Manufacturing method of recycled acrylic resin

The method improves adhesive layer removal in recycled acrylic resin production by alkali treatment and alcohol or high-temperature water immersion, enhancing efficiency and reducing defects.

JP2024146746APending Publication Date: 2024-10-15KANEKA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024009906
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-01-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing methods for recycling acrylic resin polarizer protective films with an adhesive layer are inefficient at low alkaline solution temperatures, leading to defects in optical films.

Method used

A method involving alkali treatment followed by immersion in alcohol or high-temperature water to enhance adhesive layer removal, with specific temperature and stirring conditions, and using acrylic resins with heterocyclic structural units to prevent gelation.

Benefits of technology

Increases adhesive layer removal rate at lower alkaline solution temperatures, reducing film defects and maintaining resin integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146746000001
    Figure 2024146746000001
  • Figure 2024146746000002
    Figure 2024146746000002
  • Figure 2024146746000003
    Figure 2024146746000003
Patent Text Reader

Abstract

To provide a manufacturing method of a recycled acrylic resin capable of increasing the removal ratio of an easily adhesive layer even when a temperature of an alkali aqueous solution is made low.SOLUTION: A manufacturing method of a recycled acrylic resin is a method for manufacturing the recycled acrylic resin by removing an easily adhesive layer from an acrylic resin base material to which the easily adhesive layer adheres. The manufacturing method of the recycled acrylic resin includes a step of carrying out an alkali treatment by immersing the acrylic resin base material, to which the easily adhesive layer adheres, in an alkali aqueous solution. The method further includes, after the step of carrying out the alkali treatment, a step of post-treating with an alcohol or high-temperature water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing recycled acrylic resin. [Background technology]

[0002] In a liquid crystal display device, two polarizers are usually arranged on both sides of a liquid crystal cell, and the polarizers are provided with a polarizer protective film to protect their surfaces. An acrylic film may be used as the polarizer protective film, and an easy-adhesion layer may be formed on one side of the acrylic film to improve adhesion between the film and the polarizer. In this film, the polarizer protective film is adhered to the polarizer by applying an adhesive to the easy-adhesion layer (see Patent Documents 1 and 2).

[0003] In recent years, from the perspective of making effective use of materials, efforts have been made to regenerate resin by using film scraps as part of the raw materials. However, in the case of a polarizer protective film having an easy-adhesion layer, when the scraps are used as part of the raw materials to produce a resin for an optical film, it is necessary to remove the easy-adhesion layer in order to prevent film defects caused by the easy-adhesion layer remaining as a foreign matter.

[0004] As a method for removing a layer (heterogeneous layer) made of a resin different from that of the substrate and laminated on the substrate made of a resin, for example, Patent Document 3 discloses a method in which a heterogeneous layer provided on a substrate made of a synthetic resin or an organic cellulose acid ester is removed in an alkaline aqueous solution at 105° C. or higher, and then the alkaline aqueous solution is removed from the substrate. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 168960 [Patent Document 2] JP 2010-055062 A [Patent Document 3] JP 2001-310970 A Summary of the Invention [Problem to be solved by the invention]

[0006] The method described in Patent Document 3 can also be applied to the recycling of an acrylic resin polarizer protective film having an easy-adhesion layer. However, if the temperature of the alkaline aqueous solution is low, the removal rate of the easy-adhesion layer is low, and when such a recycled resin film is used as an optical film, this leads to the occurrence of defects.

[0007] An object of the present invention is to provide a method for producing a recycled acrylic resin that can increase the removal rate of an easy-adhesion layer even when the temperature of an alkaline aqueous solution is low. [Means for solving the problem]

[0008] The present invention relates to the following:

[0009] [1] A method for producing a recycled acrylic resin by removing an easy-adhesion layer from an acrylic resin substrate having an easy-adhesion layer attached thereto, comprising the step of immersing the acrylic resin substrate having the easy-adhesion layer attached thereto in an alkaline aqueous solution to perform an alkali treatment, A method for producing a recycled acrylic resin, comprising the step of immersing the acrylic resin substrate in alcohol or an aqueous alcohol solution after the alkali treatment step.

