Polarizer and polarizing plate

A polyvinyl alcohol resin film polarizer with balanced iodine, boron, zinc, and potassium content, combined with specific processing, addresses hue changes at high temperatures by stabilizing absorbance, ensuring color stability in automotive applications.

JP2024146861APending Publication Date: 2024-10-15SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024051593
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Conventional polarizers formed from polyvinyl alcohol resin films fail to sufficiently suppress hue changes due to polyenization when exposed to high temperatures, particularly in automotive applications where temperatures exceed 115°C.

Method used

A polarizer composed of a polyvinyl alcohol resin film with specific elemental compositions and processing steps, including swelling, dyeing, crosslinking, and stretching, to maintain a balanced content of iodine, boron, zinc, and potassium, ensuring the parameter S[h] is within a predetermined range to minimize hue changes over time.

Benefits of technology

The polarizer effectively suppresses hue changes when exposed to high temperatures by maintaining a stable absorbance profile, reducing the formation of polyene chains that absorb visible light, thus maintaining color stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146861000001_ABST
    Figure 2024146861000001_ABST
Patent Text Reader

Abstract

To make it possible to suppress changes in a hue of polarizers in a state exposed to a high temperature of 115°C.SOLUTION: A polarizer is formed of a polyvinyl alcohol resin film and satisfies that an area S[h] obtained by integrating a function f(t) related to absorbance into which coefficients a to e obtained by the following steps (1) to (2) are assigned over a time t=0 to 72 hours is 0.1 h or more and 45 h or less. Step (1): In a state where the polarizer is exposed to an environment of 115°C, the absorbance at 780 nm of a pair of polarizers using a cross-Nicoll is measured at each of 0 hours, 24 hours, 48 hours, 120 hours, 240 hours, and 500 hours. Step (2): Based on seven combinations of time and absorbance obtained in Step (1) and the function f(t) related to absorbance, perform curve fitting using the least squares method is performed to obtain the coefficients a to e. f(t)=a*Exp(-b*t)+c*Exp(-d*t)+e, where t denotes a time [h], and a to e denote coefficients.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizer and a polarizing plate. [Background technology]

[0002] Conventionally, polarizers formed from a film containing a polyvinyl alcohol-based resin and iodine have been known (for example, Patent Document 1). Image display devices including polarizers are used in a wide range of applications, such as in-vehicle image display devices such as car navigation devices and rear monitors. As the applications expand, image display devices and polarizers that form part of image display devices are required to have higher durability in harsher environments (for example, high-temperature environments) than has been conventionally required. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-71241 A Summary of the Invention [Problem to be solved by the invention]

[0004] When a polarizer formed from a polyvinyl alcohol-based resin film is exposed to a high-temperature environment, polyenization of polyvinyl alcohol proceeds, and a problem of a change in hue of the polarizer due to polyenization may occur. In particular, in a high-temperature environment (e.g., 115°C) such as the above-mentioned in-vehicle application, the hue change due to polyenization tends to be more significant. However, in the case of conventional polarizers, it was not necessarily the case that the suppression of the hue change at such high temperatures was sufficient.

[0005] The present invention has been made in view of the above problems, and has an object to provide a polarizer etc. capable of suppressing change in hue of the polarizer when exposed to a high temperature of 115°C. [Means for solving the problem]

[0006] [1] A polarizer formed from a polyvinyl alcohol-based resin film, A polarizer in which the area S[h] obtained by integrating the following function f(t) regarding absorbance, into which coefficients a to e obtained by the following steps (1) and (2) are substituted, over a period of t = 0 to 72 hours, satisfies the range of 0.1h to 45h. Procedure (1): With the polarizer exposed to an environment at 115° C., the absorbance at 780 nm of the pair of polarizers in crossed Nicols is measured at 0 hours, 24 hours, 48 ​​hours, 120 hours, 240 hours, and 500 hours. Step (2): Based on the seven combinations of time and absorbance obtained in step (1) and the following function f(t) related to absorbance, curve fitting is performed by the least squares method to obtain coefficients a to e. f(t)=a·Exp(-b·t)+c·Exp(-d·t)+e t: time [h] a~e: Coefficients [2] A polarizing plate comprising the polarizer according to [1], an adhesive layer, and a protective film, in this order. Effect of the Invention

[0007] A polarizer capable of suppressing a change in hue of the polarizer when exposed to a high temperature of 115° C. is provided. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a cross-sectional view showing a polarizing plate according to an embodiment. [Diagram 2] 1 is a graph showing the combination of absorbance and time, and f(t) obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Polarizer> The polarizer according to one embodiment is formed from a polyvinyl alcohol-based resin film.

[0010] (Polyvinyl alcohol resin) As the polyvinyl alcohol resin of the polyvinyl alcohol resin film, a saponified polyvinyl acetate resin can be used. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate and other monomers copolymerizable therewith. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group. The saponification degree of the polyvinyl alcohol resin is usually about 85 mol% or more, preferably about 90 mol% or more, and more preferably about 99 mol% or more. In this specification, "(meth)acrylic" means at least one selected from acrylic and methacrylic. The same applies to "(meth)acryloyl".

[0011] The polyvinyl alcohol resin may be modified. For example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc., which are modified with aldehydes may also be used.

[0012] The average degree of polymerization of the polyvinyl alcohol resin is preferably 100 or more and 10,000 or less, more preferably 1,500 or more and 8,000 or less, and further preferably 2,000 or more and 5,000 or less. The average degree of polymerization of the polyvinyl alcohol resin can be determined in accordance with JIS K 6726 (1994). If the average degree of polymerization is less than 100, it is difficult to obtain favorable polarizing performance, and if it exceeds 10,000, the film processability may be poor.

[0013] The polyvinyl alcohol-based resin film may be a single film formed from a polyvinyl alcohol-based resin, or may be a laminated film in which a base film and a polyvinyl alcohol-based resin film are laminated. In the case of a laminated film, for example, it can be produced by applying a coating liquid containing a polyvinyl alcohol-based resin to at least one surface of a base film and drying it.

[0014] Examples of the substrate film include thermoplastic resin films. The thermoplastic resin film is preferably a film made of an optically transparent thermoplastic resin, and may be a transparent resin film made of a polyolefin resin such as a chain polyolefin resin (such as a polypropylene resin) or a cyclic polyolefin resin (such as a norbornene resin); a cellulose ester resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate, polyethylene naphthalate, or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin such as a polymethyl methacrylate resin; or a mixture or copolymer thereof.

