Method for separation and recovery of zinc
By adjusting the redox potential and pH in the zinc-containing dust slurry to form magnetite or hematite, the method effectively separates and recovers zinc with high purity and minimal chemical use, addressing the inefficiencies of previous zinc separation techniques.
Patent Information
- Application Number
- JP2024007484
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-01-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-01-22
AI Technical Summary
Existing methods for separating zinc from zinc-containing dust in steelmaking processes result in significant iron leaching, leading to reduced zinc purity and increased chemical consumption due to the solubility of metallic iron and wustite in acidic conditions, which complicates the recycling process.
A method involving redox potential adjustment using oxidizing agents to convert iron on the dust surface to magnetite or hematite, followed by controlled pH adjustments for zinc leaching and precipitation, minimizing iron leaching and maximizing zinc recovery with reduced chemical use.
The method achieves selective zinc separation with high purity and reduced chemical consumption, enhancing the economic viability of zinc recovery from zinc-containing dust.
Smart Images

Figure 2024147488000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for separating and recovering zinc. [Background technology]
[0002] Zinc-containing dust generated from steelmaking furnaces such as converters, hot metal pretreatment furnaces, and electric furnaces contains a large amount of iron dust, making it a promising recycling source for the steelmaking process. However, if all of the zinc-containing dust is recycled, the zinc continues to circulate within the steelworks, and the amount of zinc derived from the raw materials accumulates. If the amount of accumulation becomes excessive, it can cause operational problems in the blast furnace. Therefore, when recycling zinc-containing dust, it is necessary to separate the zinc beforehand.
[0003] Patent Document 1 proposes a technique for separating zinc from zinc-containing dust, in which zinc-containing steelmaking dust is brought into contact with and mixed with water in a reaction vessel while air is blown in and agitated, the hydrogen ion concentration of the water is adjusted to a pH of 3 to 6 to allow the zinc in the dust to leach into the solution, the water in which the zinc has been dissolved is separated from the iron-containing dust, and the hydrogen ion concentration of the water in which the zinc has been dissolved is subsequently adjusted to a pH of 7 to 9 to separate the zinc by precipitating it. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2000-309831 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method described in Patent Document 1, most of the iron in the zinc-containing dust is in the form of metallic iron or wustite, which is easily soluble in acid, and the hydrogen ion concentration of the water is reduced to the acidic side. Therefore, about 2 to 4% of iron, which is the main component of the dust, is leached into the solution, and hydrogen ions in the water are consumed by the leaching of iron, so the amount of acid added to control the hydrogen ion concentration of the water is significantly increased. In addition, when zinc is precipitated and separated, the iron that was leached into the solution is also precipitated, which has the disadvantage of significantly reducing the purity of the recovered zinc.
[0006] The present invention has been developed in view of the above circumstances, and an object of the present invention is to provide a method for separating zinc from zinc-containing dust with high selectivity using a small amount of chemicals. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have repeatedly studied a method for separating zinc with good selectivity while reducing the amount of chemicals. As a result, they have come up with a technology that can improve zinc separation ability while suppressing the amount of acid consumed for dissolving iron by increasing the oxidation-reduction potential of a zinc-containing dust slurry containing zinc-containing dust in advance to oxidize the iron on the dust surface to magnetite or hematite, which is insoluble in acid. The gist of the technology is as follows.
[0008] [1] A method for separating and recovering zinc from zinc-containing dust containing zinc dust and iron dust, comprising: an oxidation-reduction potential adjusting step of adjusting an oxidation-reduction potential by adding an oxidizing agent to the zinc-containing dust slurry containing the zinc-containing dust; a zinc leaching step of adjusting the pH of the adjusted zinc-containing dust slurry whose oxidation-reduction potential has been adjusted in the oxidation-reduction potential adjustment step to leach zinc, thereby obtaining a zinc leaching solution and a zinc leaching residue; a first solid-liquid separation step of separating the zinc leaching solution and the zinc leaching residue into solid-liquid; a zinc precipitation step of adjusting the pH of the separated zinc leachate to precipitate zinc as a zinc precipitate; a second solid-liquid separation step of separating the pH-adjusted zinc leachate into the zinc precipitate and a filtrate, and recovering the separated zinc precipitate; The method for separating and recovering zinc comprises the steps of:
[0009] [2] The method for separating and recovering zinc described in [1], wherein in the oxidation-reduction potential adjustment step, the oxidation-reduction potential of the zinc-containing dust slurry is adjusted to an oxidation-reduction potential that causes hematite to form on the surface of the iron dust.
