Method for manufacturing sintered body substrate and method for manufacturing light-emitting device

By creating a ceramic substrate with through holes and using a powdered mold release material to smooth the conductive surface, the method addresses the uneven surface issue in ceramic substrates, resulting in improved mounting performance and reliability of light-emitting devices.

JP2024146183APending Publication Date: 2024-10-15NICHIA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023058931
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The uneven surface of active metal brazing materials during firing in ceramic substrates complicates the mounting process, making it difficult to achieve good mounting performance.

Method used

A method involving the preparation of a ceramic substrate with through holes, application of metal and active metal powders with an organic solvent to create convex portions, firing a conductive paste to form a metal member, and using a powdered mold release material to achieve a smooth, flat conductive surface by heating and pressurizing.

Benefits of technology

This method results in a sintered body substrate with improved mounting performance by ensuring a smooth, crack-free, and flat conductive surface, enhancing the bonding strength and reliability of light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146183000001_ABST
    Figure 2024146183000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a sintered body substrate having good mountability, and a method for manufacturing a light-emitting device.SOLUTION: A method for manufacturing the sintered body substrate includes: preparing a ceramic substrate that has a first surface and a second surface opposite to the first surface, and has a through hole which penetrates the ceramic substrate so as to connect the first surface with the second surface; arranging an electroconductive paste that contains at least metal powder, active metal powder and an organic solvent in the through hole, so as to have a protrusion which protrudes from the first surface or the second surface; obtaining a metal member by firing the arranged electroconductive paste; interposing a powdery release material on a surface of the metal member, heating the metal member to a temperature at which the metal member is melted, and pressurizing the resultant metal member; and removing the powdery release material from the metal member.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a sintered body substrate and a method for manufacturing a light emitting device. [Background technology]

[0002] Conventionally, active metal brazing materials have been used for vias and wiring in ceramic substrates with high thermal conductivity, such as Si3N4 substrates. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6122561 [Patent Document 2] Patent No. 5922739 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the case of a ceramic substrate, unevenness occurs on the surface of the active metal brazing material during firing, which may make mounting difficult. An object of the embodiments of the present disclosure is to provide a method for manufacturing a sintered body substrate with good mountability and a method for manufacturing a light emitting device. [Means for solving the problem]

[0005] A manufacturing method of a sintered substrate disclosed in an embodiment includes preparing a ceramic substrate having a first surface and a second surface opposite to the first surface, the ceramic substrate having a through hole penetrating to connect the first surface and the second surface; arranging a conductive paste containing at least a metal powder, an active metal powder, and an organic solvent in the through hole so as to have a convex portion protruding from the first surface or the second surface; sintering the arranged conductive paste to obtain a metal member; interposing a powdered release material on the surface of the metal member, heating and pressurizing the metal member to a temperature at which the metal member melts; and removing the powdered release material from the metal member.

[0006] Furthermore, the manufacturing method of the light emitting device disclosed in the embodiment includes preparing a sintered substrate manufactured by the manufacturing method of the sintered substrate described above, and arranging a light emitting element on a conductive portion of the metal member from which the powdered release agent has been removed, and in arranging the light emitting element, the conductive portion and the light emitting element are electrically connected directly or indirectly. Effect of the Invention

[0007] According to the embodiments of the present disclosure, it is possible to provide a method for manufacturing a sintered body substrate and a method for manufacturing a light emitting device that have excellent mountability. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a plan view showing a schematic view of a sintered body substrate according to an embodiment. [Diagram 2] FIG. 2 is a perspective cross-sectional view taken along line II-II in FIG. [Diagram 3] 4 is a flowchart illustrating a method for manufacturing a sintered substrate according to an embodiment. [Figure 4A] FIG. 2 is a cross-sectional view that illustrates a ceramic substrate in a method for manufacturing a sintered substrate according to an embodiment. [Figure 4B] FIG. 2 is an end view showing a schematic diagram of a recess formed in a ceramic substrate in a manufacturing method for a sintered substrate according to an embodiment. [Figure 4C]3 is a schematic end view showing a through hole formed in a recess of a ceramic substrate in a manufacturing method of a sintered substrate according to an embodiment of the present invention; FIG. [Figure 4D] 4 is an end view showing a state in which a conductive paste is placed in recesses and through holes of a ceramic substrate in a manufacturing method of a sintered substrate according to an embodiment of the present invention; FIG. [Figure 5A] 4 is an end view showing a state in which a conductive paste is placed in a through hole and a recess in a method for producing a sintered body substrate according to an embodiment of the present invention; FIG. [Figure 5B] FIG. 2 is an end view that typically shows a state in which a metal member is obtained by firing a conductive paste in a manufacturing method for a sintered substrate according to an embodiment. [Figure 5C] FIG. 2 is an end view that illustrates a state in which a powdery release material is placed on a metal member in a manufacturing method for a sintered substrate according to an embodiment. [Figure 5D] FIG. 2 is an end view that shows a schematic diagram of a state in which a powdery release material is interposed between the metal member and the substrate, the metal member being heated to a temperature at which the metal member melts and pressed, in a manufacturing method for a sintered substrate according to an embodiment. [Figure 5E] 4 is an end view that typically shows the state of a metal member after heating and pressure are applied in a manufacturing method for a sintered substrate according to an embodiment. FIG. [Figure 5F] FIG. 2 is an end view that shows a schematic diagram of a sintered body substrate in which a powdery release agent is removed from a metal member to form a conductive portion in a manufacturing method for a sintered body substrate according to an embodiment. [Figure 6A] 4 is a plan view photograph illustrating a portion of an end face of a conductive portion of a sintered body substrate according to an embodiment. [Figure 6B] 1 is a plan view photograph illustrating a portion of an end face of a conventional conductive portion. [Figure 6C] 1 is a cross-sectional photograph illustrating a portion of a conventional conductive portion. [Figure 7A] FIG. 11 is a cross-sectional view that illustrates a state in which a powdery release material is placed on the side of a heat press machine in a method for producing a sintered substrate according to an application example of an embodiment. [Figure 7B] FIG. 11 is a cross-sectional view that typically illustrates a state in which a metal member is heated and pressed by a hot press machine with a powdered release material interposed therebetween in a manufacturing method for a sintered substrate according to an application example of an embodiment. [Figure 8] 1 is a cross-sectional view illustrating a schematic view of a light-emitting device according to an embodiment. [Figure 9] 4 is a flowchart illustrating a method for manufacturing a light emitting device according to an embodiment. [Figure 10A] 4 is a cross-sectional view illustrating a state in which a bonding member is disposed on a sintered body substrate in a manufacturing method for a light emitting device according to an embodiment. FIG. [Figure 10B] 4 is a cross-sectional view showing a state in which a light-emitting element is arranged in a method for manufacturing a light-emitting device according to an embodiment. FIG. [Figure 10C] 11A and 11B are cross-sectional views illustrating a state in which a light reflecting member is disposed in a manufacturing method for a light emitting device according to an application example of the embodiment. [Figure 11] FIG. 11 is a cross-sectional view illustrating a sintered body substrate according to another embodiment. [Figure 12] 10 is a flowchart illustrating a method for manufacturing a sintered substrate according to another embodiment. [Figure 13A] 10 is a cross-sectional view that illustrates a ceramic substrate having a through hole formed therein, in a method for manufacturing a sintered substrate according to another embodiment of the present invention. FIG. [Figure 13B] 10 is a cross-sectional view showing a state in which a conductive paste is disposed in a through hole so as to have a convex portion protruding from a surface of a ceramic substrate, in a manufacturing method for a sintered substrate according to another embodiment. FIG. [Figure 13C] FIG. 11 is a cross-sectional view that typically shows a state in which a conductive paste has been fired in a method for producing a sintered body substrate according to another embodiment. [Figure 13D] FIG. 11 is a cross-sectional view that typically illustrates a state in which a powdered release material is placed on a metal member and heated and pressed in a method for producing a sintered substrate according to another embodiment. [Figure 13E] FIG. 11 is a cross-sectional view that illustrates a schematic state after a powdered release material is placed on a metal member and heated and pressed in a method for producing a sintered substrate according to another embodiment. [Figure 13F] FIG. 11 is a cross-sectional view that illustrates a state in which a powdery release agent is removed from a metal member to form a conductive portion in a method for producing a sintered substrate according to another embodiment. [Figure 13G]FIG. 11 is a cross-sectional view that illustrates a schematic state in which a wiring portion and a bonding member are disposed on a conductive portion in a method for manufacturing a sintered body substrate according to another embodiment. [Figure 14] FIG. 11 is a cross-sectional view illustrating a light-emitting device according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment according to the present disclosure will be described with reference to the drawings. However, the embodiment described below is for embodying the technical idea according to the present disclosure, and the invention is not limited to the following unless otherwise specified. The contents described in one embodiment can be applied to other embodiments and modified examples. In addition, the drawings are schematic diagrams of the embodiments, and in order to clarify the description, the scale, interval, positional relationship, etc. of each member may be exaggerated, or some of the members may be omitted. The directions shown in each figure indicate the relative positions between the components, and are not intended to indicate absolute positions. In addition, even if a cross section is written for convenience of description, it may be an end face, and vice versa. In addition, the same name and symbol indicate, in principle, the same or homogeneous members, and detailed description will be omitted as appropriate. In addition, in the embodiment, "covering" is not limited to direct contact, but also includes indirect covering, for example, via other members. In addition, "disposing" is not limited to direct contact, but also includes indirect disposing, for example, via other members.

