Ferrite particle, electrophotographic developer carrier core material, electrophotographic developer carrier, and electrophotographic developer
Ferrite particles with a perovskite crystal phase and controlled composition stabilize charging characteristics across varying humidity levels, addressing environmental instability and image defects in electrophotographic developers.
Patent Information
- Application Number
- JP2023058233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional ferrite particles used as carrier core materials for electrophotographic developers exhibit insufficient charging ability and environmental stability due to the presence of unavoidable impurities like Cl, which ionize in varying humidity conditions, leading to image defects such as fogging and density issues.
Ferrite particles with a perovskite crystal phase component, controlled Zr and R content, and a specific moisture and chlorine content, along with a resin coating layer, to stabilize charging characteristics across different humidity levels.
The solution provides ferrite particles with enhanced environmental stability, maintaining consistent charging ability in high-temperature, high-humidity and low-temperature, low-humidity environments, reducing image defects and ensuring high-quality electrophotographic printing.
Smart Images

Figure 2024145749000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer. [Background technology]
[0002] The electrophotographic development method is a method of developing an electrostatic latent image formed on a photoreceptor by attaching the toner in the developer to the electrostatic latent image formed on the photoreceptor. The developer used in this method is divided into two-component developers consisting of toner and carrier, and one-component developers using only toner. As a development method using two-component developers, the cascade method was used in the past, but currently the magnetic brush method using a magnet roll is the mainstream.
[0003] In the magnetic brush method, the carrier and toner are stirred and mixed in a developing box filled with developer, giving the toner an electric charge. The carrier is then transported to the surface of the photoconductor by a developing roll that holds a magnet. At that time, the carrier transports the charged toner to the surface of the photoconductor. After a toner image is formed on the photoconductor by electrostatic action, the carrier remaining on the developing roll is collected back into the developing box, stirred and mixed with new toner, and reused for a certain period of time.
[0004] Unlike one-component developers, two-component developers have good controllability when designing developers because the magnetic and electrical properties of the carrier itself can be designed separately from the toner. Therefore, two-component developers are suitable for full-color developing devices that require high image quality and high-speed printing devices that require reliability and durability in maintaining images.
[0005] In recent years, the particle size of toner has been reduced in order to develop electrostatic latent images with high resolution. Along with the reduction in the particle size of toner, the particle size of carrier has also been reduced from the viewpoint of imparting charge to the toner. If the charging ability of the carrier is insufficient, fog due to low charge toner and memory images are likely to occur due to a decrease in the amount of toner transported to the development area.
[0006] For these reasons, various studies have been conducted on carriers with high charging ability. For example, Patent Document 1 and Patent Document 2 claim that a carrier with high charging ability to toner and high environmental stability can be obtained by adding Ti or Sr and using ferrite particles with appropriately controlled surface irregularities as a carrier core material. In addition, the present applicants have proposed a carrier with better charging ability and environmental stability than conventional carriers by obtaining ferrite particles containing a perovskite crystal phase having the composition formula RZrO3 (wherein R is an alkaline earth metal such as Sr) (see, for example, Patent Document 3, etc.). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-106262 A [Patent Document 2] Patent No. 5886336 [Patent Document 3] International Publication No. 2022 / 045097 Summary of the Invention [Problem to be solved by the invention]
[0008] However, carriers using the above-mentioned conventional ferrite particles (Patent Documents 1 and 2) as carrier core materials have insufficient charging ability and environmental stability. In general, unavoidable impurities such as Cl resulting from Fe raw materials and the like are present on the surface of ferrite particles. These unavoidable impurities are easily ionized by moisture in the atmosphere. Therefore, when such unavoidable impurities are present in large amounts on the surface of ferrite particles, the charge amount decreases as the resistance value decreases in a high-temperature and high-humidity environment, making image defects such as fogging more likely to occur.
[0009] On the other hand, the ferrite particles containing the perovskite crystal phase (Patent Document 3) can suppress the amount of moisture adsorbed on the surface of the ferrite particles to be low, and therefore can effectively suppress the decrease in resistance value in a high-temperature, high-humidity environment. However, since the amount of moisture adsorbed on the surface of the ferrite particles is low, there are cases where a lack of image density occurs due to charge-up in a low-temperature, low-humidity environment.
[0010] Therefore, an object of the present invention is to provide ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer, which are more environmentally stable. [Means for solving the problem]
[0011] In order to solve the above problems, the ferrite particles according to the present invention are ferrite particles containing a crystalline phase component made of a perovskite-type crystal represented by a composition formula of RZrO3 (wherein R is an alkaline earth metal), and the Zr content (P Zr ) is 0.35 mol% or more and 1.00 mol% or less, and the R content in the ferrite particles (P R ) is 0.50 mol% or more and 1.30 mol% or less, and the R content (P Zr ) and the Zr content (P R ) and the ratio (P R / P Zr ) is 1.10 or more and 2.60 or less, and the water content measured by Karl Fischer titration is 30 ppm or more and 70 ppm or less.
[0012] In the ferrite particles according to the present invention, it is preferable that the R is at least one element selected from the group consisting of Sr, Ca and Ba, and the Ca content is less than 0.1 mol %.
[0013] In the ferrite particles according to the present invention, when a phase composition analysis of the crystal phase constituting the ferrite particles is performed by Rietveld analysis of an X-ray diffraction pattern, the ferrite particles preferably contain 0.05 mass % or more and 1.00 mass % or less of a crystal phase component consisting of the perovskite type crystal.
[0014] In the ferrite particles according to the present invention, the amount of chlorine dissolved therefrom as measured by a dissolution method is preferably 35 ppm or more and 100 ppm or less.
[0015] In the ferrite particles according to the present invention, after exposure for 12 hours in a low temperature, low humidity environment (10°C, relative humidity 20%), the charge amount (μC / g) after 30 minutes of stirring is taken as the 30 min value, and the charge amount (μC / g) after 60 minutes of stirring is taken as the 60 min value, and when the time-dependent variation ratio of the 60 min value to the 30 min value is expressed by the following formula, it is preferable that the time-dependent variation ratio is 5% or more and 10% or less. Time-dependent change ratio (%) = (60 min value - 30 min value) / 30 min value x 100
[0016] In order to solve the above problems, the carrier core material for an electrophotographic developer according to the present invention is characterized by containing the above ferrite particles.
[0017] In order to solve the above problems, the carrier for electrophotographic developer according to the present invention is characterized by comprising the above ferrite particles and a resin coating layer provided on the surface of the ferrite particles.
[0018] In order to solve the above problems, the electrophotographic developer according to the present invention is characterized by including a carrier for electrophotographic developer and a toner.
[0019] The electrophotographic developer according to the present invention may be used as a refill developer. Effect of the Invention
[0020] According to the present invention, it is possible to provide ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer, which are more environmentally stable. [Brief description of the drawings]
[0021] [Figure 1]FIG. 2 is a diagram showing a cross section of a ferrite particle, illustrating a method for determining the degree of dispersion of Zr in the ferrite particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the embodiments of the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer according to the present invention will be described. In this specification, the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer mean an aggregate of individual particles, that is, powder, unless otherwise specified. First, the embodiments of the ferrite particles will be described. In addition, hereinafter, the ferrite particles according to the present invention will be described as being mainly used as a carrier core material for electrophotographic developer. However, the ferrite particles according to the present invention can be used for various applications such as magnetic ink, magnetic fluid, magnetic filler, various functional fillers such as fillers for bond magnets and fillers for electromagnetic wave shielding materials, electronic component materials, etc., and the application of the ferrite particles is not limited to the carrier core material for electrophotographic developer.
[0023] 1. Ferrite particles and carrier core material for electrophotographic developers First, an embodiment of the ferrite particles according to the present invention will be described. The ferrite particles according to the present invention contain a crystalline phase component (hereinafter referred to as "perovskite crystalline phase component") made of perovskite crystals represented by the composition formula RZrO3 (wherein R is an alkaline earth metal), and the R content and Zr content in the ferrite particles are within a predetermined range, and by making the R content larger than the Zr content by a predetermined range and making the moisture content within a predetermined range, it is possible to suppress environmental fluctuations in the charging characteristics while effectively suppressing fluctuations over time in the charging characteristics in a high-temperature and high-humidity environment and in a low-temperature and low-humidity environment, and the present invention has been conceived.
[0024] 1-1.R (alkaline earth metals) In the present invention, R refers to at least one element selected from the group consisting of Ca, Sr, Ba, and Ra, that is, alkaline earth metal. The alkaline earth metal has an ionic radius sufficiently larger than that of zirconium, and is expressed by the composition formula RZrO3, forming a zirconate perovskite compound having a perovskite crystal structure. In the present invention, R is more preferably at least one element selected from the group consisting of Sr, Ca, and Ba. In this case, it is also preferable that the Ca content and / or Ba content is less than 0.1 mol%. These elements react with zirconium in a solid phase under a predetermined temperature condition to form the zirconate perovskite compound. Therefore, by controlling the firing temperature within a predetermined temperature range in the manufacturing process of the ferrite particles, ferrite particles containing a perovskite crystal phase component can be obtained. In particular, by using Sr as the main R component, the firing temperature is not too high compared to Ca or Ba, and the amount of energy required for the heat treatment step when generating the perovskite crystal phase component can be reduced. In addition, it is preferable to use Sr as the main R component because it makes it easy to generate a predetermined amount of chloride by the method described below in order to adjust the moisture content within a predetermined range.
[0025] 1-2. Perovskite-type crystal phase components In the present invention, the perovskite crystal phase component is represented by the composition formula RZrO3, and has a crystal structure of a perovskite cubic system. In addition, in the present invention, "containing a perovskite crystal phase component" means that the perovskite crystal phase component is contained inside the ferrite particles. The inventors of the present invention speculate that the reason why the inclusion of a perovskite crystal phase component results in ferrite particles with high magnetization, excellent charging ability, and high environmental stability is as follows.
[0026] In recent years, multi-element ferrites are often used as the core material of electrophotographic developer carriers, rather than single-element ferrites. This is because multi-element ferrites can more easily achieve magnetic and charging properties suitable for the core material of electrophotographic developer carriers. Multi-element ferrites refer to ferrites that contain metal elements such as Mg, Mn, Sr, and Ca in addition to Fe.
[0027] When manufacturing ferrite, metal oxides, metal hydroxides, etc. containing metal elements of the desired composition are used as raw materials. To obtain highly magnetized ferrite particles, it is necessary to sufficiently advance the ferritization reaction of the raw materials so that unreacted raw materials that do not exhibit magnetism (hereinafter referred to as "unreacted raw materials") do not remain in the ferrite particles. However, the ferrite reaction only proceeds at the contact surface between the raw materials. In the case of multi-element ferrite, the ferrite formation temperature and formation speed differ depending on the combination of elements, so it is difficult to completely ferrite the raw materials under general sintering conditions. Therefore, unreacted raw materials remain in the ferrite particles.
[0028] In addition, the raw materials for ferrite contain metals or metal compounds such as Cl that are not involved in the ferrite reaction as unavoidable impurities. These unavoidable impurities do not exhibit magnetism. Therefore, in order to obtain ferrite particles with high magnetization, it is necessary to reduce the amount of unavoidable impurities. However, no matter how pure the raw materials used are, there are traces of unavoidable impurities in the raw materials, and it is not realistic to completely remove the unavoidable impurities.
[0029] Furthermore, if there is a defect in the organizational structure of the ferrite particles, the magnetization of the ferrite particles will decrease. Structural defects that cause a decrease in magnetization include defects within the ferrite particles (e.g., lattice defects, etc.). In the case of multi-element ferrite, the ferrite reaction is more complex than in single-element ferrite, so structural defects are more likely to occur.
[0030] In terms of charging characteristics, ferrite particles are generally highly resistive because they are made of metal oxides. However, when moisture adheres to the surface, the resistance decreases. In addition, the above-mentioned unavoidable impurities such as Cl are easily ionized in the presence of moisture in the atmosphere. Therefore, when the amount of unavoidable impurities in the ferrite particles increases, the resistance decreases, and the resistance value becomes more likely to vary depending on the atmospheric humidity.
[0031] For these reasons, in order to obtain ferrite particles with high resistance and low environmental dependency of resistance, it is necessary to reduce the amount of unavoidable impurities in the ferrite particles. However, as described above, it is not realistic to completely remove the unavoidable impurities. Note that, since the unreacted raw materials (excluding the unavoidable impurities) are metal oxides, the presence of unreacted raw materials does not cause the resistance of the ferrite particles to decrease.
[0032] In many cases, ferrite particles are polycrystalline, i.e., an aggregate of single crystals. Even if the composition of the ferrite particles is the same, the magnetic and electrical properties of the ferrite particles vary depending on the structural structure of the ferrite particles.
[0033] Therefore, the present inventors focused on the structural structure of ferrite particles and discovered that in order to obtain ferrite with high magnetization and high resistance and with low environmental dependency of resistance, it is important that the ferrite contains a crystalline phase component made of perovskite-type crystals represented by the composition formula RZrO3 (wherein R is an alkaline earth metal).
