Silicon single crystal manufacturing method and silicon single crystal manufacturing device

The silicon single crystal manufacturing method stabilizes convection mode and oxygen concentration using a controlled heating system with a cylindrical heater and magnetic field, addressing crucible damage and quality issues in the MCZ method.

JP2024147945AActive Publication Date: 2024-10-17SUMCO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023060710
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing silicon single crystal manufacturing methods using the MCZ method face challenges in controlling the convection mode of the silicon melt, leading to non-uniform melting of raw materials, potential damage to the crucible, and variations in oxygen concentration, which affect the quality and yield of silicon single crystals.

Method used

A silicon single crystal manufacturing method and apparatus that utilizes a cylindrical heater with semi-cylindrical first and second heat generating parts, controlled by separate power sources, allowing for uniform or non-uniform heating modes to stabilize the convection direction and oxygen concentration, using a magnetic field to fix the convection mode and prevent crucible damage.

Benefits of technology

The method stabilizes convection mode, reduces crucible damage, and minimizes oxygen concentration variations, enhancing the yield and quality of silicon single crystals while improving energy efficiency and reducing waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147945000001_ABST
    Figure 2024147945000001_ABST
Patent Text Reader

Abstract

To provide a silicon single crystal manufacturing method capable of restraining the occurrence of malfunction and a variation of an oxygen concentration per silicon single crystal during manufacture.SOLUTION: A silicon single crystal manufacturing method for pulling a silicon single crystal while applying a horizontal magnetic field to a silicon melt includes: a first heat manufacturing step for heating first and second heat evolution parts at the same heat evolution amount using a silicon single crystal manufacturing device comprising a crucible and a cylindrical heater surrounding the crucible, the heater comprising the first and second semi-cylindrical heat evolution parts having the same heat evolution characteristics, and being arranged so that heating amounts of first and second portions of the crucible respectively positioned on both sides to a vertical virtual plane including a central axis of the crucible and a central magnetic force line of the horizontal magnetic field are different from each other, when the first and second heat evolution parts generate heat at heat evolution amounts different from each other; and a second heat manufacturing step for heating the first and second heat evolution parts at the heat evolution amounts different from each other.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a silicon single crystal and an apparatus for producing a silicon single crystal. [Background technology]

[0002] As a method for producing silicon single crystals, the MCZ (magnetically coupled Czochralski) method, in which a horizontal magnetic field is applied to a silicon melt, is sometimes used. When a horizontal magnetic field is applied to a silicon melt using the MCZ method, the direction of convection in a virtual plane perpendicular to the direction of application of the horizontal magnetic field in the silicon melt may be clockwise (hereinafter, sometimes referred to as "right vortex mode") or counterclockwise (hereinafter, sometimes referred to as "left vortex mode").

[0003] Whether the convection mode is the right vortex mode or the left vortex mode is random, and the concentration of oxygen taken into the silicon single crystal varies depending on the convection mode and the environment inside the furnace. In order to obtain a silicon single crystal with a stable oxygen concentration, it is important to control the convection mode of the silicon melt during pulling. For this reason, various methods for controlling the convection mode of the silicon melt in the crucible have been studied (for example, see Patent Document 1).

[0004] Patent Document 1 discloses a method of fixing the convection mode to either the right vortex mode or the left vortex mode by making the thermal environment inside the furnace of a manufacturing apparatus asymmetrical with respect to the central axis of the crucible, thereby eliminating the variation in oxygen concentration caused by the convection mode. As a specific method, Patent Document 1 discloses a method in which the resistance value of a heater or the thickness of a heat insulating material is made different along the circumferential direction of the crucible. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-151502 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the method disclosed in Patent Document 1, a non-axisymmetric thermal environment is realized due to the internal furnace structure, and therefore the degree of non-axisymmetricity cannot be changed during the production of silicon single crystals. For this reason, for example, in the raw material melting process, the silicon raw material may melt non-uniformly in the circumferential direction of the crucible, and in this case, the solid silicon raw material floating in the silicon melt may tip over and come into strong contact with the quartz crucible, causing damage to the quartz crucible.

[0007] An object of the present invention is to provide a method and apparatus for producing silicon single crystals that can suppress the occurrence of defects during production and the variation in oxygen concentration among silicon single crystals. [Means for solving the problem]

[0008] The present invention provides a method for producing a silicon single crystal, which involves pulling up a silicon single crystal while applying a horizontal magnetic field to a silicon melt using a silicon single crystal production apparatus, the silicon single crystal production apparatus comprising: a crucible for accommodating the silicon melt; and a cylindrical heater surrounding the crucible, the heater comprising a semi-cylindrical first heating portion and a second heating portion each having the same heat generating characteristics, the first heating portion and the second heating portion being arranged such that when the first heating portion and the second heating portion generate heat at different amounts of heat, the first and second portions of the crucible located on either side of a vertical imaginary plane including a central axis of the crucible and a central magnetic field line of the horizontal magnetic field generate heat at different amounts of heat, and the silicon single crystal production method comprises: a first heating production step performed while the first heating portion and the second heating portion generate heat at the same amount of heat; and a second heating production step performed while the first heating portion and the second heating portion generate heat at different amounts of heat.

[0009] In the silicon single crystal manufacturing method of the present invention, it is preferable that the silicon single crystal manufacturing apparatus comprises a first power source and a second power source, a first power supply path that supplies power from the first power source to the first heating portion, and a second power supply path that supplies power from the second power source to the second heating portion, and that the first heating manufacturing process is performed while controlling the first power source and the second power source so that the first heating portion and the second heating portion generate heat with the same amount of heat, and that the second heating manufacturing process is performed while controlling the first power source and the second power source so that the first heating portion and the second heating portion generate heat with different amounts of heat.

[0010] In the silicon single crystal manufacturing method of the present invention, it is preferable that the silicon single crystal manufacturing apparatus includes a bypass supply path connecting the first power supply path and the second power supply path, and a rectifier unit provided in the bypass supply path for supplying power only in a direction from the first power supply path to the second power supply path, the first heating manufacturing process is performed while controlling the first power supply and the second power supply so as to supply power from the first power supply and not to supply power from the second power supply, and the second heating manufacturing process is performed while controlling the first power supply and the second power supply so as to supply power from the first power supply and the second power supply.

[0011] In the method for producing a silicon single crystal of the present invention, the method includes a silicon melt producing step of melting the silicon raw material in the crucible to produce the silicon melt, a magnetic field applying step of starting to apply the horizontal magnetic field to the silicon melt, a convection direction checking step of checking that the convection direction of the silicon melt in a virtual plane perpendicular to the central magnetic field line has been fixed in one direction, a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt, and a second growing step of growing a body portion and a tail portion by pulling up the seed crystal, and it is preferable that the silicon melt producing step and the second growing step are performed as the first heating production step, and the magnetic field applying step, the convection direction checking step, and the first growing step are performed as the second heating production step.

[0012] The method for producing a silicon single crystal of the present invention includes a silicon melt producing step of melting the silicon raw material in the crucible to produce the silicon melt, a magnetic field applying step of starting to apply the horizontal magnetic field to the silicon melt, a convection direction confirming step of confirming that the convection direction of the silicon melt in a virtual plane perpendicular to the central magnetic field line has been fixed in one direction, a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt, a reversal determining step, and a second growing step of growing a body portion and a tail portion by pulling up the seed crystal. It is preferable that the silicon melt generating process is performed as the first heating production process, the magnetic field application process, the convection direction confirmation process and the first growing process are performed as the second heating production process, and if it is determined in the reversal determination process that there is a possibility that the convection direction will be reversed when the second growing process is performed as the first heating production process based on the pulling conditions of the silicon single crystal, the second growing process is performed as the second heating production process, and if it is determined that there is no possibility that the convection direction will be reversed, the second growing process is performed as the first heating production process.