[0010] [3] The method for separating and recovering zinc described in [2], wherein in the oxidation-reduction potential adjustment step, the oxidation-reduction potential of the zinc-containing dust slurry is adjusted to 280 mV or more.
[0011] [4] The method for separating and recovering zinc according to any one of [1] to [3], wherein in the zinc leaching step, the pH of the adjusted zinc-containing dust slurry is adjusted to 3 or more and 5 or less.
[0012] [5] The method for separating and recovering zinc according to any one of [1] to [4] above, wherein in the zinc precipitation step, the pH of the zinc leachate is adjusted to 8 or more and 11 or less.
[0013] [6] The method for separating and recovering zinc according to any one of the above [1] to [5], wherein the zinc-containing dust is iron-making dust generated in an iron-making process.
[0014] [7] The method for separating and recovering zinc according to any one of the above [1] to [6], wherein the zinc-containing dust is steelmaking dust generated in a steelmaking process. Effect of the Invention
[0015] According to the present invention, zinc in zinc-containing dust can be separated with good selectivity using a small amount of chemical agent. [Brief description of the drawings]
[0016] [Figure 1] 1 is a flowchart of a method for separating and recovering zinc according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiment of the present invention will be described with reference to the drawings. The zinc separation method according to the present invention is a method for separating and recovering zinc from zinc-containing dust containing zinc dust and iron dust, and includes an oxidation-reduction potential adjustment step of adding an oxidizing agent to a zinc-containing dust slurry containing zinc-containing dust to adjust the oxidation-reduction potential, a zinc leaching step of adjusting the pH of the adjusted zinc-containing dust slurry whose oxidation-reduction potential has been adjusted in the oxidation-reduction potential adjustment step to leach zinc, and obtain a zinc leaching solution and a zinc leaching residue, a first solid-liquid separation step of separating the zinc leaching solution and the zinc leaching residue into a solid-liquid state, a zinc precipitation step of adjusting the pH of the separated zinc leaching solution to precipitate zinc as a zinc precipitate, and a second solid-liquid separation step of separating the zinc leaching solution whose pH has been adjusted into a zinc precipitate and a filtrate, and recovering the separated zinc precipitate.
[0018] <Oxidation-reduction potential adjustment process> 1 shows a flow chart of the zinc separation and recovery method according to the present invention. First, in step S1, an oxidizing agent is added to a zinc-containing dust slurry containing zinc-containing dust to adjust the oxidation-reduction potential (oxidation-reduction potential adjustment step).
[0019] The zinc-containing dust to be treated includes zinc dust and iron dust. Examples of the zinc-containing dust include iron-making dust such as blast furnace dust and rotary hearth reduction furnace (RHF) dust, and steel-making dust such as converter dust and electric furnace dust. As the zinc-containing dust, one or a combination of the above dusts can be used.
[0020] In this process, the redox potential of the zinc-containing dust slurry is adjusted by adding an oxidizing agent. More specifically, the redox potential of the zinc-containing dust slurry is increased. As the oxidizing agent to be added for this purpose, any of hydrogen peroxide, hypochlorous acid, ozone, air, etc. can be used, but hydrogen peroxide and air are preferred from the viewpoint of ease of handling and wastewater treatment.
[0021] The oxidation-reduction potential of the zinc-containing dust slurry is preferably adjusted to an oxidation-reduction potential that allows hematite to be formed on the surface of the iron dust. Specifically, when the pH is about 8 to 11, the oxidation-reduction potential of the zinc-containing dust slurry is preferably set to -300 mV or more, at which the form of magnetite or hematite is predominant. This makes it easier to suppress the leaching of iron into the zinc-containing dust slurry. It is more preferable to increase the oxidation-reduction potential of the zinc-containing dust slurry to 280 mV or more. This allows magnetite or hematite to be stably formed on the dust surface.
