Adhesive film for circuit connection, method of producing circuit connection structure, and adhesive film housing set

The adhesive film with a specific layer structure and curable composition effectively addresses the challenge of capturing conductive particles, ensuring reliable circuit connections on flexible boards by reducing resistance and preventing short circuits.

JP2024152791AInactive Publication Date: 2024-10-25RESONAC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024130845
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-03-13
Filing Date
2024-08-07
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional adhesive films used for circuit connections face challenges in efficiently capturing conductive particles between circuit electrodes, leading to poor conduction reliability and short circuits due to uncaptured particles, especially when connecting to flexible boards.

Method used

An adhesive film with a peelable support film, a first adhesive layer containing conductive particles, and a second adhesive layer, where the first adhesive layer's thickness is 0.1 to 1.0 times the average particle diameter, ensuring 90% or more conductive particles are separated, and using a curable composition with a radically polymerizable compound for enhanced connection reliability.

Benefits of technology

The solution provides a circuit connection structure with excellent reliability by efficiently capturing conductive particles, reducing connection resistance, and preventing short circuits, even when applied to flexible boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152791000005
    Figure 2024152791000005
  • Figure 2024152791000006
    Figure 2024152791000006
  • Figure 2024152791000007
    Figure 2024152791000007
Patent Text Reader

Abstract

To provide an adhesive film for circuit connection capable of obtaining a circuit connection structure excellent in connection reliability between facing circuit members even when performing circuit connection by preliminarily pasting on a flexible substrate, a method of producing a circuit connection structure using the same, and an adhesive film housing set.SOLUTION: An adhesive film 11 for circuit connection includes: a peelable support film 12; a first adhesive layer 13 containing a conductive particle P provided on the support film; and a second adhesive layer 14 laminated on the first adhesive layer 13, where a thickness of the first adhesive layer is 0.1 to 1.0 times of an average particle size of the conductive particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive film for circuit connection, a method for producing a circuit connection structure, and an adhesive film receiving set. [Background technology]

[0002] Conventionally, various adhesive materials have been used to connect circuits. For example, an adhesive film for circuit connection having anisotropic conductivity in which conductive particles are dispersed in the adhesive is used as an adhesive material for connecting a liquid crystal display and a tape carrier package (TCP), connecting a flexible printed circuit board (FPC) and a TCP, or connecting an FPC and a printed wiring board. Specifically, a circuit connection structure is obtained by bonding circuit members together through a circuit connection portion formed by the adhesive film for circuit connection, and electrically connecting electrodes on the circuit members together via the conductive particles in the circuit connection portion.

[0003] The adhesive film for circuit connection contains, for example, an adhesive component containing a thermosetting resin or the like, and conductive particles that are blended as necessary, and is formed into a film-like adhesive layer on a substrate such as a polyethylene terephthalate (PET) film. Furthermore, the adhesive film may be used in the form of a reel, which is formed by cutting a raw film into a tape of a width suitable for the application, and winding the tape around a core to form a wound body (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-34468 A Summary of the Invention [Problem to be solved by the invention]

[0005] When connecting a driver IC or the like to an LCD module using an adhesive film, conventionally the adhesive film was first transferred to the glass panel. However, in recent years, there has been a movement to reduce the amount of adhesive film used in order to reduce LCD manufacturing costs, and there is also a demand for narrow-frame panel designs, so a manufacturing method has been adopted in which the adhesive film is first attached to a flexible substrate such as a COF or FPC.

[0006] However, when conventional adhesive films were used, it was difficult to efficiently capture conductive particles between the circuit electrodes, resulting in problems such as a deterioration in electrical reliability and an increased risk of short circuits due to conductive particles that were not captured gathering between the circuits.

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide an adhesive film for circuit connection that can obtain a circuit connection structure having excellent connection reliability between opposing circuit components even when the film is first attached to a flexible substrate to make a circuit connection, a method for producing a circuit connection structure using the same, and an adhesive film storage set. [Means for solving the problem]

[0008] The adhesive film for circuit connection according to one aspect of the present invention comprises a peelable support film, a first adhesive layer containing conductive particles provided on the support film, and a second adhesive layer laminated on the first adhesive layer, wherein the thickness of the first adhesive layer is 0.1 to 1.0 times the average particle size of the conductive particles.

[0009] This adhesive film for circuit connection can provide a circuit connection structure with excellent connection reliability between opposing circuit members, even when the film is first attached to a flexible substrate for circuit connection. In the first adhesive layer, it is preferable that 90% or more of the conductive particles are separated from other conductive particles.

[0010] The first adhesive layer may be made of a cured product of a first curable composition, and the first curable composition may contain a radically polymerizable compound having a radically polymerizable group.

[0011] The second adhesive layer may be composed of a second curable composition, and the second curable composition may contain a radically polymerizable compound having a radically polymerizable group.

[0012] A method for producing a circuit connection structure according to one aspect of the present invention includes the steps of interposing a first adhesive layer and a second adhesive layer of the above-mentioned adhesive film for circuit connection between a first circuit member having a first electrode and a second circuit member having a second electrode, and thermocompressing the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other.

[0013] According to this method, even when the circuit connection is performed by first attaching the adhesive film for circuit connection to the flexible substrate, it is possible to obtain a circuit connection structure having excellent connection reliability between opposing circuit members.

[0014] That is, the method for manufacturing a circuit connection structure according to the present invention may include a step in which a first circuit member has a flexible substrate and a circuit connection adhesive film is attached to the first circuit member such that the second adhesive layer is in contact with the first circuit member.

[0015] An adhesive film storage set according to one aspect of the present invention comprises the above-mentioned adhesive film for circuit connection and a storage member for storing the adhesive film, wherein the storage member has a visible portion that allows the inside of the storage member to be viewed from the outside, and the transmittance of light at a wavelength of 365 nm in the visible portion is 10% or less. Effect of the Invention

[0016] According to the present invention, it is possible to provide an adhesive film for circuit connection that can provide a circuit connection structure having excellent connection reliability between opposing circuit components even when the film is first attached to a flexible substrate to make a circuit connection, a method for producing a circuit connection structure using the same, and an adhesive film storage set. [Brief description of the drawings]

[0017] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of an adhesive film for circuit connection according to the present invention. [Diagram 2] 3A to 3C are schematic cross-sectional views showing steps in a method for producing a circuit connection structure. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a laminate obtained through the steps of FIG. 2. [Figure 4] 3 is a schematic cross-sectional view showing a process subsequent to that shown in FIG. 2. [Diagram 5] 5 is a schematic cross-sectional view showing a circuit connection structure obtained through the steps of FIG. 4. [Figure 6] FIG. 2 is a schematic diagram showing a manufacturing process for the adhesive film for circuit connection shown in FIG. [Figure 7] FIG. 11 is a schematic diagram showing a magnetic field application step. [Figure 8] FIG. 2 is a schematic cross-sectional view showing the state of an adhesive film for circuit connection after a magnetic field application step and a drying step. [Figure 9] FIG. 8 is a schematic cross-sectional view showing a lamination step subsequent to FIG. 7. [Figure 10] 1 is a perspective view showing one embodiment of an adhesive film storage set according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings as needed. In this specification, the upper limit and lower limit values ​​described individually can be arbitrarily combined. In addition, in this specification, "(meth)acrylate" means at least one of acrylate and the corresponding methacrylate. The same applies to other similar expressions such as "(meth)acryloyl".

[0019] <Adhesive film for circuit connection> Fig. 1 is a schematic cross-sectional view showing an adhesive film for circuit connection of one embodiment. As shown in Fig. 1, the adhesive film for circuit connection 11 (hereinafter also simply referred to as "adhesive film 11") comprises a peelable support film 12, a first adhesive layer 13 provided on the support film 12, and a second adhesive layer 14 laminated on the first adhesive layer 13. The first adhesive layer 13 contains conductive particles P.

[0020] In the adhesive film 11, conductive particles P are dispersed in the first adhesive layer 13. Therefore, the adhesive film 11 is an anisotropically conductive adhesive film having anisotropic conductivity. The adhesive film 11 is used to electrically connect the first electrode and the second electrode to each other by interposing a first adhesive layer and a second adhesive layer between a first circuit member having a first electrode and a second circuit member having a second electrode, and thermocompressing the first circuit member and the second circuit member.

[0021] In addition, when the circuit component to be connected has a flexible substrate, the adhesive film for circuit connection 11 can be attached to the first circuit component so that the second adhesive layer is in contact with the first circuit component.

[0022] In this embodiment, the thickness of the first adhesive layer 13 may be 0.1 to 1.0 times, and more preferably 0.1 to 0.7 times, the average particle size of the conductive particles P. In the first adhesive layer 13, 90% or more of the conductive particles P may be separated from other conductive particles.

[0023] In this embodiment, the ratio (X / Y) of the melt viscosity X of the first adhesive layer 13 at the temperature Ty at which the second adhesive layer 14 exhibits the minimum melt viscosity Y to the minimum melt viscosity Y of the second adhesive layer 14 may be 10 or more.

[0024] From the viewpoint of improving the adhesion to the circuit member, the melt viscosity ratio (X / Y) is preferably 10 or more, more preferably 20 or more, even more preferably 50 or more, and particularly preferably 100 or more. From the viewpoint of wettability to the circuit member, the melt viscosity ratio (X / Y) may be 10,000 or less, 5,000 or less, or 1,000 or less. From these viewpoints, the melt viscosity ratio (X / Y) may be 10 to 10,000, 20 to 5,000, 50 to 5,000, or 100 to 1,000. The melt viscosity X and the minimum melt viscosity Y can be confirmed by first measuring the melt viscosity of the second adhesive layer to determine the minimum melt viscosity Y of the second adhesive layer (and the temperature Ty at which the second adhesive layer shows the minimum melt viscosity Y), and then measuring the melt viscosity of the first adhesive layer to determine the melt viscosity X of the first adhesive layer at the temperature Ty. The melt viscosity measurement can also be performed after obtaining the adhesive film.

[0025] (Support film) The support film 12 is formed of, for example, polyethylene terephthalate (PET), polyethylene, polypropylene, or the like. The support film 12 may contain any filler. The surface of the support film 12 may be subjected to a release treatment, a plasma treatment, or the like. The support film 12 can be peeled off after the first adhesive layer and the second adhesive layer are transferred to the circuit member.

