled layer 111 and discharged from the upper part of the resin-filled layer 111, but may be supplied from the upper part of the resin-filled layer 111 and discharged from the lower part of the resin-filled layer 111. In addition, a flow meter or a plurality of valves may be provided in the path, or each path may be provided with an independent pipe. On the other hand, as in the refining apparatus 1 and the refining apparatus 2, it is easier to make the device smaller when a part of each path is configured with the same pipe. In addition, a part of the plating solution delivery path, the water delivery path, the acid delivery path, etc. may be configured with a common pipe, and the chromium plating solution, water, acid, etc. may be supplied to the ion exchange resin tower by a pump provided in this common pipe. In this way, the chromium plating solution, water, acid, etc. can be delivered by a single pump. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.

[0094] <Example 1> Using the refining apparatus shown in FIG. 1, a deteriorated chromium plating solution (impurity concentrations: Fe(III) ion 6.3 g / L, Cr(III) ion 1.5 g / L) was refined.

[0095] The ion exchange resin tower has the following configuration: Cylindrical section 112a: φ30cm, H110cm ·Space 114: φ30cm, H40cm ·Resin filling layer 111: φ30cm, H70cm (49L) Cation exchange resin: Muromachi Chemical Co., Ltd., Muromac (registered trademark) XSC-1628-H (gel type, cross-linking degree 16%, particle size 315 μm to 1.25 mm)

[0096] 300L of deteriorated chrome plating solution was circulated at 500L / hr for 60 minutes. After that, the liquid in the resin was removed by air squeezing, and a batch-type water washing was performed three times by supplying water in an amount equal to the amount of resin and bubbling for one minute. Next, the liquid in the resin was removed by air squeezing, and a batch-type regeneration treatment (acid washing) was performed three times by supplying 10% sulfuric acid in an amount equal to the amount of resin and bubbling for 15 minutes. This operation from circulation of the deteriorated chrome plating solution to acid washing was considered as one cycle, and was repeated three times.

[0097] The amount of Fe removed was calculated as follows: 321 g of Fe was removed in the first circulation of the plating solution, 302 g in the second circulation, and 304 g in the third circulation. In total, 927 g of Fe was removed over the three circulations (180 min).

[0098] <Other use cases 1> A purification apparatus with the same configuration as that shown in Figure 1 was used. The resin capacity was 50 L. The impurity concentrations in the deteriorated chromium plating solution were 7.5 g / L for Fe(III) ions and 1.3 g / L for Cr(III) ions. 300 L of the deteriorated chromium plating solution was circulated at 500 L / hr for 300 minutes.

[0099] The amount of Fe removed was determined to be 561 g after 60 minutes of circulation of the plating solution, 649 g after 120 minutes, 675 g after 180 minutes, and 679 g after 300 minutes.

[0100] <Reference Example 1>: Column experiment (Column Experimental Equipment) Teflon (registered trademark) mesh was attached to both ends (suction port and discharge port) of the supply tube and to the suction port of the discharge tube. A 100 mL polypropylene gas washing bottle was filled with ion exchange resin. The supply tube was attached to the suction side of the gas washing bottle via a liquid delivery pump, and the discharge tube was attached to the discharge side of the gas washing bottle. The gas washing bottle was then connected to a container containing deteriorated chrome plating solution, forming the experimental apparatus shown in FIG. 11.

[0101] (Consideration of washing method) 500mL of deteriorated chromium plating solution was placed in a container and circulated at 1L / hr for 3 hours. The ion exchange resin was then washed with 10 times the amount of water as the resin in the gas washing bottle. The following methods (1) to (3) were used for washing, and the chromium concentration during washing was investigated depending on the washing method. - Water washing method (1): Flow washing, in which the washing water is simply poured in Water washing method (2): The plating solution remaining in the resin is removed with air, followed by flow cleaning. Water washing method (3): The plating solution remaining in the resin tower is removed with air, and then washing water is filled in batches to wash the tower.

[0102] Fig. 12 is a photograph showing the state of the cleaning solution during the water washing process, and Fig. 13 is a diagram showing the relationship between the chromium concentration in the cleaning solution and the number of washings. As shown in Fig. 13, the number of washings until the chromium concentration in the cleaning solution fell below 1000 ppm was 10 times for cleaning method (1), 5 times for cleaning method (2), and 2 times for cleaning method (3), showing that cleaning method (3) had a higher cleaning effect.

