Translucent member and light-emitting device

By polishing and treating the light extraction surface of a translucent member with an organic solvent, the method enhances light extraction efficiency in light-emitting devices, addressing the challenge of total internal reflection and improving luminous flux.

JP2024153745AActive Publication Date: 2024-10-29NICHIA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024119203
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-29
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing light-emitting devices face challenges in maximizing light extraction efficiency due to total internal reflection at the surface of wavelength conversion members, which limits the amount of light emitted.

Method used

A method involving the preparation of a translucent member containing a phosphor and resin, followed by polishing the light extraction surface and contacting it with an organic solvent to round sharp edges, reducing total reflection and enhancing light extraction efficiency.

Benefits of technology

The method increases light extraction efficiency by diffusing light more effectively through the translucent member, resulting in improved luminous flux and reduced total reflection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153745000001_ABST
    Figure 2024153745000001_ABST
Patent Text Reader

Abstract

To provide a translucent member and a light-emitting device with which it is possible to raise the efficiency of light extraction.SOLUTION: Provided is a translucent member including a particulate phosphor and a resin and being provided with a light extraction plane. On the light extraction plane is included a protrusion in a region enclosed in a square with sides of 20 μm, that has an angle within the range of over 0° to 160°in a cross sectional view and has two sides, with one side within the range of 0.5 μm to 2 μm. The number of the protrusions is from 1 to 100, and the arithmetic average roughness Ra of light extraction plane of the translucent member after being contacted with an organic solvent, as measured in conformity with JIS B0601-2001, is in the range from 0.2 μm to 4 μm.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a light-transmitting member, a light-transmitting member, and a light-emitting device. [Background technology]

[0002] Light emitting diodes (hereinafter also referred to as "LEDs") and laser diodes (hereinafter also referred to as "LDs") are widely used as light emitting elements.

[0003] In order to convert the wavelength of light emitted from a light-emitting element such as an LED or LD, a light-transmitting member containing a phosphor and a resin and including at least a light extraction surface, or a ceramic composite containing a phosphor and an aluminate is used as a wavelength conversion member. Light-emitting devices equipped with a light-emitting element and a wavelength conversion member are used in a wide range of fields as light sources for interior lighting, vehicle lighting, etc., backlight light sources for liquid crystal displays, illumination, projector light sources, etc.

[0004] Patent Document 1 discloses a wavelength conversion member that includes a phosphor and a translucent resin and has irregularities on at least a part of its planar structure to improve light scattering, as a material for use in remote phosphor technology having a configuration in which a semiconductor body including a semiconductor light emitting element and an optical element including a wavelength conversion member are arranged at an interval. Patent Document 1 discloses a method of immersing in an organic solvent, a method of applying an organic solvent and brushing, and a method of casting into a mold with irregularities to form irregularities on at least a part of the planar structure of the wavelength conversion member. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2014-192251 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of one aspect of the present invention is to provide a method for manufacturing a light-transmitting member, a light-transmitting member, and a light-emitting device that can increase the light extraction efficiency. [Means for solving the problem]

[0007] A first aspect is a method for manufacturing a light-transmitting member, the method including: preparing a light-transmitting member including a phosphor and a resin and having a light extraction surface; polishing a surface of the light extraction surface; and contacting the polished light extraction surface with an organic solvent.

[0008] A second aspect is a light-transmitting member that includes a phosphor and a resin, and has a light extraction surface, and on the light extraction surface, within an area surrounded by a square with sides of 20 μm, has a convex portion that has an angle in a cross-sectional view of more than 0° and not more than 160°, and has two sides with one side being within a range of 0.5 μm or more and 2 μm or less, and the number of the convex portions is within a range of 1 to 100.

[0009] A third aspect is a light emitting device including the above-mentioned light-transmitting member and an excitation light source. Effect of the Invention

[0010] According to one aspect of the present invention, it is possible to provide a manufacturing method for a light-transmitting member, a light-transmitting member, and a light-emitting device that can increase the light extraction efficiency. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a flow chart showing an example of a method for manufacturing a light-transmitting member according to this embodiment. [Figure 2A] FIG. 2A is a schematic perspective view showing an example of a light emitting device. [Figure 2B] FIG. 2B is a schematic cross-sectional view of the light emitting device of FIG. 2A taken along line AA'. [Figure 2C] FIG. 2C is a plan view of the light emitting device of FIG. 2A. [Diagram 3]FIG. 3 is an SEM photograph showing a part of the light extraction surface of one sample of the light-transmitting member according to Example 1 after polishing and before contact with the organic solvent. [Figure 4] FIG. 4 is an SEM photograph showing a part of the light extraction surface of one sample of the light-transmitting member according to Example 1 after polishing and after contact with an organic solvent. [Diagram 5] FIG. 5 is a schematic diagram of a protrusion having two sides measured on the light extraction surface of a light-transmitting member. [Figure 6] FIG. 6 is an SEM photograph showing a part of the light extraction surface of one sample of the light-transmitting member according to Example 1 after polishing and before contact with the organic solvent. [Figure 7] FIG. 7 is an SEM photograph showing a part of the light extraction surface of one sample of the light-transmitting member according to Example 1 after polishing and after contact with an organic solvent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, a method for manufacturing a light-transmitting member, a light-transmitting member, and a light-emitting device according to the present invention will be described based on embodiments. However, the embodiments shown below are merely examples for embodying the technical idea of ​​the present invention, and the present invention is not limited to the method for manufacturing a light-transmitting member described below. Note that the relationship between color names and chromaticity coordinates, and the relationship between the wavelength range of light and the color names of monochromatic light, etc., follow JIS Z8110.

