toner
A toner with controlled inorganic fine particles A and B structures stabilizes silicone oil and reduces contamination, enhancing transferability and image uniformity during extended printing.
Patent Information
- Application Number
- JP2023057945
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing toners face challenges in maintaining high image quality and transfer efficiency over long periods due to silicone oil contamination and uneven charging, which occurs when inorganic fine particles treated with silicone oil volatilize and contaminate charging members.
A toner formulation using a combination of inorganic fine particles A and B, where A has a specific silicone oil-stabilizing structure and B has a low affinity for silicone oil, controlled through 29Si-NMR DD/MAS measurement to achieve optimal silicone oil release and transferability, suppressing contamination.
The toner achieves high transferability and suppresses member contamination, ensuring in-plane uniformity and fine line reproducibility even after prolonged continuous printing.
Smart Images

Figure 2024145547000001 
Figure 2024145547000002 
Figure 2024145547000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jet system. [Background technology]
[0002] In recent years, full-color electrophotographic copiers have become widespread and are increasingly being applied to the printing market, where there is a growing demand for high speed, high image quality, and high productivity while being compatible with a wide range of media (paper types). Toners are added with inorganic fine particles such as silica as an external additive for the purpose of imparting fluidity and stabilizing chargeability. External additives are also used to improve transferability, and toners with high transfer efficiency and no image defects are required to achieve high image quality. Patent Document 1 discloses a toner with high transfer efficiency obtained by externally adding inorganic fine powder with a silicone oil treatment on the surface.
[0003] However, silicone oil has a problem that it is liberated from the external additive and causes contamination of components such as charging components. When component contamination occurs, unevenness or streaks occur in the image, which is undesirable. Patent Document 2 discloses a toner in which silica particles, the surface of which is treated with a silane coupling agent and then treated with silicone oil, are added externally. In the toner described in Patent Document 2, the silane coupling agent and silicone oil are used in combination to reduce component contamination. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-204065 [Patent Document 2] JP 2004-126251 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, if higher image quality is required while operating continuously for a longer period of time, a larger discharge occurs for a longer period of time in the charging process, and the device is exposed to high discharge energy. When the surface of inorganic fine particles is treated with silicone oil, the silicone oil exposed to high discharge energy volatilizes and is easily liberated from the surface of the inorganic fine particles. As a result, the liberated silicone oil is likely to cause contamination of components such as charging components. Furthermore, the contamination of components may cause uneven charging, resulting in a decrease in image uniformity.
[0006] As described above, it has become clear that it is difficult to suppress the release of silicone oil when high image quality is required during long, continuous operation, and that it is difficult to achieve a high level of both transferability and suppression of component contamination. An object of the present disclosure is to solve the above problems and provide a toner that achieves a high degree of both transferability, such as fine line reproducibility, and suppression of component contamination, such as in-plane uniformity, even after long periods of continuous printing. [Means for solving the problem]
[0007] A toner having toner particles and inorganic fine particles, the inorganic fine particles have inorganic fine particles A and inorganic fine particles B different from the inorganic fine particles A, the inorganic fine particles A and the inorganic fine particles B contain silicone oil, The inorganic fine particles were washed with hexane and then used as a sample. 29 DD / MA of Si-NMR In S measurement, The inorganic fine particles A have a structure represented by the following formula (1): a and the peak PD1w corresponding to a silicon atom represented by the following formula (2): b and a peak PD2w corresponding to a silicon atom represented by The inorganic fine particles B have a structure represented by the following formula (3): c The peak PM1w corresponds to a silicon atom represented by When the area of the peak PD1w is SD1w and the area of the peak PD2w is SD2w, the SD1w and the SD2w satisfy the following: 1.2≦(SD1w+SD2w) / SD1w≦3.8 When the area of the peak PM1w is SM1w, the SD1w and the SM1w satisfy the following: 0.20≦SD1w / SM1w≦0.90 A toner characterized by: [ka] (In the formulas (1) to (3), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate.) Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a toner that achieves a high degree of both transferability, such as fine line reproducibility, and suppression of component contamination, such as in-plane uniformity, even after long periods of continuous printing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.
[0010] The present inventors have conducted extensive research with the aim of providing a toner that can achieve both excellent transferability and suppression of member contamination even after long periods of continuous printing. As a result, they have found that the above-mentioned problems can be solved by the following toner.
[0011] The toner has toner particles and inorganic fine particles. The inorganic fine particles include inorganic fine particles A and inorganic fine particles B different from inorganic fine particles A. The inorganic fine particles A and inorganic fine particles B contain silicone oil.
[0012] Solid samples of inorganic particles after washing with hexane 29 In the Si-NMR DD / MAS measurement, the inorganic fine particles A are Si in the structure represented by the following formula (1): a and the peak PD1w corresponding to a silicon atom represented by the following formula (2): b In addition, the inorganic fine particles B have a peak PD2w corresponding to a silicon atom represented by the following formula (3): c The peak PM1w corresponds to the silicon atom represented by [ka]
[0013] In formulas (1) to (3), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate. X is, for example, an atom of silicon, titanium, aluminum, magnesium, potassium, calcium, strontium, barium, chromium, iron, cobalt, nickel, copper, zinc, gallium, germanium, etc. In formula (2), Si present on the opposite side to X (the surface structure side of the inorganic fine particle) is bonded to, for example, Si linked by an oxygen atom or a methyl group.
[0014] When the area of peak PD1w is SD1w and the area of peak PD2w is SD2w, SD1w and SD2w satisfy the following. 1.2≦(SD1w+SD2w) / SD1w≦3.8 When the area of peak PM1w is SM1w, SD1w and SM1w satisfy the following. 0.20≦SD1w / SM1w≦0.90
[0015] Although the detailed reasons why the effects of the present disclosure are obtained have not been clarified, the present inventors hypothesize the mechanism as follows.
[0016] Solid samples of inorganic particles after washing with hexane 29In the Si-NMR DD / MAS measurement, the inorganic fine particles A have a peak PD1w and a peak PD2w. This is considered to indicate that the structures represented by the formulas (1) and (2) are formed on the surface of the inorganic fine particles A.
[0017] The structure represented by formula (2) has a high affinity with silicone oil. Therefore, it is believed that if inorganic fine particles A have the structure represented by formula (2), the state of silicone oil can be stabilized. As a result, it is believed that the silicone oil can be prevented from volatilizing even when it is subjected to higher energy than before, and that contamination of components caused by silicone oil can be prevented. On the other hand, when only inorganic fine particles A are added externally to toner particles, the transferability tends to be somewhat insufficient.
[0018] Solid samples of inorganic particles after washing with hexane 29 In the Si-NMR DD / MAS measurement, the inorganic fine particles B have a peak PM1w. This is considered to indicate that the structure represented by formula (3) is formed on the surface of the inorganic fine particles B.
[0019] The structure represented by formula (3) has low affinity with silicone oil. Therefore, it is considered that when inorganic fine particles B have the structure represented by formula (3), the affinity with silicone oil is low. As a result, it is considered that the silicone oil is easily volatilized, and the transferability can be improved. On the other hand, when only inorganic fine particles B are added externally, the silicone oil is easily volatilized, and the component contamination caused by the silicone oil is easily caused.
[0020] That is, it is considered that the liberation of silicone oil can be appropriately controlled and both transferability and suppression of member contamination can be achieved by using inorganic fine particles A and inorganic fine particles B in combination. In order to accurately control the liberation of silicone oil, it is important to appropriately control the abundance ratio of inorganic fine particles A and inorganic fine particles B on the toner particle surface. The components constituting the toner will be described in detail below.
[0021] <Inorganic fine particles> The toner has toner particles and inorganic fine particles. For example, the toner can be obtained by externally adding inorganic fine particles to the toner particles by a method described later. Examples of inorganic fine particles include silica fine particles, metal oxides (e.g., titanium oxide fine particles, aluminum oxide fine particles, and strontium titanate fine particles). The inorganic fine particles are preferably silica fine particles. Examples of silica fine particles that can be used include fumed silica and sol-gel silica. The inorganic fine particles are preferably an inorganic fine particle base that has been surface-treated with a surface treatment agent. The inorganic fine particle base refers to inorganic fine particles that have not been surface-treated.
[0022] The inorganic fine particles include inorganic fine particles A and inorganic fine particles B which are different from the inorganic fine particles A. It is preferable that the inorganic fine particles A and the inorganic fine particles B contain silica fine particles. That is, it is preferable that the inorganic fine particle base of the inorganic fine particles A and the inorganic fine particles B is silica fine particles. It is preferable that the inorganic fine particles A are surface-treated with a surface treatment agent. It is also preferable that the inorganic fine particles B are surface-treated with a surface treatment agent different from the surface treatment agent used for the inorganic fine particles A. It is preferable that the inorganic fine particles A and the inorganic fine particles B have a surface-treated product formed by surface treatment.
[0023] Solid samples of inorganic particles after washing with hexane 29 In the Si-NMR DD / MAS measurement, the inorganic fine particles A are Si in the structure represented by the following formula (1): a and the peak PD1w corresponding to a silicon atom represented by the following formula (2): b and a peak PD2w corresponding to a silicon atom represented by [ka]
[0024] In formulas (1) and (2), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate. X is, for example, an atom of silicon, titanium, aluminum, magnesium, potassium, calcium, strontium, barium, chromium, iron, cobalt, nickel, copper, zinc, gallium, germanium, etc. In formula (2), Si present on the opposite side to X (the surface structure side of the inorganic fine particle) is bonded to, for example, Si connected by an oxygen atom or a methyl group.
[0025] The observation of peaks PD1w and PD2w is considered to indicate that structures represented by formulas (1) and (2) are formed on the surfaces of inorganic fine particles A.
[0026] The structures represented by formulas (1) and (2) can be formed, for example, by surface-treating inorganic fine particles with a surface treatment agent containing a siloxane bond. The method for producing inorganic fine particles A includes a first-stage reaction of surface-treating an inorganic fine particle base with a surface treatment agent containing a siloxane bond, and a second-stage reaction of surface-treating the surface-treated inorganic fine particles with silicone oil. That is, inorganic fine particles A are preferably surface-treated inorganic fine particles with a surface treatment agent containing a siloxane bond and silicone oil.
[0027] The first reaction step of surface treating the inorganic fine particle substrate with a surface treating agent containing a siloxane bond will be described below. The structure represented by the formulas (1) and (2) can be formed by treating the surface of an inorganic fine particle substrate with a surface treatment agent containing a siloxane bond. The surface treatment agent containing a siloxane bond is not particularly limited, and a known material can be used, and the surface of the inorganic fine particle substrate can be treated under the conditions described below.
[0028] Examples of surface treatment agents containing siloxane bonds include the following: Cyclic siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and decamethylcyclopentasiloxane.
[0029] The surface treatment agent containing a siloxane bond is preferably a cyclic siloxane, more preferably a cyclic siloxane having up to 10 ring members. In the cyclic siloxane, some of the methyl groups bonded to the silicon atom may have a substituent. Among the cyclic siloxanes, at least one selected from the group consisting of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and decamethylcyclopentasiloxane is preferred. From the viewpoints of ease of control of the chain length and ease of purification, it is more preferred to include octamethylcyclotetrasiloxane.
