Reflection mask blank and reflection mask production method
The reflective mask blank with a ruthenium-based protective film and layered tantalum-nitrogen absorber film addresses protective film damage during dry etching and cleaning, ensuring the multilayer reflective film's integrity and performance.
Patent Information
- Application Number
- JP2024035715
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional reflective mask blanks face issues with protective film damage during dry etching and cleaning processes, leading to reduced thickness and loss of protective function, which affects the multilayer reflective film's integrity.
A reflective mask blank design with a protective film composed of ruthenium (Ru) and an absorber film with multiple layers, including a tantalum (Ta) and nitrogen (N) layer, is used to withstand dry etching gases and cleaning agents, minimizing film thickness reduction.
The design effectively reduces damage to the protective film during dry etching and cleaning, maintaining the integrity and reflectance of the multilayer reflective film.
Smart Images

Figure 2024148148000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a reflective mask blank, which is a material for a reflective mask used in the manufacture of semiconductor devices such as LSIs, and a method for manufacturing a reflective mask from the reflective mask blank. [Background technology]
[0002] In the manufacturing process of semiconductor devices (semiconductor device), photolithography technology is repeatedly used, in which exposure light is irradiated onto a transfer mask, and the circuit pattern formed on the mask is transferred onto a semiconductor substrate (semiconductor wafer) via a reduced projection optical system. Conventionally, the wavelength of the exposure light has mainly been 193 nm using argon fluoride (ArF) excimer laser light, and a process called multi-patterning, which combines exposure processes and processing processes multiple times, has been used to ultimately form patterns with dimensions smaller than the exposure wavelength.
[0003] However, as the miniaturization of device patterns continues, the formation of even finer patterns is required, and so EUV lithography technology using extreme ultraviolet (EUV) light, which has an even shorter wavelength than ArF excimer laser light, as exposure light has come to be used. EUV light is light with a wavelength of about 0.2 to 100 nm, more specifically, light with a wavelength of about 13.5 nm. EUV light has extremely low transparency to materials, so that conventional transmission type projection optical systems and masks cannot be used, and therefore reflective optical elements are used. Therefore, reflective masks are also used for pattern transfer.
[0004] A reflective mask has a multilayer reflective film that reflects EUV light formed on a substrate, and an absorber film that absorbs EUV light formed in a pattern on the multilayer reflective film. On the other hand, a mask in a state before the absorber film is patterned (including a mask with a resist film formed thereon) is called a reflective mask blank, and is used as a material for reflective masks. A reflective mask blank generally has a basic structure including a low-thermal expansion substrate, a multilayer reflective film that reflects EUV light formed on one of the two main surfaces of the substrate, and an absorber film that absorbs EUV light formed thereon.
[0005] The multilayer reflective film is usually made by alternately stacking molybdenum (Mo) layers and silicon (Si) layers to obtain the necessary reflectance for EUV light. On the other hand, the absorber film is made of tantalum (Ta), which has a relatively large extinction coefficient for EUV light (JP Patent Publication 2002-246299 (Patent Document 1)).
[0006] Furthermore, as a protective film for protecting the multilayer reflective film, a ruthenium (Ru) film as disclosed in JP-A-2002-122981 (Patent Document 2) is formed on the multilayer reflective film. Also, a hard mask film containing chromium (Cr) may be formed on the absorber film as an etching mask when forming a pattern on the absorber film. Meanwhile, a conductive film is formed on the other main surface of the substrate. As the conductive film, a metal nitride film has been proposed for electrostatic chucking, and a film containing mainly chromium (Cr) and tantalum (Ta) is mentioned. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-246299 A [Patent Document 2] JP 2002-122981 A Summary of the Invention [Problem to be solved by the invention]
[0008] The protective film is required to have a function of protecting the reflective film. Specifically, the protective film has a function of protecting the multilayer reflective film from exposure to etching gas or cleaning liquid during pattern processing of the absorber film, and a function of suppressing a decrease in reflectance with repeated exposure during exposure using a reflective mask.
[0009] In a process for manufacturing a reflective mask using a reflective mask blank as a material, when a pattern is formed in an absorber film by dry etching, a certain degree of overetching is usually performed in order to control the pattern shape. By performing overetching, the protective film is exposed to the etching and is damaged. When the absorber film is formed of a material containing tantalum (Ta), a gas containing chlorine but not oxygen is preferably used as the etching gas, so the protective film is required to be resistant to dry etching using a gas containing chlorine but not oxygen.
[0010] In addition, when a hard mask film pattern obtained by patterning a hard mask film made of a material containing chromium (Cr) is used as an etching mask for forming a pattern in the absorber film, after forming the absorber film pattern, the hard mask film pattern is usually removed by dry etching using a gas containing chlorine and oxygen, and at that time, the protective film is also exposed to dry etching using a gas containing chlorine and oxygen. Therefore, the protective film is also required to be resistant to dry etching using a gas containing chlorine and oxygen.
[0011] Furthermore, cleaning with sulfuric acid / hydrogen peroxide (SPM) is performed to remove resist residues used in manufacturing the reflective mask and contamination that occurs during repeated use of the reflective mask, so the protective film must also be resistant to SPM.
[0012] If the protective film is damaged during dry etching in the manufacture of a reflective mask, and the film quality or thickness changes, problems such as the loss of the function of protecting the multilayer reflective film occur. For this reason, it has been proposed to add an additive element such as niobium (Nb) to a protective film containing ruthenium (Ru) to improve its resistance to dry etching and enhance the protective film's function of protecting the multilayer reflective film.
[0013] However, even if an additive element such as niobium (Nb) is added to a protective film containing ruthenium (Ru) to increase the resistance to dry etching, the thickness of the protective film decreases when the protective film is exposed to a gas containing chlorine and not containing oxygen during dry etching of an absorber film formed of a material containing tantalum (Ta). In addition, when the protective film is exposed to a gas containing chlorine and oxygen during removal of the pattern of the hard mask film, the thickness of the protective film also decreases. Furthermore, the thickness of the protective film also decreases during cleaning using sulfuric acid / hydrogen peroxide (SPM).
[0014] As such, chemical damage to the protective film is unavoidable, and physical damage will also reduce the thickness of the protective film, so it is necessary to suppress the deterioration of the protective film's function of protecting the multilayer reflective film due to the reduction in thickness.