[0013] Manufacturing method of light-transmitting member A method for manufacturing a light-transmitting member according to the present embodiment includes preparing a light-transmitting member including a phosphor and a resin and having a light extraction surface, polishing a surface of the light extraction surface, and contacting the polished light extraction surface with an organic solvent. For example, when the surface of a wavelength conversion member is polished to improve the light extraction efficiency, unevenness is formed on the surface of the wavelength conversion member, and the tips of the convex parts of the uneven structure may have an acute angle. If the tips of the convex parts of the uneven structure on the surface of the wavelength conversion member have an acute angle after polishing the surface of the wavelength conversion member, the acute angle of the tips of the convex parts may cause light to be diffused inside the wavelength conversion member, making it impossible to increase the light extraction efficiency. However, the manufacturing method of the light-transmitting member in this embodiment can increase the light extraction efficiency. That is, the acute angle part on the polished surface of the wavelength conversion member is dissolved with an organic solvent, so that the acute angle part has a slightly rounded shape. It is believed that the change in the shape of the unevenness on the surface of this wavelength conversion member changes the reflection angle from the light emitting element, reducing total reflection, and increasing the light extraction efficiency from the wavelength conversion member. In addition, although a part of the light reflected on the surface of the wavelength conversion member returns to the phosphor, the change in the shape of the unevenness on the surface of the wavelength conversion member reduces the total reflection on the surface of the wavelength conversion member. As a result, the light emitted from the phosphor decreases due to the return light from the light-emitting element caused by surface reflection, but on the other hand, the light from the light-emitting element increases, resulting in an increase in the light from the light-emitting element in the chromaticity coordinates, i.e., blue light.

[0014] Fig. 1 is a flowchart of a method for manufacturing a light-transmitting member. The steps of the method for manufacturing a light-transmitting member will be described with reference to Fig. 1. The method for manufacturing a light-transmitting member includes a step S101 of preparing a light-transmitting member, a step S102 of polishing the light extraction surface of the light-transmitting member, and a step S103 of contacting the polished light extraction surface of the light-transmitting member with an organic solvent.

[0015] Preparation of the light-transmitting material The light-transmitting member includes a phosphor and a resin, and has a light extraction surface. In the case of a light-transmitting member used in a light-emitting device, it is preferable that the light-transmitting member transmits 60% or more of the light emitted from the light-emitting element. The light-transmitting member may have a transmittance of 70% or more, 80% or more, or 90% or more of the light emitted from the light-emitting element, for example.

[0016] The resin contained in the light-transmitting member is preferably at least one resin selected from the group consisting of silicone resin, silicone-modified resin, epoxy resin, epoxy-modified resin, phenol resin, polycarbonate resin, acrylic resin, polymethylpentene resin (e.g., TPX (registered trademark)), polynorbornene resin, and mixtures thereof. Among them, at least one resin selected from the group consisting of silicone resin and epoxy resin is preferable, and silicone resin, which has excellent light resistance and heat resistance, is more preferable.

[0017] The phosphor contained in the light-transmitting member is preferably one that is excited by light from the light-emitting element. Examples of the phosphor include rare earth aluminate phosphors (YAG, LAG) activated with cerium, nitrogen-containing calcium aluminosilicate (CaO-Al2O3-SiO2) phosphors activated with europium and / or chromium, silicate ((Sr,Ba)2SiO4) phosphors activated with europium, β-sialon phosphors, nitride phosphors (CASN, SCASN) activated with europium, fluoride phosphors (KSF) activated with manganese, and sulfide phosphors activated with europium. The phosphors contained in the light-transmitting member may be used alone or in combination with two or more phosphors having different compositions.

