Method for manufacturing modified incinerated ash

The heat-treatment of incineration ash with calcium-containing waste in water simplifies and enhances the reduction of alkali metals, enabling the use of biomass ash in cement manufacturing.

JP2024146526AActive Publication Date: 2024-10-15TOKUYAMA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023059492
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Existing methods for reducing alkali metals in biomass incineration ash are complex and inefficient, limiting its use as a raw material for cement due to stringent product standards.

Method used

A method involving the heat-treatment of incineration ash with calcium-containing waste in water at specific temperatures and times, replacing sodium and potassium aluminosilicates with calcium aluminosilicates, thereby reducing alkali metal content.

Benefits of technology

Effectively reduces alkali metals in incineration ash, making it suitable for use in cement production by lowering total alkali content to acceptable levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146526000001
    Figure 2024146526000001
  • Figure 2024146526000002
    Figure 2024146526000002
  • Figure 2024146526000003
    Figure 2024146526000003
Patent Text Reader

Abstract

To provide a method for readily and efficiently reduce alkali metal from incinerated ash such as biomass ash.SOLUTION: A method for manufacturing modified incinerated ash includes a step of heating incinerated ash such as biomass ash and calcium-containing wastes in which a calcium content is 20 mass% or more in terms of CaO based on 100 mass% of solid content in the water at 60-100°C for 1-24 hours.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing modified incineration ash having reduced alkali metals. [Background technology]

[0002] Conventionally, coal ash generated in coal-fired power plants has been used as a cement raw material.

[0003] Meanwhile, in recent years, as part of the movement toward carbon neutrality, biomass power generation, which burns biomass fuels including wood chips and palm kernel shells (PKS), has become more common, and there are also plans to use the incineration ash generated by the combustion of this biomass as a raw material for cement.

[0004] However, while the content of these biomass fuels varies depending on the type and place of production, they generally contain a lot of alkali metals, especially potassium, compared to coal. Since alkali metals such as potassium cause alkali-aggregate reactions, the content of these metals in cement is strictly regulated by product standards, making it difficult to use biomass incineration ash as it is.

[0005] Under these circumstances, methods for reducing alkali metals from biomass incineration ash have been proposed.

[0006] For example, a method for removing alkali metals from fly ash resulting from the combustion of woody biomass has been proposed, which includes a step (a) of classifying the fly ash into fine powder and coarse powder, a step (b) of pulverizing the surface portion of the coarse powder obtained in step (a) to obtain a pulverized product, a step (c) of classifying the pulverized product obtained in step (b) into pulverized fine powder and pulverized coarse powder, a step (d) of heating the pulverized fine powder obtained in step (c) together with a chlorine source to obtain a heat-treated product, and a step (e) of washing the fine powder obtained in step (a) and the heat-treated product obtained in step (d) with water (see Patent Document 1).

[0007] In addition, a method for producing low-potassium wood biomass ash has been proposed, which includes a first step of heating wood biomass ash to 500 to 850°C and contacting the wood biomass ash with a gas containing hydrogen chloride, and a second step of washing the wood biomass ash after contact with water to remove soluble matter (see Patent Document 2).

[0008] However, these methods require complicated operations, and a method capable of reducing alkali metals more simply and efficiently is desired.

[0009] It is assumed that alkali metals such as sodium and potassium in incineration ash such as biomass ash are incorporated into the glass of the incineration ash. Since the slurry of incineration ash is alkaline, it was thought that it would be possible to reduce the alkali metals by dissolving the glass layer using the alkalinity of the ash itself under hydrothermal conditions, but in reality it was not possible to sufficiently reduce the alkali metals.

[0010] If it becomes possible to more simply and efficiently remove alkali metals from biomass ash, it will be possible to easily expand its applications to include cement raw materials, just as with coal ash. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent Publication No. 2021-146236 [Patent Document 2] JP 2021-104482 A Summary of the Invention [Problem to be solved by the invention]

[0012] An object of the present invention is to provide a method for simply and efficiently reducing alkali metals from incineration ash such as biomass ash. [Means for solving the problem]

[0013] As a result of intensive research aimed at solving the above problems, the inventors have found that alkali metals can be reduced simply and efficiently by heat treating incineration ash together with calcium-containing waste in water, and have thus completed the present invention.

