Quartz glass
Quartz glass with controlled composition and properties effectively suppresses particle generation during etching, enhancing semiconductor manufacturing yield by minimizing surface unevenness and contamination.
Patent Information
- Application Number
- JP2023058456
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Quartz glass members used in semiconductor manufacturing are etched by fluorocarbon gases, leading to particle generation that contaminates the semiconductor chip and lowers yield, despite existing countermeasures.
Manufacture quartz glass with specific composition and properties, such as low metal impurities (0.1 ppm) and amorphous structure, using synthetic silica powder sintered under controlled conditions to suppress particle generation during etching.
The quartz glass exhibits excellent etching resistance, minimizing surface unevenness and particle generation, thereby improving semiconductor manufacturing yield.
Smart Images

Figure 2024145889000001
Abstract
Description
[Technical field]
[0001] The present invention relates to quartz glass. [Background technology]
[0002] In the dry etching process of semiconductor manufacturing, quartz glass members are used because of their heat resistance and corrosion resistance, but just like the etching target, the quartz glass members themselves are etched by the action of fluorocarbon etching gases. When the quartz glass members are etched, particles that are generated during the etching process adhere to the semiconductor chips being processed or cause contamination inside the equipment, which reduces the yield of the semiconductor manufacturing process.
[0003] There are two known ways to deal with particles: "controlling the amount of particles generated by equipment and process conditions" and "giving etching resistance to quartz glass members" (see Patent Document 1 and Non-Patent Document 1).
[0004] However, even with these measures, particles continue to be generated, hindering improvements in yield. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-045699 A [Patent Document 2] JP 2004-142996 A [Non-patent literature]
[0006] [Non-Patent Document 1] Particle reduction and control in plasma etching equipment, T. Moriya, H. Nakayama, H. Nagaike, Y. Kobayashi, M. Shimada and K. Okuyama, IEEE Trans. Semicond. Manufact., 18, 477 (2005) Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide quartz glass having excellent etching resistance that suppresses the generation of particles during etching. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems based on an understanding of the etching mechanism of silica by fluorocarbon-based etching gases, and have found that the above problems can be solved by keeping the composition of particles generated during etching within a specific range, thereby arriving at the present invention. That is, the present invention is as follows.
[0009] [1] Gas type: CHF 3 When the particles generated during etching for 4 hours were analyzed by EDS under the conditions of ICP power 200 W, pressure 1.8 Pa, and flow rate 30 sccm, the measurement area was 0.96 mm 2 The detection signal strength of Al and Cl is 30 cps / eV or less in the range.
[0010] [2] The quartz glass of [1], wherein the amount of metal impurities in the quartz glass is 0.1 ppm or less.
[0011] [3] The quartz glass according to [1] or [2], wherein the quartz glass is amorphous. Effect of the Invention
[0012] According to the present invention, it is possible to obtain quartz glass having excellent etching resistance that suppresses the generation of particles during etching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The following describes in detail the embodiments of the present invention, but the present invention is not limited to the following embodiments and can be modified in various ways within the scope of the invention.
[0014] Approximately 90% of quartz components used in semiconductor processing are quartz glass derived from natural quartz, which inherently contains trace amounts of metal impurities on the ppm order, with aluminum (Al) being a prime example. Metal impurities such as Al are expressed as SiO 2 Since fluorocarbon gases have a higher etching resistance than metal gases, the etching speed differs between areas where metal is concentrated and areas where it is not during the etching process, resulting in unevenness on the surface of the quartz glass. When the unevenness on the quartz glass surface becomes large, relatively sharp areas called sharp edges appear, and these sharp edges periodically chip away from the main body of the quartz glass, generating silica particles.
[0015] Al combines with fluorine (F) in fluorocarbon gases and remains as a low-volatility solid. This solid also causes particles.
[0016] Differences in crystallinity can also be cited as a factor that causes differences in etching speed. Natural quartz is originally crystalline, and although some of its crystallinity is lost during the vitrification process, it does not completely lose its crystallinity. Generally, crystalline silica has greater etching resistance than amorphous silica, so differences in etching speed occur between the crystalline and non-crystalline (amorphous) parts of the quartz glass, resulting in the appearance of unevenness on the surface.
[0017] In this way, when quartz glass containing metal impurities is etched with fluorocarbon gas, a certain number of silica particles originating from the sharp edges and particles of combined compounds of Al and F are generated, and this state can be confirmed by detecting Al with a SEM-EDS (scanning electron microscope equipped with an energy dispersive X-ray detector).
[0018] On the other hand, SiCl 4 Synthetic quartz glass produced by gas phase synthesis, in which silica fume is produced from gas and then fired, does not contain metal impurities, but a certain amount of Cl from the raw gas remains on the order of ppm. This synthetic quartz glass has very fine pores due to its manufacturing process, but in the state of ordinary commercial quartz components, it is difficult to see the pores with a microscope.