[0015] The thickness of the polarizer, i.e., the polyvinyl alcohol-based resin film, may be, for example, 30 μm or less, preferably 25 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, even more preferably 14 μm or less, particularly preferably 13 μm or less, and even more particularly preferably 12 μm or less. When the thickness of the polarizer is 30 μm or less, there is a tendency that it is easy to suppress light leakage. In addition, reducing the thickness of the polarizer is advantageous for making the polarizing plate thinner. The thickness of the polarizer is usually 2 μm or more, and may be, for example, 5 μm or more.

[0016] The polyvinyl alcohol-based resin film is preferably uniaxially stretched. A dichroic dye such as iodine may be adsorbed and oriented on the uniaxially stretched polyvinyl alcohol-based resin film.

[0017] (Elemental Boron) The polyvinyl alcohol-based resin film may contain boron element. There is no particular limitation on the content of boron element in the polyvinyl alcohol-based resin film, but it may be 3.5 mass% or more and 6.0 mass% or less. The boron element may crosslink the polyvinyl alcohol-based resin in the polyvinyl alcohol-based resin film. From the viewpoint of crosslinking between polyvinyl alcohol chains, the boron content in the polyvinyl alcohol-based resin film may be 5.5 mass% or less, 5.0 mass% or less, or 4.7 mass% or less. When the content of boron element in the polarizer is within the above range, crosslinking between polyvinyl alcohol chains is easy, and even if the dehydration reaction of polyvinyl alcohol progresses when exposed to a high temperature of 115 ° C., it is expected that the polyene chains do not become long enough to absorb light in the visible light region, and the hue change tends to be easily suppressed.

[0018] (Iodine element) The polyvinyl alcohol-based resin film may contain iodine element. The content of iodine element in the polyvinyl alcohol-based resin film is not particularly limited, but may be 2.0% by mass or more and 4.0% by mass or less.

[0019] Iodine is a dichroic dye, and can exhibit polarizing properties by being adsorbed and oriented in a polyvinyl alcohol-based resin film.

[0020] The content of iodine element in the polyvinyl alcohol-based resin film may be 2.1 mass% or more, 2.2 mass% or more, or 2.3 mass% or more. The content of iodine element in the polyvinyl alcohol-based resin film may be 3.5 mass% or less, 3.2 mass% or less, 3.0 mass% or less, 2.9 mass% or less, or 2.7 mass% or less. When the content of iodine element in the polarizer is within the above range, it tends to easily satisfy the parameter S described later.

[0021] (Zinc element) The polyvinyl alcohol-based resin film may contain zinc element. There is no particular limitation on the zinc element content in the polyvinyl alcohol-based resin film, but it may be 0.01% by mass or more and 1.0% by mass or less. The zinc content in the polyvinyl alcohol-based resin film may be 0.02% by mass or more, 0.03% by mass or more, or 0.05% by mass or more. The zinc content in the polyvinyl alcohol-based resin film may be 0.9% by mass or less, 0.7% by mass or less, 0.5% by mass or less, 0.3% by mass or less, 0.2% by mass or less, or 0.15% by mass or less. The zinc element has an I5 - When the zinc element content is within the above range, parameter S tends to be satisfied.

[0022] (elemental potassium) The polyvinyl alcohol-based resin film may contain potassium element. The potassium element content in the polyvinyl alcohol-based resin film is not particularly limited, but may be 0.40 mass% or more and 1.0 mass% or less. The potassium element in the polyvinyl alcohol-based resin film is expected to act as a protective group for the hydroxyl group of polyvinyl alcohol, and when the potassium element content in the polyvinyl alcohol-based resin film is within the above range, the dehydration reaction of polyvinyl alcohol is suppressed even when exposed to a high temperature of 115°C, and yellowing of the polyvinyl alcohol-based resin film due to polyenization tends to be easily suppressed.

[0023] The potassium element content in the polyvinyl alcohol-based resin film may be 0.90 mass% or less, 0.80 mass% or less, 0.70 mass% or less, 0.65 mass% or less, 0.60 mass% or less, 0.55 mass% or less, or 0.50 mass% or less.

[0024] The polarizer of this embodiment has the property of absorbing linearly polarized light having a vibration plane parallel to its absorption axis and transmitting linearly polarized light having a vibration plane perpendicular to the absorption axis (parallel to the transmission axis), and is a so-called absorption-type polarizer.

[0025] (Parameter A) In order to suppress an increase in the degree of change in hue of a polarizer over time when exposed to high temperatures, the polarizer of the present embodiment can satisfy the following formula (A).

[0026] 0.001≦[Zn] / ([I]×[B])≦0.025 (A) In the formula (A), [Zn] represents the zinc content (% by mass) in the polyvinyl alcohol-based resin film, [I] represents the iodine content (% by mass) in the polyvinyl alcohol-based resin film, and [B] represents the boron content (% by mass) in the polyvinyl alcohol-based resin film.

[0027] [Zn] / ([I]×[B]) may be 0.002 or more, 0.003 or more, 0.004 or more, or 0.005 or more.

[0028] [Zn] / ([I]×[B]) may be 0.020 or less, 0.018 or less, 0.015 or less, 0.014 or less, 0.013 or less, or 0.010 or less.

[0029] (Parameter C) In order to suppress yellowing after exposure to high temperatures, the polarizer of the present embodiment satisfies the following formula (C).

[0030] 0.001≦[Zn] / ([I]×[B]×[K])≦0.070 (C) [In formula (C), [Zn] represents the zinc content (% by mass) in the polyvinyl alcohol-based resin film, [I] represents the iodine content (% by mass) in the polyvinyl alcohol-based resin film, [B] represents the boron content (% by mass) in the polyvinyl alcohol-based resin film, and [K] represents the potassium content (% by mass) in the polyvinyl alcohol-based resin film.

[0031] [Zn] / ([I]×[B]×[K]) may be 0.003 or more, 0.005 or more, or 0.010 or more.

[0032] [Zn] / ([I]×[B]×[K]) may be 0.060 or less, 0.050 or less, 0.040 or less, 0.030 or less, or 0.025 or less.