[0014] That is, the present invention is as follows. [1] A method for producing modified incineration ash by heat-treating incineration ash and calcium-containing waste in water. [2] The method for producing modified incineration ash described in [1], characterized in that the calcium content in 100% by mass of the solid content of the calcium-containing waste is 20% by mass or more, calculated as CaO. [3] The method for producing modified incineration ash described in [1], wherein the amount of calcium in the calcium-containing waste is 5 parts by mass or more in terms of CaO per 100 parts by mass of the incineration ash. [4] A method for producing modified incineration ash described in [1], wherein the calcium in the calcium-containing waste has at least one crystal structure selected from CaO, Ca(OH)2 and CaCO3 by X-ray diffraction method. [5] The method for producing modified incineration ash described in [1], wherein the incineration ash is at least one selected from biomass ash, coal ash, and garbage incineration ash. [6] The method for producing modified incineration ash according to [1], wherein the heating temperature in the heat treatment is 60 to 100°C and the heating time is 1 to 24 hours. [7] A method for producing cement, comprising the step of using modified incineration ash produced by the method according to any one of [1] to [6] as part of a raw material to produce cement. [8] A method for modifying incineration ash by heat treating incineration ash and calcium-containing waste in water. Effect of the Invention

[0015] According to the method of the present invention, it is possible to simply and efficiently reduce alkali metals from incineration ash such as biomass ash. It is considered that the reason why alkali metals cannot be reduced by the method of dissolving the glass layer by the alkalinity of the incineration ash slurry itself is that the dissolved alkali metals are generated on the ash surface as sodium aluminosilicate or potassium aluminosilicate. In the method of the present invention, by heat treating the incineration ash and calcium-containing waste in water, calcium in the calcium-containing waste is dissolved, and calcium aluminosilicate is preferentially generated instead of sodium aluminosilicate or potassium aluminosilicate, thereby suppressing the generation of aluminosilicate containing the dissolved alkali metal, and it is assumed that the reduction of alkali metals is made possible. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] [Manufacturing method of modified incineration ash] The method for producing modified incineration ash of the present invention is characterized by heat-treating incineration ash and calcium-containing waste in water.

[0017] The incineration ash to be treated in the method of the present invention is not particularly limited as long as it contains an alkali metal, and includes both the bottom ash accumulated in the incineration apparatus and the fly ash discharged from the incineration apparatus.

[0018] Examples of the incineration ash include biomass ash, coal ash, garbage incineration ash, etc. Specific examples of the biomass ash include wood biomass ash obtained by burning wood resources such as waste wood, palm kernel shells (PKS), white pellets, black pellets, and palm kernel fiber pellets (EFB), and biomass-coal co-combustion ash obtained by co-combusting wood biomass and coal.

[0019] The calcium-containing waste in the present invention can be any waste containing calcium without any particular limitations. The waste in the present invention also includes by-products in the manufacturing industry. The waste may or may not contain moisture, but from the viewpoint of calcium content, the waste preferably contains 10% by mass or more of solid matter, more preferably 20% by mass or more, and even more preferably 30% by mass or more, of 100% by mass of the waste.

[0020] Examples of calcium-containing wastes that can be used include slag, waste concrete, ready-mixed concrete sludge, residues from the production of milk of lime, inorganic sludge, papermaking sludge, chlorine bypass dust, desalted cake obtained by washing chlorine bypass dust, waste gypsum, egg shells, and seashells.

[0021] From the viewpoint of reactivity, the calcium content in the calcium-containing waste in the present invention is preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, calculated as CaO per 100% by mass of the solid matter in the calcium-containing waste. The calcium content in CaO terms contained in the solid matter in the calcium-containing waste can be measured by a method in accordance with JIS R 5204 "Method for fluorescent X-ray analysis of cement".

[0022] In the present invention, the amount of calcium-containing waste used depends on the calcium content in the waste, and the amount of waste used may be determined according to the amount of calcium in the waste.

[0023] In the present invention, the amount of calcium in the calcium-containing waste used is preferably 3 parts by mass or more, more preferably 4 parts by mass or more, and even more preferably 5 parts by mass or more, calculated as CaO, per 100 parts by mass of incineration ash, because alkali metals can be removed more efficiently. On the other hand, even if the amount of calcium is significantly increased, the effect of dealkalization is not increased proportionately, so the amount of calcium in the calcium-containing waste used is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less, calculated as CaO, per 100 parts by mass of incineration ash.

