Cement composition, method for manufacturing the same, and cement milk
The cement composition with air-cooled slag and polymer addresses the challenge of achieving suitable viscosity and compressive strength for semi-flexible pavements while reducing CO2 emissions by optimizing Blaine specific surface area and CO2 adsorption.
Patent Information
- Application Number
- JP2023058361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cement compositions struggle to achieve both low CO2 emissions and suitable viscosity and compressive strength for forming semi-flexible pavements when using slow-cooled slag as an admixture.
A cement composition containing cement, fine aggregate, and an admixture with air-cooled slag and a polymer, where the Blaine specific surface area and content of the air-cooled slag are within specific ranges, along with CO2 adsorption by the slag, to enhance viscosity and compressive strength.
The cement composition achieves suitable viscosity and compressive strength for semi-flexible pavements while reducing CO2 emissions by optimizing the Blaine specific surface area and CO2 adsorption of the air-cooled slag.
Smart Images

Figure 2024145836000007 
Figure 2024145836000008 
Figure 2024145836000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a cement composition and a method for producing the same, and a cement milk. [Background technology]
[0002] Semi-flexible pavements are pavements that combine the "flexibility" of asphalt pavements with the "rigidity" of concrete pavements, and can be formed by infiltrating a special cement milk into the voids of an open-graded asphalt mix.
[0003] In cement compositions for forming semi-flexible pavement, calcium carbonate is sometimes used as an admixture material with the aim of controlling the physical properties of the hardened body. For example, Patent Document 1 discloses a semi-flexible pavement injection material characterized by containing cement, calcium carbonate powder, re-emulsified powdered resin, and a water-reducing agent, and describes that the semi-flexible pavement injection material solves the problem of providing a semi-flexible pavement injection material that is easy to work with, does not cause settlement of the material during injection, and provides good physical properties of the semi-flexible pavement after injection. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-278901 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a demand for reducing carbon dioxide (CO2) emissions during the production of cement products, and there is still room for further study on admixtures that contribute to reducing CO2 emissions.
[0006] As a result of investigations, the inventors of the present invention considered that air-cooled slag is a promising admixture that contributes to reducing CO2 emissions. However, in the case of a cement composition using air-cooled slag as an admixture, it was particularly difficult to obtain a cement composition suitable for forming a semi-flexible pavement that is excellent in both viscosity when made into cement milk and compressive strength when the hardened body is prepared.
[0007] Therefore, an object of the present disclosure is to provide a cement composition containing an admixture including slowly cooled slag, which makes it possible to obtain a cement milk having a viscosity and compressive strength of the hardened body suitable for forming a semi-flexible pavement. [Means for solving the problem]
[0008] The inventors have discovered that the above problem can be solved by setting the Blaine specific surface area and content of the cooled slag in a cement composition containing cement, fine aggregate, and an admixture, the admixture including cooled slag and a polymer, within specific ranges.
[0009] This disclosure provides the following [1] to
[14] . [1] Contains cement, fine aggregate and admixtures, the admixture comprises annealed slag and a polymer; The Blaine specific surface area of the cooled slag is 2500 to 7500 cm 2 / g, A cement composition comprising 1 to 40 parts by mass of the cooled slag per 100 parts by mass of the total of the cement, the fine aggregate, and the cooled slag. [2] The cement composition according to [1], wherein the mass loss in the range of 590 to 800°C is 1.0 mass% or more in a heat loss curve obtained by thermogravimetric analysis of the cooled slag. [3] The cement composition according to [1] or [2], wherein the amount of inorganic carbon adsorbed to the air-cooled slag is 0.27 mass% or more based on the mass of the air-cooled slag. [4] The density of the cooled slag is 2.80 g / cm 3 The cement composition according to any one of [1] to [3] above. [5] The cement composition according to any one of [1] to [4], wherein the cooled slag is at least one selected from the group consisting of cooled blast furnace slag, cooled converter slag, and cooled electric furnace slag. [6] The cement composition according to any one of [1] to [5], which is mixed with water and used as cement milk for semi-flexible pavement. [7] The cement composition according to any one of [1] to [6], wherein when 50 parts by mass of water are mixed with 100 parts by mass of the cement composition to prepare cement milk, the viscosity of the cement milk at 20°C is 150 to 500 mPa s. [8] The cement composition according to any one of claims [1] to [7], wherein a bleeding rate is 3.50 volume % or less when 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk and the cement milk is allowed to stand for 3 hours. [9] A cement milk comprising the cement composition according to any one of [1] to [8] and water.
[10] The cement milk according to [9], wherein the water content is 40 to 60 parts by mass per 100 parts by mass of the cement composition.
[11] A method for constructing a semi-flexible pavement, comprising filling voids in an asphalt mixture with the cement milk described in [9] or
[10] .
[12] The slowly cooled slag is crushed to reduce the Blaine specific surface area to 2500-7500 cm 2 / g, A method for producing a cement composition, comprising: mixing an admixture containing a polymer and slowly cooled slag having an adjusted Blaine specific surface area, cement, and fine aggregate, A method for producing a cement composition, wherein the amount of the annealed slag is 1 to 40 parts by mass per 100 parts by mass of the total amount of the annealed slag, cement and fine aggregate.
[13] The manufacturing method according to
[12] , further comprising a step of adsorbing 1.0 mass% or more of CO2, based on the mass of the cooled slag, to the cooled slag having an adjusted Blaine specific surface area.