[0018] The phosphor has an average particle size measured by the Fisher Sub-Sieve Sizer method (hereinafter also referred to as the "FSSS method") of preferably 5 μm to 50 μm, more preferably 6 μm to 45 μm, and even more preferably 7 μm to 40 μm. The larger the average particle size of the phosphor, the more efficiently the wavelength of the light emitted from the light-emitting element can be converted, and the light extraction efficiency from the light extraction surface of the translucent member can be improved. On the other hand, if the average particle size of the phosphor is too large, the workability decreases. The FSSS method is a type of air permeation method, and is a method for measuring the specific surface area by utilizing the flow resistance of air and mainly determining the particle size of primary particles. The average particle size measured by the FSSS method is the Fisher Sub-Sieve Sizer's Number.

[0019] The phosphor may be, for example, a light-emitting material called nanocrystal or quantum dot. Examples of such materials include semiconductor materials, such as semiconductors of groups 2 to 6, 3 to 5, and 4 to 6, specifically, CdSe and core-shell type CdS. x Se 1-x Examples of the phosphor include nano-sized highly dispersed particles such as ZnS, GaP, etc. Perovskite, lead sulfide, and chalcopyrite can also be used. Examples of such phosphors include particles having a particle size of about 1 nm to 20 nm (10 to 50 atoms). By using such phosphors, internal scattering can be suppressed, and the light transmittance can be further improved. Since quantum dot phosphors are unstable, they may be surface-modified or stabilized with a resin such as PMMA (polymethyl methacrylate). These may be bulk bodies (e.g., plate-shaped bodies) that are mixed with a transparent resin (e.g., epoxy resin, silicone resin, etc.) that is the base material constituting the light-transmitting member and molded, or may be plate-shaped bodies sealed with a transparent resin between glass plates.

[0020] The blending ratio of the resin and the phosphor in the light-transmitting member varies depending on the type of the resin and the phosphor contained in the light-transmitting member. The total amount of the phosphor is preferably in the range of 80 parts by mass to 300 parts by mass, more preferably in the range of 100 parts by mass to 250 parts by mass, and even more preferably in the range of 120 parts by mass to 200 parts by mass, relative to 100 parts by mass of the resin in the light-transmitting member composition for forming the light-transmitting member. When the resin is a silicone resin and the KSF phosphor, the β-sialon phosphor, and the silica filler are mixed to form the light-transmitting member composition, the content of the components contained in the light-transmitting member composition can be appropriately adjusted to match the predetermined chromaticity coordinates. For example, the light-transmitting member composition can have the KSF phosphor in the range of about 70 parts by mass to 80 parts by mass, the β-sialon phosphor in the range of about 75 parts by mass to 85 parts by mass, and the filler in the range of about 1 part by mass to 8 parts by mass, relative to 100 parts by mass of the silicone resin.

[0021] The light-transmitting member may contain a filler (e.g., a filler, a diffusing agent, a colorant, etc.) in addition to the phosphor and the resin. Examples of the filler include silica, titanium oxide, zirconium oxide, magnesium oxide, glass, a crystal or sintered body of a phosphor, and a sintered body of a phosphor and an inorganic binder. The refractive index of the filler may be adjusted as desired. Examples of the refractive index of the filler include 1.8 or more.

[0022] The filler is preferably a particle. The shape of the particle may be any of crushed, spherical, hollow, and porous. The average particle size (median diameter) of the particles is preferably in the range of 0.08 μm to 10 μm, which can provide a highly efficient light scattering effect. The average particle size of the filler particles is preferably an average particle size (median diameter) in which the cumulative frequency from the small diameter side in the volume-based particle size distribution measured by, for example, a laser diffraction scattering type particle size distribution measurement method reaches 50%. In addition, when using a commercially available filler, the catalog value can be referred to for the average particle size. The filler is preferably in the range of 10% by mass to 80% by mass with respect to the total amount of the light-transmitting member. The filler contained in the light-transmitting member is preferably in the range of 0.1 parts by mass to 10 parts by mass, more preferably in the range of 0.5 parts by mass to 8 parts by mass with respect to 100 parts by mass of the resin.

[0023] The light-transmitting member is preferably a sheet-like or plate-like member having a light extraction surface and a surface opposite to the light extraction surface. When the light-transmitting member is a sheet-like or plate-like member, the light-transmitting member is easy to manufacture, and when the light-transmitting member is used in a light-emitting device, it is easy to arrange the light-transmitting member in the direction of the light emitted from the light-emitting element, and the light-emitting device is easy to manufacture. The light-transmitting member may be a layered member in which a plurality of particle layers containing particulate phosphors are laminated.