[0034] At the grain boundaries of ferrite particles, there are components that are not dissolved in ferrite, such as unreacted raw materials and unavoidable impurities. In addition, these components that are pushed out to the grain boundaries as the crystal grains grow are also present on the surface of the ferrite particles. When the crystal grains constituting the ferrite particles are large, the grain boundaries are continuously formed inside the ferrite particles like a flow path connecting one point on the surface of the ferrite particles to another point on the surface. The unavoidable impurities present on the surface and grain boundaries of the ferrite particles are easily ionized. Therefore, if unavoidable impurities such as Cl are continuously distributed at the grain boundaries continuously formed within the ferrite particles, when moisture adheres to the surface of the ferrite particles, the grain boundaries become like a conductive path, and the resistance of the ferrite particles decreases. In addition, in ferrite particles having such a structure, it is considered that the resistance also fluctuates greatly due to changes in the atmospheric humidity. In addition, as described above, it is difficult to completely remove the unreacted raw materials and unavoidable impurities in the ferrite particles.
[0035] On the other hand, the perovskite crystal phase component is not dissolved in other crystal phases having different structures such as spinel ferrite phase, and therefore the perovskite crystal phase component is dispersed in the grain boundaries of the ferrite particles. Therefore, the grain boundary volume of the ferrite particles containing the perovskite crystal phase component is relatively increased compared to the case where the perovskite crystal phase component is not contained. When the amount of inevitable impurities contained in the ferrite particles is the same, if the grain boundary volume of the ferrite particles increases relatively, the distribution density of the inevitable impurities in the grain boundaries is relatively decreased. In addition to the inevitable impurities, the perovskite crystal phase component, which is an insulating material, is present in the grain boundaries. In the ferrite particles according to the present invention, the grain boundaries are distributed in a complex manner within the particles, and the inevitable impurities and insulating materials such as the perovskite crystal phase component are distributed discontinuously within the grain boundaries. Therefore, it is possible to suppress the grain boundaries from functioning as conductive paths. For these reasons, the ferrite particles according to the present invention can reduce the environmental dependency of resistance, i.e., it is believed that the present invention can provide ferrite particles with high environmental stability whose charging characteristics are less likely to vary depending on the atmospheric temperature and humidity.
[0036] Furthermore, in order to obtain ferrite particles containing the perovskite crystal phase component, a compound containing Zr (e.g., ZrO2) and a compound containing R must be reacted in a solid state in addition to the ferritization reaction of the ferrite raw material. If the multi-element ferrite particles have a composition containing R, a compound containing Zr can be added as a raw material together with other ferrite raw materials, and the content of the unreacted raw materials remaining in the ferrite particles can be reduced by causing a solid state reaction between the raw material containing R and the compound containing Zr among the unreacted raw materials in the ferrite particles. Therefore, the occurrence of structural defects can be prevented, and ferrite particles with relatively good charging characteristics can be obtained.
[0037] 1-3.Content of each component The content of each component in the ferrite particles will be described below. (1) Zirconium (Zr) In the ferrite particles, the zirconium content (Zr content) (P Zr ) is to be 0.35 mol% or more and 1.00 mol% or less. Zr ) can be quantified by ICP elemental analysis, which will be described later. Zr ) indicates the value when the ferrite component is 100mol%. Zr When the Zr content (P Zr ) is more preferably 0.38 mol% or more, and further preferably 0.40 mol% or more. Zr) becomes too large, and the content of the perovskite crystal phase component in the ferrite particles becomes too large. In this case, the magnetization decreases, and it may become difficult to satisfy the magnetic properties required for the carrier core material for electrophotographic developer, which is not preferable. From these viewpoints, the Zr content is more preferably 0.95 mol% or less, even more preferably 0.90 mol% or less, and even more preferably 0.85 mol% or less.
[0038] (2) Alkaline earth metals In the ferrite particles, the content of alkaline earth metal (R) (R content) (P R ) is 0.50 mol% or more and 1.30 mol% or less. R content (P R ) can also be quantified by ICP elemental analysis, which will be described later. Zr ) indicates the value when the ferrite component is taken as 100 mol %. By including an alkaline earth metal (R) within this range, it is possible to realize ferrite particles that include a suitable amount of perovskite type crystal phase components for obtaining the above-mentioned effects. In order to obtain ferrite particles with less environmental fluctuation in charging properties, the R content (P R ) is more preferably 0.55 mol% or more. R ) is more preferably 1.25 mol % or less, even more preferably 1.20 mol % or less, and even more preferably 1.10 mol % or less.
[0039] (3)R content (P R ) and Zr content (P Zr ) and the ratio (P R / P Zr ) Here, the ferrite particles have a Zr content (P Zr ) and R content (P R ) is within the above range, and the R content (P R ) and Zr content (P Zr ) and the ratio (P R / P Zr) is 1.10 or more and 2.60 or less.
[0040] To obtain the above perovskite crystal phase component, 1 mol of ZrO2 is required for 1 mol of R raw material. R / P Zr ) is satisfied, the ferrite particles contain an excess of alkaline earth metal in addition to the alkaline earth metal that constitutes the perovskite crystal phase component. This excess alkaline earth metal is extruded to the grain boundaries and also to the surface of the ferrite particles. R / P Zr ), a cooling step (meaning a cooling step after holding at a predetermined firing temperature) or a firing step (meaning a step of holding at a predetermined firing temperature) and a cooling step are carried out in a predetermined chlorine atmosphere adjusted by the method described below, etc., to bond the alkaline earth metal on the surface of the ferrite particles with chlorine in the atmosphere, thereby producing an appropriate amount of alkaline earth metal chloride on the surface of the ferrite particles. The chloride is easily ionized when it comes into contact with moisture in the atmosphere, and adsorbs moisture to the surface of the ferrite particles. The above ratio (P R / P Zr ) can prevent a decrease in the amount of charge in a high-temperature, high-humidity environment while retaining an appropriate amount of moisture on the surface of the ferrite particles that can suppress charge-up in a low-temperature, low-humidity environment, thereby obtaining ferrite particles with higher environmental stability and less change in the amount of charge over time in each environment.
[0041] (4) Moisture content The ferrite particles have a moisture content of 30 ppm or more and 70 ppm or less as measured by Karl Fischer titration. By setting the moisture content of the ferrite particles within this range, it is possible to suppress the decrease in the charge amount in a high-temperature, high-humidity environment while suppressing charge-up in a low-temperature, low-humidity environment, thereby realizing ferrite particles with extremely high environmental stability. In order to set the moisture content within this range, as described above, the R content (P R ), Zr content (P Zr ) and the above ratio (PR / P Zr ) within the above-mentioned predetermined range, a cooling step, or a sintering step and a cooling step may be performed under a predetermined chlorine atmosphere. In addition, it is preferable that the BET specific surface area of the ferrite particles is within the range described below. The moisture amount is an index showing the amount of moisture chemically or physically adsorbed on the surface of the ferrite particles. The moisture amount varies by adjusting the amount of chemical species that chemically bond with water, such as alkaline earth metal chlorides present on the surface of the ferrite particles. In addition, when the value of the BET specific surface area is changed, the amount of moisture physically adsorbed varies due to the change in the uneven shape of the surface of the ferrite particles. The ferrite particles according to the present invention can obtain ferrite particles with a moisture amount within the above-mentioned specified range by controlling the amount of alkaline earth metal chlorides generated on the surface of the ferrite particles and the uneven shape of the surface to be within the range described below in the manufacturing process.
[0042] (5) Perovskite-type crystal phase component content By performing a phase composition analysis of the crystal phase constituting the ferrite particles by Rietveld analysis of the X-ray diffraction pattern, the presence or absence of the perovskite crystal phase component in the ferrite particles can be confirmed. In the present invention, the content ratio of the perovskite crystal phase component is not particularly limited, but in order to suppress the environmental variation of the charging characteristics, it is preferably 0.05 mass% or more, more preferably 0.07 mass% or more, even more preferably 0.08 mass% or more, even more preferably 0.10 mass% or more, even more preferably 0.20 mass% or more, and even more preferably 0.30 mass% or more. In addition, the upper limit value is not particularly limited, but in order to obtain ferrite particles that satisfy the magnetic properties required for the carrier core material of an electrophotographic developer and can suppress charge-up even in a low-temperature, low-humidity environment, the content of the perovskite crystal phase component is preferably 1.00 mass% or less, more preferably 0.99 mass% or less, even more preferably 0.95 mass% or less, still more preferably 0.90 mass% or less, even more preferably 0.85 mass% or less, and even more preferably 0.75 mass% or less.
[0043] If the content ratio of the perovskite type crystal phase component is within the above-mentioned preferred range, it becomes easy to uniformly disperse the perovskite type crystal phase component inside the ferrite particle, and it becomes easy to suppress the occurrence of structural defects and to reduce the environmental variation of the resistance value. In addition, when the content ratio of the perovskite type crystal phase component is within the above-mentioned range, the Zr content (P Zr ), R content (P R ) and the above ratio (P R / P Zr ) are within the above-mentioned ranges, it becomes easier to obtain ferrite particles having even higher environmental stability.
[0044] 1-4.Composition The alkaline earth metal reacts with iron in a solid state to form ferrite having a magnetoplumbite crystal structure or a precursor thereof. When the alkaline earth metal is contained within the above range, the ferrite particles may contain various components having different crystal structures, such as ferrite having a magnetoplumbite crystal structure, as subcomponents, together with zirconium dioxide derived from the zirconium raw material and a zirconate perovskite compound. If the ferrite particles are mainly composed of a spinel crystal phase component, when a subcomponent having a crystal structure different from the spinel crystal structure is present inside the particles, the main component grows in the direction of the particle surface where it is relatively easy to grow, and the unevenness of the particle surface becomes appropriate. In addition, by uniformly containing these subcomponents inside the particles, the unevenness of the particle surface can be controlled to a uniform state. In addition, by adopting the firing conditions described later, the generation of the magnetoplumbite crystal phase component can be suppressed while the perovskite crystal phase component can be favorably generated.
[0045] Therefore, the ferrite particles are preferably spinel type ferrite particles, and particularly preferably spinel type ferrite particles containing Mn. In this case, the ferrite particles preferably contain 90% by mass or more, preferably 93% by mass or more, more preferably 95% by mass or more of the spinel type crystal phase component. That is, the ferrite particles are preferably spinel type ferrite particles consisting of the perovskite type crystal phase component and the spinel type crystal phase component, excluding inevitable impurities or unreacted raw materials. The content of the spinel type crystal phase component can be determined by the ratio of metal elements when the raw materials are mixed. Generally, spinel type ferrite is produced by a solid phase reaction. In the ferritization reaction carried out in the firing process, a solid solution (spinel type crystal phase) begins to be generated at about 850°C, and the ferritization reaction is completed at about 1250°C. By appropriately adjusting the firing temperature, firing time, firing atmosphere, and cooling time in the firing step, the spinel crystal phase can be selectively generated, and the content ratio of the spinel crystal phase in the ferrite particles can be determined.
[0046] Furthermore, it is more preferable that the ferrite particles mainly contain a crystal phase component made of a spinel crystal represented by the composition formula of (MnO)x(MgO)y(Fe2O3)z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, x+y+z=100 (mol%)). By combining the above composition with a conventional ferrite manufacturing method, it is possible to obtain ferrite with a spinel crystal phase component of 50 mass% or more.
[0047] By making the composition contain Mn, the magnetization on the low magnetic field side can be increased. In addition, by making the composition contain Mn, the reoxidation of ferrite during removal from the furnace after the main firing can be prevented. In particular, by making the Mn content 15 mol% or more, the relative increase in the Fe content can be suppressed, and the content ratio of the magnetite component in the ferrite particles can be suppressed from increasing. Therefore, the decrease in magnetization on the low magnetic field side can be suppressed, and the occurrence of carrier adhesion can be suppressed. In addition, since it becomes easy to adjust the resistance value to a good value for electrophotographic printing, the occurrence of image defects such as fog, deterioration of gradation, and whiteout can be suppressed. Furthermore, the toner consumption can be kept at an appropriate level. By making the Mn content 50 mol% or less, the resistance becomes too high, and the occurrence of image defects such as whiteout can be suppressed.
[0048] By using a composition containing Mg, high-resistance ferrite particles can be obtained. Also, by setting the Mg content to 2 mol% or more, the Mn content becomes appropriate with respect to the Fe content, and it becomes easy to adjust the magnetization and resistance of the ferrite particles within a favorable range for electrophotographic printing. Therefore, it is possible to suppress the occurrence of image defects such as fogging, deterioration of gradation, occurrence of streaks, and carrier scattering. Furthermore, when magnesium hydroxide is used as the Mg raw material, if the firing temperature during the production of the ferrite particles is low, hydroxyl groups may remain in the ferrite particles. By setting the Mg content to 35 mol% or less, the amount of residual hydroxyl groups present due to the raw materials can be reduced. Therefore, it is possible to suppress the variation of electrical properties such as the charge amount and resistance of the ferrite particles due to the influence of ambient humidity, and to make the environmental dependence of the electrical properties of the ferrite particles better.
[0049] The ferrite particles are magnetic oxides mainly composed of ferric oxide. Therefore, it is premised that x < z is satisfied. By setting the Fe content to 45 mol% or more and 60 mol% or less, it becomes easy to adjust the magnetization and resistance of the ferrite particles within a favorable range for electrophotographic printing.
[0050] 1 - 5. Elution chlorine amount The ferrite particles according to the present invention preferably have an elution chlorine amount measured by the elution method of 35 ppm or more and 100 ppm or less. The measurement procedure for the elution chlorine amount by the elution method is described in the Examples section. By setting the elution chlorine amount within this range, the amount of moisture on the surface of the ferrite particles can be made appropriate, preventing a decrease in the resistance value in a high-temperature and high-humidity environment, suppressing charge-up in a low-temperature and low-humidity environment, and making the ferrite particles with extremely high environmental stability of the charging characteristics.