[0013] In the method for producing a silicon single crystal of the present invention, it is preferable that the first heating portion and the second heating portion are arranged, in a planar view, such that their maximum temperature regions are perpendicular to the vertical imaginary plane and overlap with a horizontal imaginary line including a central axis of the crucible.

[0014] The silicon single crystal manufacturing apparatus of the present invention comprises a crucible for containing the silicon melt, a cylindrical heater surrounding the crucible, and a power supply unit for supplying power to the heater, the heater comprising a first semi-cylindrical heating portion and a second heating portion each having the same heat generating characteristics, and the power supply unit comprises a first power source and a second power source, a first power supply path for supplying power from the first power source to the first heating portion, and a second power supply path for supplying power from the second power source to the second heating portion.

[0015] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the power supply unit includes a bypass supply path connecting the first power supply path and the second power supply path, and a rectifier unit provided in the bypass supply path for supplying power only in a direction from the first power supply path to the second power supply path.

[0016] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the apparatus further comprises a control unit for controlling the manufacturing process of pulling up the silicon single crystal, the manufacturing process comprising a first heating manufacturing process carried out while controlling the first power source and the second power source so that the first heating portion and the second heating portion generate heat at the same amount of heat, and a second heating manufacturing process carried out while controlling the first power source and the second power source so that the first heating portion and the second heating portion generate heat at different amounts of heat.

[0017] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that a control unit is provided for controlling the manufacturing process of pulling up the silicon single crystal, and the manufacturing process comprises a first heating manufacturing process performed while controlling the first power supply and the second power supply so as to supply power from the first power supply and not to supply power from the second power supply, and a second heating manufacturing process performed while controlling the first power supply and the second power supply so as to supply power from the first power supply and the second power supply.

[0018] In the silicon single crystal manufacturing apparatus of the present invention, the manufacturing process includes a silicon melt generating process of melting the silicon raw material in the crucible to generate the silicon melt, a magnetic field application process of starting to apply the horizontal magnetic field to the silicon melt, a convection direction confirmation process of confirming that the convection direction of the silicon melt in a virtual plane perpendicular to the central magnetic field line of the horizontal magnetic field has been fixed in one direction, a first growing process of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt, and a second growing process of growing a body portion and a tail portion by pulling up the seed crystal, and it is preferable that the control unit performs the silicon melt generating process and the second growing process as the first heating manufacturing process, and performs the magnetic field application process, the convection direction confirmation process, and the first growing process as the second heating manufacturing process.

[0019] In the silicon single crystal manufacturing apparatus of the present invention, the manufacturing process includes a silicon melt generating process of melting the silicon raw material in the crucible to generate the silicon melt, a magnetic field application process of starting to apply the horizontal magnetic field to the silicon melt, a convection direction confirmation process of confirming that the convection direction of the silicon melt in a virtual plane perpendicular to the central magnetic field line of the horizontal magnetic field has been fixed in one direction, a first growing process of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt, a reversal determination process, and a second growing process of growing a body portion and a tail portion by pulling up the seed crystal. and a step of: wherein the control unit performs the silicon melt generating step as the first heating production step, and performs the magnetic field application step, the convection direction confirmation step, and the first growing step as the second heating production step, and, in the reversal determination step, if it is determined that there is a possibility that the convection direction will be reversed when the second growing step is performed as the first heating production step based on the pulling conditions of the silicon single crystal, the control unit performs the second growing step as the second heating production step, and if it is determined that there is no possibility that the convection direction will be reversed, the control unit performs the second growing step as the first heating production step.

[0020] In the silicon single crystal manufacturing apparatus of the present invention, it is preferable that the first heating section and the second heating section are arranged, in a planar view, so that their highest temperature regions are perpendicular to a vertical imaginary plane including the central axis of the crucible and the central magnetic field line of the horizontal magnetic field and overlap with a horizontal imaginary line including the central axis of the crucible. [Brief description of the drawings]

[0021] [Figure 1] 1 is a vertical sectional view showing a schematic configuration of a silicon single crystal manufacturing apparatus according to first and second embodiments. [Diagram 2] FIG. 2 is a plan view showing a heater and a magnetic field application unit according to the first and second embodiments. [Diagram 3] FIG. 2 is a perspective view of a heater according to the first and second embodiments. [Figure 4] FIG. 2 is an equivalent circuit diagram of a heater and a power supply unit according to the first embodiment. [Diagram 5] FIG. 1 is a block diagram of a main part of a silicon single crystal manufacturing apparatus according to first and second embodiments. [Figure 6] 1 is a flowchart showing a method for producing a silicon single crystal according to first and second embodiments. [Figure 7] FIG. 11 is an equivalent circuit diagram of a heater and a power supply unit according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] [First embodiment] [Configuration of silicon single crystal manufacturing equipment] First, the configuration of a silicon single crystal manufacturing apparatus according to a first embodiment of the present invention will be described. Fig. 1 is a vertical cross-sectional view showing a schematic configuration of a silicon single crystal manufacturing apparatus. Fig. 2 is a schematic plan view showing a heater and a magnetic field application unit. Fig. 3 is a perspective view of the heater. Fig. 4 is an equivalent circuit diagram of the heater and a power supply unit. Fig. 5 is a block diagram of the main parts of the silicon single crystal manufacturing apparatus.

[0023] 1 is an apparatus for producing a silicon single crystal SM by the MCZ method, and pulls up a silicon single crystal SM having a neck portion SM1, a shoulder portion SM2, a straight body portion SM3, and a tail portion (not shown) while applying a horizontal magnetic field to a silicon melt M. The silicon single crystal production apparatus 1 includes a chamber 2 forming an outer shell, a crucible 3 arranged in the center of the chamber 2, a heater 4 arranged around the inside of the crucible 3, and a temperature measurement unit 15.

[0024] The crucible 3 has a double structure consisting of an outer graphite crucible 3A and an inner quartz crucible 3B, and the quartz crucible 3B contains silicon melt M. The graphite crucible 3A and the quartz crucible 3B are cylindrical containers with bottoms, and are circular in plan view when viewed vertically from above. The crucible 3 is fixed to the upper end of a support shaft 5 that can rotate and move up and down.

[0025] The heater 4 is a graphite heater formed in a substantially cylindrical shape and disposed around the crucible 3. Outside the heater 4, a cylindrical heat insulating material 6 is provided along the inner surface of the chamber 2.

[0026] A pulling shaft 7 is disposed above the crucible 3 and coaxially with the support shaft 5. The pulling shaft 7 is formed of a wire, etc. A seed crystal SC is attached to the lower end of the pulling shaft 7.

[0027] In the chamber 2, a cylindrical heat shield 8 is disposed above the silicon melt M in the crucible 3 to surround the silicon single crystal SM being grown. The thermal shield 8 blocks radiant heat from the silicon melt M, the side wall of the crucible 3, and the heater to the silicon single crystal SM during growth, thereby suppressing a temperature rise of the silicon single crystal SM.

[0028] A gas inlet 2A is provided at the top of the chamber 2 to introduce an inert gas such as argon gas into the chamber 2. A gas exhaust port 2B is provided at the bottom of the chamber 2 to suck and exhaust gas from within the chamber 2 by driving a vacuum pump (not shown).