[0024] The method of forming the light-transmitting member includes a method of forming the light-transmitting member into a sheet or plate-like body and bonding it by a hot melt method or with an adhesive, a method of attaching a phosphor by electrophoretic deposition and then impregnating it with a light-transmitting resin, potting, compression molding, spraying, electrostatic coating, printing, and the like. When forming the light-transmitting member using these methods, silica (aerosil) or the like may be added to adjust the viscosity or fluidity. When the light-transmitting member is to contain a phosphor, it is preferable to form the light-transmitting member using a spraying method, particularly a pulsed spraying method in which the spray is sprayed in a pulsed manner, i.e., intermittently. By forming the light-transmitting member using the pulsed spraying method, for example, the phosphor can be uniformly applied to a coating surface having an uneven shape. In addition, the pulsed spraying method can reduce the wind speed of the air without reducing the ejection speed of the slurry from the nozzle, so that a coating film having high adhesion between the phosphor contained in the light-transmitting member and the surface of another member, for example, a light-emitting element, can be formed. In addition, a thin film particle layer containing a particulate phosphor can be formed with a plurality of laminations.

[0025] For the pulse spray method, reference can be made to known methods described in, for example, JP-A-61-161175, JP-A-2003-300000, and WO 2013 / 038953.

[0026] The thickness of the light-transmitting member is not particularly limited, and may be, for example, in the range of 1 μm to 300 μm, 1 μm to 100 μm, 2 μm to 60 μm, or 5 μm to 40 μm. For example, when the light-transmitting member is used in a light-emitting device and is formed by a spray method, the light-transmitting member may have a thickness of 20 times or less, 10 times or less, 6 times or less, 4 times or less, or 3 times or less of the total thickness of the nitride semiconductor stack used in the light-emitting element.

[0027] The light extraction surface (hereinafter sometimes referred to as the "upper surface") of the light-transmitting member may be flat. In order to control the light distribution, the light extraction surface or other surfaces may be made uneven, such as convex or concave.

[0028] Polishing process The surface of the light extraction surface of the light-transmitting member is polished. Examples of the polishing method include polishing using abrasive paper, buff polishing, diamond grinding stone, etc. Polishing may be performed using a device. When using abrasive paper, abrasive paper with a grit size of 2000 (#2000) or more and 6000 (#6000) or less may be used. The light extraction surface of the light-transmitting member may be polished after cutting into a desired size or thickness. Examples of the method for cutting into a desired size or thickness include blade dicing, laser dicing, and wire saw.

[0029] The arithmetic mean roughness Ra1 of the light extraction surface of the light-transmitting member after polishing and before contacting with an organic solvent described later is preferably in the range of 0.8 μm to 5.0 μm, more preferably in the range of 0.9 μm to 4.5 μm, and even more preferably in the range of 1.0 μm to 4.0 μm. If the arithmetic mean roughness Ra1 of the light extraction surface of the light-transmitting member after polishing and before contacting with an organic solvent is in the range of 0.8 μm to 5.0 μm, in the step of contacting with an organic solvent after polishing, the sharp-angled parts of the tips of the convex parts generated by polishing on the light extraction surface are rounded, and the amount of light can be converged in a direction perpendicular to the light extraction surface by the lens effect of the curved surface of the rounded parts, thereby improving the light extraction efficiency. In the light extraction surface of the light-transmitting member, the arithmetic mean roughness of the light extraction surface before contacting with an organic solvent is Ra1, and the arithmetic mean roughness of the light extraction surface after contacting with an organic solvent is Ra2.

[0030] The arithmetic mean roughness of the light extraction surface of the light-transmitting member, the maximum height of the roughness curve described later, and the average length of the roughness curve elements can be measured in accordance with JIS B0601-2001 using, for example, a shape measuring laser microscope (VK-X200, manufactured by Keyence Corporation) whether the light extraction surface of the light-transmitting member has been polished or has been brought into contact with an organic solvent described later.

[0031] The maximum height Rz1 of the roughness curve of the light extraction surface of the light-transmitting member after polishing and before contact with an organic solvent described below is preferably in the range of 5 μm to 18 μm, more preferably in the range of 6 μm to 17 μm, and even more preferably in the range of 7 μm to 16 μm. In the roughness curve of the light extraction surface of the light-transmitting member, the maximum height before contact with the organic solvent is Rz1, and the maximum height after contact with the organic solvent is Rz2.

[0032] The average length RS1m of the roughness curve elements of the light extraction surface of the light-transmitting member after polishing and before contact with an organic solvent described below is preferably in the range of 10 μm to 20 μm, more preferably in the range of 11 μm to 19 μm, and even more preferably in the range of 12 μm to 18 μm. On the light extraction surface of the light-transmitting member, the average length of the roughness curve elements before contact with the organic solvent is designated RS1, and the average length of the roughness curve elements after contact with the organic solvent is designated RS2.

