Method for producing fire extinguishing material, method for producing fire extinguishing material package, and composition for forming fire extinguishing agent layer
A fire extinguishing material with a film-forming agent on potassium citrate and a protective packaging system addresses the deliquescence issue, achieving stable and effective fire suppression.
Patent Information
- Application Number
- JP2024069160
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-29
AI Technical Summary
Potassium citrate, used as a fire extinguishing agent, has deliquescent properties that cause it to absorb moisture from the environment, leading to instability in fire extinguishing materials.
A fire extinguishing material is developed with a film-forming agent on the surface of potassium citrate to form a protective film, combined with a base material and packaging to maintain stability, using compounds with acid anhydride or isocyanate groups to enhance hydrophobicity and suppress deliquescence.
The solution provides a fire extinguishing material with improved stability, maintaining moisture content below 5% and water vapor permeability within specified limits, ensuring effective fire extinguishing performance.
Smart Images

Figure 2024153610000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to fire extinguishing materials and fire extinguishing material packages. [Background technology]
[0002] Self-extinguishing molded articles using fire extinguishing compositions containing components that generate aerosols when burned are known (for example, Patent Document 1). Potassium salts are examples of such components, and potassium citrate is particularly preferably used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 047762 Summary of the Invention [Problem to be solved by the invention]
[0004] However, potassium citrate is deliquescent and therefore tends to absorb moisture from the surrounding environment over time. If such deliquescence can be suppressed when potassium citrate is used as a fire extinguishing agent component, the property stability of the fire extinguishing material can be further improved.
[0005] The present invention has been made in view of the above circumstances, and aims to provide a fire extinguishing material containing potassium citrate as an extinguishing agent component and having excellent property stability. Another aim of the present invention is to provide a fire extinguishing material package in which the fire extinguishing material is enclosed. [Means for solving the problem]
[0006] One aspect of the present invention includes, for example, the following embodiment. [1] A fire extinguishing agent layer containing a fire extinguishing agent including granular potassium citrate; A fire extinguishing material, wherein the potassium citrate has a coating on its surface formed from a coating forming agent. [2] The fire extinguishing material according to [1], wherein the film-forming agent contains a compound having an acid anhydride group or an isocyanate group. [3] The fire extinguishing material according to [1] or [2], further comprising potassium chlorate. [4] The fire extinguishing material according to any one of [1] to [3], wherein the potassium citrate has an average particle size D50 of 1 to 100 μm. [5] The fire extinguishing material according to any one of [1] to [4], wherein the extinguishing agent layer contains the extinguishing agent in an amount of 70 to 97% by mass. [6] The fire extinguishing material according to any one of [1] to [5], further comprising a substrate on which the fire extinguishing agent layer is disposed. [7] The fire extinguishing material according to any one of [1] to [6], wherein the water content of the fire extinguishing agent layer after the following storage test is 5 mass% or less. (Storage test) Water vapor permeability (JIS K 7129 compliant, 40℃ / 90%RH) is 0.2~0.6g / m 2 The fire extinguishing material package obtained by sealing the fire extinguishing material in a packaging material formed from a packaging film having a temperature of 100 °C / day is stored stationary for 12 hours in an environment of 85 °C / 85% RH. [8] A fire extinguishing material package comprising a packaging material and the fire extinguishing material according to any one of [1] to [7] enclosed in the packaging material. Effect of the Invention
[0007] According to the present invention, it is possible to provide a fire extinguishing material containing potassium citrate as a fire extinguishing agent component and having excellent property stability. Also, according to the present invention, it is possible to provide a fire extinguishing material package in which the fire extinguishing material is enclosed. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view of a fire extinguishing material according to one embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a fire-extinguishing material package according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Preferred embodiments of the present disclosure will be described in detail below, however, the present disclosure is not limited to the following embodiments.
[0010] <Fire extinguishing material> 1 is a schematic cross-sectional view of a fire extinguishing material according to one embodiment. The fire extinguishing material 10 includes a fire extinguishing agent layer 1 and a substrate 2 on which the fire extinguishing agent layer 1 is disposed. It can be said that the fire extinguishing material 10 includes the substrate 2 and the fire extinguishing agent layer 1 disposed on the substrate 2. The fire extinguishing material 10 may be a sheet-shaped fire extinguishing material. The fire extinguishing material 10 does not need to include the substrate 2, and in that case, may be the fire extinguishing agent layer 1 itself.