[0029] The temperature measuring unit 15 measures the temperatures of the first measurement point P1 and the second measurement point P2. The radial positions of the first measurement point P1 and the second measurement point P2 are between the outer peripheral surface of the silicon single crystal SM to be grown and the inner peripheral surface of the opening of the thermal shield 8. As described later, the convection mode of the silicon melt M can be confirmed by measuring the temperatures of the first measurement point P1 and the second measurement point P2. For example, when the convection direction of the silicon melt M is fixed to the right in FIG. 1 by heating the silicon melt M by the heater 4, that is, when the convection mode of the silicon melt M becomes the right vortex mode, the measured temperature of the first measurement point P1 is higher than the measured temperature of the second measurement point P2. Also, when the convection direction of the silicon melt M is fixed to the left by heating the silicon melt M by the heater 4, that is, when the convection mode becomes the left vortex mode, the measured temperature of the first measurement point P1 is lower than the measured temperature of the second measurement point P2.

[0030] The temperature measuring unit 15 includes a pair of reflecting units 15A and a pair of radiation thermometers 15B. The reflecting section 15A is installed inside the chamber 2. The reflecting section 15A is preferably installed such that the angle between the reflecting surface 15C and the horizontal plane is equal to or greater than 40° and equal to or less than 50°. The radiation thermometer 15B is installed outside the chamber 2. The radiation thermometer 15B receives radiant light L incident through a quartz window 2C (see FIG. 1) provided in the chamber 2, and measures the temperatures of the first measurement point P1 and the second measurement point P2 in a non-contact manner.

[0031] As shown in FIG. 2, the silicon single crystal manufacturing apparatus 1 further includes a magnetic field application unit 16. The magnetic field applying unit 16 includes a first magnetic body 16A and a second magnetic body 16B, each of which is formed of an electromagnetic coil. The first magnetic body 16A and the second magnetic body 16B are provided outside the chamber 2 so as to face each other across the crucible 3. The magnetic field applying unit 16 applies a horizontal magnetic field such that, in a plan view, a central magnetic field line 16C passing through the coil central axis intersects with a central axis 3C of the crucible 3 (hereinafter, may be referred to as the "crucible central axis 3C") and is in a direction from the second magnetic body 16B to the first magnetic body 16A (the upward direction indicated by the arrow indicating the central magnetic field line 16C in FIG. 2, and the direction from the front to the back of the paper in FIG. 1).

[0032] The heater 4 is arranged so that its central axis 4C (hereinafter, sometimes referred to as the "heater central axis 4C") is located coaxially with the crucible central axis 3C. The heat insulating material 6 is arranged so that its central axis is located coaxially with the crucible central axis 3C. In other words, the crucible 3, the heater 4, and the heat insulating material 6 are arranged so that the gap between the crucible 3 and the heater 4 and the gap between the heater 4 and the heat insulating material 6 are uniform in the circumferential direction of the crucible 3. With such an arrangement of the crucible 3, the heater 4, and the heat insulating material 6, when the heater 4 generates heat uniformly in the circumferential direction, the heating distribution by the heater 4 and the heat extraction distribution by the heat insulating material 6 become uniform in the circumferential direction of the crucible 3.

[0033] As shown in Figs. 2 and 3, the heater 4 includes a heat generating portion 40, which is a cylindrical graphite heater. The heat generating portion 40 is formed with a uniform thickness over the entire circumference. In the heat generating portion 40, a plurality of upper slits 41 extending downward from the upper end and a plurality of lower slits 42 extending upward from the lower end are formed so as to be alternately arranged in the circumference. The upper slits 41 and the lower slits 42 have the same width dimension and the same cutting depth in the up-down direction. The interval between the upper slits 41 and the lower slits 42 is also the same over the entire circumference of the heater 4.

[0034] The heating section 40 includes a semi-cylindrical first heating section 40A located on one side of a first vertical imaginary plane VF1 including the heater central axis 4C, and a semi-cylindrical second heating section 40B located on the other side and having the same heating characteristics as the first heating section 40A. The same heating characteristics means that when the same amount of power is supplied, the same portion generates the same amount of heat. The first heat generating portion 40A and the second heat generating portion 40B have the same total number of upper slits 41 and lower slits 42. In this embodiment, the first heat generating portion 40A and the second heat generating portion 40B each have four upper slits 41 and six lower slits 42, and the total number of upper slits 41 and lower slits 42 is ten each.

[0035] The silicon single crystal manufacturing apparatus 1 includes a power supply unit 9 that supplies power to the heat generating unit 40. The power supply unit 9 includes a first terminal 91A, a second terminal 91B, a third terminal 91C, and a fourth terminal 91D, a first support electrode 92A, a second support electrode 92B, a third support electrode 92C, and a fourth support electrode 92D, and four nuts 93A, 93B, 93C, and 93D. The first terminal 91A to the fourth terminal 91D are arranged at 90° intervals along the circumferential direction of the heat generating unit 40. The first terminal 91A to the fourth terminal 91D extend downward from the lower end of the portion of the heat generating portion 40 defined by the two lower slits 42, and are formed integrally with the heat generating portion 40. The first terminal 91A to the fourth terminal 91D also include connection portions 911A to 911D bent at a right angle inward from the lower end, and through holes 912A to 912D are formed in the connection portions 911A to 911D. That is, the heater 4 is configured using a graphite heater in which the cylindrical heat generating portion 40, which is a heater element, and the first terminal 91A to the fourth terminal 91D, which are heater legs, are integrally molded.

[0036] By forming upper slits 41 and lower slits 42, the heat generating portion 40 is divided into a zigzag-shaped first serpentine portion 43A, a second serpentine portion 43B, a third serpentine portion 43C and a fourth serpentine portion 43D, and these first serpentine portion 43A to fourth serpentine portion 43D form four heater elements. That is, two upper slits 41 and three lower slits 42 are alternately formed between the first terminal 91A and the second terminal 91B to form a first meandering portion 43A. Similarly, two upper slits 41 and three lower slits 42 are alternately formed between the second terminal 91B and the third terminal 91C to form a second meandering portion 43B. Between the third terminal 91C and the fourth terminal 91D, two upper slits 41 and three lower slits 42 are alternately formed to form a third meandering portion 43C. Between the fourth terminal 91D and the first terminal 91A, two upper slits 41 and three lower slits 42 are alternately formed to form a fourth meandering portion 43D. In this way, the first meandering portion 43A to the fourth meandering portion 43D, which have the same shape, have the same resistance value, and therefore generate the same amount of heat when the first meandering portion 43A to the fourth meandering portion 43D receive the same amount of current. The first heat generating portion 40A is formed by the first meandering portion 43A and the second meandering portion 43B, and the second heat generating portion 40B is formed by the third meandering portion 43C and the fourth meandering portion 43D.

[0037] 2, the heater 4 is disposed so that the heater central axis 4C is coaxial with the crucible central axis 3C, and the first heat generating portion 40A and the second heat generating portion 40B are symmetrical with respect to a second vertical imaginary plane VF2 including the crucible central axis 3C and the central magnetic field line 16C. In other words, the heater 4 is disposed so that the second vertical imaginary plane VF2 overlaps with the first vertical imaginary plane VF1 shown in FIG. It can also be said that the heater 4 is arranged such that the first heat generating portion 40A and the second heat generating portion 40B are dyad-symmetric with respect to the crucible central axis 3C. In addition, the heater 4 is arranged so that when the first heating portion 40A and the second heating portion 40B generate heat with different amounts of heat, the heating amounts of the first portion 31 and the second portion 32 of the crucible 3, which are located on either side of the second vertical imaginary plane VF2 including the crucible central axis 3C and the central magnetic field line 16C, are different from each other. In addition, in plan view, the central regions of the first and second heat generating parts 40A and 40B are the highest temperature regions 401A and 401B. It can also be said that the heater 4 is disposed such that the highest temperature regions 401A and 401B of the first and second heat generating parts 40A and 40B are perpendicular to the second vertical imaginary plane VF2 and overlap with the horizontal imaginary line VL including the crucible central axis 3C in plan view. The reason that the central regions of the first and second heat generating parts 40A and 40B are the highest temperature regions 401A and 401B is that the heat generation amounts of the regions through which the current flows in the first and second heat generating parts 40A and 40B are the same, but the regions farthest from both ends of the first and second heat generating parts 40A and 40B are the highest temperature due to heat transfer.