[0051] As described above, when the unavoidable impurities such as Cl contained in the raw material are present on the surface of the ferrite particles, they are easily ionized, and moisture in the atmosphere is adsorbed onto the surface of the ferrite particles. If the amount of these unavoidable impurities on the surface of the ferrite particles increases, for example, the resistance value will decrease significantly in a high-temperature and high-humidity environment, and the environmental fluctuation of the charging characteristics will also increase. As the Fe raw material, iron oxide by-produced from the hydrochloric acid pickling process occurring during steel production is generally used. Therefore, the Fe raw material contains Cl as an unavoidable impurity. Specifically, the content of iron oxide (III) (Fe2O3) used as the iron oxide for ferrite is 98.5 mass% or more, and contains, for example, 0.15 mass% or less of Cl (JISK1462-1981). In addition to Cl, the Fe raw material, the Mn raw material, and the Mg raw material also contain Na and K as unavoidable impurities. If seawater, sodium hydroxide, etc. are used in the manufacturing process of each raw material, the content of these unavoidable impurities will also increase. Compared with Na, K, etc., the total amount of Cl contained in the raw material as an unavoidable impurity is large, and when the amount of eluted chlorine measured by the elution method is small, the amounts of other unavoidable impurities also tend to be small.
[0052] Therefore, in order to keep the amount of eluted chlorine within the above range, it is considered to use iron oxide for ferrite with a Fe2O3 content of 98.5% or more as described above. In addition, by performing heat treatment at a high temperature (for example, the same temperature as that suitable for growing a perovskite crystal phase) in the main sintering step described later, most of the inevitable impurities in the particles can be removed. Furthermore, as described above, since the ferrite particles according to the present invention contain a perovskite crystal phase component, the crystal grains are relatively small and the grain boundary volume is relatively large. Therefore, even if the content of inevitable impurities such as Cl is about the same, it is possible to prevent these inevitable impurities from precipitating inside the ferrite particles and segregating on the surface of the ferrite particles. Therefore, compared with the case where the perovskite crystal phase component is not contained, the amount of eluted chlorine by the elution method can be reduced, and the environmental fluctuation of the charging characteristics can be reduced.
[0053] On the other hand, in the process of generating the perovskite crystal phase component, when most of the unavoidable impurities are removed and the amount of chlorine dissolved is less than 35 ppm, the amount of water chemically adsorbed to the particle surface is reduced. In this case, good charging characteristics can be maintained under high temperature and high humidity environments, but the amount of moisture on the particle surface is too small, and charging characteristics deteriorate under low temperature and low humidity conditions, such as causing charge-up. Therefore, through intensive research by the present inventors, it has been found that by adopting firing conditions suitable for generating the perovskite crystal phase component to remove most of the unavoidable impurities contained in the fired material, and using the chlorine gas released from the fired material into the atmosphere to create a chlorine atmosphere in the furnace, the alkaline earth metal on the ferrite particle surface is bonded with chlorine to generate chlorides, and an appropriate amount of moisture is adsorbed on the surface of the ferrite particles, thereby obtaining ferrite particles with higher environmental stability that can maintain good charging characteristics both under high temperature and high humidity environments and low temperature and low humidity environments.
[0054] Here, in order to suppress the charge-up in a low-temperature and low-humidity environment, the amount of eluted chlorine is preferably 40 ppm or more, more preferably 42 ppm or more, even more preferably 45 ppm or more, and even more preferably 47 ppm or more. On the other hand, if the amount of eluted chlorine is too large, the resistance value may fluctuate greatly in a high-temperature and high-humidity environment. Therefore, the amount of eluted chlorine is more preferably 95 ppm or less, even more preferably 90 ppm or less, even more preferably 85 ppm or less, and even more preferably 80 ppm or less. In addition, by adopting the firing conditions described later, the amount of eluted chlorine can be adjusted to within the above range.
[0055] 1-6.Magnetic properties Next, the magnetic properties of the ferrite particles will be described. When the ferrite particles are used as the core material of the carrier for electrophotographic developer, it is preferable that the saturation magnetization measured by VSM when a magnetic field of 1K·1000 / 4π·A / m is applied is 50 emu / g or more and 70 emu / g or less. When the saturation magnetization is 50 emu / g or more, the magnetic force of the core material is high, and carrier scattering caused by low magnetization can be effectively suppressed. In addition, although there is a trade-off between saturation magnetization and electrical resistance, when the saturation magnetization of the ferrite particles is within the above range, the balance between the two is good, and an electrophotographic developer capable of performing high-quality electrophotographic printing can be obtained. In addition, even if the magnetization is high, if the resistance is low, carrier scattering due to low resistance may occur. By setting the saturation magnetization to 70 emu / g or less, carrier scattering due to low resistance can also be effectively suppressed.
[0056] 1-7.Electrical characteristics Next, the electrical properties of the ferrite particles will be described. When measured with an electrode distance of 6.5 mm and an applied voltage of 1000 V, the resistance M in a normal temperature and humidity environment (23°C, 55% relative humidity) is 1.0×10 6 (Ω) or more 1.0×10 9.5 When the resistance value of the ferrite particles is within this range, when the ferrite particles are used as a core material and a resin coating layer is provided on the surface to form a carrier, the resin coating layer peels off during mixing with the toner, exposing the core material, and carrier scattering due to charge injection can be suppressed.
[0057] 1-8.Physical properties (1) Volume average particle size (D 50 ) When the ferrite particles are used as a core material of a carrier for an electrophotographic developer, the volume average particle diameter (D 50) is preferably 24 μm or more and 40 μm or less. However, the volume average particle diameter referred to here is a value measured in accordance with JIS Z 8825:2013 by a laser diffraction / scattering method. When the volume average particle diameter is within this range, the charge imparting property to the toner is high, and the charge imparting property can be maintained for a long period of time. Therefore, the life of the electrophotographic developer can be extended.
[0058] In contrast, the volume average particle size (D 50 If the volume average particle diameter (D 50 ) is less than 24 μm, the particle size is small, and the ferrite particles are likely to aggregate. When the ferrite particles are used as a core material and the surface is coated with a resin to form a carrier, if the ferrite particles are aggregated, the surface of each ferrite particle cannot be well coated with the resin. If the aggregate of the ferrite particles is subsequently loosened during the manufacture or use of the developer, the developer will have a high content of carrier with a large area not coated with resin. Therefore, when a developer is manufactured using a carrier having such ferrite particles as a core material, sufficient charge imparting properties to the toner may not be obtained, which is not preferable.
[0059] On the other hand, the volume average particle size (D 50 When the volume average particle size (D) exceeds 40 μm, the particle size of each particle constituting the powder becomes large. 50) is smaller than that of ferrite particles, the surface area of the carrier that contributes to triboelectric charging with the toner is smaller when viewed as a whole powder. Therefore, sufficient charge imparting ability to the toner may not be obtained. In order to improve this, by increasing the surface area of each ferrite particle by giving unevenness to the surface of each ferrite particle, the surface area of the carrier that contributes to triboelectric charging with the toner can be increased. In this case, the charge imparting ability to the toner is improved, but it is not preferable because the carrier is likely to crack or chip due to mechanical stress applied to the protrusions on the carrier surface when mixed with the toner. In other words, it may not be possible to maintain the strength of the carrier when used as a developer, which is not preferable.
[0060] From the above viewpoint, the volume average particle size (D 50 The lower limit of the volume average particle diameter (D) is more preferably 27 μm, and further preferably 30 μm. 50 The upper limit of the thickness φ is preferably 38 μm, and more preferably 36 μm.
[0061] (2) BET specific surface area The BET specific surface area of the ferrite particles is preferably within the range represented by the following formula. 0.165≦X≦0.550 In the above formula, X is the BET specific surface area (m 2 / g).
[0062] The BET specific surface area here can be a value measured using, for example, a specific surface area measuring device (Macsorb HM model-1208 (manufactured by Mountec Co., Ltd.)). Here, the moisture content of the ferrite particles varies depending on the amount of water chemically and physically adsorbed to the particle surface. When the BET specific surface area of the ferrite particles increases, the amount of water physically adsorbed to the particle surface generally increases. When the amount of water physically adsorbed to the particle surface becomes too large, the moisture content of the ferrite particles tends to fluctuate due to the influence of the atmospheric humidity, and the charging characteristics tend to be affected by the atmospheric humidity. When the BET specific surface area is within the range represented by the above formula, the amount of water physically adsorbed in the moisture content is within an appropriate range, and the charging characteristics can be prevented from fluctuating significantly even when the atmospheric humidity changes. That is, the amount of water chemically adsorbed to the particle surface is also within an appropriate range, and appropriate moisture can be retained on the surface even in a low-temperature, low-humidity environment, and excessive moisture can be prevented from being retained on the surface even in a high-temperature, high-humidity environment, so that good charging characteristics can be maintained in any environment. Furthermore, when the BET specific surface area is within the above range, the surface has appropriate irregularities, and when the ferrite particles are used as a core material, the surface can be favorably coated with a resin, which is preferable.
[0063] On the other hand, when the BET specific surface area is less than the lower limit, the amount of water physically adsorbed on the particle surface is reduced. In addition, it is generally believed that ferrite particles having a BET specific surface area less than the lower limit are sintered at high temperature for a long time, which removes surface irregularities. In this case, unavoidable impurities such as Cl are removed from the granules in the sintering process, the amount of chlorides generated on the particle surface is small, and the amount of water chemically adsorbed on the particle surface is also low. For these reasons, when the BET specific surface area is less than the lower limit, the moisture content of the ferrite particles is likely to be less than the lower limit of the range specified in the present invention, making it difficult to suppress charge-up in a low-temperature, low-humidity environment. On the other hand, when the BET specific surface area is larger than the upper limit, the moisture content of the ferrite particles is likely to be greater than the upper limit of the range specified in the present invention, which may result in a large decrease in resistance value in a high-temperature, high-humidity environment. Alternatively, the amount of water chemically adsorbed to the particle surface decreases, making it difficult to retain an appropriate amount of moisture in a low-temperature, low-humidity environment, which may cause charge-up and lead to deterioration in image quality, such as insufficient image density. In addition, it is generally believed that ferrite particles having a BET specific surface area less than the above lower limit have no surface irregularities due to long-term sintering at high temperatures. In this case, unavoidable impurities such as Cl are removed from the granulated material in the sintering process, the amount of chlorides generated on the particle surface is small, and the amount of water chemically adsorbed on the particle surface is also low.
[0064] In order to obtain the above effects, the lower limit of the above formula is more preferably 0.188, even more preferably 0.190, even more preferably 0.195, and even more preferably 0.200, and the upper limit of the above formula is more preferably 0.500, even more preferably 0.450, even more preferably 0.400, and even more preferably 0.380.
[0065] The BET specific surface area tends to increase as the alkaline earth metal content increases, and tends to decrease as the firing temperature increases. By adjusting these conditions, the BET specific surface area can be controlled to be within the above range.
[0066] (3) Apparent density The apparent density of the ferrite particles is preferably within the range represented by the following formula. 1.90≦Y≦2.50 In the above formula, Y is the apparent density of the ferrite particles (g / cm 3 )
[0067] The apparent density referred to here is a value measured by the funnel method in accordance with JIS Z 2504: 2012. When the apparent density of the ferrite particles is within the range represented by the above formula, the flowability is good and the weight is heavy, so that the frequency and strength of contact with the toner can be increased.
[0068] In order to obtain the above effects, the lower limit of the above formula is more preferably 1.95, even more preferably 2.00, and even more preferably 2.15, and the upper limit of the above formula is more preferably 2.45.
[0069] 2. Carrier for electrophotographic developer Next, the electrophotographic developer carrier according to the present invention will be described. The electrophotographic developer carrier according to the present invention is characterized by comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles. That is, the above-mentioned ferrite particles are characterized by being used as a core material of the electrophotographic developer carrier. The ferrite particles are as described above, so here, the resin coating layer will be mainly described.
[0070] (1) Type of coating resin The type of resin (coating resin) constituting the resin coating layer is not particularly limited. For example, fluororesin, acrylic resin, epoxy resin, polyamide resin, polyamideimide resin, polyester resin, unsaturated polyester resin, urea resin, melamine resin, alkyd resin, phenol resin, fluoroacrylic resin, acrylic-styrene resin, silicone resin, etc. can be used. In addition, modified silicone resins obtained by modifying silicone resins with acrylic resins, polyester resins, epoxy resins, polyamide resins, polyamideimide resins, alkyd resins, urethane resins, fluororesins, etc. may be used. For example, from the viewpoint of suppressing resin peeling due to mechanical stress received during stirring and mixing with toner, it is preferable that the coating resin is a thermosetting resin. Examples of thermosetting resins suitable for the coating resin include epoxy resins, phenol resins, silicone resins, unsaturated polyester resins, urea resins, melamine resins, alkyd resins, and resins containing them. However, as described above, the type of coating resin is not particularly limited, and an appropriate one can be selected depending on the type of toner to be combined and the usage environment.
[0071] The resin coating layer may be formed using one type of resin, or may be formed using two or more types of resin. When using two or more types of resin, one resin coating layer may be formed by mixing two or more types of resin, or multiple resin coating layers may be formed. For example, it is also preferable to provide a first resin coating layer having good adhesion to the ferrite particles on the surface of the ferrite particles, and provide a second resin coating layer on the surface of the first resin coating layer to impart the carrier with the desired charging performance.
