Medium for ultraviolet laser printing, printed matter and method for producing the same, and worked article

A UV laser printing medium with controlled titanium oxide content and crystallite size, along with a protective resin and sealant layer, addresses the issues of cost, visibility, and resin swelling in existing printing technologies, achieving clear and heat-sealable printed matter.

JP2024149010AActive Publication Date: 2024-10-18OJI HLDG CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023062642
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Existing printing methods for packages, such as thermal printers and inkjet printers, are costly and prone to errors, while laser printing methods suffer from poor visibility and environmental contamination issues, and ultraviolet laser methods face challenges with print clarity and resin swelling.

Method used

A UV laser printing medium with a specific range of titanium oxide content and crystallite size, combined with a protective resin layer and sealant layer, to achieve clear and heat-sealable printing.

Benefits of technology

The solution provides excellent print clarity and suppresses resin swelling, ensuring high-quality, heat-sealable printed matter with reduced environmental contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149010000006
    Figure 2024149010000006
  • Figure 2024149010000001
    Figure 2024149010000001
  • Figure 2024149010000002
    Figure 2024149010000002
Patent Text Reader

Abstract

To provide a medium for ultraviolet laser printing which can obtain printing spots excellent in printing clarity for one point when being irradiated with an ultraviolet laser beam, can obtain a printed matter where swelling of a protective resin layer is suppressed when being irradiated with an ultraviolet laser beam, and has heat-sealability, a printed matter in which an irradiation region is discolored by irradiating the medium for ultraviolet laser printing with an ultraviolet laser beam and a method for producing the same, and a worked article using the medium for ultraviolet laser printing or the printed matter.SOLUTION: A medium for ultraviolet laser printing has a printed layer containing titanium oxide and a protective resin layer in this order on one surface of a base material, and has a sealant layer on the other surface of the base material, wherein a content of the titanium oxide in the printed layer is 0.1 g / m2 or more and 4.0 g / m2 or less, and a crystallite size of the titanium oxide in the printed layer is 13 nm or more and 53 nm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a medium for ultraviolet laser printing, a printed matter and a method for producing the same, and a processed product. [Background technology]

[0002] 2. Description of the Related Art Conventionally, labeling or inkjet printing has been used to display dates such as manufacturing dates and shipping dates, and variable information such as bar codes, on packaging such as containers that hold contents. A method of printing by irradiation with laser light has also been proposed. For example, Patent Document 1 discloses a laser-printing laminate produced by applying white ink, black ink and overprint varnish (OP varnish) to the aluminum-vapor-deposited surface of aluminum-vapor-deposited paper, with the aim of providing a laser-printing laminate and a printed body that can produce clear printing at high speed by irradiation with laser light and have a printed portion that is excellent in various resistances. Furthermore, Patent Document 2 describes an ink composition used to form a laser marking layer that contains first titanium oxide particles having an average particle size of 150 nm or less and changes color when irradiated with an ultraviolet laser, with the aim of providing a technology that generates relatively little heat and is preferably applicable to laser marking of packaging materials. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-123607 [Patent Document 2] JP 2020-75943 A Summary of the Invention [Problem to be solved by the invention]

[0004] One method of printing on the surfaces of packages, labels, adhesive tapes, etc. is to directly apply ink to the surface of the package using a thermal printer or inkjet printer, which is currently widely used. However, consumables such as ink ribbons for thermal printers and ink for inkjet printers are expensive, and there is a problem that the running costs are high to print a lot of variable information. In addition, failure to replace these consumables may result in printing errors. Furthermore, variable information is also directly printed on the package by offset printing using UV-curable ink, but stains on the surface of the package or uneven thickness of the package may result in blurred printing or missing characters. In addition, the method described in Patent Document 1 can be performed at high speed, but since it is a technology in which the upper layer, which easily absorbs laser light, is removed by irradiating a CO2 laser light, the lower layer is exposed, and characters, etc. that are visible due to the difference in color between the upper layer and the lower layer are formed, the upper layer is limited to a material that easily absorbs laser light, and conversely, the lower layer is limited to a material that does not easily absorb laser light and has a color contrast with the upper layer. In other words, the upper layer is a carbon black-based material (black color) that easily absorbs laser light, and the lower layer is a titanium oxide-based material (white color), and the characters, etc. formed by irradiating the laser light are white characters on a black background, which is poor in visibility. In addition, when removing the upper layer, there is a problem that the ink in the upper layer turns into dust, which causes contamination of the working environment. Furthermore, when printing is performed with an ultraviolet laser on a coating layer prepared using the ink composition described in Patent Document 2, the printing clarity of each printing spot may be poor in some cases.

[0005] The present invention aims to provide an ultraviolet laser printing medium that, when irradiated with an ultraviolet laser, produces a print spot with excellent print clarity for each point, produces a printed matter in which swelling of the protective resin layer is suppressed when irradiated with a laser, and further has heat sealability. The present invention also aims to provide a printed matter and a manufacturing method thereof, in which the ultraviolet laser printing medium is irradiated with an ultraviolet laser to discolor the irradiated area. The present invention also aims to provide a processed product made of the ultraviolet laser printing medium or the printed matter. [Means for solving the problem]

[0006] The inventors have discovered that in an ultraviolet laser printing medium having a printing layer containing titanium oxide and a protective resin layer, in that order, on one side of a substrate, and a sealant layer on the other side of the substrate, the above-mentioned problems can be solved by setting the content of titanium oxide in the printing layer to a specific range and setting the crystallite size of titanium oxide to a specific range, and have thus completed the present invention. The present invention relates to the following: <1> ~ <13> Regarding. <1> A substrate is provided with a printed layer containing titanium oxide and a protective resin layer in this order, and a sealant layer is provided on the other surface of the substrate, and the content of the titanium oxide in the printed layer is 0.1 g / m 2 More than 4.0g / m 2 and wherein the crystallite size of titanium oxide in the printing layer is 13 nm or more and 53 nm or less. <2> The crystallite size of the titanium oxide in the printing layer is 30 nm or more and 53 nm or less. <1> 2. A medium for ultraviolet laser printing according to claim 1. <3> The titanium oxide in the printing layer is rutile titanium oxide, and the diffraction angle of the titanium oxide is 27.60° or less. <1> or <2> 2. A medium for ultraviolet laser printing according to claim 1. <4> The thickness of the protective resin layer is 10 μm or more. <1> ~ <3> 13. A medium for ultraviolet laser printing according to claim 12. <5> The resin constituting the protective resin layer is at least one selected from the group consisting of polyolefin, polyester, and polyvinyl alcohol. <1> ~ <4> 13. A medium for ultraviolet laser printing according to claim 12. <6> The substrate is a paper substrate, and the water retention of the pulp constituting the paper substrate is 140% or less. <1> ~ <5> 13. A medium for ultraviolet laser printing according to claim 12. <7> The substrate is a film substrate. <1> ~ <5> 13. A medium for ultraviolet laser printing according to claim 12. <8> The resin constituting the film substrate is selected from the group consisting of polyolefin, polyester, and polyvinyl chloride; <7> 2. A medium for ultraviolet laser printing according to claim 1. <9> A barrier layer is provided between the substrate and the sealant layer. <1> ~ <8> 13. A medium for ultraviolet laser printing according to claim 12. <10> <1> ~ <9> 1. A printed matter obtained from the ultraviolet laser printing medium described in any one of claims 1 to 9, wherein the printed layer has, at least in part, a printed area containing discolored titanium oxide, and the ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is 0.70 or less. <11> <1> ~ <9> 2. A medium for ultraviolet laser printing according to any one of the preceding claims, or <10> A processed product using the printed matter described in . <12> <1> ~ <9> irradiating an ultraviolet laser onto the ultraviolet laser printing medium according to any one of claims 1 to 5 with an ultraviolet laser to discolor the irradiated area, thereby forming a printed matter. <13> the printing step is a step of irradiating with an ultraviolet laser so that the ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is 0.70 or less; <12> A method for producing a printed matter according to claim 1. Effect of the Invention

[0007] According to the present invention, a medium for ultraviolet laser printing is provided which, when irradiated with an ultraviolet laser, produces a print spot with excellent print clarity for each point, produces a printed matter in which swelling of the protective resin layer is suppressed when irradiated with a laser, and further has heat sealability. Also, according to the present invention, a printed matter and a method for producing the same are provided, in which the medium for ultraviolet laser printing is irradiated with an ultraviolet laser to discolor the irradiated area. Furthermore, according to the present invention, a processed product is provided which uses the medium for ultraviolet laser printing or the printed matter. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a conceptual perspective view of an example of a liquid container having a print area. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [UV laser printing media] The ultraviolet laser printing medium of the present invention (hereinafter, also simply referred to as "printing medium") has a print layer containing titanium oxide and a protective resin layer, in this order, on one surface of a substrate, and a sealant layer on the other surface of the substrate, and the content of titanium oxide in the print layer is 0.1 g / m 2 More than 4.0g / m 2 and the crystallite size of the titanium oxide in the printed layer is 13 nm or more and 53 nm or less. According to the present invention, there is provided an ultraviolet laser printing medium which, when irradiated with an ultraviolet laser, gives printed spots with excellent printing clarity for each point, and, when irradiated with a laser, gives a printed matter in which swelling of the protective resin layer is suppressed, and further has heat sealability. Although the detailed reasons why the above-mentioned effects are obtained are unclear, some of the reasons are thought to be as follows. By having a printing layer containing titanium oxide on a substrate, the titanium oxide in the printing layer changes color by laser irradiation with an ultraviolet laser, and printing is possible. The color change of the titanium oxide is considered to be caused by a change in the ionic valence of the titanium oxide contained in the printing layer from tetravalent to trivalent, which causes oxygen defects, and the color changes from white to black, which makes it visible. The ionic valence of titanium oxide is considered to change when irradiated with light energy corresponding to the band gap of titanium oxide. The band gap of titanium oxide varies depending on the crystal system, but is generally about 3.0 to 3.2 eV, and the wavelength of light corresponding to this is 420 nm or less. Therefore, even if a laser beam with a wavelength exceeding 420 nm (for example, 532 nm, 1064 nm, 10600 nm) is used, it is difficult to perform printing due to the change in ionic valence of titanium oxide as in the present invention. In this case, the content of titanium oxide in the printing layer is 0.1 g / m 2By doing the above, a printed matter having spots with excellent visibility and excellent printing clarity for each spot can be obtained. When irradiated with an ultraviolet laser, titanium oxide changes color, resulting in a printed matter. When the titanium oxide changes color, it is reduced, causing oxygen and moisture in the printing medium, including the printing layer, to evaporate, generating water vapor. The present inventors have discovered that the generated oxygen and water vapor cause the protective resin layer in the ultraviolet laser irradiated area to swell. In the present invention, the content of titanium oxide in the printing layer is set to 4.0 g / m 2 It is believed that by keeping the temperature below this range, the amount of oxygen and water vapor generated is prevented from becoming excessive, thereby suppressing the phenomenon in which the printed matter swells and causes unevenness. Furthermore, by providing a protective resin layer, the generation of smoke accompanying irradiation with an ultraviolet laser is suppressed, and the detachment of titanium oxide accompanying the generation of smoke is suppressed, tending to result in a printed image with high print density and excellent printing clarity for each point.

[0010] In addition, when the crystallite size of titanium oxide is 13 nm or more, there are few crystal defects, the recombination of excited electrons and holes is suppressed, and titanium oxide is easily reduced and discolored, so it is believed that printed spots with excellent printing clarity were obtained. On the other hand, when the crystallite size is 53 nm or less, excessive oxygen generation is suppressed, and the protective resin layer swells when irradiated with an ultraviolet laser, suppressing the occurrence of unevenness in the printed matter. In this embodiment, the printable area refers to an area (portion) where printing by ultraviolet laser irradiation is possible because the titanium oxide in the area irradiated with the ultraviolet laser changes color from white to black, and the printable area refers to a portion of the printable area where the titanium oxide has actually changed color by irradiation with the ultraviolet laser and become visible, i.e., the portion irradiated with the ultraviolet laser. Additionally, the non-printable area refers to an area (portion) of the printable area that is not irradiated with the ultraviolet laser. Furthermore, by providing a sealant layer on the surface opposite to the surface on which the printed layer of the substrate is provided, heat sealability is imparted, and a print medium having heat sealability is provided. Furthermore, by providing a sealant layer, it is preferable that gas barrier properties are also imparted. Here, gas barrier properties mainly mean barrier properties against at least one selected from oxygen and water vapor, and may also have barrier properties against other gases. The print medium of this embodiment preferably has at least water vapor barrier properties, and in addition to this, it is also preferable that it has oxygen barrier properties. The present invention will now be described in further detail.

[0011] The ultraviolet laser printable medium has printable areas that contain titanium oxide. The printing medium has a printing layer containing titanium oxide and a protective resin layer in this order on one side of the substrate. The printing layer and the protective resin layer are formed on one side, and a sealant layer is provided on the other side. The printing medium may have the printing layer and the protective resin layer in this order on the entire surface, or may have the printing layer and the protective resin layer in this order only in a part of the area (part) where printing is desired. The sealant layer may be formed on the entire surface of the substrate, or may be provided only in a part of the area (part) where heat sealability is required. From the viewpoint of heat sealability, it is preferable that the sealant layer is provided on the outermost layer on the surface opposite to the surface on which the printing layer is formed. Furthermore, a barrier layer may be provided between the substrate and the sealant layer, and from the viewpoint of oxygen barrier property, it is preferable that a barrier layer is provided between the substrate and the sealant layer. In addition, an adhesive layer may be present between the substrate and the printed layer, between the printed layer and the protective resin layer, between the substrate and the barrier layer, between the substrate and the sealant layer, or between the sealant layer and the barrier layer.

[0012] <Print layer> The ultraviolet laser printing medium of this embodiment has a printing layer containing titanium oxide on one side of the substrate. The printing layer may be provided by coating or by lamination, and is not particularly limited. That is, the printing layer is preferably a coating layer containing titanium oxide or a laminate layer containing titanium oxide. In the present invention, the printing layer is more preferably provided by coating from the viewpoint of facilitating the provision of the printing layer only at desired locations and from the viewpoint of ease of production. The term "provided by coating" means that the printing layer is formed by a coating liquid (ink composition), and includes, for example, the case of forming the printing layer by gravure printing, inkjet printing, etc. The printing layer contains titanium oxide, and the content of titanium oxide in the printing layer is 0.1 g / m 2 More than 4.0g / m 2 The following is the result. The content of titanium oxide in the printing layer is set to 0.1 g / m in order to obtain sufficient printing density. 2 or more, preferably 0.2 g / m 2 More preferably, 0.3 g / m 2 More preferably, 0.4 g / m 2 From the viewpoints of obtaining print spots with excellent print clarity for each point, suppressing the increase in cost due to the inclusion of more than the necessary amount of titanium oxide when the print density reaches a plateau, and suppressing the occurrence of unevenness in the protective resin layer due to irradiation with an ultraviolet laser, a coating weight of 4.0 g / m 2 or less, preferably 3.0 g / m 2 Less than 2.0 g / m, more preferably 2.0 g / m 2 Less than 1.5 g / m, more preferably 2 Less than 1.0 g / m 2 The following is the result. If the content of titanium oxide in the printed layer is too high, a large amount of oxygen is generated by the reduction of titanium oxide, and it tends to be difficult to suppress swelling of the protective resin layer. It is sufficient that at least the printable area of ​​the ultraviolet laser printing medium contains titanium oxide in the above content, and in the area where printing is not performed, there may be a portion where no printing layer is provided, and the titanium oxide content is 0.1 g / m 2 Less than or equal to 4.0 g / m 2 From the viewpoint of ease of production, it is preferable that the content of titanium oxide in the entire region of the printing medium is 0.1 g / m or more. 2 More than 4.0g / m 2 It is also preferable that a printing layer is provided which is as follows:

[0013] In this embodiment, the printing medium includes an undercoat layer not containing titanium oxide or a titanium oxide content of 0.1 g / m 2 as a layer below the printing layer containing titanium oxide. 2 Less than or equal to 4.0 g / m 2 In such a case, the content of titanium oxide in the entire printed layer including the undercoat layer is 0.1 g / m 2 More than 4.0g / m 2 The following is the result.

[0014] 1m of printed layer 2 The mass (grammage, solid content) per unit is preferably 0.2 g / m from the viewpoint of print density and print clarity of each dot. 2 More preferably, 0.5 g / m 2 More preferably, 1.0 g / m 2 and preferably 50 g / m 2 Less than 20 g / m 2 More preferably, 10 g / m 2 Below are the results.

[0015] The content of titanium oxide in the printing layer (solids) is preferably 0.3% by mass or more, more preferably 1.0% by mass or more, even more preferably 2.0% by mass or more, still more preferably 5.0% by mass or more, and particularly preferably 10.0% by mass or more, from the standpoint of print density and print clarity of each dot, and is preferably 95% by mass or less, more preferably 85% by mass or less, even more preferably 75% by mass or less, and even more preferably 60% by mass or less, from the standpoint of preventing cost increases due to the inclusion of more titanium oxide than necessary when the print density reaches a plateau, from the standpoint of ease of forming the printing layer, and from the standpoint of preventing swelling of the protective resin layer when irradiated with an ultraviolet laser.

[0016] The thickness of the printed layer is preferably 0.3 μm or more, more preferably 1.0 μm or more, and even more preferably 2.0 μm or more, from the viewpoint of printing clarity for each dot and ease of forming the printed layer, and is preferably 40.0 μm or less, more preferably 30.0 μm or less, even more preferably 25.0 μm or less, and even more preferably 20.0 μm or less, from the viewpoint of plateauing of printing density and ease of forming the printed layer. The thickness of the print layer is measured from an image of a cross section of the print medium observed under a scanning electron microscope (SEM).

[0017] The substrate of the printing medium is preferably a paper substrate or a film substrate as described below, and the paper substrate or film substrate itself may contain titanium oxide.