[0038] 3, the first to fourth support electrodes 92A to 92D are rod-shaped electrodes made of conductive carbon. One end of each of the first to fourth support electrodes 92A to 92D is inserted into through-holes 912A to 912D of the terminals 91A to 91D, and carbon nuts 93A to 93D are screwed onto male threads formed on the one end of each of the first to fourth support electrodes 92A to 92D, whereby the first to fourth support electrodes 92A to 92D are electrically connected to the terminals 91A to 91D and support the heater 4.

[0039] As shown in FIG. 4, the power supply unit 9 further includes a first power source 94A and a second power source 94B, a first power supply path 95A that supplies power from the first power source 94A to the first heat generating portion 40A, and a second power supply path 95B that supplies power from the second power source 94B to the second heat generating portion 40B.

[0040] At least one of the first power source 94A and the second power source 94B is configured to be able to change the amount of power it supplies. The first power supply path 95A is composed of a second support electrode 92B and a first anode wiring 951A that connects the other end 921B of the second support electrode 92B and the anode of the first power supply 94A. The second power supply path 95B is composed of a fourth support electrode 92D and a second anode wiring 951B that connects the other end 921D of the fourth support electrode 92D and the anode of the second power supply 94B. The cathodes of the first power source 94A and the second power source 94B are grounded by a ground wiring 952A and a ground wiring 952B, respectively. The other end 921A of the first support electrode 92A and the other end 921C of the third support electrode 92C are grounded by a ground wiring 953A and a ground wiring 953B, respectively.

[0041] 4, when a current having a current value Ix flows from the first power source 94A and the second power source 94B, a current having a current value of 0.5Ix flows through the first meandering portion 43A to the fourth meandering portion 43D. As described above, the first meandering portion 43A to the fourth meandering portion 43D have the same resistance, so when the first power source 94A and the second power source 94B pass a current having the same current value Ix, that is, when the same amount of power is supplied, the first heating portion 40A and the second heating portion 40B generate the same amount of heat. On the other hand, if a current with a current value Iy flows from the first power source 94A and a current with a current value Iz different from Iy flows from the second power source 94B, in other words, if different amounts of power are supplied from the first power source 94A and the second power source 94B, a current with a current value of 0.5Iy flows through the first and second serpentine portions 43A, 43B, and a current with a current value of 0.5Iz flows through the third and fourth serpentine portions 43C, 43D, and the first heating portion 40A and the second heating portion 40B generate heat with different amounts of heat. In the following, a mode in which the first and second heating parts 40A, 40B generate heat with the same heat value may be referred to as a "uniform heating mode", and a mode in which the first and second heating parts 40A, 40B generate heat with different heat values ​​may be referred to as a "non-uniform heating mode". In addition, in FIG. 4, among the symbols attached to the arrows indicating current, the symbols outside the parentheses indicate the current value in the uniform heating mode, and the symbols inside the parentheses indicate the current value in the non-uniform heating mode. In addition, in the non-uniform heating mode, the current value of the current flowing from one of the first power source 94A and the second power source 94B may be the same as the current value in the uniform heating mode, or the current value of the current flowing from each of the first power source 94A and the second power source 94B may be different from the current value in the uniform heating mode.

[0042] When the crucible 3 is heated in the uniform heating mode, the silicon melt M in the crucible 3 is heated uniformly over the entire area in the circumferential direction of the crucible 3 . In this case, convection occurs in the silicon melt M, with the convection current rising near the side of the crucible 3 and descending near the center. In this state, due to instability of the convection current, the position of the downward flow changes randomly and may deviate from the center of the crucible 3. Then, when a horizontal magnetic field is applied to the silicon melt M, the rotation of the downward flow in the circumferential direction of the crucible 3 is gradually restricted, and eventually the direction of the convection current in an imaginary plane perpendicular to the application direction of the horizontal magnetic field is fixed. In this way, when the crucible 3 is heated in the uniform heating mode, a horizontal magnetic field is applied while the position of the downward flow is changing randomly, so that the convection mode becomes either a right vortex mode or a left vortex mode depending on the timing of application of the magnetic field.

[0043] On the other hand, when the crucible 3 is heated in the non-uniform heating mode, the silicon melt M in the crucible 3 is heated so that the temperature of the portion located on the first heating portion 40A side is different from the temperature of the portion located on the second heating portion 40B side. For example, when the second heating part 40B located on the left side of the crucible 3 generates heat with a larger heat value than the first heating part 40A located on the right side, an upward flow in the silicon melt M is stably generated on the left side of the crucible 3, and a downward flow is stably generated on the right side of the crucible 3, and the position of the downward flow does not change randomly as in the case where the first and second heating parts 40A and 40B generate heat with the same heat value. When a horizontal magnetic field is applied to the silicon melt M in this state, the convection is fixed clockwise regardless of the application timing, resulting in a right vortex mode. In particular, since the maximum temperature region 401A of the first heating part 40A overlaps with the horizontal virtual line VL in a plan view, the horizontal magnetic field is applied in a state in which the virtual line connecting the position where the upward flow is strongest and the position where the downward flow is strongest is approximately perpendicular to the generation position of the central magnetic field line 16C. Therefore, the right vortex mode can be stably generated. In order to generate the right vortex mode with a high probability regardless of the timing of application of the horizontal magnetic field, the output power bias Δ calculated by the following equation (1) is preferably 4.0% or more, and more preferably 5.0% or more. Δ(%)=(Q1 / Q2-1)×100 … (1) Q1: Output power of the first heating unit 40A Q2: Output power of the second heat generating portion 40B

[0044] Here, in order to suppress variation in oxygen concentration among the silicon single crystals SM, it is necessary to fix the direction of convection in the silicon melt M to one direction, and therefore it is preferable to heat the crucible 3 in a non-uniform heating mode. However, when the thermal environment in the chamber 2 is asymmetrical with respect to the crucible central axis 3C due to the non-uniform heating mode, the diameter of the body portion SM3 of the silicon single crystal SM is grown, and when the pulling speed is controlled to suppress the diameter variation, the fluctuation in the pulling speed may become large. Therefore, it is believed that by heating the crucible 3 in a non-uniform heating mode before pulling up the straight body portion SM3 to fix the convection of the silicon melt M in one direction, and then transitioning to a state in which the crucible 3 is heated in a uniform heating mode before pulling up the straight body portion SM3, it is possible to suppress fluctuations in the diameter of the straight body portion SM3 and fluctuations in the pulling speed.

[0045] However, when the crucible 3 is heated in the uniform heating mode, as described above, the position of the downward flow changes randomly, and the convection direction may be reversed during pulling of the body portion SM3. If such a reversal of the convection direction occurs, the concentration of oxygen taken into the body portion SM3 may vary. In addition, it is considered that whether or not the reversal of the convection direction occurs depends on the pulling conditions of the silicon single crystal SM. For this reason, it is preferable to check in advance whether or not there is a possibility that the convection direction will reverse when transitioning to the uniform heating mode after fixing the convection direction in the non-uniform heating mode, and to decide whether or not to transition to the uniform heating mode after fixing the convection mode based on the confirmation result.