[0030] The method for surface treatment of the inorganic fine particle substrate is not particularly limited, and can be carried out by contacting the inorganic fine particle substrate with a surface treatment agent containing siloxane bonds. From the viewpoint of uniformly forming the structures represented by formulae (1) and (2) on the surface of the inorganic fine particle substrate, it is preferable to contact the inorganic fine particle substrate with the surface treatment agent containing siloxane bonds in a dry state. For example, as described below, a method of contacting vapor of a surface treatment agent containing siloxane bonds with an inorganic fine particle substrate can be mentioned. Alternatively, a stock solution of a surface treatment agent containing siloxane bonds or a diluted solution with various solvents can be sprayed and contacted with an inorganic fine particle substrate.
[0031] The contact of the surface treatment agent containing siloxane bonds with the inorganic fine particle substrate is preferably carried out by contacting the vapor of the surface treatment agent with the inorganic fine particle substrate under reduced pressure or in an inert gas atmosphere such as a nitrogen atmosphere. By using the method of contacting with vapor, it is easy to remove the surface treatment agent that does not react with the surface of the inorganic fine particle substrate, and it is easy to control the amount of moisture adsorption. When using the method of contacting with vapor of the surface treatment agent, it is preferable to treat at a treatment temperature equal to or higher than the boiling point of the surface treatment agent. The contact of the inorganic fine particle substrate with the vapor of the surface treatment agent may be carried out multiple times (for example, 2 to 3 times).
[0032] In the first reaction step of surface treating the inorganic fine particle base with a surface treatment agent containing siloxane bonds, for example, the surface treatment agent containing siloxane bonds is added to the inorganic fine particle base, and heated and stirred at a temperature of 300° C. or higher. By carrying out a heating and stirring treatment at a high temperature of 300°C or more, the surface treatment agent that has reacted with the surface of the inorganic fine particle substrate can further react with the surface of another inorganic fine particle substrate. Therefore, the molecular structure of the surface treatment agent is cut, the bulk of the molecular structure is reduced, and the surface treatment agent can react more effectively with the surface of the inorganic fine particle substrate. As a result, it is believed that the structures represented by formulas (1) and (2) can be densely formed on the surface of the inorganic fine particle substrate.
[0033] As mentioned above, the solid sample was inorganic fine particles after washing with hexane. 29 In the Si-NMR DD / MAS measurement, the inorganic fine particles A have a peak PD1w and a peak PD2w. The fact that the inorganic fine particles A after washing with hexane have peaks PD1w and PD2w indicates that polar groups OR are present at the ends of the siloxane chains chemically bonded to the surfaces of the inorganic fine particles A by the above-mentioned surface treatment. It is believed that the presence of a polar group OR at the end of the siloxane chain chemically bonded to inorganic fine particles A makes it possible to more strongly adsorb the silicone oil present on the surface of the inorganic fine particles, thereby suppressing the release of the silicone oil.
[0034] The magnitude of the polarity of the polar group OR present at the end of the siloxane chain correlates with the length of the siloxane chain, which corresponds to the distance from the substrate of the inorganic fine particle A to the polar group OR. When the length of the siloxane chain is within a specific range, the polarity of the polar group OR becomes appropriate, and the balance between the inhibition of the release of silicone oil and the lubricating effect of the silicone oil becomes appropriate. As a result, it is possible to achieve a high degree of both improved transferability and inhibition of contamination of components. In addition, it is possible to obtain a toner that has excellent charging properties while providing excellent fluidity to the toner.
[0035] When the area of peak PD1w is SD1w and the area of peak PD2w is SD2w, SD1w and SD2w satisfy the relationship 1.2≦(SD1w+SD2w) / SD1w≦3.8. The fact that SD1w and SD2w satisfy the above relationship indicates that the length of the siloxane chain corresponding to the distance from the substrate of the inorganic fine particle A to the polar group OR is appropriate. When SD1w and SD2w satisfy the above relationship, it is possible to optimally control the inhibition of the release of silicone oil from the surface of inorganic fine particles and the lubricating effect. As a result, it is possible to highly simultaneously improve the transferability and inhibit the contamination of components. In addition, it is possible to provide the toner with excellent flowability. It is possible to obtain a toner having excellent chargeability while providing the toner with excellent electrostatic properties.
[0036] A ratio of SD1w+SD2w of 1.2 or more indicates that the siloxane chain is appropriately long and the distance between the polar group OR and the inorganic fine particle substrate is appropriately maintained. As a result, the lubricating effect of the silicone oil is easily obtained. On the other hand, SD1w+SD2w being 3.8 or less indicates that the siloxane chain is not too long and the distance between the polar group OR and the inorganic fine particle substrate is appropriately maintained, which makes it easier to suppress the release of silicone oil.
[0037] As described above, the surface treatment agent containing a siloxane bond used in the first stage treatment is preferably a cyclic siloxane. It is more preferable to carry out the surface treatment at a temperature of 300° C. or higher. Cyclic siloxanes react with the surface of inorganic fine particle substrates through a ring-opening reaction, and therefore tend to form the structure shown in formula (1) on the inorganic fine particle substrate. On the other hand, atoms having the structure shown in formula (1) at their terminals, which are generated as a result of the ring-opening, tend to become reaction points with other cyclic siloxanes, and tend to have long chain lengths. In contrast, by setting the treatment temperature to 300°C or higher, both the creation and scission of siloxane bonds tend to proceed in parallel. As a result, the siloxane chains are appropriately short in length and uniformly aligned.
[0038] The value of (SD1w+SD2w) / SD1w is preferably 1.5 or more, and more preferably 2.0 or more. Also, it is preferably 3.5 or less, and more preferably 3.0 or less. For example, it may be in the range of 1.5 to 3.5 or 2.0 to 3.0.
[0039] The fact that SD1w and SD2w satisfy 1.2≦(SD1w+SD2w) / SD1w≦3.8 can be achieved by increasing the treatment temperature during the reaction between the inorganic fine particle base and the surface treatment agent containing a siloxane bond. The treatment temperature varies depending on the reactivity of the surface treatment agent used, but is, for example, preferably 150° C. or higher, more preferably 280° C. or higher, and further preferably 300° C. or higher. Also, it is preferably 380° C. or lower, more preferably 350° C. or lower. For example, the ranges include 150 to 380° C., 280 to 380° C., 300 to 380° C., 280 to 350° C., and 300 to 350° C.
[0040] For example, the value of (SD1w+SD2w) / SD1w can be reduced by lowering the treatment temperature during the reaction between the inorganic particulate substrate and the surface treatment agent containing siloxane bonds, while the value of (SD1w+SD2w) / SD1w can be increased by increasing the treatment temperature.
[0041] The treatment time varies depending on the treatment temperature and the reactivity of the surface treatment agent used, but is preferably 5 minutes or more, more preferably 30 minutes or more, and even more preferably 150 minutes or more. Also, it is preferably 300 minutes or less, more preferably 250 minutes or less, and even more preferably 200 minutes or less. For example, the ranges include 5 to 300 minutes, 30 to 250 minutes, and 150 to 200 minutes. The treatment temperature and treatment time of the surface treatment are preferably within the above-mentioned ranges from the viewpoint of allowing the surface treatment agent to react sufficiently with the inorganic fine particle base and from the viewpoint of production efficiency.
[0042] The value of SD1w is preferably 4.0 to 12.0, and more preferably 6.0 to 10.0. The value of SD2w is preferably 8.0 to 16.0, and more preferably 10.0 to 14.0. When the values of SD1w and SD2w are within the above ranges, liberation of silicone oil is more easily suppressed, and contamination of components is more easily suppressed.
[0043] The amount of the surface treatment agent containing a siloxane bond added is preferably 40 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 100 parts by mass or more, relative to 100 parts by mass of the inorganic fine particle base. Also, it is preferably 180 parts by mass or less, and even more preferably 150 parts by mass or less. For example, the range may be 40 to 180 parts by mass, 70 to 180 parts by mass, 100 to 180 parts by mass, 70 to 150 parts by mass, or 100 to 150 parts by mass. In particular, when the surface treatment is carried out by contacting the surface treatment agent containing siloxane bonds with vapor, the inorganic fine particle base can be uniformly surface-treated by adding 100 parts by mass or more to the inorganic fine particle base.
[0044] When the surface treatment is performed under reduced pressure, the pressure of the vapor of the surface treatment agent containing siloxane bonds in the container is preferably controlled to 0.1 to 100 Pa, and more preferably 1.0 to 10 Pa. By setting the pressure in the above range, the frequency of contact between the molecules of the surface treatment agent in the vapor is reduced, and chemical reactions between the surface treatment agents themselves can be suppressed. As a result, the chemical reaction between the surface treatment agent in contact with the surface of the inorganic fine particle substrate and the inorganic fine particle substrate can be preferentially carried out. Furthermore, reaction by-products generated by the chemical reaction between the inorganic fine particle substrate and the surface treatment agent can be easily removed from the vicinity of the surface of the inorganic fine particle substrate. As a result, the surface treatment agent can more easily come into contact with the surface of the inorganic fine particle substrate, and the inorganic fine particle substrate can be more uniformly surface-treated.
[0045] In addition, when the surface treatment is performed under reduced pressure, it is preferable to perform a degassing treatment in which the inorganic fine particle base is heated under reduced pressure and moisture adsorbed on the surface of the inorganic fine particle base is removed before the surface treatment agent containing siloxane bonds is brought into contact with the surface of the inorganic fine particle base. In this way, the surface treatment agent containing siloxane bonds can be more easily brought into contact with the surface of the inorganic fine particle base, and the inorganic fine particle base can be more uniformly surface-treated.
[0046] From the viewpoint of making it easier for the surface treatment agent containing siloxane bonds to come into contact with the surface of the inorganic fine particle base, it is also preferable to repeatedly carry out a degassing treatment and a surface treatment of the inorganic fine particles with the surface treatment agent containing siloxane bonds.
[0047] During the degassing treatment, the pressure inside the container is preferably 0.1 Pa or less, and more preferably 0.01 Pa or less. The temperature inside the container is preferably 150 to 380°C, and more preferably 300 to 350°C.
[0048] Since inorganic fine particles A have the structures represented by formulas (1) and (2) on the surface, the silicone oil is chemically reacted with the structures represented by formulas (1) and (2) by treatment with silicone oil described later, and the inorganic fine particles A are fixed. That is, it is considered that inorganic fine particles A have a surface treatment product including a reaction product between a surface treatment agent including a siloxane bond and silicone oil. On the other hand, a portion of the silicone oil that did not contribute to the reaction remains as a free component on the surface of the inorganic fine particles A. Therefore, it is possible to suppress contamination of the member while maintaining transferability.
