Roll-shaped conductive adhesive sheet, wiring board with metal reinforcement plate, and electronic device

The rolled conductive bonding sheet with controlled adhesive and protective sheet properties addresses blocking, film thickness reduction, and adhesion issues, ensuring stable film thickness, easy peeling, and strong lamination.

JP2024149317AActive Publication Date: 2024-10-18TOYO INK MFG CO LTD +1

Patent Information

Application Number
JP2023073962
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-05
Filing Date
2023-04-28
Publication Date
2024-10-18
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Conductive bonding sheets experience issues such as blocking during unrolling, film thickness reduction due to strong winding tension, damage to protective sheets during peeling, insufficient adhesion to metal plates, and cohesive failure during lamination, leading to poor laminate strength and adhesiveness.

Method used

A rolled conductive bonding sheet with a protective sheet and conductive adhesive layer, featuring specific probe tack adhesive strength and storage modulus ranges, along with a protective sheet having a defined storage modulus, to prevent blocking, ensure film thickness stability, and enhance peelability and lamination strength.

Benefits of technology

The solution prevents blocking during unrolling, maintains film thickness, allows easy peeling of the protective sheet, and ensures high lamination strength and adhesiveness, addressing the issues of adhesion and cohesive failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149317000001_ABST
    Figure 2024149317000001_ABST
Patent Text Reader

Abstract

To provide a roll-shaped conductive adhesive sheet that does not cause blocking when unrolled, has excellent film thickness consistency, provides good peelability of the protective sheet, and has high lamination strength and adhesion, a wiring board with a metal reinforcement plate, and an electronic device.SOLUTION: A roll-shaped conductive adhesive sheet obtained by winding a conductive adhesive sheet into a roll has a protective sheet and a conductive adhesive layer, the conductive adhesive layer has a probe tack adhesive strength of 5.0 N / cm2 or less, and the conductive adhesive layer has a maximum storage modulus of 1.0×107 to 2.0×109 Pa at 25 to 30°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a roll-shaped conductive adhesive sheet, a wiring board with a metal reinforcing plate, and an electronic device. [Background technology]

[0002] Flexible printed circuit boards mounted inside electronic devices are flexible, and it is known that electromagnetic shielding layers are arranged, and reinforcing plates are arranged in connectors and other parts to prevent deformation from the viewpoint of connecting between parts. Conventionally, epoxy glass and the like have been used as reinforcing plates, but metal plates are increasingly being used to provide electromagnetic noise suppression functions. Conductive adhesives whose main component is resin are used to connect the shielding layer and metal plate to the flexible printed circuit board.

[0003] For example, Patent Document 1 discloses a conductive adhesive composition containing a polyurethane polyurea resin, an epoxy resin, and a conductive filler as a conductive bonding agent for bonding a conductive reinforcing plate (metal plate) arranged opposite a ground wiring pattern (wiring board). Patent Document 2 discloses a conductive adhesive having improved embeddability and adhesiveness by adding an organic salt, talc, carbon black, silica, or the like as a loss modulus adjuster. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2016 / 002780 [Patent Document 2] International Publication No. 2019 / 031394 Summary of the Invention [Problem to be solved by the invention]

[0005] Typically, a conductive adhesive sheet is wound up in a roll (volume) with a conductive adhesive layer laminated on a protective sheet. However, when the sheet is unwound from the roll, a problem occurs in which the conductive adhesive layer adheres to the back surface of the protective sheet, known as blocking.

[0006] In addition, when the sample is wound into a roll, tension is applied to prevent the roll from unraveling, but if the winding tension is strong, the conductive adhesive layer is stored for a long period of time under high pressure, which causes a problem of a decrease in the thickness (film thickness) of the conductive adhesive layer (film thickness guarantee).

[0007] Furthermore, after the conductive adhesive sheet is temporarily attached to an adherend such as a metal plate by thermocompression bonding, the protective sheet is deformed or damaged when peeled off, resulting in a problem that the protective sheet cannot be peeled off. (Removability of protective sheet)

[0008] Furthermore, if the conductive adhesive layer is not softened sufficiently during the temporary attachment, the adhesive layer will not have sufficient adhesion to the metal plate, causing problems such as the conductive adhesive layer peeling off from the metal plate during the process of processing the metal reinforcing plate, in which the conductive adhesive layer and the metal plate are laminated, into a desired shape, i.e., during so-called punching (lamination strength).

[0009] In addition, when a tensile force is applied to the substrate after the laminate of metal reinforcing plate / conductive adhesive layer / wiring board is heated and pressed (heat pressed) to a specified temperature (for example, 170°C) to bond the laminate, if the elastic modulus of the conductive adhesive layer at room temperature is very high, cohesive failure occurs and the laminate easily peels off (adhesion). [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that the problems of the present disclosure can be solved in the following aspect, and have thus completed the present disclosure. [1]: A roll-shaped conductive adhesive sheet obtained by winding a conductive adhesive sheet into a roll, the conductive adhesive sheet having a protective sheet and a conductive adhesive layer, the conductive adhesive layer having a probe tack adhesive strength of 5.0 N / cm 2 The conductive adhesive layer has a maximum storage modulus of 1.0×10 or less at 25 to 30° C. 7 ~2.0×10 9 Rolled conductive adhesive sheet [2] The conductive adhesive layer has a maximum storage modulus of 3.0 × 10 at 70 to 120 °C. 6 ~1.5×10 8 The roll-shaped conductive adhesive sheet according to [1], wherein the conductive adhesive sheet is a roll-shaped conductive adhesive sheet having a molecular weight of 1000 to 2000 Pa. [3] The protective sheet has a maximum storage modulus of 1.0 × 10 at 25 to 30 °C. 9 The roll-shaped conductive adhesive sheet according to [2], wherein the elastic modulus is 1.0 Pa or more. [4]: The roll-shaped conductive adhesive sheet according to any one of [1] to [3], wherein the conductive adhesive layer has at least one bond selected from the group consisting of an ester bond, an imide bond, an amide bond, a urethane bond, and a urea bond. [5]: A wiring board with a metal reinforcing plate, comprising the conductive adhesive layer according to [4] and a metal reinforcing plate. [6]: An electronic device comprising the wiring board with metal reinforcing plate described in [5]. Effect of the Invention

[0011] The present disclosure provides a roll-shaped conductive adhesive sheet that does not cause blocking when unwound, has excellent film thickness assurance, has good peelability of the protective sheet, and has high lamination strength and adhesiveness. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram showing a roll-shaped conductive adhesive sheet according to the present disclosure. [Diagram 2] 1 is a schematic diagram showing a cross section of a metal-reinforced wiring board according to the present disclosure; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The roll-shaped conductive adhesive sheet, the metal-reinforced wiring board, and the electronic device according to the present disclosure will be described below in order. Note that the numerical range indicated by "-" includes the lower and upper limits unless otherwise specified. In addition, the drawings are appropriately simplified for clarity of explanation, and the scale of each component in the drawings may differ significantly for the purpose of explanation.