[0024] The form in which calcium is present in the calcium-containing waste in the present invention is not particularly limited as long as it contains calcium atoms, but from the viewpoint of reactivity, it is preferable that calcium hydroxide, calcium oxide, or calcium carbonate is contained as a crystal structure as determined by X-ray diffraction method, and it is even more preferable that calcium hydroxide or calcium oxide is contained.

[0025] The incineration ash to be treated does not usually contain enough calcium (mass%) to produce the effect of the present invention, so calcium-containing waste is added to the incineration ash. By heat treating the incineration ash and calcium-containing waste in water, the alkali metals can be reduced more reliably.

[0026] The heating temperature in the underwater heat treatment of the method of the present invention is preferably 60 to 100°C, more preferably 70 to 100°C, even more preferably 80 to 100°C, and particularly preferably 100°C. When the treatment is performed at 100°C, heating may be performed while replenishing water to compensate for the evaporation, but from the viewpoint of efficient energy utilization, it is preferable to adopt a reflux system in which a heat exchanger is connected to the reaction tank and the evaporated water is returned to the reaction tank. Note that heating may be performed under pressure to a temperature above 100°C to about 200°C.

[0027] The heating time is preferably from 1 to 24 hours, more preferably from 2 to 12 hours, and even more preferably from 3 to 8 hours.

[0028] The heating method is not particularly limited as long as it can heat to a desired temperature. For example, heating methods using electricity, heating oil, steam, etc. are included, and a direct heating method using steam is preferred.

[0029] The heat treatment is preferably carried out with stirring. Any stirring method can be used as long as it can uniformly mix the slurry to be treated, and a general stirrer can be used.

[0030] The manufacturing method of modified incineration ash and the method of modifying incineration ash of the present invention specifically include, for example, a mixing step of mixing incineration ash, calcium-containing waste and water, a heating step of heating and stirring the mixture, and a filtering and washing step of filtering and washing the treated incineration ash. Since the important heating step of the present invention has been described above, the mixing step and the filtering and washing steps will be described below.

[0031] (Mixing process) The mixing step is a step of mixing the incineration ash, calcium-containing waste and water, and the order of mixing the incineration ash, calcium-containing waste and water does not matter. For example, the incineration ash and calcium-containing waste components may be mixed, and then water may be added and mixed, or the incineration ash and water may be mixed, and then the calcium-containing waste may be added and mixed. In the case of continuous treatment, each component may be added (after mixing as necessary) to a slurry containing all of these components during treatment and mixed.

[0032] The mixing mass ratio of incineration ash to water (incineration ash:water) is preferably in the range of 1:1.0 to 10.0, more preferably in the range of 1:1.0 to 5.0, and even more preferably in the range of 1:2.0 to 5.0. By being in this range, the incineration ash is sufficiently mixed with water, and the amount of water is not too much, so that the use of unnecessary heat energy can be suppressed.

[0033] (filtration and washing process) The filtration and washing process is a process in which the incineration ash that has been heat-treated in water in the heating process is filtered and washed. Any method can be used for the filtration, and examples include methods using a filter press, a belt filter, a drum filter, etc. The filtration temperature can be any temperature because dissolved sodium and potassium compounds (NaCl, KCl, NaOH, KOH) have high solubility and the solubility does not change significantly even if the water temperature is changed. The liquid used for washing can be industrial water, tap water, distilled water, ion-exchanged water, etc., and is preferably used in an amount three times or more, more preferably five times or more, by mass ratio relative to the incineration ash. The temperature of the washing water can also be any temperature for the above reasons.

[0034] [Cement manufacturing method] The modified incineration ash produced as described above can be used as a part of the cement material. That is, the method for producing cement of the present invention is a method for producing cement by using the modified incineration ash produced by the above-mentioned production method of the present invention as a part of the raw material. Specifically, for example, there can be mentioned a method for producing cement by using cement clinker produced by using the modified incineration ash, and a method for producing cement by using the modified incineration ash as a mixed material together with cement clinker, etc.

[0035] The total alkali content (RO) of the modified incineration ash is preferably 2.5% by mass or less, more preferably 2.0% by mass or less. The modified incineration ash of the present invention has a low total alkali content (RO), and can be used as a cement clinker raw material, a cement admixture, a concrete admixture, etc.