[0015] The present invention has been made to solve the above-mentioned problems, and has an object to provide a reflective mask blank in which an absorber film formed of a material containing tantalum (Ta) is formed on a protective film formed of a material containing ruthenium (Ru), the absorber film being capable of reducing damage to the protective film caused by over-etching in dry etching of the absorber film formed of a material containing tantalum (Ta) using a gas containing chlorine but not oxygen, and of suppressing reduction in the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen, or by cleaning with sulfuric acid / hydrogen peroxide (SPM), and a method for manufacturing a reflective mask using the reflective mask blank. [Means for solving the problem]
[0016] As a result of extensive investigations to solve the above problems, the inventors have found that, in a reflective mask blank, an absorber film made of a material containing tantalum (Ta) is formed on a protective film made of a material containing ruthenium (Ru), and the absorber film is configured to include, from the substrate side, a first layer having a composition containing tantalum (Ta) and not containing nitrogen (N), and a second layer having a composition containing tantalum (Ta) and nitrogen (N), thereby reducing damage to the protective film caused by over-etching in dry etching of the absorber film made of a material containing tantalum (Ta) using a gas containing chlorine and not containing oxygen, and also suppressing reduction in the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen or cleaning using sulfuric acid / hydrogen peroxide (SPM), thereby completing the present invention.
[0017] Accordingly, the present invention provides the following methods for producing a reflective mask blank and a reflective mask. 1. A reflective mask blank comprising: a substrate; a multilayer reflective film formed on one main surface of the substrate and reflecting exposure light; a protective film formed on and in contact with the multilayer reflective film; an absorber film formed on and in contact with the protective film and absorbing exposure light; and a hard mask film formed on and in contact with the absorber film and functioning as an etching mask when dry etching the absorber film, the hard mask film being formed on and in contact with the absorber film, the mask blank serving as a material for a reflective mask used in EUV lithography using EUV light as exposure light, The protective film is formed of a material containing ruthenium (Ru) and has a thickness of 2 nm to 5 nm, the absorber film is formed of a material containing tantalum (Ta) and is composed of two layers, a first layer and a second layer, or three layers, a first layer, a second layer, and a third layer, from the substrate side; The first layer has a composition containing tantalum (Ta) and not containing nitrogen (N), and has a thickness of 0.5 nm or more and 2 nm or less; the second layer has a composition containing tantalum (Ta) and nitrogen (N), the nitrogen (N) content being 10 atomic % or more and the oxygen (O) content being 5 atomic % or less; a total thickness of the first layer and the second layer is 50 nm or more and 80 nm or less; the third layer has a composition containing tantalum (Ta), nitrogen (N) and oxygen (O), the content of oxygen (O) being 30 atomic % or more and 70 atomic % or less, and has a thickness of 20 nm or less; The hard mask film is made of a material containing chromium (Cr) and has a thickness of 5 nm to 20 nm. A reflective mask blank comprising: 2. The reflective mask blank according to 1, wherein the composition of the first layer further contains oxygen (O). 3. The reflective mask blank according to 2, wherein the first layer has a composition in which the oxygen (O) content is 5 atomic % or more. 4. The reflective mask blank according to 1, characterized in that in the composition of the second layer, the tantalum (Ta) content is 55 atomic % or more and 70 atomic % or less, and the nitrogen (N) content is 30 atomic % or more and 45 atomic % or less. 5. The reflective mask blank according to 1, wherein the material containing ruthenium (Ru) is ruthenium (Ru) alone or an alloy of ruthenium (Ru) and niobium (Nb). 6. The reflective mask blank according to 5, wherein the alloy of ruthenium (Ru) and niobium (Nb) has an average niobium (Nb) content of 30 atomic % or less throughout the protective film. 7. (A) A step of preparing a reflective mask blank according to 1; (B) forming a resist pattern on the hard mask film; (C) dry etching the hard mask film using a gas containing chlorine and oxygen, with the resist pattern as an etching mask, to form a pattern of the hard mask film; (D) dry etching the first and second layers of the absorber film using a gas containing chlorine and not containing oxygen, with the pattern of the hard mask film as an etching mask, to form patterns of the first and second layers of the absorber film; (E) removing the resist pattern after the step (C) or (D); (F) removing the pattern of the hard mask film by dry etching using a gas containing chlorine and oxygen; A method for manufacturing a reflective mask comprising the steps of: 8. The method according to claim 7, wherein in the step (D), dry etching is performed so as to expose the protective film. 9. In the step (D), dry etching is performed so that a part of the absorber film does not remain and the protective film is not exposed; 8. The manufacturing method according to claim 7, wherein in the step (F), dry etching is performed so that the protective film is exposed. 10. Further, (G) after the step (F), a step including a treatment of contacting the exposed protective film with sulfuric acid / hydrogen peroxide (SPM) 10. The method for producing according to claim 8 or 9, comprising: 11. Further, (G) after the step (F), a step including a treatment of contacting the exposed protective film with sulfuric acid / hydrogen peroxide (SPM) Including, In the steps (D) and (F), dry etching is performed so that a portion of the absorber film does not remain and the protective film is not exposed; 8. The method according to claim 7, wherein in the step (G), the protective film is exposed. 12. The absorber film is composed of three layers, namely, a first layer, a second layer, and a third layer, from the substrate side; Furthermore, (C-1) after the step (C) and before the step (D), a step of dry etching the third layer of the absorber film using a fluorine-based gas and a pattern of the hard mask film as an etching mask to form a pattern of the third layer of the absorber film. 8. The method for producing a product according to claim 7, comprising: Effect of the Invention
[0018] According to the present invention, it is possible to reduce damage to a protective film caused by over-etching in dry etching of an absorber film formed of a material containing tantalum (Ta) using a gas containing chlorine but not oxygen. Also, the reflective mask blank of the present invention suppresses reduction in the thickness of the protective film caused by dry etching using a gas containing chlorine and oxygen or cleaning using sulfuric acid / hydrogen peroxide (SPM). [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a reflective mask blank of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of the reflective mask blank of the present invention. [Diagram 3] FIG. 1 is a schematic diagram of an etching apparatus used in an experimental example and a comparative experimental example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will now be described in further detail. The reflective mask blank of the present invention comprises a substrate, a multilayer reflective film formed on one main surface (front surface) of the substrate and reflecting exposure light, a protective film formed on the multilayer reflective film, an absorber film formed on the protective film and absorbing exposure light, and a hard mask film formed on the absorber film. The reflective mask blank of the present invention is suitable as a material for a reflective mask used in EUV lithography using EUV light as exposure light. The wavelength of EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, and is usually light with a wavelength of about 13.5 nm. The reflective mask blank and the reflective mask using EUV light as exposure light are also called EUV mask blank and EUV mask, respectively.