[0011] From the viewpoint of placing the fire extinguishing material at a desired position, the fire extinguishing material may further include an adhesive layer or a pressure-sensitive adhesive layer. The adhesive layer or the pressure-sensitive adhesive layer may be provided on the fire extinguishing agent layer 1 side or on the substrate 2 side.
[0012] (Fire extinguishing agent layer) The extinguishing agent layer contains a particulate extinguishing agent. The extinguishing agent contains an aerosol generating agent, and aerosol generated by the aerosol generating agent is generated from the extinguishing agent layer, thereby enabling extinguishing of a fire.
[0013] The fire extinguishing agent contains particulate potassium citrate as an aerosol generating agent. The potassium citrate referred to here is monopotassium citrate, dipotassium citrate, tripotassium citrate, or hydrates thereof. Potassium citrate has excellent ability to generate potassium radicals that have a negative catalytic effect on combustion. The extinguishing agent may contain other aerosol generating agents, such as organic salts such as organic potassium salts (excluding potassium citrate), organic sodium salts, organic ammonium salts, etc. From the viewpoint of usefulness in terms of the negative catalytic effect, organic potassium salts are preferred, and examples of organic potassium salts other than potassium citrate include potassium carboxylates such as potassium acetate, potassium tartrate, potassium lactate, potassium oxalate, and potassium maleate.
[0014] From the viewpoint of easily obtaining an excellent negative catalytic effect, the amount of potassium citrate contained in the aerosol generating agent can be 80 mass % or more based on the total amount of the aerosol generating agent, and may be 100 mass %.
[0015] The fire extinguishing agent may contain an oxidizer as a component other than the aerosol generating agent. The oxidizer acts on the aerosol generating agent to promote the generation of aerosol.
[0016] The extinguishing agent may contain potassium chlorate (particulate) as an oxidizer, which is effective in generating aerosols from aerosol generating agents. The extinguishing agent may contain other oxidizers, such as sodium chlorate, strontium chlorate, ammonium chlorate, magnesium chlorate, potassium nitrate, sodium nitrate, strontium nitrate, ammonium perchlorate, potassium perchlorate, basic copper nitrate, copper (I) oxide, copper (II) oxide, iron (II) oxide, iron (III) oxide, molybdenum trioxide, and the like.
[0017] From the viewpoint of easily obtaining an excellent aerosol generating effect, the amount of potassium chlorate contained in the oxidizing agent can be 80 mass % or more based on the total amount of the oxidizing agent, and may be 100 mass %.
[0018] The fire extinguishing agent may contain other agents (components) in addition to the aerosol generating agent and the oxidizing agent, such as colorants, antioxidants, flame retardants, inorganic fillers, flow agents, moisture-proofing agents, dispersants, UV absorbers, softening agents, catalysts, etc.
[0019] The amount of the aerosol generating agent and the oxidizing agent (potassium citrate and potassium chlorate, if necessary) contained in the extinguishing agent can be 60% by mass or more, based on the total amount of the extinguishing agent, from the viewpoint of easily exhibiting excellent fire extinguishing performance, and may be 90% by mass or more, or may be 100% by mass.
[0020] The amount of the oxidizing agent (potassium chlorate in some cases) contained in the fire extinguishing agent can be 5 to 1200 parts by mass per 100 parts by mass of the total amount of the aerosol generating agent (potassium citrate in some cases), from the viewpoint of easily exhibiting excellent fire extinguishing performance.
[0021] The average particle diameter D50 of potassium citrate may be 1 to 100 μm, or may be 3 to 40 μm. When the average particle diameter D50 is equal to or greater than the above lower limit, the potassium citrate is easily dispersed in the system, and when the average particle diameter D50 is equal to or less than the above upper limit, the stability of the composition when prepared for coating tends to be improved, and the smoothness of the coated surface tends to be improved.
[0022] The average particle size D50 can be measured wet using a laser diffraction particle size distribution analyzer. The average particle size D50 can be adjusted by grinding potassium citrate in a mortar or the like.
[0023] The amount of the extinguishing agent can be 70 to 97% by mass, or may be 85 to 92% by mass, based on the total amount of the extinguishing agent layer. When the amount of the extinguishing agent is equal to or less than the upper limit, it is easy to suppress deliquescence of the salt and to form a homogeneous extinguishing material, and when the amount of the extinguishing agent is equal to or more than the lower limit, it is easy to exhibit the extinguishing performance of the extinguishing material.