[14] The manufacturing method according to claim
[13] , wherein the CO2 to be adsorbed in the annealed slag comprises CO2 derived from exhaust gas from a cement plant. Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a cement composition containing an admixture including slowly cooled slag, which makes it possible to obtain a cement milk having a viscosity and a compressive strength of a hardened body suitable for forming a semi-flexible pavement. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing the results of X-ray diffraction measurement of the slowly cooled blast furnace slag used in the examples. [Diagram 2] FIG. 2 is a graph showing the change in the mass increase rate of air-cooled blast furnace slag when CO2 is adsorbed onto air-cooled blast furnace slag having a Blaine specific surface area of 3600 cm2 / g. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the following description, when it is written "X to Y" (X and Y are arbitrary numbers), it means "X or more and Y or less" unless otherwise specified.
[0013] Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.
[0014] <Cement composition> One embodiment of the cement composition according to the present disclosure includes cement, fine aggregate, and admixture, the admixture including slowly cooled slag and a polymer. The cement composition may also be referred to as a hydraulic composition.
[0015] Cement means fine powder of mineral matter that reacts with water and hardens. The cement may be Portland cement as specified in JIS R 5210:2009 "Portland cement". The Portland cement may be, for example, ordinary Portland cement, early strength Portland cement, moderate heat Portland cement, low heat Portland cement, etc. In addition, as another cement, for example, it is preferable to use at least one of blast furnace cement as specified in JIS R 5211:2009 "Blast furnace cement" and fly ash cement as specified in JIS R 5213:2019 "Fly ash cement" because it is possible to reduce carbon dioxide emissions during cement production. The cement is preferably at least one of ordinary Portland cement and early strength Portland cement.
[0016] In the above cement composition, the cement content may be 20 parts by mass or more, 30 parts by mass or more, or 33 parts by mass or more, and may be 90 parts by mass or less, or 80 parts by mass or less, per 100 parts by mass of the total of the cement, fine aggregate, and slowly cooled slag.
[0017] In the above cement composition, when the admixture contains a fast-hardening admixture described later, the cement content may be 10 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, or 35 parts by mass or more, per 100 parts by mass of the total of the cement, fine aggregate, slowly cooled slag, and fast-hardening admixture, and may be 90 parts by mass or less, 80 parts by mass or less, 70 parts by mass or less, or 65 parts by mass or less.
[0018] Fine aggregate may be one that passes entirely through a mesh sieve with 10 mm openings and 85% or more by mass through a mesh sieve with 5 mm openings. Examples of fine aggregate include silica sand, river sand, land sand, sea sand, crushed sand, etc. Fine aggregate does not include annealed slag.
[0019] In the above cement composition, the content of the fine aggregate may be 5 parts by mass or more, or 10 parts by mass or more, and may be 30 parts by mass or less, or 20 parts by mass or less, per 100 parts by mass of the total of the cement, fine aggregate, and slowly cooled slag.
[0020] In the above cement composition, when the admixture contains a rapid-hardening admixture described later, the content of the fine aggregate may be 5 parts by mass or more, or 10 parts by mass or more, and may be 30 parts by mass or less, or 20 parts by mass or less, per 100 parts by mass of the total of the cement, fine aggregate, slowly cooled slag, and rapid-hardening admixture.
[0021] Cooled slag is obtained by cooling molten slag generated in the metal manufacturing process, and is different from quenched slag (granulated slag) obtained by quenching molten slag. Cooled slag is amorphous, whereas cooled slag is crystalline. Cooled slag also tends to have a higher density than cooled slag.
[0022] Since the admixture contains a specific slowly cooled slag, an excessive increase in compressive strength is suppressed in the hardened cement milk obtained by using the cement composition containing the admixture. On the other hand, according to the study by the present inventors, when the quenched slag is used instead of the specific slowly cooled slag, such an effect cannot be obtained. Therefore, the cement composition needs to contain the slowly cooled slag instead of the quenched slag.
[0023] The annealed slag may be annealed steel slag generated in the manufacturing process of steel products. Examples of annealed steel slag include blast furnace slag generated in the pig iron manufacturing process, annealed converter slag generated in the steelmaking process using a converter, and annealed electric furnace slag generated in the steelmaking process using an electric furnace. The annealed slag may be one or more selected from the group consisting of blast furnace slag, annealed converter slag, and annealed electric furnace slag.
[0024] The cooled slag may contain SiO2. The SiO2 content in the cooled slag may be 20 mass% or more, 25 mass% or more, or 30 mass% or more, based on the total mass of the cooled slag. The SiO2 content in the cooled slag may be 50 mass% or less, 45 mass% or less, or 40 mass% or less, based on the total mass of the cooled slag. The SiO2 content in the cooled slag may be 20 to 50 mass%, or 30 to 40 mass%.
[0025] The air-cooled slag may contain Al2O3. The content of Al2O3 may be 5 mass% or more, 8 mass% or more, or 10 mass% or more, based on the total mass of the air-cooled slag. The content of Al2O3 may be 20 mass% or less, 17 mass% or less, or 15 mass% or less, based on the total mass of the air-cooled slag. The content of Al2O3 in the air-cooled slag may be 5 to 20 mass%, or 10 to 15 mass%.
[0026] The air-cooled slag may contain CaO. The CaO content may be 20 mass% or more, 30 mass% or more, or 35 mass% or more, based on the total mass of the air-cooled slag. The CaO content may be 60 mass% or less, 50 mass% or less, or 45 mass% or less, based on the total mass of the air-cooled slag. The CaO content in the air-cooled slag may be 20 to 60 mass%, or 35 to 45 mass%.