[0049] The second stage reaction in which inorganic fine particles that have been surface-treated with a surface treatment agent containing siloxane bonds are surface-treated with silicone oil will be described below. The inorganic fine particles that have been surface-treated with a surface treatment agent containing a siloxane bond are subjected to a second-stage reaction of surface treatment with silicone oil to obtain inorganic fine particles A. That is, it is preferable that the inorganic fine particles A are surface-treated with a surface treatment agent containing a siloxane bond and silicone oil. The inorganic fine particles A contain silicone oil. A part of the silicone oil is present on the surface of the inorganic fine particles A as a free component.
[0050] In the second step, the inorganic particles having the structures shown in formulas (1) and (2) are reacted with the Add corn oil and heat treatment. Silicone oil is not particularly limited, and can use known silicone oil.For example, silicone oil such as dimethyl silicone oil; silicone oils modified with organic groups at the side chain or end of dimethyl silicone oil such as methyl hydrogen silicone oil, methyl phenyl silicone oil, alkyl modified silicone oil, chloroalkyl modified silicone oil, chlorophenyl modified silicone oil, fatty acid modified silicone oil, polyether modified silicone oil, alkoxy modified silicone oil, carbinol modified silicone oil, amino modified silicone oil, and fluorine modified silicone oil can be mentioned.From the viewpoint of reactivity, it is preferable to use polydimethylsiloxane.
[0051] The content of silicone oil in inorganic fine particles A is preferably 3.0 to 15.0% by mass, more preferably 4.0 to 10.0% by mass, and even more preferably 4.5 to 8.2% by mass. When the content of silicone oil is within the above range, it is possible to highly improve transferability and prevent member contamination. In addition, it is possible to obtain a toner having excellent chargeability while imparting excellent fluidity to the toner.
[0052] Silicone oil may be added as a solution diluted with an organic solvent such as hexane. The dilution ratio when diluting silicone oil with an organic solvent is not particularly limited, but it is preferable to adjust the amount of silicone oil added relative to the mass of inorganic fine particles to be within the above range. When it is within this range, it is possible to highly improve transferability and member contamination. In addition, it is possible to obtain a toner that is excellent in chargeability while imparting excellent fluidity to the toner. For example, it is preferable to dilute silicone oil 5 to 15 times with an organic solvent such as hexane.
[0053] The treatment temperature when adding silicone oil and performing heat treatment is not particularly limited because it varies depending on the reactivity of the silicone oil used. For example, it is preferable to mix inorganic fine particles surface-treated with a surface treatment agent and silicone oil and heat-treat at a temperature of 300°C or higher. By setting the treatment temperature at 300°C or higher, the surface of the inorganic fine particles surface-treated with the surface treatment agent and the silicone oil can be easily and uniformly mixed. The upper limit of the treatment temperature is not particularly limited, but is preferably 380°C or lower, more preferably 350°C or lower. For example, it is preferably 300 to 380°C, more preferably 300 to 350°C.
[0054] The treatment time when adding silicone oil and carrying out heat treatment varies depending on the treatment temperature and the reactivity of the silicone oil used, but is preferably 5 minutes or more, more preferably 30 minutes or more, and even more preferably 60 minutes or more. Also, it is preferably 300 minutes or less, more preferably 240 minutes or less, and even more preferably 200 minutes or less. For example, it can be in the range of 5 to 300 minutes, 30 to 240 minutes, or 60 to 200 minutes. The treatment temperature and treatment time for the surface treatment are preferably within the above-mentioned ranges from the viewpoint of allowing the silicone oil to react sufficiently with the inorganic fine particles and from the viewpoint of production efficiency.
[0055] The structure represented by formula (2) formed by the first-stage treatment with a surface treatment agent containing siloxane bonds also partially reacts with silicone oil. Therefore, by setting the treatment temperature at 300°C or higher, the carbon reduction rate when the inorganic fine particles A are washed with hexane can be controlled. The carbon reduction rate when the inorganic fine particles are washed with hexane will be described later.
[0056] The kinetic viscosity of silicone oil at a temperature of 25°C is 30 mm 2 / s or more is preferable, 50 mm 2 / s or more is preferable. 2 / s or less is preferable, 200 mm 2For example, 30 to 500 mm / s or less is more preferable. 2 / s, 50~200mm 2 Examples include the range of / s.
[0057] The inorganic fine particles A can be produced, for example, by the following method. (First stage reaction) In an inert gas atmosphere such as nitrogen, the inorganic fine particle substrate is brought into contact with the vapor of a surface treatment agent containing siloxane bonds (e.g., cyclic siloxane). The surface of the inorganic fine particle substrate is treated with the surface treatment agent containing siloxane bonds by heating and stirring to obtain inorganic fine particles having the structures represented by formulas (1) and (2). (Second stage reaction) Silicone oil is added to the inorganic fine particles, and the surfaces of the inorganic fine particles are treated with the silicone oil by heating and stirring to obtain inorganic fine particles A. As described above, the heating and stirring treatment is preferably carried out at a temperature equal to or higher than the melting point of the surface treatment agent containing siloxane bonds (e.g., 330° C.). Furthermore, before mixing the inorganic fine particle base with the surface treatment agent containing siloxane bonds, a degassing treatment may be carried out as necessary.
[0058] The amount of water adsorption of inorganic fine particles can be controlled by the degree of coating of the inorganic fine particles. Specifically, by increasing the reaction time or treating at a high temperature, the degree of coating of the inorganic fine particles can be increased and the amount of water adsorption can be reduced. Also, by shortening the reaction time or treating at a low temperature, the degree of coating of the inorganic fine particles can be decreased and the amount of water adsorption can be increased.
[0059] Solid samples of inorganic particles after washing with hexane 29 In the Si-NMR DD / MAS measurement, the inorganic fine particles B are Si in the structure represented by the following formula (3): c The peak PM1w corresponds to the silicon atom represented by [ka] In formula (3), each R independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate, such as silicon, titanium, aluminum, magnesium, potassium, calcium, strontium, barium, chromium, iron, cobalt, nickel, copper, zinc, gallium, or germanium.
[0060] The observation of peak PM1w is considered to indicate that the structure represented by formula (3) is formed on the surface of inorganic fine particles B.
[0061] The structure represented by formula (3) can be formed, for example, by surface-treating an inorganic fine particle substrate with a silane compound. The method for producing inorganic fine particles B includes a first-stage reaction of surface-treating an inorganic fine particle base with a silane compound, and a second-stage reaction of surface-treating the inorganic fine particles surface-treated with the silane compound with silicone oil. That is, inorganic fine particles B are preferably inorganic fine particles surface-treated with a silane compound and silicone oil.
[0062] The first reaction step of surface treating the inorganic fine particle substrate with a silane compound will be described below. The structure represented by formula (3) can be formed by treating the surface of an inorganic fine particle substrate with a silane compound. The silane compound is not particularly limited and any known material can be used, and the surface of the inorganic fine particle substrate can be treated under the conditions described below.
[0063] Examples of the silane compound that can be used include the following: alkoxysilanes such as methoxysilane, ethoxysilane, and propoxysilane; halosilanes such as chlorosilane, bromosilane, and iodosilane; hydrosilanes; alkylsilanes; arylsilanes; vinylsilanes; acrylicsilanes; epoxysilanes; silyl compounds; siloxanes; silylureas; silylacetamides; and silane compounds having different types of substituents simultaneously that these silane compounds have. Specific examples include trimethylsilane, trimethylchlorosilane, trimethylethoxysilane, dimethyldichlorosilane, methyltrichlorosilane, allyldimethylchlorosilane, α-chloroethyltrichlorosilane, β-chloroethyltrichlorosilane, chloromethyldimethylchlorosilane, dimethyldiethoxysilane, dimethyldimethoxysilane, and hexamethyldisiloxane.
[0064] The silane compound is preferably a silazane compound. For example, the following can be used as the silazane compound. Dimethyldisilazane, trimethyldisilazane, tetramethyldisilazane, pentamethyldisilazane, hexamethyldisilazane, octamethyltrisilazane, hexamethylcyclotrisilazane, tetraethyltetramethylcyclotetrasilazane, tetraphenyldimethyldisilazane, dipropyltetramethyldisilazane, dibutyltetramethyldisilazane, dihexyltetramethyldisilazane, dioctyltetramethyldisilazane, diphenyltetramethyldisilazane, octamethylcyclotetrasilazane, etc. From the viewpoint of reactivity, the silazane compound is more preferably hexamethyldisilazane.
[0065] The method of performing the surface treatment of the inorganic fine particle substrate is not particularly limited, and can be performed by contacting a silane compound (e.g., a silazane compound) with the inorganic fine particle substrate. From the viewpoint of uniformly forming the structure represented by formula (3) on the surface of the inorganic fine particle substrate, it is preferable to contact the silane compound with the inorganic fine particle substrate in a dry manner. For example, there can be mentioned a method of contacting the vapor of the silane compound with the inorganic fine particle substrate, or a method of spraying the undiluted solution of the silane compound or a diluted solution of the silane compound with various solvents and contacting it with the inorganic fine particle substrate.
[0066] The contact of the silane compound with the inorganic fine particle substrate is preferably carried out by contacting the vapor of the silane compound under reduced pressure or in an inert gas atmosphere such as a nitrogen atmosphere. By using the method of contacting the vapor, it becomes easy to remove the silane compound that does not react with the surface of the inorganic fine particle substrate, and it becomes easy to control the amount of moisture adsorption. When using the method of contacting the vapor of the silane compound, it is necessary to carry out the treatment at a treatment temperature equal to or higher than the boiling point of the silane compound. The contact of the inorganic fine particle substrate with the vapor of the silane compound may be carried out multiple times (for example, 2 to 3 times).
[0067] In the first stage reaction of surface-treating the inorganic fine particle substrate with a silane compound, for example, a silane compound is added to the inorganic fine particle substrate, and a heating and stirring process is performed at a temperature of 200°C or higher. By performing a heating and stirring process at a high temperature of 200°C or higher, the silane compound that has reacted with the surface of the inorganic fine particle substrate can further react with the surface of another inorganic fine particle substrate. As a result, the molecular structure of the silane compound is cut, the bulk of the molecular structure is reduced, and the silane compound can react more effectively with the surface of the inorganic fine particle substrate. As a result, it is believed that the structure represented by formula (3) can be densely formed on the surface of the inorganic fine particle substrate.
[0068] Furthermore, when surface treatment is performed under reduced pressure, the pressure of the vapor of the silane compound in the container is preferably controlled to 0.1 to 100 Pa, and more preferably 1.0 to 10 Pa. By setting the pressure within the above range, the frequency with which the silane compound molecules in the vapor come into contact with each other is reduced, and chemical reactions between the silane compounds themselves can be suppressed. As a result, the chemical reaction between the silane compound in contact with the surface of the inorganic fine particle substrate and the inorganic fine particle substrate can be preferentially carried out. Furthermore, the chemical reaction between the inorganic fine particle substrate and the silane compound can be suppressed. The generated reaction by-products can be easily removed from the vicinity of the surface of the inorganic fine particle substrate, which makes it easier for the silane compound to come into contact with the surface of the inorganic fine particle substrate, thereby enabling the inorganic fine particle substrate to be surface-treated more uniformly.