[0019] However, the pores in this synthetic quartz glass are enhanced by etching using fluorocarbon gas, and grow to the order of 10 μm. At this time, unevenness appears on the surface of the synthetic quartz glass, and particles originating from sharp edges are generated as described above. Since pores exist in areas where Cl is unevenly distributed, Cl can be detected from these particles. Therefore, this state can be confirmed by detecting Cl with SEM-EDS.
[0020] When quartz glass that is free of metal impurities, Cl, bubbles, etc. is etched with fluorocarbon gas, silica becomes SiF 4 Since the gas escapes in this form and the quartz glass surface is etched uniformly without any difference in etching rate, no particles originating from the quartz glass are generated.
[0021] The etching environment may contain small amounts of components that can cause contamination, and these components may be generated as particles. However, after extensive investigations, the inventors have confirmed that when the above-mentioned elements Al and Cl are not included in the particle components, the unevenness of the quartz glass surface after etching is extremely small.
[0022] The quartz glass according to this embodiment is amorphous and is obtained by sintering synthetic silica powder to produce a sintered body, which is then polished.
[0023] The particle size of the synthetic silica powder is usually 40 to 300 μm, and preferably 80 to 200 μm.
[0024] If the particle size of the synthetic silica powder is 40 μm or more, the generation of fumes during sintering can be suppressed. If the particle size of the silica powder is 300 μm or less, the generation of grain boundaries during sintering can be suppressed.
[0025] Synthetic silica powder contains less metal impurities than natural silica powder, and can be obtained by a method known as the sol-gel method using alkoxysilane as a raw material, for example.
[0026] The sintering method is preferably pressure sintering, which can give a dense sintered body, and examples thereof include spark plasma sintering (SPS).
[0027] The sintering temperature is preferably 1200 to 1500°C, more preferably 1300 to 1400°C. If it is 1200°C or higher, a sufficient sintered body can be obtained. If it is 1500°C or lower, the generation of fumes and the progress of crystallization can be suppressed. The pressure during sintering is preferably 15 to 100 MPa, more preferably 20 to 50 MPa. If it is 15 MPa or higher, it is possible to suppress air bubbles from remaining in the sintered body. If it is 100 MPa or lower, the cost of the equipment can be reduced.
[0028] When synthetic silica powder is filled into the carbon mold during sintering, it is preferable to subject the sintered body to an annealing treatment after sintering to remove carbon from the surface.
[0029] The annealing temperature of the sintered body is preferably 600 to 1000° C., more preferably 700 to 800° C. If it is 600° C. or higher, residual stress can be sufficiently removed. If it is 1000° C. or lower, the generation of bubbles in the sintered body can be suppressed.
[0030] The annealing time is preferably 2 to 10 hours, more preferably 4 to 6 hours. If it is 2 hours or more, the residual stress can be sufficiently removed. If it is 10 hours or less, the desired productivity can be obtained.
[0031] The polishing method is not particularly limited, and examples thereof include polishing with free abrasive grains. It is preferable to polish the quartz glass so that the surface roughness Ra of the quartz glass is 0.3 μm or less.
[0032] The density of quartz glass is 2.15 to 2.25 g / cm 3 The amount of metal impurities in quartz glass is less than 0.1 ppm. The hydroxyl group content in quartz glass is less than 100 ppm.
[0033] [Evaluation method for quartz glass] The fact that quartz glass is amorphous can be confirmed by the presence or absence of detection of crystalline matter by X-ray diffraction (XRD).
[0034] As described above, when the quartz glass is manufactured using natural silica powder, etching with a fluorocarbon gas generates particles containing Al derived from the quartz glass, causing unevenness on the surface of the quartz glass.
[0035] Furthermore, when quartz glass produced by vapor phase synthesis is etched using a fluorocarbon gas, particles containing chlorine originating from the quartz glass are generated, causing irregularities on the surface of the quartz glass.
[0036] On the other hand, when quartz glass produced by a method including sintering the above-mentioned synthetic silica powder is etched using a fluorocarbon gas, no particles derived from the quartz glass are generated (the amount of particles generated is extremely small), and the occurrence of unevenness on the quartz glass surface can be suppressed.
[0037] In other words, when the Al and Cl contained in the particles produced by etching quartz glass are below a specified value, the quartz glass being evaluated is not made from natural silica or vapor-phase synthetic silica, and the unevenness of the quartz glass surface after etching is extremely small.
[0038] The method of collecting particles generated by etching of quartz glass is not particularly limited, but for example, a silicon wafer is placed in an etching device, and the quartz glass to be evaluated is placed in the center of the silicon wafer. In addition, particle collection substrates are placed on the left and right of the quartz glass with a gap of about 2 to 3 mm between them so as to sandwich the quartz glass. For example, a GaN substrate can be used as the particle collection substrate.