[0027] The cooled slag may contain MgO. The MgO content may be 1 mass% or more, 3 mass% or more, or 5 mass% or more, based on the total mass of the cooled slag. The MgO content may be 15 mass% or less, 10 mass% or less, or 8 mass% or less, based on the total mass of the cooled slag. The MgO content in the cooled slag may be 1 to 15 mass%, or 5 to 8 mass%.
[0028] The air-cooled slag may further contain one or more selected from the group consisting of Fe2O3, SO3, Na2O, K2O, Ti2O, P2O5, and MnO. The determination of whether or not the air-cooled slag contains SiO2, Al2O3, CaO, MgO, Fe2O3, SO3, Na2O, K2O, Ti2O, P2O5, and MnO and the measurement of the contents of these components can be performed in accordance with JIS R 5202:2010 "Methods for chemical analysis of cement."
[0029] The slowly cooled slag may contain melilite, a solid solution of gehlenite (2CaO·Al2O3·SiO2) and akermanite (2CaO·MgO·2SiO2).
[0030] The Blaine specific surface area of the cooled slag is 2500 to 7500 cm 2 / g. The Blaine specific surface area of the cooled slag is 2700 cm 2 / g or more, 3000cm 2 / g or more, 3200cm 2 / g or more, or 3400 cm 2 / g or more. When the Blaine specific surface area of the air-cooled slag is equal to or greater than the lower limit, it is possible to increase the amount of CO2 adsorption per unit mass of the air-cooled slag, which contributes to reducing the apparent CO2 emissions during the production of the cement composition. The apparent CO2 emissions during the production of the cement composition refer to the value calculated by subtracting the amount of CO2 consumed during the production of the cement composition from the amount of CO2 emitted during the production of the cement composition (including the production of raw materials for the cement composition; the same applies below). The Blaine specific surface area of the air-cooled slag is 7300 cm 2 / g or less, 7000cm 2 / g or less, 6800cm 2 / g or less, 6600cm 2 / g or less, 6400cm 2 / g or less, 6200cm 2 / g or less, 6000cm 2 / g or less, or 5900cm 2 / g or less. When the Blaine specific surface area of the cooled slag is equal to or less than the above upper limit, the viscosity of the cement milk is easily within a range suitable for forming semi-flexible pavement. In this specification, the Blaine specific surface area means a value measured in accordance with the method described in JIS R 5201:2015 "Physical test method for cement".
[0031] The density of the cooled slag is 2.60 g / cm 3 More than 2.70g / cm 3 More than 2.80g / cm 3 or more than 2.90g / cm 3 The density of the slowly cooled slag may be, for example, 5.00 g / cm 3 Below 4.50g / cm 3 or less than 4.00 g / cm 3 It may be the following:
[0032] In this specification, density means true density unless otherwise specified. In this specification, density of slowly cooled slag means density determined by pycnometer method using a fully automatic pycnometer.
[0033] The air-cooled slag is preferably one that has adsorbed CO2. When the air-cooled slag has adsorbed CO2, the apparent CO2 emissions during the production of the cement composition are reduced compared to when only materials that do not adsorb CO2 are used as admixtures. In addition, when the air-cooled slag has adsorbed CO2, the bulk density is smaller compared to when the air-cooled slag does not adsorb CO2. On the other hand, the bulk density of the air-cooled slag is generally larger than the bulk density of calcium carbonate. Therefore, when the air-cooled slag has adsorbed CO2, the bulk density is closer to that of calcium carbonate that has been conventionally used as an admixture, and it is easier to obtain a cement composition having physical properties closer to those of conventional products.
[0034] In the heat loss curve obtained by thermogravimetric analysis of the cooled slag, the mass loss in the range of 590 to 800 ° C may be 0.1 mass % or more, 0.5 mass % or more, 0.8 mass % or more, 1.0 mass % or more, 1.1 mass % or more, 1.3 mass % or more, or 1.5 mass % or more. In the above temperature range, it is considered that desorption of CO2 adsorbed by the cooled slag occurs, so the mass loss corresponds to the amount of CO2 adsorbed by the cooled slag. Therefore, when the mass loss is equal to or more than the lower limit, the apparent CO2 emission during the production of the cement composition is further reduced. In addition, the mass loss in the range of 590 to 800 ° C may be, for example, 32 mass % or less, 20 mass % or less, or 10 mass % or less. More specifically, the mass loss amount is determined by performing thermogravimetric analysis (TG-DTA measurement) under conditions of a nitrogen atmosphere (flow rate: 100 ml / min), a heating rate of 10°C / min, and a measurement temperature range of 20 to 1000°C.
[0035] The amount of inorganic carbon adsorbed to the annealed slag may be 0.10% by mass or more, 0.15% by mass or more, 0.20% by mass or more, 0.25% by mass or more, or 0.27% by mass or more based on the mass of the annealed slag. When the annealed slag adsorbs CO2, the amount of inorganic carbon adsorbed to the slag reflects the amount of CO2 adsorbed by the annealed slag. Therefore, when the amount of inorganic carbon is equal to or more than the lower limit, the apparent amount of CO2 emitted during the production of the cement composition is further reduced. In addition, the amount of inorganic carbon adsorbed to the annealed slag may be 9% by mass or less, 5% by mass or less, or 3% by mass or less based on the mass of the annealed slag. The amount of inorganic carbon is determined using a total organic carbon meter equipped with a solid sample combustion device.