[0010] [Sintered body substrate] A sintered body substrate 10 according to an embodiment will be described with reference to Fig. 1 and Fig. 2. Fig. 1 is a plan view showing a sintered body substrate according to an embodiment. Fig. 2 is a perspective cross-sectional view taken along line II-II in Fig. 1.

[0011] The sintered body substrate 10 includes a ceramic substrate 1 having a first surface 1A and a second surface 1B opposite to the first surface 1A, a through hole 2 penetrating the ceramic substrate 1 so as to connect the first surface 1A and the second surface 1B, and a conductive portion 3 disposed in the through hole 2. The conductive portion 3 includes a metal 45 and a reaction layer 6a of a metal compound 6 disposed on an inner wall defining the through hole. The ceramic substrate 1 will be described assuming that at least one of the first surface 1A and the second surface 1B has a recess 9 having a larger diameter than the through hole 2 and continuing to the through hole 2. Although the ceramic substrate 10 is illustrated with a bonding member 11 disposed therein, the bonding member 11 is used when bonding the sintered body substrate 10 to a light emitting element 20 or the like, and may not be included in the sintered body substrate 10. Each component of the sintered body substrate 10 will be described below.

[0012] (Ceramics Substrate) The ceramic substrate 1 is a plate-like member that serves as the base of the sintered body substrate 10. The planar shape of the ceramic substrate 1 is, for example, rectangular. The planar shape of the ceramic substrate 1 is not particularly limited. For example, the ceramic substrate 1 is preferably a ceramic substrate that has already been fired and hardened. For example, the ceramic substrate 1 is preferably one that contains at least one of silicon nitride, aluminum nitride, boron nitride, magnesium oxide, and aluminum oxide. For the ceramic substrate 1, nitride-based ceramics such as silicon nitride, aluminum nitride, and boron nitride are preferable, but oxide-based ceramics such as aluminum oxide, silicon oxide, calcium oxide, and magnesium oxide may also be used. For the ceramic substrate 1, beryllium oxide, silicon carbide, mullite, borosilicate glass, and the like may also be used.

[0013] The ceramic substrate 1 has a through hole 2 at a predetermined position in the plate thickness direction so as to communicate between the first surface 1A and the second surface 1B, and a conductive portion 3 is disposed inside the through hole 2. The ceramic substrate 1 also has a recess in at least one of the first surface 1A and the second surface 1B, the hole diameter of which is larger than that of the through hole 2 and which communicates with the through hole 2. As an example, the through hole 2 of the ceramic substrate 1 is disposed at a position within the recess 9 disposed on the first surface 1A and the second surface 1B. Here, the recess 9 includes a first recess 9a disposed on the first surface 1A and a second recess 9b disposed on the second surface 1B, and the through hole 2 is disposed so as to communicate between the first recess 9a and the second recess 9b. The first recess 9a and the second recess 9b are disposed at positions facing each other, and have a larger inner diameter than the through hole 2. Note that the inner diameter, diameter, or radius of the through hole 2 and the recess 9 is the length of the diagonal if they are rectangular. The through hole 2 is arranged in the recess 9 of the portion that requires electrical conduction from the first surface 1A side to the second surface 1B side of the ceramic substrate 1. Here, the through hole 2 is arranged so as to communicate with the recess 9 of the portion that becomes the wiring pad arranged on the ceramic substrate 1. The wiring pad is a portion that becomes an electrode on which electronic components and the like are arranged. It is preferable that the recess 9 is also arranged in the portion of the wiring that continues to the wiring pad. By having the recess 9 at a position that becomes the wiring, the adhesion between the ceramic substrate 1 and the wiring can be improved. The through hole 2 is a portion that becomes a via hole for electrically connecting the element electrode 24 of the light emitting element 20 to the wiring pad or wiring on the opposite side of the sintered body substrate 10 via the conductive portion 3 arranged inside.

[0014] In the ceramic substrate 1, as an example, the through hole 2 is illustrated as being arranged at one location approximately at the center of each recess 9. The through hole 2 may be arranged in a plurality of recesses 9. Although the through hole 2 is illustrated as having the same diameter from one end to the other end, the hole diameter on the opposite side may be larger than the side to which the element electrode is connected. In a plan view, the opening shape of the through hole 2 may be a circle or a polygon, and if it is a quadrangle, it may be a trapezoid or a parallelogram, or may be a triangle, a pentagon, or a hexagon. By making the opening shape of the through hole 2 polygonal, it can be made to match the shape of the electrode of the light-emitting element, and it is possible to increase electrical conductivity and improve heat dissipation. When the opening shape of the through hole 2 is polygonal, it is preferable that the corners of the opening shape are rounded. By making the opening shape of the through hole 2 polygonal, it is possible to increase the opening area continuing to the recess 9. The maximum diameter (diameter or diagonal length) of the through hole 2 is preferably 0.05 mm or more and 0.5 mm or less. If the through hole 2 is 0.05 mm or more, it becomes easier to fill the conductive paste 3A before firing, and the conductivity can be improved. If the through hole 2 is 0.5 mm or less, the strength can be maintained and the amount of the conductive paste 3A to be filled can be reduced. If the through hole 2 is polygonal, the maximum diameter is the length of the diagonal.

[0015] (Conductive part) The conductive part 3 is disposed in the through hole 2 or in the recess 9 of the ceramic substrate 1, or in both the through hole 2 and the recess 9. The conductive part 3 is a member that electrically connects to the light emitting element 20, either alone or together with wiring. The conductive part 3 is obtained by sintering the conductive paste 3A to become a metal member 33, as described later, heating and pressing the metal member 33 with a powdery release agent 60 interposed therebetween so that the metal member 33 melts, and removing the powdery release agent 60. Here, the conductive part 3 includes a first part 13 disposed in the through hole 2, and a second part (wiring part) 8 disposed in a recess 9 disposed in at least one of the first surface 1A and the second surface 1B in contact with the first part 13. In the drawing, the second part 8 is provided on both the first surface 1A and the second surface 1B. The second part 8 of the conductive part 3 is disposed in the recess 9 so as to be flush with the surface of the ceramic substrate 1. In addition, the second portion 8 may function as a wiring or a wiring pad of the ceramic substrate 1, either alone or together with the bonding member 11.

[0016] The conductive part 3 includes, for example, a metal 45 and a reaction layer 6a of a metal compound disposed on the inner wall that defines the through hole 2. The conductive part 3 has at least the metal 45 and the reaction layer 6a and a reactant as the metal compound 6. The conductive part 3 includes, for example, an inorganic filler 7 that does not contain metal, and the reaction product of the metal compound 6 is also disposed around the inorganic filler 7. As shown in FIG. 6B and FIG. 6C, the conventional conductive part 300 is in a stone wall state or has gaps H like bubble-like holes, so that even if the conductive part 300 is polished or ground, it is difficult to form a flat surface with few irregularities, and the amount of polishing or grinding required to make the flat surface is large. In contrast, in this embodiment, the conductive part 3 is flat, so that even if the conductive part 3 is polished or ground, it is easy to form a flat surface, and the amount of polishing or grinding required to make the flat surface can be reduced. Fig. 6A is a planar photograph illustrating a part of an end face of a conductive part of a sintered body substrate according to an embodiment, Fig. 6B is a planar photograph illustrating a part of an end face of a conventional conductive part, and Fig. 6C is a cross-sectional photograph illustrating a part of a conventional conductive part.

[0017] 2, in the conductive portion 3, the metal compound 6 is disposed as a reaction layer 6a of the metal compound 6 on the inner walls that define the recesses 9 and the through-holes 2 of the ceramic substrate 1. When the conductive portion 3 contains an inorganic filler 7, the metal compound 6 is disposed around the inorganic filler 7, and when the metal 45 contains a specific component as described below, the metal compound 6 is disposed around the specific component as a reaction product of the metal compound 6. In addition, by containing the inorganic filler 7, the conductive portion 3 disperses the components contained in the metal 45 more evenly.

[0018] As an example, the metal 45 contains the metal compound 6. The metal 45 preferably contains at least one of Ag, Al, Zn, Sn, and an Ag-Cu alloy. The metal 45 may also contain at least one of Cu, Cr, and Ni. When the metal 45 contains at least one of the above-mentioned Cu, Cr, and Ni components, the reaction product of the metal compound 6 is formed around the component.

[0019] In the conductive portion 3, the metal compound 6 includes, for example, a reaction layer 6a of the metal compound 6 and a reactant of the metal compound 6. Before firing, the metal compound 6 is an active metal powder 6A, and preferably includes at least one of TiH2 (titanium hydride), CeH2, ZrH2, and MgH2. After firing, the metal compound 6 includes a reaction layer 6a arranged on the inner wall defining the recess 9 and the through hole 2 of the ceramic substrate 1, a reactant of the metal compound 6 arranged on the surface of the component when the metal 45 includes the specific component described above, and a reactant arranged around the inorganic filler 7 when the inorganic filler 7 is included.

[0020] It is particularly preferable to use TiH2 as the metal compound 6. When the metal compound 6 contains TiH2, it reacts with nitrogen in the ceramic components of the ceramic substrate 1 when the ceramic substrate 1 contains nitrogen, forming a reaction layer 6a containing TiN at the interface with the ceramic substrate 1, improving the adhesion between the conductive portion 3 and the ceramic substrate 1, and enabling the conductive portion 3 to adhere firmly to the inner wall of the through hole 2.