[0010] [2] A method for producing a recycled acrylic resin by removing an easy-adhesion layer from an acrylic resin substrate having an easy-adhesion layer attached thereto, comprising the step of immersing the acrylic resin substrate having the easy-adhesion layer attached thereto in an alkaline aqueous solution to perform an alkali treatment, The method for producing a recycled acrylic resin comprises a step of immersing the acrylic resin substrate in high-temperature water for post-treatment after the alkali treatment step. [3] The method for producing recycled acrylic resin described in [1], wherein the alcohol or alcohol aqueous solution contains ethanol. [4] The method for producing a recycled acrylic resin according to [2], wherein the step of immersing in hot water for post-treatment is carried out at 70°C to 100°C with stirring. [5] The method for producing a recycled acrylic resin according to any one of [1] to [4], wherein the temperature of the alkaline aqueous solution is 15°C or higher and 60°C or lower. [6] The method for producing a recycled acrylic resin according to any one of [1] to [5], wherein the acrylic resin has a structural unit containing, in its main chain, one or more heterocycles selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring. [7] The acrylic resin is represented by the formula (1) [ka] (In formula (1), R1 and R2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and R3 is an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms.) The method for producing the recycled acrylic resin according to [6], which has a structural unit represented by the formula: [8] The method for producing a recycled acrylic resin according to any one of [1] to [7], wherein the easy-adhesion layer contains a urethane resin. Effect of the Invention

[0011] According to the present invention, there can be provided a method for producing a recycled acrylic resin that can increase the removal rate of an easy-adhesion layer even when the temperature of the alkaline aqueous solution is low. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described.

[0013] [Method of manufacturing recycled acrylic resin] The method for producing a recycled acrylic resin of this embodiment is a method for producing a recycled acrylic resin by removing an easy-adhesion layer from an acrylic resin substrate to which the easy-adhesion layer is attached. Specifically, the method for producing a recycled acrylic resin of this embodiment includes a step of immersing an acrylic resin substrate to which an easy-adhesion layer is attached in an alkaline aqueous solution to perform an alkali treatment. Here, since the method includes a step of immersing the acrylic resin substrate in hot water, alcohol or an alcohol aqueous solution to perform a post-treatment after the alkali treatment step, the removal rate of the easy-adhesion layer is high even if the temperature of the alkaline aqueous solution is low (for example, 60°C or less).

[0014] In the present specification and claims, the acrylic resin means a polymer of a monomer having an acryloyl group and / or a monomer having a methacryloyl group. In this case, the acrylic resin may be either a homopolymer or a copolymer. When the acrylic resin is a copolymer, the acrylic resin may be a copolymer of a monomer not having an acryloyl group or a methacryloyl group.

[0015] In the present invention, the acrylic resin substrate having an easy-adhesion layer attached thereto can be, for example, an acrylic film having an easy-adhesion layer formed on one side thereof, which is obtained by crushing scraps generated during the production of a polarizer protective film. After crushing the scraps, the scraps may be sized.

[0016] The thickness of the acrylic film is not particularly limited, but is, for example, 10 μm to 100 μm, and the thickness of the easy-adhesion layer is not particularly limited, but is, for example, 0.2 μm to 0.4 μm.

[0017] (Alkaline treatment process) In the method for producing the recycled acrylic resin of the present invention, first, the acrylic resin substrate having the easy-adhesion layer attached thereto is immersed in an alkaline aqueous solution and stirred.