[0036] In the above cement composition, the content of the annealed slag is 1 to 40 parts by mass relative to 100 parts by mass of the total of the cement, fine aggregate, and annealed slag. The content of the annealed slag may be 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, 9 parts by mass or more, 10 parts by mass or more, 13 parts by mass or more, 17 parts by mass or more, or 20 parts by mass or more relative to 100 parts by mass of the total of the cement, fine aggregate, and annealed slag. When the content of the annealed slag is equal to or more than the above lower limit, the compressive strength and bending strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement. The content of the annealed slag may be 39 parts by mass or less, 38 parts by mass or less, or 37 parts by mass or less relative to 100 parts by mass of the total of the cement, fine aggregate, and annealed slag. When the content of the annealed slag is equal to or less than the above upper limit, the compressive strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement.
[0037] In the above cement composition, the content of the annealed slag relative to 100 parts by mass of cement may be 5 parts by mass or more, 7 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, or 30 parts by mass or more. When the content of the annealed slag is equal to or more than the above lower limit, the compressive strength and bending strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement. The content of the annealed slag relative to 100 parts by mass of cement may be equal to or less than 90 parts by mass, equal to or less than 80 parts by mass, or equal to or less than 75 parts by mass. When the content of the annealed slag is equal to or less than the above upper limit, the compressive strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement.
[0038] In the above cement composition, when the admixture contains a rapid hardening admixture described later, the content of the annealed slag relative to 100 parts by mass of the cement and the rapid hardening admixture may be 5 parts by mass or more, 7 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, or 30 parts by mass or more. When the content of the annealed slag is equal to or more than the above lower limit, the compressive strength and bending strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement. The content of the annealed slag relative to 100 parts by mass of the cement and the rapid hardening admixture may be 90 parts by mass or less, 80 parts by mass or less, or 75 parts by mass or less. When the content of the annealed slag is equal to or less than the above upper limit, the compressive strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement.
[0039] In the above cement composition, when the admixture contains a rapid hardening admixture described later, the content of the annealed slag may be 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 7 parts by mass or more, 10 parts by mass or more, 13 parts by mass or more, 17 parts by mass or more, or 20 parts by mass or more, based on a total of 100 parts by mass of the cement, fine aggregate, annealed slag, and rapid hardening admixture. When the content of the annealed slag is equal to or more than the above lower limit, the compressive strength and bending strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement. The content of the annealed slag may be 40 parts by mass or less, 39 parts by mass or less, 38 parts by mass or less, or 37 parts by mass or less, based on a total of 100 parts by mass of the cement, fine aggregate, annealed slag, and rapid hardening admixture. When the content of the annealed slag is equal to or less than the above upper limit, the compressive strength of the obtained cement milk when hardened tend to be more suitable for the formation of semi-flexible pavement.
[0040] The polymer may be a known polymer for cement, a polymer for cement admixture, or the like. The polymer may be, for example, at least one selected from the group consisting of a re-emulsified powder polymer, a water-soluble polymer, and a liquid polymer. Examples of the re-emulsified powder polymer include vinyl acetate-based polymers and acrylic acid ester-based polymers. Examples of the vinyl acetate-based polymer include ethylene vinyl acetate and vinyl acetate vinyl versatate (VAVeoVa). Examples of the acrylic acid ester-based polymer include styrene acrylic acid ester and polyacrylic acid ester. Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, and polyacrylates. Examples of the cellulose derivatives include methyl cellulose and hydroxypropyl methyl cellulose. Examples of the polyacrylates include calcium polyacrylate and magnesium polyacrylate. Examples of the liquid polymer include unsaturated polyester resins and epoxy resins.
[0041] In the above cement composition, the polymer content may be 0.1 parts by mass or more, 0.5 parts by mass or more, or 0.7 parts by mass or more per 100 parts by mass of the total of the cement, the fine aggregate, and the air-cooled slag, and the polymer content may be 5 parts by mass or less, 3 parts by mass or less, or 2 parts by mass or less per 100 parts by mass of the total of the cement, the fine aggregate, and the air-cooled slag.
[0042] In the cement composition, the content of the polymer relative to 100 parts by mass of the cement may be 0.5 parts by mass or more, 0.8 parts by mass or more, or 1.0 parts by mass or more. The mass ratio may be 5.0 parts by mass or less, 4.0 parts by mass or less, or 3.0 parts by mass or less.
[0043] The admixture may include a rapid hardening admixture. Rapid hardening can be imparted to the cement milk by replacing part of the cement with the rapid hardening admixture. The rapid hardening admixture may be a mixture of calcium aluminate and gypsum.
[0044] The calcium aluminate may be 12CaO·7Al2O3, 3CaO·Al2O3, or CaO·Al2O3. The Blaine specific surface area of calcium aluminate is 4000 cm 2 / g or more, and 2 / g or less. The gypsum may be hydrofluoric gypsum (gypsum produced as a by-product in the manufacture of hydrofluoric acid) or natural gypsum. The gypsum may be anhydrous gypsum (CaSO4), hemihydrate gypsum (CaSO4·1 / 2H2O), or dihydrate gypsum (CaSO4·2H2O), but is preferably anhydrous gypsum (CaSO4). The anhydrous gypsum may be type II anhydrous gypsum or type III anhydrous gypsum. The Blaine specific surface area of the gypsum is 8000 cm 2 / g or more, 2 / g or less.
[0045] In the mixture of calcium aluminate and gypsum, the mass ratio of the calcium aluminate content to the gypsum content (calcium aluminate content / gypsum content) may be 30 / 70 or more, 35 / 65 or more, or 40 / 60 or more, and the ratio may be 70 / 30 or less, 60 / 40 or less, 55 / 45 or less, or 50 / 50 or less.