[0103] <Other use cases 2> The experiment was carried out using the same purification equipment as in Example 1. 300 L of deteriorated chromium plating solution was circulated at 450 L / hr for 1 hour. Then, the liquid in the resin was removed by air squeezing, and a batch-type water washing was carried out 1 to 3 times by supplying water in an amount equal to the amount of resin and bubbling for 5 minutes.

[0104] Figure 14 is a plot of the chromium concentration in the washing water versus the number of washings. As shown in Figure 14, it was found that the chromium in the resin could be significantly reduced by repeating washing with water multiple times. After three washings, the total chromium concentration was below 1000 ppm.

[0105] <Other use cases 3> The experiment was carried out using the same refining device as in Example 1. 300 L of deteriorated chrome plating solution was circulated at 450 L / hr for 1 hour. After that, the liquid in the resin was removed by squeezing with air, and a batch-type water washing was carried out three times by supplying water in an amount equal to the amount of resin and bubbling for 5 minutes. Next, a batch-type regeneration treatment (acid washing) was carried out 1 to 5 times by supplying 10% sulfuric acid in an amount equal to the amount of resin and bubbling for 5 minutes.

[0106] Figure 15 is a plot of the chromium concentration in acid versus the number of washes. As shown in Figure 15, the Fe(III) ions and chromium(III) ions in the resin could be reduced by acid washing, and 327.0 g of Fe(III) could be removed after three regeneration treatments. The initial amount of Fe adsorbed was 679 g, which means that approximately 50% of the resin was regenerated. After three washes, the total chromium concentration was below 1000 ppm.

[0107] <Other use cases 4> The experiment was carried out using the same refining equipment as in Example 1. 300 L of deteriorated chrome plating solution was circulated at 500 L / hr for 1 hour. After that, the liquid in the resin was removed by squeezing with air, and a batch-type water washing was carried out three times in which water was supplied in an amount equal to the amount of resin and bubbled for 1 minute. Next, the liquid in the resin was removed by squeezing with air, and a batch-type regeneration treatment (acid washing) was carried out three times in which 10% sulfuric acid was supplied in an amount equal to the amount of resin and bubbled for 5 to 15 minutes.

[0108] Figure 16 is a plot of the relationship between the acid cleaning time per cycle and the chromium concentration in the acid. Approximately 80% of the resin was regenerated by a 15-minute acid cleaning treatment per cycle.

[0109] <Reference example 2> A column packed with 50 L of cation exchange resin (Muromachi Chemical Co., Ltd., Muromac (registered trademark) XSC-1628-H) was filled with degraded chromium plating solution (Fe(III) ions 6.8 g / dm 3 , Cr(III) ion is 1.9g / dm 3 ) 300 L was forced to circulate using a pump at a rate of 500 L / hr, and the chromium plating solution in the plating tank was sampled at predetermined times to determine the concentrations of Fe ions and Cr(III) ions in the solution. FIG. 17 shows a plot of the concentrations of Fe(III) ions and Cr(III) ions in the treatment liquid versus the liquid passing time.

[0110] <Reference example 3> A column packed with 50 L of cation exchange resin (Mitsubishi Chemical Corporation, DIAION (registered trademark) PK228LH, porous type, cross-linking degree 14%, average particle size 740 μm) was filled with degraded chromium plating solution (Fe (III) ions 7.6 g / dm 3 , Cr(III) ion is 1.3g / dm 3 ) 300 L was forced to circulate using a pump at a rate of 500 L / hr, and the chromium plating solution in the plating tank was sampled at predetermined times to determine the concentrations of Fe ions and Cr(III) ions in the solution. FIG. 18 shows a plot of the concentrations of Fe(III) ions and Cr(III) ions in the treatment liquid versus the liquid passing time. [Industrial Applicability]

[0111] INDUSTRIAL APPLICABILITY According to the refining apparatus of the present invention, chromium plating solution containing accumulated impurity metal ions can be easily refined and reused, and therefore the apparatus is effective in industrial fields where chromium plating is performed. [Explanation of symbols]