[0024] The potassium citrate contained in the fire extinguishing agent has a coating formed from a film-forming agent on its surface. It can also be said that potassium citrate is surface-treated with a film-forming agent. When water molecules in the air adhere to potassium citrate, hydroxyl groups (-OH) are formed on its surface, and it is thought that these hydroxyl groups react (condense, add) with reactive groups of the film-forming agent to form a coating formed from the film-forming agent on the potassium citrate surface. For this reason, it can also be said that the film-forming agent is a coating agent that adsorbs to the surface of the fire extinguishing agent (potassium citrate) through chemical bonding. The coating may be an organosilane film or a resin film, and is preferably a hydrophobic coating. In this way, a material that is chemically attracted to the potassium citrate surface and adsorbs to the surface to form a coating is called a coating agent, and is different from materials such as binders that merely surround and physically hold the potassium citrate in place.
[0025] The film-forming agent may at least include those having reactive groups that react with the hydroxyl groups on the surface of potassium citrate as described above. The film-forming agent may be a silane coupling agent having a reactive group such as an acid anhydride group or an isocyanate group and a hydrolyzable group such as an alkoxysilyl group. It is considered that the silane coupling agent is bonded to the potassium citrate surface via the reactive group, and the hydrolysis condensation of the hydrolyzable group proceeds to form a film (organosilane film) on the potassium citrate surface. Examples of such silane coupling agents include X-12-1287A and X-12-967C manufactured by Shin-Etsu Chemical Co., Ltd.
[0026] The film-forming agent may also include a resin having a reactive group such as an acid anhydride group or an isocyanate group, and a reactive group such as a hydroxyl group, or a resin composition containing a compound having these groups separately. Such a resin may include rosin, and the resin composition may include a composition containing polyisocyanate and polyol (acrylic polyol, polyether polyol, polyester polyol, etc.). It is considered that a film (resin film) is formed on the potassium citrate surface by these resins or resin compositions. Such a resin may include Marquid No. 33 manufactured by Arakawa Chemical Industries Co., Ltd., and the resin composition may include Takenate D110N manufactured by Mitsui Chemicals, Inc. and 6AN-5000 manufactured by Taisei Fine Chemical Co., Ltd.
[0027] The film-forming agent preferably has an alkyl chain from the viewpoint of improving the hydrophobicity of the film. From the same viewpoint, the film-forming agent may have an alkene skeleton (e.g., a butadiene skeleton) or a cyclic alkane structure.
[0028] The coating may be formed (continuously) over the entire surface of the potassium citrate, or may be formed partially. The degree of coating can be adjusted in consideration of the balance between the deliquescence suppression property and reactivity of potassium citrate.
[0029] The coating on the potassium citrate surface can be observed, for example, by performing elemental analysis of the fire extinguishing agent surface (potassium citrate surface) by energy dispersive X-ray spectroscopy (EDS) using a scanning electron microscope JSM-7001F (manufactured by JEOL Ltd.). The presence or absence of a coating on the potassium citrate surface can be easily determined, for example, by adding the extinguishing agent to pure water (for example, 5% by weight). For example, if a hydrophobic coating is not formed, potassium citrate dissolves and potassium chlorate remains undissolved. On the other hand, if a hydrophobic coating is formed, the dissolution of potassium citrate, which is easily soluble in pure water, is inhibited and it forms aggregates in the water, so that the presence of the coating can be determined. Also, if a hydrophilic coating is formed, potassium chlorate, which is not soluble in pure water, dissolves, so that the presence of the coating can be determined.
[0030] The fire extinguishing agent layer may include a binder. The binder includes at least one of a thermoplastic resin and a thermosetting resin. Examples of thermoplastic resins include polyolefin resins such as polypropylene resins, polyethylene resins, poly(1-)butene resins, and polypentene resins, polystyrene resins, acrylonitrile-butadiene-styrene resins, methyl methacrylate-butadiene-styrene resins, ethylene-vinyl acetate resins, ethylene-propylene resins, polycarbonate resins, polyphenylene ether resins, acrylic resins, polyamide resins, polyvinyl chloride resins, polyvinyl alcohol (PVA), and polyvinyl acetal resins. Examples of thermosetting resins include rubbers such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), 1,2-polybutadiene rubber (1,2-BR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), nitrile rubber (NBR), butyl rubber (IIR), ethylene-propylene rubber (EPR, EPDM), chlorosulfonated polyethylene (CSM), acrylic rubber (ACM, ANM), epichlorohydrin rubber (CO, ECO), multi-vulcanized rubber (T), silicone rubber (Q), fluororubber (FKM, FZ), and urethane rubber (U); polyurethane resins (e.g., ether-based polyurethane resins), polyisocyanate resins, polyisocyanurate resins, phenolic resins, epoxy resins, and polyvinyl ether (PMVE)-maleic anhydride resins.
