Porous molded body for moving-bed adsorption
A porous molded body of aluminophosphate zeolite with specific properties addresses shape and strength issues in fluidized beds, enhancing adsorption capacity and enabling compact heat pump designs.
Patent Information
- Application Number
- JP2023058849
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing adsorbents for adsorption heat pumps face challenges in maintaining shape, particle size uniformity, and mechanical strength when used in a fluidized bed, leading to insufficient adsorption capacity and large device size.
A porous molded body composed of aluminophosphate zeolite and a binder, with specific particle size, compressive strength, and pore volume, manufactured through a process involving mixing, granulation, and firing, to ensure durability and high adsorption capacity.
The porous molded body maintains shape and particle size even in a fluidized state, offering high adsorption capacity and compact device design, suitable for applications like heat pumps in automobiles.
Smart Images

Figure 2024146123000005 
Figure 2024146123000001 
Figure 2024146123000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous molded body for moving bed adsorption, a method for producing said molded body, and a moving bed adsorption process using said molded body. [Background technology]
[0002] Zeolites include crystalline silicates and crystalline aluminophosphates as defined by the International Zeolite Association (IZA). Zeolites are widely used as adsorbents, catalysts, separation materials, and detergent builders. In recent years, from the viewpoint of energy saving, adsorption heat pumps that use porous materials such as zeolites and mesoporous materials as adsorbents have been researched and developed.
[0003] As an adsorbent for an adsorption heat pump, for example, zeolite containing at least aluminum, phosphorus, and heteroatoms in its framework structure has been proposed (Patent Document 1). However, the details of granulation have not been considered. As a method for producing an adsorbent, for example, a granulation method having a pressing step of a raw material powder and a grinding step of crushing and polishing between grinders is known, and a particle size of 0.05 to 2 mm is considered to be suitable (Patent Document 2). However, when the adsorbent is used in an adsorption heat pump, it is fixed to a heat exchanger, and the adsorbent is not necessarily satisfactory in terms of packing density and adsorption characteristics. Also, from the viewpoint of miniaturization of the device, an adsorption heat pump using an adsorbent having a bulk density of 0.5 g / cc or more is known as an adsorbent for an adsorption heat pump, and an adsorbent having a particle size of 100 to 150 μm is disclosed. However, this adsorbent is a high-density porous material mainly composed of silicon and oxygen, and is not necessarily satisfactory in terms of adsorption characteristics (Patent Document 3).
[0004] On the other hand, aluminophosphates, which contain aluminum and phosphorus in their skeletal structure, have been known to be mainly used in the field of catalysis. As a catalyst for chemical processes such as the conversion of methanol to light olefins, a catalyst has been disclosed in which silicoaluminophosphates, in which part of the phosphorus of aluminophosphates has been substituted with silicon, are granulated to tens to hundreds of μm by spray drying together with a binder component such as kaolin or silica sol (Patent Document 4 and Patent Document 5).
[0005] However, in order to increase the strength of these granules used as catalysts, the proportion of binder components needs to be extremely high, at 40 mass % or more. Therefore, when used as an adsorbent for an adsorption heat pump, there are problems such as insufficient strength and bulk density for practical use, or insufficient adsorption capacity, which requires a large device. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-372332 A [Patent Document 2] JP 2001-38188 A [Patent Document 3] Japanese Patent Application Publication No. 9-264633 [Patent Document 4] U.S. Patent No. 4,973,792 [Patent Document 5] U.S. Patent No. 5,095,163 Summary of the Invention [Problem to be solved by the invention]
[0007] To address the above-mentioned problems, a granulated material essentially containing an aluminophosphate and a binder has been proposed (JP Patent Publication 2005-272296). This granulated material has excellent strength and can achieve a high packing density when it is fixed to a heat exchanger for use as an adsorbent. A continuously operating adsorption heat pump is composed of two adsorbers, one condenser, and one evaporator. The condenser and evaporator are alternately supplied with a heat exchange fluid at ambient temperature and a heat exchange fluid at cooling and freezing return temperatures, while the two adsorbers are alternately supplied with a heat exchange fluid during the adsorption process and a heat exchange fluid at the high-temperature heat source temperature during the desorption process, making it possible to continuously extract cold for cooling and refrigeration from the evaporator. Furthermore, adsorbents such as zeolite are packed into containers before use, and when their functionality deteriorates, the container containing the zeolite is replaced. Therefore, once packed into a container, the adsorbent such as zeolite itself only needs to be able to withstand a static load, such as the weight from above, and no particular problems arose.