[0069] In addition, when the surface treatment is performed under reduced pressure, it is preferable to perform the above-mentioned degassing treatment before contacting the silane compound with the surface of the inorganic fine particle base. From the viewpoint of making it easier for the silane compound to come into contact with the surface of the inorganic fine particle base, it is also preferable to repeatedly perform the degassing treatment and the surface treatment of the inorganic fine particles with the silane compound.
[0070] The treatment time varies depending on the treatment temperature and the reactivity of the silane compound used, but is preferably 5 minutes or more, more preferably 30 minutes or more, and even more preferably 150 minutes or more. Also, it is preferably 300 minutes or less, more preferably 250 minutes or less, and even more preferably 200 minutes or less. For example, it may be in the range of 5 to 300 minutes, 30 to 250 minutes, or 150 to 200 minutes. The treatment temperature and treatment time of the surface treatment in the above-mentioned ranges are preferable from the viewpoint of sufficiently reacting the silane compound with the inorganic fine particle base and from the viewpoint of production efficiency.
[0071] The amount of the silane compound added is preferably 40 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 100 parts by mass or more, relative to 100 parts by mass of the inorganic fine particle substrate. Also, it is preferably 180 parts by mass or less, and even more preferably 150 parts by mass or less. For example, the ranges include 40 to 180 parts by mass, 70 to 180 parts by mass, 100 to 180 parts by mass, 70 to 150 parts by mass, and 100 to 150 parts by mass. In particular, when the surface treatment is performed by contacting the silane compound with steam, the inorganic fine particle substrate can be uniformly surface-treated by adding 100 parts by mass or more to the inorganic fine particle substrate.
[0072] The second stage reaction in which the inorganic fine particles, which have been surface-treated with the silane compound, are surface-treated with silicone oil will be described below. The inorganic fine particles surface-treated with the silane compound are subjected to a second-stage reaction of surface-treating with silicone oil to obtain inorganic fine particles B. That is, it is preferable that the inorganic fine particles B are surface-treated with a silane compound and silicone oil. As described above, it is preferable that the silane compound is a silazane compound. That is, it is preferable that the inorganic fine particles B are inorganic fine particles surface-treated with a silazane compound and silicone oil. The inorganic fine particles B contain silicone oil. A part of the silicone oil is present on the surface of the inorganic fine particles B as a free component.
[0073] Silicone oil is not particularly limited, and known silicone oil can be used. For example, the above-mentioned silicone oil can be used. The silicone oil contained in inorganic fine particles A and inorganic fine particles B can be the same or different. The surface treatment with silicone oil can be performed in the same manner as the surface treatment of inorganic fine particles A described above. The content of silicone oil in inorganic fine particles B is preferably 3.0 to 15.0% by mass, more preferably 4.0 to 10.0% by mass, and even more preferably 4.5 to 8.2% by mass. When the content of silicone oil is within the above range, it is possible to highly improve transferability and prevent member contamination. In addition, it is possible to obtain a toner having excellent chargeability while imparting excellent fluidity to the toner.
[0074] Since inorganic fine particles B have a structure represented by formula (3) on the surface, a part of the silicone oil reacts chemically with the structure represented by formula (3) and is fixed. That is, inorganic fine particles B are considered to have a surface treatment containing a reaction product of a silane compound and silicone oil. On the other hand, the silicone oil that did not contribute to the reaction exists as a free component on the surface of inorganic fine particles B. The structure formed on the surface of inorganic fine particles B, which is represented by formula (3), has low affinity with the silicone oil present on the surface of inorganic fine particles B. As a result, the silicone oil is volatilized. It is believed that this makes it easier for the toner to evolve, thereby improving transferability.
[0075] That is, by externally adding the inorganic fine particles B obtained by the above-mentioned surface treatment method, the silicone oil becomes easy to be liberated, and the transfer voids are suppressed, and the transferability can be improved.
[0076] The inorganic fine particles B can be produced, for example, by the following method. (First stage reaction) In an inert gas atmosphere such as nitrogen, the inorganic fine particle substrate is brought into contact with vapor of a silane compound (e.g., silazane). The surface of the inorganic fine particle substrate is treated with the silane compound by heating and stirring to obtain inorganic fine particles having a structure represented by formula (3). (Second stage reaction) Silicone oil is added to the inorganic fine particles, and the surfaces of the inorganic fine particles are treated with the silicone oil by heating and stirring to obtain inorganic fine particles B. As described above, the heating and stirring treatment is preferably carried out at a temperature equal to or higher than the melting point of the silane compound (for example, 200° C.) Before mixing the inorganic fine particle base with the silane compound, a degassing treatment may be carried out as necessary.
[0077] When the area of peak PM1w is SM1w, SD1w and SM1w satisfy the following. 0.20≦SD1w / SM1w≦0.90
[0078] The value of SD1w / SM1w in the range of 0.20 to 0.90 indicates that inorganic fine particles A and inorganic fine particles B are present at an appropriate ratio on the surface of the toner particles. When SD1w / SM1w is 0.20 or more, the liberation of silicone oil is appropriately suppressed, and contamination of components can be suppressed. In addition, good fluidity can be maintained. When SD1w / SM1w is 0.90 or less, the lubricating properties of the silicone oil are fully exhibited, and the chargeability of the toner tends to be stable.
[0079] That is, by satisfying the above relationship between SD1w and SM1w, it is possible to maximize the lubricating effect of the silicone oil contained in the inorganic fine particles A and B to improve transferability, while suppressing the liberation of the silicone oil and suppressing contamination of components. In addition, it is possible to obtain a toner that is excellent in chargeability while imparting excellent fluidity to the toner. As a result, it is possible to obtain a toner that is excellent in transferability even after long periods of continuous printing.
[0080] The value of SD1w / SM1w is preferably 0.40 or more, and more preferably 0.50 or more. Also, it is preferably 0.85 or less, and more preferably 0.80 or less. For example, it may be in the range of 0.40 to 0.85 or 0.50 to 0.80.
[0081] The value of SD1w / SM1w can be controlled by the ratio of inorganic fine particles A exhibiting SD1w to inorganic fine particles B exhibiting SM1w. For example, the value can be reduced by reducing the amount of inorganic fine particles A exhibiting SD1w. The value can be increased by reducing the amount of inorganic fine particles B exhibiting SM1w.
[0082] The value of SM1w is not particularly limited, but is preferably 6.0 to 12.0, and more preferably 7.0 to 11.0. When the value of SM1w is within the above range, silicone oil is appropriately liberated, which facilitates improvement of transferability.
[0083] The inorganic fine particles have free components on the surface thereof, and the free components contain silicone oil. The amount of free carbon in the inorganic fine particles is preferably 2.0 to 8.0% by mass.
[0084] As described above, free components such as free silicone oil are present on the surface of inorganic fine particles. The carbon content of the free components in the inorganic fine particles being within the above range indicates that the surface of the inorganic fine particles is appropriately treated with silicone oil. When the carbon content of the free components is 2.0 mass% or more, it is easier to suppress component contamination. Also, when the carbon content of the free components is 8.0 mass% or less, it is easier to improve transferability. In other words, by setting the carbon content of the free components within the above range, it is possible to achieve both improved transferability and suppression of component contamination caused by the free components.
[0085] The carbon content of the free component is more preferably 3.0% by mass or more, and even more preferably 4.0% by mass or more. Also, it is more preferably 7.0% by mass or less, and even more preferably 6.0% by mass or less. For example, it may be in the range of 3.0 to 7.0% by mass, or 4.0 to 6.0% by mass.
[0086] The carbon content of the free component can be controlled, for example, by changing the amount of silicone oil added. For example, the carbon content of the free component can be reduced by reducing the amount of silicone oil added. Also, the carbon content of the free component can be increased by increasing the amount of silicone oil added.
[0087] When the carbon content by mass of the inorganic fine particles before washing with hexane is C1 and the carbon content by mass of the inorganic fine particles after washing with hexane is C2, it is preferable that C1 and C2 satisfy the following. 0.20≦C2 / C1≦0.60
[0088] The value of C2 / C1 indicates the carbon reduction rate after washing when inorganic fine particles are washed with hexane. That is, the carbon reduction rate of inorganic fine particles when washed with hexane is preferably 20 to 60 mass%. The components removed when inorganic fine particles are washed with hexane are mainly surface treatment agents such as silicone oil. Examples of the surface treatment agent include silicone oils such as dimethyl silicone oil; silicone oils in which the side chain or end of dimethyl silicone oil is modified with an organic group, such as methyl hydrogen silicone oil, methyl phenyl silicone oil, alkyl modified silicone oil, chloro alkyl modified silicone oil, chloro phenyl modified silicone oil, fatty acid modified silicone oil, polyether modified silicone oil, alkoxy modified silicone oil, carbinol modified silicone oil, amino modified silicone oil, and fluorine modified silicone oil.
[0089] C2 / C1 being 0.20 or more and 0.60 or less indicates that the surface treatment agent such as silicone oil is sufficiently fixed to the surface of the inorganic fine particles. By controlling the carbon reduction rate when washing with hexane within the above range, the release effect of silicone oil can be sufficiently obtained. As a result, the effect of preventing transfer voids and image defects can be obtained while suppressing contamination of the charging member. When it is within this range, it is possible to achieve a high degree of both improvement in transferability and member contamination. In addition, it is possible to obtain a toner that is excellent in chargeability while imparting excellent fluidity to the toner.
[0090] The value of C2 / C1 is more preferably 0.25 or more, and even more preferably 0.30 or more. Also, it is more preferably 0.55 or less, and even more preferably 0.50 or less. For example, it is preferably in the range of 0.25 to 0.55, or 0.30 to 0.50.
[0091] By setting the treatment temperature for treating inorganic particles with silicone oil at 300 to 380°C, the carbon reduction rate when washed with hexane can be controlled. For example, the value of C2 / C1 can be reduced by low-temperature treatment. Also, the value of C2 / C1 can be increased by high-temperature treatment.
[0092] The content of silicone oil in the inorganic fine particles is preferably 4.5 to 8.2% by mass. When the content of silicone oil is within the above range, it is possible to more highly achieve both excellent transferability and suppression of member contamination.
[0093] The content of silicone oil in the inorganic fine particles is preferably 5.0% by mass or more, more preferably 6.0% by mass or more, more preferably 8.0% by mass or less, even more preferably 7.5% by mass or less, for example, in the range of 5.0 to 8.0% by mass, or 6.0 to 7.5% by mass.
[0094] The BET specific surface area of inorganic particles is 60 to 160 m 2 / g. The larger the BET specific surface area of the inorganic fine particles, the smaller the number average particle diameter of the inorganic fine particles. Also, the smaller the BET specific surface area of the inorganic fine particles, the larger the number average particle diameter of the inorganic fine particles. When the BET specific surface area of the inorganic fine particles is 60 to 160 m 2 / g or less, it is possible to achieve both improved transferability and reduced component contamination. In addition, it is possible to obtain a toner having excellent chargeability while imparting excellent fluidity to the toner.
[0095] The BET specific surface area of inorganic particles is 70m 2 / g or more is more preferable, and 80m 2 / g or more is more preferable. 2 / g or less is more preferable, and 2 For example, the range is 70 to 140 m / g or less. 2 / g, 80-130m 2 / g range.