[0031] Among the above resins, polyvinyl acetal resins or polyurethane resins can be preferably used from the viewpoint of film forming properties. Examples of polyvinyl acetal resins include polyvinyl butyral (PVB).
[0032] The binder may contain other agents (components) other than the above resins (thermoplastic resins and thermosetting resins). Examples of other agents include curing agents, and from the viewpoint of property stability, surfactants, silane coupling agents, antiblocking agents, etc. These other components can be appropriately selected depending on the type of resin.
[0033] From the viewpoint of forming a fire-extinguishing agent layer, the amount of the resin contained in the binder can be 60% by mass or more, 90% by mass or more, or may be 100% by mass based on the total amount of the binder.
[0034] The amount of the binder can be 2 to 30 parts by mass, or may be 4 to 15 parts by mass, relative to 100 parts by mass of the extinguishing agent. When the amount of the binder is equal to or less than the upper limit, the extinguishing material is likely to exhibit its fire-extinguishing performance, and when the amount of the binder is equal to or more than the lower limit, a homogeneous extinguishing material is likely to be formed.
[0035] The thickness of the extinguishing agent layer can be 80 to 600 μm, or may be 150 to 300 μm. When the thickness is equal to or more than the lower limit, the extinguishing performance is easily exhibited, and when the thickness is equal to or less than the upper limit, bending resistance is easily obtained.
[0036] The area of the main surface of the extinguishing agent layer is not particularly limited since it is adjusted according to the application, but is set to be sufficiently large compared to the area of the side surface. The area of the main surface is, for example, 10 to 624 cm. 2 It can be said that:
[0037] (base material) Considering that the temperature of a flame is generally about 700 to 900°C, a resin substrate can be selected as the substrate. For example, the substrate material may be polyolefin (LLDPE, PP, COP, CPP, etc.), polyester (PET, etc.), fluororesin (PTFE, ETFE, EFEP, PFA, FEP, PCTFE, etc.), PVC, PVA, acrylic resin, epoxy resin, polyamide, polyimide, etc. Even if the fire extinguishing material is installed so that the substrate side faces the flame, these resins melt due to the heat of the flame (generally about 700 to 900°C), and the fire extinguishing agent layer is easily exposed. In addition, by selecting these transparent materials, it becomes easier to inspect the appearance of the fire extinguishing agent layer and to check the replacement time of the fire extinguishing agent layer. The substrate may contain the above fire extinguishing agent.
[0038] From the viewpoint of adjusting the water vapor permeability, the substrate may be provided with a vapor deposition layer (alumina vapor deposition layer or silica vapor deposition layer) having water vapor barrier properties. The vapor deposition layer may be provided on one side or both sides of the substrate.
[0039] The thickness of the substrate can be adjusted appropriately depending on the expected amount of heat at the time of fire outbreak, impact, allowable installation space, etc. For example, a thick substrate can easily obtain the strength and rigidity required for a fire extinguishing material, and can be easily handled. A thin substrate can be provided in a narrow space, and can improve initial fire extinguishing properties because it melts in a short time when heated by a flame. The thickness of the substrate can be, for example, 4.5 to 100 μm, and may be 12 to 50 μm. The substrate may be a laminate having a plurality of layers.
[0040] <Fire extinguishing material manufacturing method> The fire extinguishing material can be formed using a composition (coating liquid) for forming a fire extinguishing agent layer. A method for producing the fire extinguishing material is exemplified below.
[0041] A first method for producing the fire extinguishing material includes the steps of: A step of preparing a composition for forming a fire extinguishing agent layer by mixing a fire extinguishing agent, a film forming agent, and a binder with a liquid medium; and applying the composition for forming a fire-extinguishing agent layer onto the substrate and drying the composition to form a fire-extinguishing agent layer.
[0042] A second method for producing the fire extinguishing material includes the steps of: treating the fire extinguishing agent with a film-forming agent; A step of mixing the extinguishing agent treated with the film-forming agent and the binder with a liquid medium to prepare a composition for forming a fire extinguishing agent layer; and applying the composition for forming a fire-extinguishing agent layer onto the substrate and drying the composition to form a fire-extinguishing agent layer.