[0046] 5, silicon single crystal manufacturing apparatus 1 further includes raw material supply unit 18, crucible rotation drive unit 19, pull-up drive unit 20, input unit 21, memory unit 22, and control unit 23. First power source 94A, second power source 94B, radiation thermometer 15B, magnetic field application unit 16, raw material supply unit 18, crucible rotation drive unit 19, pull-up drive unit 20, input unit 21, and memory unit 22 are connected to control unit 23 so as to be able to transmit and receive various information.

[0047] Based on the control of the control unit 23, the first power source 94A and the second power source 94B supply electric power of the same magnitude or different magnitudes to the first heat generating portion 40A and the second heat generating portion 40B, respectively. The radiation thermometer 15B outputs a signal corresponding to the measurement result to the control unit . The magnetic field application unit 16 applies a horizontal magnetic field of a predetermined strength to the silicon melt M based on the control of the control unit 23. The raw material supply unit 18 charges the silicon raw material into the crucible 3 under the control of the control unit 23. Note that the silicon single crystal manufacturing apparatus 1 may not be provided with the raw material supply unit 18, and an operator may charge the silicon raw material into the crucible 3. Under the control of the control unit 23, the crucible rotation drive unit 19 rotates the crucible 3 at a predetermined speed in a predetermined direction. The lifting drive unit 20 raises and lowers the lifting shaft 7 based on the control of the control unit 23. In addition, the lifting drive unit 20 rotates the lifting shaft 7 at a predetermined speed in the opposite direction to or in the same direction as the rotation direction of the support shaft 5 based on the control of the control unit 23.

[0048] The input unit 21 is configured with, for example, a touch panel or physical buttons. The input unit 21 is used for inputting various settings, and outputs a signal corresponding to the input operation to the control unit 23.

[0049] The storage unit 22 is configured with a well-known storage device such as an HDD (Hard Disk Drive), etc. The storage unit 22 stores various information required for controlling the pulling of the silicon single crystal SM and information for judging convection reversal. The information for determining convection reversal includes content indicating whether or not there is a possibility that the direction of convection will reverse when the convection mode of the silicon melt M is fixed in the non-uniform heating mode and then shifted to the uniform heating mode, for each pulling condition of the silicon single crystal SM and for each silicon single crystal manufacturing apparatus 1. The presence or absence of the possibility of convection reversal for each pulling condition may be confirmed by an experiment using the silicon single crystal manufacturing apparatus 1 or by manufacturing the silicon single crystal SM, or may be confirmed by a simulation.

[0050] The control unit 23 includes a CPU (Central Processing Unit). The control unit 23 controls the pulling of the silicon single crystal SM by the CPU executing a program stored in the storage unit 22.

[0051] [Method for producing silicon single crystal] Next, a description will be given of a method for producing a silicon single crystal SM using the silicon single crystal production apparatus 1. Fig. 6 is a flowchart showing a method for producing a silicon single crystal. In the first embodiment, a case is illustrated in which, in the non-uniform heating mode, the second heat generating portion 40B generates a larger amount of heat than the first heat generating portion 40A. Also, the heat generation amounts of the first and second heat generating portions 40A and 40B in the uniform heating mode may be the same as or different from the heat generation amounts of the first heat generating portion 40A or the second heat generating portion 40B in the non-uniform heating mode.

[0052] First, the operator operates the input unit 21 to input the pulling conditions for the silicon single crystal SM to be produced. As shown in FIG. 6, the control unit 23 acquires the inputted raising condition (step S1). Thereafter, the control unit 23 performs the manufacturing process of the silicon single crystal SM based on the obtained pulling conditions. Specifically, while maintaining an inert gas atmosphere under reduced pressure inside the chamber 2, turning off the heater 4 (not supplying power to the heater 4), and not applying a horizontal magnetic field, the control unit 23 controls the raw material supply unit 18 to charge the silicon raw material into the crucible 3, and then controls the crucible rotation drive unit 19 to rotate the crucible 3 in one direction (step S2). When the raw material supply unit 18 is not provided in the silicon single crystal manufacturing apparatus 1, an operator charges the silicon raw material into the crucible 3.

[0053] Next, the control unit 23 controls the first and second power sources 94A and 94B to heat the crucible 3 in a uniform heating mode by the first and second heating parts 40A and 40B of the heater 4, and melt the silicon raw material to generate silicon melt M (step S3: silicon melt generating step). In step S3, the crucible 3 is heated uniformly over the entire circumferential direction of the crucible 3. This allows the silicon raw material to be uniformly melted in the circumferential direction of the crucible 3, and prevents the solid silicon raw material floating in the silicon melt M from turning over and coming into contact with the quartz crucible 3B. As a result, damage to the quartz crucible 3B can be suppressed. Then, when all the silicon raw material is melted, the position of the downward flow generated in the silicon melt M changes randomly.

[0054] When all the silicon raw material has melted, the control unit 23 controls the first and second power sources 94A and 94B to switch from the uniform heating mode to the non-uniform heating mode (step S4). After a predetermined time has elapsed since the processing of step S4, the temperature of the left portion of the silicon melt M heated by the second heating unit 40B becomes higher than the temperature of the right portion heated by the first heating unit 40A, and an upward flow is stably generated on the left side of the crucible 3, and a downward flow is stably generated on the right side of the crucible 3. Thereafter, the control unit 23 controls the magnetic field application unit 16 to start applying a horizontal magnetic field to the silicon melt M (step S5: magnetic field application step). When the horizontal magnetic field of a predetermined strength acts on the silicon melt M by the process of step S5, the convection of the silicon melt M is fixed in a clockwise direction and becomes a right vortex mode.

[0055] Next, the control unit 23 determines whether or not the convection mode of the silicon melt M has been fixed to the right vortex mode based on a signal corresponding to the measurement result from the radiation thermometer 15B (step S6: convection direction confirmation step). When the control unit 23 determines that the convection mode is not fixed to the right vortex mode (step S6: NO), the control unit 23 performs the process of step S6 again after a predetermined time has elapsed. On the other hand, when the control unit 23 determines that the convection mode is fixed to the right vortex mode (step S6: YES), the control unit 23 controls the pulling drive unit 20 to grow the neck portion SM1 and the shoulder portion SM2 while continuing the heating in the non-uniform heating mode and the application of the horizontal magnetic field (step S7: first growth step). In step S7, the pulling drive unit 20 raises and lowers the pulling shaft 7 under the control of the control unit 23 so as to immerse the seed crystal SC in the silicon melt M and then pull up the seed crystal SC.

[0056] During or after the growth of shoulder portion SM2, control unit 23 determines, based on the pulling conditions of silicon single crystal SM and the information for convection reversal determination stored in memory unit 22, whether or not there is a possibility that the direction of convection will reverse when the non-uniform heating mode is switched to the uniform mode while the convection mode is fixed to the right vortex mode (step S8: reversal determination process).

[0057] When the control unit 23 determines that there is no possibility that the direction of convection will be reversed by switching from the non-uniform heating mode to the uniform mode (step S8: NO), it controls the first and second power sources 94A, 94B to switch from the non-uniform heating mode to the uniform mode during growth of the shoulder portion SM2 or after growth of the shoulder portion SM2 and before growth of the body portion SM3 (step S9).Then, the control unit 23 controls the pulling-up drive unit 20 to grow the body portion SM3 and the tail portion (step S10: second growth step). In this case, the thermal environment in the chamber 2 becomes symmetrical with respect to the crucible central axis 3C, so that it is possible to suppress fluctuations in the diameter of the body portion SM3 and fluctuations in the pulling speed. Furthermore, even when heating in the uniform heating mode, the direction of convection of the silicon melt M does not reverse, so that it is possible to suppress variations in the oxygen concentration in the body portion SM3.