[0014] [Conductive adhesive sheet] The conductive adhesive sheet of the present disclosure has a protective sheet and a conductive adhesive layer, and has a flat sheet shape. The conductive adhesive layer is preferably laminated directly on the protective sheet or via a release agent layer.

[0015] [Roll-type conductive adhesive sheet] The rolled conductive adhesive sheet of the present disclosure is formed by winding the above-mentioned conductive adhesive sheet into a roll. FIG. 1 shows a schematic diagram of the rolled conductive adhesive sheet of the present invention and a partially enlarged explanatory diagram thereof. The rolled conductive adhesive sheet has a winding core, and is configured such that the conductive adhesive sheet is wound around the winding core. The conductive adhesive sheet is configured such that the conductive adhesive layer is wound on the inside and the protective sheet is wound on the outside.

[0016] [Protective sheet] The protective sheet serves as a support for the conductive adhesive layer in the conductive adhesive sheet, and is located on the outermost surface of the roll of the conductive adhesive sheet in a roll-shaped conductive adhesive sheet, and serves to protect the conductive adhesive layer from damage and contamination.

[0017] Examples of protective sheets include plastic sheets such as polyethylene terephthalate, polyethylene naphthalate, polyvinyl fluoride, polyvinylidene fluoride, rigid polyvinyl chloride, polyvinylidene chloride, nylon, polyimide, polystyrene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polycarbonate, polyacrylonitrile, polybutene, flexible polyvinyl chloride, polyvinylidene fluoride, polyethylene, polypropylene, polyurethane, ethylene-vinyl acetate copolymer, polyvinyl acetate, and the like, papers such as glassine paper, fine paper, craft paper, coated paper, and the like, various nonwoven fabrics, synthetic paper, metal foil, and composite films combining these, etc. Among these, plastic sheets are preferred from the viewpoint of easy adjustment of storage modulus by blending material components, and among these, polyethylene terephthalate and polyethylene naphthalate, which have both rigidity and flexibility, are more preferred.

[0018] The surface of the protective sheet may be subjected to a matte treatment, if necessary, by methods such as sand matte, etching matte, coating matte, chemical matte, kneaded matte, etc. In the conductive adhesive sheet, the surface roughness Ra of the protective sheet on the side laminated with the conductive adhesive layer is preferably 0.01 to 1 μm from the viewpoint of improving the peelability of the protective sheet, and the surface roughness Ra of the protective sheet opposite the side laminated with the conductive adhesive layer is preferably 0.01 to 5 μm from the viewpoint of improving blocking resistance.

[0019] From the viewpoint of improving the releasability of the protective sheet, the protective sheet preferably has a release agent layer on the surface. The release agent layer is preferably formed by applying a release agent. As the release agent, a hydrocarbon resin such as polyethylene or polypropylene, higher fatty acid and its metal salt, higher fatty acid soap, wax, animal or vegetable oil, mica, talc, silicone surfactant, silicone oil, silicone resin, alkyd resin, fluorine surfactant, fluorine resin, fluorine-containing silicone resin, melamine resin, or acrylic resin can be selected, and an alkyd resin is preferred. The release agent can be applied by a conventional method such as a gravure coating method, a kiss coating method, a die coating method, a lip coating method, a comma coating method, a blade coating method, a roll coating method, a knife coating method, a spray coating method, a bar coating method, a spin coating method, or a dip coating method. The release agent layer is preferably formed on one side of the protective sheet, and more preferably on both sides.

[0020] There are no particular limitations on the thickness of the protective sheet, but a thickness of 38 μm or more is preferable because the protective sheet is less likely to be damaged when peeled off if the protective sheet has stiffness and strength, and a thickness of 100 μm or less is preferable from the viewpoint of preventing a decrease in the temporary attachment property due to a decrease in heat transmission to the conductive adhesive layer during temporary attachment.

[0021] [Storage modulus of protective sheet] The protective sheet of the present disclosure has a maximum storage modulus of 1.0 × 10 at 25 to 30°C. 9 Pa or more, 1.5×10 10 Pa or less, and 1.5×10 9 Pa or more, 1.0×10 10The following is more preferable. Furthermore, when the maximum storage modulus of the protective sheet at 25 to 30°C is within this range, the rigidity (stiffness) of the protective sheet can be sufficiently increased even after thermal lamination, and damage to the protective sheet when peeling it from the conductive adhesive layer can be prevented, realizing excellent peelability. Furthermore, winding defects such as creases during winding can be prevented. The elastic modulus of the protective sheet can be adjusted by the material, main chain skeleton, crosslinking density, and orientation of the polymer.

[0022] [Conductive adhesive layer] The conductive adhesive layer of the present disclosure is obtained by applying a conductive composition onto a protective sheet and drying it, and is a non-flowable solid at 25°C and forms a layer of a certain thickness. From the viewpoint of achieving both thin film properties and electrical conductivity, the thickness of the conductive adhesive layer in the conductive adhesive sheet is preferably 5 to 200 μm, more preferably 10 to 100 μm, and further preferably 30 to 70 μm.

[0023] [Probe tack adhesive strength of conductive adhesive layer] The probe tack adhesive strength of the conductive adhesive layer is 5.0N / cm 2 The probe tack adhesive strength of the conductive adhesive layer is 5.0 N / cm 2 By setting the conductive adhesive layer to a thickness of 3.5 N / cm or less, the adhesiveness can be reduced, and the adhesive layer can be prevented from sticking to the protective layer when wound into a roll, thereby improving blocking resistance. 2 The lower limit of the probe tack adhesive strength is preferably 0 N / cm or less. 2 is preferred.

[0024] The probe tack adhesive strength of the conductive adhesive layer in the present invention can be controlled, for example, by adjusting the amount of tackifier resin such as terpene resin, changing the main chain skeleton and side chain of resin (a-1) contained in binder (A) described later, adjusting the crosslink density by adjusting the amount of curing agent added, and the type and amount of metal particles and other fillers added. The method for controlling the probe tack adhesive strength of the conductive adhesive layer is not limited to the above-mentioned method, and any method can be used as long as it can realize the desired probe tack adhesive strength.