[0072] (2) Resin coating amount The amount of resin (amount of resin coating) covering the surface of the ferrite particles is preferably 0.1% by mass or more and 10% by mass or less with respect to the ferrite particles used as the core material. If the amount of resin coating is less than 0.1% by mass, it becomes difficult to sufficiently coat the surface of the ferrite particles with resin, and it becomes difficult to obtain the desired charge-imparting ability. If the amount of resin coating exceeds 10% by mass, aggregation of carrier particles occurs during production, which not only reduces productivity such as a decrease in yield, but also fluctuates developer properties such as the fluidity of the developer in the actual machine or the charge-imparting ability to the toner, which is not preferable.
[0073] (3) Additives The resin coating layer may contain additives such as conductive agents and charge control agents for controlling the electrical resistance, charge amount, and charging speed of the carrier. Examples of conductive agents include conductive carbon, oxides such as titanium oxide and tin oxide, and various organic conductive agents. However, since the electrical resistance of the conductive agent is low, if the amount of the conductive agent added is too large, charge leakage is likely to occur. Therefore, the content of the conductive agent is preferably 0.25% by mass or more and 20.0% by mass or less, more preferably 0.5% by mass or more and 15.0% by mass or less, and even more preferably 1.0% by mass or more and 10.0% by mass or less, based on the solid content of the coating resin.
[0074] Examples of the charge control agent include various charge control agents and silane coupling agents that are generally used for toners. The types of these charge control agents and coupling agents are not particularly limited, but charge control agents such as nigrosine dyes, quaternary ammonium salts, organometallic complexes, and metal-containing monoazo dyes, aminosilane coupling agents, and fluorine-based silane coupling agents can be preferably used. The content of the charge control agent is preferably 0.25% by mass or more and 20.0% by mass or less, more preferably 0.5% by mass or more and 15.0% by mass or less, and even more preferably 1.0% by mass or more and 10.0% by mass or less, based on the solid content of the coating resin.
[0075] 3. Electrophotographic Developer Next, an embodiment of the electrophotographic developer according to the present invention will be described The electrophotographic developer contains the above-mentioned carrier for electrophotographic developer and a toner.
[0076] As the toner constituting the electrophotographic developer, for example, either a polymerized toner produced by a polymerization method or a pulverized toner produced by a pulverization method can be preferably used. These toners may contain various additives, and may be any toner as long as they can be used as an electrophotographic developer in combination with the above carrier.
[0077] Toner volume average particle size (D 50 The volume average particle diameter (D) of the toner is preferably 2 μm or more and 15 μm or less, and more preferably 3 μm or more and 10 μm or less. 50 ) within this range, an electrophotographic developer capable of performing high-quality electrophotographic printing can be obtained.
[0078] The mixture ratio of the carrier and the toner, i.e., the toner concentration, is preferably 3% by mass or more and 15% by mass or less. An electrophotographic developer containing the toner at this concentration can easily obtain a desired image density and can more effectively suppress fogging and toner scattering.
[0079] On the other hand, when the electrophotographic developer is used as a replenishment developer, the toner is preferably present in an amount of 2 parts by mass or more and 50 parts by mass or less per part by mass of the carrier.
[0080] The electrophotographic developer can be suitably used in various electrophotographic developing devices that apply a magnetic brush development method in which a carrier is attracted and attached to a magnetic drum or the like by magnetic force to form a brush-like toner, and a visible image is formed by attaching the toner to an electrostatic latent image formed on a photoconductor or the like while applying a bias electric field. The electrophotographic developer can be used not only in electrophotographic developing devices that use a DC bias electric field when applying a bias electric field, but also in electrophotographic developing devices that use an AC bias electric field in which an AC bias electric field is superimposed on a DC bias electric field.
[0081] 4. Manufacturing method The following describes the methods for producing the ferrite powder, the carrier core material for an electrophotographic developer, the carrier for an electrophotographic developer, and the electrophotographic developer according to the present invention.
[0082] 4-1. Ferrite powder and carrier core material for electrophotographic developers The ferrite powder and the carrier core material for an electrophotographic developer according to the present invention can be produced as follows.
[0083] First, raw materials are weighed in appropriate amounts so as to obtain a desired ferrite composition, and then pulverized and mixed in a ball mill or a vibration mill for 0.5 hours or more, preferably 1 hour to 20 hours, and then calcined.
[0084] For example, in order to produce spinel ferrite particles of a desired composition in (MnO)a(MgO)b(Fe2O3)c (where a+b+c=100 (mol%), a≠0, 0≦b, c≠0), the respective raw materials are weighed and pulverized and mixed so that a, b, and c have the desired values. As the raw materials, for example, it is preferable to use Fe2O3, Mg(OH)2 and / or MgCO3, and one or more manganese compounds selected from the group consisting of MnO2, Mn2O3, Mn3O4, and MnCO3.
[0085] The ferrite particles according to the present invention contain a perovskite-type crystalline phase component represented by the formula RZrO3 (where R is an alkaline earth metal). Therefore, for the alkaline earth metal (R), an oxide of the alkaline earth metal (R) is used as a raw material, weighed out to obtain a desired amount, and pulverized and mixed with other raw materials. For Zr, ZrO2 can be used as a raw material.
[0086] At that time, the Zr content (P Zr ) is 0.50 mol% or more and 1.00 mol% or less, R content (P R ) is 0.65 mol% or more and 1.29 mol% or less, R content (P R ) and Zr content (P Zr ) and the ratio (PR / P Zr Each ingredient is weighed out so that the mass ratio (Mn) is 1.10 or more and 2.58 or less.
[0087] ZrO2 as a raw material is pulverized and mixed with other raw materials. In order to uniformly disperse zirconium dioxide inside the particles, it is desirable to add zirconium dioxide when pulverizing and mixing the raw materials. It is also preferable to pulverize and mix raw materials other than ZrO2, calcinate them in the atmosphere, add ZrO2, and further pulverize and mix them. In this case, the pulverized mixture of raw materials other than ZrO2 is pelletized using a pressure molding machine or the like, calcined in the atmosphere at a temperature of 700°C to 1200°C, and then ZrO2 is added.
[0088] After all the raw materials including ZrO2 are ground and mixed, or after raw materials other than ZrO2 are ground and mixed and calcined, a predetermined amount of ZrO2 is added to the calcined product obtained, and then it is ground in a ball mill, a vibration mill, or the like. Water is then added to the ground mixture, which is then finely ground in a bead mill or the like to obtain a slurry. The degree of grinding can be controlled by adjusting the diameter, composition, and grinding time of the beads used as the media. In order to uniformly disperse the raw materials, it is preferable to use fine beads with a particle size of 1 mm or less as the media. In addition, in order to uniformly disperse the raw materials, it is also preferable to use the volume average particle size (D 50 It is preferable to pulverize the powder so that the particle size (D) is 2.5 μm or less, and more preferably 2.0 μm or less. In order to suppress abnormal grain growth, the particle size (D 90 ) is preferably pulverized to 3.5 μm or less. By adjusting these, the perovskite crystal phase components can be dispersed more uniformly from the surface to the inside of the particles, and the above-mentioned various effects can be obtained.
[0089] Next, it is preferable to add a dispersant, a binder, etc. to the slurry thus obtained as necessary to adjust the viscosity to 2 poise to 4 poise. At this time, polyvinyl alcohol or polyvinylpyrrolidone can be used as the binder.
[0090] The slurry prepared as above is sprayed and dried using a spray dryer to obtain a granulated product. In this case, the granulation conditions are preferably set to a discharge rate of 20 Hz to 50 Hz, an atomizer disk rotation speed of 11000 rpm to 20000 rpm, and a drying temperature of 100° C. to 500° C. For example, in order to obtain ferrite particles having an apparent density within the above range, it is preferable to set the atomizer disk rotation speed to 11000 rpm to 16000 rpm and a drying temperature to 150° C. to 300° C.
[0091] Next, it is preferable to classify the granulated material before firing and remove fine particles contained in the granulated material in order to obtain a ferrite powder with a uniform particle size. The classification of the granulated material can be performed using a known air classification or a sieve.
[0092] Next, the classified granules are fired. It is preferable that the granules are fired in a firing furnace such as a rotary kiln in which the granules (material to be fired) are passed through a hot section while being fluidized, and then fired.
[0093] By carrying out the primary firing in a firing furnace such as a rotary kiln in which the granulated material is passed through a hot section while being made to flow, it is possible to remove organic substances such as binders used during granulation from the granulated material in a relatively short time and uniformly, compared to carrying out the primary firing while the granulated material is left stationary in a basin, etc. At the same time, it is possible to advance part of the ferrite reaction during the primary firing, and it is possible to suppress the occurrence of variations in the surface Rz during the subsequent main firing.
[0094] In addition, when the primary firing is performed using the above-mentioned type of firing furnace, the temperature is preferably, for example, 750°C or higher and 1050°C or lower. By performing the primary firing in this temperature range, it becomes easier to efficiently remove organic matter and perform the ferrite reaction while suppressing abnormal grain growth and suppressing the occurrence of variations in surface roughness Rz as described above. Furthermore, in order to efficiently remove organic matter and perform the ferrite reaction, it is more preferable to perform the primary firing at a temperature of 800°C or higher, and even more preferable to perform the primary firing at a temperature of 850°C or higher. In order to suppress abnormal grain growth, it is more preferable to perform the primary firing at a temperature of 1000°C or lower, and even more preferable to perform the primary firing at a temperature of 980°C or lower.
[0095] Moreover, the main firing is preferably carried out by maintaining the temperature at 850°C or higher for 1.5 hours to 24 hours in an inert atmosphere or a weakly oxidizing atmosphere. However, the main firing temperature is not particularly limited as long as the ferrite particles according to the present invention can be obtained. Here, an inert atmosphere or a weakly oxidizing atmosphere refers to an atmosphere of a mixed gas of nitrogen and oxygen in which the oxygen concentration is 5% by volume (50,000 ppm) or less, more preferably 3.5% by volume (35,000 ppm) or less, even more preferably 2.5% by volume (25,000 ppm) or less, even more preferably 1.0% by volume (10,000 ppm) or less, and even more preferably 0.5% by volume (5,000 ppm) or less.
[0096] For example, by holding the mixture at a temperature (850°C or higher and 1150°C or lower) suitable for generating a spinel crystal phase for 3 hours or more, and then holding the mixture at a temperature (for example, 1150°C or higher and 1500°C or lower) suitable for generating a perovskite crystal phase represented by the composition formula RZrO3 such as strontium zirconate for 1 hour or more for main firing, the ferrite particles can be obtained in which the zirconium component is well dispersed at the grain boundaries while sufficiently generating the spinel crystal phase. In addition, by appropriately controlling the firing temperature, firing time, and atmospheric oxygen concentration during firing according to the type of alkaline earth metal (R) and the amount of ZrO2 blended, the BET specific surface area, resistance value, apparent density, and magnetization can be controlled within a range suitable for the carrier core material for electrophotographic developer. In addition, by holding the mixture at a temperature of 1200°C or higher for 2 hours or more, it becomes easier to keep the amount of chlorine dissolved within a range appropriate for maintaining the moisture content specified in the present invention.
[0097] For example, in the case of strontium zirconate (SrZrO3), in order to generate a sufficient amount of perovskite crystal phase components while keeping the apparent density within the range of the present invention, the firing temperature is preferably maintained at a temperature of 1170°C or higher and 1400°C or lower, more preferably 1180°C or higher and 1350°C or lower, and even more preferably 1200°C or higher and 1330°C or lower, for one hour or more.
[0098] For example, in the case of calcium zirconate (CaZrO3) or barium zirconate (BaZrO3), it is preferable to pulverize the raw material, add a reaction accelerator, and then sinter at a predetermined temperature. In order to generate the perovskite crystal phase components of calcium zirconate (CaZrO3) or barium zirconate (BaZrO3), it is necessary to sinter at a high temperature of 2000°C or higher if no reaction accelerator is added. On the other hand, by pulverizing the raw material to a primary particle size of about several tens of nanometers and adding an aluminum compound (e.g., alumina (Al2O3), etc.) as a reaction accelerator, these perovskite crystal phase components can be generated even at a temperature of 1500°C or lower. In this way, the ferrite particles according to the present invention can be obtained by maintaining the temperature suitable for generating the perovskite crystal phase components according to the target composition and adjusting other conditions as necessary.
[0099] In addition, unlike the primary firing, it is preferable to use a firing furnace such as a tunnel kiln or elevator kiln in which the granulated material (material to be fired) is passed through the hot section while being moved, rather than a firing furnace such as a rotary kiln in which the granulated material is passed through the hot section while being moved. In a firing furnace such as a rotary kiln in which the granulated material is passed through the hot section while being moved, if the oxygen concentration in the firing atmosphere is low, the granulated material may adhere to the inner surface of the furnace when passing through the hot section, and the granulated material passing through the inside while flowing may not be able to be sufficiently heated. In that case, the granulated material passes through the hot section without being sufficiently sintered, so that the surface of the obtained fired material is sufficiently sintered, but the inside is often insufficiently sintered. Such fired material does not meet the strength required for a carrier core material for electrophotographic developer, and the ferrite reaction inside is insufficient, so that the magnetic properties and electrical properties required for a carrier core material for electrophotographic developer may not be met. Furthermore, if the sintering inside the fired product is insufficient, the perovskite crystal phase component represented by the composition formula RZrO3 cannot be sufficiently generated in the firing process, which makes it difficult to obtain the ferrite particles according to the present invention.