[0058] On the other hand, if the control unit 23 determines that there is a possibility that the direction of convection will be reversed when switching from the non-uniform heating mode to the uniform mode (step S8: YES), it grows the body portion SM3 and the tail portion while maintaining the non-uniform heating mode (step S10: second growth process). In this case, the continuation of the non-uniform heating mode maintains the thermal environment in the chamber 2 asymmetrical with respect to the crucible central axis 3C, which may cause fluctuations in the diameter of the body portion SM3 and fluctuations in the pulling speed. However, the continuation of heating in the non-uniform heating mode does not reverse the direction of convection of the silicon melt M, so that variations in the oxygen concentration in the body portion SM3 can be suppressed.

[0059] In the above manufacturing process of silicon single crystal SM, the silicon melt generating process in step S3 is performed as a first heating manufacturing process in which the first and second heating parts 40A, 40B are heated with the same heat value in a uniform heating mode. The magnetic field application process in step S5, the convection direction confirmation process in step S6, and the first growing process in step S7 are performed as a second heating manufacturing process in which the first and second heating parts 40A, 40B are heated with different heat values ​​in a non-uniform heating mode. The second growing process in step S10 is performed as a first heating manufacturing process if it is determined in the reversal determination process in step S8 that there is no possibility of the convection direction being reversed, and as a second heating manufacturing process if it is determined that there is a possibility of the convection direction being reversed.

[0060] [Effects of the first embodiment] The silicon single crystal manufacturing apparatus 1 includes a cylindrical heater 4 surrounding the crucible 3 as a configuration for heating the crucible 3. The heater 4 includes a first heating part 40A and a second heating part 40B each having a semi-cylindrical shape, and is arranged such that when the first heating part 40A and the second heating part 40B generate heat with different heat values, the first part 31 and the second part 32 of the crucible 3 located on both sides of the second vertical imaginary plane VF2 generate different heat values. In the manufacturing process of the silicon single crystal SM, the control part 23 of the silicon single crystal manufacturing apparatus 1 performs a first heating manufacturing process in which the first and second heating parts 40A and 40B generate heat with the same heat value, and a second heating manufacturing process in which the first and second heating parts 40A and 40B generate heat with different heat values. Therefore, for example, by generating the silicon melt M in the uniform heating mode, it is possible to prevent the silicon raw material floating in the silicon melt M from flipping over, and to prevent damage to the quartz crucible 3B. Also, by applying a horizontal magnetic field to the silicon melt M in the non-uniform heating mode, it is possible to fix the convection mode to the right vortex mode regardless of the timing of application of the horizontal magnetic field, and it is possible to suppress the variation in oxygen concentration for each silicon single crystal SM. Also, since it is possible to suppress the variation in oxygen concentration for each silicon single crystal SM, the yield of silicon single crystal SM is improved, and it is possible to realize improved energy efficiency, improved production efficiency, and reduced waste.

[0061] The silicon single crystal manufacturing apparatus 1 includes first and second power sources 94A and 94B, a first power supply path 95A that supplies power from the first power source 94A only to the first heating portion 40A, and a second power supply path 95B that supplies power from the second power source 94B only to the second heating portion 40B. Therefore, it is possible to switch between the uniform heating mode and the non-uniform heating mode simply by controlling the amount of power supplied from the first power source 94A and the second power source 94B.

[0062] [Second embodiment] Next, the configuration of a silicon single crystal manufacturing apparatus according to a second embodiment of the present invention will be described. FIG. 7 is an equivalent circuit diagram of the heater and power supply.

[0063] The silicon single crystal manufacturing apparatus 1A of the second embodiment differs from the silicon single crystal manufacturing apparatus 1 of the first embodiment in that a control unit 23A shown in FIG. 5 performs control differently from that of the control unit 23 of the first embodiment, and a power supply unit 9A shown in FIG. 7 has a configuration different from that of the power supply unit 9 of the first embodiment, but the other configurations are the same as those of the silicon single crystal manufacturing apparatus 1 of the first embodiment.

[0064] As shown in FIG. 7, the power supply unit 9A has the same configuration as the power supply unit 9 of the first embodiment, and further includes a bypass supply path 96A connecting the first power supply path 95A and the second power supply path 95B, and a rectifier 96B provided in the bypass supply path 96A and supplying power only in the direction from the first power supply path 95A to the second power supply path 95B. The bypass supply path 96A is formed of a wiring that connects the first anode wiring 951A and the second anode wiring 951B. The rectification unit 96B is formed of a diode provided midway along the second power supply path 95B.

[0065] With the heater 4 and power supply unit 9A configured as shown in FIG. 7, when a current with a current value of Ip flows from the first power source 94A and no current flows from the second power source 94B, in other words, when power is supplied from the first power source 94A and no power is supplied from the second power source 94B, a current with a current value of 0.25 Ip flows through the first meandering portion 43A to the fourth meandering portion 43D, and the first heating portion 40A and the second heating portion 40B generate heat with the same amount of heat. On the other hand, when a current with a current value of Ip flows from the first power source 94A and a current with a current value of Iq flows from the second power source 94B, in other words, when power is supplied from the first power source 94A and the second power source 94B, a current with a current value of 0.25Ip flows through the first and second serpentine portions 43A and 43B, and a current with a current value of 0.25Ip+0.5q flows through the third and fourth serpentine portions 43C and 43D, so that the second heating portion 40B generates a greater amount of heat than the first heating portion 40A. In FIG. 7, among the symbols attached to the arrows indicating current, the symbols outside parentheses indicate current values ​​in the uniform heating mode, and the symbols inside parentheses indicate current values ​​in the non-uniform heating mode.

[0066] When producing a silicon single crystal SM, the control unit 23A performs control similar to that of the control unit 23 of the first embodiment shown in FIG. 6, but differs from the control unit 23 in the control when heating the crucible 3 in the uniform heating mode and the non-uniform heating mode. The control unit 23A controls the first and second power sources 94A and 94B so that the first power source 94A supplies power and the second power source 94B does not supply power when heating the crucible 3 in the uniform heating mode. Also, the control unit 23A controls the first and second power sources 94A and 94B so that the first power source 94A and the second power source 94B supply power when heating the crucible 3 in the non-uniform heating mode.

[0067] [Effects of the second embodiment] The first heating portion 40A and the second heating portion 40B have the same heat generating characteristics. The silicon single crystal manufacturing apparatus 1A includes first and second power sources 94A and 94B, first and second power supply paths 95A and 95B, a bypass supply path 96A that connects the first power supply path 95A and the second power supply path 95B, and a rectifier 96B that is provided in the bypass supply path 96A and supplies power only in a direction from the first power supply path 95A to the second power supply path 95B. Therefore, while a predetermined amount of power is being supplied from the first power source 94A, simply by controlling whether or not power is supplied from the second power source 94B, it is possible to switch between the uniform heating mode and the non-uniform heating mode. Furthermore, since it is only necessary for the second power source 94B to supply power sufficient to produce the difference in heat generation temperature between the first heat generating portion 40A and the second heat generating portion 40B, a power source with a small capacity can be used as the second power source 94B. Furthermore, power supplies whose supply amount of power cannot be changed can be used as the first and second power supplies 94A and 94B. Furthermore, since the variation in oxygen concentration for each silicon single crystal SM can be suppressed, the yield of silicon single crystal SM can be improved, and it is possible to realize improved energy efficiency, improved production efficiency, and reduced waste.

[0068] [Variations] Although an embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and various improvements and design changes that do not deviate from the gist of the present invention are also included in the present invention.

[0069] In the first and second embodiments, the processes of steps S8 and S9 may not be performed, and the body portion SM3 and the tail portion may be grown in the non-uniform heating mode.

