Potassium-type or ammonium-type smectite slurry, method of producing the same, and dehydrated cake

By replacing interlayer cations of Na-type smectite with K or NH4 ions and dehydrating the cake, a stable smectite slurry is produced, addressing the poor dispersion stability of non-sodium smectites and reducing manufacturing costs.

JP2024148653AActive Publication Date: 2024-10-18KUNIMINE IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023061985
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-06
Publication Date
2024-10-18
Estimated Expiration
2043-04-06

AI Technical Summary

Technical Problem

Existing smectite minerals with interlayer cations other than sodium ions exhibit poor water swelling properties and dispersion stability, limiting their applications.

Method used

Replace the interlayer cations of Na-type smectite with K or NH4 ions through cation exchange, followed by salt removal and dehydration to produce a dehydrated cake, which can be mixed with water to form a slurry with excellent dispersion stability.

Benefits of technology

The resulting K-type or NH4-type smectite slurry demonstrates enhanced dispersion stability, allowing for stable smectite dispersion in water and reducing manufacturing costs by eliminating the need for drying and pulverizing steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148653000001_ABST
    Figure 2024148653000001_ABST
Patent Text Reader

Abstract

To provide K-type or NH4-type smectite slurry excellent in dispersion stability and a method of producing the same, and dehydrated cake suitable for preparing K-type or NH4-type smectite slurry.SOLUTION: The method of producing K-type or NH4-type smectite slurry includes steps of mixing Na-type smectite and a potassium salt or an ammonium salt, and water to subject the Na-type smectite to cation exchange, subsequently removing the salt, dehydrating the slurry to obtain dehydrated cake, and mixing the dehydrated cake and water to obtain K-type or NH4-type smectite slurry.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a K-type or NH4-type smectite slurry, a method for producing the same, and a dehydrated cake. [Background technology]

[0002] It is known that smectite, a clay mineral, exhibits swelling properties due to the widening of the basal gaps caused by water molecules intercalating in the gaps (basal gaps) between the basal surfaces of aluminosilicate layers (hereinafter also referred to as "crystalline layers"), which are crystalline layered compounds of silicate and aluminate that constitute smectite. In particular, Na-type smectite, in which the interlayer cations (exchangeable cations) of smectite are Na (sodium) ions, has a relatively weak electrical attraction between the crystalline layers due to the presence of Na ions. When Na-type smectite is dispersed in water, water molecules intercalate one after another between the crystalline layers, causing osmotic swelling in which the basal gaps between the crystalline layers expand to 4 nm or more, and further delamination occurs, resulting in infinite swelling. On the other hand, for example, in smectites that have monovalent cations such as K (potassium) ions and NH4 (ammonium) ions, or divalent cations such as Ca (calcium) ions and Mg (magnesium) ions as interlayer cations, the intercalation of water molecules into the basal gaps is limited, and they exhibit crystalline swelling, which is a limited microscopic expansion with a basal spacing of less than 4 nm. It is believed that whether a smectite exhibits osmotic swelling or crystalline swelling is determined by the valence and ionic radius of the interlayer cations, and the smaller the valence of the ion and the smaller the ionic radius, the more likely it is to exhibit osmotic swelling.

[0003] It is known that smectite exhibits various characteristics depending on the type of interlayer cation, and various smectites in which the interlayer cation is a cation other than Na ion can be obtained by performing cation exchange using natural Na-type smectite as a raw material. Cation exchange methods include a method in which Na-type smectite is put into an aqueous solution of a salt containing the target cation and stirred, and a method in which a dispersion of Na-type smectite is passed through a column filled with an exchange resin of the target cation. The cation-exchanged smectite is then dried and crushed, and stored in a powder form. On the other hand, non-Na-type smectite generally has poor water swelling and dispersion stability, and its applications are limited. Therefore, a technology for improving the water swelling and dispersion stability of smectite in which the interlayer cation is a cation other than Na ion is being studied. For example, Patent Document 1 discloses a dry powder of clay in which 70 to 99 mol % of the cations present between layers are hydrogen ions and the secondary particles are rosette-shaped. It has been revealed that the secondary particles of clay obtained by drying the clay in which the interlayer cations have been replaced with hydrogen ions in a specific manner are uniformly finely dispersed in water or a hydrophilic solvent and thicken and swell. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-112568 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a K-type or NH4-type smectite slurry having excellent dispersion stability and a method for producing the same. Another object of the present invention is to provide a dehydrated cake suitable for preparing the K-type or NH4-type smectite slurry. [Means for solving the problem]

[0006] The present inventors have conducted extensive research in view of the above problems. As a result, they have found that a dehydrated cake obtained by replacing interlayer cations of Na-type smectite with K ions or NH4 ions by cation exchange, followed by removal of salts and dehydration can be mixed with water to produce a slurry with excellent dispersion stability of smectite, even though the dehydrated cake is a K-type or NH4-type smectite cake. Based on these findings, the present invention has been completed through further research.