[0100] On the other hand, if the granulated material is placed in a sintering bowl or the like and passed through a hot section while remaining stationary, the inside of the sintered material can be sufficiently sintered, making it easy to obtain ferrite particles that are highly magnetized and highly resistive and in which the perovskite-type crystal phase component represented by the composition formula RZrO3 is sufficiently generated. For these reasons, it is preferable to use a tunnel kiln, elevator kiln, or the like when carrying out the main sintering step.
[0101] Continuous furnaces such as tunnel kilns and elevator kilns have multiple regions from the inlet side to the outlet side, and each region is configured so that the temperature can be controlled independently. The multiple regions provided in the furnace are appropriately divided into three zones, the temperature rising zone, the heating zone, and the cooling zone, and the temperature of each zone (or each region) and the speed at which the bowl or the like passes through each zone (or each region) are controlled, so that the granulated material can be heat-treated with a desired temperature gradient.
[0102] Here, in order to manufacture the ferrite particles according to the present invention, it is preferable to use a continuous furnace capable of adjusting the atmosphere inside the furnace (hereinafter referred to as a "continuous atmospheric furnace") and perform the above-mentioned atmosphere control. Furthermore, in order to manufacture the ferrite particles according to the present invention, it is preferable to carry out the cooling step, or the firing step and the cooling step, in a chlorine atmosphere adjusted as follows.
[0103] First, the method of controlling the firing atmosphere will be described. In the continuous atmospheric furnace, one or more inlets are provided for each of the above-mentioned regions to drive (introduce) nitrogen gas or the like into the furnace. In addition, the continuous atmospheric furnace is provided with an exhaust port for discharging the gas in the furnace to the outside. By adjusting the nitrogen flow rate and exhaust volume for each zone, the atmosphere can be controlled so that the oxygen concentration in the furnace becomes a preset oxygen concentration. In addition, an air flow is generated in the furnace in the direction from the outlet side to the inlet side, so that the firing atmosphere can efficiently come into contact with the granulated material passing through the furnace.
[0104] When controlling the atmosphere inside the furnace to achieve a specified oxygen concentration, the amount of nitrogen gas flowing into each zone is usually controlled so that the nitrogen flow rate (amount of nitrogen injected) into the heating zone is the highest and the nitrogen flow rate into the temperature rising zone is the lowest. As a result, the temperature rising zone has a more negative pressure than the heating zone, and an air flow toward the inlet side is generated inside the furnace as described above. When granulated material is fired in the temperature rising zone, decomposition gases of organic matter and chlorine gas are released into the atmosphere as the temperature of the granulated material rises. These gases released from the granulated material are directed toward the inlet side by the air flow inside the furnace and are exhausted from an exhaust port provided on the inlet side.
[0105] As a result of intensive research by the present inventors, when obtaining the ferrite particles according to the present invention, it has been found that when controlling the atmosphere in the furnace to have a predetermined oxygen concentration, nitrogen gas is introduced into each zone so that the nitrogen inflow amount in the temperature rising zone is the largest, and the nitrogen inflow amount into the heating zone and the cooling zone is made smaller than that of the temperature rising zone, thereby making it possible to adjust the cooling zone (cooling step) or the heating zone and the cooling zone (sintering step and cooling step) to a chlorine atmosphere while maintaining a predetermined oxygen concentration. According to this method, the nitrogen inflow amount into each of the temperature rising zone, heating zone, and cooling zone can be adjusted to a more positive pressure than the heating zone, and the chlorine gas released from the granulated material into the atmosphere while passing through the temperature rising zone or the heating zone remains in the cooling zone, or the heating zone and the cooling zone, making it possible to make the cooling zone, or the heating zone and the cooling zone a chlorine atmosphere while maintaining a predetermined oxygen concentration. Therefore, while using Fe raw material with a low Cl content as an inevitable impurity, an appropriate amount of alkaline earth metal chloride is generated on the surface of the ferrite particles without adding chlorine to the raw material or to the furnace, and the ferrite particles according to the present invention can be obtained. In this way, according to this method, since it is not necessary to use Fe raw material with a particularly high chlorine content or to add chlorine to the raw material or to the furnace, it is possible to produce ferrite particles with good magnetic properties and charging properties and an appropriate moisture content by simply changing the distribution of the nitrogen flow rate.
[0106] In obtaining the ferrite particles according to the present invention, the distribution of the nitrogen inflow amount to each of the temperature rising zone, the heating zone, and the cooling zone is preferably, for example, as follows. First, the total amount of nitrogen to be flowed into the furnace so that the furnace has a predetermined oxygen concentration (hereinafter, the total nitrogen inflow amount) is set to 100%. At this time, the nitrogen inflow amount to the temperature rising zone can be adjusted to 38 to 62% of the total nitrogen inflow amount, the nitrogen inflow amount to the heating zone to 19 to 31% of the total nitrogen inflow amount, and the nitrogen inflow amount to the cooling zone to 19 to 31% of the total nitrogen inflow amount. At this time, it is more preferable to adjust the nitrogen inflow amount to the temperature rising zone to 40 to 60%, the nitrogen inflow amount to the heating zone to 20 to 30%, and the nitrogen inflow amount to the cooling zone to 20 to 30%. The amount of nitrogen flowing into the heating zone and the cooling zone may be the same or different, as long as the oxygen concentration in the furnace is controlled to a desired oxygen concentration, and the chlorine gas released into the atmosphere while the granules pass through the temperature-raising zone or the heating zone is retained in the cooling zone, or the heating zone and the cooling zone, and at least the cooling zone is made into a chlorine atmosphere. In addition to the above method, an air flow from the outlet side to the inlet side is generated in the furnace, and the atmospheric oxygen concentration in the furnace is controlled to a predetermined concentration, and the air flow speed in the furnace is slowed to 3 / 4 or less of the nitrogen inflow speed generally used in the past, so that the chlorine gas volatilized from the granules remains in the heating zone and the cooling zone longer than usual.
[0107] The fired product is then crushed and classified to obtain ferrite particles. Classification methods include existing air classification, mesh filtration, sedimentation, etc. These methods are used appropriately to adjust the particle size to the desired particle size. When performing dry recovery, it is also possible to recover using a cyclone, etc. When adjusting the particle size, two or more of the above-mentioned classification methods may be selected and carried out, or the conditions may be changed in one classification method to remove coarse particles and fine particles.
[0108] Thereafter, if necessary, the surface of the ferrite particles is heated at a low temperature to perform a surface oxidation treatment, thereby adjusting the surface resistance of the ferrite particles. The surface oxidation treatment can be performed by subjecting the ferrite particles to a heat treatment at 400°C to 730°C, preferably 450°C to 650°C, in an oxygen-containing atmosphere such as air, using a rotary electric furnace, a batch electric furnace, or the like. If the heating temperature during the surface oxidation treatment is lower than 400°C, the surface of the ferrite particles cannot be sufficiently oxidized, and the desired surface resistance characteristics may not be obtained. On the other hand, if the heating temperature is higher than 730°C, in the case of manganese-containing ferrite, the oxidation of manganese proceeds too much, and the magnetization of the ferrite particles decreases, which is not preferable. To form a uniform oxide film on the surface of the ferrite particles, it is preferable to use a rotary electric furnace. However, the surface oxidation treatment is an optional step.
[0109] 4-2. Carrier for electrophotographic developer The electrophotographic developer carrier according to the present invention is a carrier in which the above-mentioned ferrite particles are used as a core material and a resin coating layer is provided on the surface of the ferrite particles. The resin constituting the resin coating layer is as described above. When forming a resin coating layer on the surface of the ferrite particles, a known method such as a brush coating method, a spray drying method using a fluidized bed, a rotary drying method, a liquid immersion drying method using a universal stirrer, etc. can be adopted. In order to improve the ratio of the resin coating area to the surface of the ferrite particles (resin coating rate), it is preferable to adopt a spray drying method using a fluidized bed. In any case, the ferrite particles can be subjected to a resin coating treatment once or multiple times. The resin coating liquid used in forming the resin coating layer may contain the above-mentioned additives. In addition, since the amount of resin coating on the surface of the ferrite particles is as described above, a description thereof will be omitted here.
[0110] After applying the resin coating liquid to the surface of the ferrite particles, baking may be performed by an external heating method or an internal heating method as necessary. For the external heating method, a fixed or flow type electric furnace, a rotary type electric furnace, a burner furnace, etc. can be used. For the internal heating method, a microwave furnace can be used. When a UV-curable resin is used as the coating resin, a UV heater is used. Baking is required to be performed at a temperature equal to or higher than the melting point or glass transition point of the coating resin. When a thermosetting resin or a condensation crosslinking type resin is used as the coating resin, baking is required at a temperature at which the curing of these resins progresses sufficiently.
[0111] 4-3.Electrophotographic developer Next, a method for producing an electrophotographic developer according to the present invention will be described. The electrophotographic developer according to the present invention contains the above-mentioned carrier for electrophotographic developer and a toner. As the toner, either a polymerized toner or a pulverized toner can be preferably used as described above.
[0112] The polymerized toner can be produced by a known method such as a suspension polymerization method, an emulsion polymerization method, an emulsion aggregation method, an ester elongation polymerization method, or a phase inversion emulsification method. For example, a colored dispersion liquid in which a colorant is dispersed in water using a surfactant is mixed and stirred with a polymerizable monomer, a surfactant, and a polymerization initiator in an aqueous medium, and the polymerizable monomer is emulsified and dispersed in the aqueous medium, and polymerized while stirring and mixing, and then a salting agent is added to salt out the polymer particles. The particles obtained by salting out are filtered, washed, and dried to obtain a polymerized toner. Thereafter, an external additive may be added to the dried toner particles as necessary.
[0113] Furthermore, when producing the polymerized toner particles, a toner composition is used that contains a polymerizable monomer, a surfactant, a polymerization initiator, a colorant, etc. The toner composition may contain a fixing improver and a charge control agent.
[0114] The pulverized toner is prepared by thoroughly mixing, for example, a binder resin, a colorant, a charge control agent, etc., in a mixer such as a Henschel mixer, then melt-kneading and uniformly dispersing in a twin-screw extruder, etc., cooling, finely pulverizing in a jet mill, etc., classifying, and then classifying, for example, with an air classifier, etc., to obtain a toner of a desired particle size. If necessary, wax, magnetic powder, viscosity modifier, and other additives may be added. Furthermore, external additives may be added after classification.
[0115] The present invention will now be described in detail with reference to examples and comparative examples, although the present invention is not limited to the following examples. EXAMPLES
[0116] (1) Ferrite particles In Example 1, spinel ferrite particles containing a perovskite crystal phase component represented by the composition formula SrZrO3 (R=Sr) and mainly containing a spinel crystal phase component were produced as follows.
[0117] First, as main component raw materials for producing ferrite, Fe2O3 raw material, MnO raw material, and MgO raw material were weighed out so that the molar ratios were Fe2O3:51.3, MnO equivalent:38.3, and MgO equivalent:10.4. In addition, ZrO2 raw material and SrO raw material were weighed out so that the ZrO2 equivalent:0.70 mol% and SrO equivalent:0.95 mol% were obtained when these main component raw materials were taken as 100 mol%. Here, trimanganese tetroxide was used as the MnO raw material, magnesium oxide was used as the MgO raw material, ferric oxide (containing 1100 ppm of Cl as an impurity) was used as the Fe2O3 raw material, strontium carbonate was used as the SrO raw material, and zirconium dioxide was used as the ZrO2 raw material.
[0118] Next, the weighed raw materials other than zirconium dioxide were pulverized for 5 hours using a dry media mill (vibration mill, stainless steel beads with a diameter of 1 / 8 inch), and the pulverized material was made into pellets of about 1 mm square using a roller compactor. The obtained pellets were passed through a vibrating sieve with a mesh size of 3 mm to remove coarse powder, and then passed through a vibrating sieve with a mesh size of 0.5 mm to remove fine powder, and then heated at 800°C for 3 hours in a continuous electric furnace to perform pre-firing. Next, the raw materials were pulverized using a dry media mill (vibration mill, stainless steel beads with a diameter of 1 / 8 inch) until the average particle size became about 5 μm. The pulverization time was 6 hours.
[0119] Water and zirconium dioxide were added to the obtained pulverized material, and the mixture was pulverized for 6 hours using a wet media mill (horizontal bead mill, zirconia beads with a diameter of 1 mm). The particle size (primary particle size of the pulverized material) of the obtained slurry was measured using a laser diffraction particle size distribution analyzer (LA-950, Horiba, Ltd.). 50 is about 1.9 μm, D 90 was 3.3 μm.
[0120] Further, an appropriate amount of dispersant was added to the slurry prepared as above, and 0.4 mass% of PVA (polyvinyl alcohol) was added as a binder based on the solid content (the amount of the pre-calcined material in the slurry), and then the mixture was granulated and dried using a spray dryer. The particle size of the resulting granulated material was adjusted, and then the mixture was heated in an air atmosphere at 950°C for 2 hours in a rotary electric furnace (rotary kiln) for primary sintering.
[0121] After that, nitrogen gas was introduced into the tunnel-type electric furnace to control the atmosphere so that the oxygen concentration in the furnace was 0.0% by volume. At that time, the nitrogen inflow to the entire furnace (total nitrogen inflow) was distributed so that the nitrogen inflow to the temperature rise zone was 60%, the nitrogen inflow to the heating zone was 20%, and the nitrogen inflow to the cooling zone was 20%. In addition, the temperature rise rate was 100°C / hour, the firing temperature (holding temperature) was 1219°C, the holding time was 3 hours, and the cooling rate was 110°C / hour.