[0096] The inorganic fine particles may contain inorganic fine particles other than the inorganic fine particles A and B. Examples of inorganic fine particles other than the inorganic fine particles A and B include metal oxides (silica, titanium oxide, aluminum oxide), etc. The amount of inorganic fine particles A and B added per 100 parts by mass of toner particles is preferably 0.3 to 3.0 parts by mass. The content of inorganic fine particles A and B in the inorganic fine particles is preferably 50% by mass or more, more preferably 75% by mass or more, based on the total mass of the inorganic fine particles.
[0097] The number average particle size of the inorganic fine particles is, for example, preferably from 5 to 100 nm, and more preferably from 10 to 70 nm.
[0098] By treating the surface of the inorganic fine particles with the above-mentioned method, the inorganic fine particles are hydrophobized as the configuration of the present disclosure is formed on the surface of the inorganic fine particles. When the inorganic fine particles are hydrophobized, the amount of water adsorption on the surface of the inorganic fine particles decreases. Therefore, by evaluating the amount of water adsorption on the surface of the inorganic fine particles after surface treatment, it can be used as an index of the extent to which the surface of the inorganic fine particles is covered with the structure having the configuration of the present disclosure.
[0099] The amount of water adsorption of inorganic particles at a temperature of 30.0°C and a relative humidity of 80.0% is 1.5 cm 3 / g or more. 3 / g or less, and 3 / g or less. For example, it is preferably 1.5 to 4.0 cm 3 / g, 1.5-5.0cm 3 / g range.
[0100] <Raw materials for toner particles> Next, the raw materials of the toner particles will be described.
[0101] <Binding resin> The toner particles contain a binder resin. As the binder resin, a general resin used in a toner for electrophotography can be used. Examples of the resin include polyester resin, styrene-acrylic acid copolymer, polyolefin resin, vinyl resin, fluororesin, phenol resin, silicone resin, and epoxy resin. Among these, it is preferable to use amorphous polyester resin from the viewpoint of improving low-temperature fixing property. In addition, from the viewpoint of achieving both low-temperature fixing property and hot offset resistance, low-molecular-weight polyester and high-molecular-weight polyester may be used in combination. In addition, from the viewpoint of further improving low-temperature fixing property and blocking resistance during storage, crystalline polyester may be used as a plasticizer. The content of the binder resin in the toner particles is not particularly limited, but is preferably 50.0 to 95.5% by mass.
[0102] <Magnetic iron oxide particles> The toner particles may contain magnetic iron oxide particles as necessary. That is, the toner particles may be magnetic toner particles containing a magnetic material. As the magnetic iron oxide particles, the following magnetic iron oxide particles can be used.
[0103] Specifically, magnetic iron oxide particles such as magnetite, maghemite, and ferrite, and magnetic iron oxide particles containing other metal oxides are included. Iron oxide (FeO), iron sesquioxide (γ-FeO), zinc iron oxide (ZnFeO), yttrium iron oxide (YFeO) 12 ), Cadmium iron oxide (Cd3Fe2O4), Gadolinium iron oxide (Gd3Fe5O 12 ), copper iron oxide (CuFe2O4), lead iron oxide (PbFe 12 O 19 ), Nickel Iron Oxide (NiFe2O4), Neodymium Iron Oxide (NdFe2O3), Barium Iron Oxide (BaFe 12 O 19 ), magnesium iron oxide (MgFe2O4), manganese iron oxide (MnFe2O4), lanthanum iron oxide (LaFeO3), iron powder (Fe), etc. Particularly suitable magnetic iron oxide particles are fine powders of iron tetroxide or gamma ferric oxide. The above-mentioned magnetic iron oxide particles can be used alone or in combination of two or more kinds. The content of the magnetic iron oxide particles in the toner particles is not particularly limited, but is preferably 50 to 150 parts by mass with respect to 100 parts by mass of the binder resin.
[0104] <Coloring agent> The toner particles may contain a colorant, if necessary. Examples of the colorant that can be contained in the toner particles include known organic pigments or oil-based dyes, carbon black, and magnetic materials.
[0105] Examples of cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Examples of magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Examples of black colorants include carbon black, magnetic materials, and those toned to black using the above-mentioned yellow colorants, magenta colorants, and cyan colorants.
[0106] The colorants can be used alone or in combination of two or more. The content of the colorant in the toner particles is not particularly limited, but is preferably 1 to 20 parts by mass with respect to 100 parts by mass of the binder resin.
[0107] <Release agent> The toner particles may contain a release agent, if necessary, for suppressing the occurrence of hot offset during heat fixing of the toner. The release agent is not particularly limited, and any known release agent may be used.
[0108] Typical examples include low molecular weight polyolefins, silicone wax, fatty acid amides, ester waxes, carnauba wax, hydrocarbon waxes, etc. Aliphatic hydrocarbon waxes such as paraffin wax are preferably used. The content of the release agent in the toner particles is not particularly limited, but is preferably 1 to 20 parts by mass with respect to 100 parts by mass of the binder resin.
[0109] <Charge control agent> The toner particles may contain a charge control agent as necessary. The charge control agent is not particularly limited, but is preferably a metal compound of an aromatic carboxylic acid from the viewpoints of being colorless, having a high charging speed of the toner, and being able to stably maintain a constant charge amount.
[0110] Examples of negative charge control agents include metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate or sulfonate ester on the side chain, polymeric compounds having carboxylate or carboxylate ester on the side chain, boron compounds, urea compounds, silicon compounds, and calixarenes. Examples of positive charge control agents include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, imidazole compounds, etc. Examples of polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group include homopolymers of sulfonic acid group-containing vinyl monomers such as styrene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, 2-methacrylamido-2-methylpropane sulfonic acid, vinyl sulfonic acid, and methacryl sulfonic acid, or copolymers of vinyl monomers and the above-mentioned sulfonic acid group-containing vinyl monomers.
[0111] The charge control agent may be added internally or externally to the toner particles. The content of the charge control agent in the toner particles is preferably 0.2 to 10 parts by mass with respect to 100 parts by mass of the binder resin in the toner particles.
[0112] <Career> In order to obtain stable images over a long period of time, the toner particles may be mixed with a magnetic carrier and used as a toner in a two-component developer. Examples of magnetic carriers include surface-oxidized iron powder, unoxidized iron powder, metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, and rare earth elements; alloy particles of the above metals; oxide particles of the above metals; magnetic materials such as ferrite; and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state.
[0113] <Method of manufacturing toner particles> Next, the procedure for producing the toner particles will be described. The method for producing the toner particles is not particularly limited, and the toner particles can be produced by a known method. For example, a pulverization method, an emulsion aggregation method, a suspension polymerization method, a dissolution suspension method, etc. are included. The toner particles produced by the pulverization method are produced, for example, as follows.
[0114] (Raw material mixing process) In the raw material mixing process, materials constituting the toner particles, such as binder resin, release agent, magnetic iron oxide particles, and, if necessary, colorant, charge control agent, etc., are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include a double cone mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.).
[0115] (Melting and kneading process) Next, the mixed materials are melt-kneaded to disperse the release agent and magnetic iron oxide particles in the binder resin. In the melt-kneading process, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used. Due to the advantage of continuous production, single-screw or twin-screw extruders are mainstream. For example, KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), PCM kneader (manufactured by Ikegai Co., Ltd.), twin-screw extruder (manufactured by KCK Corporation), Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.). The residence time during melt-kneading is preferably adjusted so that the temperature of the kneaded resin is 100 to 200°C. The kneaded product obtained by melt kneading may be rolled using a two-roll mill or cooled with water in a cooling step.
[0116] (Crushing process) The cooled kneaded product is pulverized to a desired particle size in a pulverizing process. In the pulverizing process, the product is coarsely pulverized in a pulverizer, and then finely pulverized in a fine pulverizer. Examples of pulverizers that perform coarse pulverization include a crusher, a hammer mill, and a feather mill. Examples of fine pulverizers that perform fine pulverization include a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), a Super Rotor (manufactured by Nisshin Engineering Inc.), a Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.), and a fine pulverizer using an air jet system.
[0117] Thereafter, if necessary, the toner particles are classified using a classifier or a sieve. Examples of the classifier or sieve include an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), and a Faculty (manufactured by Hosokawa Micron Corporation).
[0118] (External addition process) To the obtained toner particles, inorganic fine particles are externally added. For example, inorganic fine particles are added as an external additive to give the toner fluidity or to make the chargeability appropriate, and mixed (externally added) with the toner particles to obtain a toner. The mixing can be performed by a mixing device having a rotor having an agitating member and a main casing provided with a gap between the agitating member and the main casing.
[0119] Examples of mixing devices include a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), a Super Mixer (manufactured by Kawata Co., Ltd.), a Ribocone (manufactured by Okawara Manufacturing Co., Ltd.), a Nauta mixer, a Turbulizer, a Cyclomix, a Nobilta (manufactured by Hosokawa Micron Co., Ltd.), a Spiral Pin Mixer (manufactured by Pacific Machinery Co., Ltd.), and a Loedige Mixer (manufactured by Matsubo Co., Ltd.). In particular, a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.) is suitable for uniformly mixing the external additive and the toner particles and for breaking up aggregates of the external additive.
[0120] Mixing conditions when adding inorganic fine particles externally include, for example, the processing amount, the stirring shaft rotation speed, the stirring time, etc. For example, the processing amount is preferably 0.3 kg to 3.0 kg using a Henschel mixer SM-10C or the like. The stirring shaft rotation speed is preferably 1000 to 4000 rpm. The stirring time is preferably 0.5 min to 5 min. In cases where coarse aggregates of the external additive are present in a free state in the obtained toner, a sieving machine or the like may be used as necessary.
[0121] The methods for measuring various physical properties of the toner and raw materials are described below. <Method of measuring weight average particle size (D4) of toner particles> The weight-average particle size (D4) of the toner particles was measured using a precision particle size distribution measuring device equipped with a 50 μm aperture tube, the Coulter Counter Multisizer 3 (registered trademark, manufactured by Beckman Coulter, Inc.), which uses the narrow hole electrical resistance method, and the accompanying dedicated software for setting measurement conditions and analyzing measurement data, the Beckman Coulter Multisizer 3 Using "Beckman Coulter, Version 3.51" (manufactured by Beckman Coulter), measurements are taken with an effective number of measurement channels of 25,000, and the measurement data is analyzed and calculated. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0122] Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 1 μm or more and 30 μm or less.
[0123] The specific measurement method is as follows. (1) Pour 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube. (2) 30 ml of the above-mentioned aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by mass with ion-exchanged water is added as a dispersant. (3) A specified amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and 2 ml of the above-mentioned Conaminon N is added to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolyte solution (5) in which the toner is dispersed, into the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight average particle size (D4) is calculated. Note that the analysis / volume statistics (calculated) when the dedicated software is set to graph / volume%. The "average diameter" on the surgical average screen is the weight average particle diameter (D4).