[0033] (Parameter S) In order to suppress a change in hue when exposed to high temperatures, the polarizer according to this embodiment has an area S[h] that is calculated by integrating the following function f(t) related to absorbance, into which coefficients a to e obtained by the following steps (1) and (2) are substituted, over a period of t=0 to 72 hours, and satisfies 0.1 h or more and 45 h or less. The lower limit of the area S[h] may be 1.0 h, 3.0 h, 5.0 h, 10.0 h, or 15.0 h. The upper limit of the area S[h] may be 44 h or 43 h. Procedure (1): With the polarizer exposed to an environment at 115° C., the absorbance at 780 nm of the pair of polarizers in crossed Nicols is measured at 0 hours, 24 hours, 48 ​​hours, 120 hours, 240 hours, and 500 hours. Step (2): Based on the seven combinations of time and absorbance obtained in step (1) and the following function f(t) related to absorbance, curve fitting is performed by the least squares method to obtain coefficients a to e. f(t)=a·Exp(-b·t)+c·Exp(-d·t)+e t: time [h] a~e: Coefficients The optimization method in curve fitting is not particularly limited, but the GRG method (Generalized Reduced Gradient method) is preferable.

[0034] (Mechanism of action) In the polarizer according to this embodiment, the area S of the parameter S is within a predetermined range. Therefore, even if it is exposed to a high temperature of 115° C., the change in hue is suppressed. Since the function f(t) is the change in absorbance at 780 nm (red) over time, I5 - The value of area S is below a certain level, which means that even after 72 hours of exposure to a high temperature of 115°C, the amount of I5 - This means that the amount of I5 has decreased to some extent. - The reason why the color change due to polyenation is suppressed by reducing the amount of I5 is unclear, but even after 72 hours of exposure to a high temperature of 115°C, - In the case of a polarizer in which the amount of I2C can be maintained at a constant level, it is expected that the conversion of polyvinyl alcohol to polyene will proceed gradually, and the polyene chain will become long enough to absorb light in the visible light region, resulting in a greater change in hue. On the other hand, in the case of the present invention, when the I2C value is 150% after 72 hours of exposure to a high temperature of 115°C, - When I5 suddenly disappears from the polyvinyl alcohol resin, - Although the polyene of polyvinyl alcohol proceeds in the area where I5 ​​was present, it is believed that the polyene chain capable of absorbing light in the visible light region is not formed, and as a result, the hue change is suppressed. - If there is too little of this, the degree of polarization decreases, which is not preferable.

[0035] Although there is no particular limitation on the method for setting the parameter S within the predetermined range, it is preferable to satisfy the parameter S by containing potassium, iodine, boron, and zinc elements in the polarizer in a balanced manner. The polarizer containing potassium, iodine, boron, and zinc elements in a balanced manner is preferably a polarizer that satisfies the above parameter A or parameter C.

[0036] <Method of manufacturing polarizer> The manufacturing method according to one embodiment includes a swelling step, a dyeing step, a crosslinking step, an optional washing step, an optional drying step, and a stretching step.

[0037] (1) Swelling process The swelling treatment in this step is a treatment that is carried out as necessary for the purpose of removing foreign matter from the polyvinyl alcohol-based resin film, which is the raw film, removing plasticizers, imparting easy dyeing properties, plasticizing the film, etc., and specifically, it can be a treatment in which the polyvinyl alcohol-based resin film is immersed in a treatment liquid (swelling liquid) containing water. The polyvinyl alcohol-based resin film, which is the raw film, can be appropriately used from those exemplified in the explanation section of the polarizer. The resin film may be immersed in one swelling liquid, or may be immersed in two or more swelling liquids sequentially. The film may be uniaxially stretched before the swelling treatment, during the swelling treatment, or before and during the swelling treatment.

[0038] The thickness of the polyvinyl alcohol-based resin film, which is the raw film, is, for example, about 10 μm or more and 80 μm or less, and from the viewpoint of making the thickness of the polarizer 15 μm or less, it is preferably 40 μm or less, and more preferably 30 μm or less.

[0039] The polyvinyl alcohol-based resin film as the raw film can be prepared, for example, as a roll (wound product) of a long unstretched or stretched polyvinyl alcohol-based resin film. In this case, the polarizer is also obtained as a long product.

[0040] The swelling liquid can be water (for example, pure water), or it may be an aqueous solution containing a water-soluble organic solvent such as an alcohol.

[0041] The temperature of the swelling liquid when the raw film is immersed is usually about 10 to 70° C., preferably about 15 to 50° C., and the immersion time of the film is usually about 10 to 600 seconds, preferably about 20 to 300 seconds.

[0042] (2) Dyeing process The dyeing treatment in this step is a treatment performed for the purpose of adsorbing and orienting iodine in the polyvinyl alcohol-based resin film, and specifically, it can be a treatment of immersing the polyvinyl alcohol-based resin film in a treatment liquid (dyeing liquid) containing iodine. The film may be immersed in one dyeing liquid, or may be immersed in two or more dyeing liquids sequentially. In order to enhance the dyeability of iodine, the film to be subjected to the dyeing step may be subjected to at least a certain degree of uniaxial stretching treatment. Instead of or in addition to the uniaxial stretching treatment before the dyeing treatment, a uniaxial stretching treatment may be performed during the dyeing treatment.

[0043] Also, dichroic organic dyes can be used together with iodine. When using dichroic organic dyes, the dichroic organic dyes can be used in combination with iodine in one dyeing solution, or when using two or more dyeing tanks, they can be used in a dyeing solution different from the dyeing solution using iodine. Specific examples of dichroic organic dyes include Red BR, Red LR, Red R, Pink LB, Rubin BL, Bordeaux GS, Sky Blue LG, Lemon Yellow, Blue BR, Blue 2R, Navy RY, Green LG, Violet LB, Violet B, Black H, Black B, Black GSP, Yellow 3G, Yellow R, Orange LR, Orange 3R, Scarlet GL, Scarlet KGL, Congo Red, Brilliant Violet BK, Supra Blue G, Supra Blue GL, Supra Orange GL, Direct Sky Blue, Direct Fast Orange S, and Fast Black. The dichroic dyes may be used alone or in combination of two or more.

[0044] As the dyeing solution containing iodine, an aqueous solution containing iodine and potassium iodide can be used. Instead of potassium iodide, other iodides such as zinc iodide may be used, or potassium iodide may be used in combination with other iodides. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may be coexisted. When boric acid is added, it is distinguished from the crosslinking treatment described below in that it contains iodine. The content of iodine in the aqueous solution is usually 0.01 to 1 part by mass per 100 parts by mass of water. In addition, the content of iodides such as potassium iodide is usually 0.01 to 20 parts by mass per 100 parts by mass of water. The concentration of boric acid in the aqueous solution can be 0.1 to 5 parts by mass per 100 parts by mass of water.