[0026] (First adhesive layer) The first adhesive layer is, for example, made of a cured product of a first curable composition. The first curable composition may be a photocurable composition, a thermosetting composition, or a mixture of a photocurable composition and a thermosetting composition. The first curable composition contains, for example, (A) a polymerizable compound (hereinafter also referred to as "(A) component"), (B) a polymerization initiator (hereinafter also referred to as "(B) component"), and (C) conductive particles (hereinafter also referred to as "(C) component"). When the first curable composition is a photocurable composition, the first curable composition contains a photopolymerization initiator as the (B) component, and when the first curable composition is a thermosetting composition, the first curable composition contains a thermal polymerization initiator as the (B) component. Such a first adhesive layer can be obtained, for example, by irradiating a layer made of the first curable composition with light or heating to polymerize the (A) component and cure the first curable composition. That is, the first adhesive layer may be composed of conductive particles and an adhesive component obtained by photocuring the first curable composition. The first adhesive layer may be a cured product obtained by completely curing the first curable composition, or may be a cured product obtained by partially curing the first curable composition. That is, when the first curable composition contains the (A) component and the (B) component, the adhesive component may or may not contain unreacted (A) component and (B) component. The first adhesive layer may be composed of a resin composition other than the cured product of the curable composition. For example, the first adhesive layer may be composed of a resin composition containing a resin component such as a phenoxy resin such as PKHC, a polyester urethane resin, a polyurethane resin, or an acrylic rubber. By using such a resin component, the melt viscosity at a temperature (for example, 100°C) at which the second adhesive layer shows the minimum melt viscosity can be adjusted to about 100,000 to 10,000,000 Pa·s, and the melt viscosity ratio (X / Y) can be set to 10 or more.

[0027] [Component (A): Polymerizable compound] The component (A) is a compound that is polymerized by, for example, radicals, cations, or anions generated by a polymerization initiator (photopolymerization initiator or thermal polymerization initiator) upon irradiation with light (e.g., ultraviolet light) or heating. The component (A) may be any of a monomer, oligomer, and polymer. As the component (A), one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0028] The (A) component has at least one or more polymerizable groups. The polymerizable group is, for example, a group containing a polymerizable unsaturated double bond (ethylenically unsaturated bond). The polymerizable group is preferably a radically polymerizable group that reacts with a radical, from the viewpoint of easily obtaining a desired melt viscosity, from the viewpoint of preventing peeling between the circuit member and the circuit connection part in a high-temperature and high-humidity environment, and from the viewpoint of further improving the effect of reducing the connection resistance and providing better connection reliability. That is, the (A) component is preferably a radically polymerizable compound. Examples of the radically polymerizable group include a vinyl group, an allyl group, a styryl group, an alkenyl group, an alkenylene group, a (meth)acryloyl group, and a maleimide group. The number of polymerizable groups in the (A) component may be 2 or more from the viewpoint of easily obtaining a desired melt viscosity after polymerization and from the viewpoint of easily controlling the physical properties of the resin after curing, and may be 10 or less from the viewpoint of suppressing curing shrinkage during polymerization. In order to balance the crosslink density and cure shrinkage, a polymerizable compound having a number of polymerizable groups within the above range may be used, and then a polymerizable compound having a number outside the above range may be additionally used.

[0029] Specific examples of the component (A) include (meth)acrylate compounds, maleimide compounds, vinyl ether compounds, allyl compounds, styrene derivatives, acrylamide derivatives, nadimide derivatives, natural rubber, isoprene rubber, butyl rubber, nitrile rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, and carboxylated nitrile rubber.

[0030] Examples of (meth)acrylate compounds include epoxy (meth)acrylate, (poly)urethane (meth)acrylate, methyl (meth)acrylate, polyether (meth)acrylate, polyester (meth)acrylate, polybutadiene (meth)acrylate, silicone acrylate, ethyl (meth)acrylate, 2-cyanoethyl (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-hexyl (meth)acrylate, and 2-methylethyl (meth)acrylate. Acrylate, 2-hydroxyethyl (meth)acrylate, isopropyl (meth)acrylate, hydroxypropyl (meth)acrylate, isobutyl (meth)acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, isooctyl (meth)acrylate, n-lauryl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-(meth)acryloyloxyethyl phosphate, N,N-di Methylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, polyethylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, neo Pentyl glycol di(meth)acrylate, pentaerythritol (meth)acrylate, dipentaerythritol hexa(meth)acrylate, isocyanuric acid modified bifunctional (meth)acrylate, isocyanuric acid modified trifunctional (meth)acrylate, tricyclodecanyl acrylate, dimethylol-tricyclodecane diacrylate, 2-hydroxy-1,3-diacryloxypropane, 2,2-bis[4-(acryloxymethoxy)phenyl]propane, 2,2-bis[4-(acryloxypolyethoxy)phenyl]propane, 2,Examples include 2-di(meth)acryloyloxydiethyl phosphate and 2-(meth)acryloyloxyethyl acid phosphate.

[0031] Examples of the maleimide compound include 1-methyl-2,4-bismaleimidebenzene, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, N,N'-m-toluylene bismaleimide, N,N'-4,4-biphenylene bismaleimide, N,N'-4,4-(3,3'-dimethyl-biphenylene) bismaleimide, N,N'-4,4-(3,3'-dimethyldiphenylmethane) bismaleimide, N,N'-4,4-(3,3'-diethyldiphenylmethane) bismaleimide, N,N'-4,4-diphenylmethane bismaleimide, and N,N'-4,4-diphenylpropane. Examples of the bismaleimide include propane bismaleimide, N,N'-4,4-diphenyl ether bismaleimide, N,N'-3,3-diphenyl sulfone bismaleimide, 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane, 2,2-bis(3-s-butyl-4-8(4-maleimidophenoxy)phenyl)propane, 1,1-bis(4-(4-maleimidophenoxy)phenyl)decane, 4,4'-cyclohexylidene-bis(1-(4maleimidophenoxy)-2-cyclohexylbenzene, and 2,2'-bis(4-(4-maleimidophenoxy)phenyl)hexafluoropropane.

[0032] Examples of the vinyl ether compound include diethylene glycol divinyl ether, dipropylene glycol divinyl ether, cyclohexane dimethanol divinyl ether, and trimethylolpropane trivinyl ether.

[0033] Examples of the allyl compound include 1,3-diallyl phthalate, 1,2-diallyl phthalate, and triallyl isocyanurate.

[0034] The (A) component is preferably a (meth)acrylate compound from the viewpoint of easily obtaining a desired melt viscosity and from the viewpoint of being able to select from compounds with various structures and being easily available. The (A) component may be a (poly)urethane (meth)acrylate compound (urethane (meth)acrylate compound or polyurethane (meth)acrylate compound) from the viewpoint of obtaining further excellent adhesive properties. The (A) component may be a (meth)acrylate compound having a high Tg skeleton such as a dicyclopentadiene skeleton from the viewpoint of obtaining further excellent adhesive properties.

[0035] From the viewpoint of easily obtaining a desired melt viscosity, and from the viewpoint of balancing the crosslink density and the cure shrinkage, further reducing the connection resistance, and improving the connection reliability, the (A) component may be a compound (e.g., polyurethane (meth)acrylate) in which a polymerizable group such as a vinyl group, an allyl group, or a (meth)acryloyl group is introduced into the end or side chain of a thermoplastic resin such as an acrylic resin, a phenoxy resin, or a polyurethane resin. In this case, the weight average molecular weight of the (A) component may be 3000 or more, 5000 or more, or 10,000 or more, from the viewpoint of excellent balance between the crosslink density and the cure shrinkage. In addition, the weight average molecular weight of the (A) component may be 1,000,000 or less, 500,000 or less, or 250,000 or less, from the viewpoint of excellent compatibility with other components. The weight average molecular weight refers to a value measured using a calibration curve of standard polystyrene by gel permeation chromatography (GPC) according to the conditions described in the examples.

[0036] The component (A) preferably contains, as a (meth)acrylate compound, a radically polymerizable compound having a phosphate structure represented by the following general formula (1): In this case, the adhesive strength to the surface of an inorganic material (metal, etc.) is improved, making it suitable for bonding electrodes (for example, circuit electrodes), for example. [ka] [In the formula, n represents an integer of 1 to 3, and R represents a hydrogen atom or a methyl group.]

[0037] The radical polymerizable compound having the phosphoric acid ester structure can be obtained, for example, by reacting phosphoric anhydride with 2-hydroxyethyl (meth)acrylate. Specific examples of the radical polymerizable compound having the phosphoric acid ester structure include mono(2-(meth)acryloyloxyethyl)acid phosphate, di(2-(meth)acryloyloxyethyl)acid phosphate, etc.

[0038] The content of the (A) component may be 5% by mass or more, 10% by mass or more, or 20% by mass or more based on the total mass of the first curable composition from the viewpoint of easily obtaining a desired melt viscosity and a desired physical property of the cured product. The content of the (A) component may be 90% by mass or less, 80% by mass or less, or 70% by mass or less based on the total mass of the first curable composition from the viewpoint of suppressing cure shrinkage during polymerization.

[0039] [Component (B): Polymerization initiator] The (B) component may be a photopolymerization initiator (photoradical polymerization initiator, photocationic polymerization initiator, or photoanionic polymerization initiator) that generates radicals, cations, or anions by irradiation with light having a wavelength in the range of 150 to 750 nm, preferably light having a wavelength in the range of 254 to 405 nm, and more preferably light having a wavelength of 365 nm (for example, ultraviolet light), or may be a thermal polymerization initiator (thermal radical polymerization initiator, thermal cationic polymerization initiator, or thermal anionic polymerization initiator) that generates radicals, cations, or anions by heat. The (B) component is preferably a radical polymerization initiator (photoradical polymerization initiator or thermal radical polymerization initiator) from the viewpoint of easily obtaining a desired melt viscosity, further improving the effect of reducing the connection resistance and providing better connection reliability, and making it easier to cure at low temperature and in a short time. As the (B) component, one type of compound may be used alone, or multiple types of compounds may be used in combination. For example, the first curable composition may contain both a photopolymerization initiator and a thermal polymerization initiator as the (B) component.