[0018] The printing layer preferably contains a thermoplastic resin in addition to titanium oxide. It may further contain an inorganic pigment other than titanium oxide. Each component will be described in detail below. (Titanium dioxide) The titanium oxide contained in the printing layer is represented by the composition formula TiO2, and is also called titanium dioxide or titania. In this embodiment, the crystallite size of titanium oxide in the printing layer is 13 nm or more. If the crystallite size of titanium oxide in the printing layer is less than 13 nm, there are many crystal defects, and the recombination of excited electrons and holes excited by ultraviolet laser irradiation is likely to occur, resulting in the titanium oxide being difficult to reduce, and the printing clarity of each point is poor. The crystallite size of titanium oxide is preferably 20 nm or more, more preferably 30 nm or more, even more preferably 35 nm or more, and even more preferably 40 nm or more. In addition, the crystallite size of titanium oxide is 53 nm or less, preferably 50 nm or less, from the viewpoint of suppressing the swelling of the protective resin layer due to ultraviolet laser irradiation and from the viewpoint of dispersion stability in the coating liquid or the printing layer. If the upper limit of the crystallite size of titanium oxide is within the above range, the generation of oxygen and the like during ultraviolet laser irradiation is not excessive, and the swelling of the protective resin layer is suppressed, which is preferable. In addition, the dispersion stability of titanium oxide is good in the coating liquid or the printing layer, and the printing uniformity is excellent, which is preferable. The crystallite size of titanium oxide is measured by the method described in the Examples. The crystallite size is determined by the Scherrer equation, and the Bragg angle is the measured value of the maximum intensity derived from the 101 plane in the case of anatase titanium oxide, or the 110 plane in the case of rutile titanium oxide.

[0019] The titanium oxide may have a crystalline structure, and is preferably at least one selected from rutile titanium oxide, anatase titanium oxide, and brookite titanium oxide. From the standpoint of availability and stability, it is more preferably at least one selected from rutile titanium oxide and anatase titanium oxide, and even more preferably rutile titanium oxide. The crystal form of titanium oxide can be determined by known methods, specifically, by analysis of Raman spectrum, XRD pattern, etc. For example, when identifying from Raman spectrum, the crystal form of rutile type is generally determined as 447±10 cm -1 , 609±10cm -1 A peak was confirmed at 395±10cm for the anatase type.-1 , 516±10cm -1 , 637±10cm -1 A peak is observed at . The titanium oxide may be used alone or in combination of two or more kinds.

[0020] When the titanium oxide is rutile type titanium oxide, the diffraction angle of the titanium oxide is preferably 27.60° or less from the viewpoint of print clarity for each point. The Bragg angle of rutile type titanium oxide is originally 27.40°, but if the crystallinity is low, the diffraction angle tends to be high. If the diffraction angle of titanium oxide exceeds 27.60°, the crystallinity is low and discoloration is suppressed, so the print clarity for each point tends to be poor. When the titanium oxide is rutile type titanium oxide, the diffraction angle of the titanium oxide is preferably 27.60° or less, more preferably 27.55° or less, and even more preferably 27.50° or less. The diffraction angle of titanium oxide, in the case of rutile type, is the measured value of the maximum intensity resulting from the 110 plane, as described above.

[0021] The shape of the titanium oxide is not particularly limited, and may be any shape such as amorphous, spherical, rod-like, or needle-like. When the titanium oxide is amorphous or spherical, the average particle size of the titanium oxide is not particularly limited, but from the viewpoint of obtaining a printing medium with excellent surface smoothness, it is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.10 μm or more, even more preferably more than 0.15 μm, particularly preferably 0.16 μm or more, and preferably 20.0 μm or less, more preferably 5.0 μm or less, even more preferably 1.0 μm or less, even more preferably 0.50 μm or less, particularly preferably 0.30 μm or less.

[0022] In addition, when titanium oxide is needle-shaped, the long diameter of titanium oxide is not particularly limited, but from the viewpoint of obtaining a printing medium having excellent surface smoothness, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1.5 μm or more, and preferably 50.0 μm or less, more preferably 30.0 μm or less, and even more preferably 15.0 μm or less. In addition, the short diameter is preferably 0.01 μm or more, more preferably 0.03 μm or more, even more preferably 0.05 μm or more, and preferably 3.0 μm or less, more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. In addition, when titanium oxide is needle-shaped, the aspect ratio (long diameter / short diameter) is preferably 5 or more, more preferably 10 or more, even more preferably 15 or more, and preferably 300 or less, more preferably 100 or less, and even more preferably 30 or less. The particle diameter, major axis, and minor axis of titanium oxide are measured by the method described in the Examples. The particle diameter, major axis, and minor axis values ​​of titanium oxide used as a raw material may be adopted, or catalog values ​​of the particle diameter, major axis, and minor axis of titanium oxide used as a raw material may be adopted.

[0023] (thermoplastic resin) The thermoplastic resin used in the printing layer functions as a binder. The thermoplastic resin for the printed layer is not particularly limited, but when the printed layer is provided by coating, it may be applied as an aqueous coating liquid or an organic solvent-based coating liquid (oil-based coating liquid). When the printed layer is provided by coating, the printed layer is also referred to as a coating layer. Furthermore, the composition used to provide the coating layer is also referred to as a coating liquid or ink composition. When the coating is carried out as an aqueous coating liquid, the thermoplastic resin is preferably a water-dilutable thermoplastic resin. Examples of water-dilutable resins include water-soluble, emulsion-type and dispersion-type resins. The water-dilutable thermoplastic resin may be either a natural resin or a synthetic resin, and examples thereof include starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, acrylic resins, maleic acid resins, urethane resins, polyester resins, styrene-butadiene resins, vinyl chloride resins, and polyolefin resins. More specifically, examples of the acrylic resin include an acrylic resin copolymerized with (meth)acrylic acid and its alkyl ester or styrene as a monomer component, a styrene-maleic acid resin, a styrene-acrylic acid-maleic acid resin, a water-soluble polyurethane resin, and a water-soluble polyester resin. Among these, from the viewpoints of the stability of the coating liquid and the solvent resistance of the printed layer, at least one selected from starch derivatives, casein, shellac, polyvinyl alcohol and its derivatives, acrylic resins, maleic acid resins, and styrene-butadiene resins is preferred, at least one selected from starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, acrylic resins, maleic acid resins, and styrene-butadiene resins is more preferred, at least one selected from starch derivatives, polyvinyl alcohol, polyvinyl alcohol derivatives, acrylic resins, and styrene-butadiene resins is even more preferred, and at least one selected from polyvinyl alcohol, polyvinyl alcohol derivatives, acrylic resins, and styrene-butadiene resins is even more preferred. These resins may be used alone or in combination of two or more. When an organic solvent-based coating liquid (oil-based coating liquid) is used, it is preferable to use a known thermoplastic resin such as a cellulose-based resin (e.g., soluble cellulose, cellulose acetate, cellulose acetate propionate, etc.), a polyurethane-based resin, an acrylic-based resin, or a vinyl chloride copolymer-based resin.

[0024] The content of the thermoplastic resin is not particularly limited and may be appropriately selected depending on the type of thermoplastic resin, the content of titanium oxide and inorganic pigments described later in the coating liquid, and the like. For example, the content of the thermoplastic resin is preferably 5 mass% or more, more preferably 10 mass% or more, and even more preferably 15 mass% or more, and is preferably 99 mass% or less, more preferably 90 mass% or less, of the solid content of the coating liquid.

[0025] When the printed layer is provided by coating, the coated layer is preferably provided by applying a coating liquid and drying it. When the coating liquid is an aqueous coating liquid, the aqueous medium used may be water or a mixture of water and a water-miscible solvent. Examples of the water-miscible solvent include lower alcohols, polyhydric alcohols, and their alkyl ethers or alkyl esters.Specific examples of the water-miscible solvent include lower alcohols such as methyl alcohol, ethyl alcohol, normal propyl alcohol, and isopropyl alcohol, polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, and glycerin, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monoacetate, diethylene glycol monomethyl ether, and dipropylene glycol monomethyl ether. In the case of an organic solvent-based coating liquid (oil-based coating liquid), examples of the solvent include known solvents such as aromatic organic solvents such as toluene and xylene, ester-based organic solvents such as ethyl acetate, n-propyl acetate, isobutyl acetate, ester-based organic solvents, ketone-based organic solvents such as methyl ethyl ketone and methyl isobutyl ketone, alcohol-based organic solvents such as methanol, ethanol, isopropanol, and n-butanol, and hydrocarbon-based solvents such as methylcyclohexane.

[0026] The solids concentration of the coating liquid is not particularly limited, but from the viewpoints of obtaining a desired coating layer thickness, imparting a viscosity to the coating liquid that facilitates application, and ease of drying, it is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, and still more preferably 65% ​​by mass or less.

[0027] From the viewpoints of coatability, obtaining a desired coating layer thickness, and ease of drying, the viscosity of the coating fluid, as measured with a Brookfield viscometer, is preferably at least 10 mPa·s (20°C), more preferably at least 15 mPa·s (20°C), even more preferably at least 20 mPa·s (20°C), and is preferably at most 5000 mPa·s (20°C), more preferably at most 4000 mPa·s (20°C), even more preferably at most 3000 mPa·s (20°C), and still more preferably at most 2000 mPa·s (20°C).

[0028] When the printed layer is provided by lamination, it is preferable to laminate a film containing titanium oxide onto the substrate. When the printed layer is provided by lamination, the printed layer is also called a laminate layer. The thermoplastic resin constituting the laminate layer is not particularly limited, and may be appropriately selected from known thermoplastic resins as long as it can be processed into a film by incorporating titanium oxide.Specific examples include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyolefin resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene, polycarbonate, polyurethane, polyamide, polyacrylonitrile, and poly(meth)acrylate. Among these, the resin constituting the laminate layer is preferably a polyolefin such as polyethylene, polypropylene, ethylene-propylene copolymer, or a polyester such as polyethylene terephthalate, polybutylene terephthalate, polylactic acid, or polybutylene succinate, from the viewpoint of being versatile, having high UV transmittance, and enabling the discoloration of titanium oxide to the inside of the film, more preferably at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polylactic acid, and polybutylene succinate, and even more preferably at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polylactic acid, and polybutylene succinate. The resin constituting the laminate layer is more preferably a polyolefin, and even more preferably at least one selected from the group consisting of polyethylene and polypropylene. Polyethylene (PE) is roughly classified into linear low density polyethylene (LLDPE), low density polyethylene (LDPE), medium density polyethylene (MDPE), and high density polyethylene (HDPE). Among these, low density polyethylene (LDPE) is preferred because of its excellent extrusion lamination properties. In addition, it is preferable to use a biodegradable polyester resin as the resin constituting the laminate layer in terms of reducing the environmental load. Examples of such resins include polylactic acid and polybutylene succinate. These resins may be used alone or in combination of two or more.

[0029] From the viewpoint of obtaining a printing medium having excellent visibility and excellent printing clarity for each point, the content of the thermoplastic resin in the laminate layer is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 95% by mass or less.

[0030] (Inorganic pigments other than titanium dioxide) The printing layer may contain other components in addition to the titanium oxide and thermoplastic resin described above. Examples of other components include inorganic pigments other than titanium oxide (hereinafter, simply referred to as "inorganic pigments"). By containing inorganic pigments other than titanium oxide, heat generation of titanium oxide and softening of the protective resin layer due to ultraviolet laser irradiation are suppressed, and as a result, swelling of the protective resin layer is suppressed, which is preferable. Examples of inorganic pigments include calcium carbonate, talc, silica, kaolin, magnesium oxide, mica, aluminum hydroxide, and barium sulfate. Among these, at least one selected from the group consisting of calcium carbonate, talc, silica, kaolin, magnesium oxide, zinc oxide, and mica is preferable, and at least one selected from the group consisting of calcium carbonate and talc is more preferable. The inorganic pigments may be used alone or in combination of two or more kinds.

[0031] The shape of the inorganic pigment is not particularly limited, and may be any shape such as amorphous, spherical, plate-like, rod-like, or needle-like. When the inorganic pigment is amorphous, spherical, or plate-like, the average particle size of the inorganic pigment is not particularly limited, but from the viewpoint of obtaining a printing medium with excellent surface smoothness and from the viewpoint of suppressing the occurrence of bulging of the protective resin layer, it is preferably 0.1 μm or more, more preferably 0.15 μm or more, even more preferably 0.20 μm or more, and preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less. In addition, when the inorganic pigment is needle-shaped, the major axis of the inorganic pigment is not particularly limited, but from the viewpoint of obtaining a printing medium with excellent surface smoothness and from the viewpoint of suppressing swelling of the protective resin layer, it is preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 2.0 μm or more, and preferably 100 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. In addition, the minor axis is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1.0 μm or more, and preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 1.0 μm or less. In addition, when the inorganic particle is needle-shaped, the aspect ratio (major axis / minor axis) is preferably 1.5 or more, more preferably 2.0 or more, even more preferably 3.0 or more, and preferably 100 or less, more preferably 50 or less, and even more preferably 30 or less.

[0032] When the printed layer contains an inorganic pigment other than titanium oxide, the content of the inorganic pigment in the printed layer is, from the viewpoint of suppressing the occurrence of swelling of the protective resin layer, preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 50% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less, and even more preferably 80% by mass or less.

[0033] When the printing layer contains an inorganic pigment other than titanium oxide, the mass ratio of titanium oxide to the inorganic pigment other than titanium oxide (titanium oxide / inorganic pigment other than titanium oxide) is, from the viewpoint of suppressing the occurrence of swelling of the protective resin layer, preferably 0.01 or more, more preferably 0.03 or more, even more preferably 0.10 or more, and is preferably 2.0 or less, more preferably 1.6 or less, even more preferably 1.2 or less.

[0034] In addition to the components mentioned above, the printing layer may contain film-forming agents, pigment dispersants, pigment dispersing resins, antiblocking agents, wetting agents, viscosity adjusters, pH adjusters, antifoaming agents, general surfactants, and the like.

[0035] (Coating fluid) When the printing layer is provided by coating, if the coating liquid (ink composition) is an aqueous coating liquid, it is preferable to obtain it by mixing the above-mentioned various materials with an aqueous medium.Note that, if the coating liquid is an aqueous coating liquid, prior to mixing with an aqueous medium, titanium oxide, thermoplastic resin, water, and if necessary, inorganic pigments other than titanium oxide, water-miscible solvents, pigment dispersants, pigment dispersible resins, etc. are mixed and kneaded, and water, if necessary, water-miscible solvents, and the rest of the specified materials may be added and mixed thereto. Furthermore, when the coating liquid is an oil-based coating liquid, titanium oxide or a pigment other than titanium oxide may be added after mixing the organic solvent and the resin, and a pigment dispersant, pigment dispersing resin, etc. may be added in advance to the mixed liquid of the organic material and the resin, or may be added later. The coating liquid can be obtained by mixing and dispersing the above-mentioned components using a high-speed stirrer such as a homomixer or a lab mixer, or a dispersing machine such as a Coles disperser, a three-roll mill, or a bead mill.

[0036] The method for applying the coating liquid is not particularly limited, and the coating liquid may be applied to the substrate by flexographic printing, inkjet printing, gravure printing, screen printing, pad printing, spray coating, a Mayer bar, a gravure coater, an air knife coater, a blade coater, a rod coater, a die coater, a bar coater, or the like.

[0037] (Laminate layer) When the printed layer is a laminate layer, the film to be laminated is obtained by preparing a raw material composition by melt-kneading at least titanium oxide and a thermoplastic resin, and, if necessary, materials such as inorganic pigments, forming this into a film, and then stretching it if necessary. In preparing the raw material composition, a master batch containing titanium oxide or an inorganic pigment at a high concentration may be prepared and then mixed with the resin. Alternatively, materials that have been uniformly mixed in advance may be charged into the molding machine, or the materials may be mixed in a hopper or kneader that is integrated with the molding machine. The method for forming the composition into a film may be appropriately selected from conventionally known methods, such as melt extrusion, melt casting, and calendering.

[0038] The substrate and the film may be attached via an adhesive layer, or preferably, are laminated. The adhesive layer is not particularly limited and may be appropriately selected from known adhesive layers. Specific examples include the pressure-sensitive adhesive layer described in JP2012-57112A. Specific examples of the lamination process include laminating a substrate and a laminate layer by a thermal lamination method, a dry lamination method, a wet lamination method, an extrusion lamination method, or the like. Among these, the extrusion lamination method is preferred from the viewpoint of the manufacturing process since it does not require a step of bonding the laminate layer and the substrate.

[0039] <Base material> In this embodiment, the substrate is not particularly limited as long as it is a substrate on which a print layer can be provided, and may be appropriately selected from various substrates such as paper, nonwoven fabric, cloth, film (resin film), and metal. Among these, from the viewpoint of easy formation of the printed layer, it is more preferable that the substrate is at least one selected from paper, nonwoven fabric, cloth, and film, and even more preferable that the substrate is at least one selected from paper and film. When the substrate is paper, the substrate is also called paper substrate. When the substrate is a resin film, the substrate is also called film substrate. For example, the paper substrate may be a coated paper having a coating layer provided on the paper, and the coating layer may be provided on the printing layer side of the paper substrate or on the opposite side, without any particular limitation.