[0021] The conductive part 3 preferably has an arithmetic mean roughness Ra of 0.01 μm or more and 1.5 μm or less of the end face (surface of the second part 8) exposed from the ceramic substrate. The arithmetic mean roughness Ra of the end face of the conductive part 3 is more preferably 1.0 μm or less, even more preferably 0.5 μm or less, and most preferably 0.1 μm or less. When the arithmetic mean roughness Ra is 1.5 μm or less, the element electrode connected directly or via the bonding member 11 to the end face (surface of the second part 8) of the conductive part 3 can be stably bonded. The end face of the conductive part 3 is in a state in which the conductive paste 3A is sintered to form the metal member 33 in the manufacturing method described later, and the end face of the metal member 33 is heated and pressed via the powdered release material 60 at a temperature at which the metal member 33 melts, and then polished or ground. The arithmetic mean roughness (Ra), which is the surface roughness of the end face of the conductive portion 3 (the surface of the second portion 8), may be measured using a stylus-type measuring instrument that uses a stylus, or a non-stylus-type measuring instrument that uses a laser, in accordance with the international standard ISO 25178 surface quality (surface roughness measurement) (in accordance with JIS B 0601).

[0022] (Inorganic filler) The inorganic filler 7 is dispersed in the conductive part 3 to reduce the occurrence of cracks. The inorganic filler 7A before firing is, for example, a plurality of granular members other than metal, and examples of the ceramic filler include crystalline fillers such as aluminum oxide and silicon dioxide, and amorphous fillers such as glass. The inorganic filler 7A before firing contained in the conductive part 3 is contained in the conductive paste 3A in a content range that does not interfere with the effects of other ingredients.

[0023] (Organic solvent) Organic solvent 7B (see FIG. 5D) is a material contained in conductive paste 3A before firing. After firing, organic solvent 7B evaporates and does not remain in conductive portion 3. As an example, organic solvent 7B may be a solvent and resin material that is generally used as a via material. Note that a resin may be contained in conductive paste 3A in addition to organic solvent 7B. It is preferable to use a paste-like resin as the resin to be contained.

[0024] (Wiring section) As an example, the wiring portion is arranged as the second portion 8 of the conductive portion 3 in FIG. 1 and FIG. 2. The wiring portion is a wiring pattern arranged on the ceramic substrate 1 as the second portion 8 of the conductive portion 3 in advance, and forms a wiring pad or an external connection electrode, wiring connected thereto, and the like. The wiring portion is arranged as the second conductive paste 3A2 (see FIG. 5A) before firing, for example. The wiring portion is arranged as the second portion 8 of the conductive portion 3 so as to be continuous with the first portion 13 of the conductive portion 3, and here, is arranged as the second portion 8 of the conductive portion 3 in each of the recesses 9 on the first surface 1A side and the second surface 1B side of the ceramic substrate 1. The second portion 8 as the wiring portion is arranged so as to be flush with the surface of the ceramic substrate 1. As an example, the second portion 8 of the conductive portion 3 serving as the wiring portion has a bonding member 11 such as a plating layer arranged thereon. The wiring portion as the second portion 8 is illustrated as a rectangle in a plan view as an example, but its shape and arrangement are arbitrary and are not limited.

[0025] Also, the second portion 8, which is a wiring portion, may be made of, for example, the same material as the first portion 13 as the second portion 8 of the conductive portion 3. The material of the metal member used as the joining member 11 may be, for example, a mixture of a resin binder using a simple substance such as gold, silver, copper, platinum, and aluminum, or an alloy or mixed powder thereof and a resin. The resin used as the binder may be, for example, a thermosetting resin such as an epoxy resin or a silicone resin. Also, it is preferable that the joining member 11 contains a reducing agent such as an organic acid. This reduces oxidation in the joining member 11 and reduces the electrical resistance in the connection.

[0026] In the sintered body substrate 10 having the above-mentioned configuration, the end face of the conductive part 3 is a smooth flat surface without irregularities or cracks as shown in Fig. 6A. Therefore, when the element electrode 24 of the light emitting element 20 is connected to the conductive part 3 directly or via a bonding member 11 such as a plating layer, the sintered body substrate 10 can improve the contact state and the reliability of the substrate. In addition, since the sintered body substrate 10 has the reaction layer 6a of the metal compound disposed in the portion that defines the recess 9 and the through hole 2 of the ceramic substrate 1, the connection strength of the conductive part 3 is improved, and the performance such as the reliability of the substrate can be improved.

[0027] [Method of manufacturing sintered body substrate] Next, a method for manufacturing a sintered body substrate according to an embodiment will be described with reference to FIG. 3 to FIG. 5F. FIG. 3 is a flow chart illustrating a method for manufacturing a sintered body substrate according to an embodiment. FIG. 4A is a cross-sectional view that typically illustrates a ceramic substrate in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 4B is an end view that typically illustrates a recess formed in a ceramic substrate in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 4C is an end view that typically illustrates a through hole formed in a recess of a ceramic substrate in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 4D is an end view that typically illustrates a state in which a conductive paste is placed in the recess and the through hole of a ceramic substrate in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 5A is an end view that typically illustrates a state in which a conductive paste is placed in the through hole and the recess in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 5B is an end view that typically illustrates a state in which a metal member is obtained by firing a conductive paste in a method for manufacturing a sintered body substrate according to an embodiment. FIG. 5C is an end view that typically illustrates a state in which a powdery release agent is placed on a metal member in a method for manufacturing a sintered body substrate according to an embodiment. Fig. 5D is an end view showing a state where a metal member is heated and pressed to a temperature at which the metal member melts with a powdery release agent interposed therebetween in the method for producing a sintered body substrate according to the embodiment. Fig. 5E is an end view showing a state of the metal member after heating and pressing in the method for producing a sintered body substrate according to the embodiment. Fig. 5F is an end view showing a sintered body substrate having a conductive part obtained by removing the powdery release agent from the metal member in the method for producing a sintered body substrate according to the embodiment.

[0028] The manufacturing method S10 of the sintered body substrate includes the steps of: preparing a ceramic substrate 1 having a first surface 1A and a second surface 1B opposite to the first surface 1A, and a through hole 2 penetrating so as to connect the first surface 1A and the second surface 1B; disposing a conductive paste 3A containing at least a metal powder 45A, an active metal powder 6A, and an organic solvent 7B in the through hole 2 so as to have a protruding portion 3A3 protruding from the first surface 1A or the second surface 1B; sintering the disposed conductive paste 3A to obtain a metal member 33; interposing a powdered release material 60 on the surface of the metal member 33, heating and pressing the metal member 33 to a temperature at which the metal member 33 melts; and removing the powdered release material 60 from the metal member 33. Note that in the manufacturing method S10 of the sintered body substrate, the ceramic substrate is prepared by providing a recess 9 disposed on at least one of the first surface 1A and the second surface 1B (both in the drawing) and providing a through hole 2 at the position of the recess 9. That is, the manufacturing method S10 of the sintered substrate includes preparing a ceramic substrate S11, arranging a conductive paste so as to have a convex portion S12, sintering to obtain a metal member S13, heating and pressurizing with a powdered release agent interposed therebetween S14, and removing the powdered release agent S15.

[0029] (Prepare a ceramic substrate) Preparing a ceramic substrate S11 (hereinafter referred to as step S11) is to prepare a ceramic substrate 1 having a through hole 2 penetrating so as to connect the first surface 1A and the second surface 1B. The ceramic substrate 1 used here has already been fired and hardened. In this step S11, in the ceramic substrate 1 to be prepared, a first recess 9a is formed so as to be larger than the diameter of the opening area of ​​the through hole 2 in the first surface 1A, and a second recess 9b is formed so as to be larger than the diameter of the opening area of ​​the through hole 2 in the second surface 1B. In step S11, as an example, a flat substrate made of a material containing at least one of silicon nitride, aluminum nitride, and boron nitride is used as the ceramic substrate 1. In this step S11, the prepared ceramic substrate 1 is subjected to laser processing or the like in which laser light is irradiated from each of the first surface 1A and the second surface 1B of the ceramic substrate 1 to form the first recess 9a, the second recess 9b, and the through hole 2, which is circular in plan view, and the through hole 2 is also formed so as to communicate the first recess 9a and the second recess 9b. The ceramic substrate 1 may be prepared in a state in which the number of through holes 2 corresponds to the size of the area in which the plurality of light-emitting elements 20 are arranged and the number of element electrodes 24, or may be prepared by cutting into a size in which a predetermined number of light-emitting elements 20 are arranged.

[0030] In step S11, the through holes 2 formed in the ceramic substrate 1 are formed to have a circular shape in a plan view, and when cut in a direction perpendicular to the ceramic substrate 1, the cross section of the through holes 2 is rectangular, and the through holes 2 have a constant width. The maximum diameter of the through holes 2 is preferably 0.05 mm or more and 0.5 mm or less. Furthermore, the through holes 2 may be formed so that the opening area of ​​the second surface 1B side, which is the opposite side to the side connected to the element electrode 24 of the light emitting element 20, is wider. When the opening area of ​​the through holes 2 on the second surface 1B side is wider than that on the first surface 1A side, the heat dissipation property is excellent.