[0033] Contact with organic solvents The polished light extraction surface of the light-transmitting member is brought into contact with an organic solvent. Examples of methods for bringing the polished light extraction surface of the light-transmitting member into contact with an organic solvent include a method of immersing the polished light extraction surface of the light-transmitting member in an organic solvent, a method of applying an organic solvent to the polished light extraction surface of the light-transmitting member, and a method of dripping an organic solvent onto the polished light extraction surface of the light-transmitting member. Methods for applying an organic solvent include a dispense method, a spray method, an electrostatic application method, a printing method, and a coating method using a brush or a sponge. When an organic solvent is dripped onto the light extraction surface of the light-transmitting member, the amount of the organic solvent dripped is 1 mg / cm, depending on the type of organic solvent dripped. 2 More than 3mg / cm 2 It is preferable that the concentration is within the range of 1.2 mg / cm 2 More than 1.5g / cm 2It is more preferable that the contact time between the polished light extraction surface of the light-transmitting member and the organic solvent is within the following range: When the light extraction surface of the light-transmitting member is immersed in the organic solvent, for example, in the case of toluene, the contact time is preferably from 3 to 40 seconds, and particularly preferably from 5 to 20 seconds. However, since the contact time differs depending on the type and concentration of the organic solvent, it is adjusted appropriately.

[0034] The boiling point of the organic solvent is preferably within the range of 50° C. to 150° C. If the boiling point of the organic solvent is within the range of 50° C. to 150° C., the acute angle of the tip of the convex portion generated by polishing the light extraction surface of the light-transmitting member can be rounded, and the light distribution component in the direction perpendicular to the light extraction surface can be increased due to the lens effect of the fine convex portion, and the total reflection on the light extraction surface can be reduced, thereby further improving the light extraction efficiency.

[0035] The organic solvent is preferably at least one selected from the group consisting of an aliphatic hydrocarbon organic solvent, an aromatic hydrocarbon organic solvent, a ketone organic solvent, and an alcohol organic solvent. Examples of the aliphatic hydrocarbon organic solvent include n-hexane, n-heptane, cycloheptane, and isooctane. Examples of the aromatic hydrocarbon organic solvent include toluene, xylene, and benzene. Examples of the ketone organic solvent include acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of the alcohol organic solvent include methanol, ethanol, n-propyl alcohol, and isopropyl alcohol. In order to round the sharp-angled tip of the convex portion generated by polishing the light extraction surface of the light-transmitting member by contact with the organic solvent, it is preferable to use at least one organic solvent selected from the group consisting of toluene, xylene, n-heptane, n-hexane, benzene, and acetone, and two or more organic solvents may be used in combination. It is more preferable to use at least one organic solvent selected from the group consisting of toluene, xylene, n-heptane, n-hexane, benzene, and acetone.

[0036] After contacting the light extraction surface of the light-transmitting member with the organic solvent, it is preferable to obtain the light-transmitting member by drying the light extraction surface in a dryer for 15 minutes to 24 hours at room temperature or at a temperature range of 20° C. to 130° C. However, the drying temperature and time are appropriately adjusted since the drying state differs depending on the type and concentration of the organic solvent.

[0037] The light-transmitting member obtained by polishing the light extraction surface and then contacting it with an organic solvent preferably has the following characteristics.

[0038] The light-transmitting member contains a resin and a phosphor and has a light extraction surface. On the light extraction surface, within an area surrounded by a square with sides of 20 μm, the light extraction surface has a protrusion having an angle in the range of more than 0° and not more than 160° in cross-sectional view, and two sides with one side being in the range of 0.5 μm or more and 2 μm or less, and the number of protrusions is in the range of 1 to 100.

[0039] After the light extraction surface of the light-transmitting member is polished, many fine protrusions are formed on the light extraction surface, which have an angle of more than 0° and less than 160° in cross-sectional view and two sides each having a length of 0.5 μm to 2 μm. Some of the fine protrusions formed after polishing the light extraction surface of the light-transmitting member have an acute tip. By contacting the light extraction surface of the light-transmitting member with an organic solvent after polishing, the fine protrusions themselves or the tips of the protrusions are dissolved in the organic solvent, and the acute tips of relatively small fine protrusions having an angle of more than 0° and less than 160° in cross-sectional view and a length of 0.5 μm to 2 μm are reduced, and the tips of relatively large protrusions having a length of 0.5 μm to 2 μm are rounded. For this reason, the light-transmitting member obtained by polishing the light extraction surface and then contacting it with an organic solvent has a light extraction surface in which, within an area enclosed by a square with sides of 20 μm, the number of convex portions having an angle in a cross-sectional range of more than 0° and not more than 160° and two sides with one side being within a range of 0.5 μm or more and 2 μm or less is reduced to a range of 1 to 100. Due to the lens effect of the convex portions with rounded tips present on the light extraction surface, when the light-transmitting member is used in a light-emitting device, the light distribution component in the direction perpendicular to the light extraction surface can be increased, and total reflection at the light extraction surface can be reduced to further improve the light extraction efficiency. In the light extraction surface of the light-transmitting member, the number of convex portions having an angle in the range of more than 0° and less than 160° in cross-sectional view within a region surrounded by a square with one side of 20 μm, and having two sides with one side in the range of 0.5 μm to 2 μm, may be preferably in the range of 2 to 90, may be in the range of 3 to 85, may be in the range of 4 to 80, or may be in the range of 5 to 75. The number of convex portions or particles described later on the light extraction surface of the light-transmitting member can be measured, for example, using a shape measuring laser microscope (VK-X200, manufactured by Keyence Corporation). The convex portions having an angle in the range of more than 0° and less than 160° in cross-sectional view may be in the range of 0.5 μm to 1.5 μm, and may have two sides with one side of 1 μm.