[0043] A third method for producing the fire extinguishing material comprises the steps of: treating potassium citrate with a film-forming agent; A step of preparing a composition for forming a fire extinguishing agent layer by mixing a fire extinguishing agent containing potassium citrate treated with a film-forming agent and a binder with a liquid medium; and applying the composition for forming a fire-extinguishing agent layer onto the substrate and drying the composition to form a fire-extinguishing agent layer.
[0044] The liquid medium may be an organic solvent. The organic solvent may be a water-soluble solvent, for example, alcohols such as methanol, ethanol, isopropyl alcohol, n-propyl alcohol, etc.; ketones such as acetone, methyl ethyl ketone, etc.; glycols such as ethylene glycol, diethylene glycol, etc.; glycol ethers such as N-methylpyrrolidone (NMP), tetrahydrofuran, butyl cellosolve, etc. In view of the deliquescent nature of potassium citrate, the liquid medium may be an alcohol-based solvent, specifically, ethanol, isopropyl alcohol, or a mixture thereof.
[0045] The amount of the extinguishing agent and the binder may be adjusted so that the amount of each of them in the extinguishing agent layer is the desired amount. The amount of the liquid medium may be appropriately adjusted according to the method of using the composition for forming an extinguishing agent layer, and may be 30 to 70 mass% based on the total amount of the composition for forming an extinguishing agent layer. The composition for forming an extinguishing agent layer containing the liquid medium may be called a coating liquid for forming an extinguishing agent layer.
[0046] A method of treating an object with a film-forming agent includes mixing the object with the film-forming agent. The amount of the film-forming agent may be adjusted so that a desired film is formed on the potassium citrate surface. From the viewpoint of easily suppressing deliquescence of potassium citrate, the amount of the film-forming agent is preferably 1 part by mass or more, more preferably 5 parts by mass or more, per 100 parts by mass of potassium citrate. In addition, from the viewpoint of difficult suppression of aerosol generation from potassium citrate, the amount of the film-forming agent is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, per 100 parts by mass of potassium citrate.
[0047] The fire extinguishing agent or each component contained in the fire extinguishing agent may be pulverized in a mortar or the like to a desired particle size before being subjected to each of the above steps.
[0048] The composition for forming a fire-extinguishing agent layer can be applied by a wet coating method, such as gravure coating, comma coating, dip coating, curtain coating, spin coating, sponge roll coating, and die coating.
[0049] The drying temperature for the coating film obtained by coating is not particularly limited, but can be, for example, 60 to 100°C.
[0050] The extinguishing agent layer alone of the extinguishing material obtained as described above may be peeled off from the substrate and used as the extinguishing material. In this case, it is preferable that the substrate has been subjected to a release treatment.
[0051] In addition to the method of producing a fire extinguishing material using a composition (coating liquid) for forming a fire extinguishing agent layer as described above, a fire extinguishing material can also be produced, for example, by filling a fire extinguishing agent into a packaging bag for the fire extinguishing agent to form a fire extinguishing agent layer, and then attaching this to a substrate with an adhesive or pressure sensitive adhesive. Alternatively, the extinguishing agent layer itself, in which the extinguishing agent is filled in a packaging bag for the extinguishing agent, can be used as the extinguishing material.
[0052] The fire extinguishing agent packaging bag can be formed, for example, by heat sealing (thermal fusing) the four sides of two resin films. Examples of resins constituting the resin films include polyolefins (LLDPE, PP, COP, CPP, etc.), polyesters (PET, etc.), fluororesins (PTFE, ETFE, EFEP, PFA, FEP, PCTFE, etc.), PVC, PVA, acrylic resins, epoxy resins, polyamides, polyimides, etc. These resins melt due to the heat of a flame (generally about 700 to 900°C), and the fire extinguishing agent inside can be easily exposed.
[0053] <Fire extinguishing material package> 2 is a schematic cross-sectional view of a fire extinguishing material package according to one embodiment. The fire extinguishing material package 100 comprises a packaging material 3 and a fire extinguishing material 10 enclosed in the packaging material 3. In the figure, the fire extinguishing material 10 comprises a fire extinguishing agent layer 1 and a substrate 2, but the fire extinguishing material 10 may be the fire extinguishing agent layer 1 itself without using the substrate 2. The packaging material 3 may be in the form of a bag, ie, it may be called a packaging bag.
[0054] (packaging material) The packaging material is made of a packaging film having a resin base material such as polyolefin resin, polyester resin, fluororesin, vinyl resin, acrylic resin, epoxy resin, polyamide, polyimide, urethane resin, styrene-based resin, polycarbonate, ketone resin, sulfone-based resin, or cellulose-based resin, or a metal base material such as aluminum foil.