[0025] [Storage modulus of conductive adhesive layer] The maximum storage modulus of the conductive adhesive layer at 25 to 30°C is 1.0 × 10 7 ~2.0×10 9 It is Pa. The elastic modulus of the conductive adhesive layer at 25°C to 30°C is 1.0×10 7 By setting it to Pa or higher, When a sample of the conductive adhesive sheet is wound into a roll, the winding tension is strong, and pressure is applied to the conductive adhesive layer. Even if the sample is stored in a rolled state for a long period of time, the thickness change of the conductive adhesive layer can be suppressed. In addition, the elastic modulus of the conductive adhesive layer at 25°C to 30°C is 2.0×10 9 By setting the pressure drop to 0.1 Pa or less, cohesive failure of the conductive adhesive layer can be prevented, and high adhesive strength can be maintained. The maximum storage modulus of the conductive adhesive layer at 25 to 30°C is 1.0 × 10 7 ~1.7×10 9 Pa is preferred, 1.0×10 8 ~1.3×10 9 Pa is more preferred.

[0026] The maximum storage modulus of the conductive adhesive layer at 70 to 120°C is 3.0 × 10 6 ~1.5×10 8 Pa is preferred, 7.0×10 6 ~1.0×10 8 Pa is more preferable, and 1.0×10 7 ~8.0×10 7By setting the maximum storage modulus of the conductive adhesive layer at 70 to 120°C within the above range, the conductive adhesive layer becomes fluid when temporarily attached by thermal lamination at 110°C, for example, and the lamination strength to the substrate can be improved.

[0027] In the present invention, the maximum value of the storage modulus of the conductive adhesive layer can be controlled by, for example, changing the main chain skeleton and side chain of the resin, adjusting the amount of curing agent added to adjust the crosslink density, adding a tackifier resin and adjusting the amount added, adjusting the type and amount added of metal particles and other fillers, etc. As the tackifier resin, for example, terpene resin, terpene phenol resin, rosin, rosin derivatives, etc. are preferable.

[0028] [Conductive composition] The conductive composition includes a binder (A) and metal particles (B).

[0029] [Binder (A)] The binder (A) serves as a base for the conductive composition and has the function of dispersing and supporting the metal particles (B) and other additive fillers. The binder (A) is not particularly limited in composition, etc., as long as it has the above-mentioned function, but it is preferable that it contains a resin (a-1). The resin (a-1) in the present disclosure is defined as an organic material that is usually solid, semi-solid, or solidified, has a softening or melting range, and has a weight average molecular weight (Mw) of 5,000 or more.

[0030] [Resin (a-1)] Resin (a-1) is not particularly limited in composition, molecular structure, etc., except for the weight average molecular weight (Mw) described above, but among these, resins having one or more chemical bonds selected from the group consisting of ester bonds, imide bonds, amide bonds, urethane bonds, and urea bonds are preferred. Imide bonds, amide bonds, urethane bonds, and urea bonds can achieve strong adhesive strength by the interaction of the unshared electron pair of the nitrogen atom contained in the bond with the adherend. Examples of resins having the above-mentioned chemical bond groups include polyester resins, polyurethane resins, polyamide resins, polyimide resins, polyamideimide resins, urea resins, and polyurethane urea resins.

[0031] In addition, it is more preferable that the resin (a-1) has two or more selected from the group consisting of ester bonds, imide bonds, amide bonds, urethane bonds, and urea bonds. When the binder (A) has two or more selected from the group consisting of ester bonds, imide bonds, amide bonds, urethane bonds, and urea bonds, the interaction with the adherend is multiplied, and it is possible to develop stronger adhesion. Examples of resins having two or more selected from the group consisting of ester bonds, imide bonds, amide bonds, urethane bonds, and urea bonds include polyesteramide, polyamideimide resin, and polyurethane urea resin.

[0032] As described above, the resin (a-1) can be appropriately selected from the viewpoints of composition and molecular structure, but it is also possible to select a suitable resin depending on the properties of the resin. From the viewpoint of exerting adhesiveness by applying a thermal stimulus to the conductive composition, the resin (a-1) is preferably a thermosetting resin (a-2) or a thermoplastic resin (a-3).

[0033] [Thermosetting resin (a-2)] Thermosetting resin (a-2) is a resin (a-1) that has thermosetting properties. Thermosetting is defined as "capable of being changed into a substantially infusible and insoluble product when cured by heat or other means such as radiation, catalyst, etc."

[0034] When the thermosetting resin (a-2) has a reactive functional group such as an acidic group, the above-mentioned thermosetting property may be exhibited by a reaction between the reactive functional groups, or may be exhibited by a reaction between reactive functional groups incorporated in the thermosetting resin (a-2) and the curing agent (D) described later. When the thermosetting resin (a-2) is used in the conductive adhesive layer, the probe tack adhesive strength, the storage modulus at 25 to 30°C, and the storage modulus at 70 to 120°C of the conductive adhesive layer described above are values ​​before the thermosetting reaction.

[0035] The thermosetting resin (a-2) preferably has an acid value of 5 to 40 mgKOH / g. By having the acid value within the above range, the density of the crosslinked structure is in a suitable range, and it is possible to achieve both flexibility and toughness. The acid value is more preferably 10 to 20 mgKOH / g.

[0036] [Thermoplastic resin (a-3)] Thermoplastic resin (a-3) is a type of resin (a-1) that has thermoplastic properties. Thermoplasticity is defined as "the ability to repeatedly soften by heating and harden by cooling within a temperature range specific to plastics, and to repeatedly mold, extrude, or form articles by flowing in the softened state."

[0037] The binder (A) preferably contains at least one functional group selected from the group consisting of an epoxy group, an oxetane group, an episulfide group, and an aziridine group. When the resin (a-1) has a reactive functional group such as an acidic group, the functional group described above can cause a curing reaction between the reactive functional group or between the functional groups themselves, thereby exhibiting high adhesiveness. As a method for incorporating the functional group described above into the binder (A), for example, a resin (a-1) having the functional group described above can be added to the binder (A), or a curing agent (C) described later having the functional group described above can be added to the binder (A).

[0038] [Hardening agent (C)] The curing agent (C) in the present disclosure is a substance that accelerates or regulates the curing reaction, and is defined as a substance having a molecular weight or weight average molecular weight (Mw) of less than 5,000. The curing reaction is defined as "polymerizing and / or crosslinking a prepolymer or polymer composition by heating or other means such as radiation, catalyst, etc., and irreversibly increasing the elastic modulus." From the viewpoint of forming polymerization and / or crosslinking in the binder (A) by a stimulus such as heat, and exhibiting strong adhesiveness to the conductive composition, it is preferable that the binder (A) of the present disclosure contains a curing agent (C).