[0007] The above-mentioned object of the present invention has been achieved by the following means. [1] A method for producing a K-type or NH4-type smectite slurry, comprising: mixing Na-type smectite with a potassium salt or an ammonium salt and water to subject the Na-type smectite to cation exchange; removing the salt; dehydrating the mixture to obtain a dehydrated cake; and mixing the dehydrated cake with water to obtain a K-type or NH4-type smectite slurry. [2] The method for producing a K-type or NH4-type smectite slurry according to [1] above, wherein the water content of the dehydrated cake is 70 to 85 mass %. [3] The method for producing a K-type or NH4-type smectite slurry according to [1] or [2] above, wherein the average particle size of the smectite contained in the dehydrated cake is 1000 nm or less. [4] A dehydrated cake of K-type or NH4-type smectite obtained by mixing Na-type smectite with a potassium salt or an ammonium salt and water, subjecting the Na-type smectite to cation exchange, removing the salt, and dehydrating the mixture, the dehydrated cake being intended to be mixed with water to obtain a K-type or NH4-type smectite slurry. [5] The dehydrated cake according to [4] above, wherein the dehydrated cake has a moisture content of 70 to 85 mass %. [6] The dehydrated cake according to [4] or [5], wherein the average particle size of smectite contained in the dehydrated cake is 1000 nm or less. [7] A K-type or NH4-type smectite slurry obtained by mixing the dehydrated cake according to any one of the above [4] to [6] with water. Effect of the Invention

[0008] The K-type or NH4-type smectite slurry of the present invention has excellent dispersion stability. In addition, according to the method for producing the K-type or NH4-type smectite slurry of the present invention, a slurry of K-type or NH4-type smectite having excellent dispersion stability can be obtained. In addition, by mixing the dehydrated cake of the present invention with water, a slurry in which the K-type or NH4-type smectite is stably dispersed in water can be obtained. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph showing X-ray diffraction results of various smectite slurries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The preferred embodiments of the present invention will be described in detail below, but the present invention is not limited to these embodiments except as specified in the present invention.

[0011] [Method for producing K-type or NH4-type smectite slurry] In the method for producing a K-type or NH4-type smectite slurry of the present invention (hereinafter also referred to as the "production method of the present invention"), first, a dehydrated cake containing K-type or NH4-type smectite is produced (hereinafter, the production method of this dehydrated cake is also referred to as the "production method of the dehydrated cake of the present invention").

[0012] <Method of manufacturing dehydrated cake> The method for producing a dehydrated cake of the present invention includes a cation exchange step of exchanging interlayer cations of Na-type smectite with K ions or NH4 ions, a desalting step of removing salts after the cation exchange, and a dehydration step of dehydrating the dehydrated cake after the desalting. The dehydrated cake obtained in the dehydration step is then mixed with water to obtain a K-type or NH4-type smectite slurry having excellent dispersion stability. Each step will be described in detail.

[0013] (Cation exchange process) In the manufacturing method of the present invention, the cation exchange step is a step of mixing Na-type smectite, a potassium salt or an ammonium salt, and water as described above, and exchanging Na ions, which are interlayer cations of Na-type smectite, with K ions or NH4 ions to obtain K-type smectite or NH4-type smectite in the mixed liquid. In the cation exchange step, the above-mentioned "mixing Na-type smectite, a potassium salt or an ammonium salt, and water" means that at least Na-type smectite, potassium salt or ammonium salt, and water are mixed, and the order of mixing is not particularly limited. That is, each may be mixed independently, or any one may be mixed in advance. For example, a potassium salt or an ammonium salt may be mixed with a Na-type smectite aqueous dispersion in which Na-type smectite is dispersed in water in advance, or Na-type smectite may be mixed with an aqueous solution in which potassium salt or ammonium salt is dissolved in water in advance, and further the Na-type smectite aqueous dispersion and the aqueous solution may be mixed. Hereinafter, smectite in which the interlayer cations of Na-type smectite have been ion-exchanged with the desired cations (cations other than Na ions) is also referred to as "cation-exchanged smectite".