[0040] The photoradical polymerization initiator is decomposed by light to generate free radicals. That is, the photoradical polymerization initiator is a compound that generates radicals by applying light energy from the outside. Examples of the photoradical polymerization initiator include compounds having an oxime ester structure, a bisimidazole structure, an acridine structure, an α-aminoalkylphenone structure, an aminobenzophenone structure, an N-phenylglycine structure, an acylphosphine oxide structure, a benzyl dimethyl ketal structure, an α-hydroxyalkylphenone structure, and the like. From the viewpoint of easily obtaining a desired melt viscosity and from the viewpoint of being more excellent in the effect of reducing the connection resistance, the photoradical polymerization initiator preferably has at least one structure selected from the group consisting of an oxime ester structure, an α-aminoalkylphenone structure, and an acylphosphine oxide structure.

[0041] Specific examples of compounds having an oxime ester structure include 1-phenyl-1,2-butanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-methoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-1,2-propanedione-2-o-benzoyloxime, 1,3-diphenylpropanetrione-2-(o-ethoxycarbonyl)oxime, 1-phenyl-3-ethoxypropanetrione-2-(o-benzoyl)oxime, 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(o-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime), and the like.

[0042] Specific examples of compounds having an α-aminoalkylphenone structure include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-morpholinophenyl)-butanone-1, and the like.

[0043] Specific examples of the compound having an acylphosphine oxide structure include bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide.

[0044] The thermal radical polymerization initiator decomposes by heat to generate free radicals. That is, the thermal radical polymerization initiator is a compound that generates radicals by applying thermal energy from the outside. The thermal radical polymerization initiator can be arbitrarily selected from conventionally known organic peroxides and azo compounds. From the viewpoints of stability, reactivity, and compatibility, the thermal radical polymerization initiator is preferably an organic peroxide having a one-minute half-life temperature of 90 to 175°C and a weight average molecular weight of 180 to 1000. By having the one-minute half-life temperature in this range, the storage stability is further excellent, the radical polymerizability is sufficiently high, and curing in a short time is possible.

[0045] Specific examples of organic peroxides include 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, cumyl peroxyneodecanoate, dilauroyl peroxide, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, 1,1,3,3-Tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, t-amylperoxy-3,5,5-trimethylhexanoate peroxyneodecanoate, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, t-amyl peroxyneodecanoate, t-amyl peroxy-2-ethylhexanoate, di(3-methylbenzoyl) peroxide, dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate peroxybenzoate, 2,5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxybenzoate, dibutyl peroxytrimethyladipate, t-amyl peroxy normal octoate, t-amyl peroxy isononanoate, and t-amyl peroxybenzoate.

[0046] Specific examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile).

[0047] The content of the (B) component may be 0.1 mass% or more, or 0.5 mass% or more, based on the total mass of the first curable composition, from the viewpoint of excellent fast curing property and excellent effect of reducing connection resistance. The content of the (B) component may be 15 mass% or less, 10 mass% or less, or 5 mass% or less, based on the total mass of the first curable composition, from the viewpoint of improving storage stability and excellent effect of reducing connection resistance.

[0048] From the viewpoint of easily obtaining the desired viscosity, the first curable composition preferably contains at least one of a photopolymerization initiator and a thermal polymerization initiator as component (B), and from the viewpoint of facilitating the production of the adhesive film for circuit connection, it is more preferable for the first curable composition to contain a photopolymerization initiator.

[0049] [(C) Component: Conductive particles] The component (C) is not particularly limited as long as it is a particle having electrical conductivity, and may be a metal particle composed of a metal such as Au, Ag, Ni, Cu, or solder, or a conductive carbon particle composed of conductive carbon. The component (C) may be a coated conductive particle having a core containing non-conductive glass, ceramic, plastic (polystyrene, etc.), and a coating layer containing the above metal or conductive carbon and coating the core. Among these, metal particles formed of a heat-fusible metal, or coated conductive particles having a core containing a plastic and a coating layer containing a metal or conductive carbon and coating the core are preferably used. In this case, since the cured product of the first curable composition can be easily deformed by heating or pressure, when the electrodes are electrically connected to each other, the contact area between the electrodes and the component (C) can be increased, and the conductivity between the electrodes can be further improved.

[0050] The (C) component may be an insulating coated conductive particle comprising the above-mentioned metal particle, conductive carbon particle, or coated conductive particle, and an insulating layer containing an insulating material such as resin and coating the surface of the particle. When the (C) component is an insulating coated conductive particle, even if the content of the (C) component is high, the particle surface is coated with resin, so that the occurrence of a short circuit due to contact between the (C) components can be suppressed, and the insulation between adjacent electrode circuits can also be improved. The (C) component is used as one type of the above-mentioned various conductive particles alone or in combination of two or more types.

[0051] The maximum particle size of the (C) component must be smaller than the minimum distance between the electrodes (the shortest distance between adjacent electrodes). From the viewpoint of excellent dispersibility and electrical conductivity, the maximum particle size of the (C) component may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and electrical conductivity, the maximum particle size of the (C) component may be 50 μm or less, 30 μm or less, or 20 μm or less. In this specification, the particle size of 300 arbitrary conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the largest value obtained is defined as the maximum particle size of the (C) component. Note that, when the (C) component has protrusions or the like and is not spherical, the particle size of the (C) component is defined as the diameter of a circle circumscribing the conductive particle in the SEM image.

[0052] From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (C) component may be 1.0 μm or more, 2.0 μm or more, or 2.5 μm or more. From the viewpoint of excellent dispersibility and conductivity, the average particle size of the (C) component may be 50 μm or less, 30 μm or less, or 20 μm or less. In this specification, the particle size of 300 arbitrary conductive particles (pcs) is measured by observation using a scanning electron microscope (SEM), and the average value of the particle sizes obtained is defined as the average particle size.

[0053] In the first adhesive layer, the component (C) is preferably uniformly dispersed. From the viewpoint of obtaining a stable connection resistance, the particle density of the component (C) in the first adhesive layer is preferably 100 pcs / mm 2 It may be more than 1000pcs / mm 2 More than 2000pcs / mm 2 From the viewpoint of improving the insulating properties between adjacent electrodes, the particle density of the component (C) in the first adhesive layer may be 100,000 pcs / mm 2 may be less than 50000pcs / mm 2 It may be less than 10000pcs / mm 2 It may be the following:

[0054] The content of the (C) component may be 0.1 volume % or more, 1 volume % or more, or 5 volume % or more based on the total volume in the first adhesive layer from the viewpoint of further improving the electrical conductivity. The content of the (C) component may be 50 volume % or less, 30 volume % or less, or 20 volume % or less based on the total volume in the first adhesive layer from the viewpoint of easily suppressing short circuits. The content of the (C) component in the first curable composition (based on the total volume of the first curable composition) may be the same as the above range.

[0055] [Other ingredients] The first curable composition may further contain other components in addition to the components (A), (B) and (C). Examples of the other components include a thermoplastic resin, a coupling agent and a filler. These components may be contained in the first adhesive layer.

[0056] Examples of the thermoplastic resin include phenoxy resin, polyester resin, polyamide resin, polyurethane resin, polyester urethane resin, and acrylic rubber. When the first curable composition contains a thermoplastic resin, the first adhesive layer can be easily formed. When the first curable composition contains a thermoplastic resin, the stress of the first adhesive layer generated during curing of the first curable composition can be alleviated. When the thermoplastic resin has a functional group such as a hydroxyl group, the adhesion of the first adhesive layer is likely to be improved. The content of the thermoplastic resin may be, for example, 5% by mass or more and 80% by mass or less based on the total mass of the first curable composition.

[0057] Examples of the coupling agent include silane coupling agents having organic functional groups such as (meth)acryloyl groups, mercapto groups, amino groups, imidazole groups, and epoxy groups, silane compounds such as tetraalkoxysilanes, tetraalkoxytitanate derivatives, and polydialkyltitanate derivatives. When the first curable composition contains a coupling agent, the adhesiveness can be further improved. The content of the coupling agent may be, for example, 0.1% by mass or more and 20% by mass or less based on the total mass of the first curable composition.

[0058] Examples of the filler include non-conductive fillers (e.g., non-conductive particles). When the first curable composition contains a filler, further improvement in connection reliability can be expected. The filler may be either an inorganic filler or an organic filler. Examples of the inorganic filler include inorganic fine particles such as metal oxide fine particles such as silica fine particles, alumina fine particles, silica-alumina fine particles, titania fine particles, and zirconia fine particles; and nitride fine particles. Examples of the organic filler include organic fine particles such as silicone fine particles, methacrylate-butadiene-styrene fine particles, acrylic-silicone fine particles, polyamide fine particles, and polyimide fine particles. These fine particles may have a uniform structure or a core-shell structure. The maximum diameter of the filler is preferably less than the minimum particle diameter of the conductive particles. The content of the filler may be, for example, 0.1% by volume or more and 50% by volume or less based on the total volume of the first curable composition.

[0059] The first curable composition may contain other additives such as a softener, an accelerator, an anti-degradant, a colorant, a flame retardant, a thixotropic agent, etc. The content of these additives may be, for example, 0.1 to 10 mass% based on the total mass of the first curable composition. These additives may be contained in the first adhesive layer.

[0060] The first curable composition may contain a thermosetting resin instead of the (A) and (B) components, or in addition to the (A) and (B) components. The thermosetting resin is a resin that is cured by heat and has at least one thermosetting group. The thermosetting resin is, for example, a compound that crosslinks by reacting with a curing agent by heat. As the thermosetting resin, one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0061] The thermosetting group may be, for example, an epoxy group, an oxetane group, an isocyanate group, or the like, from the viewpoint of easily obtaining a desired melt viscosity and further improving the effect of reducing connection resistance and providing more excellent connection reliability.

[0062] Specific examples of thermosetting resins include epoxy resins such as bisphenol-type epoxy resins which are reaction products of epichlorohydrin with bisphenol A, F, AD, or the like; epoxy novolac resins which are reaction products of epichlorohydrin with phenol novolac, cresol novolac, or the like; naphthalene-based epoxy resins having a skeleton containing a naphthalene ring; and various epoxy compounds having two or more glycidyl groups in one molecule, such as glycidyl amine and glycidyl ether.

[0063] When a thermosetting resin is used instead of the components (A) and (B), the content of the thermosetting resin in the first curable composition may be, for example, 20 mass% or more and 80 mass% or less based on the total mass of the first curable composition. When a thermosetting resin is used in addition to the components (A) and (B), the content of the thermosetting resin in the first curable composition may be, for example, 30 mass% or more and 70 mass% or less based on the total mass of the first curable composition.