[0039] The above-mentioned curing reaction may be a self-reaction between the curing agents (C) themselves, or may be a reaction with other components in the binder (A), such as the resin (a-1). When the resin (a-1) and the curing agent (C) undergo a curing reaction, it is preferable that the resin (a-1) is a thermosetting resin (a-2) from the viewpoint of efficient reaction.

[0040] From the viewpoint of preventing the curing reaction from proceeding during storage and allowing the curing reaction to occur only upon heating, it is preferable to select a combination of the thermosetting resin (a-2) and the curing agent (C) that does not undergo a crosslinking reaction at 50°C but accelerates the curing reaction at 150°C. Furthermore, the crosslink density of the conductive composition in each temperature range may be controlled by appropriately combining two or more types of curing agents having different curing reaction initiation temperatures. Examples of the curing agent (C) include epoxy curing agents, oxetane curing agents, episulfide curing agents, aziridine curing agents, amine curing agents, isocyanate curing agents, and imidazole curing agents. Among them, epoxy curing agents, oxetane curing agents, episulfide curing agents, and aziridine curing agents are preferred because they efficiently undergo a curing reaction with the thermosetting resin (a-2) and can exhibit high adhesiveness.

[0041] As the epoxy curing agent, for example, a glycidyl ether type epoxy compound, a glycidyl amine type epoxy compound, a glycidyl ester type epoxy compound, a cyclic aliphatic (alicyclic) epoxy compound, or the like is preferable.

[0042] Examples of the glycidyl ether type epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, bisphenol AD ​​type epoxy compounds, cresol novolac type epoxy compounds, phenol novolac type epoxy compounds, a-1-naphthol novolac type epoxy compounds, bisphenol A type novolac type epoxy compounds, dicyclopentadiene type epoxy compounds, tetrabromobisphenol A type epoxy compounds, brominated phenol novolac type epoxy compounds, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane.

[0043] Examples of the glycidylamine type epoxy compound include tetraglycidyldiaminodiphenylmethane, triglycidyl para-aminophenol, triglycidyl meta-aminophenol, and tetraglycidyl meta-xylylenediamine.

[0044] Examples of the glycidyl ester type epoxy compound include diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate.

[0045] Examples of the cyclic aliphatic (alicyclic) epoxy compounds include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate, bis(epoxycyclohexyl)adipate, and the like.

[0046] Examples of the oxetane curing agent include 1,4-bis{[(3-ethyloxetan-3-yl)methoxy]methyl}benzene, 3-ethyl-3-{[(3-ethyloxetan-3-yl)methoxy]methyl}oxetane, 1,3-bis[(3-ethyloxetan-3-yl)methoxy]benzene, 4,4'-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl, an ester of (2-ethyl-2-oxetanyl)ethanol and terephthalic acid, an ether of (2-ethyl-2-oxetanyl)ethanol and phenol novolac resin, and an ester of (2-ethyl-2-oxetanyl)ethanol and a polyvalent carboxylic acid compound.

[0047] Examples of the episulfide curing agent include bis(1,2-epithioethyl) sulfide, bis(1,2-epithioethyl) disulfide, bis(2,3-epithiopropyl) sulfide, bis(2,3-epithiopropylthio)methane, bis(2,3-epithiopropyl) disulfide, bis(2,3-epithiopropyldithio)methane, bis(2,3-epithiopropyldithio)ethane, bis(6,7-epithio-3,4-dithiaheptyl) sulfide, bis(6,7-epithio-3,4-dithiaheptyl)disulfide, 1,4-dithiane-2,5-bis(2,3-epithiopropyldithiomethyl), 1,3-bis(2,3-epithiopropyldithiomethyl)benzene, 1,6-bis(2,3-epithiopropyldithiomethyl)-2-(2,3-epithiopropyldithioethylthio)-4-thiahexane, and 1,2,3-tris(2,3-epithiopropyldithio)propane.

[0048] Examples of the aziridine curing agent include trimethylolpropane-tri-a-2-aziridinyl propionate, tetramethylolmethane-tri-a-2-aziridinyl propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide).

[0049] Examples of the amine curing agent include diethylenetriamine, triethylenetetramine, methylenebis(2-chloroaniline), methylenebis(2-methyl-6-methylaniline), 1,5-naphthalene diisocyanate, and n-butylbenzylphthalic acid.

[0050] Examples of the isocyanate curing agent include tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, dicyclohexylmethane diisocyanate, 1,5-naphthalene diisocyanate, tetramethylxylylene diisocyanate, and trimethylhexamethylene diisocyanate.

[0051] Examples of the imidazole curing agent include 2-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methylimidazole, and 1-cyanoethyl-2-undecylimidazolium trimellitate.

[0052] The curing agent (C) may be used alone or in combination of two or more. The curing agent (C) is preferably one having a molecular weight or weight average molecular weight of 100 or more from the viewpoint of adjusting the storage modulus and glass transition temperature of the conductive composition.

[0053] The curing agent (C) is preferably blended in an amount of 0.1 to 70 parts by mass, more preferably 0.1 to 50 parts by mass, per 100 parts by mass of the thermosetting resin (a-2). By adding the curing agent (C) in an amount of 0.1 parts by mass or more, the density of the crosslinked structure of the conductive composition can be optimized, and the adhesiveness can be improved, and the film thickness can be improved. By adding the curing agent (C) in an amount of 70 parts by mass or less, the conductive composition can be prevented from becoming excessively hard, and the adhesiveness and punching processability can be improved.

[0054] [Metal particles (B)] The metal particles (B) are preferably conductive metals such as gold, platinum, silver, copper, and nickel, and alloys thereof. From the viewpoint of cost reduction, composite particles in which a coating layer that covers the surface of a metal core is formed from a material having a higher conductivity than the core, rather than particles of a single composition, are preferred. The core is preferably selected from nickel, silica, copper, and alloys thereof. The coating layer may be, for example, gold, platinum, silver, tin, manganese, indium, or alloys thereof. Among them, silver is preferably used from the viewpoints of electrical conductivity and material cost.