[0021] 1 is a cross-sectional view showing an example of a reflective mask blank of the present invention. This reflective mask blank 11 includes a substrate 1, a multilayer reflective film 2 formed on the substrate 1 in contact with the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, an absorber film 4 formed in contact with the protective film 3, and a hard mask film 5 formed in contact with the absorber film 4. In this case, the absorber film 4 has a two-layer structure of a first layer 41 and a second layer 42 from the substrate 1 side.
[0022] 2 is a cross-sectional view showing another example of the reflective mask blank of the present invention. This reflective mask blank 12 includes a substrate 1, a multilayer reflective film 2 formed on the substrate 1 in contact with the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, an absorber film 4 formed in contact with the protective film 3, and a hard mask film 5 formed in contact with the absorber film 4. In this case, the absorber film 4 has a three-layer structure of a first layer 41, a second layer 42, and a third layer 43 from the substrate 1 side.
[0023] The substrate preferably has low thermal expansion characteristics for EUV light exposure, and has a thermal expansion coefficient of, for example, ±2×10 -8 / ℃, preferably within ±5×10 -9 It is preferable that the material is made of a material having a temperature within a range of 100°C / °F. Such a material is titania-doped quartz glass (SiO 2 -TiO 2 Glass-based glass, etc. It is preferable to use a substrate having a sufficiently flat surface, and the surface roughness of the main surface of the substrate is preferably 0.5 nm or less, more preferably 0.2 nm or less, in terms of RMS value. Such a surface roughness can be obtained by polishing the substrate, etc. The size of the substrate is preferably 152 mm square for the main surface and 6.35 mm thick for the thickness. A substrate of this size is a so-called 6025 substrate (a substrate with a main surface size of 6 inches square and a thickness of 0.25 inches).
[0024] The multilayer reflective film is a film that reflects exposure light in a reflective mask. The multilayer reflective film is preferably provided in contact with one main surface of the substrate, but another film such as an undercoat film may be provided between the multilayer reflective film and the one main surface of the substrate. The multilayer reflective film has a periodic laminate structure in which a high refractive index layer having a relatively high refractive index to the exposure light and a low refractive index layer having a relatively low refractive index to the exposure light are alternately laminated.
[0025] The high refractive index layer is preferably formed of a material containing silicon (Si). The high refractive index layer may contain one or more additive elements selected from oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H), and may be composed of a multilayer of a layer containing an additive element and a layer not containing an additive element. The thickness of the high refractive index layer is preferably 3.5 nm or more, more preferably 4 nm or more, and is preferably 4.9 nm or less, more preferably 4.4 nm or less.
[0026] The low refractive index layer is preferably formed of a material containing molybdenum (Mo). The low refractive index layer may contain one or more additive elements selected from oxygen (O), nitrogen (N), carbon (C), boron (B) and hydrogen (H), and may be composed of a multilayer structure including a layer containing an additive element and a layer not containing an additive element. The thickness of the low refractive index layer is preferably 2.1 nm or more, more preferably 2.6 nm or more, and is preferably 3.5 nm or less, more preferably 3 nm or less.
[0027] The laminate structure constituting the periodic laminate structure may include a high refractive index layer and a low refractive index layer, and one or more high refractive index layers and one or more low refractive index layers may be included in one period. The number of layers included in the laminate structure is two or more, and the laminate structure may be composed of, for example, one high refractive index layer and one low refractive index layer. In addition, two or more high refractive index layers having different compositions (for example, different composition ratios, different compositions depending on the presence or absence of an additive element, etc.) may be included, and two or more low refractive index layers having different compositions (for example, different composition ratios, different compositions depending on the presence or absence of an additive element, etc.) may be included. In this case, the number of layers included in the laminate structure is three or more, and may be four or more or five or more, but is preferably eight or less. The number of periods of the laminate structure in the periodic laminate structure is preferably 30 or more, and preferably 50 or less, more preferably 40 or less.
[0028] The thickness of the multilayer reflective film having a periodic laminate structure is preferably 200 nm or more, more preferably 270 nm or more, and is preferably 400 nm or less, more preferably 290 nm or less.
[0029] Methods for forming a multilayer reflective film include a sputtering method in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and sputtering is performed, and an ion beam sputtering method in which an ion beam is irradiated onto a target. Sputtering methods include a DC sputtering method in which a direct current voltage is applied to a target, and an RF sputtering method in which a high frequency voltage is applied to a target. The sputtering method is a film formation method that utilizes the sputtering phenomenon caused by gas ions, which are generated by ionizing a gas by applying a voltage to a target with a sputtering gas introduced into a chamber, and magnetron sputtering is particularly advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering in which a negative bias applied to the target is reversed for a short period of time to prevent the target from charging up.
[0030] The multilayer reflective film can be formed by a sputtering method using, for example, a sputtering device capable of mounting a plurality of targets. Specifically, the target can be appropriately selected from a molybdenum (Mo) target for forming a layer containing molybdenum (Mo) and a silicon (Si) target for forming a layer containing silicon (Si), and the target can be formed by using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas.
[0031] In addition, when sputtering is reactive sputtering using a reactive gas, for example, when forming a film containing nitrogen (N), nitrogen (N 2 When forming a film containing oxygen (O), a nitrogen-containing gas such as oxygen (O 2 When forming a film containing nitrogen (N) and oxygen (O), nitrous oxide (N 2 O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO 2 When forming a film containing carbon (C) and oxygen (O), carbon monoxide (CO) gas, carbon dioxide (CO 2 When forming a film containing carbon oxide gas such as SiO2 gas, or hydrogen (H2O), 2 ) gas, and methane (CH 4 ) gas may be used in conjunction with a rare gas.
[0032] Furthermore, when forming a layer containing boron (B), a molybdenum (Mo) target with boron (B) added (molybdenum boride (MoB) target), a silicon (Si) target with boron (B) added (silicon boride (SiB) target), or the like can be used.