[0008] However, since the above-mentioned adsorption heat pump having two adsorbers tends to be large, a method of using an adsorbent such as zeolite while moving it like a fluidized bed is being explored. In such an embodiment, the resistance to the static load as described above is not enough, and the adsorbent such as zeolite is required to have greater hardness as the adsorbent flows, and is required to have physical properties such as wear resistance and impact resistance. Furthermore, when the adsorbent flows, in order to maintain a favorable flow state, it is preferable that the particle size of the adsorbent is uniform, and it is also preferable that the adsorbent has a specific shape. The present invention has been made to solve the above problems, and its object is to provide a porous molded body for moving bed adsorption which has excellent strength, can maintain its shape, particle size, etc. even when fluidized when used as an adsorbent in a heat exchanger, and has a high adsorption capacity, and a method for producing the same. [Means for solving the problem]
[0009] As a result of intensive research into the above-mentioned problems, the inventors have discovered that the above-mentioned problems can be solved by a porous molded body containing an aluminophosphate and a binder, being in a specific particle size range, having a specific pore volume, and having a specific compressive strength, and have arrived at the present invention.
[0010] The present invention includes the following gist. [1] A porous molded body for moving bed adsorption comprising an aluminophosphate zeolite and a binder, the porous molded body for moving bed adsorption having a particle size range of 50 to 5000 μm and a compressive strength of 2 MPa or more. [2] The porous molded body for moving bed adsorption described in [1] above, which has a relative vapor pressure region in which the change in the amount of water adsorbed is 0.12 g / g or more when the relative vapor pressure changes by 0.15 in the range of relative vapor pressures of 0.01 or more and 0.30 or less in a water vapor adsorption isotherm measured at 25°C. [3] The porous molded body for moving bed adsorption according to the above [1] or [2], in which the molar ratio of Si, P, Al, and Me (wherein Me represents a heteroatom that can replace part of Al in the aluminophosphate framework) in the porous molded body for moving bed adsorption satisfies the following formula: 1.02≦(Si+P) / (Al+Me)≦1.4 [4] The porous molded body for moving bed adsorption according to any one of [1] to [3] above, which is obtained from a reaction mixture containing at least an aluminophosphate and a binder precursor, and the binder precursor contains a compound of the following formula (I):
[0011] [ka] (In the formula (I), each R is independently an optionally substituted alkyl group, aryl group, alkenyl group, alkynyl group, alkoxy group, or aryloxy group; each R' is independently an optionally substituted alkyl group, aryl group, alkenyl group, or alkynyl group; and n is a number from 1 to 100.)
[0012] [5] The porous molded body for moving bed adsorption according to any one of the above [1] to [4], wherein the pore volume in the pore diameter range of 0.1 to 5 μm is 0.05 cc / g or more and 0.5 cc / g or less. [6] A method for producing a porous molded body for moving-bed adsorption according to any one of the above [1] to [5], wherein a reactive mixture containing at least an aluminophosphate and a binder precursor is granulated by tumbling granulation. [7] A moving bed adsorption method using the porous molded body according to any one of the above [1] to [5]. [8] The moving bed adsorption method according to [7] above, wherein the porous molded body is an adsorbent and water or carbon dioxide is an adsorbate. Effect of the Invention
[0013] According to the present invention, it is possible to provide a porous molded body for moving bed adsorption which has excellent strength, can maintain its shape, particle size, etc. even when fluidized when used as an adsorbent in a heat exchanger, and has a high adsorption capacity, and a method for producing the same. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a diagram showing water vapor adsorption isotherms of Example 1 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0016] [Porous molded body] The porous molded body of the present invention is a porous molded body for moving bed adsorption, which contains an aluminophosphate zeolite and a binder, and is characterized in that it has a particle size range of 50 to 5000 μm, a pore volume in the pore diameter range of 0.1 to 5 μm of 0.05 cc / g or more and 0.5 cc / g or less, and a compressive strength of 2 MPa or more. Here, the measurement and calculation of compressive strength is performed according to the method described in JIS28841-1993 "Compressive Strength". Specifically, the particles are compressed at a constant speed, and the stress at the time of compression (unit: N or gf) obtained is converted to compressive strength (unit: MPa) according to the "Hiramatsu method". The Hiramatsu method is described in "Japan Mining Association Journal, Vol. 81, No. 932, p. 1024 (1965)".
[0017] The shape of the porous molded body of the present invention is not particularly limited, but since it is used in a moving bed, a round shape without corners is preferable rather than a square shape. Since the round shape has no corners, it is less likely to be scraped off by friction and is less likely to become powdery. More specifically, the average sphericity is preferably 0.70 or more, more preferably 0.75 or more, and even more preferably 0.80 or more. There is no particular limit to the upper limit, and it may be 1.0 (sphericity). However, from the viewpoint of productivity, it is preferably 0.99 or less, more preferably 0.98 or less. The sphericity is a value measured by the method described in the examples.
[0018] The particle size of the porous molded body of the present invention refers to the average of the major axis and minor axis when they exist, and is measured by laser diffraction, microscope observation, etc. The average particle size of the porous molded body of the present invention is preferably 60 μm or more, while it is preferably 3000 μm or less, further preferably 1000 μm or less, more preferably 800 μm or less, and particularly preferably 600 μm or less.
[0019] If the average particle size of the porous molded body is too small, the diffusion of the adsorbate in the adsorbent layer is hindered, and if the particle size is too large, the strength of the porous molded body particles decreases. Note that porous molded bodies having the above average particle size can usually be obtained in the desired particle size range by controlling the conditions for producing the porous molded body and, if necessary, crushing and then sieving the porous molded body.