[0045] The temperature of the dye solution when the film is immersed is usually 10° C. or more and 45° C. or less, preferably 10° C. or more and 40° C. or less, and more preferably 20° C. or more and 35° C. or less, and the immersion time of the film is usually 30 seconds or more and 600 seconds or less, and preferably 60 seconds or more and 300 seconds or less.

[0046] When a dichroic organic dye is used, an aqueous solution containing the dichroic organic dye can be used as the dye solution. The content of the dichroic organic dye in the aqueous solution is usually 1×10 per 100 parts by mass of water. -4 parts by mass or more and 10 parts by mass or less, preferably 1×10 -3 The amount is from parts by mass to 1 part by mass. The dyeing solution may contain a dyeing assistant, for example, an inorganic salt such as sodium sulfate, a surfactant, etc. The dichroic organic dye may be used alone or in combination of two or more kinds. The temperature of the dyeing solution when the film is immersed is, for example, from 20°C to 80°C, preferably from 30°C to 70°C, and the immersion time of the film is usually from 30 seconds to 600 seconds, preferably from 60 seconds to 300 seconds.

[0047] (3) Crosslinking process The crosslinking treatment of the polyvinyl alcohol-based resin film after the dyeing process with a crosslinking agent is a treatment for the purpose of water resistance or color adjustment by crosslinking, and specifically, it can be a treatment of immersing the film after the dyeing process in a treatment liquid (crosslinking liquid) containing a crosslinking agent. The film may be immersed in one crosslinking liquid, or may be immersed in two or more crosslinking liquids in sequence. A uniaxial stretching treatment may be performed during the crosslinking treatment.

[0048] (Crosslinking agent) Examples of the crosslinking agent include boric acid, glyoxal, glutaraldehyde, etc., and boric acid is preferably used. Two or more crosslinking agents can be used in combination. The content of boric acid in the crosslinking liquid is usually 0.1 parts by mass or more and 15 parts by mass or less, preferably 1 part by mass or more and 10 parts by mass or less, per 100 parts by mass of water.

[0049] (Iodide) When the dichroic dye is iodine, the crosslinking liquid preferably contains iodide in addition to boric acid. The content of iodide in the crosslinking liquid is usually 0.1 parts by mass or more and 15 parts by mass or less, preferably 1 part by mass or more and 12 parts by mass or less, per 100 parts by mass of water. Examples of iodide include potassium iodide and zinc iodide.

[0050] (Zinc sulfate and potassium sulfate) The cross-linking liquid further includes zinc sulfate and potassium sulfate.

[0051] The content of zinc sulfate (ZnSO4) in the crosslinking liquid may be 0.0005 parts by mass or more and 30 parts by mass or less, preferably 0.001 parts by mass or more and 25 parts by mass or less, and more preferably 0.1 parts by mass or more and 10 parts by mass or less, per 100 parts by mass of water.

[0052] The content of potassium sulfate (K2SO4) in the crosslinking liquid may usually be 0.1 parts by mass or more and 30 parts by mass or less per 100 parts by mass of water, preferably 0.2 parts by mass or more and 25 parts by mass or less, and more preferably 0.3 parts by mass or more and 20 parts by mass or less.

[0053] (Other ingredients) The crosslinking liquid may contain other components in addition to the crosslinking agent, iodide, zinc sulfate, and potassium sulfate.

[0054] Examples of other components contained in the crosslinking liquid include zinc salts other than zinc sulfate and potassium sulfate. Examples of zinc salts other than zinc sulfate and potassium sulfate contained in the crosslinking liquid include zinc halides such as zinc chloride and zinc iodide, zinc acetate, and zinc nitrate.

[0055] Other examples of components contained in the cross-linking liquid are cobalt chloride, zirconium chloride, sodium thiosulfate, and potassium sulfite.

[0056] When the polyvinyl alcohol-based resin film is immersed in a plurality of crosslinking liquids, the concentrations of zinc sulfate and potassium sulfate in the crosslinking liquids may be different for each crosslinking liquid.

[0057] By immersing a polyvinyl alcohol-based resin film in a crosslinking liquid containing zinc sulfate and potassium sulfate, the above-mentioned parameter S of the resulting polarizer can be satisfied, and the above-mentioned polarizer can be obtained. Although it is not clear why the parameter S of the resulting polarizer can be satisfied by immersing the film in a crosslinking liquid containing zinc sulfate and potassium sulfate, it is thought that the amount of potassium and zinc in the polarizer increases, which is thought to be I5. - The content of I5 after 72 hours of exposure to a high temperature of 115°C is reduced. - It is expected that the amount of is more easily reduced and the parameter S can be satisfied.

[0058] The temperature of the crosslinking liquid when the film is immersed is usually 50° C. or more and 85° C. or less, preferably 50° C. or more and 70° C. or less, and the immersion time of the film is usually 10 seconds or more and 600 seconds or less, preferably 20 seconds or more and 300 seconds or less.

[0059] In the crosslinking step, the polyvinyl alcohol-based resin film may be immersed in two or more crosslinking liquids. In this case, the composition and temperature of each crosslinking liquid may be the same or different. When the polyvinyl alcohol-based resin film is immersed in two or more crosslinking liquids, at least one of the crosslinking liquids contains zinc sulfate and potassium sulfate.

[0060] The crosslinking liquid may have a concentration of a crosslinking agent, an iodide, etc., and a temperature according to the purpose of immersing the polyvinyl alcohol-based resin film in. The crosslinking treatment for water resistance by crosslinking and the crosslinking treatment for hue adjustment (complementary color) may each be performed in a plurality of steps (for example, in a bath containing a plurality of treatment liquids).

[0061] In general, when both a crosslinking treatment for water resistance by crosslinking and a crosslinking treatment for hue adjustment (complementary color) are performed, a crosslinking liquid (complementary color liquid) for performing the crosslinking treatment for hue adjustment (complementary color) is placed in the latter stage. The temperature of the complementary color liquid is, for example, 10°C to 55°C, preferably 20°C to 50°C. The immersion time for immersing the film in the complementary color liquid is usually 5 seconds to 600 seconds, preferably 10 seconds to 300 seconds.