[0036] Total amount of alkali (R2O) = amount of Na2O + 0.658 x amount of K2O The total alkali content (R2O) is a conversion value indicating the total alkali content specified in the JIS standard for cement (JIS R 5210). The total alkali content (R2O) in the incineration ash can be calculated, for example, by using the above formula from the amount of Na2O and the amount of K2O determined by a method based on JIS R5204 "Fluorescent X-ray analysis method for cement".

[0037] Moreover, the potassium content (K2O) of the modified incineration ash is preferably 2.5 mass% or less, more preferably 2.0 mass% or less, and even more preferably 1.5 mass% or less. EXAMPLES

[0038] [Example 1] 100g of PKS incineration ash, 20g of calcium-containing waste I, and 300g of ion-exchanged water were weighed into a 500mL three-neck flask. The calcium-containing waste I contained calcium as CaO and CaCl2. An Arlinn-type cooling tube through which cooling water adjusted to 25°C was passed using a circulating cooling water device, a thermometer (0-100°C mercury thermometer), and a PTFE stirring blade connected to a stirrer (three-one motor) were connected to the three-neck flask, and then the mixture was stirred at 200 rpm. When the three-neck flask was heated using a mantle heater, the slurry temperature in the flask reached 100°C after about 45 minutes. Six hours after reaching 100°C, the mantle heater was removed from the flask and heating was terminated. After confirming that the slurry temperature was 40°C or lower about two hours after the end of heating, stirring using the stirrer was stopped, and the slurry in the flask was suction filtered (Advantec 5B filter paper) to filter out the solids. The filtered solid was washed with 500 mL of ion-exchanged water and then dried at 105°C to obtain modified incineration ash.

[0039] The compositions of the raw incineration ash and calcium-containing waste used were analyzed using a method in accordance with JIS R 5204 "Fluorescent X-ray analysis method for cement", and are shown in Tables 1 and 2. In addition, the state of calcium in the raw incineration ash and calcium-containing waste was measured using an X-ray diffractometer (Burker, D8 ADVANCE) with a measurement range of 2θ5-65 deg, a step width of 0.02 deg, and a scan speed of 0.25 deg / min. The measurement results are shown in Table 2.

[0040] When the modified incineration ash was analyzed using a method in accordance with JIS R 5204 "Method for fluorescent X-ray analysis of cement," the potassium content (KO) was 3.1% by mass, the sodium content (NaO) was 0.4% by mass, and the RO content was 2.5% by mass.

[0041] [Example 2] The modification treatment was carried out in the same manner as in Example 1, except that calcium-containing waste II was used and the amount added was changed to 10 g. The calcium-containing waste II contained calcium as CaO. The potassium content (KO) of the modified incineration ash was 2.8% by mass, the sodium content (NaO) was 0.1% by mass, and RO was 1.9% by mass.

[0042] [Example 3] Except for changing the amount of calcium-containing waste II to 30 g, the modification treatment was carried out in the same manner as in Example 1. The potassium content (KO) of the modified incineration ash was 2.2 mass%, the sodium content (NaO) was undetectable, and the RO was 1.4 mass%.

[0043] [Example 4] The modification treatment was carried out in the same manner as in Example 1, except that calcium-containing waste III was used and the amount added was changed to 10 g. The calcium-containing waste III contained calcium as CaO, Ca(OH)2, and CaCO3. The potassium content (KO) of the modified incineration ash was 2.1% by mass, the sodium content (NaO) was 0.3% by mass, and the RO was 1.7% by mass.

[0044] [Example 5] Except for changing the amount of calcium-containing waste III to 20 g, the modification treatment was carried out in the same manner as in Example 1. The potassium content (KO) of the modified incineration ash was 1.6 mass%, the sodium content (NaO) was undetectable, and the RO was 1.0 mass%.

[0045] [Example 6] The modification treatment was carried out in the same manner as in Example 1, except that the amount of calcium-containing waste IV was changed to 20 g. The calcium-containing waste IV contained calcium as CaCO3. The potassium content (KO) of the modified incineration ash was 2.3 mass%, the sodium content (NaO) was 0.3 mass%, and the RO was 1.8 mass%.