[0033] The protective film is a film for protecting the multilayer reflective film. The protective film is provided in contact with the multilayer reflective film. The protective film is formed of a material containing ruthenium (Ru). Examples of the material containing ruthenium (Ru) include ruthenium (Ru) alone, and an alloy of ruthenium (Ru) and a metal or semimetal different from ruthenium (Ru). Examples of the metal or semimetal different from ruthenium (Ru) include niobium (Nb), zirconium (Zr), titanium (Ti), chromium (Cr), and silicon (Si). Examples of the material containing ruthenium (Ru) are particularly preferably ruthenium (Ru) alone and an alloy of ruthenium (Ru) and niobium (Nb). The content of the metal or semimetal different from ruthenium (Ru) in the protective film is preferably 30 atomic % or less, more preferably 20 atomic % or less, on average throughout the film. The lower limit of the content of the metal or metalloid other than ruthenium (Ru) in the protective film is not particularly limited, but is preferably 5 atomic % or more, and more preferably 10 atomic % or more.
[0034] The protective film may be a single layer structure or a multilayer structure in which multiple layers with different compositions are combined, and each layer constituting the single layer or multiple layers may have a gradient composition structure in which the composition changes continuously in the thickness direction. In particular, one or both of the side of the protective film closest to the multilayer reflective film (in the case of a multilayer structure, the layer closest to the multilayer reflective film) and the side furthest from the multilayer reflective film (in the case of a multilayer structure, the layer furthest from the multilayer reflective film) may be made of ruthenium (Ru).
[0035] In addition, when the protective film has a multilayer structure or a gradient composition structure, it is preferable that the content of a metal or metalloid other than ruthenium (Ru) increases from the multilayer reflective film side toward the side away from the multilayer reflective film in a part or all of the thickness direction of the protective film. In particular, when niobium (Nb) is contained as a metal or metalloid other than ruthenium (Ru), the inclusion of niobium (Nb) is also effective in improving resistance to dry etching using a gas containing chlorine and oxygen, so it is preferable that the content of niobium (Nb) increases from the multilayer reflective film side toward the side away from the multilayer reflective film in a part or all of the thickness direction of the protective film.
[0036] The thickness of the protective film is preferably 2 nm or more, more preferably 3 nm or more, and is preferably 5 nm or less, more preferably 4 nm or less.
[0037] The protective film can be formed by sputtering using a ruthenium (Ru) target and, if necessary, a metal or semimetal target different from ruthenium (Ru), specifically, a niobium (Nb) target, a zirconium (Zr) target, a titanium (Ti) target, a chromium (Cr) target, a silicon (Si) target, etc., as a target, and using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas. Magnetron sputtering is preferable for sputtering.
[0038] The absorber film is a film that absorbs the exposure light and reduces the reflectance in the reflective mask. The absorber film is provided in contact with the protective film. The absorber film is a film that absorbs the EUV light, which is the exposure light, and reduces the reflectance of the exposure light. In the reflective mask, a transfer pattern is formed by the difference in reflectance between the part where the absorber film is formed and the part where the absorber film is not formed.
[0039] The absorber film is formed of a material that absorbs EUV light, is patternable, and contains tantalum (Ta). The material containing tantalum (Ta) may contain oxygen (O), nitrogen (N), carbon (C), boron (B), etc. Examples of the material for the absorber film include materials containing tantalum (Ta), and specific examples of the material include simple Ta and tantalum (Ta) compounds such as TaO, TaN, TaON, TaC, TaCO, TaCN, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCOB, TaCNB, and TaCONB.
[0040] In particular, a material containing tantalum (Ta) and nitrogen (N) is preferred because it has a high etching selectivity in dry etching using a gas containing chlorine and not oxygen, relative to both a protective film formed from a material containing ruthenium (Ru) and a hard mask film formed from a material containing chromium (Cr), and therefore provides good processability during pattern formation of the absorber film. On the other hand, a material containing tantalum (Ta) but not nitrogen (N) is less likely to be etched by dry etching using a gas containing chlorine and oxygen, compared to a material containing tantalum (Ta) and nitrogen (N).
[0041] The absorber film preferably has a microcrystalline structure or an amorphous structure. The absorber film may contain at least one selected from hydrogen (H), boron (B), carbon (C), silicon (Si), molybdenum (Mo), zirconium (Zr), chromium (Cr), germanium (Ge) and aluminum (Al), particularly at least one of carbon (C) and boron (B), as long as the total content of the element is 20 atomic % or less.
[0042] The absorber film of the present invention can be composed of two layers, a first layer and a second layer, from the substrate side. In the case of an absorber film with a two-layer structure, it is preferable that the first layer has a composition containing tantalum (Ta) but not nitrogen (N), and the second layer has a composition containing tantalum (Ta) and nitrogen (N).
[0043] The first layer preferably contains oxygen (O). When oxygen (O) is contained, the resistance to dry etching using a gas containing chlorine and oxygen is high, but on the other hand, even if the absorber film remains in a portion other than the pattern of the absorber film on the protective film, if only a small amount of the absorber film remains, it is advantageously removed by cleaning with sulfuric acid / hydrogen peroxide (SPM). When the first layer contains oxygen (O), the content of oxygen (O) is preferably 5 atomic % or more, more preferably 20 atomic % or more, and even more preferably 50 atomic % or more. The upper limit of the content of oxygen (O) is not particularly limited, but is preferably 71.4 atomic % or less.
[0044] The thickness of the first layer is preferably 2 nm or less, and more preferably 0.5 nm or more, and more preferably 1 nm or more. If the first layer is too thick, when forming a pattern of the absorber film, the absorber film may remain on the protective film in a portion other than the absorber film pattern, which may reduce the reflectance of the reflective mask.
[0045] The second layer is preferably easily etched by dry etching using a gas containing chlorine but not oxygen. Therefore, the nitrogen (N) content of the second layer is preferably 10 atomic % or more, more preferably 15 atomic % or more, and even more preferably 30 atomic % or more. The upper limit of the nitrogen (N) content is preferably 60 atomic % or less, more preferably 45 atomic % or less. The oxygen (O) content of the second layer is preferably 5 atomic % or less, and it is more preferable that the second layer does not contain oxygen (O). On the other hand, the tantalum (Ta) content of the second layer is preferably 40 atomic % or more, more preferably 55 atomic % or more, and also preferably 90 atomic % or less, more preferably 70 atomic % or less.