[0031] (Placing conductive paste) The step S12 of disposing the conductive paste (hereinafter referred to as step S12) is to dispose the conductive paste 3A in the through holes 2 and the recesses 9 formed in the ceramic substrate 1. In this step S12, the conductive paste 3A is disposed through a mask MA so as to have protruding portions 3A3 protruding from the first surface 1A and the second surface 1B of the ceramic substrate 1. In this step S12, the conductive paste 3A is applied to both surfaces of the ceramic substrate 1 through the mask MA by, for example, screen printing, so that the conductive paste 3A is disposed in the through holes 2 and the recesses 9 as well so as to have protruding portions 3A3. The conductive paste 3A is disposed on the first surface 1A of the ceramic substrate 1 by screen printing with a constant thickness through the mask MA, and is further disposed on the second surface 1B of the ceramic substrate 1 by screen printing with a constant thickness through the mask MA. It is preferable that the first conductive paste 3A1 in the portion that will become the first portion 13 after firing and the second conductive paste 3a2 in the portion that will become the second portion 8 are arranged continuously or by the same series of screen printing or the like. Note that the protruding portion 3A3 of the conductive paste 3A is finally removed by polishing or grinding.

[0032] It is preferable that the conductive paste 3A is made of the same material for the portion that is disposed in the through hole 2 and becomes the first portion 13 after firing, and the portion that becomes the second portion 8 after firing. The conductive paste 3A includes at least a metal powder 45A, an active metal powder 6A, and an organic solvent 7B, and may further include a resin. The metal powder 45A may include at least one of Ag, Al, Zn, Sn, and an Ag-Cu alloy. In addition to the metal powder 45A, the conductive paste 3A may further include Cu, Cr, and Ni components. The conductive paste 3A includes, for example, 63% to 85% by mass of the metal powder 45A, 1% to 15% by mass of the active metal powder 6A, 5% to 15% by mass of the organic solvent 7B as a solvent, and includes an inorganic filler 7A other than metal and a resin in an allowable range of mass%. It is more preferable that the active metal powder 6A is contained in an amount of 1 part by weight or more and 5 parts by weight or less when the total weight of the other components is taken as 100. The conductive paste 3A (first conductive paste 3A1 and second conductive paste 3A2) used in step S12 has fluidity by containing a paste-like resin together with the organic solvent 7B, and can be freely filled into through holes 2 and recesses 9 of any shape, and can be applied and arranged in any shape and thickness to have protrusions 3A3.

[0033] In this step S12, the metal powder 45A preferably contains at least one of Ag, Al, Zn, Sn, and Ag-Cu alloy powder, and as an example, Ag-Cu alloy powder is used. Furthermore, the metal powder 45A may contain at least one of Cu, Cr, and Ni, and as an example, Cu powder is used. When the metal powder 45A is at least one of Ag, Al, Zn, Sn, and Ag-Cu alloy powder, the melting point of the metal powder component is preferably 200°C or more and 1000°C or less. Furthermore, when the metal powder 45A contains at least one of Cu, Cr, and Ni, the melting point of the metal powder component is preferably 1050°C or more and 2500°C or less. In this step S12, the median diameter of the metal powder 45A is preferably 1 μm or more and 50 μm or less.

[0034] In this step S12, the active metal powder 6A preferably contains at least one of TiH2, CeH2, ZrH2, and MgH2, and as an example, TiH2 is used. The content of the active metal powder 6A is preferably 1 part by weight or more and 5 parts by weight or less, as described above. By making the content of the active metal powder 6A 1 part by weight or more, the reaction layer 6a of the metal compound 6 after firing and the reaction product can be formed with the minimum necessary. Furthermore, if the content of the active metal powder 6A is 5 parts by weight or less, the reaction layer 6a of the metal compound 6 after firing and the reaction product can be formed inexpensively.

[0035] In step S12, for example, when the conductive paste 3A is disposed by screen printing, the mask MA is disposed on the first surface 1A and the second surface 1B of the ceramic substrate 1 at positions other than the recesses 9, and therefore, once the disposition of the conductive paste 3A is completed, the mask disposed on the first surface 1A and the second surface 1B of the ceramic substrate 1 may be removed. Moreover, the mask MA may be removed by firing when the conductive paste 3A is fired in the next step.

[0036] (Firing conductive paste to obtain metal parts) Next, the conductive paste is fired to obtain a metal material S13 (hereinafter referred to as step S13). In this step S13, a firing furnace such as an electric furnace is used, and the firing temperature is set to 780°C or more and 1100°C or less. The firing temperature is preferably set to 850°C or more and 1050°C or less. In addition, in the case of firing in step S13, the firing atmosphere is preferably a vacuum atmosphere of 10 Pa or less or an Ar atmosphere of 99.9% or more. By performing this step S13, the surface of the protruding portion 3A3 of the conductive paste 3A arranged on the ceramic substrate 1 becomes a stone wall state, and becomes the metal member 33 in which the gap H is formed. In addition, the ceramic substrate 1 has already been fired and hardened at the stage of step S11, and is not fired and hardened in this step S13.

[0037] In addition, it is preferable to dry the conductive paste before carrying out this step S13. In drying the conductive paste 3A, the conductive paste 3A having the convex portion 3A3 formed thereon is dried, for example, by natural drying, using a drying furnace, or the like. To dry the conductive paste 3A, a firing furnace to be used in the next step may be used. To dry the conductive paste 3A using a firing furnace, the temperature in the firing furnace may be kept, for example, at 20°C or higher and 60°C or lower for a predetermined time, thereby drying the conductive paste 3A. This drying of the conductive paste is carried out in a firing furnace, so that the drying and step S13 can be carried out successively. By carrying out step S13, the conductive paste 3A is fired to become the metal member 33, and the metal member 33 contains the metal 45 and the metal compound 6. In addition, the metal compound 6 contains the reaction layer 6a and the reaction product.

[0038] (heating and pressing with powdered release agent in between) Next, heating and pressurizing with a powdery release agent interposed therebetween is performed (hereinafter, referred to as step S14). In this step S14, the powdery release agent 60 is placed on the surface of the metal member 33, and heated and pressurized at a temperature at which the fired metal member 33 melts. For example, as the powdery release agent 60, a powder material having a melting point of 800°C or more, preferably 870°C or more, and a powder having an average particle size of 5 μm or less is placed on the surface of the ceramic substrate 1 so as to cover the metal member 33, and in this state, heated and pressurized at a temperature at which the metal member 33 melts. For example, if the metal member 33 is an Ag-Cu alloy, it is heated at 780°C or more and pressurized at 5 MPa or more and 50 MPa or less. In this step S14, when pressurized, in addition to heating at 5 MPa or more, the metal member 33 does not become a stone wall state, and the gap H can be reduced to form a smooth plane. In step S14, if the pressure is 50 MPa or less, the metal member 33 will not turn into a stone wall when heated, the gap H will be reduced, and the ceramic substrate 1 will be made smooth and flat without being damaged. The powdered release material 60 preferably has a melting point equal to or higher than the firing temperature, and preferably has a melting point at least 20° C. higher than the firing temperature. Since the powdered release material 60 placed on the surface of the metal member 33 is not molten, it can be easily released from the heat press machine PA.

[0039] The powdered release material 60 used in step S14 is preferably at least one of nitrides, carbides, oxides, and carbon clusters, for example. When heating and pressing using the powdered release material 60, the metal member 33 is heated and pressed to a temperature at which it melts. In addition, when heating and pressing in step S14, it is preferable to perform the heating and pressing in a vacuum atmosphere, a nitrogen atmosphere, or an argon atmosphere of 10 Pa or less. When heating and pressing in step S14, it is preferable to use a heat press machine PA. By performing step S14, the stone wall state and gaps H formed in the metal member 33 are eliminated. That is, by performing step S14, the stone wall state and gaps H formed on the end surface of the metal member 33 are melted by heating and pressing, and the active metal spreads more wetly to form a smooth plane. In addition, since the powdered release material 60 is arranged on the surface of the metal member 33, it can be easily released from the heat press machine PA after heating and pressing.

[0040] (Remove the powder release agent) The step of removing the powdery release agent S15 (hereinafter referred to as step S15) is to remove the surface of the metal member 33 on which the powdery release agent 60 is placed by polishing or grinding together with the powdery release agent 60. The surface side of the metal member 33 removed in step S15 is a portion that is previously protruded from the surface of the ceramic substrate 1 as the convex portion 3A3 of the conductive paste 3A, so that only a small amount is removed. By performing step S15, the metal member 33 can be made into a conductive portion 3 without a stone wall state or gap H. Therefore, the end surface of the metal member 33 after performing step S15, that is, the conductive portion 3, can obtain a smooth plane such that the arithmetic mean roughness Ra is in the range of 0.01 μm to 1.5 μm. By performing this step S15, the first surface 1A and the second surface 1B of the ceramic substrate 1 are exposed, and the end surface of the conductive portion 3 also becomes flush with the surface of the ceramic substrate 1. 6A, the end face of the metal member 33 is smooth and flat because it is heated and pressurized at a temperature at which the metal member 33 melts. By heating and pressurizing the metal member 33 at a temperature at which the metal member 33 melts, the active metal powder 6A wets and spreads within the metal powder 45A, forming a smooth flat surface without any stone wall-like structure or gaps H.