[0062] The content of the crosslinker in the complementary color liquid is, for example, 1 part by mass or more and 5 parts by mass or less per 100 parts by mass of water. The content of the iodide in the complementary color liquid is, for example, 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of water. As described above, the complementary color liquid can contain zinc salts and other components. When the complementary color liquid contains zinc sulfate, the content of zinc sulfate may be 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of water, and preferably 1 part by mass or more and 10 parts by mass or less. When the complementary color liquid contains potassium sulfate, the content of potassium sulfate may be 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of water, and preferably 1 part by mass or more and 10 parts by mass or less.

[0063] In the method for producing a polarizer of this embodiment, it is preferable that the polyvinyl alcohol-based resin film is uniaxially stretched (stretching step) at any one or more stages from before the swelling step to the crosslinking step. From the viewpoint of improving the dyeability of the dichroic dye, it is preferable that the film to be subjected to the dyeing step is a film that has been subjected to at least some degree of uniaxial stretching, or it is preferable to perform uniaxial stretching during the dyeing step instead of or in addition to the uniaxial stretching before the dyeing step.

[0064] The uniaxial stretching process may be either dry stretching in air or wet stretching in liquid, or both of these may be performed. The uniaxial stretching process may be inter-roll stretching, which involves longitudinal uniaxial stretching with a difference in peripheral speed between two nip rolls, hot roll stretching, tenter stretching, etc., but preferably includes inter-roll stretching. The stretching ratio based on the original film (when stretching is performed in two or more stages, the cumulative stretching ratio) is about 3 times or more and 8 times or less. In order to impart good polarization properties, the stretching ratio is preferably 4 times or more, more preferably 5 times or more.

[0065] (4) Cleaning process The cleaning treatment in this step is a treatment carried out as necessary for the purpose of removing excess crosslinking agent or chemicals such as dichroic dye attached to the polyvinyl alcohol-based resin film, and is a treatment of cleaning the polyvinyl alcohol-based resin film after the crosslinking step using a cleaning solution containing water. Specifically, it can be a treatment of immersing the polyvinyl alcohol-based resin film after the crosslinking step in a cleaning solution. The film may be immersed in one cleaning solution, or may be immersed in two or more cleaning solutions sequentially. Alternatively, the cleaning treatment may be a treatment of spraying the cleaning solution as a shower onto the polyvinyl alcohol-based resin film after the crosslinking step, or the above-mentioned immersion and spraying may be combined.

[0066] The cleaning liquid may be water (e.g., pure water) or an aqueous solution containing a water-soluble organic solvent such as alcohols. The temperature of the cleaning liquid may be, for example, about 5°C or higher and 40°C or lower.

[0067] The washing step is an optional step and may be omitted, or may be performed during the drying step as described below. Preferably, the film after the washing step is subjected to a drying step.

[0068] (5) Drying process The drying step is a step for drying the polyvinyl alcohol-based resin film after the crosslinking step or the cleaning step, and the polyvinyl alcohol-based resin film after the crosslinking step or the cleaning step can be subjected to a drying treatment, thereby obtaining a polarizer.

[0069] The drying treatment is carried out using a film drying means (heating means). A suitable example of the drying means is a drying oven. The drying oven is preferably capable of controlling the temperature inside the oven. The drying oven is, for example, a hot air oven capable of increasing the temperature inside the oven by supplying hot air or the like. The drying treatment by the drying means may be a treatment in which the polyvinyl alcohol-based resin film after the crosslinking step or the washing step is adhered to one or more heating bodies having a convex curved surface, or a treatment in which the film is heated using a heater.

[0070] The heating body may be a roll (such as a guide roll that also functions as a heating roll) that has a heat source (such as a heat medium such as hot water or an infrared heater) inside and can increase the surface temperature. Examples of the heater may include an infrared heater, a halogen heater, a panel heater, etc.

[0071] The temperature of the drying treatment (for example, the temperature inside the drying oven, the surface temperature of the heat roll, etc.) is usually 30° C. or more and 100° C. or less, and preferably 50° C. or more and 90° C. or less. The drying time is not particularly limited, but is, for example, 30 seconds or more and 600 seconds or less.

[0072] Through the above steps, a polarizer in which a dichroic dye is adsorbed and oriented on a uniaxially stretched polyvinyl alcohol-based resin film can be obtained.

[0073] <Polarizing plate> 1, a polarizing plate 100 according to one embodiment of the present invention includes the above-mentioned polarizer 102, a first protective film 101 provided on one surface of the polarizer, and a second protective film 103 provided on the other surface of the polarizing plate. The polarizing plate does not necessarily have to include the second protective film 103.

[0074] The first and second protective films may be transparent resin films made of thermoplastic resins, for example, polyolefin resins such as linear polyolefin resins (polypropylene resins, etc.) and cyclic polyolefin resins (norbornene resins, etc.); cellulose ester resins such as triacetyl cellulose and diacetyl cellulose; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate resins; (meth)acrylic resins such as polymethyl methacrylate resins; or mixtures, copolymers, etc. of these. The first and second protective films may be made of the same material or different materials.

[0075] Either or both of the first and second protective films may be a protective film having optical functions such as a retardation film, a brightness enhancing film, etc. For example, a retardation film having an arbitrary retardation value can be obtained by stretching (uniaxially or biaxially stretching, etc.) a transparent resin film made of the above-mentioned material, or by forming a liquid crystal layer or the like on the film.

[0076] A surface treatment layer (coating layer) such as a hard coat layer, an antiglare layer, an antireflection layer, an antistatic layer, or an antifouling layer may be formed on the surface of the first protective film 101 and / or the second protective film 103 opposite the polarizer 102.

[0077] The thickness of the first and second protective films is preferably thin from the viewpoint of making the polarizing plate 100 thinner, but if the film is too thin, the strength decreases and the processability tends to be poor, so the thickness is preferably 5 to 150 μm, more preferably 5 to 100 μm, and even more preferably 10 to 50 μm.