[0022] If acid is added in the subsequent zinc leaching process without increasing the redox potential of the water, the iron remaining on the dust surface, derived from iron compounds that are easily soluble in acid, such as metallic iron and wustite, will also be leached out along with the zinc. Furthermore, zinc-containing dust is characterized by being mostly composed of fine particles of 100 μm or less, and the specific surface area of iron compounds that are easily soluble in acid, such as metallic iron and wustite, is also large. Therefore, when acid is added to zinc-containing dust, the surface area of the newly exposed iron compounds that are easily soluble in acid due to the leaching of iron is also large, and the leaching of iron and the surface generation of iron compounds that are easily soluble in acid continue in a chain reaction. Therefore, if acid is added even a little earlier, even if the redox potential is increased later, (1) the control of the dust surface to a sparingly soluble iron compound form and (2) the surface generation of iron compounds that are easily soluble in acid will compete with each other, making it difficult to suppress the leaching of iron by turning the entire dust surface into magnetite or hematite. This not only results in the consumption of extra chemicals for leaching iron and controlling the form of iron compounds on the dust surface, but also significantly reduces the degree of zinc enrichment in the zinc-enriched residue compared to the initial dust in the subsequent zinc precipitation process, reducing its value as a zinc raw material due to iron contamination, making it uneconomical.
[0023] <Zinc leaching process> Next, in step S2, the pH of the adjusted zinc-containing dust slurry whose oxidation-reduction potential has been adjusted in the oxidation-reduction potential adjustment step is adjusted to leach zinc, thereby obtaining a zinc leachate and a zinc leach residue (zinc leaching step).
[0024] The pH of the adjusted zinc-containing dust slurry can be adjusted by adding an acid to the adjusted zinc-containing dust slurry. The acid to be added can be any of inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as citric acid and butyric acid. Among them, it is preferable to use sulfuric acid as the acid from the viewpoint of cost and wastewater treatment.
[0025] In this step, it is preferable to adjust the pH of the adjusted zinc-containing dust slurry to 3 or more and 5 or less. By adjusting the pH of the adjusted zinc-containing dust slurry to 3 or more, it is possible to suppress the leaching of iron into the slurry regardless of the form of the compound. In addition, by adjusting the pH of the adjusted zinc-containing dust slurry to 5 or less, it is possible to increase the leaching rate of zinc.
[0026] The reaction time after the acid is added to the adjusted zinc-containing dust slurry is preferably 20 minutes or more and 120 minutes or less from the viewpoint of the zinc leaching rate and treatment efficiency.
[0027] <First solid-liquid separation step> Subsequently, in step S3, solid-liquid separation is performed into the zinc leaching solution obtained in the zinc leaching step and a zinc leaching residue (first solid-liquid separation step).
[0028] The solid-liquid separation can be carried out by any commonly used method, such as filtration, filter press, centrifugation, or gravity settling.
[0029] <Zinc precipitation process> Thereafter, in step S4, the pH of the separated zinc leachate is adjusted to precipitate zinc as a zinc precipitate (zinc precipitation step).
[0030] The pH of the zinc leaching solution can be adjusted by adding an alkali to the zinc leaching solution. The alkali to be added can be any common alkali, such as sodium hydroxide, calcium hydroxide, or potassium hydroxide. Since zinc is an amphoteric element and dissolves in both strong acids and strong alkalis, it is preferable to adjust the pH of the zinc leaching solution to 8 or more and 10 or less. This minimizes the solubility of zinc, allowing zinc to be precipitated and separated at a high precipitation rate, and increasing the zinc recovery rate.
[0031] <Second solid-liquid separation step> Then, in step S5, the zinc leachate whose pH has been adjusted in the zinc precipitation step is subjected to solid-liquid separation into a zinc precipitate and a filtrate, and the separated zinc precipitate is collected (second solid-liquid separation step).