[0055] In addition to the above-mentioned base material, the packaging film may have a heat-sealable sealant layer. The sealant layer is not particularly limited, and examples thereof include a CPP (non-oriented polypropylene) film and an L-LDPE (linear low-density polyethylene) film.
[0056] The packaging film desirably has water vapor barrier properties and may be a so-called barrier film (water vapor barrier film). The water vapor permeability of the packaging film (based on JIS K 7129, under conditions of 40°C / 90% RH) is 10 g / m 2 / day or less, and 2 / day or less, and 2 / day or less. The lower limit of the water vapor transmission rate is not particularly limited, but is, for example, 0.2 g / m 2 / day. From the viewpoint of adjusting the water vapor permeability, the packaging material film may be one having a resin substrate (for example, a polyester resin layer such as a PET layer) having a metal oxide vapor deposition layer such as an alumina vapor deposition layer or a silica vapor deposition layer. When the resin substrate has a metal oxide vapor deposition layer, the metal oxide vapor deposition layer may face the fire extinguishing material side.
[0057] The packaging material is made by making a packaging film into a bag. A sealing portion is provided at the peripheral portion of the packaging material where the packaging films face each other. In the sealing portion, for example, the packaging films may be joined together by a joining material such as a heat seal material, adhesive, or pressure sensitive adhesive, or, in the case where the packaging film itself has heat sealability (thermal fusion property) such as when the packaging film has a sealant layer, the packaging films may be joined together by heat sealing. Such a sealing portion prevents the fire extinguishing material from coming into contact with air, and deterioration of the fire extinguishing agent contained in the fire extinguishing material can be suppressed.
[0058] The fire extinguishing material package may be prepared by enclosing the fire extinguishing material in a packaging material prepared in advance, or by laminating the packaging material film and the fire extinguishing material and then sealing the edges of the packaging material film (or by thermally laminating the entire surface).
[0059] The adhesive strength between the packaging films at the sealed portion may be 5 N / 15 mm or more, and from the viewpoint of stably sealing the fire extinguishing agent, may be 7 N / 15 mm or more, or 10 N / 15 mm or more. The adhesive strength can be varied by adjusting the base material, the bonding material such as an adhesive, the heat sealing conditions (heat sealing temperature, pressure, time), etc. The adhesion strength between packaging films is measured as follows. That is, a sample is prepared in which packaging films are bonded together by heat fusion or with a bonding material. The heat fusion or bonding part of this sample is cut to a width of 15 mm, and a T-shaped peel is performed at a peel speed of 300 mm / min using a tensile tester placed in a room temperature environment of 23°C in accordance with JIS K6854-3. The average strength from the start of peeling to the separation of the heat fusion or bonding part is taken as the adhesion strength between the packaging films.
[0060] The above-mentioned fire extinguishing material has excellent property stability, so that, for example, the moisture content of the fire extinguishing agent layer after the following storage test using a fire extinguishing material package can be 5 mass % or less, preferably 4 mass % or less, or 3 mass % or less. (Storage test) Water vapor permeability (JIS K 7129 compliant, 40℃ / 90%RH) is 0.2~0.6g / m 2 The fire extinguishing material package obtained by sealing the fire extinguishing material in a packaging material (packaging bag) formed from a packaging material film having a moisture content of 10 ...