[0122] The obtained sintered product was crushed by a hammer crusher, and further classified by a gyro sifter (vibrating sieve) and a turbo classifier (air classifier) to adjust the particle size, and then subjected to surface oxidation treatment at 450°C in a rotary electric furnace equipped with a hot section and a cooling section following the hot section, and then low magnetic products were separated by magnetic separation to obtain ferrite particles. The main production conditions for the ferrite particles of Example 1 are shown in Table 1.
[0123] (2) Carrier for electrophotographic developer The above ferrite particles were used as a core material, and the ferrite particles were coated with a silicone resin as follows to obtain a carrier of Example 1.
[0124] First, a silicone resin solution (resin solid content 10% by mass) was prepared by mixing silicone resin (KR-350, manufactured by Shin-Etsu Silicone Co., Ltd.) and toluene. The resin solution was mixed with the ferrite particles of Example 1 using a universal stirrer to coat the surfaces of the ferrite particles with the resin solution. At that time, an amount of the resin solution was used such that the resin solid content was 1.0% by mass relative to the ferrite particles. Next, the ferrite particles to which the resin solution was attached were heated with stirring at 250°C for 3 hours using a heat exchange type stirring and heating device, and the volatile components contained in the resin solution were volatilized to dry the ferrite particles. As a result, a carrier for electrophotographic developer of Example 1 having a resin coating layer on the surfaces of the ferrite particles was obtained. EXAMPLES
[0125] In this example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.60 mol% and the SrO equivalent was 0.70 mol% when the main component raw material was 100 mol%, and the ferrite particles of Example 2 were produced in the same manner as in Example 1, except that the firing temperature (retention temperature) was set to 1221° C. The main production conditions of Example 2 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0126] In this example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.90 mol% and the SrO equivalent was 1.20 mol% when the main component raw material was 100 mol%, and the ferrite particles of Example 3 were produced in the same manner as in Example 1, except that the firing temperature (retention temperature) was set to 1217° C. The main production conditions of Example 3 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0127] The ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.50 mol% and the SrO equivalent was 0.65 mol% when the main component raw material was 100 mol%, and the sintering temperature (holding temperature) was set to 1212°C, the nitrogen inflow rate to the temperature rising zone was 40%, the nitrogen inflow rate to the heating zone was 25%, and the nitrogen inflow rate to the cooling zone was 35%. Ferrite particles of Example 4 were produced in the same manner as in Example 1. The main production conditions of Example 4 are shown in Table 1. In addition, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0128] The ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.50 mol% and the SrO equivalent was 1.29 mol% when the main component raw material was 100 mol%, and the sintering temperature (holding temperature) was 1200°C, the nitrogen inflow rate to the temperature rise zone was 50%, the nitrogen inflow rate to the heating zone was 20%, and the nitrogen inflow rate to the cooling zone was 30%. Ferrite particles of Example 5 were produced in the same manner as in Example 1. The main production conditions of Example 5 are shown in Table 1. In addition, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0129] In this example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 1.00 mol% and the SrO equivalent was 1.10 mol% when the main component raw material was 100 mol%, and the firing temperature (holding temperature) was set to 1232°C, the nitrogen inflow rate to the temperature rise zone was 55%, the nitrogen inflow rate to the heating zone was 25%, and the nitrogen inflow rate to the cooling zone was 20%. The ferrite particles of Example 6 were produced in the same manner as in Example 1. The main production conditions of Example 6 are shown in Table 1. In addition, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0130] In this example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 1.00 mol% and the SrO equivalent was 1.29 mol% when the main component raw material was 100 mol%, and the firing temperature (holding temperature) was set to 1225°C, the nitrogen inflow rate to the temperature rise zone was 60%, the nitrogen inflow rate to the heating zone was 20%, and the nitrogen inflow rate to the cooling zone was 20%. The ferrite particles of Example 7 were produced in the same manner as in Example 1, except that the ferrite particles were used as a core material. EXAMPLES
[0131] In this embodiment, ferrite particles containing a perovskite-type crystal phase component having a composition formula of CaZrO3 with R=Ca were manufactured. At that time, CaCO3 was used as the CaO raw material instead of the SrO raw material, and the ZrO2 raw material and the CaO raw material were weighed so that the ZrO2 equivalent: 0.50 mol% and the CaO equivalent: 0.65 mol% were weighed when the main component raw material was 100 mol%, and the sintering temperature (holding temperature) was set to 1235°C, the nitrogen inflow amount to the temperature rise zone was 40%, the nitrogen inflow amount to the heating zone was 35%, and the nitrogen inflow amount to the cooling zone was 25%. The ferrite particles of Example 8 were manufactured in the same manner as in Example 1, except that the ferrite particles were used as the core material. Comparative Example
[0132] [Comparative Example 1] In this comparative example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.50 mol% and the SrO equivalent was 1.29 mol% when the main component raw material was 100 mol%, and the sintering temperature (holding temperature) was set to 1215°C, the nitrogen inflow rate to the temperature rise zone was 20%, the nitrogen inflow rate to the heating zone was 30%, and the nitrogen inflow rate to the cooling zone was 50%. The ferrite particles of Comparative Example 1 were produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0133] [Comparative Example 2] In this comparative example, the ZrO2 raw material and the SrO raw material were weighed so that the ZrO2 equivalent was 0.50 mol% and the SrO equivalent was 1.29 mol% when the main component raw material was 100 mol%, and the firing temperature (holding temperature) was set to 1205°C, the nitrogen inflow rate to the temperature rise zone was 20%, the nitrogen inflow rate to the heating zone was 45%, and the nitrogen inflow rate to the cooling zone was 35%, and the atmosphere was controlled so that the atmospheric oxygen concentration was 0.1 volume%. The ferrite particles of Comparative Example 2 were produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0134] [Comparative Example 3] In this comparative example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 0.50 mol% and the SrO equivalent was 1.29 mol% when the main component raw material was 100 mol%, and primary firing was not performed. In addition, the firing temperature (retention temperature) during main firing was set to 1200°C, and the nitrogen inflow rate to the temperature rise zone was 50%, the nitrogen inflow rate to the heating zone was 25%, and the nitrogen inflow rate to the cooling zone was 25%. The ferrite particles of Comparative Example 3 were produced in the same manner as in Example 1. The main production conditions of Comparative Example 3 are shown in Table 1. In addition, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0135] [Comparative Example 4] In this comparative example, the ZrO2 raw material and the SrO raw material were weighed out so that the ZrO2 equivalent was 1.00 mol% and the SrO equivalent was 0.65 mol% when the main component raw material was 100 mol%, and the firing temperature (holding temperature) was set to 1236°C, the nitrogen inflow rate to the temperature rise zone was 50%, the nitrogen inflow rate to the heating zone was 25%, and the nitrogen inflow rate to the cooling zone was 25%. The ferrite particles of Comparative Example 4 were produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0136] [Comparative Example 5] In this comparative example, the ZrO2 raw material was not added, and the SrO raw material was weighed so that the SrO equivalent was 0.80 mol% when the main component raw material was 100 mol%, and the primary firing temperature was 970°C, the firing temperature (retention temperature) was 1150°C, the nitrogen inflow rate to the temperature rise zone was 50%, the nitrogen inflow rate to the heating zone was 25%, and the nitrogen inflow rate to the cooling zone was 25%. The ferrite particles of Comparative Example 5 were produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0137] [Comparative Example 6] In this comparative example, the ZrO2 raw material was not added, and the SrO raw material was weighed so that the SrO equivalent was 0.80 mol% when the main component raw material was 100 mol%, and the firing temperature (holding temperature) was set to 1190°C, the nitrogen inflow rate to the temperature rise zone was 20%, the nitrogen inflow rate to the heating zone was 30%, and the nitrogen inflow rate to the cooling zone was 50%, and the atmosphere was controlled so that the atmospheric oxygen concentration was 0.5 volume%. The ferrite particles of Comparative Example 6 were produced in the same manner as in Example 1. The main production conditions of Comparative Example 6 are shown in Table 1. In addition, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material.
[0138] <evaluation> The ferrite particles of each Example and Comparative Example obtained as described above were measured for (1) perovskite type crystal phase component content, (2) spinel type crystal phase content and element composition, (3) Zr element dispersion degree, (4) water content, (5) chlorine elution amount, (6) volume average particle size, (7) saturation magnetization, and (8) BET specific surface area. In addition, electrophotographic developers were prepared using the carriers for electrophotographic development of each Example and Comparative Example obtained as described above, and evaluations were performed for (9) charging characteristics, (10) image density, and (11) fogging. The evaluation methods / measurement methods and evaluation results are described below.
[0139] 1. Evaluation method / measurement method (1) Perovskite crystal phase component content (mass%) The ferrite particles produced in each Example and Comparative Example were used as samples, and the perovskite crystal phase component content in each ferrite particle was determined by Rietveld analysis of the powder X-ray diffraction pattern. Although it may be difficult to identify and quantify each crystal phase by waveform separation of the powder X-ray diffraction pattern, Rietveld analysis based on a crystal structure model makes it possible to identify and quantify each phase.
[0140] The X-ray diffraction device used was the "X'PertPRO MPD" manufactured by PANalytical. The X-ray source was a Co tube (CoKα rays). The optical system used was a focused optical system and a high-speed detector, the "X'Celarator". The measurement conditions were as follows. Scan speed: 0.08° / sec Divergence slit: 1.0° Scattering slit: 1.0° Receiving slit: 0.15mm Voltage and current of the sealed tube: 40kV / 40mA Measurement range: 2θ=15°~90° Number of times: 5
[0141] Based on the obtained measurement results, the crystal structure was identified as follows from the structure disclosed in the National Institute for Materials Science, "AtomWork" (URL: http: / / crystdb.nims.go.jp / ). Phase A: Manganese ferrite (spinel type crystal phase) Crystal structure: space group F d -3 m (No. 227) Phase B: Perovskite-type crystal phase represented by the composition formula RZrO3 Crystal structure: Space group P nma (No. 62) Phase C: Zirconium dioxide (zirconia) Crystal structure: Space group P -4 2 m (No. 111) However, in the space group Fd-3m assigned to the A phase, the Wyckoff positions of each atom were set as follows: 8b for the Mn atom, 16c for the Fe atom, and 32e for the O atom.
[0142] Next, the identified crystal structure was refined using the analytical software "RIETAN-FP v2.83 (http: / / fujioizumi.verse.jp / download / download.html)" to calculate the mass-converted abundance ratio as the phase composition ratio of each crystal phase. The profile function was the pseudo-Voigt function of Thompson, Cox and Hasting, and was asymmetrized by Howard's method. After confirming that the Rwp and S values, which indicate the accuracy of the fitting, were Rwp: 2% or less and S value: 1.5 or less, respectively, and that the main peaks of phases B and C were fitted at 2θ = 35 to 37°, each parameter was optimized.
[0143] Based on the results of the Rietveld analysis of the X-ray diffraction pattern obtained as described above, the content (mass%) of the perovskite-type crystal phase component (B phase) was determined when a phase composition analysis of the crystal phase constituting the ferrite particles was performed.
[0144] (2) Spinel-type crystal phase component content (mass%) and elemental composition (mass%) The results of the X-ray diffraction measurements of phases A, B, and C obtained above were analyzed with Fe2O3 (phase D), Mn2O3 (phase E), and strontium ferrite (phase F) added to determine the content (mass%) of the spinel-type crystal phase component in each ferrite particle.
[0145] The elemental composition of each ferrite particle was determined by ICP analysis as follows: First, 0.2 g of each ferrite particle was weighed, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added to the weighed ferrite particle, and the mixture was heated to prepare an aqueous solution in which the ferrite particles were completely dissolved, and the contents (mass%) of Fe, Mn, Mg, Sr, and Zr were measured using an ICP analyzer (Shimadzu ICPS-1000IV).
[0146] (3) Dispersion degree of Zr element For the ferrite particles produced in each of the Examples and Comparative Examples, the degree of dispersion of Zr element defined by the following formula was measured. Dispersion degree of Zr = Zr(s) / Zr(c) however, Zr(s): Zr content (mass%) in the surface area of the particle cross section measured by energy dispersive X-ray analysis Zr(c): Zr content (mass%) in the center of the particle cross section measured by energy dispersive X-ray analysis
[0147] Here, an explanation will be given with reference to Fig. 1. The central part of a cross section (particle cross section) of a ferrite particle is defined as follows. When the maximum diameter in the particle cross section (for example, an SEM image) is defined as a line segment Dx, the midpoint of the line segment Dx is defined as the center C of the particle cross section, and the end points of the line segment Dx are defined as points P. Then, the center C is defined as the central position of a square, and the length of one side is 35% of the length of the line segment Dx, which is defined as a square S. The area surrounded by this square S is defined as the central part.
[0148] The surface part of the cross section of the particle is defined as follows. Point P' is a point on the line segment Dx, and is located at a distance of 15% of the length of the line segment Dx from point P toward the center C. Rectangle R1 is a rectangle having a long side that is a line segment having a length of 35% of the length of the line segment Dx, perpendicular to the line segment Dx, and having point P or point P' as a midpoint, and a short side that is a line segment having a length of 15% of the length of the line segment Dx. In the present invention, the area surrounded by this rectangle R1 in the cross section of the ferrite particle is defined as the surface part. Note that FIG. 1 shows the cross-sectional shape of the ferrite particle 100 simplified to a circular shape for the purpose of explanation, and does not show the actual cross-sectional shape of the ferrite particle according to the present invention.