[0055] The composite microparticles preferably have a coating layer in a ratio of 1 to 40 parts by mass, more preferably 5 to 30 parts by mass, per 100 parts by mass of the core. Coating with 1 to 40 parts by mass allows for further cost reduction while maintaining electrical conductivity. It is preferable that the coating layer of the composite microparticles completely covers the core. However, in practice, there are cases where part of the core is exposed. Even in such cases, electrical conductivity is easily maintained as long as 70% or more of the core surface area is covered with a conductive material.

[0056] The metal particles (B) may be used alone or in combination of two or more kinds.

[0057] The shape of the metal particles (B) is not limited as long as it can obtain the desired electrical conductivity.Specific examples include spherical, flake, leaf, dendritic, plate, needle, rod, grape, and amorphous mass.Note that, from the viewpoint of improving electrical conductivity, spherical, flake, leaf, dendritic, and plate are more preferable.

[0058] The average particle diameter of the metal particles (B) is D 50 The average particle diameter D is preferably 1 to 50 μm, more preferably 3 to 30 μm, and further preferably 5 to 20 μm. 50 When the average particle diameter D is in this range, a suitable conductive path can be formed, and the electrical conductivity can be improved. 50 can be determined by a laser diffraction / scattering particle size distribution measuring device.

[0059] The average particle diameter of the metal particles (B) is D 90 The average particle diameter D is preferably 1 to 120 μm, and more preferably 5 to 70 μm. 90 When the thickness is within this range, the occurrence of blocking can be suppressed.

[0060] The thickness of the conductive adhesive layer is the average particle diameter D of the metal particles (B). 50 The value X obtained by dividing by is preferably 1 to 35. When X is 35 or less, a conductive path of the metal particles (B) is effectively formed in the conductive adhesive layer, improving the conductivity. From the viewpoint of improving the conductivity, it is more preferable that X is 18 or less. Furthermore, when X is 1 or more, the contact area between the adherend and the binder (A) is increased without excessively increasing the number of contact points between the adherend and the metal particles (B), improving the adhesiveness. It is more preferable that X is 5 or more.

[0061] The metal particles (B) are preferably contained in an amount of 40 to 90 mass% of the total solid content of the conductive composition. By setting the content within the above range, blocking resistance, film thickness assurance, and adhesiveness can be achieved at the same time. The content of the metal particles (B) is more preferably 45 to 80 mass%, and further preferably 50 to 70 mass%.

[0062] The conductive composition in the present embodiment may contain other optional components such as a heat stabilizer, an inorganic filler, an organic filler, a pigment, a dye, a tackifier resin, a plasticizer, a silane coupling agent, an ultraviolet absorber, an antifoaming agent, and a leveling adjuster.

[0063] Examples of inorganic fillers include silica, alumina, aluminum hydroxide, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, talc, montmorrinite, kaolin, bentonite, etc. When the conductive composition contains an inorganic filler, it is possible to control the suppression of probe tack, and further to control the storage modulus and the film thickness guarantee.

[0064] Examples of the organic filler include urethane resin particles, acrylic resin particles, phenolic resin particles, nylon particles, etc. By including an organic filler in the conductive composition, the temporary adhesion property can be ensured, and further, the storage modulus can be controlled, and the film thickness can be controlled.

[0065] [Method of manufacturing conductive adhesive sheet] The conductive adhesive sheet of the present disclosure can be obtained, for example, by coating a conductive composition on a protective sheet, drying, and further B-stage curing as necessary. The conductive composition after drying is called a conductive adhesive layer. The coating method may be appropriately selected from known methods in consideration of the film thickness of the conductive adhesive layer. Specific examples of the coating method include gravure coating, kiss coating, die coating, lip coating, comma coating, blade coating, roll coating, knife coating, spray coating, bar coating, spin coating, and dip coating.

[0066] B-stage curing is a method in which the conductive adhesive layer is heated at a specified temperature for a specified time to partially cause a curing reaction. By performing B-stage curing, the strength of the conductive adhesive layer can be increased while maintaining its adhesive power.

[0067] [Method of manufacturing roll-shaped conductive adhesive sheet] The conductive adhesive sheet can be wound up while pressing its leading end against a winding core material to obtain a roll-shaped conductive adhesive sheet.

[0068] The winding core of the present invention is not particularly limited, but examples thereof include a paper tube, a metal tube, and a plastic tube. It is a tube long in the width direction and is generally used in a winding device attached to a manufacturing device such as a printing machine, a coating machine, a molding machine, or a glazing machine. The winding core generally has a diameter of about 1 to 40 cm. The width of the winding core is not particularly limited as long as it can be installed in the winding device. It is generally about 2 mm to 6 m.

[0069] Another example of a method for winding the conductive adhesive sheet is to fix the tip of the conductive adhesive sheet to a winding core using an adhesive member. The adhesive member can be a double-sided adhesive tape, a cast adhesive tape, or a single-sided adhesive tape. A first example of the method is to fix the tip of the conductive adhesive layer surface of the conductive adhesive sheet to the winding core using a double-sided adhesive tape. A second example of the method is to place the protective sheet of the conductive adhesive sheet on the lower side, and fix the tip to the winding core using an adhesive tape.

[0070] The tension when winding the conductive adhesive sheet varies depending on the material of the protective sheet, and is not particularly limited, but it is necessary to set the tension so that the substrate does not deform and does not sag. For example, when PET is used as the substrate, the tension is preferably 0.5 N / cm to 2.5 N / cm.

[0071] [Metal reinforcement plate] The metal reinforcing plate of the present disclosure has a conductive adhesive layer laminated to a metal plate. The aforementioned metal plate may be, for example, a conductive metal such as gold, silver, copper, iron, or stainless steel. Among these, stainless steel is preferred in terms of strength, cost, and chemical stability as a metal plate. The thickness of the metal plate is generally about 0.04 to 1 mm. The metal plate is preferably provided with a nickel layer formed on the entire surface of the metal plate. The nickel layer is preferably formed by electrolytic nickel plating. The nickel layer is preferably about 0.5 to 5 μm, and more preferably 1 to 4 μm. The conductive adhesive layer provided on the metal reinforcing plate is a non-fluid solid at 25° C., and forms a layer of a certain thickness.

[0072] [Wiring board with metal reinforcement plate] A wiring board 100 with a metal reinforcing plate according to this embodiment (see FIG. 2) includes a wiring board 20 in which a ground circuit 22 is disposed on an insulating film 21, the ground circuit 22 is covered with a coverlay 23, and a part of the ground circuit 22 is exposed through an opening 30, and a metal reinforcing plate is disposed on the wiring board 20. A conductive adhesive layer 1 of the metal reinforcing plate is layered and bonds the wiring board 20 and the metal plate 2. In the wiring board according to this embodiment, a part of the conductive adhesive layer 1 is filled in the opening 30, so that the ground circuit 22 and the metal plate 2 are electrically connected via the conductive adhesive layer 1. The wiring board 20 may further be provided with a signal wiring.