[0061] [When the extinguishing material has only an extinguishing agent layer] Using a heat and dry moisture meter, heat the extinguishing agent layer at 140°C for 5 minutes, and calculate the moisture content of the extinguishing agent layer from the difference in weight between before and after heating using the following formula. Moisture content (%) = (moisture content of extinguishing agent layer (g) / weight of extinguishing agent layer before heating (g)) x 100 [When the fire extinguishing material has a base material and a fire extinguishing agent layer] Using a heat and dry moisture meter, heat the extinguishing material at 140°C for 5 minutes, and measure the moisture content of the extinguishing material from the weight difference before and after heating. Similarly, measure the moisture content of the base material alone from the weight difference before and after heating. Then, calculate the moisture content of the extinguishing agent layer using the following formula. Moisture content (%) = {(moisture content of extinguishing material (g) - moisture content of base material (g)) / (weight of extinguishing material before heating (g) - weight of base material before heating (g))} x 100
[0062] The extinguishing material can be placed on or near an object that may catch fire. The extinguishing material package can be placed in the same manner, or the packaging material may be removed and only the extinguishing material placed. Installation methods include pasting, placing, and bundling. Examples of items that may catch fire include electric wires, distribution boards, control panels, storage batteries (lithium ion batteries, etc.), building materials such as wallpaper for building materials and ceiling materials, lithium ion battery collection boxes, trash cans, automobile-related parts, electrical outlets, and electrical outlet covers. For example, in a device in which a fire extinguishing material or a fire extinguishing material package is installed, initial fire extinguishing is automatically performed in the device in response to a fire occurring in the device, and therefore such a device can be said to have an automatic fire extinguishing function. EXAMPLES
[0063] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0064] Example 1 A fire extinguishing agent was prepared by crushing potassium chlorate (KClO3) and tripotassium citrate in an agate mortar to an average particle size D50 of 12 μm or less. This fire extinguishing agent was mixed with various materials in the following compounding ratios to obtain a composition for forming a fire extinguishing agent layer. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 81 parts by weight Film-forming agent (silane coupling agent X-12-1287A, Shin-Etsu Chemical Co., Ltd.) 4 parts by weight Ethanol 87 parts by weight
[0065] The composition for forming a fire extinguishing agent layer was applied to one side of a polyethylene terephthalate (PET) substrate (product name: E7002, manufactured by Toyobo Co., Ltd., thickness 50 μm) using an applicator so that the fire extinguishing agent layer would be 150 μm thick after drying, and the composition was dried at 75° C. for 7 minutes to obtain a fire extinguishing material.
[0066] Example 2 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 45 parts by weight Film-forming agent (silane coupling agent X-12-1287A, Shin-Etsu Chemical Co., Ltd.) 8 parts by weight Ethanol 87 parts by weight
[0067] Example 3 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 81 parts by weight Film-forming agent (silane coupling agent X-12-967C, Shin-Etsu Chemical Co., Ltd.) 4 parts by weight Ethanol 87 parts by weight
[0068] Example 4 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 81 parts by weight Film-forming agent (Rosin Malkied No. 33, Arakawa Chemical Industries Co., Ltd.) 4 parts by weight Ethanol 87 parts by weight
[0069] Example 5 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 81 parts by weight Film-forming agent (6AN-5000 (acrylic polyol resin, Taisei Fine Chemical Co., Ltd.) 7.8 parts by weight, Takenate D110N (isocyanate resin, Mitsui Chemicals Co., Ltd.) 1.1 parts by weight) 8.9 parts by weight Ethanol 87 parts by weight
[0070] Example 6 A film-forming agent (X-12-1287A, Shin-Etsu Chemical Co., Ltd.) was added to tripotassium citrate, and the mixture was ground and mixed in an agate mortar so that the average particle diameter D50 of tripotassium citrate was 12 μm or less, thereby obtaining tripotassium citrate with a film (organosilane film) formed on the surface. A fire extinguishing material was obtained in the same manner as in Example 1, using a composition for forming a fire extinguishing agent layer obtained by mixing this tripotassium citrate with various materials in the following compounding ratios. Fire extinguishing agent components (potassium chlorate, tripotassium citrate, film-forming agent mixture) 91 parts by weight Ether-based urethane resin solution (a solution obtained by dissolving 100 parts by weight of ether-based polyurethane resin in 210 parts by weight of isopropyl alcohol) 28 parts by weight Ethanol 148 parts by weight
[0071] Comparative Example 1 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 118 parts by weight Ethanol 87 parts by weight
[0072] Comparative Example 2 A fire extinguishing material was obtained in the same manner as in Example 1, except that various materials were prepared as follows. Fire extinguishing agent components (potassium chlorate, tripotassium citrate) 87 parts by weight Polyvinyl butyral resin solution (a solution obtained by dissolving 11 parts by weight of polyvinyl butyral resin in 80 parts by weight of ethanol and 9 parts by weight of isopropyl alcohol) 81 parts by weight Silane coupling agent X-12-1267B (Shin-Etsu Chemical Co., Ltd.) 4 parts by mass Ethanol 87 parts by weight
[0073] (Evaluation: Coating observation) Using a scanning electron microscope JSM-7001F (JEOL Ltd.), elemental analysis of the tripotassium citrate particle surface was performed by energy dispersive X-ray spectroscopy (EDS) to confirm the presence or absence of a coating. The results are shown in Table 1.