[0014] The mixed liquid of the Na-type smectite, the potassium salt or the ammonium salt, and water is preferably subjected to cation exchange while being stirred. From the viewpoint of improving the cation exchange efficiency, the stirring time is preferably 1 to 24 hours. Furthermore, from the viewpoint of further improving the cation exchange efficiency, it is preferable to concentrate or dehydrate the mixed liquid after the stirring, mix the concentrated or dehydrated smectite with the water and the salt (or the aqueous solution), and mix again by stirring. For example, it is preferable to mix the Na-type smectite with the potassium salt or ammonium salt and water two or more times, and more preferably three or more times. The conditions for the concentration or dehydration can be those usually used in the cation exchange process of smectite, and for example, the dehydration conditions described in the desalting process below can also be applied.

[0015] -Na-type smectite- In the present invention, the term "X-type smectite" (X is a type of cation) refers to a smectite in which the amount of X ions (unit: meq / 100g) in the amount of leached cations (i.e., the total amount of leached cations, unit: meq / 100g, the same applies below) is 70% or more (preferably 80% or more, more preferably 90% or more, more preferably 92% or more, and even more preferably 95% or more). For example, the term Na-type smectite refers to a smectite in which the amount of Na ions (unit: meq / 100g) in the amount of leached cations of the smectite is 70% or more (preferably 80% or more, more preferably 90% or more, more preferably 92% or more, and even more preferably 95% or more). In this specification, the amount of leached cations of smectite is measured by the method described in the Examples (improved SFSA method).

[0016] Smectite has a layered structure in which thin plate-like crystals with a thickness of about 1 nm are stacked, and cations such as alkali metals and alkaline earth metals are generally present between the layers of the crystals. In this ion exchange process, the main cations present between the crystal layers of the raw smectite to replace the interlayer cations of the smectite with K ions or NH4 ions are Na ions (i.e., the raw smectite is Na-type smectite). The type of smectite used in the production method of the present invention is not particularly limited, and may be natural smectite or synthetic smectite. Examples of smectite used in the production method of the present invention include montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite, and montmorillonite is preferable.

[0017] -Potassium salt or ammonium salt- Examples of the potassium salt include potassium chloride, potassium acetate, potassium carbonate, potassium sulfate, etc. Examples of the ammonium salt include ammonium chloride, ammonium acetate, ammonium carbonate, ammonium sulfate, etc. The amount of the salt to be mixed is not particularly limited, and by adjusting the amount of the salt, the ratio of the target cation (K ion, NH4 ion) in the leached cations of the obtained cation-exchanged smectite can be appropriately adjusted.

[0018] -water- The water is not particularly limited, and may be, for example, tap water, distilled water, deionized water, etc. From the viewpoint of improving the dispersibility of Na-type smectite and from the viewpoint of obtaining smectite ion-exchanged with the target cation (K ion, NH4 ion) with high purity, the water is preferably deionized water. The amount of water to be mixed can be appropriately set according to the amount of Na-type smectite to be mixed in. For example, the amount of water to be mixed can be set so that the content of Na-type smectite in the mixed liquid is 1 to 10 mass %.

[0019] (Desalination process) The mixed liquid containing the cation-exchanged smectite obtained by the cation exchange step is then subjected to a desalting step. This desalting step can remove the salt mixed in the cation exchange step, ions derived from the salt, and Na ions expelled from between the crystal layers of the smectite by ion exchange. There are no particular limitations on the desalting method, and any ordinary method capable of desalting the mixed liquid can be used. For example, washing with water or desalting using a semipermeable membrane or the like can be used. In this specification, the term "removal" includes both complete removal and reduction. In a preferred embodiment of the present invention, the desalting step can be carried out by washing with water. This washing with water preferably includes a dehydration stage and a running water washing stage. By passing through the dehydration stage and the running water washing stage, salts, ions, etc. liberated in the mixed liquid can be removed with high efficiency. The dehydration stage and the running water washing stage will be described below.

[0020] -Dehydration stage- The dehydration conditions in the dehydration step are not particularly limited as long as they are conditions that can reduce water. For example, natural filtration, reduced pressure filtration, pressure filtration, centrifugal filtration, and other filtration methods can be used, and the filter medium can be a filter medium used in normal filtration.