[0040] When the light extraction surface of the light-transmitting member is polished, fine shavings are generated, and these shavings are present on the light extraction surface of the light-transmitting member as particles separate from the light-transmitting member. When the light extraction surface of the light-transmitting member is polished and then brought into contact with an organic solvent, the fine particles are also dissolved in the organic solvent, and the number of particles is reduced. In the light extraction surface of the light-transmitting member, it is preferable that within an area surrounded by a square with one side of 20 μm, there are 30 or less particles with a diameter measured in a planar view ranging from 0.2 μm to 20 μm. The shape of the particles may be spherical, ellipsoidal, polyhedral, or crushed. The diameter of the particles present on the light extraction surface of the light-transmitting member is usually in the range of 0.2 μm to 5 μm, and may be in the range of 0.2 μm to 3 μm, measured in a planar view. In the light extraction surface of the light-transmitting member, within an area surrounded by a square with one side of 20 μm, the number of particles having a diameter of 0.2 μm or more and 20 μm or less measured in a plan view may be 25 or less, 20 or less, or 18 or less. In the light extraction surface of the light-transmitting member, within an area surrounded by a square with one side of 20 μm, the number of particles having a diameter of 0.2 μm or more and 20 μm or less measured in a plan view may be 0 or 1 or more. In the light extraction surface of the light-transmitting member, when the number of particles having a diameter of 0.2 μm or more and 20 μm or less measured in a plan view within an area surrounded by a square with one side of 20 μm is 30 or less, the diffuse reflection of light caused by the particles present on the light extraction surface can be suppressed, and the light distribution component in the direction perpendicular to the light extraction surface can be increased, thereby further improving the light extraction efficiency.

[0041] The arithmetic mean roughness Ra2 of the light extraction surface of the light-transmitting member is preferably in the range of 0.2 μm to 4 μm, more preferably in the range of 0.3 μm to 3.5 μm, and even more preferably in the range of 0.4 μm to 3 μm. If the arithmetic mean roughness Ra2 of the light extraction surface of the light-transmitting member after polishing and contacting with an organic solvent is in the range of 0.2 μm to 4 μm, the tips of the fine convex portions formed by polishing the light extraction surface of the light-transmitting member become rounded by contacting with the organic solvent, and the lens effect of the curved surface of the rounded portions allows the amount of light to be focused in a direction perpendicular to the light extraction surface, thereby increasing the light extraction efficiency.

[0042] In the light-transmitting member, the maximum height Rz2 of the roughness curve of the light extraction surface is preferably 15 μm or less. After polishing the light extraction surface of the light-transmitting member, the light-transmitting member is brought into contact with an organic solvent, so that the tips of the fine convex parts formed by polishing are rounded, and the maximum height Rz2 of the roughness curve of the light extraction surface is reduced to 15 μm or less, and the lens effect of the curved surface of the rounded part allows the amount of light to be converged in a direction perpendicular to the light extraction surface, thereby increasing the light extraction efficiency. In the light-transmitting member, the maximum height Rz2 of the roughness curve of the light extraction surface is more preferably 12 μm or less, even more preferably 10 μm or less, even more preferably 8 μm or less, and particularly preferably 6 μm or less. The maximum height Rz2 of the roughness curve of the light extraction surface of the light-transmitting member may be 1 μm or more.

[0043] The average length RS2 of the roughness curve element of the light extraction surface of the light-transmitting member is preferably in the range of 1 μm to 12 μm, more preferably in the range of 2 μm to 10 μm, and even more preferably in the range of 3 μm to 8 μm. If the average length RS2 of the roughness curve element of the light extraction surface of the light-transmitting member after polishing and contacting with an organic solvent is in the range of 1 μm to 12 μm, the tips of the fine convex portions formed by polishing the light extraction surface of the light-transmitting member become rounded and small when contacted with the organic solvent, and the lens effect of the curved surface of the rounded and small portions allows the amount of light to be focused in a direction perpendicular to the light extraction surface, thereby increasing the light extraction efficiency.