[0078] The polarizing plate 100 can be obtained by laminating (stacking) the first protective film 101 and the second protective film 103 on both sides of the polarizer 102 via an adhesive. Examples of adhesives used for laminating the polarizer and the protective films include active energy ray curable adhesives such as ultraviolet curable adhesives, aqueous solutions of polyvinyl alcohol resins or aqueous solutions containing a crosslinking agent, and water-based adhesives such as urethane emulsion adhesives. When the protective films are laminated on both sides of the polarizer 102, the adhesives forming the two adhesive layers may be the same or different. For example, when the protective films are laminated on both sides of the polarizer, one side may be laminated using an aqueous adhesive, and the other side may be laminated using an active energy ray curable adhesive. The ultraviolet curable adhesive may be a mixture of a radically polymerizable (meth)acrylic compound and a photoradical polymerization initiator, a mixture of a cationic polymerizable epoxy compound and a photocationic polymerization initiator, or the like. It is also possible to use a cationically polymerizable epoxy compound and a radically polymerizable (meth)acrylic compound in combination, and to use a photocationic polymerization initiator and a photoradical polymerization initiator in combination as initiators.

[0079] When an active energy ray curable adhesive is used, the adhesive is cured by irradiating it with active energy rays after lamination. The light source of the active energy rays is not particularly limited, but active energy rays (ultraviolet rays) having an emission distribution of wavelengths of 400 nm or less are preferred, and specifically, low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, chemical lamps, black light lamps, microwave excited mercury lamps, metal halide lamps, etc. are preferably used.

[0080] In order to improve the adhesion between the polarizer and the protective film, prior to bonding of the polarizer and the thermoplastic resin film, the bonding surfaces of the polarizer and / or the protective film may be subjected to surface treatment such as corona treatment, flame treatment, plasma treatment, ultraviolet irradiation treatment, primer coating treatment, and saponification treatment.

[0081] When protective films are laminated on both sides of the polarizer 102, the method further includes a second laminating step of laminating a second protective film to the polarizer surface of the polarizing plate with a first protective film on one side using an adhesive.

[0082] (Application) The polarizing plate can be used in a display device. The display device may be any type such as a liquid crystal display device or an organic EL display device, but is preferably a liquid crystal display device. The liquid crystal display device includes a liquid crystal panel having a liquid crystal cell as an image display element, and a backlight. In constructing a liquid crystal display device, the polarizing plate may be used as a polarizing plate disposed on the viewing side, may be used as a polarizing plate disposed on the backlight side, or may be used as a polarizing plate on both the viewing side and the backlight side.

[0083] In particular, the polarizing plate is suitable for an in-vehicle display device. For example, in an in-vehicle display device, the polarizing plate is attached to an image display cell with a pressure-sensitive adhesive or adhesive, and a light-transmitting member such as a glass plate or a touch panel is attached to the opposite side of the surface attached to the image display cell with a pressure-sensitive adhesive or adhesive. The polarizing plate of the in-vehicle display device may be used for a long time under relatively high temperatures, and yellowing tends to occur easily in such cases, so the polarizer according to the present embodiment is highly effective.

[0084] The polarizing plate is suitable for an in-vehicle display device including, in this order, a polarizing plate, a light-transmitting member disposed on the first protective film side of the polarizing plate, and a display device disposed on the second protective film side of the polarizing plate. The light-transmitting member may be a glass plate, a light-transmitting resin film, or the like.

[0085] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples. EXAMPLES

[0086] <Example 1> (Manufacture of polarizers) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in 30° C. water (deionized water) for 86 seconds to cause swelling, and then dyed by immersing for 160 seconds in an aqueous solution of iodine / potassium iodide / water with a mass ratio of 1.0 / 2.0 / 7.0 and a dyeing solution of boric acid / water with a mass ratio of 0.4 / 2.0 / 97.6 at a temperature of 30° C. Here, the film was stretched at stretch ratios of 2.00 times and 1.51 times at the swelling and dyeing stages, respectively, and stretching was continued so that the cumulative stretch ratio up to the dyeing tank was 3.02 times.

[0087] Next, the film was immersed in a crosslinking solution (crosslinking step) heated to 60°C for 76 seconds to crosslink the film while being stretched at a stretch ratio of 1.86 times.

[0088] Furthermore, the film was immersed in a crosslinking solution (a 2.6 / 4.4 / 2.3 / 2.7 / 88.0 mass ratio aqueous solution of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water) heated to 45°C for 12 seconds (complementary color stage) for crosslinking, and stretched 1.04 times. At this time, the total cumulative stretch ratio of the swelling, dyeing, crosslinking, and complementary color stages was set to 5.83 times.

[0089] After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60°C for 200 seconds to produce a polarizer. The thickness of the polarizer was about 20 μm. The value of the area S of the parameter S was 39.8h.

[0090] <Example 2> (Manufacture of polarizers) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) having a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in 30° C. water (deionized water) for 86 seconds to cause it to swell, and then dyed by immersing for 160 seconds in an aqueous solution of iodine / potassium iodide / water with a mass ratio of 1.0 / 2.0 / 7.0 and a dyeing solution of boric acid / water with a mass ratio of 0.4 / 2.0 / 97.6 at a temperature of 30° C. Here, the film was stretched at stretch ratios of 2.00 times and 1.51 times at the swelling and dyeing stages, respectively, and stretching was continued so that the cumulative stretch ratio up to the dyeing tank was 3.02 times.

[0091] Next, the film was immersed in a crosslinking solution (crosslinking step) heated to 60°C for 76 seconds to crosslink the film while being stretched at a stretch ratio of 1.86 times.

[0092] Furthermore, the film was immersed in a crosslinking solution (a 2.9 / 5.0 / 4.8 / 6.2 / 100 mass ratio aqueous solution of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water) heated to 45°C for 12 seconds (complementary color stage) for crosslinking and stretched 1.04 times, so that the total cumulative stretch ratio in the swelling, dyeing, crosslinking, and complementary color stages was 5.83 times.

[0093] After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60° C. for 200 seconds to prepare a polarizer. The thickness of the polarizer was about 20 μm.

[0094] <Comparative Example 1> (Manufacture of polarizers) A transparent unstretched polyvinyl alcohol film (TS4500, manufactured by Kuraray Co., Ltd.) with a thickness of 45 μm and a saponification degree of 99.9% or more was immersed in 30° C. water (deionized water) for 86 seconds to cause swelling, and then dyed by immersing for 160 seconds in an aqueous solution of iodine / potassium iodide / water with a weight ratio of 1.0 / 2.0 / 7.0 and a dyeing solution of boric acid / water with a mass ratio of 0.4 / 2.0 / 97.6 at a temperature of 30° C. Here, the film was stretched at a stretch ratio of 2.00 times and 1.51 times at the swelling and dyeing stages, respectively, and stretching was continued so that the cumulative stretch ratio up to the dyeing tank was 3.02 times.