[0040] (Paper base material) In this embodiment, a paper substrate may be used as the substrate. Examples of raw pulp constituting the paper base material include wood pulp, non-wood pulp, and deinked pulp. Examples of wood pulp include, but are not limited to, chemical pulp such as bleached hardwood kraft pulp (LBKP), unbleached hardwood kraft pulp (LUKP), bleached softwood kraft pulp (NBKP), unbleached softwood kraft pulp (NUKP), sulfite pulp (SP), dissolving pulp (DP), soda pulp (AP), and oxygen bleached kraft pulp (OKP), semi-chemical pulp such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP), mechanical pulp such as groundwood pulp (GP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP), and the like. Examples of non-wood pulp include, but are not limited to, cotton-based pulp such as cotton linters and cotton lint, and non-wood pulp such as hemp, straw, bamboo, and bagasse. The deinked pulp is not particularly limited, but may be deinked pulp made from waste paper. The raw pulp may be one of the above-mentioned types alone or a mixture of two or more types. The raw pulp may be mixed with organic synthetic fibers such as polyamide fibers and polyester fibers, regenerated fibers such as polynosic fibers, and inorganic fibers such as glass fibers, ceramic fibers, and carbon fibers. From the viewpoint of availability, the raw material pulp is preferably wood pulp and deinked pulp. From the viewpoint of uniformity of texture, the raw material pulp is preferably chemical pulp among wood pulps, more preferably kraft pulp, further preferably one or more selected from hardwood kraft pulp such as eucalyptus and acacia, and softwood kraft pulp such as pine and cedar, still further preferably one or more selected from hardwood bleached kraft pulp (LBKP) and softwood bleached kraft pulp (NBKP), and particularly preferably LBKP.

[0041] The length-weighted average fiber length of the pulp constituting the paper base material is, from the viewpoint of suppressing coating unevenness and improving the clarity of each printed dot, preferably 0.6 mm or more, more preferably 0.65 mm or more, even more preferably 0.7 mm or more, and preferably 3.5 mm or less, more preferably 2.5 mm or less, even more preferably 2.0 mm or less, still more preferably 1.5 mm or less, and particularly preferably 1.0 mm or less. When the length-weighted average fiber length of the pulp constituting the paper base material is equal to or less than the above upper limit, the pulp particles become densely entangled, reducing the voids in the paper base material, and when a coating layer is provided, coating unevenness is suppressed, resulting in a printed matter with excellent printing clarity for each point, which is preferable. Furthermore, when the length-weighted average fiber length of the pulp constituting the paper base material is equal to or greater than the lower limit, the strength of the paper base material is improved and paper dust is reduced, which is preferable as it also suppresses falling off of printed areas. The length-weighted average fiber length of the pulp constituting the paper base material is measured by the method described in the Examples.

[0042] The average fiber width of the pulp fibers constituting the paper base material is preferably 14.0 μm or more, more preferably 15.0 μm or more, even more preferably 15.5 μm or more, still more preferably 16.0 μm or more, and preferably 35.0 μm or less, preferably 33.0 μm or less, more preferably 31.0 μm or less, even more preferably 28.0 μm or less, still more preferably 24.0 μm or less, and still more preferably 21.0 μm or less. When the average fiber width of the pulp fibers constituting the paper base material is 35.0 μm or less, the pulps are densely intertwined with each other, smoothing the surface of the paper base material, suppressing uneven coating when a printed layer is provided, and the smoothing of the printed layer surface results in a printed matter with excellent print clarity for each point, which is preferable. Also, when the average fiber width is 14.0 μm or more, the strength of the paper base material is improved and further paper dust is reduced, which is preferable because it suppresses the falling off of printed parts. The average fiber width of the pulp fibers constituting the paper base material can be measured by the method described in the Examples.

[0043] In the pulp constituting the paper base material, the proportion of fine fibers having a fiber length of 0.2 mm or less is preferably 4% or more, more preferably 5% or more, even more preferably 6% or more, still more preferably 10% or more, particularly preferably 15% or more, and is preferably 40% or less, more preferably 30% or less, and even more preferably 20% or less. A ratio of fine fibers of 40% or less is preferable because it ensures the strength of the paper base material and also prevents the loss of printed areas due to the detachment of fine fibers. A ratio of fine fibers of 4% or more is preferable because the fine fibers are arranged to fill the gaps between the fibers, reducing voids in the paper base material and preventing uneven coating when a coating layer is provided, thereby improving the print clarity and uniformity of each point. The percentage of fine fibers with a fiber length of 0.2 mm or less in the pulp constituting the paper base material is calculated by disintegrating the paper base material using the method described in the Examples, and measuring the fiber length of the resulting pulp slurry using a fiber length measuring device (e.g., Valmet Model FS-5 with UHD base unit). Fibers with a fiber length of 0.2 mm or less and a fiber width of 75 μm or less are defined as fine fibers, and the percentage of the number of fine fibers relative to the number of measured pulp fibers is calculated.

[0044] The water retention of the pulp fibers that make up the paper base material is preferably 140% or less, more preferably 130% or less, and even more preferably 125% or less, from the viewpoint of suppressing the occurrence of swelling of the protective resin layer due to ultraviolet laser printing, and while there is no particular lower limit, it is preferably 95% or more, more preferably 100% or more, even more preferably 105% or more, even more preferably 110% or more, and even more preferably 115% or more. It is believed that the titanium oxide absorbs the ultraviolet laser light and generates heat, which in turn heats the pulp that composes the paper base material located directly below, generating water vapor. If the water retention is high, a large amount of water vapor is generated, and this water vapor tends to cause the protective resin layer to swell. The water retention of pulp fibers tends to be higher when the hemicellulose content in the pulp fibers is high, so when a dissolving pulp with a high α-cellulose content and a reduced hemicellulose content is used as the raw pulp, the water retention tends to decrease. In addition, the higher the degree of beating of pulp fibers, the higher the water retention tends to be. Therefore, when pulp fibers with a small Canadian Standard Freeness (CSF) and high degree of beating are used, the water retention tends to increase. The water retention of the pulp fibers constituting the paper base material is measured by the method described in the Examples.

[0045] The Canadian Standard Freeness (CSF) of the wood pulp used for the paper base material is, from the viewpoint of obtaining the desired fiber width and fiber length, and the smoothness of the printed layer surface, preferably 150 mL or more, more preferably 300 mL or more, even more preferably 400 mL or more, and is preferably 800 mL or less, more preferably 750 mL or less, even more preferably 700 mL or less, and even more preferably 600 mL or less. Here, CSF refers to Canadian Standard Freeness according to JIS P 8121-2:2012.

[0046] The paper base material can be obtained by making paper from a pulp slurry to which internal additives have been added as necessary. In addition to the above-mentioned pulp, known internal additives for papermaking, such as fillers, sizing agents, dry strength agents, wet strength agents (e.g., polyamidepolyamine epichlorohydrin), retention aids (e.g., aluminum sulfate), drainage aids, pH adjusters, softeners, antistatic agents, defoamers, dyes, pigments, etc., may be added to the paper base material as necessary. Examples of fillers include kaolin, talc, titanium oxide, heavy calcium carbonate, light calcium carbonate, calcium sulfite, gypsum, calcined kaolin, white carbon, amorphous silica, delaminated kaolin, diatomaceous earth, magnesium carbonate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, and the like. Examples of sizing agents include rosin-based, alkyl ketene dimer-based, alkenyl succinic anhydride-based, styrene-acrylic, higher fatty acid-based, and petroleum resin-based sizing agents.

[0047] In the papermaking of the paper base material, a known wet papermaking machine, such as a Fourdrinier papermaking machine, a gap former type papermaking machine, a cylinder papermaking machine, a short wire papermaking machine, etc., can be appropriately selected and used. Next, the paper layer formed by the papermaking machine is transported on a felt and dried in a dryer. A multi-stage cylinder dryer may be used as a pre-dryer before drying with the dryer.

[0048] The paper base material obtained as described above may be subjected to a surface treatment using a calendar to make the thickness and profile uniform and improve printability. A known calendaring machine can be appropriately selected and used for the calendaring.

[0049] The paper substrate may be appropriately selected from conventionally known paper substrates such as liner base paper, kraft paper, wood-free paper, and coated paper. The paper base material may be a single layer or a multi-layer, and may have a multi-layer construction with different pulp compositions.

[0050] The basis weight of the paper base material is preferably 30 g / m from the viewpoint of improving the strength as a printing medium and printability. 2 More preferably, 35 g / m 2 and preferably 1000 g / m 2 Less than 700g / m 2 The following is the result. The basis weight is measured according to the method specified in JIS P 8124:2011.

[0051] The thickness of the paper base material is not particularly limited, but from the viewpoint of improving the strength as a printing medium and printability, it is preferably 30 μm or more, more preferably 35 μm or more, even more preferably 40 μm or more, still more preferably 50 μm or more, and preferably 900 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less. The thickness of the paper base material can be measured by the method described in JIS P 8118:2014.

[0052] The density of the paper base material is not particularly limited, but from the viewpoint of improving the strength as a printing medium and printability, it is preferably 0.6 g / cm 3 More preferably, 0.7 g / cm 3 and preferably 1.2 g / cm 3 Less than 1.0 g / cm, more preferably 1.0 g / cm 3 Less than 0.9 g / cm, more preferably 0.9 g / cm 3 The following is the result. The density of the paper substrate is calculated from the basis weight and thickness of the paper substrate described above.

[0053] (Film substrate) The resin constituting the film substrate (hereinafter also simply referred to as "resin") is not particularly limited as long as it can be processed into a film and may be appropriately selected from among known thermoplastic resins. Specific examples include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate; polyolefin-based resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene; polycarbonate; polyurethane; polyamide; polyacrylonitrile; poly(meth)acrylate; and the like. Among these, from the viewpoint of versatile use, the resin constituting the film substrate preferably contains polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers, polyesters such as polyethylene terephthalate, polybutylene terephthalate, polylactic acid, and polybutylene succinate, and polyvinyl chloride, more preferably contains at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymers, polyethylene terephthalate, polylactic acid, and polybutylene succinate, and even more preferably contains at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymers, polyethylene terephthalate, polylactic acid, and polybutylene succinate. The resin constituting the film substrate is even more preferably polyolefin, even more preferably at least one selected from the group consisting of polyethylene and polypropylene, and particularly preferably contains at least polypropylene. In addition, it is preferable to use a biodegradable resin, polyester, as the resin constituting the film substrate in terms of reducing the environmental load. Examples of such resins include polylactic acid and polybutylene succinate. These resins may be used alone or in combination of two or more.

[0054] The film substrate may be stretched or unstretched, and is not particularly limited. For example, when the film substrate is a polypropylene film, it may be a non-stretched polypropylene film (CPP) or a biaxially stretched polypropylene film (OPP).

[0055] In the present embodiment, in addition to the above-mentioned resin, other components may be added to the film substrate within a range that does not impair the effects of the present invention. Examples of such components include pigments containing titanium oxide, antistatic agents, antiblocking agents, antioxidants, UV absorbers, HALS, plasticizers, lubricants, flame retardants, release agents, and colorants.

[0056] From the viewpoint of improving strength, the thickness of the film substrate is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, and is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 100 μm or less. The thickness of the film is measured by the method described in the Examples.

[0057] [Method of manufacturing film substrate] The film substrate may be prepared by preparing a raw material composition by melt-kneading a resin and, if necessary, materials such as an inorganic pigment, forming the composition into a film, and then stretching the film appropriately. In addition, when preparing the raw material composition, if the film substrate contains an inorganic pigment containing titanium oxide, a master batch containing the inorganic pigment at a high concentration may be prepared and then mixed with the resin. Also, materials that have been uniformly mixed in advance may be charged into a molding machine, or may be mixed in a hopper or kneader integrated with the molding machine. The method for forming the composition into a film may be appropriately selected from conventionally known methods, such as melt extrusion, melt casting, and calendering.

[0058] When the film substrate of the present embodiment is subjected to a stretching treatment, the stretching treatment may be uniaxial stretching or biaxial stretching. The stretching treatment is preferably performed at least in the longitudinal direction, and may also be performed in the transverse direction.

[0059] (cloth, non-woven fabric) When the substrate is a cloth or nonwoven fabric, examples of raw materials constituting the cloth or nonwoven fabric include natural fibers such as cotton, hemp, cellulose fibers, wool, etc.; synthetic fibers such as polycarbonate, polyetherimide, polyester, polyurethane, polyamide (nylon), etc.; and regenerated fibers such as rayon, acetate, etc.

[0060] As the substrate, a commercially available substrate may be used as appropriate. For example, various types of commercially available paper may be used as the paper substrate, and a resin film of various resins may be used as the film substrate.

[0061] <Protective resin layer> The printing medium of this embodiment further has a protective resin layer on the printing layer from the viewpoints of improving the water resistance of the printing medium, functioning as a protective layer, achieving high print density and improving print clarity for each dot, and suppressing smoke generation during ultraviolet laser printing.

[0062] The total light transmittance of the protective resin layer is preferably 40% or more, more preferably 60% or more, even more preferably 70% or more, still more preferably 80% or more, particularly preferably 90% or more, and 100% or less. There is no particular upper limit. The total light transmittance is measured in accordance with JIS K 7361-1:1997.

[0063] The resin constituting the protective resin layer is not particularly limited as long as it has a total light transmittance of preferably 40% or more and can be provided on the substrate on which the printed layer is provided. From the viewpoint of transparency and ease of providing the protective resin layer, it is preferable to attach the protective resin layer and the substrate on which the printed layer is provided via an adhesive layer, attach the protective resin layer and the substrate on which the printed layer is provided via an adhesive layer, or laminate the protective resin layer and the substrate on which the printed layer is provided by lamination processing. In the above case, examples of the resin constituting the protective resin layer include polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate; polyvinyl alcohol; and starch, and among these, at least one selected from the group consisting of polyolefins, polyesters, and polyvinyl alcohol is preferable, at least one selected from polyethylene, polypropylene, polyethylene terephthalate, and polyvinyl alcohol is more preferable, and polyethylene and polypropylene are even more preferable, and polypropylene is particularly preferable. The protective resin layer may be stretched or unstretched, and is not particularly limited. When the protective resin layer is provided by coating, examples of the resin include acrylic resins, styrene-maleic acid resins, water-soluble polyurethane resins, and water-soluble polyester resins. Examples of acrylic resins include resins obtained by copolymerizing (meth)acrylic acid with other monomers, such as alkyl esters thereof, styrene, unsaturated carboxylic acids other than (meth)acrylic acid, ethylene, and propylene. Specific examples include ethylene-(meth)acrylic acid copolymers and styrene-acrylic acid-maleic acid resins, with ethylene-(meth)acrylic acid copolymers being preferred.

[0064] The protective resin layer and the substrate having a printed layer may be laminated by any method, and there is no particular limitation. However, from the viewpoint of ease of production, it is preferable to attach the protective resin layer and the substrate having a printed layer via an adhesive layer, or to laminate them, or to apply a transparent paint in the form of a liquid paint, or to attach the protective resin layer having a printed layer and the substrate via an adhesive layer. When the protective resin layer is provided locally, it is preferable to attach it via an adhesive from the viewpoint of ease of production. When the protective resin layer is provided over a wide area, it is preferable to use a lamination process. The adhesive layer is not particularly limited and may be appropriately selected from known adhesive layers. Specific examples include the pressure-sensitive adhesive layer described in JP2012-57112A.

[0065] The thickness of the protective resin layer is not particularly limited, but from the viewpoint of suppressing swelling of the protective resin layer due to irradiation with an ultraviolet laser, obtaining clear printing, and improving the handleability of the printed matter and printing medium, it is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 12 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 50 μm or less. If the protective resin layer is thin, the protective resin layer is likely to swell due to irradiation with an ultraviolet laser.

[0066] <Sealant layer> The print medium of this embodiment has a sealant layer on the opposite side to the side on which the printed layer is provided of the substrate. The sealant layer is a layer that melts and adheres by heating, ultrasonic waves, etc. The print medium of this embodiment may have a sealant layer on both sides of the substrate. In addition, from the viewpoint of imparting heat sealability, the sealant layer is provided as the uppermost layer on at least one side, and two or more sealant layers may be formed on one side. It is sufficient that the sealant layer is provided at least on the side opposite to the side on which the printed layer is provided of the substrate, but it may also be provided on the side on which the printed layer is provided.

[0067] The resin constituting the sealant layer (hereinafter also referred to as "sealant layer resin") is not particularly limited, and examples thereof include vinyl chloride resin, vinyl acetate resin, vinyl chloride-vinyl acetate copolymer, acrylic resin, polyester resin, olefin resin, styrene resin, styrene-acrylic resin (e.g., styrene-acrylic acid copolymer), ethylene-acrylic resin (ethylene-(meth)acrylic acid copolymer), and modified products thereof. The sealant layer resin may be used alone or in combination of two or more kinds.

[0068] The resin for the sealant layer may be either a synthetic product or a commercially available product. As the commercially available product, the one used in the examples may be used.

[0069] The sealant layer may be formed by laminating with melt extrusion, adhesive, etc., and may be formed by preparing a coating liquid for the sealant layer and applying the coating liquid. A known adhesive may be used as the adhesive. The sealant layer may be formed of two or more layers. When the sealant layer is laminated with a resin film for the sealant layer with an adhesive, etc., the resin film may be unstretched or may be uniaxially or biaxially stretched.

[0070] When the sealant layer is formed by lamination, from the viewpoints of heat sealability and gas barrier property, the resin for the sealant layer more preferably contains at least one selected from the group consisting of polyolefin resins, polyamide resins, polyester resins, and polyvinylidene chloride resins, more preferably contains a polyolefin resin, and even more preferably is a polyolefin resin. When the sealant layer is a laminated sealant layer consisting of two or more layers, from the viewpoint of heat sealability, the surface opposite to the substrate (outermost layer) is preferably a polyolefin resin layer, more preferably a polyethylene resin layer.

[0071] From the viewpoint of heat sealability and gas barrier property, the polyolefin resin is more preferably at least one selected from the group consisting of polyethylene, polypropylene and an ethylene-propylene copolymer, and even more preferably at least one of polyethylene and polypropylene. The polyethylene may be low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), or high density polyethylene (HDPE).

[0072] Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 66, nylon 610, and nylon 612.

[0073] Examples of polyester resins include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and derivatives thereof. Many of the biodegradable resins described below also fall under the category of polyester resins.