[0044] In the light-transmitting member, the average roughness ratio Ra2 / Ra1 of the arithmetic mean roughness Ra2 of the light-extracting surface after polishing and contacting with the organic solvent to the arithmetic mean roughness Ra1 of the light-extracting surface after polishing and before contacting with the organic solvent is preferably in the range of 0.2 to 0.8, more preferably in the range of 0.3 to 0.7, and even more preferably in the range of 0.4 to 0.6. In the light-transmitting member, the fine convex parts formed on the light-extracting surface by polishing can be dissolved or the tips of the convex parts can be rounded by contacting the fine convex parts with the organic solvent. In the light-transmitting member, when the average roughness ratio Ra2 / Ra1 of the light-extracting surface before and after polishing and contacting with the organic solvent is in the range of 0.2 to 0.8, the lens effect of the curved surface of the rounded convex parts can converge the amount of light in a direction perpendicular to the light-extracting surface, thereby increasing the light extraction efficiency.

[0045] In the light-transmitting member, the maximum height ratio Rz2 / Rz1 of the maximum height Rz2 of the roughness curve of the light extraction surface after polishing and contacting with an organic solvent to the maximum height Rz1 of the roughness curve of the light extraction surface after polishing and before contacting with an organic solvent is preferably in the range of 0.1 to 0.9, more preferably in the range of 0.2 to 0.8, even more preferably in the range of 0.3 to 0.7, and particularly preferably in the range of 0.4 to 0.6. In the light-transmitting member, the fine convex parts formed on the light extraction surface by polishing can be dissolved or the tips of the convex parts can be rounded by contacting the fine convex parts with an organic solvent. In the light-transmitting member, when the maximum height ratio Rz2 / Rz1 of the roughness curve of the light extraction surface after polishing and before and after contacting with an organic solvent is in the range of 0.1 to 0.9, the lens effect of the curved surface of the rounded convex parts can converge the amount of light in a direction perpendicular to the light extraction surface, thereby increasing the light extraction efficiency.

[0046] In the light-transmitting member, the average length ratio RS2 / RS1 of the average length RS1 of the roughness curve element of the light extraction surface after polishing and before contact with the organic solvent to the average length RS2 of the roughness curve element of the light extraction surface after polishing and after contact with the organic solvent is preferably in the range of 0.1 to 0.9, more preferably in the range of 0.2 to 0.8, and even more preferably in the range of 0.3 to 0.7. In the light-transmitting member, by contacting the fine convex parts formed on the light extraction surface by polishing with an organic solvent, the fine convex parts can be dissolved or the tips of the convex parts can be rounded and small. In the light-transmitting member, when the average length ratio RS2 / RS1 of the roughness curve element of the light extraction surface after polishing and before and after contact with the organic solvent is in the range of 0.1 to 0.9, the lens effect of the curved surface of the rounded and small convex parts can converge the amount of light in a direction perpendicular to the light extraction surface, thereby increasing the light extraction efficiency.

[0047] Light-emitting device The light emitting device includes the light-transmitting member and an excitation light source. The excitation light source is preferably a light emitting element.

[0048] Hereinafter, an embodiment of the light emitting device will be described with reference to the drawings. The light emitting device described below is intended to embody the technical idea of ​​the present invention, and unless otherwise specified, the present invention is not limited to the following. Furthermore, the contents described in the embodiments and examples can be applied to other embodiments and examples. The size and positional relationship of the components shown in each drawing may be exaggerated to clarify the explanation.

[0049] 2A is a perspective view showing an outline of a light emitting device 1 according to an embodiment. The light emitting device 1 is a so-called side-view type light emitting device in which the surface adjacent to the light extraction surface is used as the mounting surface. The light emitting device 1 can also be applied to a so-called top-view type light emitting device in which the surface opposite to the light extraction surface is used as the mounting surface.

[0050] Fig. 2B is a schematic cross-sectional view of the light emitting device 1 in Fig. 2A taken along line A-A', and Fig. 2C is a schematic plan view of the light emitting device 1. The light emitting device 1 includes a light emitting element 5 mounted on a base 4, and a light-transmitting member 10 disposed on the light emitting element 5.

[0051] The substrate 4 includes a base material 2 and a connection terminal 3. The base material 2 includes a first main surface 2a having a longitudinal direction and a lateral direction perpendicular to the longitudinal direction, a second main surface 2b opposite to the first main surface 2a, a first end surface 2c extending in the longitudinal direction, and a second end surface 2d extending in the lateral direction. The connection terminals 3 are provided on the first main surface 2a of the base material, with at least a pair of positive and negative terminals. Here, the connection terminals 3 may be laminated from the base material 2 side toward the upper surface, which is the first main surface 2a of the base material 2, the second end surface 2d extending in the lateral direction, and the lower surface, which is the second main surface 2b.