[0046] The total thickness of the first layer and the second layer is preferably 50 nm or more, more preferably 55 nm or more, and is preferably 80 nm or less, more preferably 70 nm or less. The first layer and the second layer can be etched by dry etching using a gas containing chlorine and not containing oxygen.
[0047] The absorber film may have a two-layer structure, but if the part of the absorber film farthest from the protective film contains oxygen, the reflectance of the inspection wavelength during defect inspection performed during mask processing decreases. Therefore, the absorber film can be provided with a third layer farthest from the protective film, and the absorber film can be composed of three layers, the first layer, the second layer, and the third layer from the substrate side. In this case, it is preferable that the third layer has a composition containing tantalum (Ta), nitrogen (N), and oxygen (O).
[0048] The oxygen (O) content of the third layer is preferably 30 atomic % or more, more preferably 50 atomic % or more, and preferably 70 atomic % or less. The tantalum (Ta) content of the third layer is preferably 30 atomic % or more, more preferably 40 atomic % or more, and preferably 70 atomic % or less, more preferably 60 atomic % or less. On the other hand, the nitrogen (N) content of the third layer is preferably 50 atomic % or less, more preferably 40 atomic % or less. The lower limit of the nitrogen (N) content is not particularly limited, but is preferably 5 atomic % or more, more preferably 10 atomic % or more.
[0049] The thickness of the third layer is preferably 20 nm or less, more preferably 10 nm or less, and even more preferably 5 nm or less. The lower limit of the thickness of the third layer is not particularly limited, but is preferably 1 nm or more, and more preferably 3 nm or more. The third layer can be etched by dry etching using a fluorine-based gas (fluorine-based dry etching).
[0050] The sheet resistance of the absorber film is preferably 1×10 6 Ω / □ or less, more preferably 1×10 5 The surface roughness Sq of the absorber film is preferably 0.8 nm or less, and more preferably 0.6 nm or less.
[0051] The absorber film (each layer constituting the absorber film) can be formed by sputtering, and magnetron sputtering is preferred. Specifically, a tantalum (Ta) target or a tantalum (Ta) compound target (a target containing tantalum (Ta) and oxygen (O), nitrogen (N), carbon (C), boron (B), or the like) is used, and a rare gas such as helium (He) gas, neon (Ne) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas is used as a sputtering gas. Alternatively, a rare gas may be used in combination with an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas, specifically, oxygen (O 2 ) gas, nitrogen (N 2 ) gas, nitrogen oxide (N 2 O, NO, NO 2 ) gas, carbon oxide (CO, CO 2 The film can be formed by reactive sputtering using a reactive gas such as a SiO 2 gas.
[0052] Among the layers constituting the absorber film, a part of the third layer on the side furthest from the protective film of the second layer is oxidized by oxygen (O 2 Alternatively, after forming the second layer, a part of the second layer on the side farthest from the protective film may be oxidized by natural oxidation in a gas atmosphere containing oxygen (O 2 Alternatively, the insulating layer may be formed by oxidizing the insulating layer by heat treatment in a gas atmosphere containing the .alpha.-nitrogen sulphide (N) gas.
[0053] A hard mask film (an etching mask film for the absorber film) having etching characteristics different from those of the absorber film can be provided on the side of the absorber film that is away from the substrate. This hard mask film functions as an etching mask when the absorber film is dry-etched. The hard mask film is provided in contact with the absorber film.
[0054] The material of the hard mask film may be a material containing chromium (Cr). When processing an absorber film formed of a material containing tantalum (Ta), the material containing chromium (Cr) has different etching characteristics from the absorber film, and a hard mask film formed of a material containing chromium (Cr) that functions as an etching mask when dry etching the absorber film is preferable. Therefore, it is preferable that the material of the hard mask film does not contain tantalum (Ta).
[0055] Examples of materials containing chromium (Cr) include CrO, CrN, CrON, CrC, CrOC, CrNC, and CrONC. In the process of manufacturing a reflective mask, a hard mask film formed of a material containing chromium (Cr) is usually removed by dry etching using a gas containing chlorine and oxygen. Therefore, a hard mask film having a high etching rate in such dry etching is preferable, and from this viewpoint, CrONC is more preferable as a material containing chromium (Cr). The content of chromium (Cr) in a hard mask film formed of a material containing chromium (Cr) is preferably 60 atomic % or less, more preferably 50 atomic % or less, and also preferably 30 atomic % or more, more preferably 40 atomic % or more.
[0056] After forming the absorber film pattern, the hard mask film may be left on the reflective mask as a reflectance reducing layer for reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection, or may be removed so that it does not remain on the reflective mask. A hard mask film formed of a material containing chromium (Cr) is particularly suitable when the absorber film is formed of a material containing tantalum (Ta) but not containing chromium (Cr).
[0057] The hard mask film can be formed on the second layer of the absorber film. In addition, when the absorber film has a third layer having a function of reducing the reflectance at the wavelength of light used in inspection such as pattern inspection, the hard mask film can be formed on the third layer of the absorber film. The hard mask film can be formed, for example, by magnetron sputtering. The thickness of the hard mask film is not particularly limited, but if it is too thin, it may not function as an etching mask, and if it is too thick, the processing characteristics may deteriorate, so that it is preferably 5 nm or more, and preferably 20 nm or less, more preferably 10 nm or less.
[0058] The hard mask film can be formed by sputtering, preferably magnetron sputtering. Specifically, a chromium (Cr) target or a chromium compound target (a target containing Cr, oxygen (O), nitrogen (N), carbon (C), boron (B), or the like) is used, and a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas is used as a sputtering gas. Alternatively, a rare gas may be used in combination with an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas, specifically, oxygen (O 2 ) gas, nitrogen (N 2 ) gas, nitrogen oxide (N 2 O, NO, NO 2 ) gas, carbon oxide (CO, CO 2 The film can be formed by reactive sputtering using a reactive gas such as a SiO 2 gas.
[0059] A conductive film used for electrostatically chucking the reflective mask to an exposure device may be provided on the other main surface (rear surface) of the substrate, which is the surface opposite to the one main surface, preferably in contact with the other main surface.