[0074] Polyvinylidene chloride resin (PVDC) is a synthetic resin obtained by polymerizing vinylidene groups containing chlorine, and may be a copolymer with vinyl chloride, acrylonitrile, or the like.

[0075] Examples of biodegradable resins include polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and 3-hydroxybutanoic acid-3-hydroxyhexanoic acid copolymer (PHBH). Among these, polylactic acid (PLA) and polybutylene succinate (PBS) are preferred, and polybutylene succinate (PBS) is more preferred.

[0076] As the sealant layer, a laminate film in which two or more resins are laminated may be used, such as a polyethylene / polypropylene laminate film, a polyamide resin / polyvinylidene chloride resin laminate film, or a polyethylene / polyester resin laminate film.

[0077] When an adhesive is used to bond the sealant layer or the barrier layer described below, the adhesive used is not particularly limited and may be any of a solvent-free type, an organic solvent type, a water-based type, etc., but from the viewpoint of ensuring the shape stability of the paper base material, it is preferable to use an organic solvent-based adhesive or a solvent-free adhesive. Examples of the main component constituting the adhesive include (meth)acrylic acid ester copolymers, α-olefin copolymers, ethylene-vinyl acetate copolymers, polyvinyl alcohol, polyurethane, styrene-butadiene copolymers, polyvinyl chloride, epoxy resins, melamine resins, silicone resins, natural rubber, casein, starch, etc. Among these, from the viewpoints of easy availability and obtaining good adhesive properties, (meth)acrylic acid ester copolymers, ethylene-vinyl acetate copolymers, and polyurethanes are preferred, and polyurethanes are more preferred. As the adhesive, a commercially available adhesive may be used as appropriate, for example, a combination of Nipporan ID-816 (manufactured by Tosoh Corporation) and HARDENER 300 (manufactured by Tosoh Corporation), or a combination of Dikdry LX-500 (manufactured by DIC Corporation) and Dikdry KW-75 (manufactured by DIC Corporation). Note that, an adhesive may be applied to the sealant layer or barrier layer, and then the sealant layer or barrier layer and the substrate may be laminated thereon; an adhesive may be applied to the substrate, and then the substrate and the sealant layer or barrier layer may be laminated thereon; or an adhesive may be applied to both the sealant layer or barrier layer and the substrate, and then the two may be laminated thereon; although there are no particular limitations, from the viewpoint of shape stability, it is preferable to apply an adhesive to the sealant layer or barrier layer and then laminate the substrate.

[0078] The method for applying the adhesive may be appropriately selected from conventionally known methods, and is not particularly limited. Examples of the method include a roll coater, a die coater, a gravure coater, and a spray coater. The amount of adhesive applied is not particularly limited, but the amount applied (coating amount) after drying is preferably 1 g / m from the viewpoint of enhancing adhesion between the sealant layer or barrier layer and the substrate. 2 More preferably, 2 g / m 2 More preferably, 3 g / m 2 and preferably 40 g / m 2 Less than 20 g / m 2 More preferably, 10 g / m 2 The following is the result.

[0079] When the sealant layer is formed using a coating liquid, the resin for the sealant layer is not particularly limited as long as it has heat-sealing properties, but is more preferably one or more selected from styrene-butadiene copolymers; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; biodegradable resins; polyolefin resins such as polyethylene and polypropylene; and acrylic resins such as methyl acrylate copolymers, methyl methacrylate copolymers, styrene-acrylic copolymers, and styrene-methacrylic copolymers.

[0080] Among these, it is more preferable that the resin is at least one selected from a styrene-acrylic acid copolymer and an olefin-unsaturated carboxylic acid copolymer. In this specification, the acrylic resin does not include an olefin-unsaturated carboxylic acid copolymer.

[0081] The olefin-unsaturated carboxylic acid copolymer may be a salt in which the carboxyl groups derived from the unsaturated carboxylic acid monomer are partially or completely neutralized with an alkali metal hydroxide, ammonia, an alkylamine, an alkanolamine, or the like. Examples of the olefin monomer of the olefin-unsaturated carboxylic acid copolymer include ethylene, propylene, butadiene, etc. These may be used alone or in combination of two or more. Among these, ethylene is preferred.

[0082] Examples of the unsaturated carboxylic acid monomer of the olefin-unsaturated carboxylic acid copolymer include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butene tricarboxylic acid; unsaturated polycarboxylic acid alkyl esters having at least one carboxy group such as itaconic acid monoethyl ester, fumaric acid monobutyl ester, and maleic acid monobutyl ester; unsaturated sulfonic acid monomers or salts thereof such as acrylamidopropanesulfonic acid, acrylic acid sulfoethyl sodium salt, and methacrylic acid sulfopropyl sodium salt; and the like. These may be used alone or in combination of two or more. Among these, unsaturated carboxylic acids are preferred, acrylic acid and methacrylic acid are more preferred, and acrylic acid is particularly preferred. Therefore, the olefin-unsaturated carboxylic acid copolymer is preferably at least one of an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer.

[0083] The ethylene-unsaturated carboxylic acid copolymer is preferably obtained by emulsion polymerization of ethylene and the unsaturated carboxylic acid monomer. As the ethylene-unsaturated carboxylic acid copolymer, ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer are preferable. As long as the effect of the present invention is not impaired, the copolymer may contain a monomer composed of another compound copolymerizable with ethylene and the unsaturated carboxylic acid monomer.

[0084] Specific examples of ethylene-unsaturated carboxylic acid copolymers include ZAIXXEN (registered trademark) A, ZAIXXEN (registered trademark) AC (both manufactured by Sumitomo Seika Chemicals Co., Ltd.), Chemipearl S series (manufactured by Mitsui Chemicals, Inc.), MFHS1279, MP498345N, MP4983R, MP4990R (all manufactured by Michaelman LLC).

[0085] The biodegradable resin is preferably one or more selected from polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and poly(3-hydroxybutyrate-co-hydroxyhexanoate) (PHBH), more preferably one or more selected from polylactic acid and polybutylene succinate, and particularly preferably polylactic acid. Packaging materials using a paper substrate have the advantage of reducing the environmental load compared to packaging materials made of resin films, but by using a biodegradable resin as the sealant layer in this embodiment, the environmental load can be further reduced.

[0086] The polylactic acid may be either a commercially available product or a synthetic product. Examples of commercially available products include Randy PL-1000 and Randy PL-3000 (aqueous dispersion of polylactic acid, manufactured by Miyoshi Oil & Fat Co., Ltd.).

[0087] When the sealant layer is provided by coating, the coating liquid for the sealant layer may contain, in addition to the resin for the sealant layer (water-dispersible polymer), a lubricant, a pigment, an antifoaming agent, a viscosity adjuster, a surfactant, a leveling agent, a colorant, etc. Since these other components tend to deteriorate the heat sealability, the total content of the other components is preferably 30 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less, of the solid content of the sealant layer.

[0088] From the viewpoint of obtaining high heat seal peel strength, the content of the resin for the sealant layer in the solid content of the coating liquid for the sealant layer is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.

[0089] The device used for applying the coating liquid for the sealant layer is not particularly limited, and may be appropriately selected from commonly used coating devices, such as an air knife coater, a blade coater, a gravure coater, a rod blade coater, a roll coater, a reverse roll coater, a Mayer bar coater, a curtain coater, a die slot coater, a champlex coater, a metering blade type size press coater, a short dwell coater, a spray coater, a gate roll coater, and a lip coater.

[0090] The drying conditions for the sealant layer are not particularly limited, but the drying temperature is preferably 50 to 120° C., and the drying time is preferably 5 to 120 seconds. The drying equipment for drying the applied sealant layer is not particularly limited, and known equipment can be used. Examples of the drying equipment include a hot air dryer, an infrared dryer, an explosion-proof dryer, and a hot plate.

[0091] The amount of the sealant layer applied is preferably 1 g / m from the viewpoint of heat seal peel strength. 2 More preferably, 2 g / m 2 and preferably 30 g / m 2 Less than 20 g / m 2 When the print medium has two or more sealant layers, the total amount of the sealant applied is preferably within the above range.

[0092] <Barrier layer> The print medium of the present embodiment preferably has a barrier layer between the substrate and the sealant layer. The barrier layer is a layer having a function of mainly preventing the permeation of oxygen gas. The barrier layer may be formed by applying a coating liquid containing a polymer selected from the group consisting of water-dispersible polymers and water-soluble polymers, by laminating a resin having a barrier property by melt extrusion, adhesive, or the like, by forming a vapor deposition layer selected from the group consisting of a metal vapor deposition layer and an inorganic vapor deposition layer, or by laminating a resin film having a vapor deposition layer selected from the group consisting of a metal vapor deposition layer and an inorganic vapor deposition layer.

[0093] (Water-suspended polymer) In this embodiment, the water-suspendable polymer used in the barrier layer is a polymer having a solubility of 10 g / L or less in water at 25° C. In this embodiment, the water-suspendable polymer is preferably derived from a polymer (particle) dispersed in an emulsion. The water-suspendable polymer and water-soluble resin used in the barrier layer are not particularly limited, but examples thereof include urethane-based resins, vinylidene chloride-based resins, olefin resins, polyester resins, nylon resins, epoxy resins, melamine resins, polyvinyl alcohol-based resins, acrylonitrile-based resins, polycarboxylic acid-based resins, and silicone resins. The water-suspendable polymer may be used alone or in combination of two or more. Among them, the water-suspendable polymer is preferably at least one selected from the group consisting of urethane-based resins and vinylidene chloride-based resins. By forming the barrier layer using these resins, excellent gas barrier properties (oxygen barrier properties) can be exhibited.

[0094] The urethane resin can be produced by a known production method. For example, the urethane resin can be obtained by reacting a polyisocyanate compound (e.g., a diisocyanate compound) with a polyhydroxy acid (e.g., a dihydroxy acid). In addition, for example, the urethane resin can be obtained by reacting a polyol compound (e.g., a polyester polyol, a polyether polyol) and / or a chain extender with the polyisocyanate compound and the polyhydroxy acid. The urethane resin preferably contains at least one selected from the group consisting of a structural unit derived from meta-xylylene diisocyanate and a structural unit derived from hydrogenated meta-xylylene diisocyanate. Such a urethane resin exhibits high cohesive strength due to hydrogen bonds and a stacking effect between xylylene groups, so that the barrier layer is likely to exhibit excellent gas barrier properties. The structural unit derived from meta-xylylene diisocyanate refers to a monomer unit in a urethane resin that is reacted with meta-xylylene diisocyanate. The same applies to the structural unit derived from hydrogenated meta-xylylene diisocyanate and the structural unit derived from polyisocyanate. The monomer unit refers to a form in which a monomer substance in a polymer is reacted.

[0095] In the urethane resin, the total mol% of the meta-xylylene diisocyanate-derived structural units and the hydrogenated meta-xylylene diisocyanate-derived structural units is preferably 50 mol% or more, more preferably 60 mol% or more, based on the total amount of polyisocyanate-derived structural units in the urethane resin. There is no particular upper limit, but it is preferably 95 mol% or less, more preferably 90 mol% or less. The mol% of the structural units is 1 The identification can be performed using known analytical techniques such as H-NMR.

[0096] The urethane resin may have a hydroxyl group, and the hydroxyl value is preferably 50 mgKOH / g or more, more preferably 100 mgKOH / g or more, and even more preferably 150 mgKOH / g or more. The upper limit of the hydroxyl value is not particularly limited, but is preferably 1000 mgKOH / g or less, more preferably 800 mgKOH / g or less, and even more preferably 600 mgKOH / g or less. When the hydroxyl value of the urethane resin is within the above range, the barrier layer is more likely to exhibit oxygen barrier properties. In addition, by setting the hydroxyl value of the urethane resin within the above range, the thermal fusion property of the barrier layer can be improved, and as a result, the heat sealability of the printing medium can also be improved. The hydroxyl value is measured in accordance with JIS K0070-1992, and the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of the sample is acetylated is measured.

[0097] Urethane resin has an oxygen permeability of 100.0 mL / (m2) at 23°C and 50% relative humidity when converted into a 25 μm thick sheet. 2 ·day·atm) or less, and 50.0mL / (m 2 ·day·atm) or less, and 25.0mL / (m 2 ·day·atm) or less, and more preferably 10.0 mL / (m 2 ·day·atm) or less, and more preferably 3.0 mL / (m 2 It is particularly preferable that the oxygen permeability of the film is 0 mL / (m 2 ·day ·atm) or less when converted into a 25 μm thick sheet at 23°C and a relative humidity of 50%. 2 ·day·atm). The oxygen permeability converted to a 25 μm thick sheet is measured by forming a 25 μm thick sheet using the target urethane resin. In this specification, the oxygen permeability of the sheet is measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) at 23° C. and a relative humidity of 50%.

[0098] The glass transition temperature of the urethane resin is preferably 150° C. or less, more preferably 140° C. or less, and particularly preferably 135° C. or less. The glass transition temperature of the urethane resin is measured in accordance with JIS K 7122:2012.

[0099] As the urethane-based resin, a synthetic product may be used, and examples of the synthetic product include the urethane-based resins described in International Publication No. 2015 / 016069. As the urethane-based resin, a commercially available product may be used, and examples include "Takelac W series (product name)", "Takelac WPB series (product name)", and "Takelac WS series (product name)" manufactured by Mitsui Chemicals, Inc., and specifically, Takelac WPB-341 is exemplified. Other commercially available products include "HPU W-003" (hydroxyl value 235 mg KOH / g) manufactured by Dainichiseika Chemicals Co., Ltd.

[0100] The vinylidene chloride resin can be produced by a known production method. For example, the vinylidene chloride resin can be obtained from a homopolymer of vinylidene chloride (polyvinylidene chloride, PVDC), a copolymer of vinylidene chloride and a monomer copolymerizable with vinylidene chloride, etc. The monomer copolymerizable with vinylidene chloride is not particularly limited, but includes vinyl chloride, (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, acrylonitrile, isobutylene, and vinyl acetate.

[0101] As the vinylidene chloride resin, commercially available products may be used, for example, "Saran Latex L549B" manufactured by Asahi Kasei Corporation, or Diofan B204 manufactured by Solvay.

[0102] The weight average molecular weight of the water-suspendable polymer is preferably from 1000 to 20,000,000, and more preferably from 5,000 to 5,000,000. The weight average molecular weight is measured by gel permeation chromatography and expressed in terms of polystyrene.

[0103] The average particle size of the water-suspendable polymer in the emulsion is preferably 0.001 μm or more and 100 μm or less, more preferably 0.01 μm or more and 10 μm or less. The average particle size can be measured by a dynamic light scattering method.

[0104] (Water-soluble polymer) A water-soluble polymer is a resin that can be dissolved in water. A water-soluble resin is a polymer whose skeleton polymer has a solubility in water at 25°C of more than 10 g / L. Examples of polymers that serve as the backbone of the water-soluble polymer include polyvinyl alcohol, modified polyvinyl alcohol, starch and its derivatives, cellulose derivatives, polyvinylpyrrolidone, polyacrylic acid and its salts, casein, polyethyleneimine, etc. Among these, from the viewpoint of improving the gas barrier property, the water-soluble polymer is preferably one or more selected from the group consisting of polyvinyl alcohol and modified polyvinyl alcohol, and more preferably modified polyvinyl alcohol. Examples of modified polyvinyl alcohol include ethylene-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, silicon-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, diacetone-modified polyvinyl alcohol, etc. Among these, the modified polyvinyl alcohol is preferably one or more selected from the group consisting of ethylene-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, silicon-modified polyvinyl alcohol, and acetoacetyl-modified polyvinyl alcohol, more preferably one or more selected from the group consisting of ethylene-modified polyvinyl alcohol and carboxy-modified polyvinyl alcohol, and even more preferably ethylene-modified polyvinyl alcohol. Polyvinyl alcohol and modified polyvinyl alcohol are available in fully saponified and partially saponified forms, with fully saponified being preferred. Fully saponified means that the degree of saponification is greater than 96%. The degree of saponification is a value measured according to a method in accordance with JIS K 6726:1994.

[0105] As the water-soluble polymer, a commercially available product may be used, for example, modified polyvinyl alcohol such as "Exceval (product name)" manufactured by Kuraray Co., Ltd.

[0106] From the viewpoint of improving the barrier properties, the content of the water-suspendable polymer and water-soluble polymer in the barrier layer is preferably 10 mass % or more, more preferably 30 mass % or more, even more preferably 50 mass % or more, and still more preferably 60 mass % or more, of the solid content of the barrier layer, with the upper limit being 100 mass %.

[0107] The barrier layer may be formed by applying a coating liquid for a barrier layer to a paper substrate, or by laminating a resin film to which the coating liquid for a barrier layer has been applied in advance. The resin film may be a sealant layer.

[0108] When the barrier layer is formed by coating, it is preferable to contain a layered inorganic compound in addition to at least one selected from the water-suspendable polymer and the water-soluble polymer. That is, it is preferable that the barrier layer contains a water-suspendable polymer and a layered inorganic compound, or a water-soluble polymer and a layered inorganic compound. By containing a layered inorganic compound in the barrier layer, the barrier properties can be further improved (oxygen permeability can be further reduced).

[0109] The average length of the layered inorganic compound is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 50 μm or less, and even more preferably 3 μm or more and 20 μm or less. Here, the average length of the layered inorganic compound refers to the average length of the major axis in the planar direction of the layered inorganic compound. When the average length is 1 μm or more, the layered inorganic compound in the barrier layer is easily arranged parallel to the paper support. Also, when the average length is 100 μm or less, there is less concern that a part of the layered inorganic compound will protrude from the barrier layer.