[0021] The dehydration step forms a dehydrated cake (also referred to as "dehydrated cake A") with a reduced moisture content before desalting (before washing with running water). The moisture content of the dehydrated cake A obtained by the dehydration step is preferably 85% by mass or less, more preferably 82% by mass or less, and even more preferably 80% by mass or less. The moisture content of the dehydrated cake A is usually 50% by mass or more, and from the viewpoint of preventing the dehydrated cake A from drying out, it is practical to make the moisture content 60% by mass or more.

[0022] -Running water cleaning stage- The dehydrated cake A obtained in the dehydration step is then washed by pouring water into it (running water washing) in the running water washing step, thereby removing salt contained in the dehydrated cake A. In this specification, the "running water washing" refers to a method of washing the smectite by passing water through it while maintaining the shape of the cake to some extent by simultaneously pouring and draining water. In the running water washing step, it is preferable to inject water in an amount 100 times or more by mass, more preferably 150 times or more by mass, and even more preferably 200 times or more by mass, based on the smectite (solid content) contained in the dehydrated cake A. Usually, water is injected in an amount 500 times or less by mass. The injected water is preferably drained by natural filtration. For example, when the dewatering in the dehydration step is filtered by reduced pressure filtration or the like, the water can be poured on the filter medium used and filtered naturally. The water injection speed is preferably about the same as the drainage speed. The above-mentioned "desalting step" is completed in the state of a mixed liquid of smectite and water (so-called a state in which the water content is higher than that of the dehydrated cake). That is, the mixed liquid of smectite and water obtained in the desalting step is subjected to a subsequent dehydration step to obtain the target dehydrated cake. Note that the dehydration step subsequent to the desalting step can also remove the remaining salt together with the water, so that the dehydration step can also serve as a desalting treatment. In other words, in the present invention, "removing salts and dehydrating to obtain a dehydrated cake" means to include all methods by which a dehydrated cake from which salts have been removed can be obtained from the mixed liquid after the cation exchange step.

[0023] (Dehydration process) The mixture after the desalting step is then subjected to a dehydration step, which forms a dehydrated cake having a reduced moisture content. The dehydration method in the dehydration step is not particularly limited, and filtration methods such as reduced pressure filtration, pressure filtration, and centrifugal filtration can be used, and as the filter medium, a filter medium used in normal filtration can be used.

[0024] From the perspective of further improving the handleability by reducing the volume, the water content of the dehydrated cake is preferably 85% by mass or less, more preferably 83% by mass or less, and even more preferably 80% by mass or less. Further, from the perspective of further improving the dispersion stability of the K-type or NH4-type smectite contained in the dehydrated cake with respect to water when the dehydrated cake is mixed with water, the water content of the dehydrated cake is preferably 60% by mass or more, more preferably 65% by mass or more, and even more preferably 70% by mass or more.

[0025] <Preparation of K-type or NH4-type smectite slurry> The dehydrated cake obtained through the above dehydration step is mixed with water to obtain a K-type or NH4-type smectite slurry. The K-type or NH4-type smectite contained in this dehydrated cake is excellent in dispersion stability in water. That is, despite the interlayer cations of the smectite being K ions or NH4 ions, the smectite can be redispersed well in water and form a slurry with stable properties. As the water, the same water as that mixed in the above ion exchange step can be used. The solid content concentration of the K-type or NH4-type smectite slurry obtained by mixing the dehydrated cake obtained in the dehydration step and water is not particularly limited and is appropriately set according to the purpose. For example, it can be 0.1 to 5.0% by mass, or can also be 5.0 to 20.0% by mass.

[0026] The mixing of the dehydrated cake and water may be carried out by mixing with water immediately after the production of the dehydrated cake, or may be carried out by mixing with water after the dehydrated cake is manufactured and stored. For example, after the dehydrated cake is manufactured, it can be transported in the state of the dehydrated cake to the site where the slurry is actually used, and then mixed with water and stirred at the site to obtain a slurry. During the storage period, the dehydrated cake is stored without being dried. The storage is preferably carried out so that the dehydrated cake can maintain the above water content, and the storage period is preferably within 5 years, more preferably within 3 years, and even more preferably within 1 year.