[0041] As described above, the sintered body substrate 10 can be manufactured by steps S11 to S15. The sintered body substrate 10 may have a bonding member 11 such as a plating layer disposed on the conductive portion 3 after step S15. The sintered body substrate 10 does not have a stone wall shape or gap H as in the conventional conductive portion 300 as shown in FIG. 6B, for example, but has a smooth flat surface without irregularities or cracks as shown in FIG. 6A. Therefore, the sintered body substrate 10 has improved bonding strength of the element electrodes 24 and the like connected to the conductive portion 3 directly or via the bonding member 11.

[0042] In the sintered body substrate 10, a reaction layer 6a of the metal compound 6 is formed on the inner surface of the through hole 2 in the conductive portion 3, and further, when the reactant is at least one of Cu, Cr, and Ni in the metal powder 45A, the metal compound 6 is located around the fired metal 5, and when the reactant contains inorganic filler 7, the metal compound 6 is also located around the inorganic filler 7. Therefore, in the sintered body substrate 10, the bonding strength between the through hole 2 and the recess 9 and the conductive portion 3 is improved.

[0043] In the above-mentioned step S14, as shown in Fig. 7A and Fig. 7B, a powdered release material may be placed on the heat press machine PA side, and the metal member 33 may be heated and pressed. Fig. 7A is a cross-sectional view showing a state where a powdered release material is placed on the press machine side in a method for producing a sintered body substrate according to an application example of the embodiment. Fig. 7B is a cross-sectional view showing a state where a metal member is heated and pressed by a press machine via a powdered release material in a method for producing a sintered body substrate according to an application example of the embodiment. A powdered release agent 60 is applied to the plate surfaces of the heat press machines PA arranged above and below the ceramic substrate 1, and heated and pressed under the above-mentioned conditions. The powdered release agent 60 is preferably arranged in a slurry state so that it can be applied to the plate surfaces of the heat press machine PA.

[0044] [Light emitting device] Next, the light emitting device 100 according to the embodiment will be described with reference to Fig. 8. Fig. 8 is a cross-sectional view that illustrates the light emitting device according to the embodiment. The light emitting device 100 is a device in which a light emitting element 20 is arranged on a sintered body substrate 10 to emit light, and comprises the sintered body substrate 10 and the light emitting element 20 having an element electrode 24, with the conductive portion 3 of the sintered body substrate 10 and the element electrode 24 being electrically connected. The light emitting device 100 includes the sintered body substrate 10 already described, and the light emitting element 20 electrically connected to the conductive portion 3 that serves as the wiring portion of the sintered body substrate 10. The light emitting device 100 will be described as having a light reflecting member 30 arranged to cover the side surface of the light emitting element 20 and the top of the sintered body substrate 10, as an example. The light emitting device 100 will be described as having a configuration in which a bonding member 11 is arranged on the conductive portion 3 of the sintered body substrate 10 for electrical connection.

[0045] In the light emitting device 100, the light emitting element 20 having the element electrode 24 is disposed on the sintered body substrate 10, and a plating layer is disposed as a bonding member 11 on the conductive portion 3 that serves as a wiring portion on the first surface 1A and the second surface 1B of the ceramic substrate 1. In the light emitting device 100, the conductive portion 3 is exposed on the same plane as the first surface 1A and the second surface 1B of the ceramic substrate 1, and the bonding member 11 is disposed on the conductive portion 3. The end surface of the conductive portion 3 is a flat and smooth surface with almost no irregularities or cracks. Therefore, when a plating layer that serves as the bonding member 11 is applied, the surface of the plating layer also becomes a flat and smooth surface without irregularities or cracks. Therefore, when the element electrode 24 is bonded, it is easy to bond and the bonding strength is improved.

[0046] (Light emitting element) The light emitting element 20 includes a pair of element electrodes 24 , a light-transmitting member 23 disposed on the light extraction surface side of the light emitting element 20 , an element substrate 22 , and a semiconductor laminate 21 . The light emitting element 20 has, as an example, a semiconductor laminate 21 on an element substrate 22. In this embodiment, a light-transmitting member 23 is disposed on the upper surface side of the element substrate 22, which is the light extraction surface, and the semiconductor laminate 21 is provided on the lower surface side of the element substrate 22, and a pair of element electrodes 24 are provided on the semiconductor laminate 21 side. The semiconductor laminate 21 may have any composition depending on the desired emission wavelength. For example, a nitride semiconductor (In X Al Y Ga 1-X-Y N, 0≦X, 0≦Y, X+Y≦1), GaP, or GaAlAs or AlInGaP capable of emitting red light can be used. The size and shape of the light emitting element 20 can be appropriately selected depending on the purpose of use.

[0047] As an example, a sapphire substrate, a silicon substrate, or a GaN substrate is used as the element substrate 22. The thickness of the element substrate 22 is, for example, 20 μm to 2 mm, preferably 50 μm to 500 μm, and more preferably 80 μm to 160 μm. The element substrate 22 is disposed such that its lower surface faces the semiconductor laminate 21 and its upper surface faces the light-transmitting member 23. Note that the element substrate 22 and the light-transmitting member 23 are preferably directly bonded to each other or bonded to each other via a bonding member.

[0048] The light-transmitting member 23 may be made of, for example, a light-transmitting resin material, glass, aluminum oxide, or an inorganic material such as a phosphor. The light-transmitting member 23 may be made of, for example, an epoxy resin, a silicone resin, or a resin mixture thereof. The light-transmitting member 23 may be made of a resin material or an inorganic material containing a phosphor, or may be made of only a phosphor. The light-transmitting member 23 may emit white light by, for example, containing a phosphor that absorbs blue light from the light-emitting element 20 and emits yellow light. The light-transmitting member 23 may also contain multiple types of phosphors, and may also emit light from the light-emitting element 20 as white light through the light-transmitting member 23 by, for example, containing a phosphor that absorbs blue light from the semiconductor laminate 21 and emits green light and a phosphor that emits red light.

[0049] Examples of such phosphors include yttrium-aluminum-garnet phosphors (e.g., Y3(Al,Ga)5O 12 :Ce), lutetium aluminum garnet phosphors (e.g., Lu3(Al,Ga)5O 12 :Ce), terbium aluminum garnet phosphors (e.g., Tb3(Al,Ga)5O 12 :Ce), β-sialon phosphors (e.g., (Si,Al)3(O,N)4:Eu), α-sialon phosphors (e.g., Mz(Si,Al) 12 (O,N) 16(However, 0 < z ≤ 2, and M is Li, Mg, Ca, Y, and lanthanide elements excluding La and Ce), nitride-based phosphors such as CASN-based phosphors (e.g., CaAlSiN3:Eu) or SCASN-based phosphors (e.g., (Sr,Ca)AlSiN3:Eu), fluoride-based phosphors such as KSF-based phosphors (e.g., K2SiF6:Mn), KSAF-based phosphors (e.g., K2(Si,Al)F6:Mn), or MGF-based phosphors (e.g., 3.5MgO·0.5MgF2·GeO2:Mn), or quantum dot phosphors such as perovskite and chalcopyrite can be used.

[0050] The element electrode 24 is connected to the second portion 8 of the conductive portion 3 that serves as the wiring portion of the sintered body substrate 10 via the metal bump 12 or / and the joining member 11. One of the element electrodes 24 is a p-electrode, and the other is arranged at a distance that does not electrically short-circuit with the n-electrode. As an example, the element electrode 24 is configured to arrange the p-electrode and the n-electrode at one location each, but it may also be configured such that one of them is at two locations and the other is at one location.

[0051] The metal bump 12 or / and the joining member 11 electrically connect the element electrode 24 and the conductive portion 3 that serves as the wiring portion. The metal bump 12 may be arranged on the element electrode 24 side or on the conductive portion 3 side that serves as the wiring portion. Also, the shape, size, and number of the metal bumps 12 can all be appropriately set as long as they can be arranged within the area range of the element electrode 24. Further, the size of the metal bump 12 can be appropriately adjusted according to the size of the semiconductor laminate, the required light emission output of the light emitting element, etc., and for example, a size with a diameter of about several tens of μm to several hundreds of μm can be mentioned.

[0052] The metal bump 12 can be formed of, for example, Au, Ag, Cu, Al, Sn, Pt, Zn, Ni, or an alloy thereof, and can be formed by a stud bump known in the art. The stud bump can be formed by a stud bump bonder, a wire bonding device, etc. The metal bump 12 may also be formed by a method known in the art, such as electrolytic plating, electroless plating, vapor deposition, sputtering, etc. Examples of the bonding member 11 include tin-bismuth (SnBi)-based, tin-copper-based, tin-silver-based, gold-tin-based, or tin-silver-copper (SAC)-based solders, eutectic alloys such as alloys mainly composed of Au and Sn, alloys mainly composed of Au and Si, and alloys mainly composed of Au and Ge, paste materials such as silver, gold, and palladium, anisotropic conductive materials such as ACP and ACF, brazing materials of low-melting point metals, conductive adhesives combining these, conductive composite adhesives, etc. The bonding member 11 is applied, for example, onto the conductive portion 3 that will become the wiring portion by plating.

[0053] (Light reflecting material) The light reflecting member 30 is a member having light reflectivity. The light reflecting member 30 is disposed so as to cover the upper surface of the sintered body substrate 10 and also to cover the side surface of the light emitting element 20. The light reflecting member 30 is disposed so as to expose the light extraction surface of the light emitting element 20 and to be flush with the light transmissive member 23 of the light emitting element 20. The light reflecting member 30 is also disposed, for example, between the lower surface of the light emitting element 20 and the upper surface (first surface) of the sintered body substrate 10.