[0060] The conductive film preferably has a sheet resistance of 100Ω / □ or less, and there is no particular restriction on the material. Examples of the material of the conductive film include materials containing tantalum (Ta) or chromium (Cr). In addition, the materials containing tantalum (Ta) or chromium (Cr) may contain oxygen (O), nitrogen (N), carbon (C), boron (B), and the like. Examples of materials containing tantalum (Ta) include Ta alone, and tantalum (Ta) compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing chromium (Cr) include Cr alone, and chromium (Cr) compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.
[0061] The thickness of the conductive film is not particularly limited as long as it functions as an electrostatic chuck, but is usually about 20 to 300 nm. The thickness of the conductive film is preferably formed so that the film stress is balanced with the multilayer reflective film, the protective film, and the absorber film pattern after forming the reflective mask, that is, after forming the absorber film pattern. The conductive film may be formed before forming the multilayer reflective film, or after forming all the films on the multilayer reflective film side of the substrate, or after forming a part of the film on the multilayer reflective film side of the substrate, the conductive film may be formed, and then the remaining film on the multilayer reflective film side of the substrate may be formed. The conductive film can be formed, for example, by magnetron sputtering.
[0062] The reflective mask blank of the present invention may have a resist film formed on the side farthest from the substrate. The resist film is preferably an electron beam (EB) resist.
[0063] From the reflective mask blank, for example, a reflective mask can be manufactured having a substrate, a multilayer reflective film formed on one main surface of the substrate, a protective film formed in contact with the multilayer reflective film, and an absorber pattern (absorber film pattern) formed in contact with the protective film by patterning an absorber film. In the reflective mask, a transfer pattern is formed due to the difference in reflectance between a portion where the absorber film is formed and a portion where the absorber film is not formed.
[0064] A hard mask film formed of a material containing chromium (Cr) can be dry-etched using a gas containing chlorine and oxygen to form a pattern of the hard mask film (hard mask pattern). A absorber film formed of a material containing tantalum (Ta) can be dry-etched using a gas containing chlorine and not containing oxygen to form a pattern of the absorber film (absorber pattern). During this etching, the pattern of the hard mask film functions as an etching mask. After the absorber pattern is formed, the hard mask pattern can be removed by dry etching using a gas containing chlorine and oxygen. After the hard mask pattern is removed, the absorber film remaining in the portion other than the absorber pattern and the exposed protective film can be subjected to a process of contact with sulfuric acid / hydrogen peroxide (SPM), for example, cleaning with sulfuric acid / hydrogen peroxide (SPM).
[0065] Specifically, the reflective mask of the present invention comprises: (A) preparing a reflective mask blank; (B) forming a resist pattern on the hard mask film; (C) dry etching the hard mask film using a gas containing chlorine and oxygen, with the resist pattern as an etching mask, to form a pattern of the hard mask film; (D) dry etching the first layer and the second layer of the absorber film using a gas containing chlorine and not containing oxygen, with the pattern of the hard mask film as an etching mask, to form a pattern of the first layer and the second layer of the absorber film; (E) after step (C) or (D), a step of removing the resist pattern; (F) removing the pattern of the hard mask film by dry etching using a gas containing chlorine and oxygen; The method can be produced by a method comprising the steps of:
[0066] The protective film can be dry etched in step (D) so as to expose the protective film. Also, the protective film can be dry etched in step (D) so as to leave a part of the absorber film, preferably a part or all of the first layer, and not to expose the protective film, and can be dry etched in step (F) so as to expose the protective film.
[0067] The method for producing a reflective mask of the present invention may further include, after steps (G) and (F), a step including a treatment in which the exposed protective film is brought into contact with sulfuric acid / hydrogen peroxide (SPM).
[0068] In the manufacturing method of the reflective mask of the present invention, when the process (G) is included, in the processes (D) and (F), dry etching may be performed so that a part of the absorber film does not remain and the protective film is not exposed, and in the process (G), the protective film may be exposed.
[0069] When the absorber film is composed of three layers, that is, a first layer, a second layer, and a third layer from the substrate side, Furthermore, (C-1) after the step (C) and before the step (D), a step of dry etching the third layer of the absorber film using a fluorine-based gas and the pattern of the hard mask film as an etching mask to form a pattern of the third layer of the absorber film. It is preferred that the compound contains EXAMPLES
[0070] The present invention will be described in detail below with reference to Experimental Examples and Comparative Experimental Examples, but the present invention is not limited to the following Examples.
[0071] [Experimental Example 1] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A RuNb film (Ru:Nb=82:18 (atomic ratio)) was formed as a protective film (thickness 3.9 nm) on the main surface of a tungsten-based glass substrate. The RuNb film was formed by placing the low-thermal expansion glass substrate in the chamber of a multi-cathode sputtering device equipped with a Ru target and a Nb target, and by DC pulse magnetron sputtering while rotating the substrate. The RuNb film was formed by introducing Ar gas (flow rate: 10 sccm) into the chamber, setting the pressure in the chamber to 0.016 Pa, and applying a power of 400 W to the Ru target and 200 W to the Nb target.
[0072] Next, a 1.0 nm thick TaO layer (Ta:O=70:30 (atomic ratio)) and a 59.0 nm thick TaN layer (Ta:N=57:43 (atomic ratio)) were formed in this order on the RuNb film as an absorber film (thickness 60.0 nm) to obtain a film-coated substrate for evaluation. The TaO layer and TaN layer were formed by placing the substrate on which the RuNb film was formed in the chamber of another sputtering device equipped with a Ta target, and by DC pulse magnetron sputtering while rotating the substrate. The TaO layer was formed by sputtering Ar gas (flow rate: 40 sccm) and O 2 The TaN layer was formed by applying a power of 1,000 W to the Ta target while introducing Ar gas (flow rate: 70 sccm) and N 2 Gas (flow rate: 120 sccm) was introduced, the pressure inside the chamber was set to 0.48 Pa, and a power of 1,800 W was applied to the Ta target to form the film.
[0073] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0074] [Experimental Example 2] A substrate with a film for evaluation was obtained in the same manner as in Experimental Example 1, except that the TaO layer was a 1.5 nm thick TaO layer (Ta:O=80:20 (atomic ratio)) and the TaN layer was 58.5 nm thick. The TaO layer was formed by evaporating Ar gas (flow rate: 40 sccm) and O 2 Gas (flow rate: 30 sccm) was introduced, the pressure inside the chamber was set to 0.14 Pa, and a power of 1,800 W was applied to the Ta target to form the film.