[0073] The area of ​​the opening 30 in the wiring board 20 is 0.16 mm 2 More than 0.81mm 2 The area of ​​the opening 30 may be 0.16 mm 2 By setting the area of ​​the opening 30 to 0.81 mm or more, it is possible to improve the filling property of the conductive adhesive layer in the opening 30. 2 By setting the area of ​​the opening 30 to 0.25 mm or less, the area of ​​the opening 30 in the wiring board 20 can be reduced. 2 More than 0.64mm 2 Less than 0.36 mm, more preferably 2 More than 0.49mm 2 When the area of ​​the opening 30 is within this range, the conductive adhesive layer can be filled into the opening 30 satisfactorily, and the contact resistance between the conductive adhesive layer and the ground circuit 22 can be reduced.

[0074] The shape of the opening 30 when viewed from above may be rectangular or circular. When the opening 30 is rectangular, it is particularly difficult to fill the four corners of the rectangular opening with the conductive adhesive layer, and gaps are likely to be formed at the four corners. However, by using the conductive adhesive layer according to the present embodiment in which the resin flow is controlled within a suitable range, the conductive adhesive layer can be satisfactorily filled into the opening even if the opening is rectangular.

[0075] [Electronic equipment] Such a wiring board with a metal reinforcing plate can be mounted on electronic devices such as mobile phones, smartphones, notebook PCs, digital cameras, liquid crystal displays, etc. It can also be suitably mounted on transportation equipment such as automobiles, trains, ships, and aircraft. EXAMPLES

[0076] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples. Note that the "parts" and "%" below are values ​​based on "parts by mass" and "% by weight", respectively. In addition, the acid value and weight average molecular weight (Mw) of the resin (a-1), and the D of the metal particles (B) are 50 The average particle size was measured by the following method.

[0077] [Acid value of resin (a-1)] The acid value (mgKOH / g) was calculated by converting the measured value into solid content according to the neutralization titration method of JIS K 0070. Approximately 1g of sample was precisely weighed and placed in a stoppered Erlenmeyer flask, and 100mL of a tetrahydrofuran / ethanol (volume ratio: tetrahydrofuran / ethanol = 2 / 1) mixture was added and dissolved. Phenolphthalein test solution was added as an indicator, and titration was performed with 0.1N alcoholic potassium hydroxide solution. The end point was when the indicator retained a pale pink color for 30 seconds. The acid value was calculated using the following formula (unit: mgKOH / g). Acid value (mgKOH / g)=(5.611×a×F) / S however, S: Amount of sample collected (g) a: Consumption of 0.1N alcoholic potassium hydroxide solution (mL) F: Potency of 0.1N alcoholic potassium hydroxide solution

[0078] [Weight average molecular weight (Mw) of resin (a-1)] Mw was measured using a GPC (gel permeation chromatograph) "HPC-8020" (manufactured by Tosoh Corporation). GPC is a liquid chromatograph that separates and quantifies substances dissolved in a solvent (THF; tetrahydrofuran) based on the difference in their molecular size. This measurement was performed using two "LF-604" columns (manufactured by Showa Denko KK: GPC column for rapid analysis: 6 mm ID x 150 mm size) connected in series, with a flow rate of 0.6 mL / min and a column temperature of 40°C. Mw was determined in polystyrene equivalent.

[0079] [Metal particles (B) D 50 Average particle size] D 50 The average particle size was measured using a laser diffraction / scattering particle size distribution analyzer LS13320 (manufactured by Beckman Coulter). The value was obtained by measuring the conductive filler using a Tornado dry powder sample module, and is the particle size at which the cumulative value in the cumulative particle size distribution is 50%. The refractive index was set to 1.6.

[0080] <Raw materials> [Binder (A)] (a-1)-1: Polyester resin: acid value 36 mgKOH / g, Mw=27,000 (manufactured by Toyochem) (a-1)-2: Polyimide resin: acid value 18 mgKOH / g, Mw=55,000 (manufactured by Toyochem) (a-1)-3: Polyamide resin: acid value 22 mgKOH / g, Mw=49,000 (manufactured by Toyochem) (a-1)-4: Polyurethane resin: acid value 16 mgKOH / g, Mw=98,000 (manufactured by Toyochem) (a-1)-5: Polyurethane urea resin: acid value 15 mgKOH / g, Mw=100,000 (manufactured by Toyochem) (a-1)-6: Styrene elastomer: acid value 55 mg KOH / g, Mw = 120,000 (manufactured by Toyochem) [Metal particles (B)] B1: Silver coated copper powder: D 50 =5.7μm, dendritic (Mitsui Mining & Smelting) B2: Silver coated copper powder: D50 =31.2μm, dendritic (manufactured by Mitsui Mining & Mining Co., Ltd.) B3: Silver coated copper powder: D 50 =10.8μm, spherical (manufactured by Resonac) B4: Silver coated copper powder: D 50 =7.5μm, spherical (manufactured by Resonac) B5: Silver coated copper powder: D 50 =11.3μm, flake-shaped (manufactured by DOWA Holdings) [Hardening agent (C)] C1: Ti chelate compound (TC100, molecular weight = 364, Matsumoto Fine Chemical) C2: Bisphenol A type epoxy compound (jER (registered trademark) 828, molecular weight = 370, manufactured by Mitsubishi Chemical) C3: Isophthalic oxetane compound (ETERNACOLL (registered trademark) OXIPA, molecular weight = 362, manufactured by Ube Industries) C4: Hydrogenated bisphenol A episulfide compound (TBIS (registered trademark)-AHS, molecular weight = 384, manufactured by Taoka Chemical Co., Ltd.) C5: Polyfunctional aziridine compound (ChemiTite (registered trademark) PZ-33, molecular weight = 425, manufactured by Nippon Shokubai) C6: Polycarbodiimide compound (Carbodilite V-05, molecular weight = 1200, manufactured by Nisshinbo Chemical) [Tackifier resin] Terpene resin (YS Resin PX300N, Yasuhara Chemical) [Protective Sheet D] D1: PET film (Cerapeel PJ271, film thickness 50 μm, surface treatment: one side treated with alkyd-based release agent, made by Toray) D2: Paper film (G62 White AA (N7-82), film thickness 58 μm, surface treatment: both sides treated with silicone release agent, manufactured by Lintec) D3: Polypropylene film (Torayfan #30-2500H, film thickness 50 μm, surface treatment: both sides treated with alkyd-based release agent, manufactured by Toray) D4: Polyethylene film (Ube poly sheet, film thickness 70 μm, surface treatment: both sides treated with alkyd-based release agent, made by Ube Film) D5: Polyvinyl chloride film (general-purpose PVC film, thickness 120 μm, surface treatment: both sides treated with alkyd-based release agent, made by Okamoto)