[0027] It is practically difficult to directly and appropriately specify the technical features of the K-type or NH4-type smectite slurry of the present invention obtained by mixing the dehydrated cake with water, based on its structure, composition, and properties. Therefore, in the present invention, in order to clarify the invention by clearly indicating the difference from the prior art, the manufacturing method (process) of the K-type or NH4-type smectite slurry is specified.

[0028] [Dehydrated cake] The dehydrated cake of the present invention is a dehydrated cake obtained through the above-mentioned cation exchange step, desalting step, and dehydration step. That is, it is a dehydrated cake of K-type or NH4-type smectite obtained by mixing Na-type smectite, a potassium salt or an ammonium salt, and water, subjecting the Na-type smectite to cation exchange, removing salts, and dehydrating the Na-type smectite, and is a dehydrated cake to be mixed with water to obtain a K-type or NH4-type smectite slurry. Mixing the dehydrated cake with water means mixing the dehydrated cake with water without drying it.

[0029] The dehydrated cake of the present invention is excellent in dispersion stability in water, even though it is a dehydrated cake of K-type or NH4-type smectite. K-type or NH4-type smectite is known to have poor dispersion stability in water, but the dehydrated cake of the present invention can be mixed with water as it is without drying to obtain a slurry of K-type or NH4-type smectite with excellent dispersion stability. The reason for this is unclear, but the following is considered. When Na-type smectite is dispersed in water and cation exchange is performed, it is presumed that the resulting cation-exchanged smectite maintains a state of interlayer peeling to some extent immediately after cation exchange, since the Na-type smectite is dispersed in water. In particular, when the interlayer cation is K ion or NH4 ion, it is considered that the crystal layers are difficult to stack even if they are aligned because the electric attraction is relatively weak compared to divalent cations. Therefore, even if the smectite is closely approached by subsequent dehydration, it can maintain the peeled state as long as a certain degree of water content is maintained, and it is considered that the dispersion stability in water is excellent. In addition, in the case of cation-exchanged smectite in which the cation is a divalent cation rather than K ion or NH4 ion, even if a dehydrated cake is obtained by the same method as above, the dispersion stability in water is poor as shown in the [Example] section described later.

[0030] In the present invention, "having dispersion stability" and "excellent dispersion stability" mean, for example, that no or almost no free water is generated even when smectite is dispersed in water and allowed to stand. As an example, when smectite is mixed with water to a solid content of 3 mass% to form a slurry, and the slurry is allowed to stand overnight at 25°C, if the rate of free water generated is 5% or less, the smectite can be evaluated as "having dispersion stability" and "excellent dispersion stability". The rate of free water can be calculated by the following (Equation 1). The "free water" refers to the supernatant when the slurry is allowed to stand and phase-separated. Percentage of free water (%) = [volume of free water / total volume of dispersion] × 100 (Equation 1) When the dehydrated cake of the present invention is mixed with water to evaluate the proportion of free water, the proportion of free water is preferably 5% or less, more preferably 3% or less, more preferably 1% or less, and even more preferably 0% (no free water is generated).

[0031] (pH) From the viewpoint of further improving the dispersion stability in water, the dehydrated cake of the present invention preferably has a pH of 6.5 to 10.5, more preferably 7.0 to 9.0, and even more preferably 7.0 to 8.5, when dispersed in water at a concentration of 2.0% by mass (25°C). The pH can be measured, for example, using a personal pH meter (model number: SPH71, manufactured by Sanshosha).

[0032] (conductivity) From the viewpoint of further improving the dispersion stability in water, the dehydrated cake of the present invention has a conductivity of preferably 600 μS / cm or less, more preferably 300 μS / cm or less, and even more preferably 150 μS / cm or less when dispersed in water at a concentration of 2.0 mass % (25° C.). The conductivity can be measured, for example, using an electric conductivity meter (model number: ES-51, manufactured by Horiba, Ltd.).

[0033] (Average particle size) In the dehydrated cake of the present invention, the average particle size of the smectite is preferably 2000 nm or less, more preferably 1500 nm or less, and even more preferably 1000 nm or less. The average particle size is usually 200 nm or more. The average particle size is a cumulant diameter obtained by cumulant analysis. The average particle size of the smectite in the dehydrated cake can be measured according to a conventional method. For example, it can also be measured by the method described in the Examples.