[0075] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0076] [Experimental Example 3] Except for replacing the TaO layer with a Ta layer having a thickness of 1.5 nm, a film-coated substrate for evaluation was obtained in the same manner as in Experimental Example 2. The Ta layer was formed by introducing Ar gas (flow rate: 18 sccm) into the chamber, setting the pressure inside the chamber to 0.07 Pa, and applying a power of 500 W to the Ta target.
[0077] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0078] [Comparative Experiment Example 1] A film-coated substrate for evaluation was obtained in the same manner as in Experimental Example 1, except that the TaO layer was not formed and the thickness of the TaN layer was set to 60.0 nm.
[0079] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0080] [Experimental Example 4] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A Ru film was formed as a protective film (thickness 3.9 nm) on the main surface of a low-thermal expansion glass substrate (a tungsten-based glass substrate). The Ru film was formed by placing the low-thermal expansion glass substrate in the chamber of a sputtering device equipped with a Ru target, and by DC pulse magnetron sputtering while rotating the substrate. The Ru film was formed by introducing Ar gas (flow rate: 10 sccm) into the chamber, setting the pressure inside the chamber to 0.016 Pa, and applying 400 W of power to the Ru target.
[0081] Next, a 2.0 nm thick TaO layer (Ta:O=60:40 (atomic ratio)) and a 58.0 nm thick TaN layer (Ta:N=57:43 (atomic ratio)) were formed in this order on the Ru film as an absorber film (thickness 60.0 nm) to obtain a film-coated substrate for evaluation. The TaO layer and TaN layer were formed by placing the substrate on which the Ru film was formed in the chamber of another sputtering device equipped with a Ta target, and by DC pulse magnetron sputtering while rotating the substrate. The TaO layer was formed by sputtering Ar gas (flow rate: 15 sccm) and O 2 The TaN layer was formed by applying a power of 500 W to the Ta target while introducing Ar gas (flow rate: 70 sccm) and N 2 Gas (flow rate: 120 sccm) was introduced, the pressure inside the chamber was set to 0.48 Pa, and a power of 1,800 W was applied to the Ta target to form the film.
[0082] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0083] [Comparative Experiment Example 2] A film-coated substrate for evaluation was obtained in the same manner as in Experimental Example 4, except that the TaO layer was not formed and the thickness of the TaN layer was set to 60.0 nm.
[0084] When the substrate with the resulting protective film and absorber film formed thereon was removed from the chamber into the atmosphere, it was confirmed that a TaON layer (Ta:O:N = 40:30:30 (atomic ratio), thickness 1.0 nm) formed by natural oxidation was formed on the surface portion of the TaN layer furthest from the protective film.
[0085] <Evaluation of protective film and absorber film> The evaluation film-coated substrates obtained in the experimental examples and comparative experimental examples were subjected to the following treatments (i) to (iii) in order, and the thickness of the film remaining on the substrate was measured after each of treatments (i), (ii), and (iii). The film thickness was measured using an X-ray diffraction device (SmartLab, manufactured by Rigaku Corporation). The results are shown in Table 1.
[0086] First, in order to remove the TaON layer, dry etching was carried out using a fluorine-based gas.
[0087] The etching was carried out under the following conditions using the etching apparatus shown in Fig. 3. Fig. 3 is a schematic diagram of the dry etching apparatus (same for the following dry etching) used for dry etching, and the dry etching apparatus 100 includes a chamber 101, an earth 102, a lower electrode 103, an antenna coil 104, and high frequency power sources RF1 and RF2. In this case, a substrate to be processed (substrate with a film for evaluation) 105 is placed on the lower electrode 103.
[0088] <Conditions for dry etching using fluorine-based gas> RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 54W RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 325W Pressure: 5mTorr (0.67Pa) science fiction 6 :18sccm He: 130sccm Processing time: 10 seconds
[0089] (i) Dry etching using a gas that contains chlorine but does not contain oxygen The etching was carried out under the following conditions using the etching apparatus shown in Fig. 3. During etching, the emission spectrum from the plasma was measured using an optical emission spectrometer (OES) equipped in the etching apparatus, and the intensity of the emission from nitrogen (N) was monitored. The point at which the intensity of the emission from nitrogen (N) began to decrease was automatically detected as the endpoint, and the processing time was determined to be 120% of the time (t), which was the time from the start of etching to the endpoint, with 20% added as an overetching time. The processing times are shown in Table 1.
[0090] <Etching conditions for process (i)> RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 625V RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 300W Pressure: 5mTorr (0.67Pa) Cl 2 :150sccm He: 10sccm
[0091] (ii) Dry etching using gases containing chlorine and oxygen The etching was carried out using the etching apparatus shown in FIG. 3 under the following conditions.
[0092] <Etching conditions for treatment (ii)> RF1 (RIE: Reactive Ion Etching): CW (Continuous Discharge) 625V RF2 (ICP: Inductively Coupled Plasma): CW (Continuous Discharge) 300W Pressure: 5mTorr (0.67Pa) Cl 2 :150sccm O 2 :30sccm He: 10sccm Processing time: 20 seconds
[0093] (iii) Sulfuric acid peroxide (SPM) cleaning The evaluation film-coated substrate was immersed in sulfuric acid / hydrogen peroxide (SPM), a mixture of 90% by mass sulfuric acid and 30% by mass hydrogen peroxide (sulfuric acid:hydrogen peroxide = 3:1 (volume ratio)), at room temperature (25°C) for 6 minutes.
[0094] [Table 1]
[0095] In the evaluation film-coated substrates not having a first layer (Comparative Experimental Examples 1 and 2), the thickness of the protective film is reduced after process (i), whereas in the evaluation film-coated substrates having a first layer (Experimental Examples 1 to 4), the protective film is able to remain at approximately the same thickness as when it was formed after process (i).
[0096] The processing time for the process (i) of the evaluation film-coated substrate having an absorber film having a TaO layer as the first layer (Experimental Examples 1, 2, and 4) was longer than that for the evaluation film-coated substrate not having a first layer (Comparative Experimental Examples 1 and 2). This is thought to be because nitrogen (N) diffuses from the TaN layer to the interface between the TaO layer and the TaN layer to form a TaON layer, which delays the detection of the etching endpoint.
[0097] In the evaluation film-coated substrates having a first layer (Experimental Examples 1 to 4), the film loss due to process (i) was smaller than that in the evaluation film-coated substrates not having a first layer (Comparative Experimental Examples 1 and 2). In particular, in Experimental Examples 2 to 4, a part of the absorber film (a part of the first layer) remained after process (i).