[0081] <Preparation of conductive composition and conductive bonding sheet> [Example 1] 100 parts by mass of ((a-1)-1) as resin (a-1), 167 parts by mass of (B1) as metal particles (B), 10 parts by mass of terpene resin (YS Resin PX300N) as tackifier resin, and methyl ethyl ketone as solvent were added and mixed so that the non-volatile content concentration was 40% by mass. Next, 1.5 parts by mass of (C1) as curing agent (C) was added, and the mixture was stirred with a stirrer for 10 minutes to prepare a conductive composition solution. Next, the conductive composition solution prepared above was applied onto one of the release-treated surfaces of a 300 mm wide protective sheet (D) D1 (release agent: alkyd-based release agent) using a comma head coater with a line speed of 2 m / min so that the thickness after drying would be 60 μm, and the sheet was dried by passing through a 2 m electric oven A set at 100°C and a 2 m electric oven B set at 120°C to form a conductive adhesive layer on the protective sheet, and the sheet was wound around a plastic core with a diameter of 8.8 cm so that the conductive adhesive layer of the conductive adhesive sheet was on the inside, to obtain a roll-shaped conductive adhesive sheet.

[0082] [Examples 2 to 36, Comparative Examples 1 to 4] The same procedure as in Example 1 was carried out except that the types and amounts of each component to be blended were as shown in Tables 1 to 6, to obtain roll-shaped conductive adhesive sheets of Examples 2 to 36 and Comparative Examples 1 to 4.

[0083] [Measurement of probe tack adhesive strength] The conductive adhesive sheet was unwound from each of the obtained rolls, and probe tack measurements were carried out in accordance with the 17th Revised Japanese Pharmacopoeia, General Test Methods, 6. Preparation Test Methods, 6.12 Adhesive Strength Test Method, 3.4 Probe Tack Test Method. The conductive adhesive sheet was cut into 2 cm squares to obtain samples. The samples were attached to a weight ring, and a load was applied by placing a total of 200 g of weights on top of them, and the probe tack adhesive strength (unit: N / cm) was measured using a probe tack tester (TE-6001 probe tack tester, manufactured by Tester Sangyo Co., Ltd.). 2 ) was measured.

[0084] [Measurement of storage modulus] The storage modulus of each conductive adhesive layer and protective sheet was measured using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.). The conductive adhesive layer and protective sheet were cut to a width of 5 mm and a length of 5 cm to obtain samples. The device was set to a constant temperature rise rate (10°C / min), and measurements were performed in tensile mode at a measurement frequency of 10 Hz in the temperature range of -50°C to 300°C to measure the storage modulus (unit: Pa) at each temperature, and the maximum values ​​at 25 to 30°C and 70 to 120°C were obtained.

[0085] <Evaluation> The obtained roll-shaped conductive adhesive sheets were evaluated for blocking resistance, film thickness assurance, peelability of the protective sheet, lamination strength, and adhesiveness according to the following methods. The evaluation results are shown in Tables 1 to 5.

[0086] [Blocking resistance] The rolled conductive adhesive sheets prepared in each Example and Comparative Example were slit to a width of 249 mm and a length of 10 m, and wound around a plastic tube with a diameter of 8.8 cm at a winding tension of 1.6 N / cm so that the conductive adhesive layer was on the inside to prepare a roll sample, which was then left in an atmosphere at 50° C. for 24 hours. The conductive adhesive sheet was then unwound from the roll, and the blocking property was evaluated according to the following criteria. +++: The conductive adhesive layer does not stick to the protective sheet surface (very excellent) ++: Part of the conductive adhesive layer sticks to the protective sheet surface, but the conductive adhesive layer does not float (excellent) +: Part of the conductive adhesive layer sticks to the protective sheet surface, and part of the conductive adhesive layer floats (practical). NG: The conductive adhesive layer sticks to the protective sheet surface and is partially broken (not practical).

[0087] [Film thickness guarantee] The roll-shaped conductive adhesive sheet prepared in each Example and Comparative Example was slit to a width of 249 mm and a length of 20 m, and then wound around a plastic tube with a diameter of 8.8 cm at a winding tension of 1.9 N / cm with the conductive adhesive layer facing inside to prepare a roll sample, which was then left in an atmosphere at 50°C for 240 hours.

[0088] Next, 10 m of the roll sample was unwound from the outside of the roll, and a 5 cm square sample was taken, and the thickness (H1) of the conductive adhesive layer was measured using a contact thickness meter. The initial thickness of the conductive adhesive layer of the conductive adhesive sheet, 60 μm, was defined as H2, and ΔH=H1 / H2 was calculated for each example and comparative example, and evaluated according to the following evaluation criteria. +++: ΔH is 0.6 or more (very good) ++: ΔH is 0.5 or more and less than 0.6 (excellent) +: ΔH is 0.4 or more and less than 0.5 (practical) NG: ΔH is less than 0.4 (not practical)

[0089] [Protective sheet removability] A conductive adhesive sheet having a width of 25 mm and a length of 100 mm was cut from the roll-shaped conductive adhesive sheet produced in each Example and Comparative Example, and the conductive adhesive sheet was laminated on a SUS plate having a width of 30 mm and a length of 150 mm (a commercially available SUS304 plate having a thickness of 0.2 mm and a nickel layer having a thickness of 2 μm formed on the surface) so that the conductive adhesive layer was in contact with the sheet. Then, the conductive adhesive sheet was laminated on the SUS plate having a width of 30 mm and a length of 150 mm so that the conductive adhesive layer was in contact with the sheet. The laminate was then laminated on a roll laminator at 130° C. and 3 kgf / cm. 2The conductive adhesive sheet was laminated onto the SUS plate at a speed of 0.5 m / min, and the protective sheet was then peeled off from the conductive adhesive layer. The remaining area of ​​the protective sheet remaining on the conductive adhesive layer was then measured, and the remaining rate of the protective sheet was calculated using the following formula and evaluated according to the following criteria. Remaining rate of protective sheet = remaining area of ​​protective sheet / area of ​​conductive adhesive layer x 100 +++: 0% of the protective sheet remains. (Very good) ++: The remaining rate of the protective sheet is greater than 0% and less than 1% (excellent). +: The remaining rate of the protective sheet is 1% or more and less than 2%. (Practical) NG: The remaining rate of the protective sheet is 2% or more. (Not practical)