[0095] Next, the film was immersed in a crosslinking solution (crosslinking step) heated to 60°C for 76 seconds to crosslink the film, while being stretched at a stretch ratio of 1.86 times.

[0096] Furthermore, the film was immersed in a crosslinking solution (a 2.7 / 4.6 / 1.1 / 91.6 mass ratio aqueous solution of potassium iodide / boric acid / zinc chloride / water) heated to 45°C for 12 seconds (complementary color stage) for crosslinking and stretched 1.04 times. At this time, the total cumulative stretching ratio in the swelling, dyeing, crosslinking, and complementary color stages was set to 5.83 times.

[0097] After the crosslinking was completed, the polyvinyl alcohol film stretched 5.83 times was dried in an oven at 60° C. for 200 seconds to prepare a polarizer. The thickness of the polarizer was about 20 μm.

[0098] [Curve Fitting] From the results of the durability test for Single Δab evaluation described below, the coefficients a to e were calculated based on the data of the combination of time and absorbance and the function f(t) using the Generalized Reduced Gradient method in the solver of Excel 2016. The initial values ​​of the coefficients a to e in the formula (A) were set to 0. As a result of curve fitting, the coefficients a to e obtained from the polarizer obtained in Example 1 were: coefficient a=1.1, coefficient b=0.36, coefficient c=0.40, coefficient d=0.0084, and coefficient e=0.21. The coefficients a to e obtained from the polarizer obtained in Example 2 were: coefficient a=1.0, coefficient b=0.36, coefficient c=0.39, coefficient d=0.0075, and coefficient e=0.22. The coefficients a to e obtained from the polarizer obtained in Comparative Example 1 were: coefficient a=0.51, coefficient b=0.0094, coefficient c=1.1, coefficient d=0.31, and coefficient e=0.32.

[0099] The coefficients a to e obtained from the fitting curve were substituted into the function f(t), and the area S was obtained by integrating t = 0 to 72 hours in the function f(t). Regarding the area S obtained by the above method, in Example 1 it was 39.8 [h], in Example 2 it was 40.7 [h], and in Comparative Example 1 it was 53.0 [h].

[0100] [Durability Test for Yellow Index Evaluation] The polarizers of the examples and comparative examples were cut to 30 mm in the MD direction (polarizer absorption axis direction) and 25 mm in the TD direction (polarizer transmission axis direction). The polarizers were sandwiched between two metal plates with a length of 40 mm, a width of 40 mm, and a thickness of 2 mm, and having a 20 mm diameter hole in the center, and the four sides were fixed with Kapton tape.

[0101] The evaluation samples fixed to the metal plates were placed upright in a heating oven at 115 °C, taken out after 500 Hr elapsed, and evaluated.

[0102] [Evaluation of Yellow Index] Using a spectrophotometer (manufactured by Hitachi, Ltd., U4100), in accordance with JIS K 7373 (2006), the initial yellow index of the polarizer sample before the durability test was measured. Next, similarly for the sample after the durability test, using a spectrophotometer (manufactured by Hitachi, Ltd., U4100), in accordance with JIS K 7373 (2006), the yellow index was obtained.

[0103] Based on the obtained yellow index, the difference ΔYI in the yellow index before and after the durability test was calculated by the following formula.

[0104] ΔYI = (Yellow Index after Durability Test) - (Initial Yellow Index) When the difference in the obtained yellow index was less than 30 at the time of 115 °C and 500 Hr elapsed, it was evaluated as good, and when it was 30 or more, it was evaluated as bad.

[0105] [Durability Test for Single Δab Evaluation] An evaluation sample was prepared by cutting a polarizer to a size of 50 mm × 40 mm so that the absorption axis of the polarizer was parallel to the long side. For the evaluation sample thus obtained, spectral measurement before the durability test was performed using a spectrophotometer U-4100 manufactured by Hitachi High-Technologies Corporation (measurement wavelength: 280 to 900 nm). Thereafter, the single transmittance of the same sample was measured at regular intervals in an environment of 115°C, and the hue (a, b) was determined. The measurement times were after 24 h, 48 h, 120 h, 240 h, and 500 h of the durability test. SingleΔab was calculated using the following formula, and this was used as an evaluation of the hue change.

[0106] SingleΔab = √{(a after durability test - a before durability test) 2 + (b after durability test - b before durability test) 2}

[0107] [Change in SingleΔab between 240 h and 500 h] Based on the results of the <SingleΔab evaluation durability test>, the steep change in SingleΔab between 240 h and 500 h was calculated using the following formula.

[0108] Steep change in SingleΔab between 240 h and 500 h = SΔab at 500 h elapsed - SΔab at 240 h elapsed

[0109] [Measurement of the thickness of the polarizer] Measurement was performed using a digital micrometer “MH-15M” manufactured by Nikon Corporation.

[0110] Table 1 shows the characteristics of the obtained polarizer. Figure 2 shows the combination of absorbance and time obtained in Example 1 and Comparative Example 1, and f(t) with coefficients a to e substituted. The black circles are the data of Example 1, the solid line is the regression curve of Example 1, the Xs are the data of Comparative Example 1, and the dotted line is the regression curve of Comparative Example 1.

[0111]

Table 1

[0112] <Example 3> A polarizer was produced in the same manner as in Example 1, except that the dyeing solution was an aqueous solution having an iodine / potassium iodide / water mass ratio of 1.0 / 2.0 / 7.0 and a boric acid / water mass ratio of 0.4 / 2.8 / 96.8, the crosslinking solution was an aqueous solution having a potassium iodide / boric acid / zinc sulfate / potassium sulfate / water mass ratio of 2.4 / 5.5 / 2.4 / 2.6 / 100 and a temperature of 66° C., and the complementary liquid was an aqueous solution having a potassium iodide / boric acid / zinc sulfate / potassium sulfate / water mass ratio of 2.5 / 6.1 / 2.5 / 2.7 / 100 and a temperature of 47° C. The polarizer had a thickness of about 20 μm.

[0113] <Example 4> A polarizer was produced in the same manner as in Example 1, except that the dyeing solution was an aqueous solution of iodine / potassium iodide / water with a mass ratio of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid and water of 0.2 / 2.0 / 97.8, the temperature of the crosslinking solution in the crosslinking stage was 62° C., and the temperature of the solution in the complementary color stage was 47° C. The polarizer had a thickness of about 20 μm.