[0098] In the evaluation film-coated substrates (Experimental Examples 1 to 3, Comparative Experimental Example 1) in which the protective film is a RuNb film, there is no film loss due to process (ii) in Experimental Examples 1 to 3, but in Experimental Example 1 and Comparative Experimental Example 1, in which the protective film (RuNb film) is exposed after process (i), there is a greater film loss due to process (iii) compared to Experimental Examples 2 to 4 in which part of the absorber film (part of the first layer) remains after process (i).
[0099] In the evaluation film-coated substrates (Experimental Example 4, Comparative Experimental Example 2) in which the protective film is a Ru film, in Experimental Example 4, where part of the absorber film (part of the first layer) remains after process (i), there is no film loss due to process (ii), but in Comparative Experimental Example 2, in which the protective film (Ru film) is exposed after process (i), there is an extremely large film loss due to process (ii).
[0100] In Experimental Example 1 and Comparative Experimental Example 1, in which the protective film (RuNb film) was exposed after process (i) on a film-coated substrate for evaluation having a RuNb protective film, the film loss due to process (iii) was greater than in Comparative Experimental Example 2, in which the protective film (Ru film) was exposed after process (i) on a film-coated substrate for evaluation having a Ru protective film, whereas in Experimental Examples 2 to 4, in which the protective film was a RuNb film but part of the absorber film (part of the first layer) remained after process (i), the film loss due to process (iii) was less. [Explanation of symbols]
[0101] 1 Board 2 Multilayer reflective film 3 Protective film 4. Absorber membrane 41 First Layer 42 Second Layer 43 Third Layer 5. Hard mask film 11, 12 Reflective mask blanks 100 Dry Etching Equipment 101 Chamber 102 Earth 103 Lower electrode 104 antenna coil, 105 Substrate to be processed (substrate with film for evaluation) RF1, RF2 High frequency power supply
Claims
1. A reflective mask blank comprising: a substrate; a multilayer reflective film formed on one main surface of the substrate and reflecting exposure light; a protective film formed on and in contact with the multilayer reflective film; an absorber film formed on and in contact with the protective film and absorbing exposure light; and a hard mask film formed on and in contact with the absorber film and functioning as an etching mask when dry etching the absorber film, the hard mask film being formed on and in contact with the absorber film, the reflective mask blank being a material for a reflective mask used in EUV lithography using EUV light as exposure light, The protective film is formed of a material containing ruthenium (Ru) and has a thickness of 2 nm to 5 nm, the absorber film is formed of a material containing tantalum (Ta) and is composed of two layers, a first layer and a second layer, or three layers, a first layer, a second layer, and a third layer, from the substrate side; the first layer has a composition containing tantalum (Ta) and not containing nitrogen (N) and has a thickness of 0.5 nm or more and 2 nm or less; the second layer has a composition containing tantalum (Ta) and nitrogen (N), the nitrogen (N) content being 10 atomic % or more and the oxygen (O) content being 5 atomic % or less; a total thickness of the first layer and the second layer is 50 nm or more and 80 nm or less; the third layer has a composition containing tantalum (Ta), nitrogen (N) and oxygen (O), the content of oxygen (O) being 30 atomic % or more and 70 atomic % or less, and has a thickness of 20 nm or less; The hard mask film is made of a material containing chromium (Cr) and has a thickness of 5 nm to 20 nm. A reflective mask blank comprising:
2. 2. The reflective mask blank according to claim 1, wherein the composition of the first layer further contains oxygen (O).
3. 3. The reflective mask blank according to claim 2, wherein the first layer has a composition in which the oxygen (O) content is 5 atomic % or more.
4. 2. The reflective mask blank according to claim 1, characterized in that in the composition of the second layer, the tantalum (Ta) content is 55 atomic % or more and 70 atomic % or less, and the nitrogen (N) content is 30 atomic % or more and 45 atomic % or less.
5. 2. The reflective mask blank according to claim 1, wherein the material containing ruthenium (Ru) is ruthenium (Ru) alone or an alloy of ruthenium (Ru) and niobium (Nb).
6. 6. The reflective mask blank according to claim 5, wherein the alloy of ruthenium (Ru) and niobium (Nb) has an average niobium (Nb) content of 30 atomic % or less throughout the protective film.
7. (A) preparing a reflective mask blank according to claim 1; (B) forming a resist pattern on the hard mask film; (C) dry-etching the hard mask film using a gas containing chlorine and oxygen, with the resist pattern as an etching mask, to form a pattern of the hard mask film; (D) dry-etching the first and second layers of the absorber film using a gas containing chlorine and not containing oxygen, with the pattern of the hard mask film as an etching mask, to form patterns of the first and second layers of the absorber film; (E) removing the resist pattern after the step (C) or (D); (F) removing the pattern of the hard mask film by dry etching using a gas containing chlorine and oxygen; A method for manufacturing a reflective mask comprising the steps of:
8. 8. The method according to claim 7, wherein in the step (D), dry etching is performed so that the protective film is exposed.
9. In the step (D), dry etching is performed so that a portion of the absorber film does not remain and the protective film is not exposed; 8. The method according to claim 7, wherein in the step (F), dry etching is performed so that the protective film is exposed.
10. Further, after the step (F), a step (G) includes a step of contacting the exposed protective film with sulfuric acid / hydrogen peroxide (SPM). The method according to claim 8 or 9, comprising:
11. Further, after the step (F), a step (G) includes a step of contacting the exposed protective film with sulfuric acid / hydrogen peroxide (SPM). Including, In the steps (D) and (F), dry etching is performed so that a portion of the absorber film does not remain and the protective film is not exposed; The manufacturing method according to claim 7 , wherein in the step (G), the protective film is exposed.
12. the absorber film is composed of three layers, that is, a first layer, a second layer, and a third layer, from the substrate side; Furthermore, (C-1) after the step (C) and before the step (D), a step of dry etching the third layer of the absorber film using a fluorine-based gas and a pattern of the hard mask film as an etching mask to form a pattern of the third layer of the absorber film. The method of claim 7, further comprising:
Citation Information
Patent Citations
Reflective photomask
JP2002122981A
Reflecting type exposure mask, its manufacturing method and semiconductor element
JP2002246299A