[0046] The content of the fast-setting admixture may be 10 parts by mass or more, 15 parts by mass or more, or 18 parts by mass or more, based on 100 parts by mass of the total of the cement and the fast-setting admixture. The content of the fast-setting admixture may be 40 parts by mass or less, 35 parts by mass or less, or 32 parts by mass or less, based on 100 parts by mass of the total of the cement and the fast-setting admixture.
[0047] The admixture may contain other components (hereinafter simply referred to as "other components") other than the cooled slag, the fast-hardening admixture, and the polymer. Examples of the other components include thickeners, antifoaming agents, water reducing agents, air-enhancing agents, water retention agents, hardening accelerators, setting regulators (setting retarders, etc.), rebar rust inhibitors, expanding agents, silica fume, etc. The content of the other components may be 0.01 parts by mass or more and 0.3 parts by mass or less relative to 100 parts by mass of the total of the cement, fine aggregate, and cooled slag.
[0048] The cement composition can be mixed with water to prepare cement milk. The cement milk obtained by mixing the cement composition with water is suitable for semi-flexible pavement. Therefore, the cement composition may be mixed with water and used as cement milk for semi-flexible pavement.
[0049] When 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk, the viscosity of the cement milk at 20°C may be 150 to 500 mPa·s. The viscosity may be 200 to 400 mPa·s, or may be 250 to 400 mPa·s. When the viscosity is equal to or greater than the lower limit, the occurrence of bleeding is easily suppressed. When the viscosity is equal to or less than the upper limit, the filling property of the cement milk tends to be improved. The viscosity of the cement milk at 20°C means a value measured by a B-type viscometer. More specifically, the viscosity of the cement milk at 20°C is measured by the method described in the Examples.
[0050] When 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare cement milk and the cement milk is left for 3 hours, the bleeding rate may be 3.50% by volume or less. The bleeding rate may be 3.30% by volume or less, 3.00% by volume or less, or 2.70% by volume or less.
[0051] The bleeding rate means a value obtained by the following method. In an environment of 20±3°C, 1000 mL of cement milk is poured into a watertight and strong container, the container is covered, and the container is left on a horizontal table for 3 hours from the time of pouring water during the production of the cement milk. The amount of water that seeps out onto the surface (bleeding water amount) is measured in 1 mL units. Based on the measured value, the bleeding rate is calculated by the following formula. More specifically, the bleeding rate is measured by the method described in the Examples. The bleeding rate value is rounded off to two decimal places to obtain a value to two decimal places. Bleeding rate (volume%) = (Bleeding water volume (mL) / 1000mL) x 100
[0052] <Cement milk> One embodiment of the cement milk according to the present disclosure includes the above-mentioned cement composition and water. The content of water may be 20 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more, relative to 100 parts by mass of the cement composition. The content of water may be 80 parts by mass or less, 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, relative to 100 parts by mass of the cement composition. The content of water may be 30 to 70 parts by mass, or 40 to 60 parts by mass.
[0053] As described above, the cement milk obtained by mixing the cement composition with water is suitable for semi-flexible pavement. The present disclosure can also be said to provide a method for constructing semi-flexible pavement, which includes filling voids in an asphalt mixture with the cement milk. The asphalt mixture may be, for example, a mixture of aggregate (crushed stone, sand, etc.), filler (stone powder, etc.), and asphalt. The construction method may include spreading the asphalt mixture evenly. In the spread asphalt mixture, voids exist between particles of aggregate, etc. A semi-flexible pavement can be constructed by filling voids in the asphalt mixture with cement milk and then hardening the cement milk.
[0054] <Method of manufacturing cement composition> In one embodiment of the method for producing a cement composition according to the present disclosure, cooled slag is crushed to have a Blaine specific surface area of 2500 to 7500 cm 2 / g (hereinafter also referred to as the "specific surface area adjusting step"), and a step of mixing an admixture containing a polymer and slow-cooled slag whose Blaine specific surface area has been adjusted, cement, and fine aggregate (hereinafter also referred to as the "mixing step").
[0055] In the specific surface area adjustment step, the cooled slag used as a raw material may be any of the cooled slags described above as the admixtures in the cement composition. The density of the cooled slag used as a raw material may be within the range described above as the density range of the cooled slags included in the admixtures in the cement composition.
[0056] Usually, the annealed slag used as the raw material is commercially available with large particle size and small Blaine specific surface area. In the specific surface area adjustment process, the raw annealed slag is crushed to adjust the Blaine specific surface area to 2500-7500 cm. 2 / g, the Blaine specific surface area of the cooled slag is adjusted. 2 / g or more, 3000cm 2 / g or more, 3200cm 2 / g or more, or 3400 cm 2 / g or more. By adjusting the Blaine specific surface area of the air-cooled slag to the above lower limit or more, it is possible to increase the CO2 adsorption amount per unit mass of the air-cooled slag, which contributes to reducing the apparent CO2 emissions during the production of the cement composition. In addition, in the above process, the Blaine specific surface area may be adjusted to 7300 cm 2 / g or less, 7000cm 2 / g or less, 6800cm 2 / g or less, 6600cm 2 / g or less, 6400cm 2 / g or less, 6200cm 2 / g or less, 6000cm 2 / g or less, or 5900cm 2 By adjusting the Blaine specific surface area of the cooled slag to the above upper limit or less, the viscosity of the cement milk produced using the produced cement composition can be made to fall within a range more suitable for forming semi-flexible pavement.
[0057] The admixture used in the mixing step includes a polymer and cooled slag with an adjusted Blaine specific surface area. As the polymer, the polymer described above as the polymer in the cement composition can be used. The amount of the polymer to be mixed with 100 parts by mass of the cooled slag with an adjusted Blaine specific surface area, the cement, and the fine aggregate may be within the numerical range described above as the polymer content to 100 parts by mass of the cooled slag, the cement, and the fine aggregate in the cement composition. The amount of the polymer to be mixed with 100 parts by mass of the cement may be within the numerical range described above as the polymer content to 100 parts by mass of the cement in the cement composition.