[0124] <Method for measuring number average particle size of inorganic fine particles> The number-average particle size of inorganic fine particles is calculated from images of inorganic fine particles separated from toner (mixture with pigment if the toner contains pigment) taken with a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). The image taking conditions for the S-4800 are as follows: (1) Sample preparation Apply a thin layer of conductive paste to a sample stage (aluminum sample stage 15 mm x 6 mm), then spray the inorganic particles separated from the toner onto the paste. Then, use air to remove excess inorganic particles from the sample stage and allow to dry thoroughly. Set the sample stage in the sample holder and adjust the sample stage height to 36 mm using the sample height gauge. (2) S-4800 observation condition setting The number average particle size is calculated using the image obtained by backscattered electron image observation with the S-4800. Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 housing until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2 and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the sample holder into the sample chamber of the S-4800 housing. Press [Origin] on the control panel to move the sample holder to the observation position. Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [1.1kV] and the emission current to [20μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], and select [LA100] in the selection box to the right of [+BSE] to set the mode to observation with backscattered electron images. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [4.5mm]. Press the [ON] button in the accelerating voltage display of the control panel to apply the accelerating voltage. (3) Focus adjustment Rotate the focus knob [COARSE] on the operation panel, and adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog, and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture], and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or to minimize its movement. Close the aperture dialog, and adjust the focus using autofocus. After that, set the magnification to 80,000 (80k), and adjust the focus using the focus knob and STIGMA / ALIGNMENT knob in the same way as above, and then adjust the focus using autofocus again. Repeat this operation to adjust the focus. Here, if the inclination angle of the observation surface is large, the measurement accuracy of the number average particle size tends to be low, so when adjusting the focus, select an observation surface that is in focus at the same time and has as little surface inclination as possible for analysis. (4) Image storage Adjust the brightness in ABC mode, take a photo at a size of 640 x 480 pixels, and save it. Use this image file for the following analysis. To measure the particle diameters of at least 500 inorganic microparticles and calculate the number-average particle diameter, take images at multiple locations so as to obtain the required number of particles, without taking images of the same inorganic microparticles. (5) Image analysis Measure the particle size of at least 500 inorganic particles to obtain the number-average particle size. The number-average particle diameter is calculated by binarizing the images obtained by the above-mentioned method using image analysis software Image-Pro Plus ver.5.0. If the inorganic fine particles separated from the toner contain pigments or other contaminants, they are first subjected to elemental analysis using an energy dispersive X-ray analyzer (EDS) and identification based on particle size and shape to eliminate particles other than the inorganic fine particles to be measured before measurement.
[0125] <Method for separating inorganic fine particles from toner> 20 g of a 10% by weight aqueous solution of "Contaminon N" (a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, an anionic surfactant, and an organic builder) is weighed into a 50 mL vial and mixed with 1 g of toner. The mixture is placed in a KM Shaker (model: V.SX) manufactured by Iwaki Sangyo Co., Ltd., and shaken for 30 seconds at a speed of 50. This causes the inorganic fine particles to migrate from the surface of the toner particles to the aqueous solution. In the case of a magnetic toner containing a magnetic material, the silica fine particles that have migrated to the supernatant liquid are then separated while the toner particles are held in place using a neodymium magnet, and the precipitated toner is dried in a vacuum (40°C / 24 hours) to obtain inorganic fine particles. In the case of non-magnetic toner, the toner is separated from the inorganic fine particles that have migrated to the supernatant liquid using a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.) (at 1000 rpm for 5 minutes). In addition, when an external additive other than inorganic fine particles is added to the toner, the inorganic fine particles can be separated from the other external additives by centrifuging the external additives separated from the toner by the above-mentioned method. Even when multiple types of inorganic fine particles are added to the toner, they can be separated by centrifuging as long as they have different particle size ranges. For example, separation can be performed using CS120FNX; manufactured by Hitachi Koki Co., Ltd., under conditions of 40,000 rpm and 20 minutes.
[0126] <Solid 29 Si-NMR measurement method> The inorganic fine particles obtained by the above method were washed with hexane, and the washed inorganic fine particles were used as a sample for NMR measurement. solid 29 The measurement conditions for Si-NMR are as follows: Equipment: JNM-ECA400 (JEOL RESONANCE) Calibration: TMS (tetramethylsilane) 0 ppm Temperature: room temperature Measurement method: DD / MAS method 29 Si 45° Sample tube: Zirconia 8.0mmφ Sample: Test tube filled with silica particles in powder form Sample rotation speed: 6kHz Relaxation delay: 90 seconds Scan:5640
[0127] In the NMR spectrum obtained under the above measurement conditions, the peak corresponding to the siloxane chain, which appears around -20 ppm, was separated to obtain the Si a and the peak PD1w corresponding to a silicon atom represented by the following formula (2): b The peak areas SD1w and SD2w are calculated from the respective peaks. Similarly, the Si c A peak PM1w corresponding to the silicon atom represented by the formula: is obtained, and the peak area SM1w is calculated. [ka] (In the formulas (1) to (3), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate.)
[0128] Peak separation is carried out as follows. (Peak separation method) The NMR spectrum data obtained by the above method is analyzed to perform peak separation. Peak separation may be performed using commercially available software or a program created independently, as long as it is performed according to the procedure described below. The positions of peaks PD1w, PD2w, and PM1w are fixed at −18.2 ppm, −21.0 ppm, and 14.3 ppm, respectively, and peak separation processing is performed using a Voigt function.
[0129] <Method of Specifying Inorganic Fine Particle Substrate> The inorganic particles separated from the toner are subjected to fluorescent X-ray measurement to identify the substrate. The measurement of fluorescent X-rays for each element conforms to JIS K 0119-1969, and specifically, is as follows. The measurement equipment used is a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. A proportional counter (PC) is used to measure light elements, and a scintillation counter (SC) is used to measure heavy elements. The measurement sample was prepared by placing 4 g of inorganic fine particles separated from the toner into a special aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (manufactured by Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of 2 mm and a diameter of 39 mm. Measurements are performed under the above conditions, and the elements are identified based on the positions of the obtained X-ray peaks.
[0130] <Method for measuring silicone oil content in inorganic fine particles> (Method for separating inorganic fine particles from toner) 20 g of a 10% by weight aqueous solution of "Contaminon N" (a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, an anionic surfactant, and an organic builder) is weighed into a 50 mL vial and mixed with 1 g of toner. The mixture is placed in a KM Shaker (model: V.SX) manufactured by Iwaki Sangyo Co., Ltd., and shaken for 30 seconds at a speed of 50. This causes the inorganic fine particles to migrate from the surface of the toner particles to the aqueous solution. In the case of a magnetic toner containing a magnetic material, the silica fine particles that have migrated to the supernatant liquid are then separated while the toner particles are held in place using a neodymium magnet, and the precipitated toner is dried in a vacuum (40°C / 24 hours) to obtain inorganic fine particles. In the case of non-magnetic toner, the toner is separated from the inorganic fine particles that have migrated to the supernatant liquid using a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.) (at 1000 rpm for 5 minutes). (Extraction of desorbed silicone oil) (1) Place 0.5 g of inorganic fine particles A and 40 ml of chloroform in a beaker and stir for 2 hours. (2) Stop stirring and let stand for 12 hours. (3) Filter the sample and wash three times with 40 ml of chloroform. (4) Remove the chloroform by drying under reduced pressure. (Method of measuring silicone oil content) By the above-mentioned method, the free component (silicone oil) is extracted from the inorganic fine particles. As described below, the sample is burned at 1100°C under an oxygen stream, and the amounts of CO and CO2 generated are measured by IR absorbance to measure the amount of carbon in the inorganic fine particles after the free components are extracted. (1) 2 g of inorganic fine particles A are placed in a cylindrical mold as a sample and pressed. (2) 0.15 g of the pressed sample is precisely weighed, placed on a combustion board, and measured using a Horiba EMA-110. The total carbon content in 0.5 g of a sample is measured in advance, and the silicone oil content is calculated from the difference between this total carbon content and the silicone oil content.
[0131] <Method for measuring the amount of free carbon in inorganic fine particles> By the above-mentioned method, the free component (silicone oil) is extracted from the inorganic fine particles. As described below, the sample is burned at 1100°C in an oxygen stream, the amount of CO and CO2 generated is measured by IR absorbance, and the amount of carbon in the free components in the inorganic fine particles is measured. The amount of carbon before and after extraction of the free components is then compared to calculate the amount of carbon in the free components in the inorganic fine particles. (1) 2 g of inorganic fine particles A are placed as a sample in a cylindrical mold and pressed. (2) 0.15 g of the pressed sample is precisely weighed, placed on a combustion board, and measured using a Horiba EMA-110. The amount of free carbon in the inorganic fine particles is calculated as follows. Carbon content of free components (mass%) = (carbon content before extraction of free components - carbon content after extraction of free components) / carbon content before extraction of free components
[0132] <Method for measuring carbon reduction rate when inorganic fine particles are washed with hexane> 1.0 g of inorganic fine particles is weighed into a 50 ml screw tube, and 20 ml of normal hexane is added. Then, the mixture is extracted for 10 minutes with an ultrasonic homogenizer (VP-050 manufactured by TAITEC) at a strength of 20 (output of 10 W). The obtained extract is separated with a centrifuge, and the liquid phase (silicone oil) is separated and collected. The infrared absorption spectrum of the separated and recovered material is obtained and compared with that of a silicone oil prepared as a standard, thereby confirming that the inorganic fine particles have free components on their surfaces and that the free components contain silicone oil. The supernatant is removed, and normal hexane is removed from the resulting wet sample using an evaporator to obtain inorganic fine particles after washing with hexane. The carbon content (C content) of inorganic fine particles before and after hexane washing is measured using a total nitrogen / total carbon measuring device (Sumika Chemical Analysis Center, Sumigraph NC-22F). The carbon content of the inorganic fine particles based on mass before washing with hexane is defined as C1, and the carbon content of the inorganic fine particles based on mass after washing with hexane is defined as C2, and the value of C2 / C1 is calculated.
[0133] <Measurement of BET specific surface area of inorganic fine particles> The BET specific surface area of the inorganic fine particles can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method in accordance with the BET method (BET multipoint method). Using a specific surface area measuring device (product name: Gemini 2375 Ver. 5.0, manufactured by Shimadzu Corporation), nitrogen gas was adsorbed onto the surface of the sample, and the BET specific surface area (m 2 / g) can be calculated by the following procedure. Measured at. After measuring the mass of the empty sample cell, fill the sample cell with the measurement sample so that it becomes 80% of the cell volume. Next, set the sample cell filled with the sample in the degassing device and degas at room temperature for 7 hours. After degassing is completed, measure the mass of the entire sample cell, and calculate the exact mass of the sample from the difference with the empty sample cell. Next, set an empty sample cell in the balance port and analysis port of the BET measurement device. Set a Dewar bottle containing liquid nitrogen in the designated position, and measure the saturated vapor pressure (P0) using the command to measure P0. After measuring P0, set the degassed sample cell in the analysis port, enter the sample mass and P0, and then start the measurement using the BET measurement command. The BET specific surface area will then be calculated automatically.