[0034] The dehydrated cake of the present invention can be redispersed well in water to form a slurry with stable properties, even though the interlayer cations of the smectite are K ions or NH4 ions. Therefore, the cake can be stored and transported in a state in which the volume is reduced by filtration, and can be redispersed in water when necessary to form a stable slurry for various applications. In addition, since a drying and grinding process is not required, the production cost can be reduced. EXAMPLES

[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0036] <Experimental Example 1: Production of dehydrated cake> Example 1 -Cation exchange process- To 1000 ml of a 0.7 mol / l aqueous potassium chloride solution (potassium chloride: special grade, manufactured by Kanto Chemical Co., Ltd.), 50 g (0.5 mass%) of Na-type smectite (product name: Kunipia F, manufactured by Kunimine Industries Co., Ltd.) was added to prepare a mixed solution, which was stirred at 25° C. overnight. The mixed solution after stirring was poured into a Buchner funnel with filter paper (hard filter paper No. 4A, Advantec Co., Ltd.) set, and suction filtration was performed by applying a suction pressure of 700 mmHg (about 93.31 kPa, calculated as 1 mmHg = 0.1333 kPa) with a vacuum pump. The smectite after suction filtration was again poured into 1000 ml of the potassium chloride aqueous solution in its entirety and stirred (second time), and then suction filtration was performed. The smectite after suction filtration was again poured into 1000 ml of the potassium chloride aqueous solution in its entirety and stirred (third time), obtaining a mixed solution containing K-type smectite in which the interlayer cations of the smectite were cation-exchanged from Na ions to K ions.

[0037] -Desalination process- After the cation exchange step was completed (after the third stirring), suction filtration was performed in the same manner as described above (dehydration step). Before the surface of the smectite after suction filtration dried, 10 L of distilled water was slowly poured on top of the smectite to perform running water washing (filtration washing by natural filtration) (running water washing step).

[0038] -Dehydration process- Thereafter, the mixture was dehydrated by suction filtration under the same conditions as above to obtain a dehydrated cake of K-type smectite.

[0039] The degree of dehydration, desalting and cation exchange of the obtained dehydrated cake was confirmed by the following methods.

[0040] -Moisture content of dehydrated cake- A part of the dehydrated cake was weighed, dried in an incubator set at 105° C. for 24 hours, and the weight after drying was measured again to calculate the moisture content (mass%) of the dehydrated cake after suction filtration. The results are shown in Table 1 below.

[0041] -pH, conductivity- A part of the dehydrated cake was dried overnight at 105°C and further pulverized in a cup mill. The dried and pulverized product was dispersed in water to a concentration of 2% by mass to prepare an aqueous dispersion, and the pH and electrical conductivity of the aqueous dispersion were measured. The pH was measured using a personal pH meter (model number: SPH71, manufactured by Sanshosha) and the electrical conductivity was measured using an electrical conductivity meter (model number: ES-51, manufactured by Horiba, Ltd.), and the measurement temperature was room temperature (25°C). As a control sample, smectite powder (Na-type smectite, product name: Kunipia F, manufactured by Kunimine Industries Co., Ltd.) was used as the smectite powder in Reference Example 1, and the pH and conductivity were measured in the same manner as above to prepare an aqueous dispersion. The results are shown in Table 1 below.

[0042] -Cation composition- The interlayer cation composition of each smectite was measured by the improved SFSA method (Jiban Kogaku Journal Vol. 17, No. 1, 61-71) using the dried and pulverized product (dried and pulverized product of the dehydrated cake of Example 1) and the smectite powder of Reference Example 1. The measurement results are shown in Table 1 below.

[0043] Example 2 A dehydrated cake of NH4-type smectite was obtained through the cation exchange process, desalting process, and dehydration process in the same manner as in Example 1 above, except that a 0.7 mol / l aqueous ammonium chloride solution (special grade ammonium chloride, manufactured by Kanto Chemical Co., Ltd.) was used instead of the 0.7 mol / l aqueous potassium chloride solution. The moisture content, pH, and electrical conductivity of the obtained dehydrated cake were measured in the same manner as above, and the results are shown in Table 1 below.

[0044] Comparative Example 1 A dehydrated cake of Ca-type smectite was obtained through the cation exchange process, desalting process, and dehydration process in the same manner as in Example 1 above, except that a 0.7 mol / l aqueous calcium chloride solution (calcium chloride: special grade, manufactured by Kanto Chemical Co., Ltd.) was used instead of the 0.7 mol / l aqueous potassium chloride solution. The moisture content, pH, electrical conductivity, and interlayer cation composition of the obtained dehydrated cake were measured in the same manner as above. The results are shown in Table 1 below.