[0058] It is preferable to adsorb CO2 to the cooled slag having the adjusted Blaine specific surface area. The above-mentioned production method may further include a step of adsorbing 1.0 mass% or more of CO2 based on the mass of the cooled slag to the cooled slag having the adjusted Blaine specific surface area (hereinafter, also referred to as a "CO2 adsorption step"). The CO2 adsorption step may be performed before the blending step or after the blending step.
[0059] An example of a method for allowing the cooled slag with an adjusted Blaine specific surface area to adsorb 1.0 mass% or more of CO2 based on the mass of the cooled slag is to leave the cooled slag with an adjusted Blaine specific surface area in a tank set to a high CO2 concentration (e.g., 1000 ppm or more). The period of leaving the slag may be, for example, 30 days or more and 60 days or less. In the CO2 adsorption step, the CO2 adsorbed by the cooled slag may include CO2 derived from exhaust gas from a cement plant.
[0060] In the CO2 adsorption step, the amount of CO2 adsorbed in the annealed slag is 1.0 mass% or more, based on the mass of the annealed slag, and may be 1.1 mass% or more, 1.3 mass% or more, or 1.5 mass% or more. The amount of CO2 adsorbed in the annealed slag may be, for example, 3.5 mass% or less. The amount of CO2 adsorbed in the annealed slag is determined as the mass loss in the range of 590 to 800 °C in a heat loss curve obtained by thermogravimetric analysis of the annealed slag having adsorbed CO2 (after the CO2 adsorption step).
[0061] In a heat loss curve obtained by thermogravimetric analysis of the cooled slag having an adjusted Blaine specific surface area, the mass loss in the range of 590 to 800°C may be within the above-mentioned numerical range for the mass loss in the range of 590 to 800°C in the heat loss curve obtained by thermogravimetric analysis of the cooled slag in the cement composition. In addition, the amount of inorganic carbon adsorbed in the cooled slag having an adjusted Blaine specific surface area may be within the above-mentioned numerical range for the amount of inorganic carbon adsorbed in the cooled slag in the cement composition.
[0062] The amount of the cooled slag with an adjusted Blaine specific surface area is 1 to 40 parts by mass relative to 100 parts by mass of the total amount of the cooled slag, cement, and fine aggregate. The amount of the cooled slag with an adjusted Blaine specific surface area relative to 100 parts by mass of the total amount of the cooled slag, cement, and fine aggregate may be within the above-mentioned numerical range as the content of the cooled slag relative to 100 parts by mass of the total amount of the cooled slag, cement, and fine aggregate in the cement composition.
[0063] The amount of annealed slag with an adjusted Blaine specific surface area per 100 parts by mass of cement may be within the numerical range described above as the content of annealed slag per 100 parts by mass of cement in the above cement composition.
[0064] When the admixture contains a rapid-hardening admixture, the amount of the slow-cooled slag with adjusted Blaine specific surface area per 100 parts by mass of the combined amounts of the slow-cooled slag with adjusted Blaine specific surface area, the rapid-hardening admixture, cement, and fine aggregate may be within the numerical range described above as the content of the slow-cooled slag per 100 parts by mass of the combined amounts of the slow-cooled slag, the rapid-hardening admixture, cement, and fine aggregate in the cement composition.
[0065] The amount of cooled slag with adjusted Blaine specific surface area per 100 parts by mass of cement and rapid-hardening admixture may be within the above-mentioned numerical range as the content of cooled slag per 100 parts by mass of the total of cement and rapid-hardening admixture in the cement composition.
[0066] The admixture may include a fast-setting admixture and may include other components. As the fast-setting admixture and other components, the fast-setting admixture and other components described above as the fast-setting admixture and other components in the cement composition can be used, respectively.
[0067] The amount of the rapid-hardening admixture per 100 parts by mass of the total amount of the cement and the rapid-hardening admixture in the cement composition may be within the above-mentioned numerical range as the content of the rapid-hardening admixture per 100 parts by mass of the total amount of the cement and the rapid-hardening admixture.
[0068] The amount of other components to be mixed per 100 parts by mass of the total of the cooled slag, cement, and fine aggregate having an adjusted Blaine specific surface area may be within the above-mentioned numerical range as the content of other components based on 100 parts by mass of the total of the cooled slag, cement, and fine aggregate in the above cement composition.
[0069] As the cement and the fine aggregate, the cement and the fine aggregate described above as the cement and the fine aggregate in the cement composition can be used, respectively.
[0070] The amounts of cement and fine aggregate per 100 parts by mass of the total of the cooled slag, cement, and fine aggregate having an adjusted Blaine specific surface area may be within the numerical ranges described above as the contents of cement and fine aggregate per 100 parts by mass of the total of the cooled slag, cement, and fine aggregate in the above cement composition.
[0071] When the admixture contains a rapid-hardening admixture, the amounts of cement and fine aggregate per 100 parts by mass of the combined amounts of the cooled slag with adjusted Blaine specific surface area, the rapid-hardening admixture, cement, and fine aggregate may be within the numerical ranges described above as the contents of cement and fine aggregate per 100 parts by mass of the combined amounts of the cooled slag, the rapid-hardening admixture, cement, and fine aggregate in the cement composition. EXAMPLES
[0072] The present disclosure will be described in more detail below with reference to examples, comparative examples, and reference examples. However, the present disclosure is not limited to the following examples.