[0134] <Method for measuring water adsorption amount> The amount of moisture adsorption of inorganic fine particles is measured by an adsorption equilibrium measuring device (BELSORP-aqua3: manufactured by BEL Japan Co., Ltd.). This device measures the amount of adsorption of a target gas (water vapor). The inorganic fine particles obtained by the above-mentioned method were used as a measurement sample for the amount of moisture adsorption.
[0135] (Degassing) Before measurement, degas the moisture adsorbed in the sample. Attach the cell, filler rod, and cap, and weigh the empty sample. Weigh out 0.3 g of sample and place it in the cell. Place the filler rod in the cell, attach the cap, and attach it to the degassing port. Once all the cells to be measured are attached to the degassing port, open the helium valve. Turn on the button for the port to be degassed, and press the "VAC" button. Continue degassing in this manner for at least one day.
[0136] (measurement) Turn on the power to the measurement unit (there is a switch on the back of the unit). At the same time, start the vacuum pump. Turn on the power to the circulating water unit and the operation panel. Launch "BELaqua3.exe" (measurement software) in the center of the PC screen. Temperature control of the high temperature air chamber: Double-click "SV" in the "TIC1" box on the "Flow path diagram" window to open the "Temperature setting" window. Enter the temperature (80°C) and click Set. Control of adsorption temperature: Double-click "SV" of "Adsorption temperature" in the "Flow path diagram" window and input the "SV value" (adsorption temperature). Click "Circulation start" and "External temperature control", and click setting. Press the "PURGE" button to stop degassing, turn off the port button, remove the sample, attach cap 2, weigh the sample, and then attach the sample to the main body measurement section. On the PC, click "Measurement Conditions" to open the "Measurement Conditions Settings" window. The measurement conditions are as follows: Air thermostat temperature: 80.0℃ Adsorption temperature: 30.0℃ Adsorbate name: H2O Equilibrium time: 500sec Temperature waiting time: 60 min Saturated vapor pressure: 4.245kPa Sample tube pumping speed: Normal Chemisorption measurement: No Initial introduction amount: 0.20cm 3 (STP)·g -1 Number of relative pressure measurement ranges: 4 Select the number of samples to be measured, enter the "measurement data file name" and "sample weight." Start the measurement.
[0137] (analysis) The analysis software was started and the amount of water adsorption per unit mass (cm) at a temperature of 30.0°C and a relative humidity of 80.0% was calculated. 3 / g) is calculated. EXAMPLES
[0138] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. In the following examples, unless otherwise specified, the parts are based on parts by weight.
[0139] <Examples of binder resin production> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane: 72.0 parts by mass (0.20 moles; 100.0 mole parts based on the total number of moles of polyhydric alcohol) Terephthalic acid: 28.0 parts by mass (0.17 moles; 100.0 mole parts based on the total number of moles of polycarboxylic acids) · Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts by mass The above materials were weighed into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the reaction was carried out for 8 hours while stirring at a temperature of 220°C. The pressure in the reaction vessel was reduced to 8.3 kPa, and after maintaining this for 1 hour, it was cooled to 180°C and returned to atmospheric pressure. Trimellitic anhydride: 3 parts by mass (0.01 mole; 4.0 mole parts based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts by mass Thereafter, the above materials were added, the pressure in the reaction vessel was reduced to 8.3 kPa, and the reaction was carried out for 1 hour while maintaining the temperature at 180° C., to obtain a binder resin. The softening point of the obtained binder resin, measured according to ASTM D36-86, was 110° C.
[0140] <Production Example of Inorganic Fine Particles A1> BET specific surface area 110m 2 500 parts by mass of fumed silica (inorganic fine particle substrate) having a molecular weight of 1.0 g / g was placed in a reaction vessel and heated with stirring under nitrogen purging. The temperature and pressure inside the reaction vessel were controlled to be 330° C. and 1.0 Pa. Next, octamethylcyclotetrasiloxane was supplied in a vapor state as a surface treatment agent into the reaction vessel at 10 parts by mass / min for 60 minutes, and then heated and stirred at 330°C for 180 minutes to perform surface treatment of the inorganic fine particle substrate. After removing the unreacted surface treatment agent, polydimethylsiloxane (kinetic viscosity at 25°C: 100mm) was added with stirring under nitrogen purging. 2 A solution prepared by diluting 50 parts by mass of hexane with 500 parts by mass of hexane was sprayed and supplied using a sprayer. Thereafter, the mixture was heated and stirred at 330° C. for 120 minutes for surface treatment to obtain inorganic fine particles A1. Table 1 shows the physical properties of inorganic fine particles A1.
[0141] <Production Example of Inorganic Fine Particles A2> BET specific surface area 110m 2 500 parts by mass of strontium titanate microparticles (inorganic microparticle substrate) having a molecular weight of 1 / g were placed in a reaction vessel, which was then heated with stirring under a nitrogen purge, and the temperature inside the reaction vessel was controlled to 330°C. Next, octamethylcyclotetrasiloxane was supplied as a surface treatment agent in a vapor state to the reaction vessel at 10 parts by mass / min for 60 minutes, and then heated and stirred for 180 minutes to perform surface treatment of the strontium titanate substrate. After removing the unreacted surface treatment agent, polydimethylsiloxane (kinetic viscosity at 25°C: 100 mm) was added to the reaction vessel while stirring under nitrogen purging. 2 A solution prepared by diluting 50 parts by mass of hexane with 500 parts by mass of hexane was sprayed and supplied using a sprayer. Thereafter, the mixture was heated and stirred for 120 minutes for surface treatment to obtain inorganic fine particles A2. Table 1 shows the physical properties of inorganic fine particles A2.
[0142] <Production Examples of Inorganic Fine Particles A3 to 23> Inorganic fine particles A3 to 23 were obtained by producing them in the same manner as inorganic fine particles A1, except that the inorganic fine particle base, the surface treatment agent and the treatment conditions were changed as shown in Table 1. Table 1 shows the physical properties of inorganic fine particles A3 to 23.
[0143] In addition, for the inorganic fine particles A1 to A23, the solids after washing with hexane 29 In the Si-NMR DD / MAS measurement, peaks PD1w and PD2w were observed. [Table 1] In Table 1, the substrate is an inorganic fine particle substrate. BET is the BET specific surface area (m 2 The C amount indicates the amount of carbon (% by mass) of free components in the inorganic fine particles A. The oil amount indicates the silicone oil content (% by mass) in the inorganic fine particles A.
[0144] <Production Example of Inorganic Fine Particles B1> BET specific surface area 110m 2 500 parts by mass of fumed silica (inorganic fine particle substrate) having a molecular weight of 1.0 g / g was placed in a reaction vessel, which was then heated with stirring under nitrogen purging. The temperature in the reaction vessel was controlled to 200° C. and the pressure to 1.0 Pa. Next, hexamethyldisilazane was supplied in a vapor state as a surface treatment agent into the reaction vessel at 10 parts by mass / min for 60 minutes, and then heated and stirred at 200°C for 180 minutes to perform surface treatment of the inorganic fine particle substrate. After removing the unreacted surface treatment agent, polydimethylsiloxane (kinetic viscosity at 25°C: 100mm) was added to the reaction vessel while stirring under nitrogen purging. 2 A solution prepared by diluting 50 parts by mass of hexane with 500 parts by mass of hexane was sprayed and supplied using a sprayer. Thereafter, the mixture was heated and stirred at 330° C. for 120 minutes for surface treatment to obtain inorganic fine particles B1. Table 2 shows the physical properties of inorganic fine particles B1.
[0145] <Production Example of Inorganic Fine Particles B2> BET specific surface area 110m 2500 parts by mass of strontium titanate microparticles (inorganic microparticle substrate) having a molecular weight of 1 / g were placed in a reaction vessel, which was then heated with stirring under a nitrogen purge, and the temperature inside the reaction vessel was controlled to 200°C. Next, hexamethyldisilazane was supplied in a vapor state as a surface treatment agent into the reaction vessel at 10 parts by mass / min for 60 minutes, and then heated and stirred at 200°C for 180 minutes to perform surface treatment of the strontium titanate microparticle substrate. After removing the unreacted surface treatment agent, polydimethylsiloxane (kinetic viscosity at 25°C: 100mm) was added while stirring under nitrogen purging. 2 A solution prepared by diluting 50 parts by mass of hexane with 500 parts by mass of hexane was sprayed and supplied using a sprayer. Thereafter, the mixture was heated and stirred at 200° C. for 120 minutes for surface treatment to obtain inorganic fine particles B2. Table 2 shows the physical properties of inorganic fine particles B2.
[0146] <Production Examples of Inorganic Fine Particles B3 to B24> Inorganic fine particles B3 to 24 were obtained by producing them in the same manner as inorganic fine particles B1, except that the inorganic fine particle base, the surface treatment agent and the treatment conditions were changed as shown in Table 2. Table 2 shows the physical properties of inorganic fine particles B3 to 24.
[0147] In addition, for inorganic fine particles B1 to B24, the solid after washing with hexane 29 In the Si-NMR DD / MAS measurement, the peak PM1w was observed. [Table 2] In Table 2, the substrate is an inorganic fine particle substrate. BET is the BET specific surface area (m 2 The C amount indicates the amount of carbon (% by mass) of free components in inorganic fine particles B. The oil amount indicates the silicone oil content (% by mass) in inorganic fine particles B.
[0148] <Toner 1 Manufacturing Example> The materials used in producing Toner 1 are shown below. Binder resin 1: 100 parts by weight Paraffin wax (number average molecular weight 500, melting point 75°C): 3 parts by weight Magnetic iron oxide particles 1: 95 parts by weight First, the above materials were premixed in a Henschel mixer, and then melt-kneaded using a twin-screw kneading extruder. At this time, the residence time was adjusted so that the temperature of the kneaded resin was 150°C. The obtained kneaded material was cooled, coarsely pulverized using a hammer mill, and then pulverized using a turbo mill. The obtained fine particles were classified using a multi-division classifier (product name: Elbow Jet Classifier, manufactured by Nittetsu Mining Co., Ltd.) that utilizes the Coanda effect, and toner particles with a weight average particle size (D4) of 7.3 μm were obtained.
[0149] The following was added to 100 parts by mass of the obtained toner particles. ·Inorganic fine particles A1: 0.95 parts by mass ·Inorganic fine particles B1: 0.35 parts by mass Strontium titanate (number average particle size: 1.6 μm): 3.0 parts by weight The above materials were mixed in a Henschel mixer 10C, and inorganic fine particles were externally added to the toner particles. The mixing conditions during external addition were processing amount: 1 kg, stirring shaft rotation speed: 3000 rpm, and stirring time: 3 min. The mixture was then sieved through a mesh with 150 μm openings to obtain Toner 1. The physical properties of the obtained Toner 1 are shown in Table 3. [Table 3] In Table 3, BET is the BET specific surface area (m 2 The carbon content (mass%) of free components in the inorganic fine particles is shown. The oil content (mass%) of silicone oil in the inorganic fine particles is shown.
[0150] <Example 1> The evaluation was carried out using a digital copier manufactured by Canon Inc. (product name: imageRUNNER2202N).