[0064] When the first curable composition contains a thermosetting resin, the first curable composition may contain the above-mentioned curing agent for the thermosetting resin. Examples of the curing agent for the thermosetting resin include a thermal radical generator, a thermal cation generator, and a thermal anion generator. The content of the curing agent may be, for example, 0.1 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the thermosetting resin.

[0065] The first adhesive layer may contain components derived from the first curable composition, such as unreacted (A) component and (B) component. When the adhesive film of this embodiment is stored and transported in a conventional storage member, the unreacted (B) component remains in the first adhesive layer, and during storage and transport, a part of the second curable composition in the second adhesive layer is cured, and it is presumed that problems such as peeling between the circuit member and the circuit connection part in a high temperature and high humidity environment and a decrease in the effect of reducing the connection resistance of the adhesive film occur. Therefore, from the viewpoint of suppressing the occurrence of the above problems, the content of the (B) component in the first adhesive layer may be 15% by mass or less, 10% by mass or less, or 5% by mass or less based on the total mass of the first adhesive layer. The content of the (B) component in the first adhesive layer may be 0.1% by mass or more based on the total mass of the first adhesive layer. When the first adhesive layer contains a photopolymerization initiator as the component (B), the occurrence of the above problems can be suppressed by storing the adhesive film in a storage member described below.

[0066] The melt viscosity X of the first adhesive layer at the temperature Ty at which the second adhesive layer exhibits the minimum melt viscosity Y may be 1000 Pa·s or more, 10000 Pa·s or more, or 50000 Pa·s or more, from the viewpoint of making peeling less likely to occur. The melt viscosity X may be 10000000 Pa·s or less, 1000000 Pa·s or less, or 500000 Pa·s or less, from the viewpoint of excellent wettability to the substrate. The melt viscosity X can be adjusted by changing the composition of the first curable composition, changing the curing conditions of the first curable composition, or the like.

[0067] The thickness of the first adhesive layer may be 0.1 times or more, 0.2 times or more, or 0.3 times or more of the average particle size of the conductive particles, from the viewpoint of making the conductive particles more easily trapped between the electrodes and further reducing the connection resistance. The thickness of the first adhesive layer 2 may be 1.0 times or less, 0.8 times or less, or 0.7 times or less of the average particle size of the conductive particles, from the viewpoint of making the conductive particles more easily crushed when sandwiched between the opposing electrodes during thermocompression bonding and further reducing the connection resistance. From these viewpoints, the thickness of the first adhesive layer may be 0.1 to 0.7 times, 0.2 to 0.8 times, or 0.3 to 0.7 times the average particle size of the conductive particles. The thickness of the adhesive layer refers to the thickness of the adhesive layer located in the space between adjacent conductive particles. When the thickness of the first adhesive layer and the average particle size of the conductive particles satisfy the above-mentioned relationship, for example, as shown in Fig. 1, some of the conductive particles P in the first adhesive layer 13 may protrude from the first adhesive layer 13 toward the second adhesive layer 14. In this case, the boundary S between the first adhesive layer 13 and the second adhesive layer 14 is located in the space between adjacent conductive particles P. The conductive particles P are not exposed on the surface of the first adhesive layer 13 opposite the second adhesive layer 14, and the opposite surface may be a flat surface.

[0068] The thickness of the first adhesive layer may be appropriately set according to the height of the electrodes of the circuit members to be bonded. The thickness of the first adhesive layer may be, for example, 0.5 μm or more and 20 μm or less. In addition, when a part of the conductive particles is exposed from the surface of the first adhesive layer (for example, protruding to the second adhesive layer side), the distance from the surface of the first adhesive layer opposite to the second adhesive layer side to the boundary S between the first adhesive layer and the second adhesive layer located in the spaced portion between the adjacent conductive particles is the thickness of the first adhesive layer, and the exposed portion of the conductive particles is not included in the thickness of the first adhesive layer. The length of the exposed portion of the conductive particles may be, for example, 0.1 μm or more and 20 μm or less. The thickness of the adhesive layer can be measured by the following method. The adhesive film was sandwiched between two pieces of glass (thickness: approximately 1 mm) and a resin composition consisting of 100 g of bisphenol A type epoxy resin (product name: JER811, manufactured by Mitsubishi Chemical Corporation) and 10 g of a hardener (product name: Epomount Hardener, manufactured by Refine Tech Co., Ltd.) was poured into the mold. The cross section was then polished using a polishing machine, and the thickness of each adhesive layer was measured using a scanning electron microscope (SEM, product name: SE-8020, manufactured by Hitachi High-Tech Science Corporation).

[0069] (Second adhesive layer) The second adhesive layer is, for example, made of a second curable composition. The second curable composition contains, for example, (a) a polymerizable compound (hereinafter also referred to as (a) component) and (b) a polymerization initiator (hereinafter also referred to as (b) component). The second curable composition may be a thermosetting composition containing a thermal polymerization initiator as the (b) component, a photocurable composition containing a photopolymerization initiator as the (b) component, or a mixture of a thermosetting composition and a photocurable composition. The second curable composition constituting the second adhesive layer is an uncured curable composition that can flow when a circuit is connected, for example, an uncured curable composition.

[0070] [Component (a): Polymerizable compound] The component (a) is a compound that is polymerized by radicals, cations, or anions generated by a polymerization initiator (photopolymerization initiator or thermal polymerization initiator) by irradiation with light (e.g., ultraviolet light) or heating. The compounds exemplified as the component (A) can be used as the component (a). The component (a) is preferably a radical polymerizable compound having a radical polymerizable group that reacts with a radical, from the viewpoint of facilitating connection at low temperature in a short time and easily obtaining a desired melt viscosity, and from the viewpoint of further improving the effect of reducing the connection resistance and providing better connection reliability. Examples of preferred radical polymerizable compounds in the component (a) and combinations of preferred radical polymerizable compounds are the same as those for the component (A). When the component (a) is a radical polymerizable compound and the component (B) in the first adhesive layer is a photoradical polymerization initiator, the adhesive film is accommodated in a storage member described later, which tends to significantly suppress the curing of the second curable composition during storage or transportation of the adhesive film.

[0071] Component (a) may be any of a monomer, oligomer, or polymer. As component (a), one type of compound may be used alone, or multiple types of compounds may be used in combination. Component (a) may be the same as or different from component (A).

[0072] The content of the (a) component may be 10 mass % or more, 20 mass % or more, or 30 mass % or more based on the total mass of the second curable composition, from the viewpoint of easily obtaining a crosslink density required for reducing connection resistance and improving connection reliability. The content of the (a) component may be 90 mass % or less, 80 mass % or less, or 70 mass % or less based on the total mass of the second curable composition, from the viewpoint of suppressing cure shrinkage during polymerization and obtaining good reliability.

[0073] [Component (b): Polymerization initiator] As the component (b), a polymerization initiator similar to the polymerization initiator exemplified as the component (B) can be used. The component (b) is preferably a radical polymerization initiator. Examples of preferred radical polymerization initiators for the component (b) are the same as those for the component (B). As the component (b), one type of compound may be used alone, or multiple types of compounds may be used in combination.

[0074] The content of the (b) component may be 0.1 mass % or more, 0.5 mass % or more, or 1 mass % or more, based on the total mass of the second curable composition, from the viewpoint of facilitating connection at low temperature in a short time and from the viewpoint of more excellent connection reliability. The content of the (b) component may be 30 mass % or less, 20 mass % or less, or 10 mass % or less, based on the total mass of the second curable composition, from the viewpoint of pot life.

[0075] [Other ingredients] The second curable composition may further contain other components in addition to the components (a) and (b). Examples of the other components include a thermoplastic resin, a coupling agent, a filler, a softener, an accelerator, an anti-degradant, a colorant, a flame retardant, a thixotropic agent, etc. Details of the other components are the same as those of the other components in the first adhesive layer.

[0076] The second curable composition may contain a thermosetting resin instead of the (a) component and the (b) component, or in addition to the (a) component and the (b) component. When the second curable composition contains a thermosetting resin, the second curable composition may contain a curing agent used to cure the thermosetting resin. As the thermosetting resin and the curing agent, the same thermosetting resin and curing agent as the thermosetting resin and the curing agent exemplified as the other components in the first curable composition can be used. When a thermosetting resin is used instead of the (a) component and the (b) component, the content of the thermosetting resin in the second curable composition may be, for example, 20% by mass or more and 80% by mass or less based on the total mass of the second curable composition. When a thermosetting resin is used in addition to the (a) component and the (b) component, the content of the thermosetting resin in the second curable composition may be, for example, 20% by mass or more and 80% by mass or less based on the total mass of the second curable composition. The content of the curing agent may be in the same range as that described above for the content of the curing agent in the first curable composition.

[0077] The content of the conductive particles in the second adhesive layer may be, for example, 1 mass % or less, or may be 0 mass %, based on the total mass of the second adhesive layer. It is preferable that the second adhesive layer does not contain conductive particles.

[0078] The minimum melt viscosity Y of the second adhesive layer may be 50 Pa·s or more, 100 Pa·s or more, or 300 Pa·s or more, from the viewpoint of obtaining excellent blocking resistance. The minimum melt viscosity Y may be 100,000 Pa·s or less, 10,000 Pa·s or less, or 5,000 Pa·s or less, from the viewpoint of obtaining excellent filling property (resin filling property) between the electrodes. The minimum melt viscosity Y can be adjusted by changing the composition of the second curable composition, etc.

[0079] The thickness of the second adhesive layer may be appropriately set according to the height of the electrodes of the circuit member to be bonded. The thickness of the second adhesive layer may be 5 μm or more and 200 μm or less from the viewpoint of being able to sufficiently fill the space between the electrodes to seal the electrodes and obtain better reliability. In addition, when a part of the conductive particles is exposed from the surface of the first adhesive layer (for example, protruding toward the second adhesive layer), the thickness of the second adhesive layer is the distance from the surface of the second adhesive layer opposite to the first adhesive layer side to the boundary S between the first adhesive layer and the second adhesive layer located in the space between the adjacent conductive particles.