[0073] In the following Examples, Comparative Examples, and Reference Examples, the components shown in Table 1 below were used as raw materials.
[0074] [Table 1]
[0075] [Preparation and analysis of cooled slag] <Adjustment of Blaine specific surface area> The blast furnace slag was crushed using a crushing device (HERZOG HP-MA) to obtain a Blaine specific surface area of 2000 cm 2 The Blaine specific surface area of the slag was 3600, 5000, and 8000 cm2 by changing the operating conditions of the grinding machine. 2 The Blaine specific surface area was measured in accordance with the method described in JIS R 5201:2015 "Physical test methods for cement."
[0076] <Analysis> Blaine specific surface area is 3600cm 2 X-ray diffraction measurements were performed on air-cooled blast furnace slag with a specific surface area of 3600 cm2 / g. The results are shown in Figure 1. As shown in Figure 1, the X-ray diffraction pattern of melilite was observed, indicating that the air-cooled blast furnace slag contains melilite. In addition, in accordance with JIS R 5202:2010 "Methods for chemical analysis of cement," the Blaine specific surface area was 3600 cm2. 2 The chemical composition of the slowly cooled blast furnace slag with a Blaine specific surface area of 3600 cm was determined. The results are shown in Table 2. 2 The true density of the cooled blast furnace slag, which has a density of 3.00 g / cm3, was measured using an automatic pycnometer (manufactured by Anton Paar Japan Co., Ltd., product name "Automatic Pycnometer Pentapyc5200e"). As a result, the true density was 3.00 g / cm3. 3 For reference, the ignition loss (sometimes written as ig. loss) values are also shown in Table 2. The ignition loss was measured in accordance with the method described in "5.3 For blast-furnace cement and blast-furnace slag" in "5. Quantitative method for ignition loss" of JIS R 5202:2010.
[0077] [Table 2]
[0078] <CO2 adsorption into slowly cooled blast furnace slag> Blaine specific surface areas of 2000, 3600, 5000, and 8000 cm 2 The following treatment was carried out for each of the slowly cooled blast furnace slags with a sample size of 1000 g / m2 / g. The slowly cooled blast furnace slags were placed in a container, spread evenly inside the container, and placed on the bottom two shelves of a sealable test tank with three shelves. After that, the slags were placed in polyethylene bags (CO2 permeability: 20-30 g / m2) filled with CO2 at a concentration of 99.9% by volume or more. 2 The tank was sealed and left for 49 days to allow the blast furnace slag to adsorb and absorb CO2. The CO2 concentration in the layer was 2000 ppm (0.2 vol%) or more.
[0079] <Mass increase behavior due to CO2 adsorption> In the above method, when CO2 was adsorbed on the slowly cooled blast furnace slag with a Blaine specific surface area of 3600 cm 2 / g for 49 days, the change in the mass increase rate of the slowly cooled blast furnace slag ({(mass of the slowly cooled blast furnace slag at each time point - mass of the slowly cooled blast furnace slag before CO2 adsorption) / mass of the slowly cooled blast furnace slag before CO2 adsorption}×100) is shown in Figure 2. As shown in Figure 2, the mass increase rate reached a constant value in about 30 days. Similarly, for the slowly cooled blast furnace slag with Blaine specific surface areas of 2000, 5000, and 8000 cm 2 / g, the mass increase rate also reached a constant value in about 30 days.
[0080] <Thermogravimetric analysis of CO2 adsorption amount> After adsorbing CO2 by the above method, for the slowly cooled blast furnace slag with Blaine specific surface areas of 2000, 3600, 5000, and 8000 cm 2 / g, thermogravimetric analysis (TG-DTA measurement) was carried out under a nitrogen atmosphere (flow rate: 100 ml / min) at a heating rate of 10 °C / min and a measurement temperature range of 20 to 1000 °C. In the obtained thermogravimetric curve, the mass reduction amount in the range of 590 to 800 °C was determined. The results are shown in Table 3.
[0081] <Analysis of inorganic carbon content> After adsorbing CO2 by the above method, for the slowly cooled blast furnace slag with Blaine specific surface areas of 2000, 3600, 5000, and 8000 cm 2 / g, the inorganic carbon content was determined using a total organic carbon meter equipped with a solid sample combustion device (manufactured by Shimadzu Corporation, trade name "TOC-L type, SSM-5000A型"). More specifically, phosphoric acid was added to the slowly cooled blast furnace slag until the pH of the supernatant liquid became 3 or less and mixed. By heating the obtained mixture at 200 °C, CO2 was released, and the inorganic carbon content was measured by an NDIR detector, and the inorganic carbon content based on the mass of the slowly cooled blast furnace slag used in the measurement was calculated. The results are shown in Table 3.
[0082]
Table 3
[0083] [Production of Cement Composition and Cement Milk] Cement compositions (cement compositions according to Comparative Examples 1-1 to 1-4, Reference Examples 1-1 to 1-3, and Examples 1-1 to 1-4) composed of the respective components shown in Tables 4 and 5 were produced. The blending ratios of the respective components are as shown in Tables 4 and 5. The "-" in Tables 4 and 5 indicates that the corresponding component was not blended. Further, 50 parts by mass of water was added to 100 parts by mass of each cement composition, and using a Three One Motor BL1200 (with turbine blades), kneading was performed at a rotational speed of 800 rpm for 2 minutes to prepare cement milk according to Comparative Examples 1-1 to 1-4, Reference Examples 1-1 to 1-3, and Examples 1-1 to 1-4.