[0020] The porous molded body of the present invention is not particularly limited, but the pore volume of pores having a diameter of 0.1 to 5 μm is usually 0.05 cc / g or more and 0.5 cc / g or less, preferably 0.1 cc / g or more, while it is preferably 0.45 cc / g or less, more preferably 0.4 cc / g or less. If the pore volume is equal to or greater than these lower limits, the diffusion of the adsorbate into the pores becomes faster, and the adsorption rate becomes higher, which is preferable. On the other hand, if the pore volume is equal to or less than the upper limits, the bulk density falls within an appropriate range, and the adsorption efficiency of the adsorbate becomes higher, which is preferable. The pore volume in the pore diameter range of 0.1 to 5 μm is measured by mercury intrusion porosimetry. The porous molded body of the present invention has a compressive strength of 2 MPa or more, more preferably 2.5 MPa or more, and particularly preferably 3 MPa or more. The higher the compressive strength, the more preferable it is, but it is usually about 4 MPa or less. If the compressive strength is too low, problems such as powdering may occur when used in a fluidized state.
[0021] Considering that when used in a fluid state, they will likely slide against each other, that they may fall, and that many molded pieces will move like an avalanche, this value is insufficient for the compression strength required for tableting, which has been widely used in the past. As an example, even when considering a single particle, when a silicoaluminophosphate molded body is used for a moving bed, it is considered necessary that it has a strength strong enough not to break even if it is dropped from a height of 100 cm. Assuming that the specific gravity of zeolite is 2, the mass of one 2 mm diameter molded body particle used in the example is 0.00837 g, and ignoring air resistance, v = √2gh, so it hits another molded body or the bed at 4.43 m / s, and the impact force F (N) is calculated as F = 3.70 N and pressure 1.18 MPa assuming an action time of 10 ms. Considering that many molded bodies will actually move at the same time, it is considered that a compressive strength of at least 2 MPa is necessary.
[0022] The bulk density is usually 0.5 g / cc or more, preferably 0.6 g / cc or more. When the bulk density is equal to or more than the lower limit, the adsorption efficiency of the adsorbate in the fluidized porous molded body can be maintained.
[0023] In the porous molded body of the present invention, in a water vapor adsorption isotherm measured at 25°C, when the relative vapor pressure changes by 0.15 in the range of 0.01 to 0.30, the amount of water adsorption preferably changes by 0.12 g / g or more, more preferably changes by 0.15 g / g or more, and even more preferably changes by 0.17 g / g or more. When the change in the amount of adsorption is large, the amount of adsorbent can be reduced when used in an adsorption heat pump or the like, which is advantageous in that the device can be made compact. In addition, in the water vapor adsorption isotherm, the amount of adsorption at a relative vapor pressure of 0.01 is preferably 0.15 g / g or less, more preferably 0.12 g / g or less, and particularly preferably 0.10 g / g or less.
[0024] The molding method of the porous molded body of the present invention is not particularly limited as long as the above physical properties are satisfied, but in particular, it is possible and preferable to obtain the porous molded body of the present invention by granulating an aluminophosphate with a silicon-containing binder, more specifically, a silicone or a silicic acid liquid, as described below, and adjusting the particle size by sieving, etc., if necessary. Furthermore, it is preferable that the molar ratio of Si, P, Al, and Me (heteroatoms) in the granulated product of the present invention derived from the binder precursor satisfies the following formula. 1.02≦(Si+P) / (Al+Me)≦1.4
[0025] Incidentally, Me is a heteroatom which can substitute for a part of Al in the aluminophosphate framework, and the content thereof may be zero. When an aluminophosphate contains Si and / or Me in its framework, a part of Al is replaced by Me and a part of P is replaced by Si, so that the composition formula of such aluminophosphates is Al. 1-x Me x P 1-y S yO4, and as is clear from this composition formula, the molar ratio of (P+Si) / (Al+Me) is 1. Here, if the binder precursor is mainly composed of silicon, silicon is introduced from a component other than the aluminophosphate framework, so the molar ratio of (P+Si) / (Al+Me) is greater than 1. In the porous molded body of the present invention, the molar ratio of (P+Si) / (Al+Me) is preferably 1.02 or more, more preferably 1.05 or more. If this value is too small, the strength tends to decrease. On the other hand, it is preferably 1.4 or less, more preferably 1.2 or less. If this value is too large, the ratio of the binder to the aluminophosphates increases, so the adsorption capacity tends to decrease. The proportions of these elements in the porous molded body are determined by calcining the porous molded body at 550°C in an oxygen-containing atmosphere, dissolving it in hydrochloric acid, hydrofluoric acid, etc., and performing elemental analysis using the ICP method, etc. Furthermore, since silica contained in the binder in the porous molded body does not dissolve in hydrochloric acid, which dissolves aluminophosphates that contain silicon as a framework component, it is possible to quantify it separately from silicoaluminophosphates.