[0110] The aspect ratio of the layered inorganic compound is preferably 200 or more, more preferably 300 or more, even more preferably 500 or more, and even more preferably 800 or more. The upper limit of the aspect ratio of the layered inorganic compound is not particularly limited, but is preferably 10,000 or less, more preferably 5,000 or less, and even more preferably 2,000 or less. When the aspect ratio of the layered inorganic compound is within the above range, the barrier property is improved, and the coating amount of the barrier layer can be reduced, thereby improving the recyclability and lightness of the printing medium. Here, the aspect ratio is a value calculated from a microscopic magnified photograph of the cross section of the barrier layer, and is the average value (arithmetic mean value of 20 to 30 samples) of the length of the layered inorganic compound divided by its thickness.

[0111] The thickness of the layered inorganic compound is preferably 100 nm or less, more preferably 50 nm or less, and further preferably 30 nm or less. The lower limit of the thickness of the layered inorganic compound is not particularly limited, but is preferably 2 nm or more. Here, the thickness of the layered inorganic compound is the average thickness of the layered inorganic compound measured from a microscopic magnified photograph of the cross section of the barrier layer (arithmetic mean value of 20 to 30 samples). The thickness is measured in the direction perpendicular to the long axis of the layered inorganic compound. By setting the average thickness of the layered inorganic compound within the above range, the number of layers of the layered inorganic compound in the barrier layer increases, so that the barrier layer can exhibit higher oxygen barrier properties. In particular, when a layered inorganic compound having a large aspect ratio and a small thickness is used, the barrier layer forms a dense film without voids. This phenomenon can also be observed from a microscopic magnified photograph of the cross section of the barrier layer.

[0112] Specific examples of the layered inorganic compound include mica such as mica group and brittle mica group, bentonite, kaolinite (kaolin mineral, hereinafter also referred to as "kaolin"), pyrophyllite, talc, smectite, vermiculite, chlorite, septe chlorite, serpentine, stilpnomelane, montmorillonite, etc. Among these, from the viewpoint of improving the water vapor barrier property, the layered inorganic compound is preferably at least one selected from the group consisting of mica, bentonite, and kaolin, and more preferably at least one selected from mica and kaolin. Examples of mica include synthetic mica, white mica (muscovite), sericite (sericite), phlogopite mica (phlocopite), black mica (biotite), fluorine phlogopite (artificial mica), red mica, soda mica, vanadium mica, illite, chin mica, paragonite, brittle mica, etc. Among them, the mica is preferably swellable mica because of its high aspect ratio. The kaolin may be a natural product or a synthetic product (engineered kaolin). Among these, at least one selected from the group consisting of mica, bentonite and kaolin is preferable, and at least one selected from mica and kaolin is more preferable. By containing the layered inorganic compound as described above in the barrier layer, the barrier property of the printing medium under high humidity conditions can be more effectively improved.

[0113] When a layered inorganic compound is contained in the barrier layer, the content of the layered inorganic compound is not particularly limited, but is preferably from 0.5 to 500 parts by mass, more preferably from 1 to 300 parts by mass, even more preferably from 2 to 200 parts by mass, still more preferably from 5 to 150 parts by mass, and particularly preferably from 10 to 70 parts by mass, relative to 100 parts by mass of the water-suspendable polymer or water-soluble polymer in the barrier layer. By setting the content of the layered inorganic compound within the above range, the barrier property of the printing medium under high humidity conditions can be more effectively improved.

[0114] The barrier layer may contain, in addition to at least one selected from a water-dispersible polymer and a water-soluble polymer and a layered inorganic compound, a pigment, a dispersant, a surfactant, a defoamer, a wetting agent, a dye, a color adjuster, a thickener, etc.

[0115] When the barrier layer is provided by coating, the coating amount of the coating solution for the barrier layer is preferably 0.1 g / m in terms of solid content. 2 More than 10g / m 2 Less than 0.5 g / m 2 More than 5g / m 2 The following is the result.

[0116] (Resin with barrier properties) When the barrier layer is formed by laminating a resin having a barrier property by melt extrusion, adhesive or the like, examples of the resin having a barrier property include ethylene-vinyl alcohol copolymer (EVOH) and MX nylon. As the EVOH, commercially available products may be used, for example, the EVAL series manufactured by Kuraray Co., Ltd. An example of MX nylon is MXD6 manufactured by Mitsubishi Gas Chemical Company, Inc.

[0117] (deposited layer) The barrier layer may be formed by forming a vapor deposition layer directly on the paper substrate, or by laminating a resin film on which a vapor deposition layer has been formed. The vapor-deposited layer is selected from the group consisting of a metal vapor-deposited layer and an inorganic vapor-deposited layer. An example of the metal to be deposited in the metal deposition layer is aluminum (Al), and an example of the inorganic compound to be deposited in the inorganic deposition layer is silica (SiOx) or alumina (AlOx). The thickness of the metal vapor deposition layer is not particularly limited as long as the desired barrier properties are obtained.

[0118] As the barrier layer, an adhesive may be applied to a resin film provided with a vapor deposition layer, and the resin film may be laminated with a paper substrate. Examples of the resin film include polyester-based resin films such as polyethylene terephthalate (PET), polyamide-based resin films such as various nylons, polyethylene-based resins, polypropylene-based resins, cyclic polyolefin resins, polystyrene-based resins, acrylonitrile-styrene copolymers (AS resins), acrylonitrile-butadiene-styrene copolymers (ABS resins), polyolefin films such as polybutene resin films, polyvinyl chloride-based resins, polycarbonate-based resins, polyimide-based resins, polyamideimide-based resins, polyarylphthalate resins, silicone-based resins, polysulfone-based resins, polyphenylene sulfide-based resins, polyethersulfone-based resins, polyurethane-based resins, cellulose-based resins, poly(meth)acrylic resins, polyvinylidene chloride films, acetal-based resin films, fluorine-based resins, and the like. In particular, polypropylene-based resins, polyester-based resins, and polyamide-based resins are preferred.

[0119] [Printed matter and method of manufacturing printed matter] The printed matter of this embodiment is a printed matter obtained from the above-mentioned ultraviolet laser printing medium, and has a printed area having discolored titanium oxide in at least a part thereof. The ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is preferably 0.70 or less. The printed area having discolored titanium oxide is an area containing titanium oxide discolored by irradiation with an ultraviolet laser, and is an ultraviolet laser irradiated area, i.e., a printed area. The method for producing a printed matter according to the present embodiment also includes a step of irradiating the above-mentioned printing medium with an ultraviolet laser to discolor the irradiated area, thereby printing. Examples of the printing medium used in the method for producing a printed matter of this embodiment include the above-mentioned printing media, and the preferred ranges are also the same. In the method for producing a printed matter of this embodiment, it is sufficient that a printing layer is provided at least in the ultraviolet laser irradiated area, and a printing layer does not have to be provided in the non-irradiated area.

[0120] In the method for producing a printed matter, it is preferable to irradiate with an ultraviolet laser so that the ratio of the Raman intensity due to titanium oxide in the printed area to the Raman intensity due to titanium oxide in the non-printed area is 0.70 or less. In addition, in the printed matter, the printed area means an area (part) in the printable area that contains discolored titanium oxide, and is an area (part) that is printed with an ultraviolet laser. The non-printed area means an area (part) in the printable area that is not printed. The printable area means the entire area containing titanium oxide, including the area printable with an ultraviolet laser and, if present, the area (part) that is printed with an ultraviolet laser, in the ultraviolet laser printing medium or printed matter, and the non-printable area means an area other than the printable area in the ultraviolet laser printing medium or printed matter. It is preferable to print so that the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area (Raman intensity of the printed area / Raman intensity of the non-printed area) is 0.70 or less. By keeping the ratio of Raman intensities within the above range, a printed matter with excellent visibility can be obtained. The ratio of the above Raman intensities (Raman intensity in the printed area / Raman intensity in the non-printed area) is 447±10 cm when rutile titanium oxide is used as the titanium oxide, which is the Raman intensity derived from titanium oxide. -1 In addition, when anatase-type titanium oxide is used as the titanium oxide, the Raman intensity at 516±10 cm is compared. -1 The Raman intensities of the maximum values ​​in the wavenumber range are compared. In addition, when rutile titanium oxide and anatase titanium oxide coexist, the Raman intensity derived from rutile titanium oxide is used for comparison.

[0121] In the printed matter obtained in this embodiment, it is preferable that the non-printed areas are white and the printed areas are black. The non-printed areas preferably have a value of 10 on the Munsell color system, i.e., are white. On the other hand, the printed areas preferably have a value of any one of 0 to 8 on the Munsell color system, more preferably 0 to 6, and even more preferably 0 to 4. In order to obtain a color in the Munsell color system described above, it is preferable to appropriately adjust the titanium oxide content of the printing layer in the printing medium, the crystallite size of the titanium oxide, the thickness of the protective resin layer, other characteristics (resin type, thickness of the printing layer, etc.), and the irradiation conditions of the ultraviolet laser (e.g., average output, repetition frequency, wavelength, etc.).

[0122] [UV laser irradiation conditions] From the viewpoint of improving the visibility of the printed area, the wavelength of the ultraviolet laser is preferably 370 nm or less, more preferably 365 nm or less, even more preferably 360 nm or less, and is preferably 260 nm or more, more preferably 340 nm or more, even more preferably 350 nm or more.

[0123] From the viewpoint of improving the visibility of the printed area, the average output of the ultraviolet laser is preferably 0.3 W or more, more preferably 0.8 W or more, even more preferably 1.2 W or more, and even more preferably 1.8 W or more, and from the viewpoint of economy, it is preferably 30 W or less, more preferably 25 W or less, even more preferably 20 W or less, even more preferably 15 W or less, even more preferably 10 W or less, and even more preferably 6 W or less.

[0124] From the viewpoint of improving the visibility of the printed area, the repetition frequency (frequency) of the ultraviolet laser is preferably 10 kHz or more, more preferably 20 kHz or more, even more preferably 30 kHz or more, and is preferably 100 kHz or less, more preferably 80 kHz or less, even more preferably 60 kHz or less.

[0125] From the viewpoint of obtaining a clear image and ease of printing, the spot diameter of the ultraviolet laser is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and is preferably 300 μm or less, more preferably 240 μm or less, even more preferably 180 μm or less, even more preferably 120 μm or less.

[0126] From the viewpoints of high-speed printing and visibility of the printed area, the scanning speed of the ultraviolet laser is preferably 500 mm / sec or more, more preferably 1000 mm / sec or more, even more preferably 2000 mm / sec or more, and is preferably 7000 mm / sec or less, more preferably 6000 mm / sec or less, even more preferably 5000 mm / sec or less.

[0127] From the viewpoint of obtaining a clear image and of the ease of obtaining the equipment, the filling interval (line pitch) of the ultraviolet laser is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and is preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less.

[0128] [Embodiments of the method for producing printed matter] The method for producing a printed matter of the present invention can be carried out in various modes. Various examples of the printed matter manufacturing method of the present embodiment are described below, but the printed matter manufacturing method of the present embodiment is not limited to the following examples. The information to be printed is not particularly limited, but is preferably variable information. The method for producing a printed matter according to the present embodiment is preferably carried out in-line. (1) Direct printing on packaging A first embodiment of the method for producing printed matter of this embodiment is a method for printing information on a packaging body having the printing medium of this embodiment, and includes a step of printing directly on the packaging body using an ultraviolet laser while it is moving on a packaging line or while it is intermittently stopped. In the first method for producing a printed matter, a package is produced using the ultraviolet laser printing medium of the present embodiment, and is directly printed with an ultraviolet laser. Note that it is sufficient that at least the outermost layer of the printed area of ​​the package is produced using the printing medium. Furthermore, examples of the packaging include cardboard and boxes, and it is preferable to print directly on the side or top surface of the packaging with an ultraviolet laser.

[0129] The packaging line may also have a coating mechanism, such as a contact printer, a pad printer, or a spray coater. In this embodiment, the process includes a step of applying a printing layer and a protective resin layer by a coating mechanism while the packaging body is moving on the packaging line, and a step further downstream of the process of directly printing on the packaging body with an ultraviolet laser while the packaging body is moving on the packaging line or during intermittent stops.

[0130] (2) Printing on labels A second embodiment of the method for producing a printed matter of this embodiment is a method for printing information on a label having the print medium of this embodiment. The print medium constituting the printing surface of the label is the print medium of this embodiment. The printed label is preferably applied to the package using a label application device, of which various types have been proposed, and which has a printing layer and a protective resin layer on the surface to be irradiated with ultraviolet light. The first label application device applies adhesive to a roll of label base paper and then applies the label base paper to an article. More specifically, a roll labeler includes a cutting means for cutting the roll of label base paper into a predetermined length one by one, a gluing conveying means for receiving the label base paper cut by the cutting means with a label base paper holder coated with adhesive and applying the adhesive to the back surface of the label base paper, and an application means for receiving the label base paper (label) to which adhesive has been applied from the gluing conveying means and applying the label to an article such as a container. A roll labeler having a rotating conveying means with a label holding surface on its outer surface provided between the cutting means and the gluing conveying means is exemplified in JP-A-6-64637. Further examples include a roll labeler having a cutting means for cutting the rolled label base paper one sheet at a time to a specified length, a transfer roll for transferring the label base paper to the application roll, and a gluing roll for applying glue to the label base paper held by the application roll, and an embodiment in which the transfer roll is not required. The ultraviolet laser irradiation is preferably performed before cutting the rolled label base paper to a predetermined length, or after cutting and before transferring to the next roll, etc. Depending on the type of roll labeler, the front or back surface of the rolled label base paper will be the front or back surface when affixed to a package, so the ultraviolet laser irradiation is performed accordingly. The label base paper does not only refer to a case where the substrate is paper, but also refers to a case where the substrate is a film substrate.

[0131] The second labeling device uses an adhesive label roll as the label. In this case, at least the surface to be irradiated with the ultraviolet laser, which is the surface opposite to the surface to which the adhesive is applied, has a print layer and a protective resin layer. In the case of using an adhesive label roll with a release paper, for example, an application device having a release paper separating means for separating the adhesive label from the release paper, a delivery roll for receiving the adhesive label from which the release paper has been separated, and an application roll for sucking the adhesive label from the delivery roll and applying it to an article (package) is exemplified. Irradiation with an ultraviolet laser is preferably performed before separating the release paper, or after separating the release paper and before the label is carried by the application roll. Another example is an apparatus that sets an adhesive label roll with a release paper, has a mechanism for separating the adhesive label from the release paper, and has a mechanism for attaching a label immediately after separation, and performs printing with an ultraviolet laser before the release paper is separated from the set adhesive label roll. The above-mentioned adhesive label attachment method is also called flow attachment. Further, a label application device is exemplified that has a mechanism for setting an adhesive label roll with a release paper, separating the release paper from the adhesive label, and attaching the adhesive label to an article (package), the mechanism being a syringe type, an air jet type, or a robot arm type. Irradiation with an ultraviolet laser is preferably performed until the release paper is separated from the set adhesive label roll with the release paper.

[0132] A linerless adhesive label may be used as the label. A linerless adhesive label is a label without a release paper, and has the characteristics that the number of labels per roll is greater than when an adhesive label roll with a release paper is used, and that the absence of a release paper makes it inexpensive. When a linerless adhesive label is used, a printing layer is formed on the surface irradiated with the ultraviolet laser, which is the opposite side to the surface to which the adhesive is applied. An example of a label application device using linerless adhesive labels is a device having a mechanism for setting a linerless label roll, a cutting mechanism for cutting the linerless labels one by one, and an application mechanism for applying the cut linerless labels to an article (package), the application mechanism being of a cylinder type or a robot arm type. Printing by irradiation with an ultraviolet laser is preferably performed between the mechanism for setting the linerless label roll and the cutting mechanism, or while the cut linerless labels are being sent to the application mechanism.

[0133] The third label application device applies the print medium of the present embodiment to an article (package), and then prints with an ultraviolet laser. For the method of attaching the label, reference is made to the first and second devices described above.

[0134] (3) Printing on adhesive tape In a third embodiment of the method for producing a printed matter according to the present embodiment, the printing medium is an adhesive tape. In this case, a printing layer is provided on the surface opposite to the surface on which the adhesive is applied. That is, the method for producing a printed matter of the third embodiment includes a step of attaching an adhesive tape made from the printing medium to an item (packaging material), and a step of printing with an ultraviolet laser before or after the attaching step. A printing device incorporating an ultraviolet laser printer in a cardboard sealing machine may also be used. Specifically, the printing device has a mechanism for setting the adhesive tape winding, a conveyor for transporting the cardboard, a mechanism for folding the flaps of the cardboard, a mechanism for sealing the cardboard by applying adhesive tape, and a mechanism for printing on the adhesive tape with an ultraviolet laser during or after the application of the adhesive tape.

[0135] The method for producing a printed matter according to the present embodiment is not limited to the above-described embodiment, but can be applied to various uses where printing is required.

[0136] In this embodiment, the printed matter obtained by the method for producing a printed matter is suitable for use as packaging materials, labels, adhesive tapes, and the like. Examples of packaging bodies include outer bags, outer boxes, milk cartons, aseptic paper cartons, paper cups and other liquid containers for beverages (preferably liquid containers for beverages), and skin packs; examples of labels include label base paper, adhesive labels, and adhesive sheets; and examples of adhesive tapes include adhesive tapes and craft tapes.

[0137] [Processed products] The ultraviolet laser printing medium and the printed matter of the present embodiment are applied to various processed products. That is, the processed products of the present embodiment are made by using the ultraviolet laser printing medium of the present embodiment or the printed matter of the present embodiment. Suitable processed products of this embodiment include packaging, labels, and adhesive tapes. Examples of packaging bodies include liner paper for cardboard (particularly the outermost liner paper), outer boxes, liquid containers for beverages such as milk cartons and paper cups (preferably liquid containers for beverages), food trays, skin packs, pillow packaging, standing pouches, three-side and four-side sealed packaging, etc. Examples of labels include label paper, adhesive labels, and adhesive sheets, and examples of adhesive tapes include adhesive tapes and craft tapes. 1, a liquid container 10 as an example of a package has, for example, a print area 20 on its surface. The print area 20 is irradiated with an ultraviolet laser and has characters such as a date printed thereon.