[0149] The central portion and the surface portion of the particle cross section thus defined are subjected to energy dispersive X-ray analysis (EDX analysis) to measure the content of Zr element in each region. The specific measurement method is as follows.
[0150] (a) Ferrite particles are embedded in resin and cross-sectionally processed by ion milling to prepare a cross-sectional sample for measurement. Ion milling is performed using an IM4000PLUS manufactured by Hitachi High-Technogies Corporation, with the ion beam acceleration voltage set to 6.0 kV in an argon atmosphere. The ferrite single particles to be analyzed here are those containing ferrite particles (powder) with a volume average particle size of D 50 Then, the maximum diameter Dx is D 50 ×0.8≦Dx≦D 50 The particles are in the range of ×1.2.
[0151] (b) The cross section of the ferrite particle to be analyzed is observed using a scanning electron microscope (SEM, Hitachi High-Technogies SU8020) with an acceleration voltage of 15 kV and a working distance of 15 mm for the obtained cross section sample. The magnification is set so that only one ferrite particle to be analyzed is present in the field of view and the entire particle fits within the field of view.
[0152] (c) Then, EDX analysis is performed on the center and surface (regions defined above) of the ferrite particle cross section. In the EDX analysis, mapping collection is performed for Fe, Mn, Mg, Sr, and Zr using an energy dispersive X-ray analyzer (Horiba, Ltd. EMax X-Max50), and the amount of each element (mass%) is calculated from the obtained X-ray spectrum peaks. The amount of Zr in the center of the obtained particle cross section is designated as "Zr(c)", and the amount of Zr in the surface of the particle cross section is designated as "Zr(s)".
[0153] The amount of Zr in the center of the particle cross section (Zr(c)) and the amount of Zr in the surface of the particle cross section (Zr(s)) obtained by EDX analysis can be substituted into the above-mentioned formula (1) to obtain the degree of dispersion of Zr in the ferrite particles being analyzed.
[0154] In this case, the amount of Zr in the surface region of the particle cross section was defined as four regions enclosed by rectangle R2 defined similarly to rectangle R1, and rectangles R3 and R4 defined based on points Q and Q' defined similarly to points P and P' above for a line Dy passing through center C of the particle cross section and perpendicular to line Dx, and the surface region was determined as the average amount of Zr in each region. Rectangles R1, R2, R3, and R4 were arranged at approximately equal intervals along the contour of the particle cross section.
[0155] Here, when there are multiple line segments Dx, which are the maximum diameters, for one ferrite particle, the line segments Dy (line segment QQ') that have a length of 0.5 or more relative to the line segment Dx are taken as Dx and Dy. The ferrite particles manufactured in each example are approximately spherical. Therefore, when the length of the line segment Dy (line segment QQ') is less than 0.5 relative to the line segment Dx, there is a high probability that such particles are particles that have cracks or chips. Therefore, the ferrite single particle to be analyzed is one in which the length of the line segment Dy (line segment QQ') relative to the line segment Dx is 0.5 or more.
[0156] (4) Moisture content Using a Karl Fischer moisture meter (MKC-510S, Kyoto Electronics Manufacturing Co., Ltd.) of the coulometric titration method, the amount of moisture generated when 2 g of the sample was heated to 230°C with a moisture vaporizer (ADP-511) was measured, and this value was taken as the moisture content of each ferrite particle. When measuring, the sample was exposed to room temperature and humidity (23°C, relative humidity 55%) for 12 hours.
[0157] (5) Amount of chlorine dissolved First, the sample was accurately weighed to within 50.000g + 0.0002g and placed in a 150ml glass bottle. Next, 50ml of phthalate (pH 4.01) was added to the glass bottle. Then, 1ml of ionic strength adjuster was added to the glass bottle and the lid was closed. Then, the sample in the glass bottle was stirred for 10 minutes using a paint shaker. After that, a magnet was placed on the bottom of the 150ml glass bottle, and the carrier was filtered into a PP (50ml) container using No. 5B filter paper, while being careful not to drop it. The voltage of the obtained supernatant was measured with a pH meter. Similarly, solutions with different chlorine concentrations (pure water, 1ppm, 10ppm, 100ppm and 1000ppm) prepared for the calibration curve were measured, and the amount of chlorine dissolved from the sample was calculated from those values.
[0158] (6) Volume average particle size (D 50 ) Volume average particle size (D 50 ) was measured using a Microtrack particle size analyzer (Model 9320-X100) manufactured by Nikkiso Co., Ltd., as follows. The ferrite particles manufactured in each Example and Comparative Example were used as samples, and 10 g of each sample and 80 ml of water were placed in a 100 ml beaker, 2 to 3 drops of a dispersant (sodium hexametaphosphate) were added, and an ultrasonic homogenizer (UH-150 type manufactured by SMT.Co.LTD.) was used with an output level set to 4 to disperse for 20 seconds, and bubbles formed on the surface of the beaker were removed to prepare a sample, and the volume average particle size of the sample was measured using the Microtrack particle size analyzer.
[0159] (7) Saturation magnetization The saturation magnetization was measured using a vibrating sample magnetic measurement device (model: VSM-C7-10A (manufactured by Toei Kogyo Co., Ltd.)). The specific measurement procedure is as follows. First, the ferrite particles produced in each Example and Comparative Example were used as samples, and the samples were filled into a cell with an inner diameter of 5 mm and a height of 2 mm and set in the above-mentioned device. Then, a magnetic field was applied and swept up to 1 K·1000 / 4π·A / m (=1 kOe). Next, the applied magnetic field was reduced, and a hysteresis curve was created on a recording paper. From the data of this curve, the magnetization at an applied magnetic field of 1 K·1000 / 4π·A / m was read and taken as the saturation magnetization.
[0160] (8) BET specific surface area The ferrite particles produced in each Example and Comparative Example were used as samples, and the BET specific surface area was determined using a specific surface area measuring device (Macsorb HM model-1208, Mountec Co., Ltd.) according to the following procedure. First, about 20 g of the sample was placed in a glass petri dish, and then degassed to -0.1 MPa using a vacuum dryer. After degassing and confirming that the degree of vacuum in the glass petri dish had reached -0.1 MPa or less, the sample was heated at 200°C for 2 hours. About 5 to 7 g of the sample subjected to these pretreatments was placed in a standard sample cell dedicated to the specific surface area measuring device. The mass of the sample placed in the standard sample cell was accurately weighed using a precision balance. Then, the standard sample cell containing the sample was set in the measurement port, and the BET specific surface area was measured by the one-point method at a temperature of 10°C to 30°C and a relative humidity of 20% to 80%. The mass of the sample was input at the end of the measurement, and the calculated value was taken as the measured value of the BET specific surface area.
[0161] (9) Charging characteristics Using the carrier for electrophotographic developer produced in each of the Examples and Comparative Examples, an electrophotographic developer was prepared by the following method, and the charge amount was determined.
[0162] The electrophotographic developer carrier and toner produced in each Example and Comparative Example were mixed in a Turbula mixer to obtain 50 g of developer (toner concentration 9.5% by weight). Here, a commercially available negative toner (average particle size about 5.8 μm) used in full-color printers was used as the toner. The developer was exposed to a low-temperature, low-humidity environment (10°C, relative humidity 20%) for 12 hours or more. Thereafter, the developer was placed in a 50 cc glass bottle and stirred at a rotation speed of 100 rpm in the same low-temperature, low-humidity environment. The developer was removed 30 and 60 minutes after the start of stirring to prepare samples for measuring the charge amount.
[0163] The charge measurement device used was a magnetic roll with a total of eight magnets (magnetic flux density 0.1 T) arranged with alternating north and south poles inside a cylindrical aluminum tube (hereinafter referred to as the sleeve) with a diameter of 31 mm and a length of 76 mm, and a cylindrical electrode with a gap of 5.0 mm between it and the sleeve, which was placed on the outer periphery of the sleeve.
[0164] After uniformly attaching 0.5 g of the above sample onto the sleeve, a DC voltage of 2000 V was applied between the outer electrode and the sleeve for 60 seconds while rotating the inner magnet roll at 100 rpm with the outer aluminum tube fixed, and the toner in the developer was transferred to the outer electrode. At this time, an electrometer (KEITHLEY insulation resistance meter model 6517A) was connected to the cylindrical electrode to measure the charge of the transferred toner. After 60 seconds had elapsed, the applied voltage was turned off, the rotation of the magnet roll was stopped, the outer electrode was removed, and the weight of the toner that had transferred to the electrode was measured. The charge amount was calculated from the measured charge amount and the weight of the transferred toner.
[0165] At this time, the charge amount measured for the sample with a stirring time of 30 minutes was defined as the "30 min value (LL)", and the charge amount measured for the sample with a stirring time of 60 minutes was defined as the "60 min value (LL)", and the charge amount change ratio over time was calculated based on the following formula.
[0166] Time-dependent change ratio (%) = (60min value (LL) - 30min value (LL)) / 30min value (LL) x 100
[0167] In addition, after exposing to a high temperature and high humidity environment (30°C, relative humidity 80%) for 12 hours or more in the same manner as above, the developer was stirred in the same high temperature and high humidity environment in the same manner as above, and 60 minutes after the start of stirring, the developer was removed and used as a sample for measuring the charge amount. The charge amount measured for the sample was defined as the "60 min value (HH)", and the environmental variation ratio of resistance was calculated based on the following formula.
[0168] Environmental fluctuation ratio = 60 min value (LL) / 60 min value (HH)
[0169] (10) Image Density The image density was evaluated as follows using the electrophotographic developer manufactured in each Example and Comparative Example. The image density was evaluated by printing 1000 (1k) test images under suitable exposure conditions using a full-color electrophotographic developer (imagio MP C2500 manufactured by Ricoh Corporation) in a constant temperature and humidity room where the atmospheric temperature and humidity were adjusted under a low temperature and low humidity environment (10°C, relative humidity 20%), and then printing a solid image. The image density of the solid image was measured using a spectrophotometric densitometer (Model 938 manufactured by X-Rite Corporation) and evaluated according to the following criteria.
[0170] "◎": 1.3 or higher "○": 1.2 or more and less than 1.3 "△": 1.0 or more and less than 1.2 "x": Less than 1.0
[0171] (11) Coverage The electrophotographic developers manufactured in each of the Examples and Comparative Examples were used to evaluate fogging as follows. Fog was evaluated by printing 10,000 (10k) test images at a print rate of 10% using a full-color electrophotographic developer (imagio MP C2500 manufactured by Ricoh Corporation) in a constant temperature and humidity room where the atmospheric temperature and humidity were adjusted under a high temperature and high humidity environment (30°C, relative humidity 80%), and then measuring the fogging value of the blank area using a color difference meter Z-300A manufactured by Nippon Denshoku Industries Co., Ltd. The average value of the four locations was taken as the measured value, and the density difference from the blank density of the unprinted area was evaluated as follows.
[0172] "◎": 0.05 or less "○": 0.05 or more and 0.1 or less "△": 0.1 or more and 0.3 or less "×": greater than 0.3
[0173] 2. Evaluation results Tables 2 to 4 show the measurement results of each of the above evaluation items.
[0174] (1) Perovskite-type crystal phase component content and Zr element dispersion degree As shown in Table 2, it was confirmed that the ferrite particles of Examples 1 to 8 were obtained by using an oxide containing an alkaline earth metal (R) and zirconium dioxide as raw materials, and thus the ferrite particles contained 0.40 mass % to 0.99 mass % of a perovskite-type crystal phase component represented by the composition formula RZrO3. Also, it was confirmed that the degree of dispersion of Zr in the ferrite particles of Examples 1 to 8 was 1.0, and the perovskite-type crystal phase component was well dispersed in the ferrite particles.
[0175] The ferrite particles obtained in Comparative Examples 1 to 4 also contained 0.44 mass % to 0.52 mass % of the perovskite crystal phase component and had a Zr dispersion degree of 1.0. On the other hand, in Comparative Examples 5 and 6, since "SrO" was not used as a raw material, ferrite particles containing the perovskite crystal component were not obtained.
[0176] (2) Spinel-type crystal phase component content The spinel crystal phase component contents in the ferrite particles of each Example and Comparative Example are as shown in Table 2, and it was confirmed that all of them were spinel ferrite particles containing 90 mass% or more, more specifically 96 mass% or more of the spinel crystal phase component. In addition, when the composition ratio of the spinel crystal phase component was calculated based on the measured value of ICP elemental analysis, it was confirmed that the composition ratio was approximately the same although it varied from the charged molar ratio.
[0177] (3) Zr content (P Zr ), R content (P R ), ratio (P R / P Zr ) From the results of ICP elemental analysis, the ferrite particles of Examples 1 to 8 had a Zr content (P Zr ) is 0.39 mol% to 0.81 mol%, and the Sr content as the R content (P R ) is 0.55mol% to 1.05mol%, and the Ca content as R content (P R ) is 0.56 mol%, and the ratio (P R / P Zr) was confirmed to be in the range of 1.22 to 2.53.
[0178] The ferrite particles of Comparative Examples 1 to 3 have a Zr content (P Zr ), Sr content (P R ) and ratio (P R / P Zr ) was confirmed to be within the range specified by the present invention. In addition, in Comparative Example 4, the Zr content (P Zr ) is within the range specified in the present invention, but the Sr content (P R ) and ratio (P R / P Zr ) was found to be outside the range specified by the present invention. Furthermore, in Comparative Example 5 and Comparative Example 6, the Sr content (P R ) is within the range specified by the present invention, but since no Zr raw material is used, the Zr content (P Zr ) and ratio (P R / P Zr ) does not meet the scope of the present invention.