[0074] (Evaluation: property stability) A barrier film (water vapor permeability is 0.2 to 0.6 g / m) comprising a sealant layer (L-LDPE (linear low-density polyethylene) resin, thickness 30 μm) and a base layer (PET (polyethylene terephthalate) resin with a silica vapor deposition film, thickness 12 μm). 2 / day, 40℃ / 90% RH conditions) were prepared. Two sheets of this barrier film were used to cover each example of fire extinguishing material, and the four sides of the barrier film were heat sealed to enclose the fire extinguishing material in the packaging material. The heat sealing conditions were 140°C for 2 seconds, and the seal width was 10 mm. This was used as the evaluation sample (fire extinguishing material package). The evaluation sample was stored at 85°C / 85% RH for a specified time, and the change in total light transmittance Δ was calculated from the total light transmittance before and after storage. The total light transmittance was measured using a haze meter BYK-Gardner Haze-Guard Plus (manufactured by BYK) with the sample fixed in place so that the light entering the integrating sphere from the light source passed through the fire extinguishing material. Change in total light transmittance Δ(%)=Total light transmittance value after storage-Total light transmittance value before storage From the obtained change in total light transmittance Δ, the property stability was evaluated according to the following criteria. The results are shown in Table 1. A: After storage for 168 hours, the change in total light transmittance Δ was 40% or less. B: After storage for 12 hours, the change in total light transmittance Δ was 40% or less. C: After storage for 12 hours, the change in total light transmittance Δ was more than 40%.
[0075] (Evaluation: Moisture content) The extinguishing material obtained in each example was cut into 5 cm squares and enclosed in a packaging material in the same manner as in the above property stability evaluation to obtain a fire extinguishing material package. This fire extinguishing material package was left to stand for 12 hours under 85°C / 85% RH and then opened, and the fire extinguishing material in the packaging material was used as an evaluation sample. Each evaluation sample was heated at 140°C for 5 minutes using a heat-drying moisture meter (METTLER TOLEDO, HB43-S), and the moisture content of the fire extinguishing material was measured from the weight difference before and after heating. Similarly, the moisture content of the base material alone was measured from the weight difference before and after heating. The moisture content of the fire extinguishing agent layer was then calculated using the following formula. The results are shown in Table 1. Moisture content (%) = {(moisture content of extinguishing material (g) - moisture content of base material (g)) / (weight of extinguishing material before heating (g) - weight of base material before heating (g))} x 100
[0076] [Table 1]
[0077] The fire extinguishing materials of the examples showed good property stability because a coating was formed on the deliquescent tripotassium citrate.The fire extinguishing materials of the examples showed excellent property stability because the coating agent had an alkene skeleton (butadiene skeleton) that forms a hydrophobic structure or a cyclic alkane structure. In the fire extinguishing material of the comparative example, a coating was not formed on the tripotassium citrate, and therefore the property stability was inferior to that of the examples. [Explanation of symbols]
[0078] 1...fire extinguishing agent layer, 2...substrate, 3...packaging material, 10...fire extinguishing material, 100...fire extinguishing material package.
Claims
1. A fire extinguishing agent layer containing a fire extinguishing agent including granular potassium citrate, A fire extinguishing material, wherein the potassium citrate has a coating on its surface formed from a coating forming agent.
2. The fire extinguishing material according to claim 1 , wherein the film-forming agent comprises a compound having an acid anhydride group or an isocyanate group.
3. 3. The fire extinguishing material according to claim 1 or 2, wherein the extinguishing agent further comprises potassium chlorate.
4. The fire extinguishing material according to claim 1 or 2, wherein the potassium citrate has an average particle size D50 of 1 to 100 μm.
5. The fire extinguishing material according to claim 1 or 2, wherein the extinguishing agent layer contains 70 to 97% by mass of the extinguishing agent.
6. 3. The fire-extinguishing material of claim 1 or 2, further comprising a substrate on which the fire-extinguishing agent layer is disposed.
7. The fire extinguishing material according to claim 1 or 2, wherein the water content of the fire extinguishing agent layer after the following storage test is 5 mass% or less. (Storage test) Water vapor permeability (JIS K 7129 compliant, 40°C / 90% RH conditions) is 0.2 to 0.6 g / m 2 The fire extinguishing material package obtained by sealing the fire extinguishing material in a packaging material formed from a packaging film having a temperature of 100° C. / day is stored stationary for 12 hours in an environment of 85° C. / 85% RH.
8. A fire extinguishing material package comprising a packaging material and the fire extinguishing material according to claim 1 or 2 enclosed in the packaging material.
Citation Information
Patent Citations
Self-extinguishing molded article