[0045] Comparative Example 2 A dehydrated cake of Mg-type smectite was obtained through the cation exchange step, desalting step, and dehydration step in the same manner as in Example 1 above, except that a 0.7 mol / l aqueous magnesium chloride solution (magnesium chloride: special grade, manufactured by Kanto Chemical Co., Ltd.) was used instead of the 0.7 mol / l aqueous potassium chloride solution. The moisture content, pH, and electrical conductivity of the obtained dehydrated cake were measured in the same manner as above, and the results are shown in Table 1 below.

[0046] Comparative Example 3 A dehydrated cake of Cs (cesium)-type smectite was obtained through the cation exchange process, desalting process, and dehydration process in the same manner as in Example 1 above, except that a 0.7 mol / l aqueous cesium chloride solution (special grade cesium chloride, manufactured by Kanto Chemical Co., Ltd.) was used instead of the 0.7 mol / l aqueous potassium chloride solution. The moisture content, pH, and electrical conductivity of the obtained dehydrated cake were measured in the same manner as above, and the results are shown in Table 1 below.

[0047] Comparative Example 4 A dehydrated cake of Al (aluminum) type smectite was obtained through the cation exchange step, desalting step, and dehydration step in the same manner as in Example 1 above, except that a 0.7 mol / l aqueous aluminum chloride solution (special grade aluminum chloride, manufactured by Kanto Chemical Co., Ltd.) was used instead of the 0.7 mol / l aqueous potassium chloride solution.

[0048] <Test Example> The obtained dehydrated cakes of Examples 1 and 2 and Comparative Examples 1 to 4 were subjected to the following tests to evaluate the dispersibility of the dehydrated cakes.

[0049] (X-ray diffraction) The dehydrated cakes of Examples 1 and 2 and Comparative Examples 1 to 3 were applied to the recesses of a slide glass having a recess to flatten the surface, and the slide glass was set in the apparatus, and X-ray diffraction was performed under the following conditions. -X-ray diffraction conditions- X-ray diffraction equipment: Ultima IV, Rigaku Corporation X-ray: 40kV / 20mA Monochromator: Fixed monochromator Divergence slit: 1° Divergence vertical limit slit: 10mm Scattering slit: 1° Receiving slit: 0.3 mm Monochrome receiving slit: 0.8 mm

[0050] The results of X-ray diffraction are shown in Figure 1. In Figure 1, the positions indicated with "*" are 12.5 Å positions, "**" are 15 Å positions, and "***" are 18 Å positions, which correspond to the width of one (12.5 Å), two (15 Å), and three (18 Å) layers of water molecules intercalated between the crystal layers of smectite, respectively. In other words, the peaks at each position indicate the presence of a certain amount of smectite that is not exfoliated and dispersed but is stacked in layers. The presence or absence of peaks due to X-ray diffraction was determined from the distribution in Figure 1. The results are shown in Table 1 below.

[0051] (Free water measurement test) The dehydrated cakes of Examples 1 and 2, Comparative Examples 1 to 4, and the smectite powder of Reference Example 1 were added to water so that the solid content was 3 mass %, and the mixture was stirred at 25°C for 24 hours using a shaker (Yamato Scientific SA300, shaking speed memory 4) to form a uniform slurry (100 mL), which was then transferred to a measuring cylinder and allowed to stand overnight at 25°C to measure the volume of free water generated, and the percentage of free water (%) was calculated using the following formula 1. The results are shown in Table 1 below. Percentage of free water (%) = [volume of free water / total volume of dispersion] × 100 (Equation 1)

[0052] (Average particle size measurement test) The dehydrated cakes of Examples 1 and 2, Comparative Examples 1 and 2, and the smectite powder of Reference Example 1 were added to water so that the solid content was 0.05 mass %, and the mixture was stirred at 25°C for 24 hours using a shaker (Yamato Scientific SA300, shaking speed memory 4) to form a uniform slurry. The average particle size of the smectite in the slurry (cumulant size by cumulant analysis) was measured using a dynamic light scattering device (model number: SZ-100, manufactured by HORIBA). The results are shown in Table 1 below.