[0026] <Aluminophosphate zeolite> The aluminophosphate zeolite used in the porous molded body of the present invention means a crystalline aluminophosphate as defined by the International Zeolite Association (IZA), in which the atoms constituting the framework are aluminum and phosphorus, some of which may be substituted with other atoms (Me: heteroatoms). Among these, (I) Me-aluminophosphate in which aluminum is partially substituted with a heteroatom represented by Me1 (wherein Me1 represents at least one element selected from elements belonging to the 3rd or 4th period of the periodic table and belonging to groups 2A, 7A, 8, 1B, 2B, and 3B (excluding Al)), (II) Me-aluminophosphate in which phosphorus is substituted with a heteroatom represented by Me2 (wherein Me2 represents a group 4B element belonging to the 3rd or 4th period of the periodic table), or (III) Me-aluminophosphate in which both aluminum and phosphorus are substituted with heteroatoms Me1 and Me2, respectively, are preferred in terms of adsorption properties.
[0027] Here, the molar ratios of Me, Al and P constituting the skeletal structure are usually those of the following formulas 1-1 to 3-1, and preferably those of the following formulas 1-2 to 3-2. If x is smaller than the above range, the amount of adsorption in the low pressure region of the adsorbate tends to be small and synthesis tends to be difficult, while if it is larger than the above range, impurities tend to be easily mixed in during synthesis. Also, if y and z are outside the above ranges, synthesis is difficult. 0≦x≦0.3 1-1 (x represents the molar ratio of Me to the total of Me, Al, and P) 0.2≦y≦0.6 2-1 (y represents the molar ratio of Al to the total of Me, Al, and P) 0.3≦z≦0.6 3-1 (z represents the molar ratio of P to the total of Me, Al, and P) 0.01≦x≦0.3 1-2 (x represents the molar ratio of Me to the total of Me, Al, and P) 0.3≦y≦0.5 2-2 (y represents the molar ratio of Al to the total of Me, Al, and P) 0.4≦z≦0.5 3-2 (z represents the molar ratio of P to the total of Me, Al, and P)
[0028] Me may be one or more. Preferred Me (Me1, Me2) is an element belonging to the third or fourth period of the periodic table. Me1 preferably has an ionic radius of 0.3 Å or more and 0.8 Å or less in a divalent state, and more preferably has an ionic radius of 0.4 Å or more and 0.7 Å or less in a divalent, tetracoordinated state. Among the above, from the viewpoints of ease of synthesis and adsorption characteristics, at least one element selected from Fe, Co, Mg, and Zn is preferred, and Fe is particularly preferred. Me2 is a Group 4B element belonging to the third or fourth period of the periodic table, and is preferably Si.
[0029] The aluminophosphates of the present invention usually have a framework density (FD) of 13 T / nm 3 More than 20T / nm 3 Less than or equal to 13.5T / nm, preferably 3 More preferably, it is 14 T / nm or more. 3 On the other hand, 19T / nm 3 Less than 17.5T / nm is preferred 3 More preferably, T / nm 3 is the unit volume nm 3 T atoms present per nm of zeolite 3 The framework density (FD) is the number of elements other than oxygen that constitute the framework per unit area, and is a unit that indicates the framework density (FD). If it is less than the above range, the structure tends to become unstable, causing a problem of reduced durability, while if it exceeds the above range, the adsorption capacity tends to become small, making it unsuitable for use as an adsorbent.
[0030] The structure of the aluminophosphates of the present invention can be represented by the codes defined by the International Zeolite Association (IZA), which include AEI, AEL, AET, AFI, AFN, AFR, AFS, AFT, AFX, ATO, ATS, CHA, ERI, LEV, and VFI. Among these, from the standpoint of adsorption characteristics and durability, any one selected from AEI, AEL, AFI, CHA, and LEV is preferred, with CHA and AFI being particularly preferred.
[0031] <Binder> The binder in the present invention is a component that binds the aluminophosphate zeolite in the porous molded body. Since the porous molded body of the present invention is obtained by granulating and heating a mixture containing at least the aluminophosphate zeolite and the binder precursor, the binder is usually a binder precursor, which will be described later, modified by crosslinking or the like. However, the binder also includes a component that is added as necessary during molding and remains in the porous molded body.
[0032] As the binder precursor of the present invention, inorganic binders such as silicones, silicic acid liquid, specific silica sol or alumina sol are used. Here, silicones refer to oligomers having polysiloxane bonds in the main chain, including those in which a part of the substituent of the main chain of the polysiloxane bond is hydrolyzed to become an OH group. Among them, binder precursors that are silicon-containing compounds that undergo condensation at low temperatures of room temperature to 300°C are preferred. Condensation reaction of silicates and silicic acid liquid proceeds at low temperatures of about room temperature to 300°C. The above-mentioned "specific silica gel" means one that undergoes condensation reaction at such low temperatures. In addition, it is also preferable to use silica sol because of its simplicity and high safety. From the viewpoint of the compressive strength of the porous molded body, silicones or silicic acid liquid are preferred, and among these, silicic acid liquid is most preferred because it does not generate organic compounds such as alcohols due to hydrolysis during the granulation process. Silicones are compounds having a polysiloxane bond, and examples thereof include compounds having the following structures or partial hydrolysates thereof.