[0070] In the first and second embodiments, an operator may perform at least one of the processes of switching the heating mode in steps S3, S4, and S9, the process of starting the application of a horizontal magnetic field in step S5, the process of determining the convection mode in step S6, and the process of determining the possibility of convection reversal in step S8. In the first and second embodiments, the second heating manufacturing process is exemplified as a process of fixing the convection mode to the right vortex mode by heating the left portion of the silicon melt M so that the temperature of the left portion is higher than the temperature of the right portion. However, a process of fixing the convection mode to the left vortex mode by heating the right portion of the silicon melt M so that the temperature of the right portion is higher than the temperature of the left portion may also be performed.

[0071] In the first and second embodiments, the heater 4 may be disposed so that when the first heating portion 40A and the second heating portion 40B generate heat with different amounts of heat, the amounts of heat applied to the first portion 31 and the second portion 32 of the crucible 3 are different from each other, and may be disposed in a state rotated clockwise or counterclockwise by an angle of less than 45° from the state shown in Fig. 2, or may be disposed in a state rotated clockwise or counterclockwise by an angle of more than 45° and less than 90°. In other words, the heater 4 may be disposed so that the second vertical imaginary plane VF2 does not overlap the first vertical imaginary plane VF1 shown in Fig. 3. EXAMPLES

[0072] Next, examples of the present invention will be described, but the present invention is not limited to the examples.

[0073] [Experimental conditions] Comparative Example First, the silicon single crystal manufacturing apparatus 1 of the first embodiment was prepared. Then, the first and second power sources 94A and 94B were controlled to heat the crucible 3 in the uniform heating mode, thereby generating the silicon melt M. Next, a horizontal magnetic field was applied to the silicon melt M while maintaining the uniform heating mode, and after it was confirmed that the convection mode was fixed, a silicon single crystal SM having a straight body portion SM3 with a diameter of 300 mm and a total length of 2000 mm was grown. In this case, the output power bias Δ calculated by the above formula (1) is 0%.

[0074] [Examples 1 to 8] In Example 1, the crucible 3 was heated in the uniform heating mode to generate the silicon melt M, and then the first and second power sources 94A and 94B were controlled so that the output power bias Δ was 3.0%, and the uniform heating mode was switched to the non-uniform heating mode. After the temperature of the silicon melt M was stabilized, a horizontal magnetic field was applied to the silicon melt M, and after it was confirmed that the convection mode was fixed, a silicon single crystal SM of the same size as that of Comparative Example 1 was grown. In Examples 2, 3, 4, 5, 6, 7, and 8, the crucible 3 was heated in a uniform heating mode to generate silicon melt M, and then a silicon single crystal SM of the same size as in Comparative Example 1 was grown under the same conditions as in Example 1, except that the first and second power sources 94A and 94B were controlled so that the output power bias Δ was 4.0%, 5.0%, 6.0%, -3.0%, -4.0%, -5.0%, and -6.0%, respectively.

[0075] [evaluation] Ten silicon single crystals SM were grown for each of the comparative example and Examples 1 to 8, and the convection mode occurrence rate, oxygen concentration, and variation in oxygen concentration were evaluated. The oxygen concentration was evaluated as follows. First, a wafer was obtained from a position 1000 mm below the top end of the straight body portion SM3 of each silicon single crystal SM of the comparative example and Examples 1 to 8, and the oxygen concentration of the wafer was measured by FTIR (Fourier transform infrared spectrophotometer). Then, normalization was performed using the average value of the oxygen concentrations in the wafers obtained from the 10 silicon single crystal SMs of the comparative example, and the upper and lower limit values ​​of the oxygen concentration in each of the comparative example and Examples 1 to 8 were calculated. In addition, the difference between the upper and lower limit values ​​of the oxygen concentration was calculated as the variation in the oxygen concentration.

[0076] [Table 1]

[0077] [Occurrence rate of convection mode] In the comparative example, the occurrence rate of the left vortex mode was 50%, and the right vortex mode and the left vortex mode occurred substantially randomly. On the other hand, in Examples 1 to 4, the occurrence rate of the right vortex mode exceeded 50%, and the larger the output power bias Δ, the higher the occurrence rate of the right vortex mode. In particular, in Examples 2 to 4 where the output power bias Δ was 4.0% or more, the occurrence rate of the right vortex mode was 90% or more, and in Examples 3 and 4 where the output power bias Δ was 5.0% or more, the occurrence rate of the right vortex mode was 100%. Furthermore, in Examples 5 to 8, a similar tendency to that in Examples 1 to 4 was confirmed, and in Examples 6 to 8 where the output power bias Δ was -4.0% or less, the occurrence rate of the left vortex mode was 90% or more, and in Examples 7 and 8 where the output power bias Δ was -5.0% or less, the occurrence rate of the left vortex mode was 100%.

[0078] From the above, it was confirmed that the convection mode can be easily fixed to one mode regardless of the application timing of the horizontal magnetic field by controlling the first and second power sources 94A and 94B so that the absolute value of the output power bias Δ is 4.0% or more. In particular, it was confirmed that the convection mode can be fixed to one mode regardless of the application timing of the horizontal magnetic field by controlling the first and second power sources 94A and 94B so that the absolute value of the output power bias Δ is 5.0% or more.

[0079] [Variation in oxygen concentration] The variation in oxygen concentration in the comparative example was 0.40. On the other hand, the oxygen concentration variation in Examples 1 to 8 was 0.30 or less, and the greater the absolute value of the output power bias Δ, the smaller the oxygen concentration variation. In particular, in Examples 2 to 4 and 6 to 8, where the absolute value of the output power bias Δ was 4.0% or more, the oxygen concentration variation was 0.25 or less, which was nearly half the size of the comparative example, and in Examples 3, 4, 7, and 8, where the absolute value of the output power bias Δ was 5.0% or more, the oxygen concentration variation was 0.05, which was extremely small compared to the comparative example.

[0080] From the above, it was confirmed that by controlling the first and second power sources 94A, 94B so that the absolute value of the output power bias Δ is 4.0% or more, the variation in the oxygen concentration in the straight body portion SM3 can be reduced, and in particular, by controlling the first and second power sources 94A, 94B so that the absolute value of the output power bias Δ is 5.0% or more, the variation in the oxygen concentration in the straight body portion SM3 can be extremely reduced. [Industrial Applicability]

[0081] The silicon single crystal manufacturing method and silicon single crystal manufacturing apparatus of the present invention can suppress the occurrence of defects during manufacturing and the variation in oxygen concentration for each silicon single crystal, thereby improving the yield of silicon single crystals, improving energy efficiency, improving production efficiency, and reducing waste. [Explanation of symbols]

[0082] 1,1A...silicon single crystal manufacturing apparatus, 3...crucible, 3C...crucible central axis, 4...heater, 9,9A...power supply unit, 16C...central magnetic field line, 23,23A...control unit, 31...first portion, 32...second portion, 40A...first heating unit, 40B...second heating unit, 94A...first power source, 94B...second power source, 95A...first power supply path, 95B...second power supply path, 96A...bypass supply path, 96B...rectifier unit, 401A,401B...maximum temperature region, M...silicon melt, SM...silicon single crystal, SM1...neck portion, SM2...shoulder portion, SM3...straight body portion, VF1...first vertical imaginary plane, VF2...second vertical imaginary plane.