[0080] The ratio of the thickness of the first adhesive layer 2 to the thickness of the second adhesive layer (thickness of the first adhesive layer / thickness of the second adhesive layer) may be 1 or more and 1000 or less, from the viewpoint of being able to sufficiently fill the space between the electrodes to seal the electrodes and obtain better reliability.

[0081] The thickness of the adhesive film (the total thickness of all layers constituting the adhesive film) may be, for example, 5 μm or more and 200 μm or less.

[0082] The above-mentioned adhesive film for circuit connection comprises a peelable support film and an adhesive layer provided on the support film, the adhesive layer containing an adhesive component and conductive particles, the conductive particles being unevenly distributed on the support film side and dispersed in a direction perpendicular to the thickness direction of the adhesive layer, and the adhesive layer may have, in the thickness direction of the adhesive layer from the support film side, a first region containing the cured product of the above-mentioned first curable composition and a second region containing the above-mentioned second curable composition. The ranges of the first region and the second region in the thickness direction of the adhesive layer can be set in the same manner as the thicknesses of the above-mentioned first adhesive layer and second adhesive layer, respectively. The conductive particles can also be set in the same manner as the above-mentioned conditions.

[0083] Although the adhesive film for circuit connection of this embodiment has been described above, the present invention is not limited to the above embodiment.

[0084] [Method of manufacturing circuit connection structure] The method for producing a circuit connection structure of this embodiment is a method for producing a circuit connection structure in which a first circuit member provided with a first circuit electrode and a second circuit member provided with a second circuit electrode corresponding to the first circuit electrode are connected via the adhesive film for circuit connection of this embodiment described above.

[0085] The method of the present embodiment includes, for example, a preparation step of preparing the adhesive film for circuit connection of the present embodiment described above; a laminating step of laminating the adhesive film for circuit connection onto the first circuit member such that the second adhesive layer side of the adhesive film for circuit connection faces the surface of the first circuit member on which the circuit electrodes are provided; a heating and pressurizing step of placing a second circuit member on a first circuit member laminated with an adhesive film for circuit connection such that the first circuit electrode and the second circuit electrode face each other, and pressing the first circuit member and the second circuit member in a direction in which the first circuit electrode and the second circuit electrode face each other while heating the adhesive film for circuit connection; Equipped with.

[0086] (preparation process) In this step, the adhesive film for circuit connection of the present embodiment described above can be produced. The method for producing an adhesive film for circuit connection of this embodiment may, for example, include a preparation step (first preparation step) of preparing the above-mentioned first adhesive layer, and a lamination step of laminating the above-mentioned second adhesive layer on the first adhesive layer. The method for producing an adhesive film for circuit connection may further include a preparation step (second preparation step) of preparing a second adhesive layer.

[0087] In the first preparation step, for example, the first adhesive layer is formed on a support film to obtain a first adhesive film, thereby preparing the first adhesive layer. Specifically, first, the (A) component, the (B) component, and the (C) component, as well as other components added as necessary, are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc., to prepare a varnish composition. Thereafter, the varnish composition is applied to a substrate that has been subjected to a release treatment using a knife coater, roll coater, applicator, comma coater, die coater, etc., and the organic solvent is volatilized by heating to form a layer made of the first curable composition on the substrate. Next, the layer made of the first curable composition is irradiated with light or heated to cure the first curable composition, thereby forming a first adhesive layer on the substrate (curing step). This results in a first adhesive film.

[0088] The organic solvent used in the preparation of the varnish composition is preferably one that has the property of dissolving or dispersing each component uniformly, and examples thereof include toluene, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, propyl acetate, butyl acetate, etc. These organic solvents can be used alone or in combination of two or more. The stirring and mixing and kneading in the preparation of the varnish composition can be performed using, for example, a stirrer, a grinding machine, a three-roll mill, a ball mill, a bead mill, or a homodisper.

[0089] The support film is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent when the first curable composition is cured by light, and is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent and the heating conditions when curing the first curable composition when the first curable composition is cured by heating. As the support film, for example, a substrate (for example, a film) made of oriented polypropylene (OPP), polyethylene terephthalate (PET), polyethylene naphthalate, polyethylene isophthalate, polybutylene terephthalate, polyolefin, polyacetate, polycarbonate, polyphenylene sulfide, polyamide, polyimide, cellulose, ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, synthetic rubber, liquid crystal polymer, etc. can be used. From the viewpoint of high versatility, polyethylene terephthalate can be preferably used.

[0090] The heating conditions for volatilizing the organic solvent from the varnish composition applied to the support film are preferably conditions that allow the organic solvent to volatilize sufficiently, for example, at 40° C. or higher and 120° C. or lower for 0.1 minutes or longer and 10 minutes or shorter.

[0091] For the light irradiation in the curing step, it is preferable to use irradiation light having a wavelength in the range of 150 to 750 nm (for example, ultraviolet light). The light irradiation can be carried out using, for example, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a metal halide lamp, or the like. The amount of light irradiation may be adjusted so that the melt viscosity ratio (X / Y) is 10 or more. The amount of light irradiation is, for example, 100 mJ / cm2 in terms of the integrated light amount of light with a wavelength of 365 nm. 2 or more, and 2 or more, and 2 The amount of light irradiation may be, for example, 10,000 mJ / cm2 in terms of the integrated light amount of light with a wavelength of 365 nm. 2 may be less than 5000 mJ / cm 2 or less than 3000 mJ / cm 2The greater the amount of light irradiation (integrated amount of light), the greater the melt viscosity X tends to be, and the greater the melt viscosity ratio (X / Y) tends to be.

[0092] The heating conditions in the curing step may be adjusted so that the melt viscosity ratio (X / Y) is 10 or more. The heating conditions may be, for example, 30°C to 300°C for 0.1 to 5000 minutes, or 50°C to 150°C for 0.1 to 3000 minutes. The higher the heating temperature, the higher the melt viscosity X tends to be, and the higher the melt viscosity ratio (X / Y) tends to be. Also, the longer the heating time, the higher the melt viscosity X tends to be, and the higher the melt viscosity ratio (X / Y) tends to be.

[0093] In the second preparation step, the second adhesive layer is prepared by forming a second adhesive layer on a substrate to obtain a second adhesive film in the same manner as in the first preparation step, except that the (a) component, the (b) component, and other components added as necessary are used, and the curing step is not performed (light irradiation and heating are not performed). The substrate may be the same as the support film described above.

[0094] In the lamination process, the second adhesive layer may be laminated onto the first adhesive layer by bonding the first adhesive film and the second adhesive film together, or the second adhesive layer may be laminated onto the first adhesive layer by applying a varnish composition obtained using components (a) and (b) and other components added as necessary onto the first adhesive layer and volatilizing the organic solvent.

[0095] Examples of the method for bonding the first adhesive film and the second adhesive film include hot pressing, roll lamination, vacuum lamination, etc. Lamination may be performed under heating conditions of, for example, 0 to 80°C.

[0096] In addition, in this embodiment, when using an adhesive film for circuit connection in which 90% or more of the conductive particles P are separated from other conductive particles in the first adhesive layer, such a dispersed state can be formed by a magnetic field application step described later. In this case, as the conductive particles P, particles containing nickel are preferably used from the viewpoint of performing dispersion by the magnetic field application step. In general, iron, cobalt, and nickel are ferromagnetic materials and are known to be magnetized by an external magnetic field, but among these, the use of nickel is significant in that it can achieve both electrical conductivity and dispersibility by applying a magnetic field. In addition, in order to obtain storage stability of the conductive particles P, the surface layer of the conductive particles P may be made of platinum group precious metals such as gold and silver instead of nickel. In addition, the surface of nickel may be coated with precious metals such as Au. Furthermore, non-conductive glass, ceramic, plastic, etc. coated with a conductive material such as the above metal may be used, and in this case, a nickel layer may also be provided to form a multilayer structure.

[0097] In addition, since the magnetism of nickel is affected by the phosphorus concentration contained in the nickel plating, it is preferable to adjust the magnetism required for dispersing the conductive particles P by the magnetic field as needed. The magnetism of the conductive particles P can be measured, for example, by a vibrating sample magnetometer (VSM). In order to disperse the conductive particles P by an external magnetic field, it is preferable that the saturation magnetization is in the range of 5.0 emu / g to 50 emu / g in the VSM measurement. If it is 5.0 emu / g or more, it becomes easy to sufficiently disperse the conductive particles P. On the other hand, if it is 50 emu / g or less, the magnetization of the conductive particles P does not become too large, and the conductive particles P are suppressed from bonding in the thickness direction of the first adhesive layer 13, and the dispersibility of the conductive particles P tends to be high.

[0098] The average particle size of the conductive particles P is preferably 1.0 μm or more and 10.0 μm or less. When the average particle size of the conductive particles P is 1.0 μm or more, the coating accuracy on the support film is high, and it is easy to disperse the conductive particles P well in the first adhesive layer. When the average particle size of the conductive particles P is 10.0 μm or less, there is a tendency that good insulation between adjacent circuit electrodes of the connection structure is obtained. In order to obtain good dispersibility of the conductive particles P, the average particle size of the conductive particles P is more preferably 2.0 μm or more, and even more preferably 2.5 μm or more. On the other hand, from the viewpoint of ensuring insulation between adjacent circuit electrodes of the connection structure, the average particle size of the conductive particles P is more preferably 8.5 μm or less, more preferably 7 μm or less, and even more preferably 6.0 μm or less.

[0099] The amount of conductive particles P is preferably 1 to 100 parts by volume per 100 parts by volume of the components other than the conductive particles P in the first adhesive layer. From the viewpoint of preventing short-circuiting between adjacent circuit electrodes due to the presence of an excessive amount of conductive particles P, the amount of conductive particles P is more preferably 10 to 50 parts by volume. Furthermore, when the average particle size of the conductive particles is in the range of 1.0 μm or more and 10.0 μm or less, the particle density of the conductive particles is more preferably 1000 particles / mm 2 More than 50000 pieces / mm 2 In this case, it is possible to more suitably achieve both the dispersibility of the conductive particles P and the insulation between adjacent circuit electrodes.