[0033] [ka]
[0034] (In the formula (I), each R is independently an optionally substituted alkyl group, aryl group, alkenyl group, alkynyl group, alkoxy group, or aryloxy group; each R' is independently an optionally substituted alkyl group, aryl group, alkenyl group, or alkynyl group; and n is a number from 1 to 100.) R is preferably a C1 to C6 alkyl group, 12 an aryl group of C2 to C6, an alkenyl group of C2 to C6, an alkynyl group of C1 to C6, an alkoxy group of C6 to C 12 These may be optionally substituted. More preferred are independently unsubstituted alkoxy groups, alkyl groups and aryloxy groups, particularly preferred are alkoxy groups, of which ethoxy groups and methoxy groups are preferred, and most preferred is methoxy group.
[0035] R' is preferably a C1 to C6 alkyl group, 12 an aryl group having 1 to 5 carbon atoms, a C2 to C6 alkenyl group, or a C2 to C6 alkynyl group, which may be optionally substituted. An unsubstituted C1 to C5 alkyl group is preferred, a methyl group or an ethyl group is more preferred, and a methyl group is most preferred.
[0036] The partial hydrolysate of the above formula (I) is one in which at least a part of R and R' has been converted to an OH group by hydrolysis. The repeating unit n is usually 2-100, preferably 2-50, and more preferably 3-30. Depending on the value of n, the compounds of formula (I) are present here either in monomeric form or in the form of longer chains, optionally branched oligomeric longer chains. The silicones of the present invention include alkyl silicates commonly known as methyl silicate and ethyl silicate.
[0037] The silicic acid solution in the present invention is obtained by removing alkali metal ions from an alkali silicate solution. The alkali metal ions can be removed by a known method such as ion exchange. For example, as described in Japanese Patent No. 3540040 and Japanese Patent Laid-Open No. 2003-26417, a sodium silicate solution is dissolved in H + It is prepared by contacting with a cation exchange resin of the type
[0038] As the alkali silicate, in addition to sodium silicate, potassium silicate or a mixture of these can be used, but sodium silicate is preferred from the viewpoint of availability. + The cation exchange resin is a commercially available product, such as Diaion SKT-20L or Amberlite IR-120B, which is dissolved in water in a 100% aqueous solution. + It is used after ion exchange in a mold. The amount of cation exchange resin required to be used is selected based on known knowledge, but is usually an amount that provides a cation exchange capacity equal to or greater than the amount of alkali metal ions in the alkali silicate. Ion exchange can be performed either by flow-through or batch-wise, but the flow-through type is usually used.
[0039] The SiO2 concentration in the silicic acid solution is usually 1 to 10% by mass, preferably 2 to 8% by mass. If the concentration is too low, the strength of the porous molded body tends to decrease, while if the concentration is too high, the stability of the silicic acid solution tends to decrease. The silicic acid solution may contain a small amount of an organic base such as an alkali metal ion, an organic amine, or a quaternary ammonium as a stabilizer. The concentration of these stabilizers, for example, alkali metal ions, is usually 1% by mass or less, preferably 0.2% by mass or less, and particularly preferably 0.0005 to 0.15% by mass.
[0040] If the alkali metal ion concentration is higher than this range, the adsorption capacity tends to decrease. The alkali metal ion concentration can be controlled by adding a soluble salt such as an alkali metal hydroxide or sodium silicate to the silicic acid solution from which the alkali metal ions have been removed to about 100 ppm or less, or by controlling the residual alkali metal ion concentration by adjusting the ion exchange conditions.
[0041] In order to obtain the porous molded body of the present invention, it is particularly preferable to use silicones or a silicic acid liquid as the binder precursor and to select the firing temperature in the third step described below from a preferred range.
[0042] (Granulation method) The porous molded body of the present invention is produced by a process including the following three steps. (1) A first step of mixing at least an aluminophosphate and a binder precursor to prepare a reaction mixture. (2) The reaction mixture obtained in the first step is extruded, stirred, or spray-granulated, and then crushed and / or sieved as necessary to obtain a granulated precursor. (3) A third step of calcining the granulated precursor obtained in the second step at a temperature in the range of 150°C to 700°C.
[0043] (1st step) In the first step, at least an aluminophosphate and a binder precursor are mixed to prepare a reaction mixture. The mixing ratio of the aluminophosphate and the binder precursor in the reaction mixture is usually 2 to 40 parts by mass, preferably 5 to 30 parts by mass of the binder precursor calculated as oxide, per 100 parts by mass of the aluminophosphate. If the amount is less than this range, the compressive strength tends to decrease, and if the amount is too much, the adsorption capacity tends to decrease.