[0032] In this step, the zinc precipitate is separated into a zinc precipitate and a filtrate from which zinc ions have been precipitated and removed, and the zinc precipitate is recovered. As for the method of the solid-liquid separation, as in the first solid-liquid separation step, any general method such as filtration, filter press, centrifugation, gravity sedimentation, etc. can be selected. EXAMPLES
[0033] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0034] (Examples 1 to 5) As the zinc-containing dust, converter dust with a zinc concentration of 1 to 2 mass% and an iron concentration of 60 to 70 mass% was prepared. 150 ml of distilled water was added to 30 g of each converter dust to prepare a converter dust slurry sample. Next, hydrogen peroxide was added to the converter dust slurry to increase the redox potential to more than 100 mV (redox potential adjustment step), and sulfuric acid was added to control the pH of the slurry at a constant state of 3 (invention examples 1, 2, 4, and 5), or 5 (invention example 3) for 1 hour (zinc leaching step). After 1 hour, the zinc leaching solution and zinc leaching residue were separated by filtration (first solid-liquid separation step), and sodium hydroxide was added to the obtained zinc leaching solution to control the pH of the zinc leaching solution at a constant state of 8 (invention example 4), 10 (invention examples 1 to 3), or 11 (invention example 5) for 1 hour (zinc precipitation step). After 1 hour, the zinc leaching solution whose pH had been adjusted by filtration was separated into zinc precipitate and filtrate (second solid-liquid separation step), and zinc precipitate was obtained. Details of each invention example are shown in Table 1. In addition, the zinc and iron concentrations of the converter dust in Table 1 were analyzed by inductively coupled plasma (ICP) atomic emission spectrometry. The pH of the slurry was controlled to be constant by a pH controller, and the oxidation-reduction potential of the slurry was measured by an ORP meter.
[0035] Comparative Example 1 Zinc was recovered from zinc-containing dust in the same manner as in Example 1. However, the oxidation-reduction potential adjustment step was not performed, and sulfuric acid was added to the converter dust slurry to reduce the pH of the slurry to 3 once, and then sulfuric acid and hydrogen peroxide were added to control the pH of the slurry at a constant state of 3 for 1 hour. All other conditions were the same as in Example 1.
[0036] Comparative Example 2 Zinc was recovered from zinc-containing dust in the same manner as in Example 1. However, in the zinc leaching process, the pH of the slurry was controlled to a constant value of 2 for one hour. All other conditions were the same as in Example 1.
[0037] Comparative Example 3 Zinc was recovered from zinc-containing dust in the same manner as in Example 1. However, in the zinc leaching process, the pH of the slurry was controlled to a constant value of 6 for one hour. All other conditions were the same as in Example 1.
[0038] Comparative Example 4 Zinc was recovered from zinc-containing dust in the same manner as in Example 1. However, in the zinc precipitation step, the pH of the slurry was controlled to a constant value of 7 for one hour. All other conditions were the same as in Example 1.
[0039] Comparative Example 5 Zinc was recovered from zinc-containing dust in the same manner as in Example 1. However, in the zinc precipitation step, the pH of the slurry was controlled to a constant value of 12 for one hour. All other conditions were the same as in Example 1.
[0040] [Table 1]
[0041] In Examples 1 to 5 of the present invention shown in Table 1, the amount of chemicals consumed is smaller than that in Comparative Example 1, and the degree of zinc concentration in the zinc precipitate relative to the initial converter dust (i.e., the zinc content in the zinc precipitate relative to the zinc content in the initial converter dust) is higher. In particular, the difference is remarkable in Examples 2 to 5 of the present invention, in which the oxidation-reduction potential of the water before the addition of sulfuric acid is 280 mV or more. In Comparative Example 1, since the addition of sulfuric acid was performed when the oxidation-reduction potential of the slurry was low, some iron was also leached and sulfuric acid was excessively consumed. In addition, since the iron leached when sodium hydroxide was added in the zinc precipitation step precipitated together with zinc, sodium hydroxide was excessively consumed, and it is considered that the degree of zinc concentration in the zinc precipitate relative to the initial converter dust was also low.