[0138] [Ink composition] The ink composition of this embodiment contains titanium oxide having a crystallite size of 13 nm or more and 53 nm or less, and is used to form a printed layer that changes color when irradiated with an ultraviolet laser. By printing on an ultraviolet laser printing medium having a printed layer formed with the ink composition of this embodiment by irradiating with an ultraviolet laser, an image with excellent printing clarity for each point can be obtained. The titanium oxide contained in the ink composition and its content therein are exemplified by the titanium oxide contained in the printing layer of the above-mentioned ultraviolet laser printable medium and the content of titanium oxide in the coating liquid, and the preferred ranges are also the same. Further, other components contained in the ink composition may include each of the components that may be contained in the coating liquid described above, such as a thermoplastic resin, an inorganic pigment, a film-forming agent, a pigment dispersant, a pigment dispersing resin, an antiblocking agent, a wetting agent, a viscosity adjuster, a pH adjuster, an antifoaming agent, a general surfactant, etc., and preferred aspects of these components are the same as the preferred aspects of the coating liquid described above. EXAMPLES

[0139] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. In addition, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.

[0140] [Titanium oxide] The titanium oxides used in the examples and comparative examples are as shown in Table 1 below.

[0141] [Table 1]

[0142] <Synthesis method of titanium oxide F, G, I, J> Titanium oxide (amorphous) was synthesized by hydrolysis and condensation polymerization of titanium tetraisopropoxide (TTIP), and was crystallized by calcination. Specifically, the synthesis was carried out according to the following steps (1) to (6). (1) The following solutions A to C were prepared using TTIP (Tokyo Chemical Industry Co., Ltd., product code: T0133), isopropanol (Tokyo Chemical Industry Co., Ltd., purity 99.5% or higher, product code: I0163), and ion-exchanged water. Solution A: 35.6 parts by weight of TTIP, 200 parts by weight of isopropanol Solution B: 200 parts by weight of isopropanol, 6.3 parts by weight of ion-exchanged water Solution C: 200 parts by weight of isopropanol, 24.4 parts by weight of ion-exchanged water (2) While stirring solution A with a Teflon (registered trademark) stirring blade, solution B was slowly added dropwise, and stirring was continued for 10 minutes. (3) Solution C was slowly added dropwise to the mixture of Solution A and Solution B obtained in (2) above, and the mixture was stirred for 1 minute and then allowed to stand at room temperature for 24 hours. (4) The precipitate was separated into solid and liquid using a membrane filter (manufactured by Advantec, material: cellulose acetate). (5) After washing with isopropanol, it was dried at 100°C for 5 hours to obtain titanium oxide (amorphous). (6) The mixture was fired in a muffle furnace to crystallize the titanium oxide. The firing was performed at the temperatures shown in the table, with a temperature rise rate of 10° C. / min and firing for 2 hours after the temperature rise.

[0143] [Example 1-1] <Manufacturing of paper base material> A pulp slurry of bleached hardwood kraft pulp (LBKP, α-cellulose 88%) was beaten using a double disc refiner to a disintegration freeness (CSF: Canadian Standard Freeness) of 450 mL to obtain a pulp slurry. To 100 parts of the obtained pulp slurry (solid content), 0.30 parts (solid content equivalent) of an amphoteric polyacrylamide-based paper strength agent (Seiko PMC Corporation, DS4430) as an internal paper strength agent, 0.5 parts (solid content equivalent) of a rosin sizing agent (Arakawa Chemical Industries, Ltd., Size Pine N-811) as an internal sizing agent, and 1.0 part (solid content equivalent) of aluminum sulfate were added to prepare a paper stock. Using this paper stock, a basis weight of 40 g / m was obtained.2 The thickness of the paper base material was 55 μm.

[0144] <Preparation of coating liquid> To 100 parts by mass of gravure ink medium (DIC Corporation, Lami CP Medium, resin component: nitrocellulose, solids concentration: 24.1%), 16.1 parts by mass of the titanium oxide shown in the table was added as solids, and using a Corless disperser, ink A for gravure printing with a titanium oxide concentration of 40% in the solids was prepared.

[0145] <Formation of printing layer> A gravure printing machine (10-color machine, plate depth: 50 μm, drying temperature after printing: 80° C., printing speed: 80 m / min) was used to coat the substrate with the titanium oxide content shown in the table. The printing layer was applied to the smoother side of the paper base material.

[0146] <Formation of protective resin layer> PE resin (manufactured by Japan Polyethylene Corporation, product number: LC522) was put into a single-screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., 50C150), melt-laminated on the printed layer to a resin thickness of 15 μm, and then rapidly cooled while being sandwiched between cooling rolls adjusted to 20° C., forming a protective resin layer on the printed layer. The melting temperature was 320° C.

[0147] <Formation of sealant layer> PE (low density polyethylene, manufactured by Japan Polyethylene Co., Ltd., Novatec (registered trademark) LD LC522) was fed into a single screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., D2025), and extrusion laminated (melt laminated) on the side opposite to the side on which the printed layer of the paper substrate was provided so that the resin had a thickness of 15 μm, and then it was quickly quenched while being sandwiched between cooling rolls adjusted to 20° C. to provide a sealant layer, thereby obtaining a medium for ultraviolet laser printing. The melting temperature of the resin in the extrusion lamination was 320° C.

[0148] [Examples 1-2 to 1-7, Comparative Examples 1-1 to 1-3] In preparing the coating liquid, the titanium oxide used was changed to the titanium oxide shown in Table 2, and inks B to G and inks H to J were prepared and used as the coating liquid. Except for this, ultraviolet laser printing media were obtained in the same manner as in Example 1-1.

[0149] [Examples 1-8] An ultraviolet laser printing medium was obtained in the same manner as in Example 1-4, except that Ink D prepared in Example 1-4 was used, the printing plate of the gravure printing machine was changed to a printing plate with a plate depth of 15 μm, and the substrate was coated with the titanium oxide content shown in the table.

[0150] [Examples 1-9, 1-10] An ultraviolet laser printing medium was obtained in the same manner as in Example 1-4, except that Ink D prepared in Example 1-4 was used, the number of prints on the gravure printing machine was changed to two (Example 1-9) or three (Example 1-10), and the substrate was coated with the titanium oxide content shown in the table.

[0151] [Examples 1-11 and 1-12] An ultraviolet laser printable medium was obtained in the same manner as in Example 1-4, except that the thickness of the protective resin layer was changed to the thickness shown in the table.

[0152] [Examples 1-13] An ultraviolet laser printing medium was obtained in the same manner as in Example 1-4, except that in the production of the paper base material, hardwood bleached kraft pulp (LBKP, 85% α-cellulose) was used and beaten to a disintegrated freeness of 350 mL.

[0153] [Examples 1-14] An ultraviolet laser printing medium was obtained in the same manner as in Example 1-4, except that in the production of the paper base material, hardwood dissolving pulp (LBDP, 94% α-cellulose) was used and beaten to a disintegrated freeness of 550 mL.

[0154] [Examples 1-15] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> On the surface of a PE film (linear low-density polyethylene film (LLDPE), Futamura Chemical Co., Ltd., LL-XLTN, thickness 25 μm), an isocyanate adhesive (a mixture of 10 parts of DIC Corporation's Dick Dry LX-500 and 1 part of DIC Corporation's Dick Dry KW-75) was applied at a rate of 5 g / m. 2 After coating with the ink, the substrate side of the substrate on which the print layer and protective layer were formed was attached to obtain an ultraviolet laser printable medium.

[0155] [Example 1-16] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> A sealant layer was formed in the same manner as in Example 1-4, except that PE was changed to PP (polypropylene, manufactured by Mitsubishi Chemical Corporation, Novatec PP MA-3) and the melting temperature was changed to 330° C., to obtain an ultraviolet laser printing medium.

[0156] [Example 1-17] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> A sealant layer was formed in the same manner as in Example 1-15, except that the PE film was changed to a CPP film (non-oriented polypropylene film, manufactured by Futamura Chemical Co., Ltd., FHK2-L, thickness 25 μm), and an ultraviolet laser printing medium was obtained. The film was a laminated film of COPP (copolymerized polypropylene) / CoPP (copolymerized polypropylene) / special PP, and the corona-treated CoPP surface was placed on the paper substrate side.

[0157] [Example 1-18] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> Water was added to a water-based heat sealant (ethylene-acrylic acid copolymer (Et-AA in the table), Michaelman, MFHS1279, solids concentration 42%) to dilute it to a solids concentration of 20%, and a coating amount (solids content) of 5 g / m was applied to the side of the paper base opposite the side on which the printed layer was provided. 2 The coating was then dried at 120° C. for 60 seconds to form a sealant layer, thereby obtaining an ultraviolet laser printing medium.

[0158] [Example 1-19] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> A sealant layer was formed and an ultraviolet laser printing medium was obtained in the same manner as in Example 1-18, except that an aqueous heat sealing agent (ethylene-methacrylic acid copolymer (Et-MAA in the table), Mitsui Chemicals, Inc., Chemipearl S-300, solids concentration 35%) was used with a solids concentration adjusted to 20%.

[0159] [Example 1-20] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Formation of sealant layer> A sealant layer was formed and an ultraviolet laser printing medium was obtained in the same manner as in Example 1-18, except that an aqueous heat sealing agent (styrene-acrylic acid copolymer (St-AA in the table), manufactured by Seiko PMC Corporation, SEIKOAT RE-2016, solids concentration 35%) was used with a solids concentration adjusted to 20%.

[0160] [Example 1-21] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Barrier layer formation> EVOH (ethylene-vinyl alcohol copolymer, EVAL E105B, manufactured by Kuraray Co., Ltd.) was put into a single screw extruder (D2025, manufactured by Toyo Seiki Seisakusho Co., Ltd.) and extrusion laminated (melt laminated) on the side opposite the printed layer of the substrate so that the resin had a thickness of 15 μm, and then it was quickly quenched while being sandwiched between cooling rolls adjusted to 20°C to form a barrier layer. The melting temperature of the resin in the extrusion lamination was 215°C. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 1-4 to obtain an ultraviolet laser printable medium.

[0161] [Example 1-22] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Barrier layer formation> To 100 parts of an aqueous solution of ethylene-modified polyvinyl alcohol (fully saponified, Kuraray Co., Ltd., Exeval AQ-4104) with a solid content concentration of 15 mass%, 50 parts of an aqueous dispersion of a layered inorganic compound (layered inorganic compound=synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: about 1000, thickness: about 5 nm), solid content concentration of 6 mass%, Topy Industries, Ltd., NTO-05) was added, and dilution water was further added thereto to adjust the solid content concentration to 10 mass%, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was applied in a coating amount of 2.0 g / m 2 The coating was then applied to the opposite side of the substrate from the side on which the printed layer was formed using a Mayer bar so that the coating had a thickness of 100 μm. Thereafter, the substrate was dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 1-18 to obtain an ultraviolet laser printing medium.

[0162] [Example 1-23] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Barrier layer formation> A water dispersion of a layered inorganic compound (layered inorganic compound = synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: approximately 1000, thickness: approximately 5 nm), solid content concentration 6 mass%, manufactured by Topy Industries, Ltd., NTO-05) was mixed with a urethane emulsion (solid content concentration 30 mass%, glass transition temperature 130°C, oxygen permeability when formed into a 25 μm thick sheet was 2.0 mL / (m 2 1.0 g / m2 (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc.) was added to the mixture so that the mass ratio of solids (layered inorganic compound:urethane resin) was 2:10, and the mixture was stirred. Further, dilution water was added so that the solids concentration was 20 mass %, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was diluted with 1.0 g / m2 of the mixture so that the coating amount of the barrier layer was 2.0 g / m2. 2 After coating the substrate on the side opposite the printed layer with a Mayer bar so as to obtain a coating composition as shown in FIG. 1, the substrate was dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 1-18 to obtain an ultraviolet laser printing medium.

[0163] [Example 1-24] A print layer and a protective layer were formed on a paper substrate in the same manner as in Example 1-4. <Barrier layer formation> Aluminum-deposited PP film (base material = CPP (non-oriented polypropylene film), manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: ML, thickness 20 μm, water vapor permeability 0.2 g / m 2 ·day, oxygen permeability 50mL / m 2 On the surface of the PP film of the 100-m2 ... 2 After coating, the adhesive was attached to the surface of the substrate opposite to the surface on which the printed layer was provided. <Formation of sealant layer> A sealant layer was formed in the same manner as in Example 1-4, and an ultraviolet laser printable medium was obtained.

[0164] [Example 1-25] In forming the barrier layer, an aluminum-deposited PET film (substrate: PET (polyethylene terephthalate), manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: ML, thickness: 12 μm, water vapor permeability: 1 g / m 2 ·day, oxygen permeability 10mL / m 2 An ultraviolet laser printing medium was obtained in the same manner as in Example 1-24, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PET) side of the aluminum-deposited PET film.

[0165] [Example 1-26] In forming the barrier layer, a silica-deposited PP film (substrate: PP, manufactured by Toppan Printing Co., Ltd., product name: GL-LP, thickness: 17 μm, water vapor permeability: 0.5 g / m 2 ·day, oxygen permeability 1mL / m 2 An ultraviolet laser printing medium was obtained in the same manner as in Example 1-24, except that a 1000-milliliter (1.0-1.0-cm2) UV laser printing medium was obtained using ...

[0166] [Example 1-27] In forming the barrier layer, a silica-deposited PET film (substrate = PET, manufactured by Toppan Printing Co., Ltd., product name: GL-AE, thickness 12 μm, deposition layer thickness 400 nm, water vapor permeability 0.6 g / m 2 ·day, oxygen permeability 0.2mL / m 2 An ultraviolet laser printable medium was obtained in the same manner as in Example 1-24, except that a 1000-milliliter (1.0-1.0-g / kg) ...

[0167] [Example 1-28] In forming the barrier layer, an alumina-deposited PET film (substrate: PET, manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: TL, thickness: 12 μm, water vapor permeability: 1.5 g / m 2 ·day, oxygen permeability 15mL / m 2 An ultraviolet laser printing medium was obtained in the same manner as in Example 1-24, except that a 1000-milliliter (1.0-1.0 m / s) ...

[0168] [Example 1-29] To form the barrier layer, a PET film coated with PVDC (polyvinylidene chloride) (manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: V Barrier, thickness 12 μm, water vapor permeability 0.2 g / m 2 ·day, oxygen permeability 0.8mL / m 2 An ultraviolet laser printable medium was obtained in the same manner as in Example 1-24, except that a PVDC-coated PET film was used. The adhesive was applied to the substrate (PET) side of the PVDC-coated PET film.

[0169] [Comparative Example 1-4] In preparing the coating liquid, the titanium oxide used was changed to the titanium oxide shown in Table 2, and 0.05 parts by mass of the titanium oxide shown in the table was added as solid content to 100 parts by mass of gravure ink medium (manufactured by DIC Corporation, Lami CP medium, resin component: nitrocellulose, solid content concentration: 24.1%), and a Corless disperser was used to prepare ink K for gravure printing with a titanium oxide concentration of 0.2% in the solid content. A medium for ultraviolet laser printing was obtained in the same manner as in Example 1-1, except that ink K was used to coat the substrate so as to obtain the titanium oxide content shown in the table.

[0170] [Comparative Example 1-5] An ultraviolet laser printing medium was obtained in the same manner as in Example 1-4, except that Ink D prepared in Example 1-4 was used, the number of prints on the gravure printing machine was changed to 9, and the substrate was coated with the titanium oxide content shown in the table.

[0171] [Comparative Example 1-6] An ultraviolet laser printable medium was obtained in the same manner as in Example 1-4, except that the sealant layer was not formed.

[0172] [Example 2-1] <Film substrate> The film substrate used was CPP film (manufactured by Futamura Chemical Co., Ltd., product number: FCMLVK, thickness 25 μm). <Preparation of coating liquid> Ink A prepared in Example 1-1 was used. <Formation of Printing Layer and Protective Layer> Using a gravure printing machine (10-color machine, plate depth: 50 μm, drying temperature after printing: 80°C, printing speed: 80 m / min), the protective resin layer was reverse-printed to the titanium oxide content shown in the table. Then, a polyether urethane laminating adhesive (TM320 / CAT13B manufactured by Toyo-Morton Co., Ltd.) was applied at a solid content of 1.5 g / m 2 The coated surface was coated and dried so that the above-mentioned condition was satisfied, and then the coated surface was attached to a film substrate and dry laminated to obtain a medium for ultraviolet laser printing. As the protective resin layer, an OPP film (manufactured by Futamura Chemical Co., Ltd., product number: FOS-BT, thickness 30 μm) was used.

[0173] <Formation of sealant layer> PE (low density polyethylene, manufactured by Japan Polyethylene Co., Ltd., Novatec (registered trademark) LD LC522) was fed into a single screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., D2025), and extrusion laminated (melt laminated) on the side opposite to the side on which the printed layer of the paper substrate was provided so that the resin had a thickness of 15 μm, and then it was quickly quenched while being sandwiched between cooling rolls adjusted to 20° C. to provide a sealant layer, thereby obtaining a medium for ultraviolet laser printing. The melting temperature of the resin in the extrusion lamination was 320° C.

[0174] [Examples 2-2 to 2-5] An ultraviolet laser printable medium was obtained in the same manner as in Example 2-1, except that the coating liquid used in Example 2-1 was changed to Ink B to Ink E shown in Table 3.

[0175] [Example 2-6] A print layer and a protective layer were formed on the film substrate in the same manner as in Example 2-4. <Barrier layer formation> EVOH (ethylene-vinyl alcohol copolymer, EVAL E105B, manufactured by Kuraray Co., Ltd.) was put into a single screw extruder (D2025, manufactured by Toyo Seiki Seisakusho Co., Ltd.) and extrusion laminated (melt laminated) on the side opposite the printed layer of the substrate so that the resin had a thickness of 15 μm, and then it was quickly quenched while being sandwiched between cooling rolls adjusted to 20°C to form a barrier layer. The melting temperature of the resin in the extrusion lamination was 215°C. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 2-4 to obtain an ultraviolet laser printable medium.