[0044] In addition, water is usually added to the reaction mixture. The mixing ratio varies depending on the molding method, but is usually 10 to 500% by mass based on the aluminophosphates. For example, in the case of extrusion molding or stirring granulation, the mixing ratio is 10 to 50 parts by mass, preferably 10 to 30 parts by mass, and in the case of spray drying, the mixing ratio is 30 to 400 parts by mass, preferably 40 to 220 parts by mass. Depending on the characteristics during kneading and extrusion, the reaction mixture may be added with a plasticizer such as celluloses such as methyl cellulose, starch, polyvinyl alcohol, etc., for the purpose of increasing fluidity. The mixing ratio is 0.1 to 5 parts by mass, preferably 0.5 to 2 parts by mass, per 100 parts by mass of aluminophosphate. If the amount added is too large, the strength of the granulated product tends to decrease. The average particle size of the raw material aluminophosphate used for granulation is usually 15 μm or less, preferably 10 μm or less, and the lower limit is usually 1 μm. If necessary, dry pulverization using a jet mill or the like or wet pulverization using a ball mill or the like may be performed.
[0045] (2nd process) In the second step, the reaction mixture obtained in the first step is extrusion molded, stirred granulated or spray granulated, and if necessary, pulverized and / or sieved to obtain a granulated product precursor. The apparatus used for extrusion molding, stirring granulation, or spray granulation may be a known extrusion molding machine, stirring granulator, or spray dryer. When the particle size is in the range of 50 to 200 μm, spray granulation is suitable, and when the particle size is in the range of 200 μm to 5000 μm, particularly 500 to 5000 μm, rolling granulation or stirring granulation is suitable.
[0046] In the case of stirring granulation, the aluminophosphates, binder precursor, and plasticizer are usually mixed at room temperature, and then a specified amount of water is added and granulation (stirring) is performed. There is no particular limit to the granulation time, but it is usually 1 to 120 minutes, preferably 2 to 30 minutes. If the granulation time is too short, granulation is insufficient and the particle size distribution of the granulated product becomes wide, and if the granulation time is too long, the water in the system evaporates during granulation, making water management difficult. After granulation, the granulated product precursor is obtained by drying at 50°C to 150°C as necessary.
[0047] By employing rolling granulation, it is possible to obtain, after firing, spherical granules having a particle size of about 1 mm, a high compressive strength of 6 to 10 MPa, and a pore volume of 0.1 to 5 μm of 0.2 to 0.4 ml / g, even if the binder is about 10 mass % in terms of oxide. When making the particle size about 1 mm, particles of silica, alumina, silica-alumina, etc. may be used as nuclei as necessary, and the binder and aluminophosphate may be attached around the nuclei to perform granulation.
[0048] In the case of extrusion molding, aluminophosphates, binder precursor, plasticizer and water are usually added and kneaded, and then molded with an extruder. There is no particular restriction on the pressure during molding, but it is usually 5 to 500 kgf / cm. 2 After granulation, the mixture is usually dried at a temperature of about 50°C to 150°C, pulverized, and classified to obtain the desired granulated product precursor. In the case of spray drying, a slurry obtained by adding and mixing aluminophosphates, binder precursor, plasticizer and water is introduced into a spray dryer. As for the conditions, the solid concentration of the raw material slurry is usually about 20 to 70 mass%, the inlet temperature of the spray dryer is preferably about 150 ° C to 450 ° C, and the outlet temperature is preferably in the range of about 60 ° C to 225 ° C. The particle size of the granulated precursor depends on the size of the sprayed droplets, and also depends on the slurry supply speed, the slurry concentration, and the spray type. In addition, by lowering the spray drying temperature, the strength of the granulated product tends to be increased and the bulk density tends to be high density, but if the temperature is too low, the proportion of particles that reach the wall surface before drying increases and the yield decreases, so it is preferable to set the temperature relatively high within the above range. The above conditions are preferably selected so that the aluminophosphates in the granules contain the template used in the synthesis thereof and are carried out up to the second step.
[0049] (3rd step) In the third step, the granule precursor obtained in the second step is calcined at a temperature in the range of 150°C to 900°C. The temperature is preferably 200°C or higher, more preferably 250°C or higher, and particularly preferably 300°C or higher. On the other hand, it is preferably 800°C or lower, more preferably 700°C or lower. By calcining within the above temperature range, the cross-linking of the binder precursor is substantially achieved, a high compressive strength of the granule is obtained, and the adsorption and catalytic properties of the produced granule are also good. If the calcination temperature is too high, the structure of the aluminophosphate is destroyed, and the adsorption capacity is reduced. On the other hand, if the calcination temperature is too low, the cross-linking of the binder precursor, preferably the alkyl silicate, does not proceed sufficiently, and the template is not sufficiently removed, tending to reduce the adsorption capacity.