[0084] [Evaluation] The following tests were conducted on the produced cement milk and cement compositions, and the evaluation values in each test were determined. The results are shown in Tables 4 and 5. Also, for reference, the suitable ranges of each evaluation value are shown in Table 6.
[0085] [Viscosity] The viscosity of the cement milk immediately after production (within 60 seconds after production) was measured using a B-type rotational viscometer (manufactured by BROOK FIELD, product name "LVDV-A"). The measurement was carried out in an environment at room temperature of 20°C.
[0086] [P-Funnel Flow Time] In accordance with JSCE-F521-1999 "Test Method for Fluidity of Injection Mortar for Prepacked Concrete (Method Using P-Funnel)", the P-funnel flow time of the cement milk was measured. The measurement was carried out in an environment at room temperature of 20°C.
[0087] [Bleeding Rate] A watertight and sturdy container with a capacity of 1000 mL (manufactured by AS ONE Corporation, product name "Disposable Cup (Blow Molding) 1000 mL") was prepared. The following test was performed in an environment of 20 ± 3 ° C. Cement milk was poured into the prepared container up to the 1000 mL line, and the container was lightly tapped so that the surface of the sample was smooth. Next, the container containing the sample was placed on a horizontal stand that did not vibrate, and the lid was covered with a plastic plate. During the test, the lid was always on except when water was being sucked up. After 3 hours had passed from the time of pouring water during the production of cement milk, the water that had seeped out onto the surface of the sample was sucked up. The amount of water sucked up (bleeding water amount) was measured in 1 mL units using a measuring cylinder. Based on the results of the above tests, the bleeding rate was calculated using the following formula. The value was rounded off to two decimal places to obtain a value with two decimal places. Bleeding rate (volume%) = (Bleeding water volume (mL) / 1000mL) x 100
[0088] <Condensation time> The setting time (initial and final setting) was calculated according to JIS R 5201:2015 9.4.3 "Measurement of initial and final setting of setting". However, the measurement interval was 10 minutes.
[0089] <Compressive strength and flexural strength of hardened body> The above cement milk was used instead of the specified mortar for the preparation of the test specimens, and 4cm x 4cm x 16cm test specimens were prepared in accordance with JIS R 5201:2015. However, the test specimens were prepared by pouring the cement milk, demolded the next day, and cured in water for 7 days, and the compressive strength and flexural strength of the test specimens (hardened bodies) were measured at 7 days. The tests were conducted in an environment at room temperature of 20℃.
[0090] [Table 4]
[0091] [Table 5]
[0092] [Table 6]
[0093] As shown in Table 5, it was confirmed that the cement milk prepared in Examples 1-1 to 1-4 all exhibited viscosity and compressive strength of the hardened body suitable for forming a semi-flexible pavement. In addition, when the evaluation value is within the suitable range shown in Table 6, it can be said that the cement milk is particularly suitable for forming a semi-flexible pavement.
Claims
1. Contains cement, fine aggregate and admixtures, the admixture comprises annealed slag and a polymer; The Blaine specific surface area of the slowly cooled slag is 2500 to 7500 cm 2 / g, The content of the slowly cooled slag is 1 to 40 parts by mass per 100 parts by mass of the total of the cement, the fine aggregate, and the slowly cooled slag.
2. The cement composition according to claim 1, wherein the mass loss curve obtained by thermogravimetric analysis of the cooled slag is 1.0 mass% or more in the range of 590 to 800 ° C.
3. 3. The cement composition according to claim 1, wherein the amount of inorganic carbon adsorbed to the cooled slag is 0.27 mass% or more based on the mass of the cooled slag.
4. The density of the slowly cooled slag is 2.80 g / cm 3 The cement composition according to claim 1 or 2.
5. 3. The cement composition according to claim 1, wherein the cooled slag is at least one selected from the group consisting of cooled blast furnace slag, cooled converter slag, and cooled electric furnace slag.
6. 3. The cement composition according to claim 1 or 2, which is mixed with water and used as a cement milk for semi-flexible paving.
7. The cement composition according to claim 1 or 2, wherein the viscosity of the cement milk at 20°C is 150 to 500 mPa·s when 50 parts by mass of water is mixed with 100 parts by mass of the cement composition to prepare the cement milk.
8. 3. The cement composition according to claim 1 or 2, wherein the bleeding rate is 3.50 vol% or less when 50 mass parts of water are mixed with 100 mass parts of the cement composition to prepare cement milk and the cement milk is allowed to stand for 3 hours.
9. A cement milk comprising the cement composition according to claim 1 or 2 and water.
10. The cement milk according to claim 9, wherein the water content is 40 to 60 parts by mass per 100 parts by mass of the cement composition.
11. A method for constructing a semi-flexible pavement, comprising filling voids in an asphalt mixture with the cement milk according to claim 9.
12. The slowly cooled slag is crushed to have a Blaine specific surface area of 2500 to 7500 cm 2 / g; A method for producing a cement composition, comprising: mixing an admixture containing a polymer and the cooled slag having an adjusted Blaine specific surface area, cement, and fine aggregate, A method for producing a cement composition, wherein the amount of the annealed slag is 1 to 40 parts by mass per 100 parts by mass of the total of the annealed slag, the cement, and the fine aggregate.
13. The cooled slag having the adjusted Blaine specific surface area is added with 1.0 mass% or more of CO based on the mass of the cooled slag. 2 The method of claim 12, further comprising the step of adsorbing
14. The CO adsorbed on the slowly cooled slag 2 However, CO from exhaust gases from cement factories 2 The method of claim 13, comprising:
Citation Information
Patent Citations
Half-flexible grouting material and pavement construction using the same