[0176] [Example 2-7] A print layer and a protective layer were formed on the film substrate in the same manner as in Example 2-4. <Barrier layer formation> To 100 parts of an aqueous solution of ethylene-modified polyvinyl alcohol (fully saponified, Kuraray Co., Ltd., Exeval AQ-4104) with a solid content concentration of 15 mass%, 50 parts of an aqueous dispersion of a layered inorganic compound (layered inorganic compound=synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: about 1000, thickness: about 5 nm), solid content concentration of 6 mass%, Topy Industries, Ltd., NTO-05) was added, and dilution water was further added thereto to adjust the solid content concentration to 10 mass%, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was applied in a coating amount of 2.0 g / m 2 The coating was then dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 2-4 to obtain an ultraviolet laser printable medium.

[0177] [Example 2-8] A print layer and a protective layer were formed on the film substrate in the same manner as in Example 2-4. <Barrier layer formation> A water dispersion of a layered inorganic compound (layered inorganic compound = synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: approximately 1000, thickness: approximately 5 nm), solid content concentration 6 mass%, manufactured by Topy Industries, Ltd., NTO-05) was mixed with a urethane emulsion (solid content concentration 30 mass%, glass transition temperature 130°C, oxygen permeability when formed into a 25 μm thick sheet was 2.0 mL / (m 2 1.0 g / m2 (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc.) was added to the mixture so that the mass ratio of solids (layered inorganic compound:urethane resin) was 2:10, and the mixture was stirred. Further, dilution water was added so that the solids concentration was 20 mass %, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was diluted with 1.0 g / m2 of the mixture so that the coating amount of the barrier layer was 2.0 g / m2. 2 After coating with a Mayer bar so as to obtain a coating composition as shown in the figure, the coating composition was dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 2-4 to obtain an ultraviolet laser printable medium.

[0178] [Example 2-9] A print layer and a protective layer were formed on the film substrate in the same manner as in Example 2-4. <Barrier layer formation> Aluminum-deposited PP film (base material = CPP (non-oriented polypropylene film), manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: ML, thickness 20 μm, water vapor permeability 0.2 g / m 2 ·day, oxygen permeability 50mL / m 2 On the surface of the PP film of the 100-m2 ... 2 After coating, the coating was applied to the surface of the film substrate opposite to the surface on which the printed layer was provided. <Formation of sealant layer> A sealant layer was formed in the same manner as in Example 2-4, and an ultraviolet laser printable medium was obtained.

[0179] [Example 2-10] In forming the barrier layer, an aluminum-deposited PET film (substrate: PET (polyethylene terephthalate), manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: ML, thickness: 12 μm, water vapor permeability: 1 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 10mL / m 2 An ultraviolet laser printing medium was obtained in the same manner as in Example 2-9, except that a 1000-milliliter (1.0-1.0 m / s) ...

[0180] [Example 2-11] In forming the barrier layer, a silica-deposited PP film (substrate: PP, manufactured by Toppan Printing Co., Ltd., product name: GL-LP, thickness: 17 μm, water vapor permeability: 0.5 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 1mL / m 2 An ultraviolet laser printable medium was obtained in the same manner as in Example 2-9, except that a 1000-milliliter (1.0-1.0-g / cm2) ... was used. The adhesive was applied to the substrate (PP) side of the silica-deposited PP film.

[0181] [Example 2-12] In forming the barrier layer, a silica-deposited PET film (substrate: PET, manufactured by Toppan Printing Co., Ltd., product name: GL-AE, thickness: 12 μm, deposition layer thickness: 400 nm, water vapor permeability: 0.6 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 0.2mL / m 2 An ultraviolet laser printing medium was obtained in the same manner as in Example 2-9, except that a 1000-milliliter (1.0-1.0 m / s) ...

[0182] [Example 2-13] In forming the barrier layer, an alumina-deposited PET film (substrate: PET, manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: TL, thickness: 12 μm, water vapor permeability: 1.5 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 15mL / m 2An ultraviolet laser printing medium was obtained in the same manner as in Example 2-9, except that a 1000-milliliter (1.0-1.0 m / s) ...

[0183] [Example 2-14] In forming the barrier layer, instead of the aluminum-deposited PP film, a PET film coated with PVDC (polyvinylidene chloride) (manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: V Barrier, thickness 12 μm, water vapor permeability 0.2 g / m) was used. 2 ·day, oxygen permeability 0.8mL / m 2 An ultraviolet laser printable medium was obtained in the same manner as in Example 2-9, except that a PVDC-coated PET film (1000 psi, ...

[0184] [Measurement and Evaluation] The substrates and ultraviolet laser printing media obtained in the examples and comparative examples, as well as various raw materials, were subjected to the following measurements and evaluations.

[0185] [Average particle size of titanium oxide] The average particle size of titanium oxide was measured by the following method. From the ultraviolet laser printing media obtained in the examples and comparative examples, the printing layer was scraped off using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769), and only the collected printing layer was used as a sample, and the ash obtained by burning it in a muffle furnace was calculated from an SEM image (secondary electron image) obtained with a scanning electron microscope (SEM, manufactured by Hitachi High-Tech Corporation, SU7000, etc.). Note that the protective resin layer provided on the printing layer was removed by scraping it off using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769), and then a sample of the printing layer was obtained. The ash was obtained by firing and incinerating it at 450°C using a muffle furnace (manufactured by Yamato Scientific Co., Ltd., model number FO300). The obtained ash was dispersed in ethanol for 5 minutes using an ultrasonic cleaner (manufactured by AS ONE Corporation, such as LSC-63) to obtain a 0.1 mass% slurry. Then, 0.1 mL was cast onto an aluminum dish and dried at 100 °C to prepare a sample for measurement. The entire aluminum dish was subjected to observation with a scanning electron microscope (SEM, manufactured by Hitachi High-Tech Corporation, such as SU7000). Particles that could be clearly distinguished from adjacent particles were visually selected, and the particle size was calculated from the geometric mean of the major axis and minor axis of one particle. At this time, even if primary particles and aggregated secondary particles were mixed, they were counted as one particle each if they could be clearly distinguished, and the average diameter of 100 randomly selected particles was taken as the average particle size. The magnification during SEM image observation was appropriately selected according to the particle size of titanium oxide and was set to about 20,000 times. Also, when particles other than titanium oxide were included, particles containing titanium element were measured using an energy dispersive X-ray analyzer (manufactured by Horiba, Ltd., such as EMAX) attached to the SEM. In the case of needle-shaped particles, the major axis was measured for 100 particles, and the average was taken as the average particle size.

[0186] 〔Method for calculating crystallite size〕 <Method for preparing measurement sample> From the media for ultraviolet laser printing obtained in the examples and comparative examples, the printing layer was scraped off using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769), and only the collected printing layer was used as a sample. The crystallite size was calculated from the SEM image (secondary electron image) obtained from a scanning electron microscope (SEM, manufactured by Hitachi High-Tech Corporation, such as SU7000) of the ash obtained by burning in a muffle furnace. The protective resin layer provided on the printing layer was removed by scraping using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769) to obtain a sample of the printing layer. The ash was obtained by firing at 450 °C using a muffle furnace (manufactured by Yamato Scientific Co., Ltd., model number FO300) to incinerate.

[0187] <Measurement by X-ray diffraction method> The test sample obtained by ashing was filled into a sample holder and measured using a high-speed detector. During filling, the height adjustment jig was appropriately used according to the sample amount to adjust the sample measurement surface to the same height as the edge of the sample holder. (Measurement conditions) X-ray diffractometer: RINT-Ultima III manufactured by Rigaku Corporation Voltage: 40 kV Current: 40 mA Optical system: Parallel beam (CBO) Detector: High-speed detector D / teX Ultra 2 manufactured by Rigaku Corporation Goniometer: Ultima III horizontal goniometer Tube target: Cu Wavelength: 1.541 Å (Kα1) Scan mode: CONTINUOUS Scan speed: 1.0000 deg / min Step width: 0.0500 deg Scan axis: 2Theta / Theta Scan range: 5.0000~60.0000 deg Incident slit: 1.0 mm Longitudinal limiting slit: 10 mm Receiving slit 1: Open Receiving slit 2: Open Sample holder: ASC-6 sample holder (product number 2455E442) Material: Aluminum Dimensions: φ23 mm × 2.0 mm Holder height adjustment jig: Transparent disc-shaped plate (self-made) Material: Poly(methyl acrylate) Dimensions: φ23 mm × 0.8 mm

[0188] <Processing of data obtained by X-ray diffraction> For the obtained diffraction profile, background processing and profile fitting processing were performed using integrated powder X-ray analysis software (PDXL2 manufactured by Rigaku Corporation). Regarding the settings for data processing, all those not specifically described were performed with the software default settings. Based on the information of the peak position and peak intensity of the diffraction profile, the crystal phase was identified using the database (ICDD).

[0189] <Calculation of crystallite size based on the data obtained by X-ray diffraction> The full width at half maximum (FWHM) and the Bragg angle (θ) of the strongest diffraction line obtained from the diffraction profile after data processing were substituted into the Scherrer equation to calculate the crystallite size. The X-ray diffraction peaks of titanium oxide used in the calculation are as follows. Anatase: (101) plane Rutile: (110) plane The Scherrer equation is as follows.

[0190]

Equation

[0191] D: Crystallite size (nm) K: Scherrer constant λ: Wavelength of X-ray (nm) B: FWHM (rad) θ: Bragg angle (rad) The value of K was 0.89, B was the value of FWHM obtained by measurement, the value of λ was 0.154, and the value of θ was the measured value of the maximum intensity derived from the (101) plane for anatase and the (110) plane for rutile.

[0192] 〔CSF〕 The Canadian Standard Freeness (CSF) of the raw pulp was measured in accordance with JIS P 8121-2:2012.

[0193] 〔Grammage of paper substrate〕 As a pretreatment for the obtained ultraviolet laser printing medium, layers other than the paper base material, such as the protective resin layer, printing layer, sealant layer, and barrier layer, were removed by grinding using a grinding device (manufactured by Sagawa Corporation, grinding wheel dimensions φ50.8 × 12.7 mm) while checking the layer boundaries under a microscope. Next, in cases where the paper has a printing layer, a sealant layer, a barrier layer, etc. formed by coating, since parts of these layers are immersed in the paper base material, the printing paper that had been pretreated as described above was immersed in xylene at 100°C to dissolve the resin components. The obtained paper base material was conditioned for one day in an environment of 23° C. and 50% humidity. After the conditioned humidity, the basis weight of the paper base material was measured in accordance with JIS P 8124:2011.

[0194] [Thickness of paper base material] The thickness of the paper substrate was measured in accordance with JIS P 8118: 2014. The thicknesses of the protective resin layer, the printing layer, the barrier layer and the heat seal layer were calculated from SEM images as described below, and were subtracted from the values ​​measured in accordance with JIS P 8118: 2014.

[0195] [Length-weighted average fiber length, fiber width, and fine fiber content of pulp fibers constituting the paper base material] The length-weighted average fiber length, fiber width and fine fiber content of the pulp constituting the paper base material were measured by the following methods. The printing media of the examples and comparative examples were cut into 40 cm squares, and about 50 times the mass of ion-exchanged water was added thereto, followed by immersion for 24 hours. After soaking for 24 hours, the pulp was disintegrated into fibers using a standard disintegrator (Kumagaya Riki Kogyo Co., Ltd.) until no undisintegrated fibers remained. The slurry (dispersion of pulp fibers) after disintegration, excluding the protective resin layer, printing layer, heat seal layer, barrier layer, etc., was sampled and the "length-weighted average fiber length (ISO)", "fine fiber content", and "fiber width" were measured using a fiber length measuring instrument (Model FS-5 with UHD base unit, Valmet Co., Ltd.). The "length-weighted average fiber length (ISO)" is the length-weighted average fiber length calculated by selecting fibers that are 0.2 mm to 7.6 mm inclusive. The "fine fiber content" is the percentage of fine fibers with a fiber width of 75 μm or less and a length of 0.08 mm to 0.20 mm inclusive among the defibrated pulp fibers. The "fiber width" is the length-weighted average fiber width calculated by selecting fibers that are 10 μm to 75 μm inclusive.

[0196] [Water retention] The ultraviolet laser printing media of the examples and comparative examples were subjected to the following pretreatment before measurement. The printing layer provided by coating, the sealant layer provided by coating, the barrier layer provided by coating, and the protective resin layer provided by coating were scraped off and removed using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769). In addition, when the sealant layer provided by lamination and the barrier layer provided by coating were present, the sealant layer and the barrier layer were scraped off and removed in the pretreatment using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769). In addition, in the case where the printing layer provided by coating and the protective resin layer provided by lamination were present, the printing layer and the protective resin layer were scraped off and removed in the same manner. After that, ion-exchanged water was added to the printing paper that had been pretreated as described above in an amount of about 50 times the mass of the printing paper, and the paper was left to stand for 24 hours. After standing for 24 hours, the paper was treated with a standard disintegrator (manufactured by Kumagai Riki Kogyo Co., Ltd.) until no undisintegrated fibers remained, and the pulp was disintegrated into a fibrous form. When the printing paper subjected to the defibration treatment had any layer selected from the group consisting of a printing layer provided by lamination, a sealant layer provided by lamination, a barrier layer provided by lamination, and a protective resin layer provided by lamination that had not been removed by the pretreatment, these laminate layers were removed from the slurry after defibration, and ion-exchanged water was added to adjust the concentration to 0.5%. Ion-exchanged water was added to the slurry after defibration (dispersion of pulp fibers) to adjust the concentration to 0.5%. The water retention of the obtained pulp fiber was measured according to JAPAN TAPPI No. 26 (2000) (Pulp - Water Retention Test Method).

[0197] [Titanium oxide content] 1. When non-printable areas are included in the printing medium (Preparation of test specimens) The printable area and non-printable area (area where no coating layer is provided) of the printing medium were each cut out to an appropriate size to prepare samples (test pieces), and the areas of the cut out pieces were recorded. (Dissolution of test specimen) A mixed solvent of nitric acid:hydrofluoric acid = 50:5 (volume %) and the test piece were placed in a Teflon (registered trademark) container of an autoclave device (MARS5, manufactured by CEM Japan), and the test piece was dissolved by autoclaving at 210°C for 120 minutes. The area of ​​the test piece may be appropriately changed, and if the test piece remains undissolved, the ratio of nitric acid and hydrofluoric acid, the treatment temperature, the treatment time, etc. may be appropriately changed. After dissolving the test piece, the solution was accurately adjusted to a fixed volume using ultrapure water. (Measurement of titanium oxide content in solution) (1) The ICP apparatus and measurement conditions are as follows: ICP device: ICP-OEC device (Rigaku Corporation, CIROS1-20) Measurement conditions: Carrier gas: Argon gas Argon gas flow rate: 0.9L / min Plasma gas flow rate: 14 L / min Plasma power 1400W Pump RPM: 2 ·Measurement wavelength Ti: 334.941nm (2) Preparation of calibration curve A general-purpose mixed standard solution (manufactured by SPEX, XSTC-622B) was accurately measured to give the following concentrations, and subjected to measurement under the above measurement conditions, and the intensity at 334.941 nm, which corresponds to the emission wavelength of titanium atoms, was measured. Concentrations for creating calibration curves: 0 ppm, 0.01 ppm, 0.05 ppm, 0.1 ppm, 0.5 ppm, 1.0 ppm, 3.0 ppm, 5.0 ppm (3) Measurement of titanium oxide content in the solution The solution in which the test pieces were dissolved was diluted with ultrapure water so that the solution was within the range of the above calibration curve, and then subjected to ICP measurement. (4) Titanium dioxide content calculation method The titanium oxide content was calculated using the following formula: (molecular weight of titanium oxide / atomic weight of titanium) ≈ 1.669. Titanium oxide content (g / m 2 ) = ICP measured concentration (ppm) × dilution ratio × fixed volume (L) × 1.669 × 1000 ÷ area (m 2 ) The titanium oxide content in the coating layer was determined by subtracting the titanium oxide content in the non-printable area from the titanium oxide content in the printable area.

[0198] 2. When the non-printable area is not included in the printing medium (Preparation of test specimens) Two pieces of printing media were cut to appropriate size and the area of ​​the cut out pieces was recorded. One of the cut test pieces was taken using a grinding device (manufactured by Sagawa Corporation, grinding wheel dimensions φ50.8 × 12.7 mm) to remove only the protective resin layer and the printed layer, and used as a reference sample. The cross section was observed using an electron microscope as appropriate to avoid excessive scraping. (Subsequent processing) The same treatment as in 1 was repeated, and the difference in the titanium oxide content of the two sheets was taken as the titanium oxide content of the printed layer.

[0199] [Content of inorganic pigment] The content of inorganic pigments was measured in the same manner as the measurement of titanium oxide content, except that the measurement wavelength of the ICP was changed to a measurement wavelength specific to the metal atom contained in each inorganic pigment. Calcium element was measured at a measurement wavelength of 422.673 nm, and magnesium element was measured at a measurement wavelength of 285.213 nm.