[0018] In the alkali treatment step, the temperature of the alkaline aqueous solution is preferably 15°C or higher and 60°C or lower, more preferably 20°C or higher and 50°C or lower, and even more preferably 25°C or higher and 40°C or lower. When the temperature of the alkaline aqueous solution is 15°C or higher, the removal rate of the easy-adhesion layer is high, and when it is 60°C or lower, it is easy to handle. Furthermore, when the acrylic resin has a structural unit containing one or more heterocycles selected from the group consisting of glutarimide ring, lactone ring, maleic anhydride ring, maleimide ring, and glutaric anhydride ring in the main chain, if the temperature of the alkaline aqueous solution is 60°C or lower, the recycled acrylic resin is less likely to gel. For this reason, the manufacturing method of the recycled acrylic resin of this embodiment is preferably applied to an acrylic resin having a structural unit containing a specific heterocycle in the main chain. The exact mechanism of gelation of the recycled acrylic resin is not clear. For example, it is considered that the recycled acrylic resin having a structural unit containing a glutarimide ring in the main chain gels by hydrolysis of glutarimide, and the resulting amide group and carboxyl group become reaction points and intermolecular crosslinking. The same is thought to be true for acrylic resins that have structural units containing heterocycles other than glutarimide rings in the main chain. When gelled recycled acrylic resin is melt-formed into a film, fish-eye defects result due to localized differences in fluidity. Whether or not recycled acrylic resin has gelled can be easily determined by dissolving it in a solvent such as methylene chloride and then visually checking whether or not there is any insoluble matter.

[0019] The time for immersing the acrylic resin substrate in the alkaline aqueous solution is not particularly limited, but may be, for example, 10 minutes to 60 minutes, or 10 minutes to 35 minutes. For example, when post-treatment is performed with alcohol or an alcohol aqueous solution, the time may be 10 minutes to 35 minutes, and when post-treatment is performed with high-temperature water, the time may be 10 minutes to 60 minutes.

[0020] The base contained in the alkaline aqueous solution is not particularly limited, but may be, for example, one or more aqueous solutions selected from sodium hydroxide, lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, and magnesium hydroxide. Among them, it is preferable to use one or more aqueous solutions selected from lithium hydroxide, sodium hydroxide, and potassium hydroxide, and it is particularly preferable to use one or more aqueous solutions selected from sodium hydroxide and potassium hydroxide. The pH of the alkaline aqueous solution is not particularly limited, but may be, for example, 10 to 14.

[0021] (Post-processing) After the acrylic resin substrate is subjected to an alkali treatment, the substrate is immersed in hot water, alcohol, or an alcohol aqueous solution. The alcohol treatment step of immersing the substrate in alcohol or an alcohol aqueous solution and the high-temperature water treatment step of immersing the substrate in hot water are described below.

[0022] (Alcohol treatment process (post-treatment process)) In the alcohol treatment step, the acrylic resin substrate is subjected to an alkali treatment, and then the substrate is immersed in alcohol or an aqueous alcohol solution.

[0023] The alcohol used in this step may be one or more selected from methanol, ethanol, propanol, isopropyl alcohol (IPA), etc., but from the viewpoint of being able to remove the easy-adhesion layer more efficiently, one or more selected from ethanol and isopropyl alcohol are preferred, and ethanol is more preferred.

[0024] The concentration of the aqueous alcohol solution is preferably 50% by weight to 100% by weight, more preferably 80% by weight to 100% by weight, and 100% by weight, i.e., only alcohol may be used. When only alcohol is used, the easy-adhesion layer can be removed more efficiently. In this case, the alcohol may be a mixture of multiple alcohols.

[0025] The alcohol treatment is carried out by placing the substrate in a container and leaving it to stand for 5 minutes or more or by stirring. From the viewpoint of productivity, stirring is preferable. Stirring can be carried out using a magnetic stirrer or the like.

[0026] After carrying out the alkali treatment with alcohol or an aqueous alcohol solution, it is preferable to have a step of filtering the alcohol or the aqueous alcohol solution in which the acrylic resin substrate has been immersed, a step of washing the filtered residue with water, and a step of drying the washed filtered residue.