[0114] <Example 5> A polarizer was produced in the same manner as in Example 1, except that the dyeing solution was an aqueous solution of iodine / potassium iodide / water with a mass ratio of 1.0 / 2.0 / 7.0 and a mass ratio of boric acid and water of 0.3 / 2.0 / 97.7, the temperature of the crosslinking solution in the crosslinking stage was 64° C., and the temperature of the solution in the complementary color stage was 47° C. The polarizer had a thickness of about 20 μm.

[0115] <Example 6> A polarizer was produced in the same manner as in Example 1, except that the crosslinking liquid was a solution with a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 5.4 / 3.9 / 2.4 / 2.6 / 100, the complementary liquid was an aqueous solution with a mass ratio of potassium iodide / boric acid / zinc sulfate / potassium sulfate / water of 5.5 / 4.3 / 2.4 / 2.6 / 100, the temperature of the crosslinking liquid in the crosslinking stage was 62° C., and the temperature of the liquid in the complementary stage was 47° C. The polarizer had a thickness of about 20 μm.

[0116] [Curve Fitting] From the results of the durability test for Single Δab evaluation described below, the coefficients a to e were calculated based on the data of the combination of time and absorbance and the function f(t) using the Generalized Reduced Gradient method in the solver of Excel 2016. The initial values ​​of the coefficients a to e in the formula (A) were set to 0. As a result of curve fitting, the coefficients a to e obtained from the polarizer obtained in Example 3 were: coefficient a=1.1, coefficient b=0.42, coefficient c=0.24, coefficient d=0.013, and coefficient e=0.14. The coefficients a to e obtained from the polarizer obtained in Example 4 were: coefficient a = 0.71, coefficient b = 0.37, coefficient c = 0.18, coefficient d = 0.012, and coefficient e = 0.12. The coefficients a to e obtained from the polarizer obtained in Example 5 were: coefficient a = 1.03, coefficient b = 0.41, coefficient c = 0.28, coefficient d = 0.01, and coefficient e = 0.15. The coefficients a to e obtained from the polarizer obtained in Example 6 were: coefficient a = 0.87, coefficient b = 0.37, coefficient c = 0.21, coefficient d = 0.01, and coefficient e = 0.13.

[0117] The coefficients a to e obtained from the fitting curve were substituted into the function f(t), and the area S was determined by integrating the time period t=0 to 72 in the function f(t). Regarding the area S calculated by the above method, the area S was 24.1 [h] in Example 3, 18.9 [h] in Example 4, 27.2 [h] in Example 5, and 22.3 [h] in Example 6.

[0118] [Durability test for yellow index evaluation] The polarizers of the Examples and Comparative Examples were cut to a length of 30 mm in the MD direction (polarizer absorption axis direction) and 25 mm in the TD direction (polarizer transmission axis direction). The polarizer was sandwiched between two metal plates measuring 40 mm in length, 40 mm in width, and 2 mm in thickness with a hole of 20 mm in diameter in the center, and the four sides were fixed with Kapton tape.

[0119] The evaluation sample fixed to the metal plate was placed in a heating oven at 115°C and taken out after 500 hours for evaluation.

[0120] [Evaluation of Yellow Index] Using a spectrophotometer (U4100, manufactured by Hitachi, Ltd.), in accordance with JIS K 7373 (2006), the initial yellow index of the polarizer sample before the durability test was measured. Next, similarly for the sample after the durability test, using a spectrophotometer (U4100, manufactured by Hitachi, Ltd.), in accordance with JIS K 7373 (2006), the yellow index was determined.

[0121] Based on the obtained yellow index, the difference ΔYI in the yellow index before and after the durability test was calculated by the following formula.

[0122] ΔYI = (Yellow index after durability test) - (Initial yellow index) When the obtained difference in the yellow index was less than 30 at 115°C after 500 hours, it was evaluated as good, and when it was 30 or more, it was evaluated as bad.

[0123] <Durability Test for Single Δab Evaluation> The evaluation sample was prepared by cutting it to a size of 50 mm × 40 mm so that the absorption axis of the polarizer was parallel to the long side. For the evaluation sample obtained in this way, spectral measurement before the durability test was performed using a spectrophotometer U - 4100 manufactured by Hitachi High - Technologies Corporation (measurement wavelength: 280 - 900 nm). Then, for the same sample in an environment at 115°C, the single - body transmittance was measured at regular intervals, and the hue (a, b) was determined. The measurement times were after 24 hours, 48 hours, 120 hours, 240 hours, and 500 hours of the durability test. Single Δab was calculated using the following formula.

[0124] Single Δab = √{(a after durability test - a before durability test) 2 +(b after durability test - b before durability test) 2}

[0125] [Change of SingleΔab between 240h and 500h] Based on the results of the <SingleΔab evaluation durability test>, the steep change of SingleΔab between 240h and 500h was calculated using the following formula.

[0126] Steep change of SingleΔab between 240h and 500h = SΔab at 500h elapsed - SΔab at 240h elapsed

[0127] Table 2 shows the characteristics of the polarizers of Examples 3 - 6.

[0128]

Table 2

Explanation of symbols

[0129] 100…Polarizing plate, 101…First protective film, 102…Polarizer, 103…Second protective film.

Claims

1. A polarizer formed from a polyvinyl alcohol-based resin film, A polarizer in which an area S[h] obtained by integrating the following function f(t) regarding absorbance into which coefficients a to e obtained by the following steps (1) and (2) are substituted over a period of t = 0 to 72 hours satisfies 0.1 h or more and 45 h or less. Procedure (1): The polarizer is exposed to an environment of 115° C., and the absorbance at 780 nm of the pair of polarizers in crossed Nicols is measured at 0 hours, 24 hours, 48 ​​hours, 120 hours, 240 hours, and 500 hours. Step (2): Based on the seven combinations of time and absorbance obtained in step (1) and the following function f(t) related to absorbance, curve fitting is performed by the least squares method to determine coefficients a to e. f(t)=a・Exp(-b・t)+c・Exp(-d・t)+e t: time [h] a to e: Coefficients

2. A polarizing plate comprising the polarizer according to claim 1 , an adhesive layer, and a protective film in this order.

Citation Information

Patent Citations

  • Polarizer and manufacturing method therefor

    JP2020071241A