[0090] [Laminate strength] A conductive adhesive sheet having a width of 25 mm and a length of 100 mm was cut from the roll-shaped conductive adhesive sheet produced in each Example and Comparative Example, and the conductive adhesive sheet was laminated on a SUS plate having a width of 30 mm and a length of 150 mm (a commercially available SUS304 plate having a thickness of 0.2 mm and a nickel layer having a thickness of 2 μm formed on the surface) so that the conductive adhesive layer was in contact with the sheet. Then, the conductive adhesive sheet was laminated on the SUS plate having a width of 30 mm and a length of 150 mm so that the conductive adhesive layer was in contact with the sheet. The laminate was then laminated on a roll laminator at 130° C. and 3 kgf / cm. 2 The conductive adhesive sheet and the SUS plate were roll-laminated under conditions of 130° C., 3 kgf / cm 2 , and 0.5 m / min., and then the protective sheet was peeled off from the conductive adhesive layer. Copper foil (thickness: 25 μm) was placed on the surface where the conductive adhesive layer was exposed. The laminate was then laminated using a roll laminator at 130° C., 3 kgf / cm 2 . 2 The conductive adhesive layer and the copper foil were roll-laminated at a rolling speed of 0.5 m / min to obtain a sample for evaluation.

[0091] Next, using a tensile testing machine (small tabletop testing machine EZ-TEST, manufactured by Shimadzu Corporation) at a tensile speed of 50 mm / min, the adhesive strength of the conductive adhesive layer of the evaluation sample to the SUS plate in a 90° peel test was used as an index to evaluate the temporary attachment property according to the following evaluation criteria. +++: Adhesive strength is 3N / cm or more (very good) ++: Adhesive strength is 2N / cm or more and less than 3N / cm (excellent) +: Adhesive strength is 1N / cm or more and less than 2N / cm (practical) NG: Adhesive strength is less than 1N / cm (not practical)

[0092] [Adhesiveness] A conductive adhesive sheet having a width of 25 mm and a length of 100 mm was cut from the roll-shaped conductive adhesive sheet produced in each Example and Comparative Example, and the conductive adhesive sheet was laminated on a metal plate having a width of 30 mm and a length of 150 mm (a commercially available SUS304 plate having a thickness of 0.2 mm and a nickel layer having a thickness of 2 μm formed on the surface) so that the conductive adhesive layer was in contact with the metal plate. Next, the conductive adhesive sheet was laminated on the metal plate by a roll laminator at 130° C. and 3 kgf / cm. 2 The conductive sheet and the metal plate were roll-laminated under conditions of 130° C., 3 kgf / cm 2 , and 0.5 m / min., and then the protective sheet was peeled off from the conductive adhesive layer. A copper foil (thickness: 25 μm) was placed on the surface where the conductive adhesive layer was exposed. The laminate was then laminated by a roll laminator at 130° C., 3 kgf / cm 2 , and 0.5 m / min. 2 The conductive adhesive layer and the copper foil were roll-laminated at a speed of 0.5 m / min to obtain a laminate, which was then pressure-bonded at 170°C, 2 MPa, and 3 minutes, and then heated in an electric oven at 160°C for 60 minutes to obtain a sample for evaluation.

[0093] Next, using a tensile testing machine (small tabletop testing machine EZ-TEST, manufactured by Shimadzu Corporation) at a tensile speed of 50 mm / min, the adhesive strength of the conductive composition to the metal plate of the evaluation sample in a 90° peel test was used as an index to evaluate the adhesiveness according to the following evaluation criteria. +++: Adhesive strength is 4N / cm or more (very good) ++: Adhesive strength is 3N / cm or more and less than 4N / cm (excellent) +: Adhesive strength is 1N / cm or more and less than 3N / cm (practical) NG: Adhesive strength is less than 1N / cm. (Not practical)

[0094] [Table 1]

[0095] [Table 2]

[0096] [Table 3]

[0097] [Table 4]

[0098] [Table 5]

[0099] [Table 6] [Explanation of symbols]

[0100] 1 Conductive adhesive layer 2 metal plate 3 Protective sheet 4. Rolled conductive adhesive sheet 20 Wiring board 21 Insulating film 22 Ground Circuit 23 Coverlay 30 Opening 100 Wiring board with metal reinforcement plate

Claims

1. A roll-shaped conductive adhesive sheet obtained by winding a conductive adhesive sheet into a roll shape, The conductive adhesive sheet has a protective sheet and a conductive adhesive layer, The conductive adhesive layer has a probe tack adhesive strength of 5.0 N / cm 2 is as follows: The conductive adhesive layer has a maximum storage modulus of 1.0×10 at 25 to 30° C. 7 ~2.0 x 10 9 A roll-shaped conductive adhesive sheet having a thickness of 100 mm or less.

2. The conductive adhesive layer has a maximum storage modulus of 3.0×10 at 70 to 120° C. 6 ~1.5 x 10 8 The roll-shaped conductive adhesive sheet according to claim 1 , wherein the viscosity is 0.05 Pa.

3. The protective sheet has a maximum storage modulus of 1.0×10 at 25 to 30° C. 9 The roll-shaped conductive adhesive sheet according to claim 2 , having a compressive strength of 100 Pa or more.

4. The conductive adhesive layer comprises a resin having one or more chemical bonds selected from the group consisting of an ester bond, an imide bond, an amide bond, a urethane bond, and a urea bond. The roll-shaped conductive adhesive sheet according to any one of claims 1 to 3.

5. A wiring board with a metal reinforcing plate, comprising the conductive adhesive layer according to claim 4 and a metal reinforcing plate.

6. An electronic device comprising the wiring board with a metal reinforcing plate according to claim 5.

Citation Information

Patent Citations

  • Method and apparatus for producing laminate

    JP2007136835A

  • Curable resin composition, adhesive epoxy resin paste, adhesive epoxy resin sheet, conductive connection paste, conductive connection sheet, and electronic component joined body

    JP2009013416A

  • Adhesive composition, adhesive and adhesive sheet

    JP2015010192A

  • Electroconductive adhesive composition

    WO2016002780A1

  • Conductive adhesive

    WO2019031394A1

Cited By

  • Conductive adhesive sheet, connection structure, and solar cell module

    WO2026186793A1