[0054] The light reflecting member 30 preferably has high reflectance and is white in order to effectively utilize the light from the light emitting element 20. The reflectance of the light reflecting member 30 is preferably, for example, 90% or more, and more preferably 94% or more, at the wavelength of the light emitted by the light emitting element 20. The light reflecting member 30 may be made of a resin containing a light diffusing material. Examples of the resin used in the light reflecting member include thermoplastic resins such as acrylic resin, polycarbonate resin, cyclic polyolefin resin, polyethylene terephthalate resin, polyethylene naphthalate resin, and polyester resin, and thermosetting resins such as epoxy resin and silicone resin. Examples of the light diffusing material may include known materials such as titanium oxide, silicon oxide, aluminum oxide, zinc oxide, and glass.

[0055] As an example, the sintered body substrate 10 is connected to an external wiring board or the like. The external wiring board is electrically connected to the conductive portion 3 arranged on the second surface 1B of the ceramic substrate 1 via a bonding member 11. The configuration of the external wiring board is not particularly limited as long as it is used in this type of light emitting device 100.

[0056] In the light emitting device 100 having the above-mentioned configuration, the surfaces of the conductive parts 3 on the first and second surfaces of the sintered body substrate 10 are smooth and flat without cracks or irregularities, and the surfaces of the bonding members 11 are also smooth and free of cracks or irregularities, improving the bonding strength with the element electrodes 24 and improving the reliability of the device. Also, in the light emitting device 100, it is possible to stabilize the connection of the element electrodes without increasing the amount of the bonding members 11 that become the plating layer. In the light emitting device 100, one light emitting element 20 is treated as one unit and the brightness and on / off control unit is set, but one unit may include a plurality of light emitting elements 20 and each of the included light emitting elements 20 may be used as a unit for on / off control, and the size and number of the light emitting elements 20 may be two or more than two types. For example, one unit may include light emitting elements 20 of the same size in one row and four columns, or four light emitting elements 20 in two rows and two columns, or nine light emitting elements 20 in three rows and three columns. Also, one unit may include light emitting elements 20 of different sizes arranged in an arbitrary arrangement according to size.

[0057] [Manufacturing method of light emitting device] Next, a method for manufacturing a light emitting device according to an embodiment will be described with reference to Fig. 10A to Fig. 10C. Fig. 10A is a cross-sectional view illustrating a state in which a bonding member is disposed on a sintered body substrate in the method for manufacturing a light emitting device according to an embodiment. Fig. 10B is a cross-sectional view illustrating a state in which a light emitting element is disposed in the method for manufacturing a light emitting device according to an embodiment. Fig. 10C is a cross-sectional view illustrating a state in which a light reflecting member is disposed in the method for manufacturing a light emitting device according to an embodiment. The manufacturing method S20 of the light emitting device includes preparing the sintered body substrate manufactured by the manufacturing method S10 of the sintered body substrate already described, and arranging the light emitting element on the conductive part from which the powdery release agent of the metal member has been removed, and in arranging the light emitting element, the conductive part and the light emitting element are directly or indirectly electrically connected. That is, the manufacturing method S20 of the light emitting device includes preparing the sintered body substrate S21 and arranging the light emitting element S22. In preparing the sintered body substrate S21, the conductive paste 3A filled in the through hole 2 becomes the metal member 33 by firing the ceramic substrate 1, and the end of the metal member 33 is polished or ground by removing the powdery release agent 60, and the light emitting element is arranged on the conductive part 3. Note that, as an example, after arranging the light emitting element S22, arranging the light reflective member S23 covering the side surface of the light emitting element 20 and the top of the sintered body substrate 10 is performed.

[0058] (Preparing a sintered body substrate) Preparing a sintered body substrate S21 (hereinafter referred to as step S21) refers to preparing a sintered body substrate 10 manufactured by the sintered body substrate manufacturing method S10 already described. In the sintered body substrate 10, the end faces of the conductive parts 3 and the bonding members 11 on the first surface 1A and the second surface 1B are in a flat state without a stone wall state, without gaps H being formed, and without cracks or unevenness. Note that the sintered body substrate 10 may be sized to be divided into individual light emitting devices 100 or for each light emitting device 100 after arranging a plurality of regions for arranging the light emitting elements 20 and arranging the light reflecting members 30 described later.

[0059] (Placing light-emitting elements) Arranging the light-emitting element S22 (hereinafter referred to as step S22) means arranging the light-emitting element 20 on the sintered body substrate 10. The light-emitting element 20 is arranged with the translucent member 23 already connected to the element substrate 22. When joining the translucent member 23 to the element substrate 22, a translucent joining material is used. In this step S22, the element electrode 24 of the light-emitting element 20 is connected via the joining member 11 arranged on the second portion (wiring portion) 8 of the conductive portion 3, which becomes the wiring portion, or via the metal bump 12.

[0060] (Placing light reflecting material) Arranging the light reflecting member S23 (hereinafter referred to as step S23) means arranging the light reflecting member 30 so as to cover the upper surface of the sintered body substrate 10 and also to cover the side surface of the light emitting element 20. In this step S23, the light reflecting member 30 is arranged on the sintered body substrate 10 so as to surround the light emitting element 20 and expose the upper surfaces of each light-transmitting member 23 which become the light extraction surface of the light emitting element 20. The light reflecting member 30 is arranged so as to be rectangular in a plan view.

[0061] In the manufacturing method S20 of the light emitting device, after the work of step S23 is completed, a singulation work is performed as necessary. The light emitting device 100 has a unit or a unit set in advance according to the number of light emitting elements 20 used. Therefore, when a plurality of light emitting devices 100 are manufactured at once, a singulation work is performed. When the singulation work is performed, a plurality of light emitting devices 100 are manufactured by cutting in a lattice shape. In addition, as a cutting method, for example, a disk-shaped rotary blade, an ultrasonic cutter, laser light irradiation, etc. can be used.

[0062] In the manufacturing method S20 for a light-emitting device having the above-mentioned configuration, by the manufacturing method S10 for a sintered substrate, the end face of the conductive part 3, which is the end face of the metal member 33 of the sintered substrate 10, and the joining member 11 become flat without cracks or unevenness, without a stone wall state or gap H, thereby improving the joining strength with the element electrode 24 and improving the joining strength of the conductive part 3 arranged in the through hole 2, thereby improving reliability and enabling stable control of the light-emitting element 20.

[0063] Next, a sintered body substrate 10A showing an application example will be described with reference to Fig. 11. Fig. 11 is a cross-sectional view of a sintered body substrate showing another embodiment. The sintered body substrate 10A differs from the sintered body substrate 10 already described in that it does not have a recess 9, and that the conductive portion 3 is a first portion 13 and has a wiring portion 18 connected to the conductive portion 3 as a second portion on the surface of the ceramic substrate 1. The sintered body substrate 10A has a first surface 1A and a second surface 1B opposite to the first surface 1A, and includes a ceramic substrate 1 having a through hole 2 penetrating the ceramic substrate 1 so as to connect the first surface 1A and the second surface 1B, and a conductive portion 3 disposed in the through hole 2. The conductive portion 3 includes a metal 45 and a reaction layer 6a of a metal compound disposed on an inner wall defining the through hole 2. The conductive portion 3 includes a wiring portion 18 disposed on the surface of the ceramic substrate 1. All or a part of the wiring portion 18 plays the same role as the second portion continuous with the first portion 13 of the conductive portion 3, and is connected to the element electrode 24 via the bonding member 11.

[0064] Ceramic substrate 1 has the same configuration and materials as those already described, except that it does not have recessed portion 9. Ceramic substrate 1 has through holes 2 of the same diameter that continue from first surface 1A to second surface 1B. The conductive portion 3 includes a portion (first portion) 13 disposed in the through hole 2 of the ceramic substrate 1, and a wiring portion (second portion) 18 disposed on the surface of the ceramic substrate 1. The conductive portion 3 includes the first portion 13 of the ceramic substrate 1 described above within the range of the plate thickness of the ceramic substrate 1. The conductive portion 3 includes a second portion disposed so as to be in contact with at least a part of the first portion 13, as the wiring portion 18 disposed on the surface of the ceramic substrate 1. In the conductive portion 3, the first portion 13 and the wiring portion 18 are preferably formed of the same material, for example. The conductive portion 3 including the first portion 13 and the wiring portion 18 includes a metal 45, and a reaction layer 6a of a metal compound on the inner wall defining the through hole 2 and on the joint surface where the wiring portion 18 contacts the surface of the ceramic substrate 1.

[0065] The arithmetic mean roughness Ra of the end face side of the conductive part 3, that is, the end face of the first part 13 and the surface side of the wiring part 18, is preferably 0.01 μm or more and 1.5 μm or less. The method for measuring the arithmetic mean roughness Ra of the surface side of the first part 13 and the wiring part 18 is the same as the method already described. The components of the conductive part 3 and the components contained therein are also the same as those already described. In the sintered body substrate 10, the surfaces of the wiring part 18 and the bonding member 11, which are the end faces of the conductive part 3, are smooth and flat without cracks or unevenness, so that the element electrodes 24 and the like can be stably connected. In addition, the sintered body substrate 10A has a reaction layer 6a of the metal compound 6 at the contact portion between the ceramic substrate 1 and the conductive part 3, so that the bonding strength between the conductive part 3 including the wiring part 18 and the ceramic substrate 1 can be improved. In addition, the opening area of ​​the through hole 2 is larger on the second surface 1B side than on the first surface 1A, so that the heat dissipation is excellent when the light emitting element 20 is connected.