[0046] [Example 7] The modification treatment was carried out in the same manner as in Example 5, except that the heating time after reaching 100°C was changed to 3 hours. The potassium content (KO) of the modified incineration ash was 2.2 mass%, the sodium content (NaO) was 0.3 mass%, and the RO was 1.7 mass%.

[0047] [Example 8] As in Example 5, the incineration ash, calcium-containing waste III, and ion-exchanged water were weighed, and a cooling tube, a thermometer, and a stirrer were connected, followed by stirring at 200 rpm. The three-neck flask was placed in a water bath and heated, and the slurry temperature in the flask reached 80°C after about 20 minutes. After that, the mixture was heated and stirred for 6 hours while adjusting the water bath temperature so that the slurry temperature was 80°C. After the heating was completed, the modification treatment was carried out in the same manner as in Example 1. The potassium content (K2O) of the modified incineration ash was 2.2% by mass, the sodium content (Na2O) was undetectable, and the R2O was 1.4% by mass.

[0048] [Comparative Example 1] Except for not adding calcium-containing waste, the modification treatment was carried out in the same manner as in Example 1. The potassium content (K2O) of the modified incineration ash was 4.4%, the sodium content (Na2O) was 0.2 mass%, and the R2O was 3.2 mass%.

[0049] [Comparative Example 2] The modification treatment was carried out in the same manner as in Example 5, except that instead of performing a heat treatment, stirring was carried out for 6 hours at room temperature. The potassium content (KO) of the modified incineration ash was 4.1%, the sodium content (NaO) was 0.2% by mass, and the RO was 2.9% by mass.

[0050] [Comparative Example 3] The modification treatment was carried out in the same manner as in Example 1, except that 12 g of sodium hydroxide (FUJIFILM Wako Pure Chemical Industries, Ltd., special grade reagent) was used instead of calcium-containing waste. The potassium content (KO) of the modified incineration ash was 4.3%, the sodium content (NaO) was 3.3%, and the RO was 6.2%.

[0051] The above results are summarized in Table 3.

[0052] [Table 1]

[0053] [Table 2]

[0054] [Table 3]

[0055] As shown in Table 3, in the examples of the present invention, the potassium content (K2O) and total alkali content (R2O) were effectively reduced. On the other hand, in Comparative Example 1, in which the calcium-containing waste required for the present invention was not added, and Comparative Example 2, in which heat treatment was not performed, almost no reduction in the potassium content or total alkali content was observed. Moreover, in Comparative Example 3, in which an alkali metal component (sodium hydroxide) was used instead of the calcium-containing waste, not only was there almost no reduction in the potassium content, but the sodium content increased. This is thought to be because the modified incineration ash took on a zeolite structure and sodium was incorporated.

[0056] The modified incineration ash produced by the method of the present invention can be used as a cement material, etc., and therefore the present invention is industrially useful.

Claims

1. A method for producing modified incineration ash by heat treating incineration ash and calcium-containing waste in water.

2. 2. The method for producing modified incineration ash according to claim 1, characterized in that the calcium content in 100% by mass of the solid content of the calcium-containing waste is 20% by mass or more in terms of CaO.

3. The method for producing modified incineration ash according to claim 1, wherein the amount of calcium in the calcium-containing waste is 5 parts by mass or more in terms of CaO per 100 parts by mass of the incineration ash.

4. The calcium in the calcium-containing waste is determined by X-ray diffraction to be CaO, Ca(OH), 2 and CaCO 3 The method for producing modified incineration ash according to claim 1, wherein the modified incineration ash has at least one crystal structure selected from the following:

5. The method for producing modified incineration ash according to claim 1, wherein the incineration ash is at least one selected from biomass ash, coal ash, and garbage incineration ash.

6. The method for producing modified incineration ash according to claim 1, wherein the heating temperature in the heat treatment is 60 to 100° C. and the heating time is 1 to 24 hours.

7. A method for producing cement, comprising the steps of: producing cement by using modified incineration ash produced by the method according to any one of claims 1 to 6 as a part of raw materials.

8. A method for modifying incineration ash by heat treating incineration ash and calcium-containing waste in water.

Citation Information

Patent Citations

  • Manufacturing method of low potassium woody biomass ash, potassium reduction method of woody biomass ash, manufacturing method of cement, and method of converting woody biomass ash to cement resource

    JP2021104482A

  • Alkali metal removal method and alkali metal removal device

    JP2021146236A