[0112] 1, 2 Purification equipment 10 Plating bath 11, 20, 30, 43, 45, 62, 72, 82 Connection 40 Tank 50a, 51a, 51b, 51c, 52a, 52b, 52c end 70 Wastewater tank 80 Acid waste tank 100a Unit 1 100b 2nd unit 110 Ion exchange resin tower 111 Resin filled layer 112 Cabinet 112a Cylindrical part 113 Support plate 114 Space 115 Level Sensor 120, 120a, 120b trolley 130 Control Unit 131 Input section 132 Control section A acid G Gas H10a, H10b, H22, H32, H44, H70b, H80b hose L12, L13, L14, L15, L21, L31, L32, L33, L41, L42, L42b, L46, L50, L51, L52, L53, L54, L61, L71, L81 Piping P1, P2 pumps R1 Plating solution delivery path R2 Water supply route R3a, R3b Gas injection route R4, R4a, R4b Acid delivery path R5a, R5b, R5c, R5d, R5e Excretion Pathways S Chromium plating solution V1, V2, V3a, V3b, V4, V5a, V5b, V6, V7, V8 Valves W water

Claims

1. A portable purification device for purifying a chromium plating solution containing impurity metal ions, The refining device comprises: an ion exchange resin tower provided with a resin packed bed packed with a cation exchange resin for removing impurity metal ions; A tank containing an acid for regenerating the resin-filled bed; a plating solution delivery path for supplying the chromium plating solution in the chromium plating bath to the ion exchange resin tower; A water supply path for supplying water to the ion exchange resin tower; a gas blowing path for blowing a gas into the ion exchange resin tower; an acid supply path for supplying the acid contained in the tank to the ion exchange resin tower; a discharge path for discharging the chromium plating solution, the water, the gas, and the acid from the ion exchange resin tower; A cart for moving the refining apparatus; A refining apparatus comprising:

2. The gas blowing path has a first gas blowing path for blowing a gas into the resin-filled bed or from below the resin-filled bed, and a second gas blowing path for blowing a gas from above the resin-filled bed, 2. The purification apparatus according to claim 1, wherein the discharge path includes a discharge path for discharging the gas blown from the first gas blowing path to the outside of the ion exchange resin tower through an area above the resin packed bed, and a discharge path for discharging the gas blown from the second gas blowing path to the outside of the ion exchange resin tower through the resin packed bed.

3. The purification apparatus according to claim 1 or 2, wherein the amount of the cation exchange resin packed therein is 45 to 200 L.

4. 3. The refining apparatus according to claim 1, further comprising a control unit for automatically controlling opening and closing of one or more of the valves, the control unit being provided with valves in the plating solution supply path, the water supply path, the gas blowing path, the acid supply path and the exhaust path.

5. 3. The purification apparatus according to claim 1, wherein the volume of the tank is at least twice as large as the volume of the resin-filled bed.

6. A method for purifying a chrome plating solution containing impurity metal ions, comprising: The plating solution purification process includes passing the chromium plating solution through an ion exchange resin tower having a resin packed layer packed with a cation exchange resin to obtain a purified chromium plating solution, and regenerating the cation exchange resin after the plating solution purification process. The resin regeneration treatment comprises: a batch-type water washing step of supplying water to the ion exchange resin tower and then stirring the water to wash the cation exchange resin; a batch-type regeneration step of supplying an acid to the ion exchange resin tower after the water-washing step, and then stirring the acid to regenerate the cation exchange resin.

7. A method for purifying a chromium plating solution containing impurity metal ions, using the purification apparatus according to claim 1, comprising: The chromium plating solution is passed through the ion exchange resin tower to obtain a purified chromium plating solution, and a resin regeneration process is performed to regenerate the cation exchange resin after the plating solution purification process. The resin regeneration treatment comprises: a batch-type water washing step of supplying water to the ion exchange resin tower and then stirring the water to wash the cation exchange resin; a batch-type regeneration step of supplying an acid to the ion exchange resin tower after the water-washing step, and then stirring the acid to regenerate the cation exchange resin.

8. 8. The purification method according to claim 6, wherein the stirring in the water-washing step and the stirring in the regeneration step are carried out by bubbling a gas.

9. The purification method according to claim 6 or 7, wherein the washing time in the regeneration step is 5 to 60 minutes per washing.

10. The purification method according to claim 6 or 7, wherein the water-washing step and the regeneration step are each carried out consecutively two or more times.

11. 8. The purification method according to claim 6 or 7, wherein the water-washing step is carried out two or more times in succession, and waste liquid discharged in a first water-washing step is returned to the chromium plating bath containing the chromium plating solution.

Citation Information

Patent Citations

  • Method for purifying chromium plating solution or chromate solution and device therefor

    JP1997228069A

  • Apparatus for refining and recycling waste chromium solution and method for using the same

    JP3816547B2