Claims

1. A method for producing a silicon single crystal, comprising the steps of: applying a horizontal magnetic field to a silicon melt while pulling up the silicon single crystal using a silicon single crystal production apparatus, The silicon single crystal manufacturing apparatus comprises: a crucible for containing the silicon melt; a cylindrical heater surrounding the crucible; the heater includes a semi-cylindrical first heating portion and a second heating portion each having the same heat generating characteristics, and is arranged such that when the first heating portion and the second heating portion generate heat with mutually different heat amounts, the first portion and the second portion of the crucible located on both sides of a vertical imaginary plane including a central axis of the crucible and a central magnetic line of force of the horizontal magnetic field are heated with mutually different amounts; The method for producing a silicon single crystal comprises: A first heating manufacturing process is performed while the first heating section and the second heating section are heated with the same amount of heat; a second heating production step in which the first heating portion and the second heating portion are heated at different heat values.

2. 2. The method for producing a silicon single crystal according to claim 1, The silicon single crystal manufacturing apparatus comprises: a first power source and a second power source; a first power supply path that supplies power from the first power source to the first heat generating portion; a second power supply path that supplies power from the second power source to the second heat generating portion, The first heating manufacturing step is performed while controlling the first power source and the second power source so that the first heat generating portion and the second heat generating portion generate heat with the same amount of heat; A method for producing a silicon single crystal, wherein the second heating process is performed while controlling the first power source and the second power source so as to cause the first heating portion and the second heating portion to generate heat at different amounts of heat.

3. The method for producing a silicon single crystal according to claim 2, The silicon single crystal manufacturing apparatus comprises: a bypass supply path connecting the first power supply path and the second power supply path; a rectifier provided in the bypass supply path and supplying power only in a direction from the first power supply path to the second power supply path, the first heating manufacturing step is performed while controlling the first power source and the second power source so as to supply power from the first power source and not to supply power from the second power source; The method for producing a silicon single crystal, wherein the second heating production step is performed while controlling the first power source and the second power source so as to supply electric power from the first power source and the second power source.

4. 2. The method for producing a silicon single crystal according to claim 1, a silicon melt generating step of melting the silicon raw material in the crucible to generate the silicon melt; a magnetic field application step of starting application of the horizontal magnetic field to the silicon melt; a convection direction confirmation step of confirming that the direction of convection of the silicon melt in a virtual plane perpendicular to the central magnetic field line is fixed in one direction; a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt; a second growth step of growing a body portion and a tail portion by pulling up the seed crystal, the silicon melt generating step and the second growing step are carried out as the first heating manufacturing step, The method for producing a silicon single crystal, wherein the magnetic field application step, the convection direction confirmation step, and the first growth step are performed as the second heating production step.

5. 2. The method for producing a silicon single crystal according to claim 1, a silicon melt generating step of melting the silicon raw material in the crucible to generate the silicon melt; a magnetic field application step of starting application of the horizontal magnetic field to the silicon melt; a convection direction confirmation step of confirming that the direction of convection of the silicon melt in a virtual plane perpendicular to the central magnetic field line is fixed in one direction; a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt; An inversion determination step; a second growth step of growing a body portion and a tail portion by pulling up the seed crystal, The silicon melt generating step is carried out as the first heating manufacturing step, the magnetic field application step, the convection direction confirmation step, and the first growth step are carried out as the second heating production step, In the inversion determination step, if it is determined that there is a possibility that the direction of convection will be reversed when the second growth step is performed as the first heating production step based on the pulling conditions of the silicon single crystal, then the second growth step is performed as the second heating production step, and if it is determined that there is no possibility that the direction of convection will be reversed, then the second growth step is performed as the first heating production step.

6. The method for producing a silicon single crystal according to any one of claims 1 to 5, A method for producing a silicon single crystal, wherein the first heating portion and the second heating portion are arranged, in a planar view, such that their highest temperature regions are perpendicular to the vertical imaginary plane and overlap with a horizontal imaginary line including a central axis of the crucible.

7. A silicon single crystal manufacturing apparatus that pulls up a silicon single crystal while applying a horizontal magnetic field to a silicon melt, a crucible for containing the silicon melt; A cylindrical heater surrounding the crucible; a power supply unit that supplies power to the heater; the heater includes a first heating portion and a second heating portion each having a semi-cylindrical shape and the first heating portion and the second heating portion each having the same heat generating characteristics; The power supply unit includes: a first power source and a second power source; a first power supply path that supplies power from the first power source to the first heat generating portion; a second power supply path that supplies power from the second power source to the second heat generating portion.

8. The silicon single crystal manufacturing apparatus according to claim 7, The power supply unit includes: a bypass supply path connecting the first power supply path and the second power supply path; a rectifier provided in the bypass supply path and configured to supply power only in a direction from the first power supply path to the second power supply path.

9. The silicon single crystal manufacturing apparatus according to claim 7, a control unit for controlling the manufacturing process of pulling the silicon single crystal; The manufacturing process includes: a first heating manufacturing process performed while controlling the first power source and the second power source so that the first heating portion and the second heating portion generate heat with the same amount of heat; a second heating production process performed while controlling the first power source and the second power source so as to cause the first heating portion and the second heating portion to generate heat at different amounts of heat.

10. 9. The silicon single crystal manufacturing apparatus according to claim 8, a control unit for controlling the manufacturing process of pulling the silicon single crystal; The manufacturing process includes: a first heating manufacturing step performed while controlling the first power source and the second power source so as to supply power from the first power source and not supply power from the second power source; a second heating production step performed while controlling the first power source and the second power source so as to supply power from the first power source and the second power source.

11. The silicon single crystal manufacturing apparatus according to claim 9 or 10, The manufacturing process includes: a silicon melt generating step of melting the silicon raw material in the crucible to generate the silicon melt; a magnetic field application step of starting application of the horizontal magnetic field to the silicon melt; a convection direction confirmation step of confirming that the direction of convection of the silicon melt in a virtual plane perpendicular to the central magnetic field line of the horizontal magnetic field is fixed in one direction; a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt; a second growth step of growing a body portion and a tail portion by pulling up the seed crystal, The control unit is The silicon melt generating step and the second growing step are performed as the first heating manufacturing step, The silicon single crystal manufacturing apparatus performs the magnetic field application step, the convection direction confirmation step, and the first growth step as the second heating manufacturing step.

12. The silicon single crystal manufacturing apparatus according to claim 9 or 10, The manufacturing process includes: a silicon melt generating step of melting the silicon raw material in the crucible to generate the silicon melt; a magnetic field application step of starting application of the horizontal magnetic field to the silicon melt; a convection direction confirmation step of confirming that the direction of convection of the silicon melt in a virtual plane perpendicular to the central magnetic field line of the horizontal magnetic field is fixed in one direction; a first growing step of growing a neck portion and a shoulder portion by pulling up a seed crystal immersed in the silicon melt; An inversion determination step; a second growth step of growing a body portion and a tail portion by pulling up the seed crystal, The control unit is The silicon melt generating step is carried out as the first heating manufacturing step, The magnetic field application step, the convection direction confirmation step, and the first growth step are performed as the second heating production step, In the inversion determination process, if it is determined that there is a possibility that the direction of convection will be reversed when the second growth process is performed as the first heating manufacturing process based on the pulling conditions of the silicon single crystal, the second growth process is performed as the second heating manufacturing process, and if it is determined that there is no possibility that the direction of convection will be reversed, the second growth process is performed as the first heating manufacturing process.

13. The silicon single crystal manufacturing apparatus according to any one of claims 7 to 10, The silicon single crystal manufacturing apparatus, wherein the first heating section and the second heating section are arranged, in a plan view, so that their highest temperature regions are perpendicular to a vertical imaginary plane including a central axis of the crucible and a central magnetic line of the horizontal magnetic field, and overlap with a horizontal imaginary line including the central axis of the crucible.

Citation Information

Patent Citations

  • Production method of silicon single crystal

    JP2017095323A

  • Method for controlling convection pattern of silicon melt, method for manufacturing silicon single crystal and apparatus for pulling silicon single crystal

    JP2019151502A