[0027] (High-temperature water treatment process (post-treatment process)) In this specification, "high temperature water" means water at normal pressure having a temperature of 70°C or higher and 100°C or lower. The temperature of the high temperature water is preferably 80°C or higher and 100°C or lower, and more preferably 85°C or higher and 95°C or lower.

[0028] The high-temperature water treatment can be carried out by placing the substrate in a container and leaving it to stand for 5 minutes or more, stirring, shaking, or the like, or by a combination of these. From the viewpoint of productivity, the high-temperature water treatment is preferably carried out with stirring. Stirring can be carried out using a magnetic stirrer or the like.

[0029] The recycled acrylic resin produced by the method of the present embodiment may be mixed with virgin acrylic resin as required for use.

[0030] The recycled acrylic resin can be applied to electronic materials, etc., without being particularly limited. For example, a film containing the recycled acrylic resin can be used as an antenna substrate, a display substrate, a touch panel substrate, etc. Examples of display substrates include a film for a liquid crystal display, a surface protective film, a polarizer protective film, etc. The film containing the recycled acrylic resin can be particularly suitably used in known optical applications such as the periphery of a liquid crystal display device, such as an optically isotropic film, a polarizer protective film, a transparent conductive film, etc., by utilizing its optical properties. In addition, the film containing the recycled acrylic resin can be attached to a polarizer and used as a polarizing plate. That is, the film containing the recycled acrylic resin can be used as a polarizer protective film of a polarizing plate.

[0031] [Acrylic resin] The acrylic resin used for regeneration may have a structural unit containing one or more heterocyclic rings selected from the group consisting of glutarimide ring, lactone ring, maleic anhydride ring, maleimide ring, and glutaric anhydride ring in the main chain. In this case, if the temperature of the alkaline aqueous solution in which the acrylic resin substrate having the easy-adhesion layer is immersed is high, the regenerated acrylic resin may gel.

[0032] As the acrylic resin having a structural unit containing a heterocycle in the main chain, a known material can be used (see, for example, Patent Documents 1 and 2). The structural unit containing a glutarimide ring in the main chain can be, for example, a compound represented by the formula (1):

[0033] [ka]

[0034] (In formula (1), R1 and R2 are each independently a hydrogen atom or an alkyl group having from 1 to 8 carbon atoms, and R3 is an alkyl group having from 1 to 18 carbon atoms, a cycloalkyl group having from 3 to 12 carbon atoms, or an aryl group having from 6 to 10 carbon atoms.) An acrylic resin having a structural unit represented by formula (1) can be obtained, for example, by imidizing a methyl methacrylate resin and then esterifying it. In addition, an example of a commercially available acrylic resin having a structural unit containing a lactone ring in the main chain is Acriview (manufactured by Nippon Shokubai).

[0035] The content of the structural unit containing a heterocycle in the main chain in the acrylic resin is not particularly limited, but is, for example, 2% by weight or more and 80% by weight or less. The glass transition temperature of the acrylic resin is not particularly limited, but is, for example, 110° C. or more and 160° C. or less. The average refractive index of the acrylic resin is not particularly limited, but is, for example, 1.45 or more and 1.55 or less.

[0036] The acrylic resin may not have a ring structure. Examples of the acrylic resin having no ring structure include, but are not limited to, methyl methacrylate resin.

[0037] [Easy adhesive layer] The easy-adhesion layer contains a resin and may further contain a crosslinking agent. The easy-adhesion layer is formed, for example, by applying an easy-adhesive containing a resin and then drying it. Here, the resin may be a thermosetting resin or a thermoplastic resin. In addition, the easy-adhesion layer may have thermosetting properties by itself or may not have thermosetting properties.

[0038] The resin is not particularly limited, but examples thereof include urethane resin, epoxy resin, etc. Among these, urethane resin is preferable.