[0053] [Table 1]

[0054] The dehydrated cakes of Examples 1 and 2 and Comparative Examples 1 to 3 all had a pH of about 7 to 8, and the electrical conductivity was also reduced compared to that of the smectite powder of Reference Example 1. This indicated that excess ions were sufficiently removed in the "desalting step" in the manufacturing process of the dehydrated cakes. Furthermore, analysis of the cation composition using the smectite powder of Reference Example 1 and the dehydrated cakes of Example 1 and Comparative Example 1 indicated that at least the interlayer cations of the Na-type smectite were replaced with the desired cations by the above method. Furthermore, the moisture content of the obtained dehydrated cakes was 80 mass% or less, and the volume was sufficiently reduced.

[0055] On the other hand, the results of X-ray diffraction using the obtained dehydrated cakes of Examples 1 and 2 and Comparative Examples 1 to 3 showed that Comparative Examples 1 to 3 had sharp peaks at positions of 12.5 Å, 15.0 Å, and 18.0 Å, respectively, as shown in Fig. 1, whereas no sharp peaks were detected in the dehydrated cakes of Examples 1 and 2. That is, it was suggested that the smectite in the dehydrated cakes of Comparative Examples 1 to 3 was ordered and existed in layers, whereas the smectite in the dehydrated cakes of Examples 1 and 2 had low regularity and high dispersion stability. Furthermore, when the dehydrated cakes of Examples 1 and 2, Comparative Examples 1 to 4, and the smectite powder of Reference Example 1 were redispersed in water and allowed to stand, a large amount of free water was generated in Comparative Examples 1 to 4, whereas no free water was generated in Examples 1, 2, and Reference Example 1. Furthermore, whereas the average particle diameter in the aqueous dispersions of Comparative Examples 1 and 2 was 6 μm or more, the average particle diameter in Examples 1 and 2 was as small as 1 μm or less, indicating excellent peelability (dispersion stability).

[0056] <Experimental Example 2: Drying of dehydrated cake> (Comparative Examples 5 and 6) The dehydrated cakes of Examples 1 and 2 were dried overnight at 105° C. and then pulverized in a cup mill, and the resulting dried and pulverized products were designated as Comparative Examples 5 and 6. The moisture contents of the dried and pulverized products of Comparative Examples 5 and 6 were measured in the same manner as above, and were all 8.0% by mass or less.

[0057] The resulting dried and pulverized product was dispersed in water in the same manner as above, and the free water content and average particle size were measured. The results are shown in Table 2 below.

[0058] [Table 2]

[0059] The above results show that the dispersion stability of the dehydrated cake is significantly reduced by subjecting the dehydrated cake to a drying and pulverizing treatment.

Claims

1. The Na-type smectite is mixed with a potassium salt or an ammonium salt and water to subject the Na-type smectite to cation exchange, and then the salt is removed and the resulting mixture is dehydrated to obtain a dehydrated cake. The dehydrated cake is mixed with water to obtain a K-type or NH 4 obtaining a K-type or NH-type smectite slurry; 4 Method for producing smectite slurry.

2. The K-type or NH-type according to claim 1, wherein the moisture content of the dehydrated cake is 70 to 85% by mass. 4 Method for producing smectite slurry.

3. 3. The K-type or NH-type smectite according to claim 1 or 2, wherein the average particle size of the smectite contained in the dehydrated cake is 1000 nm or less. 4 Method for producing smectite slurry.

4. The Na-type smectite is mixed with a potassium salt or an ammonium salt and water, and the Na-type smectite is subjected to cation exchange, and then the salt is removed and dehydrated to obtain a K-type or NH 4 Dehydrated cake of smectite type K or NH type, which is mixed with water 4 Dewatered cake to obtain type smectite slurry.

5. The dehydrated cake according to claim 4, wherein the moisture content of the dehydrated cake is 70 to 85% by mass.

6. 5. The dehydrated cake according to claim 4, wherein the average particle size of smectite contained in the dehydrated cake is 1000 nm or less.

7. A K-type or NH-type sintered product obtained by mixing the dehydrated cake according to any one of claims 4 to 6 with water. 4 Type smectite slurry.

Citation Information

Patent Citations

  • Inkjet recording medium

    JP2008201110A

  • Smectite slurry

    JP2018193276A

  • Mineral Processing

    JP2021506725A

  • Gas barrier structure and film laminate

    WO2020175505A1

  • Clay powder having hydrogen ion existing between layers and method for producing the same

    JP2013112568A