[0042] In addition, in the invention examples 1 to 5 shown in Table 1, the zinc concentration of the zinc precipitate with respect to the initial converter dust is higher than that in the comparative examples 2 to 5. In the comparative example 2, the pH of the slurry after the addition of sulfuric acid was as low as 2, so that iron was partially leached, and the leached iron precipitated together with zinc when sodium hydroxide was added, so that sulfuric acid was consumed excessively. In addition, it is considered that sodium hydroxide was consumed excessively in the zinc precipitation step, so that the zinc concentration of the zinc precipitate with respect to the initial converter dust was also reduced. In the comparative example 3, the pH of the slurry after the addition of sulfuric acid was as high as 6, so that the zinc leaching rate was low, and it is also considered that the zinc concentration of the zinc precipitate with respect to the initial converter dust precipitated and recovered when sodium hydroxide was added was reduced. In the comparative example 4, the pH of the slurry when sodium hydroxide was added in the zinc precipitation step was as low as 7, so that some zinc remained in the liquid when sodium hydroxide was added, so that the zinc concentration of the zinc precipitate with respect to the initial converter dust precipitated and recovered was also reduced. In Comparative Example 5, since the pH of the slurry when sodium hydroxide was added in the zinc precipitation step was as high as 11, some zinc remained in the liquid when sodium hydroxide was added, and it is believed that the degree of zinc concentration in the zinc precipitate relative to the initial converter dust precipitated and recovered was also low. [Industrial Applicability]
[0043] According to the present invention, zinc in zinc-containing dust can be separated with high selectivity using a small amount of chemical agent.
Claims
1. A method for separating and recovering zinc from zinc-containing dust containing zinc dust and iron dust, comprising the steps of: an oxidation-reduction potential adjusting step of adjusting an oxidation-reduction potential by adding an oxidizing agent to the zinc-containing dust slurry containing the zinc-containing dust; a zinc leaching step of adjusting the pH of the adjusted zinc-containing dust slurry whose oxidation-reduction potential has been adjusted in the oxidation-reduction potential adjustment step to leach zinc, thereby obtaining a zinc leaching solution and a zinc leaching residue; a first solid-liquid separation step of separating the zinc leaching solution and the zinc leaching residue into solid-liquid; a zinc precipitation step of adjusting the pH of the separated zinc leachate to precipitate zinc as a zinc precipitate; a second solid-liquid separation step of separating the pH-adjusted zinc leachate into the zinc precipitate and a filtrate, and recovering the separated zinc precipitate; The method for separating and recovering zinc comprises the steps of:
2. 2. The method for separating and recovering zinc according to claim 1, wherein in the oxidation-reduction potential adjustment step, the oxidation-reduction potential of the zinc-containing dust slurry is adjusted to an oxidation-reduction potential that causes hematite to form on the surface of the iron dust.
3. 3. The method for separating and recovering zinc according to claim 2, wherein the oxidation-reduction potential of the zinc-containing dust slurry is adjusted to 280 mV or more in the oxidation-reduction potential adjustment step.
4. The zinc separation and recovery method according to any one of claims 1 to 3, wherein in the zinc leaching step, the pH of the adjusted zinc-containing dust slurry is adjusted to 3 or more and 5 or less.
5. The method for separating and recovering zinc according to any one of claims 1 to 3, wherein in the zinc precipitation step, the pH of the zinc leaching solution is adjusted to 8 or more and 11 or less.
6. The method for separating and recovering zinc according to any one of claims 1 to 3, wherein the zinc-containing dust is iron-making dust generated in an iron-making process.
7. The method for separating and recovering zinc according to any one of claims 1 to 3, wherein the zinc-containing dust is steelmaking dust generated in a steelmaking process.
Citation Information
Patent Citations
Method for recovering zinc from iron making dust
JP1987136535A
Method for recovering zinc
JP1990250928A
Method for removing zinc from steelmaking dust
JP2000309831A
Wet smelting method for nickel oxide ore
JP2014205901A
Method for reducing the amount of zinc (zn) and lead (pb) in materials containing iron (fe)
JP2017506700A
Cited By
Zinc recovery method
JP2025101724A
Zinc recovery method
JP7921264B2