[0039] The etching gas used in the etching is not particularly limited, but may be, for example, CF 4 , CHF 3 , C.H. 2 F 2 etc. can be used.
[0040] The quartz glass described in the present invention is a gas containing CHF 3 When the particles generated during etching for 4 hours were analyzed by EDS under the conditions of ICP power 200 W, pressure 1.8 Pa, and flow rate 30 sccm, the measurement area was 0.96 mm 2 In this range, the detection signal intensities of Al and Cl are both 30 cps / eV or less. As described above, after etching, the particles present on the particle collection substrate are analyzed by SEM-EDS. If the detection signal intensities of Al and Cl in a measurement area of a given size are both below a given value, the quartz glass to be evaluated can be judged to have excellent etching resistance with almost no unevenness on the surface after etching.
[0041] In one embodiment of the silica glass according to the present invention, the amount of metal impurities in the silica glass is 0.1 ppm or less. The amount of metal impurities in the present invention is measured by ICP-mass and calculated based on the amount of metal elements relative to the amount of elements (Si, O) derived from the quartz glass. EXAMPLES
[0042] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0043] [Example 1] A carbon mold with a diameter of 20 mm was filled with synthetic silica powder (PS400, Mitsubishi Chemical Corporation, D50: 180 μm), and a pellet-shaped sintered body with a thickness of 7 mm was obtained using an SPS device at a sintering temperature of 1300°C and a pressure of 100 MPa. The sintered body was then annealed in an electric furnace at 800°C to remove carbon from the surface, and a transparent glass body with an Ra of 0.03 μm was polished to prepare an etching test sample. XRD measurement of this etching test sample confirmed that no peak was observed at 2θ of 26 to 27°, which indicates the presence of crystals, and that the sample was completely amorphous. The density was 2.2 g / cm 3 It was confirmed that there was no significant difference from general quartz glass.
[0044] A silicon wafer was placed in a parallel plate reactive ion etching (RIE) device, and an etching test sample and a GaN substrate for particle collection were placed side by side in the center. 3 Etching was carried out for 4 hours under conditions of an ICP power of 200 W, a pressure of 1.8 Pa, and a flow rate of 30 sccm.
[0045] After etching, particles on the GaN substrate were analyzed by SEM-EDS, and the measurement area was 0.96 mm 2 The measurements were performed in the range of 100 to 200 nm. Table 1 shows the detection signal strengths of Al and Cl, excluding Si, F, and O, which were detected in all Examples and Comparative Examples and originate from the etching gas and silica powder. In addition, the surface roughness of the etching test samples after etching was measured. The measurement results are shown in Table 1.
[0046] [Example 2] A glass body (model GE012, Momentive Performance Materials Japan LLC) manufactured by sintering synthetic silica powder was processed to a size of 10 x 10 x 3 mmt, and both sides were fire-finished to a transparent glass body with Ra: 0.03 μm. Etching was performed in the same manner as in Example 1, except that the etching test sample was a transparent glass body with Ra: 0.03 μm. Particle analysis and surface roughness measurement were performed. The measurement results are shown in Table 1.
[0047] [Comparative Example 1] A glass body (type N, Tosoh Corporation) manufactured from natural silica was processed to a size of 10 x 10 x 3 mmt, and both sides were fire-finished to a transparent glass body with Ra: 0.03 μm. Except for this, etching was performed in the same manner as in Example 1, and particle analysis and surface roughness measurement were performed. The measurement results are shown in Table 1.
[0048] [Comparative Example 2] A glass body (SH110, Shin-Etsu Quartz Co., Ltd.) manufactured using vapor-phase synthetic silica as a raw material was processed to a size of 10 x 10 x 3 mmt, and both sides were fire-finished to a transparent glass body with Ra: 0.03 μm. Etching was performed in the same manner as in Example 1, except that the etching test sample was a transparent glass body with Ra: 0.03 μm. Particle analysis and surface roughness measurement were performed. The measurement results are shown in Table 1.
[0049] [Table 1]
Claims
1. Gas type: CHF 3 When the particles generated during etching for 4 hours were analyzed by EDS under the conditions of ICP power 200 W, pressure 1.8 Pa, and flow rate 30 sccm, the measurement area was 0.96 mm 2 The quartz glass has detection signal intensities of 30 cps / eV or less for both Al and Cl in the range of 100 cps / eV.
2. 2. The quartz glass according to claim 1, wherein the amount of metal impurities in the quartz glass is 0.1 ppm or less.
3. The quartz glass of claim 1 , wherein the quartz glass is amorphous.
Citation Information
Patent Citations
Quartz glass thermal sprayed componentt and method for producing the same