[0039] The urethane resin is not particularly limited, but known materials can be used (for example, see Patent Document 2). The urethane resin preferably has a carboxyl group. Examples of urethane resins having a carboxyl group include polyester urethane resins having a carboxyl group. Examples of commercially available polyester urethane resins having a carboxyl group include Superflex 210 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).

[0040] The crosslinking agent is not particularly limited as long as it is a material capable of crosslinking with the resin, and known materials can be used (for example, see Patent Document 2). Examples of materials capable of crosslinking with a urethane resin having a carboxyl group include compounds and polymers having an epoxy group, a carbodiimide group, or an oxazoline group. Examples of commercially available polymers having an oxazoline group include Epocross WS700 (manufactured by Nippon Shokubai).

[0041] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. EXAMPLES

[0042] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0043] (Glutarimide ring content) The 1H-NMR measurement of the acrylic resin was carried out using a nuclear magnetic resonance apparatus AvanceIII (manufactured by BRUKER) (400 MHz). At this time, the molar ratio of the structural unit containing a glutarimide ring in the main chain to the structural unit derived from methyl methacrylate not containing a heterocycle in the main chain was calculated, and then the content of the glutarimide ring was calculated by converting it into weight. Specifically, the molar ratio was calculated using the area A of the peak derived from the O-CH3 proton of methyl methacrylate around 3.5 to 3.8 ppm and the area B of the peak derived from the N-CH3 proton of the glutarimide ring around 3.0 to 3.3 ppm.

[0044] (glass transition temperature) Using a differential scanning calorimeter DSC7020 (manufactured by SII), measurements were performed in a nitrogen atmosphere at a temperature rise rate of 20° C. / min with a sample weight of 10 mg, and the glass transition temperature was determined by the midpoint method.

[0045] (average refractive index) The average refractive index was measured using an Abbe refractometer 3T (manufactured by Atago).

[0046] (Acrylic resin) As the acrylic resin, commercially available HTX-Z (content of glutarimide rings: 6% by weight, glass transition temperature: 125° C., average refractive index: 1.50, manufactured by Kaneka) was used.

[0047] (Preparation of original film) After drying the acrylic resin at 100°C for 5 hours, a raw film was produced using a 15mm diameter intermeshing co-rotating twin screw extruder (L / D=30) equipped with a T-die at the outlet. At this time, the acrylic resin was supplied from the hopper at 2kg / hr, the set temperature of each temperature control zone of the extruder was 270°C, and the screw rotation speed was 100rpm. The sheet-like molten resin extruded from the T-die was cooled with a cooling roll to obtain a raw film. The raw film had a width of 160mm and a thickness of 160μm.

[0048] (Preparation of easy-to-adhesive) 20 g of Epocross WS700 (manufactured by Nippon Shokubai), a resin with an oxazoline group and a solid content of 25% by weight, was added to 100 g of Superflex 210 (manufactured by Daiichi Kogyo Seiyaku), a polyester urethane resin with a solid content of 33% by weight and a carboxyl group, and then the mixture was stirred for 3 minutes to obtain an easy-to-use adhesive.

[0049] (Preparation of raw film with easy-adhesion layer) After corona discharge treatment was performed on one side of the raw film, an easy-adhesive was applied using a bar coater (wire size #6). The raw film with the easy-adhesive applied was placed in a hot air dryer and dried at 80°C for about 1 minute to form an easy-adhesive layer, and an raw film with an easy-adhesive layer was obtained.

[0050] (Preparation of stretched film with easy-adhesion layer) Using a simultaneous biaxial stretching machine IMC-1905 (manufactured by Imoto Manufacturing Co., Ltd.), the raw film with the easy-adhesion layer was stretched at 145°C at a stretch ratio of 2 times in MD and TD to obtain a stretched film with the easy-adhesion layer. The stretched film with the easy-adhesion layer had a thickness of 40 μm, and the easy-adhesion layer had a thickness of 0.35 μm.