[0151] <Evaluation of transfer defect rate (transferability)> The development contrast of the copier was adjusted in a H / H environment (temperature 30°C, humidity 80%). The reflection density of the image output as a FFH image was measured with an optical densitometer, and the reflection density was set to 1.50. The evaluation paper was CS-068 (A4 paper, basis weight 68.0 g / m 2 Using the above settings, an image pattern with a black monochrome image ratio of 1% to the paper surface was printed 50,000 times in succession, and then a 500μm horizontal line pattern (with lines 500μm wide printed) was printed on one sheet. The printed thin lines were enlarged with a digital microscope (digital microscope RX-100, manufactured by Hirox) to examine the image. After the image was acquired, it was subjected to binarization. In the obtained binarized image, the ratio of the area where hollows occurred within the line width to the area of the entire line width was calculated as the hollow loss rate. The area where hollows occurred within the line width where the white background was visible was defined as the area where hollows occurred. For example, a hollow loss rate of 50% means that 50% of the white background was visible within the line width. The transfer hollow loss rate was evaluated from the obtained hollow loss rate according to the following criteria. A: Missing rate is less than 1% B: Missing rate is 1% or more and less than 5% C: Missing rate 5% or more but less than 10% D: Missing rate 10% to less than 20% E: Missing rate 20% or more
[0152] <Evaluation of image uniformity (material contamination)> The development contrast of the copier was adjusted in a N / L environment (temperature 23°C, humidity 5%). The reflection density of the image output as a FFH image was measured with an optical densitometer, and the reflection density was set to 1.50. The evaluation paper was CS-068 (A4 paper, basis weight 68.0 g / m 2 (Sold by Canon Marketing Japan Inc.) was used. With the above settings, an image pattern with a black monochrome image ratio of 40% to the paper surface was output continuously 100,000 sheets, and then three halftone images with a density of 96H (hexadecimal) were output over the entire surface of A3 paper, and the third image was used for evaluation. Image uniformity was evaluated by measuring image density at five locations and calculating the difference between the maximum and minimum values. A small difference between the maximum and minimum image density values indicates excellent image uniformity. Since image uniformity decreases when contamination of components such as the charging roller occurs, the degree of component contamination was evaluated by evaluating image uniformity. Image density was measured using a spectrodensitometer 500 series (X-Rite Corporation) and evaluated according to the following criteria. A: Concentration difference is less than 0.03 B: Density difference is 0.03 or more and less than 0.06 C: Density difference is 0.06 or more and less than 0.09 D: Density difference is 0.09 or more and less than 0.12 E: Density difference is 0.12 or more
[0153] <Toner 2-30 Manufacturing Example> Toners 2 to 30 were produced in the same manner as Toner 1, except that the types, amounts added, and treatment conditions of inorganic fine particles A and inorganic fine particles B were changed as shown in Table 3. The physical properties of Toners 2 to 30 are shown in Table 3.
[0154] <Examples 2 to 23 and Comparative Examples 1 to 7> The evaluation was carried out in the same manner as in Example 1, except that the toner was changed as shown in Table 4. The evaluation results are shown in Table 4. [Table 4]
[0155] In Comparative Example 1, the ratio of inorganic fine particles A present on the toner particle surface is low. Since the liberation of silicone oil is suppressed, the image uniformity, which indicates the degree of member contamination, is maintained at an excellent level, but the transfer void, which indicates the transferability, is inferior to that of the Examples. In Comparative Example 2, the ratio of inorganic fine particles B present on the toner particle surface is low. Since the release of silicone oil is not sufficiently suppressed, the transfer void property, which indicates the transferability, is maintained at an excellent level, but the image uniformity, which indicates the degree of member contamination, is inferior to that of the Examples.
[0156] In Comparative Example 3, the value of (SD1w+SD2w) / SD1w is outside the lower limit. A low value of this value indicates that the surface treatment is insufficient, and the silicone oil is less likely to be liberated. Since the liberation of silicone oil is suppressed, the image uniformity, which indicates the degree of member contamination, is excellent. Although the results are on the same level as in the examples, the transfer voids, which indicate the transferability, are inferior to those in the examples. In Comparative Example 4, the value of (SD1w+SD2w) / SD1w is outside the upper limit. This low value indicates that the surface treatment is insufficient, and silicone oil is easily released. Since the release of silicone oil is not sufficiently suppressed, the transfer void property, which indicates the transferability, is maintained at an excellent level, but the image uniformity, which indicates the degree of member contamination, is inferior to that of the Examples.
[0157] In Comparative Example 5, inorganic fine particles A are not added to the toner particles. Since the release of silicone oil is further suppressed, the image uniformity, which indicates the degree of member contamination, is maintained at an excellent level, but the transfer void, which indicates the transferability, is inferior to that of the Examples. In Comparative Example 6, inorganic fine particles B are not added to the toner particles. Since the release of silicone oil is not sufficiently suppressed, the transfer void property, which indicates the transferability, is maintained at an excellent level, but the image uniformity, which indicates the degree of member contamination, is inferior to that of the Examples. In Comparative Example 7, silicone oil is not added to the inorganic fine particles A and the inorganic fine particles B. Since the inorganic fine particles do not contain silicone oil, the transferability is further inferior to that of the Examples.
[0158] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles and inorganic fine particles, the inorganic fine particles have inorganic fine particles A and inorganic fine particles B different from the inorganic fine particles A, the inorganic fine particles A and the inorganic fine particles B contain silicone oil, The inorganic fine particles were washed with hexane and then used as a sample. 29In Si-NMR DD / MAS measurement, The inorganic fine particles A have a structure represented by the following formula (1): a and the peak PD1w corresponding to a silicon atom represented by the following formula (2): b and a peak PD2w corresponding to a silicon atom represented by The inorganic fine particles B have a structure represented by the following formula (3): c The peak PM1w corresponds to a silicon atom represented by When the area of the peak PD1w is SD1w and the area of the peak PD2w is SD2w, the SD1w and the SD2w satisfy the following: 1.2≦(SD1w+SD2w) / SD1w≦3.8 When the area of the peak PM1w is SM1w, the SD1w and the SM1w satisfy the following: 0.20≦SD1w / SM1w≦0.90 A toner characterized by: [ka] (In the formulas (1) to (3), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate.) (Configuration 2) The toner according to configuration 1, wherein the inorganic fine particles A and the inorganic fine particles B are silica fine particles. (Configuration 3) the inorganic fine particles have free components on the surface thereof, The free component contains the silicone oil, 3. The toner according to configuration 1 or 2, wherein the amount of carbon in the free component in the inorganic fine particles is 2.0 to 8.0% by mass. (Configuration 4) When the carbon content of the inorganic fine particles before washing with hexane is C1 and the carbon content of the inorganic fine particles after washing with hexane is C2, The toner according to any one of Configurations 1 to 3, wherein C1 and C2 satisfy the following: 0.20≦C2 / C1≦0.60 (Configuration 5) 5. The toner according to any one of configurations 1 to 4, wherein the content of the silicone oil in the inorganic fine particles is 4.5 to 8.2% by mass. (Configuration 6) The BET specific surface area of the inorganic fine particles is 60 to 160 m 2 / g. (Configuration 7) the inorganic fine particles A are surface-treated with a surface treatment agent, The toner according to any one of Configurations 1 to 6, wherein the inorganic fine particles B are surface-treated with a surface treatment agent different from the surface treatment agent used for the inorganic fine particles A. (Configuration 8) The toner according to any one of Configurations 1 to 7, wherein the inorganic fine particles A are surface-treated with a cyclic siloxane and the silicone oil. (Configuration 9) The toner according to any one of configurations 1 to 8, wherein the inorganic fine particles B have been surface-treated with silazane and the silicone oil. (Configuration 10) 10. The toner according to any one of configurations 1 to 9, wherein the silicone oil is polydimethylsiloxane. (Configuration 11) 9. The toner according to embodiment 8, wherein the cyclic siloxane is octamethylcyclotetrasiloxane. (Configuration 12) 10. The toner of embodiment 9, wherein the silazane is hexamethyldisilazane.
Claims
1. A toner having toner particles and inorganic fine particles, the inorganic fine particles have inorganic fine particles A and inorganic fine particles B different from the inorganic fine particles A, the inorganic fine particles A and the inorganic fine particles B contain silicone oil, The inorganic fine particles were washed with hexane and then used as a sample. 29 In the Si-NMR DD / MAS measurement, The inorganic fine particles A are Si in a structure represented by the following formula (1): a and a peak PD1w corresponding to a silicon atom represented by the following formula (2): b and a peak PD2w corresponding to a silicon atom represented by The inorganic fine particles B are Si in a structure represented by the following formula (3): c having a peak PM1w corresponding to a silicon atom represented by When the area of the peak PD1w is SD1w and the area of the peak PD2w is SD2w, the SD1w and the SD2w satisfy the following: 1.2≦(SD1w+SD2w) / SD1w≦3.8 When the area of the peak PM1w is SM1w, the SD1w and the SM1w satisfy the following: 0.20≦SD1w / SM1w≦0.90 A toner characterized by: 【Chemistry 1】 (In formulas (1) to (3), R each independently represents a hydrogen atom, a methyl group, or an ethyl group, and X represents an atom of the inorganic fine particle substrate.)
2. The toner according to claim 1 , wherein the inorganic fine particles A and the inorganic fine particles B are silica fine particles.
3. the inorganic fine particles have free components on the surface thereof, The free component contains the silicone oil, 3. The toner according to claim 1, wherein the amount of carbon in the free component in the inorganic fine particles is 2.0 to 8.0% by mass.
4. The carbon content of the inorganic fine particles before washing with hexane is defined as C1, and the carbon content of the inorganic fine particles after washing with hexane is defined as C2. When the carbon content based on the latter mass is C2, The toner according to claim 1 or 2, wherein C1 and C2 satisfy the following: 0.20≦C2 / C1≦0.60
5. 3. The toner according to claim 1, wherein the content of the silicone oil in the inorganic fine particles is 4.5 to 8.2% by mass.
6. The BET specific surface area of the inorganic fine particles is 60 to 160 m 2 The toner according to claim 1 or 2, wherein the toner has a molecular weight of 1 / g.
7. the inorganic fine particles A are surface-treated with a surface treatment agent, 3. The toner according to claim 1, wherein the inorganic fine particles B are surface-treated with a surface treatment agent different from the surface treatment agent used for the inorganic fine particles A.
8. 3. The toner according to claim 1, wherein the inorganic fine particles A are surface-treated with a cyclic siloxane and the silicone oil.
9. 3. The toner according to claim 1, wherein the inorganic fine particles B are surface-treated with silazane and the silicone oil.
10. 3. The toner according to claim 1, wherein the silicone oil is polydimethylsiloxane.
11. The toner of claim 8, wherein said cyclic siloxane is octamethylcyclotetrasiloxane.
12. 10. The toner of claim 9, wherein said silazane is hexamethyldisilazane.
Citation Information
Patent Citations
Toner for developing electrostatic charge image, image forming method and process cartridge
JP1997204065A
Toner and image forming method
JP2004126251A