[0200] [Thickness of the printing layer, protective resin layer, barrier layer and sealant layer] The thicknesses of the print layer, protective resin layer, barrier layer and sealant layer were measured from image data obtained by a scanning electron microscope. (1) Preparation of measurement samples The sample was embedded in a photocurable resin (D-800, manufactured by Toagosei Co., Ltd.), and the cross section of the printing medium was extracted using an ultramicrotome. A diamond knife was used for cutting at room temperature. The cut cross section was coated with gold vapor deposition to a thickness of about 20 nm and subjected to measurement using a scanning electron microscope. (2) Measurement equipment and conditions Measuring device: S-3600 (Hitachi High-Tech Corporation) Measurement conditions: 2000x magnification The type of scanning microscope is not limited to the above, but an apparatus that displays a scale bar was used. When the printing layer, protective resin layer, barrier layer and sealant layer were thin, the image data was obtained by selecting an appropriate magnification. (3)Measurement method After confirming that the printing layer to be observed contains titanium element using an energy dispersive X-ray spectrometer attached to a scanning electron microscope, image data was obtained at a magnification of 2000 times. After printing the obtained image data on a printing medium, the thicknesses of the target printing layer, protective resin layer, barrier layer, and sealant layer (the length from the boundary with other layers to the boundary) were measured with a ruler, and the actual thicknesses of the printing layer, protective resin layer, barrier layer, and sealant layer were measured by comparing with the scale bar. Image data of five randomly selected points was obtained from one measurement sample, and the thicknesses of the thickest and thinnest printing layers were measured from the image data of one point, and the average of the 10 points was taken as the thickness of the printing layer. In addition, the thicknesses of the thickest and thinnest protective resin layers were measured, and the average of the 10 points was taken as the thickness of the protective resin layer. In the same manner, the thicknesses of the barrier layer and the sealant layer were measured. The observation magnification may be changed depending on the thicknesses of the printing layer, protective resin layer, barrier layer, and sealant layer to be observed.

[0201] [Measurement of Raman spectrum] The Raman spectrum was measured by the following method: In this example, the Raman spectrum was measured on a print obtained by the clarity of a single printed dot described below. <Measurement conditions> The measurement conditions for Raman spectrum are as follows, but if the laser used for measurement causes damage to the printed matter, if the fluorescence is strong, if the peak intensity is weak, etc., the measurement conditions below such as laser output and irradiation time can be changed as appropriate. However, the Raman intensities of the printed and non-printed areas are measured under the same conditions. Equipment: Renishaw inVia Raman microscope QUONTOR Excitation laser: 532nm Laser power: 50mW (at 100% output) Laser power: 50% Measurement mode: Confocal mode Irradiation time: 2.0sec Number of times: 30 Laser spot diameter: 2.5μm Objective lens: 20x

[0202] <Measurement method> The measurements were carried out by the following method. (1) The Raman shift position was calibrated using a standard sample (single crystal silicon, manufactured by Renishaw) (520.5 cm for single crystal silicon). -1 ). (2) The sheet-shaped sample was placed on the sample stage. If necessary, a presser was installed to keep the sheet flat. (3) The device was focused and observed (the focus was set to the smallest using the simulated laser). When measuring the printed area, the darkest part that could be visually confirmed was measured to be at the center of the guide displayed during measurement. When measuring the non-printed area, the measurement was made at a distance of 300 μm or more from the printed area. (4) The obtained Raman spectrum was subjected to baseline correction (intelligent correction) using the processing software attached to the device (Renishaw, Wire5.2). The baseline was corrected using polynomial 11 of the processing software. (5) Rutile titanium dioxide: 447±10cm -1 , 516±10cm for anatase titanium dioxide -1The maximum value (maximum intensity) in the wavenumber range was read, and the Raman intensity ratio was calculated according to the following formula. Raman intensity ratio = maximum intensity in printed area ÷ maximum intensity in non-printed area (6) Ten points were measured in each of the printed area (printed portion) and non-printed area (non-printed portion), and the average value was used as the measurement result. From the viewpoint of suppressing the variation of the measured values, it is preferable to measure the Raman intensity count of the printed area in a range of 10,000 or less. Therefore, the measurement conditions were appropriately changed so that the Raman intensity count of the printed area was in a range of 10,000 or less. In addition, 10 measurements were performed under the following measurement conditions, and values ​​that deviated beyond the average value ± 2SD (standard deviation) were excluded, and the average was calculated again to obtain the average value of the Raman intensity. The Raman intensity ratio was evaluated according to the following A to C. A: Raman intensity ratio is 0.3 or less B: Raman intensity ratio is greater than 0.3 and less than or equal to 0.7 C: Raman intensity ratio exceeds 0.7

[0203] [Clarity of a single printed point] <Laser marking method> For the substrates obtained in the Examples and Comparative Examples, a 10 mm square was printed on the sample surface using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C). (Printing conditions) Wavelength: 355nm Output: 50% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.3mm Scan speed: 8000mm / sec Spot variable: 0

[0204] <Clarity evaluation> A digital microscope (manufacturer: Keyence Corporation, model number: VHX-8000) was used to obtain a depth-composite image of the printed area to be evaluated. A depth-composite image is an image in which multiple images are obtained by changing the focal length, and the in-focus parts of each are extracted and reconstructed into a single image. The depth-composite image was obtained using the live depth-composite function built into the digital microscope. After that, the brightness extraction mode of the automatic area measurement function was used to measure the area of ​​areas in the printed portion that were darker than the threshold. The brightness extraction mode is a mode that classifies the brightness level of the image into a hierarchy from -255 to 255, and extracts areas above or below an arbitrary threshold. For the printed portion, the more areas with a brightness level lower than the threshold, the more "darker the print" is deemed to be. (Settings when taking images) Shutter speed: Auto mode (set value 70) Gain: 0dB Magnification: 1000x Lighting: Ring lighting (Brightness Extraction Mode Settings) Magnification when acquiring depth stacking image: 1000x Illumination: 100% coaxial epi-illumination Threshold: -5 Extraction area: Inside a circle with a radius of 45 μm from the center of the printed area (Evaluation criteria for print density) A: The area of ​​the area with a luminance level lower than -5 is 65% or more of the extracted area. B: The area of ​​the area with a luminance level lower than -5 is 60% or more but less than 65% of the extracted area C: The area of ​​the area with a luminance level lower than -5 is between 50% and 60% of the extracted area. D: The area of ​​the area with a luminance level lower than -5 is less than 50% of the extracted area.

[0205] [Suppression of swelling of protective resin layer] <Laser marking method> The printing media obtained in the examples and comparative examples were cut to MD: 50 mm × CD: 100 mm. The characters "2021" (font: Arial, width: 9 mm, height: 3 mm) were printed on the surface of the cut sample using an ultraviolet laser irradiation machine (manufactured by Keyence Corporation, model number: MD-U1020C). The following conditions were used during the measurements: ·Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Spot diameter: 40μm (when focused) Spot variable: 60 Fill spacing: 0.04mm Scan speed: 3000mm / sec In adjusting the focal position of the laser, a height correction function attached to the device was used, and the focal position of the laser was corrected with the above spot variable value.

[0206] <Evaluation of swelling> The difference in height between the printed and non-printed parts of the obtained print was measured using a surface roughness meter (Keyence Corporation, model number: VR-3000) and evaluated according to the following criteria. The following conditions were used for the measurement. Magnification: 50x -For the reference plane settings, specify the area: continuous area (extraction method: plane, tolerance level: 4, expansion / contraction level: 3) Surface shape correction: Waviness removal (correction strength 5) Measurement type: Line roughness Cutoff value: λs = None Cutoff value: λc = None The evaluation criteria are as follows: A: Height difference is less than 15 μm B: Height difference is 15 μm or more and less than 30 μm C: Height difference is 30μm or more and less than 45m D: Height difference is 45 μm or more

[0207] [Water vapor barrier properties] Measurements were performed in accordance with JIS-Z-0208:1976 (cup method) Method B (40°C ± 0.5°C, relative humidity 90% ± 2%) with the sealant layer facing inward. The water vapor barrier property was evaluated according to the following criteria. (Evaluation criteria for water vapor barrier properties) A: Water vapor permeability is 30g / m 2 ·day or less B: Water vapor permeability is 30g / m 2 · Over 40g / m 2 ·day or less C: Water vapor permeability is 40g / m 2 · Over 50g / m 2 ·day or less D: Water vapor permeability is 50g / m 2 ·Over the day

[0208] Laser irradiation was performed under the following conditions, and the water vapor permeability of the ultraviolet laser printed matter after the laser irradiation was similarly measured. Note that for Comparative Example 1-6, the water vapor barrier property was evaluated as D before the ultraviolet laser irradiation, so it was not measured. <Laser irradiation> For the ultraviolet laser printing papers obtained in the examples and comparative examples, a 10 cm square was printed on the sample surface (printing layer side) using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed 1000mm / sec Spot variable: 0

[0209] [Oxygen Barrier Properties] The oxygen permeability of the ultraviolet laser printing media of Examples 1-21 to 1-29 and Examples 2-6 to 2-14 was measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) under conditions of a temperature of 23° C. and a relative humidity of 85%. Specifically, the oxygen permeability of the laminated sheet was measured at a temperature of 23° C. and a relative humidity of 85% in accordance with JIS K7126-2:2006. The lower the oxygen permeability value, the better the oxygen barrier property. The oxygen barrier property was evaluated according to the following criteria. (Evaluation criteria for oxygen barrier properties) A: Oxygen permeability is 3.0mL / m 2 ·day · atm or less B: Oxygen permeability is 3.0mL / m 2 ·day·atm, 5.0mL / m 2 ·day · atm or less C: Oxygen permeability is 5.0mL / m 2 ·day·atm, 15mL / m 2 ·day · atm or less D: Oxygen permeability is 15mL / m 2 ·day·exceeds ATM

[0210] Laser irradiation was also carried out under the following conditions, and the oxygen permeability of the ultraviolet laser print after laser irradiation was similarly measured. <Laser irradiation> For the ultraviolet laser printing media obtained in the examples and comparative examples, a 10 cm square was printed on the sample surface (printing layer side) using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed 1000mm / sec Spot variable: 0

[0211] [Barrier property reduction rate after UV laser irradiation (barrier property reduction rate)] The decrease in barrier property (barrier property decrease rate) due to ultraviolet laser irradiation was evaluated based on the water vapor permeability and oxygen permeability before and after ultraviolet laser irradiation according to the following evaluation criteria. (Evaluation criteria for barrier property deterioration rate) A: The rate of decrease (reduction) in water vapor permeability and oxygen permeability is 5.0% or less B: The decrease (reduction rate) of water vapor permeability or oxygen permeability exceeds 5.0%. The rate of decrease in water vapor permeability is calculated as follows. Decrease rate of water vapor permeability = (water vapor permeability after UV laser irradiation (g / m 2 ·day)-Water vapor permeability before UV laser irradiation (g / m 2 ·day) / Water vapor permeability before UV laser irradiation (g / m 2 ·day)×100 Similarly, the decrease in oxygen permeability is calculated as follows. Decrease rate of oxygen permeability = (oxygen permeability before and after ultraviolet laser irradiation (mL / m 2 ·day·atm)-Oxygen permeability before UV laser irradiation (mL / m 2 ·day·atm) / Oxygen permeability before UV laser irradiation (mL / m 2 ·day·atm)×100

[0212] [Heat seal peel strength and rate of decrease in heat seal peel strength (rate of decrease in peel strength)] Two sheets of ultraviolet laser printing media were stacked with the sealant layers facing each other, and heat sealed at 160°C, 0.2 MPa, and 1 second using a heat seal tester (Tester Sangyo, TP-701-B). The heat-sealed test pieces were left to stand for more than 4 hours in a room with a temperature of 23°C ± 1°C and a humidity of 50% ± 2%. The heat-sealed test pieces were then cut to a width of 15 mm and T-peeled at a tensile speed of 300 mm / min using a tensile tester, and the maximum load recorded was taken as the heat seal peel strength. The heat seal peel strength was evaluated according to the following criteria. (Evaluation criteria for heat seal peel strength) A: Heat seal peel strength is 10N / 15mm or more B: Heat seal peel strength is 6.0N / 15m or more and less than 10N / 15mm C: Heat seal peel strength is 3.0N / 15mm or more and less than 6.0N / 15mm D: Heat seal peel strength is less than 3.0N / 15mm <Laser irradiation> For the ultraviolet laser printing media obtained in the examples and comparative examples, a 10 cm square was printed on the sample surface (printing layer side) using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed 1000mm / sec Spot variable: 0 (Evaluation criteria for heat seal peel strength reduction rate) The decrease in barrier property (barrier property decrease rate) due to ultraviolet laser irradiation was evaluated based on the heat seal peel strength before and after ultraviolet laser irradiation according to the following evaluation criteria. Note that for Comparative Example 1-6, the heat seal peel strength before ultraviolet laser irradiation was evaluated as D, so it was not measured. (Evaluation criteria for the rate of decrease in heat seal peel strength) A: Heat seal peel strength reduction rate (reduction rate) is 5.0% or less B: The rate of decrease (reduction) in heat seal peel strength exceeds 5.0%. The rate of decrease in heat seal peel strength is calculated as follows. Reduction rate of heat seal peel strength = (heat seal peel strength before UV laser irradiation (N / 15mm) - heat seal peel strength before UV laser irradiation (N / 15mm)) / heat seal peel strength before UV laser irradiation (N / 15mm) x 100

[0213] [Table 2-1]

[0214] [Table 2-2]

[0215] [Table 3]

[0216] According to the results in Tables 2 and 3, by using the printing medium of the embodiment and printing with an ultraviolet laser, a printed matter was obtained having a printed image with excellent print clarity for each dot and suppressed swelling of the protective resin layer. Furthermore, they had heat sealability and excellent water vapor barrier properties. The ultraviolet laser printable media of Examples 1-21 to 1-29 and 2-6 to 2-14, in which a barrier layer was formed, also had excellent oxygen barrier properties. Furthermore, the deterioration of barrier properties and heat sealability due to printing with an ultraviolet laser was suppressed. On the other hand, when printing was performed with an ultraviolet laser using the printing media of Comparative Example 1-1 and Comparative Example 1-2, in which the crystallite size of the titanium oxide in the printing layer was less than 13 nm, sufficient print clarity was not obtained for each point. Also, when printing was performed with an ultraviolet laser using the printing medium of Comparative Example 1-3, in which the crystallite size of the titanium oxide in the printing layer was more than 53 nm, swelling of the protective resin layer occurred. Furthermore, the content of titanium oxide in the printing layer is 0.1 g / m 2 When printing was performed with an ultraviolet laser using the printing medium of Comparative Example 1-4, in which the titanium oxide content in the printing layer was less than 4.0 g / m, sufficient print clarity for each point was not obtained. 2 When printing was performed with an ultraviolet laser using the printing medium of Comparative Example 1-5 exceeding the above-mentioned temperature, swelling of the protective resin layer occurred. Moreover, when the print medium of Comparative Example 1-6, which did not have a sealant layer, was used, the heat sealability and water vapor barrier property were not obtained. [Industrial Applicability]

[0217] The printing medium of the present invention can provide a printed matter with excellent visibility by discoloring the titanium oxide by irradiation with an ultraviolet laser, and further, the print clarity of each point is excellent and the swelling of the protective resin layer is suppressed. The ultraviolet laser printing medium of the present invention is suitably applied to processed products such as packages, labels, and adhesive tapes on which variable information such as dates and bar codes are printed. Furthermore, the method for producing a printed matter of the present invention is suitably applied to printing variable information on packages, labels, adhesive tapes, etc.

Claims

1. A substrate has a printed layer containing titanium oxide and a protective resin layer in this order on one surface of the substrate, A sealant layer is provided on the other surface of the substrate; The content of the titanium oxide in the printing layer is 0.1 g / m 2 4.0g / m or more 2 is as follows: The crystallite size of the titanium oxide in the printing layer is 13 nm or more and 53 nm or less. UV laser printing media.

2. 2. The ultraviolet laser printable medium according to claim 1, wherein the crystallite size of the titanium oxide in the printing layer is 30 nm or more and 53 nm or less.

3. 2. The ultraviolet laser printable medium according to claim 1, wherein the titanium oxide in the print layer is rutile titanium oxide, and the diffraction angle of said titanium oxide is 27.60[deg.] or less.

4. 2. The ultraviolet laser printable medium according to claim 1, wherein the protective resin layer has a thickness of 10 [mu]m or more.

5. 2. The ultraviolet laser printable medium according to claim 1, wherein the resin constituting the protective resin layer is at least one selected from the group consisting of polyolefins, polyesters, and polyvinyl alcohols.

6. 2. The ultraviolet laser printable medium according to claim 1, wherein the substrate is a paper substrate, and the water retention of pulp constituting the paper substrate is 140% or less.

7. The ultraviolet laser printable medium of claim 1 , wherein the substrate is a film substrate.

8. 8. The ultraviolet laser printable medium according to claim 7, wherein the resin constituting the film substrate is selected from the group consisting of polyolefins, polyesters, and polyvinyl chlorides.

9. 10. The ultraviolet laser printable medium of claim 1 further comprising a barrier layer between the substrate and the sealant layer.

10. A printed matter obtained from the ultraviolet laser printing medium according to any one of claims 1 to 9, the printed layer has, at least in part, a printed area containing discolored titanium oxide; A printed matter, in which the ratio of the Raman intensity originating from titanium oxide in a printed area to the Raman intensity originating from titanium oxide in a non-printed area is 0.70 or less.

11. A processed product using the ultraviolet laser printing medium according to any one of claims 1 to 9.

12. A processed product obtained by using the printed matter according to claim 10.

13. A step of printing by irradiating the ultraviolet laser printing medium according to any one of claims 1 to 9 with an ultraviolet laser to discolor the irradiated area, A method for producing printed matter.

14. 14. The method for producing a printed matter according to claim 13, wherein the printing step is a step of irradiating with an ultraviolet laser so that the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area is 0.70 or less.

Citation Information

Patent Citations

  • Thermoplastic resin composition for laser marking, resin molded article and method for laser marking

    JP1998237319A

  • Polyacetal resin composition for laser-marking and laser-marked molded article

    JP2001089632A

  • Resin composition for laser processing and joined resin member comprising the same

    JP2006291196A

  • Polyamide resin composition for laser marking and laser-marked polyamide resin molding

    JP2007098939A