[0051] (Examples 1 to 3, Comparative Examples 1 to 5) The stretched film with the easy-adhesion layer was cut with a shredder to obtain small pieces of about 5 mm x 15 mm. The obtained small pieces of the stretched film with the easy-adhesion layer were acrylic resin substrates with the easy-adhesion layer attached.

[0052] In a flask equipped with a stirrer, 100 g of a strip of the stretched film with an easy-adhesion layer was immersed in 1000 ml of 4 wt % NaOH aqueous solution and stirred for 15 minutes under the specified conditions (see Table 1) to perform an alkali treatment. After that, it was filtered through a 200 mesh stainless steel filter, and the filtered material was placed in another flask equipped with a stirrer and immersed in 1000 ml of 100 wt % alcohol for post-treatment. After that, it was filtered through a 200 mesh stainless steel filter, and the filtered material was washed with water and then dried to obtain a regenerated acrylic resin.

[0053] As post-treatment, in Example 1, 100% by weight of ethanol was used, and in Example 2, 100% by weight of IPA (isopropyl alcohol) was used, and the flask was stirred at room temperature (25°C) for 5 minutes. In Example 3, post-treatment was performed with high-temperature water (purified water) at 90°C. In the post-treatment process, the flask containing high-temperature water at 90°C was stirred for 5 minutes. In Comparative Examples 1 and 5, water (purified water) was used instead of alcohol as post-treatment, and stirring was performed at room temperature (25°C) for 5 minutes. In Comparative Examples 2 to 4, no post-treatment was performed. In Comparative Example 4, no alkali treatment was performed, and water (purified water) was used instead of the 4% by weight NaOH aqueous solution.

[0054] (Production of recycled pellets) The recycled acrylic resin was mixed with the unused acrylic resin at 15% by weight, and the mixture was dry-blended, and then recycled pellets were obtained using a 15 mm diameter intermeshing co-rotating twin screw extruder (L / D=30). At this time, the temperature setting of each temperature control zone of the extruder was 260°C, and the screw rotation speed was 100 rpm.

[0055] (Production of recycled film) A recycled film was obtained in the same manner as in (Preparation of original film) except that the recycled pellets were used.

[0056] (Removal rate of easily adhesive layer) 0.1 g of the recycled acrylic resin and 9 g of a 4 wt% NaOH aqueous solution were placed in a test tube, and then heated at 90°C for 3 hours to dissolve the components of the easy-adhesion layer remaining in the recycled acrylic resin, obtaining a solution. The resulting solution was placed in a glass cell with an optical path length of 1 cm, and the absorbance Ab1 at a wavelength of 250 nm was measured using a UV-Visible Spectrophotometer V-550 (manufactured by JASCO). The absorbance Ab2 at a wavelength of 250 nm was measured in the same manner as above, except that a strip of the stretched film with an easy-adhesion layer was used instead of the recycled acrylic resin. formula (1-Ab1 / Ab2) x 100 The removal rate of the easy-adhesion layer was calculated by the above. It is assumed that the light absorption at a wavelength of 250 nm is mainly due to the aromatic rings of the polyester that constitutes the urethane resin contained in the easy-adhesion layer.

[0057] (Gelling of recycled acrylic resin) The recycled acrylic resin was dissolved in methylene chloride to a solid content of 10% by weight, and the presence or absence of insoluble matter was visually confirmed to evaluate the gelation of the recycled acrylic resin. The gelation criteria for the recycled acrylic resin were as follows: A: When insoluble matter is not present B: When insoluble matter is present

[0058] (Defects in recycled film) The recycled film was visually inspected for defects within a 10 cm x 10 cm area and evaluated for defects. The criteria for judging the defects of the recycled film are as follows: A: If there is no defect B: If there are 1 to 2 defects C: If there are three or more defects Table 1 shows the evaluation results of the removal rate of the easy-adhesion layer, the gelation of the recycled acrylic resin, and defects in the recycled film.