[0050] In the calcination step, known calcination methods such as fixed bed, fluidized bed, and rotary kiln can be applied, but from the viewpoint of uniformity of calcination and ease of temperature control, fluidized bed and rotary kiln are preferred. The calcination gas is preferably circulated in order to quickly remove volatile substances and moisture generated by calcination. As the calcination gas, oxygen-containing gas such as air and inert gas such as nitrogen can be used, but diluted oxygen-containing gas obtained by diluting air with inert gas such as nitrogen is preferably used in order to control heat generation due to combustion of organic templates and the like derived from the raw material for synthesis of aluminophosphates.
[0051] [Moving bed adsorption method] The porous molded body of the present invention can be suitably used in a moving bed adsorption method, and it is particularly preferred to use the porous molded body of the present invention as an adsorbent and water or carbon dioxide as an adsorbate. EXAMPLES
[0052] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the following examples.
[0053] (Evaluation method) <Particle size> Regarding particle size measurement, if the target particle size is large (usually 500 μm or more), it is sufficient to measure about 50 particles of standard size by visual inspection or, if necessary, using an optical microscope, excluding particles that are clearly fragments, and take the average value. A simple method is to sift the particles, take the median value of the sieve as the particle size, and use the weighted average value. If the target particle size is 500 μm or less, it is sufficient to take several SEM photographs with an SEM at a magnification where 10 or more particles are visible, measure the average particle size of 50 or more particles, and take the average.
[0054] <Pore volume> The pore volume in the pore diameter range of 0.1 to 5 μm was obtained from the pore distribution curve by the mercury intrusion method. Specifically, an Autopore 9200 pore distribution measuring device manufactured by Micrometrics was used, and the measurement conditions were equilibration time 10 seconds, contact angle 130 degrees, surface tension 484 dyne / cm, and measurement pressure range 20 to 59,500 psi.
[0055] <Sphericity> Sphericity is an index expressed by the ratio (M1 / M2) of the minimum length (minor axis length M1) to the maximum length (major axis length M2) of a non-aggregated primary particle sandwiched between parallel lines (sphericity S=M1 / M2), and the higher the sphericity, the closer it is to a perfect sphere. The average sphericity is the average value. In the present invention, molded bodies that were particularly irregular in shape as determined by SEM observation were excluded, and the sphericity of 10 randomly selected molded bodies was measured, and the average was calculated to obtain the average sphericity.
[0056] <Compressive strength of adsorbent granules> Using an Instron "5940 single column tabletop universal material testing machine," the strength of the granules was evaluated according to the Japanese Industrial Standard JIS Z 8841 (granules - strength test method). The diameter of the granules was measured in the vertical and horizontal directions, and the average diameter was used. In the measurement, the sample shape was granular, and the displacement speed was 2 mm / min. In order to reduce measurement errors due to differences in each particle, 10 points were measured for each type of sample, and the average value was used as the measurement value.
[0057] <Water vapor adsorption isotherm> The water vapor adsorption isotherm at 35°C was measured using an adsorption isotherm measuring device (Belsorp 18, manufactured by Nippon Bell Co., Ltd.). The zeolite membrane composite was cut to an appropriate size in advance so as to fit into the measurement cell, and heated and dried at 120°C for 5 hours while evacuating to a vacuum before use. The measurements were performed at an air thermostat temperature of 50°C, an adsorption temperature of 35°C, and an initial introduction pressure of 3 torr (4.00 × 10 2 Pa), saturated vapor pressure 42.181torr (56.237×10 2 Pa) and equilibration time was 500 seconds.
[0058] Example 1 (Preparation of Silicoaluminophosphate) To a mixture of 210.5 parts by mass of water and 83.7 parts by mass of 85% phosphoric acid, 56.4 parts by mass of pseudoboehmite (containing 25% by mass of water, CATAPAL C1 manufactured by SASOL) was slowly added and mixed with stirring for 3 hours. A slurry of 6.2 parts by mass of fumed silica (Aerosil 200) suspended in 210.5 parts by mass of water was added, followed by the addition of 32.5 parts by mass of morpholine and 41.5 parts by mass of triethylamine, and the mixture was stirred for 3 hours to obtain a starting reactant having the following composition. 0.25SiO2 / Al2O3 / 0.875P2O5 / 0.9Morpholine / 0.99Triethylamine / 60H2O
[0059] The above starting reactants were charged into a stainless steel autoclave and reacted at 185°C for 2 days with stirring. After the reaction, the mixture was cooled, the supernatant was removed by decantation, and the precipitate was collected. The precipitate was washed with water three times by decantation, filtered, and dried at 100°C. XRD measurement confirmed that the precipitate was a pure CHA-structure silicoaluminophosphate.