[0100] (Lamination process) 2 is a schematic cross-sectional view showing a lamination step in the manufacturing method of the connection structure of this embodiment. In this step, as shown in the figure, the circuit connection adhesive film 11 is laminated onto the first circuit member 2 so that the second adhesive layer 14 side of the circuit connection adhesive film 11 faces the surface of the first circuit member 2 on which the first circuit electrode 6 is provided. If the circuit connection adhesive film 11 has a release film provided on the second adhesive layer 14, the second adhesive layer 14 can be laminated onto the first circuit member 2 after or while peeling off the release film so that the second adhesive layer 14 is in close contact with the first circuit member 2.

[0101] The first circuit member 2 has a circuit electrode 6 on the mounting surface 5a side of the main body 5. Examples of the first circuit member 2 include members having a flexible substrate such as COP, FCP, and polyimide. Examples of the circuit electrode 6 include copper plated with a metal such as tin. Note that an insulating layer may be formed on the mounting surface 5a in a portion where the circuit electrode 6 is not formed.

[0102] A known laminator can be used as a means for lamination. The lamination conditions can be appropriately set.

[0103] FIG. 3 is a schematic cross-sectional view showing a laminate obtained through a lamination process.

[0104] (Heat and pressure process) 4 is a schematic cross-sectional view showing a heating and pressurizing step in the manufacturing method of the connection structure of this embodiment. In this step, as shown in the figure, the second circuit member 3 is placed on the first circuit member 2 on which the circuit connection adhesive film (second adhesive layer 14 and first adhesive layer 13) is laminated so that the first circuit electrode 6 and the second circuit electrode 8 face each other, and while heating the circuit connection adhesive film (second adhesive layer 14 and first adhesive layer 13), the first circuit member 2 and the second circuit member 3 are pressed in a direction in which the first circuit electrode 6 and the second circuit electrode 8 face each other.

[0105] The second circuit member 3 is, for example, a glass substrate or plastic substrate on which a circuit is formed using ITO, IZO, or a metal used in liquid crystal displays, a ceramic wiring board, etc. The second circuit member 3 has second circuit electrodes 8 corresponding to the first circuit electrodes 6 on the mounting surface 7a side of the main body 7, as shown in Fig. 4.

[0106] The circuit electrodes 8 are, for example, rectangular in plan view and have a thickness of, for example, about 100 nm to 1000 nm. The surfaces of the circuit electrodes 8 are made of one or more materials selected from, for example, gold, silver, copper, tin, ruthenium, rhodium, palladium, osmium, iridium, platinum, indium tin oxide (ITO), and indium zinc oxide (IZO). An insulating layer may also be formed on the mounting surface 7a in the areas where the circuit electrodes 8 are not formed.

[0107] As the heating means, a known thermocompression bonding device can be used. The heating temperature of the circuit connection adhesive film (the second adhesive layer 14 and the first adhesive layer 13) is preferably equal to or higher than the temperature at which active polymerization species are generated in the curing agent and polymerization of the polymerization monomer is initiated. The heating temperature is, for example, 80°C to 200°C, and preferably 100°C to 180°C. The heating time is, for example, 0.1 seconds to 30 seconds, and preferably 1 second to 20 seconds. When the heating temperature is 80°C or higher, a sufficient curing speed is easily obtained, and when it is 200°C or lower, undesired side reactions are less likely to proceed. When the heating time is 0.1 seconds or higher, the curing reaction is easily allowed to proceed sufficiently, and when it is 30 seconds or shorter, the productivity of the cured product is easily maintained, and undesired side reactions are also less likely to proceed.

[0108] As the pressing means, a known thermocompression device can be used. The pressure and time of pressing can be appropriately set.

[0109] 5 is a schematic cross-sectional view showing a circuit connection structure obtained through a heating and pressing process. In the heating and pressing process, the adhesive component of the circuit connection adhesive film (the second adhesive layer 14 and the first adhesive layer 13) flows, and the distance between the first circuit electrode 6 and the second circuit electrode 8 is shortened and the conductive particles P are interlocked, and the second adhesive layer and the first adhesive layer are cured. By curing the second adhesive layer and the first adhesive layer, the first circuit electrode 6 and the second circuit electrode 8 are electrically connected, and adjacent circuit electrodes 6, 6 and adjacent circuit electrodes 8, 8 are electrically insulated from each other, and a cured product 4 of the circuit connection adhesive film (the second adhesive layer 14 and the first adhesive layer 13) is formed, and the circuit connection structure 1 shown in FIG. 5 is obtained. In the obtained circuit connection structure 1, the cured product 4 of the circuit connection adhesive film (second adhesive layer 14 and first adhesive layer 13) sufficiently prevents the distance between the first circuit electrode 6 and the second circuit electrode 8 from changing over time, while also ensuring the long-term reliability of the electrical characteristics.

[0110] The cured product 4 of the adhesive film for circuit connection (second adhesive layer 14 and first adhesive layer 13) has a first region 9 formed by curing the first adhesive layer 13, and a second region 10 formed by curing the second adhesive layer 14. In this embodiment, the first region 9 is located on the second circuit member 3 side, and the second region 10 is located on the first circuit member 2 side.

[0111] The conductive particles P are interposed between the first circuit electrode 6 and the second circuit electrode 8 in a state where they are slightly deformed into a flat shape by compression bonding. This realizes an electrical connection between the first circuit electrode 6 and the second circuit electrode 8. Furthermore, the conductive particles P are spaced apart between adjacent first circuit electrodes 6, 6 and between adjacent second circuit electrodes 8, 8, realizing electrical insulation between adjacent first circuit electrodes 6, 6 and adjacent second circuit electrodes 8, 8.

[0112] [Method of manufacturing circuit connecting adhesive film] Fig. 6 is a schematic diagram showing the manufacturing process of the adhesive film for circuit connection shown in Fig. 1. In the example shown in the figure, a long support film 12 is transported at a predetermined speed by a pay-out roller 21 and a take-up roller 22. A coater 23 for applying an adhesive paste W, which is a material for forming the first adhesive layer 13, is arranged on the transport path of the support film 12, and the adhesive paste W in which conductive particles P are dispersed is applied onto the support film 12 by the coater 23 (application process). The thickness of the adhesive paste W applied onto the support film 12 by the coater 23 varies from time to time depending on the proportion of the solvent contained in the resin composition, but is preferably less than 1.6 times the average particle size of the conductive particles P.

[0113] The viscosity of the adhesive paste W can be varied depending on the application and application method, but is usually preferably 10 mPa·s to 10,000 mPa·s. From the viewpoint of suppressing separation of the components in the adhesive paste W and improving compatibility, it is more preferable to set it to 50 mPa·s to 5,000 mPa·s. Furthermore, in order to improve the appearance of the circuit connection adhesive film 11, it is preferable to set it to 100 mPa·s to 3,000 mPa·s. If it is 10,000 mPa·s or less, it becomes difficult to suppress the dispersion of the conductive particles P in the subsequent magnetic field application step, and if it is 10 mPa·s or more, separation of the components in the adhesive paste W becomes difficult to occur.

[0114] The method of applying the adhesive paste W is not limited to the above, and known methods can be used. Examples include spin coating, roller coating, bar coating, dip coating, microgravure coating, curtain coating, die coating, spray coating, doctor coating, kneader coating, flow coating, screen printing, and casting. The bar coating, die coating, and microgravure coating methods are suitable for producing the circuit connection adhesive film 11, and the microgravure coating method is particularly suitable from the viewpoint of the accuracy of the film thickness.

[0115] A pair of magnets 24, 25 are arranged facing each other vertically on the rear side of the coater 23, sandwiching the support film 12. In this embodiment, as shown in Fig. 7, the magnet 24 arranged on the upper side is the north pole, and the magnet 25 arranged on the lower side is the south pole, and a magnetic field is formed in a substantially vertical direction from the magnet 24 to the magnet 25. Therefore, when the support film 12 is transported between the magnets 24, 25, the conductive particles P in the adhesive paste W are magnetized, and a state is formed in which the conductive particles P, P are separated from each other in the in-plane direction of the adhesive paste W due to repulsive force (magnetic field application process).

[0116] In addition, in order to maintain the separated state of the conductive particles P in the magnetic field application process, the adhesive paste W is dried by hot air or the like while the support film 12 passes between the magnets 24 and 25 (drying process). This increases the viscosity of the adhesive paste W, and as shown in FIG. 8, the first adhesive layer 13 is formed on the support film 12 in which 70% or more, preferably 90% or more of the conductive particles P are separated from adjacent conductive particles P. In addition, the thickness of the adhesive paste W is reduced by the drying process, and as described above, by setting the thickness of the adhesive paste W to less than 1.6 times the average particle diameter of the conductive particles P, it becomes easy to set the thickness of the first adhesive layer 13 to 0.6 times or more and less than 1.0 times the average particle diameter of the conductive particles P. In addition, by using an adhesive paste (varnish) diluted with an organic solvent (e.g., methyl ethyl ketone, etc.), it is also possible to reduce the thickness of the adhesive layer to about 0.1 times the average particle diameter of the conductive particles P. The amount of organic solvent used for dilution is not particularly limited, but it is preferable to add 50 to 500 parts by mass per 100 parts by mass of the adhesive component.

[0117] The drying temperature of the adhesive paste W is preferably, for example, 20°C to 80°C. The conveying speed of the support film 12 is preferably, for example, 30mm / s to 160mm / s. The thickness of the adhesive paste W is preferably, for example, 5µm to 10µm when conductive particles P with an average particle size of 3µm are used. When the conveying speed of the support film 12 is 30mm / s or more, the adhesive paste W dries in a state in which the conductive particles P are sufficiently spaced apart, so that the dispersion tends to be sufficient. When the conveying speed of the support film 12 is 160mm / s or less, the application of the magnetic field tends to end after drying, so that re-aggregation of the conductive particles P can be suppressed. When the thickness of the adhesive paste W is 5µm or more, the gap of the coater 23 can be suppressed from being insufficient, and the number of the conductive particles P in the first adhesive layer 13 can be suppressed from being insufficient. When the thickness of the adhesive paste W is 10 μm or less, the gap of the coater 23 can be prevented from becoming excessive, and the number of conductive particles P in the first adhesive layer 13 can be prevented from becoming excessive.

[0118] After the first adhesive layer 13 is formed, as shown in Fig. 9, a second adhesive layer 14 formed separately on a release film 15 is laminated onto the first adhesive layer 13 (lamination process). This results in the adhesive film 11 for circuit connection shown in Fig. 2. For example, a hot roll laminator can be used for laminating the second adhesive layer 14. Also, without being limited to lamination, an adhesive paste that is the material for the second adhesive layer 14 may be applied onto the first adhesive layer 13 and dried.