[0059] [Table 1]

[0060] From Table 1, it can be seen that in Examples 1 to 3, although the temperature of the alkaline aqueous solution is low, the removal rate of the easy-adhesion layer is high, and therefore defects in the recycled film are few. In particular, in Example 1, in which post-treatment was performed using ethanol, the removal rate of the easy-adhesion layer (urethane resin) is high, and defects in the recycled film are suppressed, despite the low temperature of the alkaline aqueous solution and the short immersion time. In addition, in Examples 1 to 3, an acrylic resin having a constitutional unit represented by formula (1) is used, and gelation of the recycled acrylic resin is suppressed.

[0061] In contrast, in Comparative Example 1, since post-treatment is performed with water instead of alcohol, the removal rate of the easy-adhesion layer (urethane resin) is low, and the recycled film has many defects. In Comparative Example 2, since the temperature of the alkaline aqueous solution is low and post-treatment with alcohol is not performed, the removal rate of the easy-adhesion layer is low and the recycled film has many defects. In Comparative Example 3, since the temperature of the alkaline aqueous solution is high and an acrylic resin having a constitutional unit represented by formula (1) is used, the recycled acrylic resin gels and the recycled film has many defects. In Comparative Example 4, since no alkaline treatment is performed, the recycled film has many defects. In Comparative Example 5, since post-treatment is performed with water (25°C) instead of high-temperature water, the removal rate of the easy-adhesion layer (urethane resin) is low and the recycled film has many defects.

Claims

1. A method for producing a recycled acrylic resin by removing an easy-adhesion layer from an acrylic resin substrate to which the easy-adhesion layer is attached, comprising: The acrylic resin substrate having the easy-adhesion layer attached thereto is immersed in an alkaline aqueous solution to perform an alkali treatment, A method for producing a recycled acrylic resin, comprising the step of immersing the acrylic resin substrate in alcohol or an aqueous alcohol solution after the alkali treatment step.

2. A method for producing a recycled acrylic resin by removing an easy-adhesion layer from an acrylic resin substrate to which the easy-adhesion layer is attached, comprising: The acrylic resin substrate having the easy-adhesion layer attached thereto is immersed in an alkaline aqueous solution to perform an alkali treatment, The method for producing a recycled acrylic resin comprises a step of immersing the acrylic resin substrate in high-temperature water for post-treatment after the alkali treatment step.

3. The method for producing recycled acrylic resin according to claim 1 , wherein the alcohol or aqueous alcohol solution contains ethanol.

4. The method for producing a recycled acrylic resin according to claim 2, wherein the step of immersing in hot water for post-treatment is carried out at 70°C to 100°C with stirring.

5. The method for producing a recycled acrylic resin according to claim 1 or 2, wherein the temperature of the alkaline aqueous solution is 15°C or higher and 60°C or lower.

6. 3. The method for producing a recycled acrylic resin according to claim 1, wherein the acrylic resin has a structural unit containing in its main chain one or more heterocycles selected from the group consisting of a glutarimide ring, a lactone ring, a maleic anhydride ring, a maleimide ring, and a glutaric anhydride ring.

7. The acrylic resin is represented by the formula (1) 【Chemistry 1】 (In formula (1), R1 and R2 are each independently a hydrogen atom or an alkyl group having 1 to 8 carbon atoms, and R3 is an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms.) The method for producing the recycled acrylic resin according to claim 5, which has a structural unit represented by the following formula:

8. The method for producing a recycled acrylic resin according to claim 1 or 2, wherein the easy-adhesion layer contains a urethane resin.

Citation Information

Patent Citations

  • Method for recovering synthetic resin materials

    JP2001310970A

  • Polarizer-protecting film, and polarizing plate and image display device using polarizer-protecting film

    JP2010055062A

  • Stretched film and method for producing stretched film

    WO2018168960A1