[0066] Next, the manufacturing method SA10 of the sintered body substrate 10A will be described with reference to FIG. 12 to FIG. 13G. In addition, in the manufacturing method S10 of the sintered body substrate already described, the description will be omitted if the same procedure or configuration is used. FIG. 12 is a flow chart illustrating a manufacturing method of a sintered body substrate according to another embodiment. FIG. 13A is a cross-sectional view that shows a ceramic substrate having a through hole formed therein in the manufacturing method of a sintered body substrate according to another embodiment. FIG. 13B is a cross-sectional view that shows a state in which a conductive paste is arranged in the through hole so as to have a convex portion protruding from the surface of the ceramic substrate in the manufacturing method of a sintered body substrate according to another embodiment. FIG. 13C is a cross-sectional view that shows a state in which the conductive paste is fired in the manufacturing method of a sintered body substrate according to another embodiment. FIG. 13D is a cross-sectional view that shows a state in which a powdered release agent is arranged on a metal member and heated and pressed in the manufacturing method of a sintered body substrate according to another embodiment. FIG. 13E is a cross-sectional view that shows a state after a powdered release agent is arranged on a metal member and heated and pressed in the manufacturing method of a sintered body substrate according to another embodiment. Fig. 13F is a cross-sectional view showing a state where a powdery release agent is removed from a metal member to form a conductive part in a method for producing a sintered body substrate according to another embodiment. Fig. 13G is a cross-sectional view showing a state where a wiring part and a bonding member are arranged on the conductive part in a method for producing a sintered body substrate according to another embodiment.

[0067] A manufacturing method SA10 for a sintered body substrate includes preparing a ceramic substrate 1 having a first surface 1A and a second surface 1B opposite to the first surface 1A, and having a through hole 2 penetrating to connect the first surface 1A and the second surface 1B, arranging a first conductive paste 3A1 in the through hole 2 so as to have a convex portion 3A3 protruding from the surface of the ceramic substrate 1, firing the first conductive paste 3A1 and the convex portion 3A3 arranged in the through hole 2, interposing a powdered release material 60 on the surface of the fired metal member 33, heating and pressurizing the metal member 33 to a temperature at which the metal member 33 melts, and removing the powdered release material 60 from the metal member. In other words, the manufacturing method SA10 of the sintered substrate includes the steps of preparing a ceramic substrate SA11, arranging a conductive paste so as to have a convex portion SA12, firing the conductive paste SA13, heating and pressurizing with a powdered release agent interposed therebetween SA14, and removing the powdered release agent SA15.

[0068] In preparing a ceramic substrate SA11 (hereinafter referred to as step SA11), a ceramic substrate 1 that has a through hole 2 penetrating so as to connect a first surface 1A and a second surface 1B and that has already been fired and hardened is prepared. In this step SA11, the through hole 2 is formed but the recess 9 is not. The ceramic substrate 1 has the same configuration and material as those already described, except that the recess 9 is not formed.

[0069] Arranging the conductive paste so as to have a convex portion SA12 (hereinafter referred to as step SA12) is to arrange a first conductive paste 3A1, which will become the conductive paste 3A, in the through hole 2 of the ceramic substrate 1 so as to have a convex portion 3A3 protruding from the surfaces of the first surface 1A and the second surface 1B of the ceramic substrate 1. In this step SA12, the conductive paste 3A is arranged in the through hole 2 by, for example, screen printing or by injecting with a nozzle. The conductive paste 3A used in this step SA12 has the same components as the conductive paste 3A already described.

[0070] The step SA13 of firing the conductive paste (hereinafter referred to as step SA13) is performed under the same firing atmosphere, temperature conditions, etc. as the steps already described. Furthermore, before firing the conductive paste 3A, the conductive paste 3A may be dried as described above. When this step SA15 is performed, the conductive paste 3A is fired to become the metal member 33, and the surface of the portion that was the protruding portion 3A3 of the metal member 33 becomes like a stone wall or a gap H is formed. Furthermore, by this step SA13, the conductive paste 3A is fired to become the metal member 33, and the metal member 33 contains the metal 45 and the metal compound 6, and a reaction layer 6a of the metal compound 6 is formed on the inner surface of the through hole 2.

[0071] Next, heating and pressing with a powdered release material is performed (hereinafter, referred to as step SA14). In this step SA14, a powdered release material is placed on the surface of the metal member 33 that has been formed by firing the conductive paste 3A, and the metal member 33 is heated and pressed at a temperature at which the metal member 33 melts. When heating and pressing in this step SA14, as already described, the heat press machine PA is used to apply pressure of 5 MPa to 50 MPa while heating at a temperature at which the metal member 33 melts.

[0072] Next, the powdery release agent is removed (hereinafter, referred to as step SA15). In this step SA15, the powdery release agent 60 is removed together with a part of the metal member 33 using a polishing device or a grinding device. When removing the powdery release agent 60 from the surface of the metal member 33, the part protruding from the surface of the ceramic substrate 1, or the protruding part and a part of the surface of the ceramic substrate 1, are removed together with the powdery release agent 60. When this step SA15 is performed, only a small amount of the conductive part 3 after firing is polished or ground on the end face side. After this step SA16 is performed, the sintered body substrate 10A has a smooth flat surface without gaps H and does not have a stone wall state, so that the element electrodes 24 and the like can be stably connected via the joining member 11.

[0073] In the sintered body substrate 10A, the reaction layer 6a of the metal compound 6 is formed on the inner wall of the through hole 2 and on the part in contact with the surface of the ceramic substrate 1 in the conductive portion 3, and further, when the reactant contains the specific metal component, the metal compound 6 is located around the fired metal component, or around the inorganic filler 7 if the reactant contains the inorganic filler 7. Therefore, the sintered body substrate 10A has improved bonding strength between the through hole 2 and the ceramic substrate 1 and the metal member 33 and the wiring portion 18. In the sintered body substrate 10A, the wiring portion 18 may be disposed on the conductive portion 3, and a bonding member 11 such as a plating layer may be disposed on the wiring portion 18.

[0074] Next, a light emitting device 100A using a sintered body substrate 10A will be described with reference to Fig. 14. Fig. 14 is a cross-sectional view of a light emitting device showing an application example. Note that the same configuration as that already described will not be described. The light emitting device 100A includes a sintered body substrate 10A and a light emitting element 20 having an element electrode 24, and electrically connects the conductive portion 3 (wiring portion 18) of the sintered body substrate 10A to the element electrode 24. As an example, the sintered body substrate 10A connects the element electrode 24 to the wiring portion 18 in contact with the conductive portion 3 via a plating layer that is a bonding member 11. The light emitting device 100A includes a light reflecting member 30, as in the light emitting device 100 already described. The wiring portion 18 does not become like a stone wall, does not have a gap H formed therein, and has a smooth flat surface without cracks or irregularities. Therefore, even if the bonding member 11 that becomes a plating layer is disposed, the flat surface without cracks or irregularities can be maintained. Therefore, in the light emitting device 100A, it is possible to stabilize the connection of the element electrodes without increasing the amount of the plating layer.

[0075] The manufacturing method of the light emitting device 100A involves the same steps as the manufacturing method S20 of the light emitting device 100 already described. That is, the steps include preparing a sintered body substrate 10A, arranging a conductive portion 3 in the through hole 2 of the ceramic substrate 1, and electrically connecting an element electrode 24 to the conductive portion 3. In arranging the conductive portion 3, the element electrode 24 is electrically connected to the conductive portion 3 via a bonding member 11 such as a wiring portion 18 or a plating layer applied to the wiring portion 18. Furthermore, the light reflective member 30 is arranged to manufacture the light emitting device 100A.

[0076] In addition, the through hole 2 of the sintered body substrate 10 has an opening area on the second surface 1B larger than that on the first surface 1A to which the mounting component electrodes are bonded, thereby improving the thermal conductivity of the sintered body substrate 10 and increasing heat dissipation, and also enabling the substrate 10 to be made thinner and have improved performance such as reliability while maintaining its strength and rigidity. The through hole 2 can be formed, for example, by laser processing, mechanical processing, or chemical processing such as etching. The through hole 2 is preferably circular, but may also be polygonal, and the polygon referred to here may be one other than one in which the apex angles of two consecutive sides are strictly connected to each other by straight lines. The polygon may be, for example, a polygonal shape in which the corners are rounded such that the straight lines are connected to each other by small arcs. In addition, when forming the recess 9 in the manufacturing method of the sintered body substrate, a blasting process or an etching process may be performed.