[0119] As described above, in the adhesive film for circuit connection 11, 70% or more, preferably 90% or more of the conductive particles P can be separated from adjacent conductive particles P in the first adhesive layer 13. In this case, the aggregation of adjacent conductive particles P, P is suppressed when connecting the first circuit member 2 and the second circuit member 3, and the insulation between adjacent first circuit electrodes 6, 6 and between adjacent second circuit electrodes 8, 8 can be ensured. In addition, in this adhesive film for circuit connection 11, the thickness of the first adhesive layer 13 can be set to 0.1 times or more and 1.0 times or less, 0.1 times or more and 0.7 times or less, or 0.6 times or more and less than 1.0 times the average particle size of the conductive particles P. In this case, the flow of the conductive particles P during pressure bonding is suppressed, and the capture efficiency of the conductive particles P between the first circuit electrode 6 and the second circuit electrode 8 can be improved. Therefore, the connection reliability between the first circuit member 2 and the second circuit member 3 can be ensured.

[0120] <Adhesive film storage set> Fig. 10 is a perspective view showing an adhesive film storage set of one embodiment. As shown in Fig. 10, the adhesive film storage set 120 includes an adhesive film 11 for circuit connection, a reel 121 around which the adhesive film 11 is wound, and a storage member 122 for storing the adhesive film 11 and the reel 121.

[0121] As shown in Fig. 10, the adhesive film 11 is, for example, in the form of a tape. The tape-shaped adhesive film 11 is produced, for example, by cutting a sheet-shaped raw material into a long piece with a width according to the application. The adhesive film 11 may have a support film 12 on the first adhesive layer side. As the support film 12, a base material such as the above-mentioned PET film can be used.

[0122] The reel 121 includes a first side plate 124 having a winding core 123 around which the adhesive film 11 is wound, and a second side plate 125 arranged to face the first side plate 124 with the winding core 123 in between.

[0123] The first side plate 124 is, for example, a disk made of plastic, and has an opening with a circular cross section provided in the center portion of the first side plate 124 .

[0124] The winding core 123 of the first side plate 124 is a portion around which the adhesive film 11 is wound. The winding core 123 is made of, for example, plastic, and has a circular shape with a thickness similar to the width of the adhesive film 11. The winding core 123 is fixed to the inner surface of the first side plate 124 so as to surround the opening of the first side plate 124. In addition, a shaft hole 126 into which a rotating shaft of a winding device or a payout device (not shown) is inserted is provided in the center of the reel 121. When the rotating shaft of the winding device or the payout device is inserted into this shaft hole 126 and the rotating shaft is driven, the reel 121 rotates without spinning freely. A desiccant container containing a desiccant may be fitted into the shaft hole 126.

[0125] The second side plate 125, like the first side plate 124, is a circular plate made of, for example, plastic, and has an opening in the central portion of the second side plate 125 that is circular in cross section and has the same diameter as the opening of the first side plate 124.

[0126] The storage member 122 is, for example, bag-shaped, and stores the adhesive film 11 and the reel 121. The storage member 122 has an insertion opening 127 for storing (inserting) the adhesive film 11 and the reel 121 inside the storage member 122.

[0127] The storage member 122 has a visual confirmation portion 128 that allows the inside of the storage member 122 to be visually confirmed from the outside. The storage member 122 shown in FIG.

[0128] The visual confirmation section 128 is transparent to visible light. For example, when the light transmittance in the visual confirmation section 128 is measured in the wavelength range of 450 to 750 nm, there is at least one region with a wavelength width of 50 nm between 450 and 750 nm where the average light transmittance is 30% or more. The light transmittance of the visual confirmation section 28 is obtained by cutting the visual confirmation section 128 to a predetermined size to prepare a sample and measuring the light transmittance of the sample with an ultraviolet-visible spectrophotometer. Since the storage member 122 has such a visual confirmation section 128, various information such as the product name, lot number, and expiration date attached to, for example, the reel 121 inside the storage member 122 can be confirmed from the outside of the storage member 122. This is expected to prevent mixing of different products and improve the efficiency of the sorting work.

[0129] The transmittance of light having a wavelength of 365 nm in the visual observation portion 128 is 10% or less. Since the transmittance of light having a wavelength of 365 nm in the visual observation portion 128 is 10% or less, when a photopolymerization initiator is used as the component (B), it is possible to suppress the curing of the second curable composition caused by light entering from the outside to the inside of the storage member 122 and the photopolymerization initiator remaining in the first adhesive layer. From the viewpoint of further suppressing the generation of active species (e.g., radicals) from the photopolymerization initiator, the transmittance of light having a wavelength of 365 nm in the visual observation portion 128 is preferably 10% or less, more preferably 5% or less, even more preferably 1% or less, and particularly preferably 0.1% or less.

[0130] From the same viewpoint, the maximum transmittance of light in the wavelength region capable of generating radicals, cations or anions from the above-mentioned photopolymerization initiator (component (B)) in the visualizing portion 128 is preferably 10% or less, more preferably 5% or less, even more preferably 1% or less, and particularly preferably 0.1% or less. Specifically, the maximum transmittance of light in the wavelength range of 254 to 405 nm in the visualizing portion 128 is preferably 10% or less, more preferably 5% or less, even more preferably 1% or less, and particularly preferably 0.1% or less.

[0131] The visual confirmation section 128 (the storage member 122) is formed of a sheet having a thickness of, for example, 10 to 5000 μm. The sheet is made of a material that has a transmittance of 10% or less of light with a wavelength of 365 nm in the visual confirmation section 128. Such a material may be made of one type of component or may be made of multiple types of components. Examples of such materials include low-density polyethylene, linear low-density polyethylene, polycarbonate, polyester, acrylic resin, polyamide, glass, and the like. These materials may contain an ultraviolet absorbing agent. The visual confirmation section 128 may have a layered structure formed by laminating multiple layers having different light transmittances. In this case, each layer constituting the visual confirmation section 128 may be made of the above-mentioned material.

[0132] The insertion opening 127 may be sealed by being closed, for example, by a sealer, in order to prevent air from entering from the outside when the reel 121 is stored. In this case, it is preferable to remove the air from inside the storage member 122 by suction before closing the insertion opening 127. This is expected to reduce the humidity inside the storage member 122 from the initial stage of storage, and to prevent air from entering from the outside. In addition, by closely contacting the inner surface of the storage member 122 with the surface of the reel 121, which may cause foreign matter to be generated due to rubbing between the inner surface of the storage member 122 and the surface of the reel 121 caused by vibration during transportation, and to prevent damage to the outer surfaces of the side plates 124, 125 of the reel 121.

[0133] In the above embodiment, the housing member is configured so that the entire housing member is the visual confirmation portion, but in another embodiment, the housing member may have a visual confirmation portion in a part of the housing member. For example, the housing member may have a rectangular visual confirmation portion in approximately the center of a side surface of the housing member. In this case, the portion of the housing member other than the visual confirmation portion may be black so as not to transmit, for example, ultraviolet light and visible light.

[0134] In the above embodiment, the shape of the container is a bag, but the container may be, for example, a box. It is preferable that the container has a notch for opening. In this case, the container can be easily opened when in use. EXAMPLES

[0135] The present invention will be specifically described below based on examples, but the present invention is not limited to these.

[0136] <Method for preparing polyester urethane resin> In a stainless steel autoclave equipped with a stirrer, a thermometer, a condenser, a vacuum generator, and a nitrogen gas inlet tube, 48 parts by mass of isophthalic acid and 37 parts by mass of neopentyl glycol were added, and 0.02 parts by mass of tetrabutoxy titanate as a catalyst was added. The mixture was then heated to 220°C under a nitrogen stream and stirred for 8 hours. The mixture was then depressurized to atmospheric pressure (760mmHg) and cooled to room temperature, after which a white precipitate was taken out, washed with water, and vacuum dried to obtain a polyester polyol.

[0137] The polyester polyol obtained by the reaction of the dicarboxylic acid and the diol described above was thoroughly dried, dissolved in MEK, and charged into a four-neck flask equipped with a stirrer, a dropping funnel, a reflux condenser, and a nitrogen gas inlet tube. In addition, dibutyltin laurate was charged as a catalyst in an amount of 0.05 parts by mass relative to 100 parts by mass of the polyester polyol, and 4,4'-diphenylmethane diisocyanate dissolved in MEK was charged in an amount of 50 parts by mass relative to 100 parts by mass of the polyester polyol using a dropping funnel, and the mixture was stirred at 80°C for 4 hours to obtain the desired polyester urethane resin.

[0138] <Synthesis of polyurethane acrylate (UA1)> Into a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser having a calcium chloride drying tube, and a nitrogen gas inlet tube, 2500 parts by mass (2.50 mol) of poly(1,6-hexanediol carbonate) (trade name: Duranol T5652, manufactured by Asahi Kasei Chemicals Corporation, number average molecular weight 1000) and 666 parts by mass (3.00 mol) of isophorone diisocyanate (manufactured by Sigma-Aldrich Co.) were uniformly dropped over 3 hours. Next, after sufficient nitrogen gas was introduced into the reaction vessel, the inside of the reaction vessel was heated to 70 to 75°C to cause a reaction. Next, 0.53 parts by mass (4.3 mmol) of hydroquinone monomethyl ether (Sigma-Aldrich) and 5.53 parts by mass (8.8 mmol) of dibutyltin dilaurate (Sigma-Aldrich) were added to the reaction vessel, and then 238 parts by mass (2.05 mol) of 2-hydroxyethyl acrylate (Sigma-Aldrich) were added and reacted at 70°C for 6 hours under air atmosphere. This resulted in polyurethane acrylate (UA1). The weight-average molecular weight of polyurethane acrylate (UA1) was 15,000. The weight-average molecular weight was measured by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene under the following conditions. (Measurement conditions) Equipment: Tosoh Corporation GPC-8020 Detector: Tosoh RI-8020 Column: Gelpack GLA160S+GLA150S manufactured by Hitachi Chemical Co., Ltd. Sample concentration: 120mg / 3mL Solvent: Tetrahydrofuran Injection volume: 60μL Pressure: 2.94×10 6 Pa(30kgf / cm 2 ) Flow rate: 1.00mL / min

[0139] <Preparation of conductive particles> A layer of nickel was formed on the surface of the polystyrene particles to a thickness of 0.2 μm, thus obtaining conductive particles with an average particle size of 4 μm, a maximum particle size of 4.5 μm, and a specific gravity of 2.5.