[0179] (4) Moisture content and amount of dissolved chlorine As shown in Table 3, the moisture content of the ferrite particles in Examples 1 to 8 was 43.9 ppm to 66.7 ppm, which was within the range specified by the present invention. The amount of chlorine dissolved from the ferrite particles in Examples 1 to 8 was 46.0 ppm to 80.0 ppm. Here, when Examples 1 to 3 are compared, the ratio (P R / P Zr There was a tendency that the larger the value of ) the larger the water content and the amount of dissolved chlorine. In contrast to this, the moisture contents of the ferrite particles of Comparative Examples 1 to 6 were all outside the range specified in the present invention, and the amounts of eluted chlorine were also outside the preferred range of the present invention.
[0180] Comparative Example 1 and Comparative Example 2 were produced in the same manner as Example 5, except that the sintering temperature and the distribution of the nitrogen inflow to the temperature rising zone, heating zone, and cooling zone during the atmosphere control in the furnace were different from those in Example 5. During the atmosphere control in the furnace, in Examples 1 to 8, the nitrogen inflow to the temperature rising zone was 40 to 60%, and the nitrogen inflow to the heating zone and cooling zone was 35% to 20%, so that the nitrogen inflow to the temperature rising zone was greater than that of other zones, and the temperature rising zone side was controlled to have a more positive pressure than the heating zone side, whereas in Comparative Example 1 and Comparative Example 2, the nitrogen inflow to the temperature rising zone was 20%, which was less than that of other zones, and the temperature rising zone side was controlled to have a more negative pressure than the heating zone side. As a result, in each Example, the temperature rising zone side was made positive pressure, so that the chlorine gas released from the granules was retained on the heating zone and cooling zone sides, and these zones were adjusted to a chlorine atmosphere, and therefore chlorides such as strontium chloride could be appropriately generated on the particle surface, and it is considered that the moisture content of each ferrite particle was within the specified range of the present invention. On the other hand, in Comparative Example 1 and Comparative Example 2, the temperature rising zone was under negative pressure, so the chlorine gas released from the granules flowed into the temperature rising zone, and it was considered that the heating zone and the cooling zone could not be adjusted to a chlorine atmosphere. As a result, it was considered that the above-mentioned chlorides could not be appropriately generated on the particle surface, and the moisture content and the amount of chlorine dissolved showed low values.
[0181] Comparative Example 3 was produced in the same manner as Example 5, except that the primary calcination was not performed and the distribution of the amount of nitrogen flowing into the temperature rising zone, heating zone, and cooling zone during the atmosphere control in the furnace was slightly different. Since the primary calcination was not performed in Comparative Example 3, the amount of chlorine gas released from the granules into the atmosphere during the main calcination was greater than that in Example 5, and the chlorine concentration in the atmosphere in the heating zone and cooling zone was greater than that in Example 5. Therefore, it is considered that an appropriate amount of chlorides such as strontium chloride was generated on the particle surface, and the amount of chlorine released was greater than that in Examples 1 to 8, and the amount of moisture was greater.
[0182] In Comparative Example 4, the distribution of the nitrogen inflow amount during the atmosphere control was almost the same as in Example 5, but the zirconium content (P Zr ) is the strontium content (PR ) than the ratio (P R / P Zr ) is smaller than the range specified in the present invention. Therefore, although the heating zone and the cooling zone could be adjusted to a chlorine atmosphere, Sr was consumed to form the perovskite crystal phase components, and the amount of Sr for generating chlorides was insufficient, so strontium chloride could not be generated on the particle surface, and in this case too, the amount of chlorine dissolved was less than that in Examples 1 to 8.
[0183] The ferrite particles of Comparative Example 5 had a Zr content (P Zr ) is "0", and does not contain any perovskite crystal phase component. Therefore, it is considered that the Sr contained in the ferrite particles of Comparative Example 5 combines with chlorine in the atmosphere on the particle surface to become strontium chloride, and the amount of chlorine dissolved is larger than that of Examples 1 to 8, and the amount of moisture is larger. On the other hand, Comparative Example 6 has a higher firing temperature than Comparative Example 5, and the BET specific surface area is smaller than that of Comparative Example 6. In Comparative Example 6, the amount of nitrogen flowing into the temperature-raising zone is small, and the heating zone and cooling zone are not in a chlorine atmosphere, so the amount of chlorine dissolved is smaller than that of Comparative Example 5. From these factors, it is considered that the amount of moisture in Comparative Example 6 is smaller.
[0184] (5) BET specific surface area The BET specific surface area of the ferrite particles of Examples 1 to 8 is 0.192 (m 2 / g)~0.325(m 2 / g). In Example 8, R=Ca, and the BET specific surface area was smaller than in the other Examples. In Examples 1 to 7, R=Sr. It was confirmed that the lower the firing temperature (retention temperature), the larger the BET specific surface area tends to be. Furthermore, the firing temperatures in Example 5 and Comparative Examples 1 and 2 were different, and it was also confirmed from the comparison results that the lower the firing temperature, the larger the BET specific surface area.
[0185] (6) Moisture content, amount of dissolved chlorine and BET specific surface area The amount of water adsorbed on the particle surface increases with an increase in the amount of alkaline earth metal chloride produced on the particle surface, resulting in a chemically adsorbed amount, while the amount of water adsorbed increases with an increase in the BET specific surface area. In this regard, the BET specific surface area of Example 5 was the largest among Examples 1 to 8, and the water amount was also the largest. Here, the BET specific surface area of Example 5 was 0.325 (m 2 / g), and the BET specific surface area of Comparative Example 3 is 0.352 (m 2 / g) are approximately equivalent. If we look only at the BET specific surface area, the moisture contents of both are considered to be approximately equivalent, but the moisture content of Comparative Example 3 is as large as 129.3 ppm, whereas the moisture content of Example 5 is suppressed to 66.7 ppm. That is, although the physical adsorption amounts of water are equivalent in Example 5 and Comparative Example 3, it is considered that the moisture content of Comparative Example 3 is large due to the chemical adsorption amount of water based on the difference in the amount of chlorine dissolved (the difference in the amount of chloride generated on the surface of the ferrite particles). Furthermore, the ferrite particles of Comparative Example 6 have an amount of chlorine dissolved of 56.9 ppm, which is approximately the same as the amount of chlorine dissolved of the ferrite particles of Example 3 (55.0 ppm), for example. However, the BET specific surface area of the ferrite particles of Comparative Example 6 is 0.151 (m 2 / g) and the BET specific surface area of Example 3 (0.249 (m 2 / g), and as a result, the moisture content was also low at 28.9 ppm.
[0186] (7) Saturation magnetization and volume average particle size (D 50 ) The saturation magnetization and volume average particle size (D 50 ) are as shown in Table 3. The saturation magnetization of the ferrite particles of Examples 1 to 8 was 59.8 emu / g to 62.6 emu / g, which was within a suitable range for a carrier core material of an electrophotographic developer.
[0187] (8) Charging characteristics Next, the charging characteristics will be described with reference to Table 4. The electrophotographic developers of Examples 1 to 8 measured in a low-temperature, low-humidity environment had a time-varying ratio of 6.99 to 11.09, and an environmental variation ratio of 1.08 to 1.19. In contrast, the electrophotographic developers of Comparative Examples 1, 2, and 4 had a time-varying ratio of 12.67 to 15.38, and an environmental variation ratio of 1.24 to 1.35, all of which were larger than those of the respective Examples. In addition, the electrophotographic developers of Comparative Examples 3 and 5 had a small time-varying ratio of 2.54 to 2.56, but a large environmental variation ratio of 1.45 to 1.50. Furthermore, the electrophotographic developer of Comparative Example 6 had a time-varying ratio of 8.71, which was comparable to that of the electrophotographic developers of Examples 1 to 8, but had a large environmental variation ratio of 1.36.
[0188] From the above results, it was confirmed that the electrophotographic developers of Examples 1 to 8 have smaller time-varying ratios than the electrophotographic developers of Comparative Examples 3 and 5 in which ferrite particles with a high moisture content are used as the core material, and show environmental variation ratios equivalent to those of the electrophotographic developers of Comparative Examples 1, 2, 4, and 6 in which ferrite particles with a low moisture content are used as the core material. That is, it was confirmed that by using the ferrite particles according to the present invention as the core material, the charge amount changes little over time in a low-temperature, low-humidity environment, charge-up can be suppressed, and the charge amount can be prevented from decreasing even when the environment is changed from a low-temperature, low-humidity environment to a high-temperature, high-humidity environment, and the required charge amount can be maintained. That is, it was confirmed that an electrophotographic developer with higher environmental stability can be obtained compared to Comparative Examples 1 to 6.
[0189] In contrast, the electrophotographic developers of Comparative Examples 3 and 5 use ferrite particles with a high moisture content as a core material, and therefore can suppress the change in charge amount over time even in a low-temperature, low-humidity environment, but the environmental fluctuation ratio is large, and it was confirmed that the charge amount decreases in a high-temperature, high-humidity environment. Also, the electrophotographic developers of Comparative Examples 1, 2, 4, and 6 use ferrite particles with a low moisture content as a core material, and therefore although the environmental fluctuation ratio is small compared to Comparative Examples 3 and 5, it is not sufficient compared to each Example, and it was confirmed that the change in charge amount over time in a low-temperature, low-humidity environment cannot be suppressed, and there is a high probability that charge-up occurs.
[0190] (9) Image density and fog From Table 4, it was confirmed that the electrophotographic developers of Examples 1 to 8 have little change in charge amount over time in a low-temperature, low-humidity environment, and charge-up is suppressed, so that practically sufficient image density can be maintained even when a large amount of printing is performed. In addition, it was confirmed that all of them have good fog and can print with high quality in a high-temperature, high-humidity environment. In addition, "△" in the evaluation means that the image density is practically sufficient.
[0191] In contrast, the electrophotographic developers of Comparative Examples 1, 2, 4, and 6, which use ferrite particles with a low moisture content as the core material, were evaluated as "x" for image density, and it was confirmed that there is a high probability that image quality will deteriorate when a large amount of printing is performed in a low-temperature, low-humidity environment. Also, the electrophotographic developers of Comparative Examples 3 and 5, which use ferrite particles with a high moisture content as the core material, were evaluated as "x" for fogging, and it was confirmed that there is a high probability that fogging will occur and image quality will deteriorate in a high-temperature, high-humidity environment.
[0192] [Table 1]
[0193] [Table 2]
[0194] [Table 3]
[0195] [Table 4] [Industrial Applicability]
[0196] According to the present invention, it is possible to provide ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer, each of which has higher environmental stability in terms of charging characteristics.
Claims
1. RZrO 3 Ferrite particles containing a crystalline phase component made of a perovskite-type crystal represented by the following composition formula (wherein R is an alkaline earth metal): The Zr content in the ferrite particles (P Zr ) is 0.35 mol % or more and 1.00 mol % or less, The R content in the ferrite particles (P R ) is 0.50 mol % or more and 1.30 mol % or less, The R content (P R ) and the Zr content (P Zr ) and the ratio (P R / P Zr ) is 1.10 or more and 2.60 or less, Ferrite particles having a moisture content of 30 ppm or more and 70 ppm or less as measured by Karl Fischer titration.
2. 2. The ferrite particles according to claim 1, wherein the R is at least one element selected from the group consisting of Sr, Ca and Ba, and the Ca content is less than 0.1 mol %.
3. 2. The ferrite particles according to claim 1, wherein when a phase composition analysis of the crystal phase constituting the ferrite particles is performed by Rietveld analysis of an X-ray diffraction pattern, the ferrite particles contain 0.05 mass% or more and 1.00 mass% or less of a crystal phase component consisting of the perovskite type crystal.
4. 2. The ferrite particles according to claim 1, wherein the amount of chlorine dissolved therefrom as measured by an elution method is 35 ppm or more and 100 ppm or less.
5. 2. The ferrite particles according to claim 1, wherein, after 12 hours of exposure in a low temperature and low humidity environment (10°C and 20% relative humidity), the charge amount (μC / g) after 30 minutes of stirring is taken as the 30 min value, the charge amount (μC / g) after 60 minutes of stirring is taken as the 60 min value, and the time-dependent variation ratio of the 60 min value to the 30 min value is expressed by the following formula, the time-dependent variation ratio is 5% or more and 10% or less. Time-dependent change ratio (%)=(60 min value−30 min value) / 30 min value×100
6. A carrier core material for an electrophotographic developer, comprising the ferrite particles according to any one of claims 1 to 5.
7. 6. A carrier for electrophotographic developer comprising the ferrite particles according to claim 1 and a resin coating layer provided on the surface of the ferrite particles.
8. 8. An electrophotographic developer comprising the carrier for electrophotographic developer according to claim 7 and a toner.
9. The electrophotographic developer according to claim 8, which is used as a replenishment developer.
Citation Information
Patent Citations
Ventilating fan
JP1983086336A
Electrophotographic developer ferrite carrier core material, ferrite carrier and manufacturing method of electrophotographic developer ferrite carrier core material, and ferrite carrier, and electrophotographic developer ferrite carrier core material using ferrite carrier
JP2016106262A
Ferrite particle, carrier core material for electrophotographic developer, carrier for electrophotographic developer, and electrophotographic developer
WO2022045097A1