[0077] In the present invention, the following relationships among the items may be used. [Section 1] Preparing a ceramic substrate having a first surface and a second surface opposite to the first surface, the ceramic substrate having a through hole penetrating the first surface and connecting the first surface and the second surface; disposing a conductive paste including at least a metal powder, an active metal powder, and an organic solvent in the through hole so as to have a protrusion protruding from the first surface or the second surface; Firing the disposed conductive paste to obtain a metal member; and a powdered release agent is placed on the surface of the metal member, and the metal member is heated and pressurized to a temperature at which the metal member melts; and removing the powdered release agent from the metal member. [Section 2] Item 2. The method for producing a sintered substrate according to item 1, wherein the ceramic substrate is provided with a recess disposed on at least one of the first surface and the second surface, and the through hole is provided at a position of the recess. [Section 3] 3. The method for producing a sintered substrate according to item 1 or 2, wherein the heating and pressurizing are performed in a vacuum atmosphere, a nitrogen atmosphere, or an argon atmosphere of 10 Pa or less. [Section 4] Item 4. The method for producing a sintered substrate according to any one of items 1 to 3, wherein the heating and pressurizing are performed using a heat press machine, and the powdery release material is interposed by applying the powdery release material to a platen surface of the heat press machine. [Section 5] 5. The method for producing a sintered substrate according to any one of items 1 to 4, wherein in the heating and pressurizing, the pressure is 5 MPa or more and 50 MPa or less. [Section 6] Item 6. The method for producing a sintered body substrate according to any one of items 1 to 5, wherein in the heating and pressing, the powdery release agent is a powder having a melting point of 800° C. or higher and an average particle size of 5 μm or less. [Section 7] Item 7. The method for producing a sintered body substrate according to any one of items 1 to 6, wherein in the heating and pressing, the powder of the powdery release agent is at least one of nitrides, carbides, oxides, and carbon clusters. [Section 8] 8. The method for manufacturing a sintered body substrate according to any one of items 1 to 7, wherein in preparing the ceramic substrate, a laser beam is irradiated from the first surface side of the ceramic substrate to form the through hole. [Section 9] Item 2 to 8, in which the ceramic substrate is prepared by irradiating the first surface side or the second surface side of the ceramic substrate with laser light to form the recesses. The method for manufacturing a sintered substrate according to any one of items 2 to 8, in which item 2 is cited. [Section 10] Item 11. The method for producing a sintered body substrate according to any one of items 1 to 10, wherein, in disposing the conductive paste, the content of the active metal powder is 1 part by weight or more and 5 parts by weight or less. [Section 11] Item 11. The method for producing a sintered body substrate according to any one of items 1 to 10, wherein the metal powder in the conductive paste is at least one of Ag, Al, Zn, Sn, and Ag-Cu alloy powder. [Section 12] Item 12. The method for producing a sintered substrate according to any one of items 1 to 11, wherein in disposing the conductive paste, the metal powder further contains at least one of Cu, Cr, and Ni. [Section 13] Item 13. The method for producing a sintered substrate according to any one of items 1 to 12, wherein in disposing the conductive paste, the active metal powder contains at least one of TiH2, CeH2, ZrH2, and MgH2. [Section 14] Item 14. The method for producing a sintered substrate according to any one of items 1 to 13, wherein in disposing the conductive paste, the conductive paste further contains a resin. [Section 15] Item 15. The method for producing a sintered substrate according to any one of items 1 to 14, wherein the conductive paste further contains a plurality of inorganic fillers other than metals in disposing the conductive paste. [Section 16] Item 16. The method for producing a sintered substrate according to any one of items 1 to 15, wherein the sintering temperature in obtaining the metal members is 780° C. or higher and 1100° C. or lower. [Section 17] Item 17. The method for producing a sintered substrate according to any one of items 1 to 16, wherein the sintering atmosphere is a vacuum atmosphere of 10 Pa or less or an Ar atmosphere of 99.9% or more, in obtaining the metal members. [Section 18] Item 18. The method for producing a sintered body substrate according to any one of items 1 to 17, wherein, in removing the powdery release agent, an arithmetic mean roughness Ra of an end surface of the metal member after removing the powdery release agent from the metal powder is 0.01 μm or more and 1.5 μm or less. [Section 19] Preparing a sintered body substrate manufactured by the method for manufacturing a sintered body substrate according to any one of items 1 to 18; and disposing a light emitting element on the conductive portion of the metal member from which the powdery release agent has been removed; A method for manufacturing a light emitting device, comprising the steps of: disposing the light emitting element; electrically connecting the conductive portion and the light emitting element directly or indirectly; [Industrial Applicability]

[0078] The light emitting device according to the embodiment of the present disclosure can be used as a light source for a headlamp with variable light distribution. In addition, the light emitting device according to the embodiment of the present disclosure can be used as a backlight source for a liquid crystal display, various lighting fixtures, a large display, various display devices such as advertisements and destination guides, and further, an image reading device in a digital video camera, a facsimile, a copy machine, a scanner, a projector device, and the like. [Explanation of symbols]

[0079] 1. Ceramic substrate 1A 1st page 1B 2nd side 2 Through holes 3 Conductive Part 3A conductive paste 6 Metal compounds 6A active metal powder 6a Reaction layer 7 Inorganic filler: after firing 7A Inorganic filler: before firing 7B Organic Binder 8 Second conductive part (wiring part) 10. Sintered ceramic substrate 11 Joining materials 12 Metal bump 20 Light emitting element 21 Semiconductor layer 22 Element substrate 23 Translucent material 24 Element electrode 30 Light reflecting material 45 metal 45A metal powder 100 Light emitting device S10 Manufacturing method of sintered body substrate S11 Prepare a ceramic substrate S12 Placing conductive paste S13 Placing conductive paste S14 Firing ceramic substrates S20 Manufacturing method of light emitting device S21 Preparing a sintered body substrate S22 Arranging light-emitting elements S23 Arrangement of light reflecting members

Claims

1. preparing a ceramic substrate having a first surface and a second surface opposite to the first surface, the ceramic substrate having a through hole penetrating the first surface and connecting the first surface and the second surface; disposing a conductive paste including at least a metal powder, an active metal powder, and an organic solvent in the through hole so as to have a protrusion protruding from the first surface or the second surface; Firing the disposed conductive paste to obtain a metal member; and a powdered release agent is placed on the surface of the metal member, and the metal member is heated and pressurized to a temperature at which the metal member melts; and removing the powdered release agent from the metal member.

2. The method for manufacturing a sintered substrate according to claim 1 , wherein the ceramic substrate is prepared by providing a recessed portion disposed on at least one of the first surface and the second surface, and the through hole is provided at a position of the recessed portion.

3. 2. The method for producing a sintered substrate according to claim 1, wherein the heating and pressurizing are performed in a vacuum atmosphere of 10 Pa or less, a nitrogen atmosphere, or an argon atmosphere.

4. 2. The method for producing a sintered substrate according to claim 1, wherein the heating and pressurizing are performed using a heat press machine, and the powdered release agent is interposed by applying the powdered release agent to a platen surface of the heat press machine.

5. 2. The method for producing a sintered substrate according to claim 1, wherein in the heating and pressurizing, the pressure is 5 MPa or more and 50 MPa or less.

6. 2. The method for producing a sintered substrate according to claim 1, wherein in the heating and pressing, the powdered release agent is a powder having a melting point of 800[deg.] C. or higher and an average particle size of 5 [mu]m or less.

7. 7. The method for producing a sintered substrate according to claim 6, wherein in the heating and pressing, the powder of the powdered release agent is at least one of nitrides, carbides, oxides, and carbon clusters.

8. 2 . The method for producing a sintered substrate according to claim 1 , wherein in preparing the ceramic substrate, the through holes are formed by irradiating the ceramic substrate with laser light from the first surface side.

9. 3. The method for producing a sintered substrate according to claim 2, wherein in preparing the ceramic substrate, the recesses are formed by irradiating the ceramic substrate with laser light from the first surface side or the second surface side.

10. 2. The method for producing a sintered substrate according to claim 1, wherein the content of the active metal powder in the conductive paste is 1 part by weight or more and 5 parts by weight or less.

11. 2. The method for producing a sintered substrate according to claim 1, wherein in disposing the conductive paste, the metal powder contains at least one of Ag, Al, Zn, Sn, and Ag--Cu alloy powder.

12. 2. The method for producing a sintered substrate according to claim 1, wherein in disposing the conductive paste, the metal powder contains at least one of Cu, Cr, and Ni.

13. In disposing the conductive paste, the active metal powder is TiH 2 , CeH 2 , ZrH 2 , and MgH 2 The method for producing a sintered substrate according to claim 10, comprising at least one of the following:

14. The method for producing a sintered substrate according to claim 1 , wherein in disposing the conductive paste, the conductive paste further contains a resin.

15. 2. The method for producing a sintered substrate according to claim 1, wherein in disposing the conductive paste, the conductive paste further contains a plurality of inorganic fillers other than metal.

16. 2. The method for producing a sintered substrate according to claim 1, wherein the sintering temperature in obtaining the metal member is 780° C. or higher and 1100° C. or lower.

17. 2. The method for producing a sintered substrate according to claim 1, wherein the sintering atmosphere in obtaining the metal member is a vacuum atmosphere of 10 Pa or less or an Ar atmosphere of 99.9% or more.

18. 2. The method for manufacturing a sintered substrate according to claim 1, wherein, in removing the powdery release material, an arithmetic mean roughness Ra of an end surface of the metal member after the powdery release material is removed from the metal powder is 0.01 μm or more and 1.5 μm or less.

19. preparing a sintered body substrate manufactured by the method for manufacturing a sintered body substrate according to claim 1 or 2; and disposing a light emitting element on the conductive portion of the metal member from which the powdery release agent has been removed; A method for manufacturing a light emitting device, comprising the steps of: disposing the light emitting element; electrically connecting the conductive portion and the light emitting element directly or indirectly;

Citation Information

Patent Citations

  • Tyre vulcanizer

    JP1984022739A

  • Method of producing vertical miniature lamp

    JP1986022561A