[0140] <Preparation of Varnish (Varnish Composition) for Conductive Particle-Containing Layer> The components shown below were mixed in the amounts (parts by mass) shown in Table 1 to prepare a varnish of photocurable composition 1. The conductive particle content (volume %) and filler content (volume %) shown in Table 1 are based on the total volume of the photocurable composition. (polymerizable compound) A1: Dicyclopentadiene diacrylate (product name: DCP-A, manufactured by Toagosei Co., Ltd.) A2: Polyurethane acrylate (UA1) synthesized as described above A3: 2-Methacryloyloxyethyl acid phosphate (product name: Light Ester P-2M, manufactured by Kyoeisha Chemical Co., Ltd.) (Photopolymerization initiator) B1: B1: 1,2-Octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)] (trade name: Irgacure® OXE01, manufactured by BASF) (Thermal polymerization initiator) C1: Benzoyl peroxide (product name: Niper BMT-K40, manufactured by NOF Corporation) (Conductive particles) D1: Conductive particles prepared as described above (thermoplastic resin) E1: Polyester urethane resin synthesized above (Coupling Agent) F1: 3-methacryloxypropyltrimethoxysilane (product name: KBM503, manufactured by Shin-Etsu Chemical Co., Ltd.) (filling material) G1: Silica fine particles (product name: R104, manufactured by Nippon Aerosil Co., Ltd., average particle size (primary particle size): 12 nm) (solvent) H1: Methyl ethyl ketone

[0141] [Table 1]

[0142] <Preparation of Thermosetting Composition Varnish (Varnish Composition)> The polymerizable compounds a1 to a3, thermoplastic resin e1, coupling agent f1, filler g1, and solvent h1 were the same as the polymerizable compounds A1 to A3, thermoplastic resin E1, coupling agent F1, filler G1, and solvent H1 in the photocurable composition, and these components and the thermal polymerization initiator shown below were mixed in the amounts (parts by mass) shown in Table 2 to prepare a varnish of a thermosetting composition 1. The content (volume %) of the filler shown in Table 2 is based on the total volume of the thermosetting composition. (Thermal polymerization initiator) c1: Benzoyl peroxide (product name: Niper BMT-K40, manufactured by NOF Corporation)

[0143] [Table 2]

[0144] Example 1 [Preparation of the first adhesive film] The varnish of the photocurable composition 1 was applied onto a PET film having a thickness of 50 μm using a coating device. Next, hot air drying was performed at 70° C. for 3 minutes, and a magnetic field was simultaneously applied to form a layer of the photocurable composition 1 having a thickness (thickness after drying) of 4 μm on the PET film. The thickness was measured using a contact thickness meter. Note that the size of the conductive particles is reflected when using a contact thickness meter, and the thickness of the region where the conductive particles are present is measured. Therefore, after laminating the second adhesive layer to prepare a two-layer circuit connection adhesive film, the thickness of the first adhesive layer located in the space between adjacent conductive particles was measured by the method described below. Next, a metal halide lamp was used to apply a cumulative light dose of 1500 mJ / cm 2 to the layer made of the photocurable composition 1. 2 The polymerizable compound was polymerized by irradiating the film with light so that the photocurable composition 1 was cured to form a first adhesive layer. The above operations resulted in a first adhesive film having a first adhesive layer with a thickness of 4 μm (the thickness of the region where the conductive particles are present) on the PET film. The conductive particle density at this time was about 7000 pcs / mm2 It was.

[0145] [Evaluation of monodispersity of conductive particles] The monodispersity of the conductive particles (the ratio of conductive particles present in a state where they are separated from adjacent conductive particles (monodispersed state)) of the first adhesive film was evaluated, and the monodispersity was 70% or more. The monodispersity ratio is expressed as follows: Monodispersity ratio (%) = (2500 μm 2 Number of monodispersed conductive particles in / 2500μm 2 The number of conductive particles was calculated by multiplying the number of conductive particles by 100. The number of conductive particles was measured by observing with a metal microscope at a magnification of 200 times.

[0146] [Preparation of the second adhesive film] The varnish of the thermosetting composition 1 was applied onto a PET film having a thickness of 50 μm using a coating device. Then, hot air drying was performed at 70° C. for 3 minutes to form a second adhesive layer (a layer made of the thermosetting composition 1) having a thickness of 8 μm on the PET film. Through the above operations, a second adhesive film having a second adhesive layer on the PET film was obtained.

[0147] [Preparation of adhesive film for circuit connection] The first adhesive film and the second adhesive film were laminated together with the PET film substrate at 40°C using a roll laminator. At this time, the PET film on the second adhesive film side was peeled off. This produced an adhesive film for circuit connection having a laminated structure in which the PET film, the first adhesive layer, and the second adhesive layer were laminated in this order. The thickness of the first adhesive layer of the prepared circuit connection adhesive film was measured by the above-mentioned method. Specifically, it was measured by the following method. The circuit connection adhesive film was sandwiched between two pieces of glass (thickness: about 1 mm), and a resin composition consisting of 100 g of bisphenol A type epoxy resin (product name: JER811, manufactured by Mitsubishi Chemical Corporation) and 10 g of a hardener (product name: Epomount hardener, manufactured by Refine Tech Co., Ltd.) was poured into the mold, and the cross section was polished using a polishing machine, and the thickness of the first adhesive layer located in the space between adjacent conductive particles was measured using a scanning electron microscope (SEM, product name: SE-8020, manufactured by Hitachi High-Tech Science Corporation). The thickness of the first adhesive layer was 2 μm.

[0148] [Fabrication of circuit connection structure] A 25μm pitch COF (manufactured by FLEXSEED) and a glass substrate (manufactured by Geomatec) with a thin-film electrode (height: 1200Å) made of amorphous indium tin oxide (ITO) on a glass substrate were connected over a width of 1mm using a thermocompression bonding device (heating method: constant heat type, manufactured by Taiyo Kikai Seisakusho Co., Ltd.) at 170°C and 6MPa for 4 seconds to produce a circuit connection structure (connection structure). Note that, when connecting, the circuit connection adhesive film was first attached to the COF substrate from the second adhesive layer side, and after peeling off the separator, it was placed opposite the glass substrate and heated and pressed.

[0149] [Evaluation of circuit connection structures] The connection resistance between the opposing electrodes of the resulting circuit connection structure immediately after connection was measured with a multimeter, and was calculated as the average value of resistance between the opposing electrodes at 16 points. Next, 10 μm × 200 μm (= 2000 μm) on each electrode 2 The number of captures in the area was counted and the average value of 20 lines was calculated. The results are shown in Table 3. The particle dispersion after mounting was also observed under a microscope and was rated as 1 if the state before mounting was maintained, 3 if it was not maintained at all, and 2 as intermediate. Levels 1 and 2 are at levels that pose no practical problems.

[0150] (Reference example 1) Evaluation was performed in the same manner as in Example 1, except that an adhesive film for circuit connection having a laminated structure in which the first adhesive layer, the second adhesive layer, and the PET film were laminated in this order by peeling off the PET film on the first adhesive layer side after laminating the first adhesive layer and the second adhesive layer was produced. Note that, when connecting, the adhesive film for circuit connection was first attached to the COF substrate from the first adhesive layer side, and after peeling off the separator, it was placed opposite the glass substrate and heated and pressed. The results are shown in Table 3.

[0151] (Examples 2 and 3) Except for changing the thickness of the first adhesive layer to 1.5 μm and 3.0 μm, adhesive films for circuit connection and circuit connection structures were produced in the same manner as in Example 1. The produced circuit connection structures were evaluated in the same manner as in Example 1. The results are shown in Table 3. The monodispersity rates of the conductive particles in the first adhesive layer were each 70% or more.

[0152] [Table 3]

[0153] It was found that when the adhesive film for circuit connection obtained in Example 1 was first attached to a COF substrate and then mounted, the number of captured conductive particles was greater than in Reference Example 1, and the fluidity of the particles was also suppressed. [Explanation of symbols]

[0154] 1...circuit connection structure, 2...first circuit member, 3...second circuit member, 6...first circuit electrode, 8...second circuit electrode, 11...adhesive film for circuit connection, 12, 15...support film (peel film), 13...first adhesive layer, 14...second adhesive layer, P...conductive particles, W...adhesive paste.

Claims

1. The adhesive tape comprises a peelable support film, a first adhesive layer containing conductive particles provided on the support film, and a second adhesive layer laminated on the first adhesive layer; An adhesive film for circuit connection, wherein the thickness of the first adhesive layer is 0.1 to 1.0 times the average particle size of the conductive particles.

2. the first adhesive layer is made of a cured product of a first curable composition, 2. The adhesive film for circuit connection according to claim 1, wherein the first curable composition contains a radically polymerizable compound having a radically polymerizable group.

3. the second adhesive layer comprises a second curable composition; 3. The adhesive film for circuit connection according to claim 1, wherein the second curable composition contains a radically polymerizable compound having a radically polymerizable group.

4. A method for producing a circuit connection structure, comprising the steps of: interposing the first adhesive layer and the second adhesive layer of the adhesive film for circuit connection according to any one of claims 1 to 3 between a first circuit member having a first electrode and a second circuit member having a second electrode; and thermocompression bonding the first circuit member and the second circuit member to electrically connect the first electrode and the second electrode to each other.

5. the first circuit member having a flexible substrate; 5. The method for producing a circuit connection structure according to claim 4, further comprising a step of attaching the circuit connection adhesive film to the first circuit member so that the second adhesive layer is in contact with the first circuit member.

6. An adhesive film for circuit connection according to any one of claims 1 to 3, and a housing member for housing the adhesive film, the storage member has a visual confirmation portion that allows the inside of the storage member to be visually confirmed from the outside, The adhesive film storage set has a transmittance of 10% or less for light having a wavelength of 365 nm in the visible portion.

Citation Information

Patent Citations

  • Packaging material and packaging container for medicine for promoting nutrition using it

    JP2007290269A

  • Anisotropic conductive film, connection method, and connection structure

    JP2011192651A

  • Reel member and film winding method

    JP2003034468A