[0060] (Production of molded bodies: rolling granulation) 100 parts by mass of silicoaluminophosphate and 1 part by mass of Shin-Etsu Chemical's Metrose (SM-100) as a plasticizer were charged into an agitation granulator and mixed with stirring. Next, 20 parts by mass of methyl silicate (MKS Silicate (registered trademark) MS51, manufactured by Mitsubishi Chemical Corporation, the average value of n in the general formula (I): about 5) was added as a binder precursor and mixed with stirring. While rotating at 30 rpm, water was sprayed to the pot mixer charged with the mixed raw materials to grow the particles to 1 to 2 mm. Thereafter, the granules were removed from the mixer and air-dried, then dried at 100°C for 4 hours under reduced pressure, and sieved to 1.60 to 2.38 mm to recover, to obtain granules. The granules were fired in a batch rotary kiln at 700°C for 6 hours under 5% oxygen flow to obtain the porous molded body of the present invention. The sphericity of this porous molded body was 0.96, and the compressive strength was 4.03 MPa. In addition, the particle size range was 1.60 to 2.38 mm due to sieving.
[0061] Comparative Example 1 Silicoaluminophosphate was press molded and crushed, and then sieved to 1.70-2.36 mm. The sphericity of the granules was 0.69, and the compressive strength was 1.84 MPa. The particle size range was 1.70-2.38 mm due to sieving.
[0062] Comparative Example 2 The water vapor adsorption isotherm of the silicoaluminophosphate obtained in Example 1, which was not granulated but was calcined at 700°C for 6 hours, showed the same profile as the water vapor adsorption isotherm of Example 1 of the present application. That is, the molded body of this example showed almost no deterioration in the adsorption properties due to granulation, and it was found that the adsorption properties of the silicoaluminophosphate were maintained. The results are shown in Figure 1. Figure 1 shows that there is a relative vapor pressure region where the change in the amount of water adsorption is 0.12 g / g or more when the relative vapor pressure changes by 0.15 in the range of relative vapor pressures of 0.01 or more and 0.30 or less. Cases where such a region is present are marked with an "O" in Table 1. For example, in Example 1, it can be seen that the amount of water adsorption rises rapidly in the region of relative vapor pressures of 0.01 or more, and that the amount of water adsorption increases by about 0.2 g / g when the relative vapor pressure changes by only about 0.1, where the relative vapor pressure is 0.15 or less.
[0063] [Table 1] [Industrial Applicability]
[0064] According to the porous molded body of the present invention, it is possible to provide a porous molded body that has excellent physical properties such as abrasion resistance and impact resistance, can maintain its shape and particle size even when used in a fluidized state, and exhibits high adsorption capacity, even in a heat pump in which an adsorbent such as zeolite is moved like a moving bed. By using the porous molded body of the present invention, it is possible to miniaturize the heat pump, and it can be suitably used for applications such as automobiles. Therefore, this technology is an industrially valuable technology.
Claims
1. The porous molded body for moving bed adsorption contains an aluminophosphate zeolite and a binder, and has a particle size range of 50 to 5000 μm and a compressive strength of 2 MPa or more.
2. 2. The porous molded body for moving bed adsorption according to claim 1, which has a relative vapor pressure region in which the change in the amount of water adsorbed is 0.12 g / g or more when the relative vapor pressure changes by 0.15 in the range of relative vapor pressures of 0.01 or more and 0.30 or less in a water vapor adsorption isotherm measured at 25°C.
3. 2. The porous molded body for moving bed adsorption according to claim 1, wherein the molar ratio of Si, P, Al, and Me (wherein Me represents a heteroatom that can substitute for part of Al in the aluminophosphate framework) in the porous molded body for moving bed adsorption satisfies the following formula: 1.02≦(Si+P) / (Al+Me)≦1.4
4. 2. The porous molded body for moving bed adsorption according to claim 1, characterized in that it is obtained from a reaction mixture containing at least an aluminophosphate and a binder precursor, and the binder precursor contains a compound of the following formula (I) or silica sol: 【Chemistry 1】 (In formula (I), each R is independently an optionally substituted alkyl group, aryl group, alkenyl group, alkynyl group, alkoxy group, or aryloxy group; each R' is independently an optionally substituted alkyl group, aryl group, alkenyl group, or alkynyl group; and n is a number from 1 to 100.)
5. 2. The porous molded body for moving bed adsorption according to claim 1, wherein the pore volume in the pore diameter range of 0.1 to 5 μm is 0.05 cc / g or more and 0.5 cc / g or less.
6. 6. The method for producing a porous molded body for adsorption according to claim 1, wherein a reactive mixture containing at least an aluminophosphate and a binder precursor is granulated by tumbling granulation.
7. A moving bed adsorption method using the porous molded body according to any one of claims 1 to 5.
8. 8. The moving bed adsorption process of claim 7, wherein the porous shaped body is the adsorbent and water or carbon dioxide is the adsorbate.
Citation Information
Patent Citations
Alumino-phosphate granule and method for manufacturing the same
JP2005272296A
Method for synthesizing aluminophosphates
JP2006273710A
Crystalline silica aluminophosphate and method of synthesizing the same
JP2012091997A
Improved method for producing zeolite-metal chloride hybrid moisture adsorbent, method for producing moisture adsorbent produced by same, and method for producing moisture adsorbent composition for surface coating containing the same
JP2018518358A
Improved method of the manufacturing for the zeolite-metal halide hybrid adsorbent, and the adsorbent produced thereby, and method of manufacturing for coating composite comprising the same