[0052] The base 4 may have a recess 25 on the first end surface 2c of the base material 2, which is continuous with the first main surface 2a and the second end surface 2d and / or the second main surface 2b and the second end surface 2d. The recess 25 may be formed so that the length (width) w in the longitudinal direction is greater than the depth d in the lateral direction. The connection terminal 3 may be provided so as to extend onto the recess 25. The recess 25 may be provided on both sides of the base material 2 in the longitudinal direction.

[0053] A light-emitting element 5 is mounted on the first main surface 2a of the base 4 and is connected to the connection terminal 3. More specifically, one light-emitting element 5 is flip-chip mounted on the protruding pattern 3a of the connection terminal 3. The light-emitting element 5 has a pair of positive and negative electrodes each connected to the protruding patterns 3a of the pair of connection terminals 3 of the base 4 by a bonding member 6.

[0054] A sealing member 7 is provided on the first main surface 2a of the base 4 so as to contact the light emitting element 5 and cover the entire periphery of the side surface. The sealing member 7 is also provided on the surface side of the light emitting element 5 facing the base 4. More specifically, the sealing member 7 almost completely covers the surface (periphery) of the joining member 6, and is further provided between the light emitting element 5 and the base 4. This allows light to be efficiently extracted upward from the light emitting element 5. In addition, by providing the sealing member 7 on the surface side of the light emitting element 5 facing the base 4, the light emitting element 5 can be more firmly connected to the base 4. The upper surface of the sealing member 7 almost coincides with the upper surface of the light emitting element 5.

[0055] The above-mentioned light-transmitting member 10 is disposed on the light-emitting element 5, that is, on the surface opposite to the pair of positive and negative electrodes. The surface 10b of the light-transmitting member 10, which faces the light-extracting surface 10a, is disposed on the light-emitting element 5 side. The light-transmitting member 10 may cover the upper surface of the sealing member 7, and the end surface of the light-transmitting member 10 may be substantially coincident with the end surface of the sealing member 7. The light-transmitting member 10 disposed on the light-emitting element 5 has the above-mentioned characteristics, and therefore, when used in a light-emitting device, the light distribution component in the direction perpendicular to the light-extracting surface can be increased due to the lens effect of the convex portion with a rounded tip present on the light-extracting surface, and the total reflection on the light-extracting surface can be reduced, thereby further improving the light-extracting efficiency.

[0056] On the first main surface 2a side of the base material of the substrate 4, a part of the narrow portion of the connection terminal 3 and the external connection portion 3b are exposed from the sealing member 7 on both sides of the sealing member 7 on the substrate 4. On the second main surface 2b side of the base material, a metal layer 3d is arranged for reinforcement, heat dissipation, etc. in the portion where the connection terminal 3 is not arranged. Two insulating films 8 are formed in the region including this metal layer 3d. The two insulating films 8 are different in size and can function as marks to distinguish the anode and cathode of the light emitting device.

[0057] The sealing member 7 may be disposed so as to be in contact with a part or the whole of at least one side surface of the light-emitting element 5 and cover the side surface of the light-emitting element 5, or may be disposed so as to be in contact with the light-emitting element 5 and to surround the entire periphery of the light-emitting element 5. The sealing member 7 may be provided thin on a side surface (7a in FIG. 2C ) extending in the longitudinal direction of the light-emitting device 1 and thick on a side surface (7b in FIG. 2C ) extending in the lateral direction.

[0058] For the materials, size, characteristics, and manufacturing method of each member constituting the light emitting device, refer to JP 2015-220426 A. EXAMPLES

[0059] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0060] Example 1 Preparation of the light-transmitting material The silicone resin is mixed with the KSF phosphor, the β-sialon phosphor, and the silica filler, and the content is appropriately adjusted to match the predetermined chromaticity coordinates. For example, the KSF phosphor is in the range of about 70 parts by mass to 80 parts by mass, the β-sialon phosphor is in the range of about 75 parts by mass to 85 parts by mass, and the filler is in the range of about 1 part by mass to 8 parts by mass, relative to 100 parts by mass of the silicone resin. The KSF phosphor and the β-sialon phosphor are mixed with the silicone resin to produce a composition for a light-transmitting member. The composition for a light-transmitting member is cured into a sheet to obtain a sheet-like light-transmitting member having a thickness of 20 μm.

[0061] Polishing process One surface of the obtained light-transmitting member, which was to become a light extraction surface, was polished using abrasive paper having grit sizes of 2000 (#2000) to 6000 (#6000).

[0062] Contact with organic solvents Toluene was dropped onto the polished surface of the light-transmitting member and spread over the entire surface of the polished surface, so that the light extraction surface of the light-transmitting member was brought into contact with the toluene. After the light extraction surface of the light-transmitting member was brought into contact with the toluene, the light-transmitting member was dried to obtain a light-transmitting member. The amount of toluene dropped was 1 mg / cm. 2 to 3 mg / cm 2 More specifically, the range was 1.2 mg / cm 2 More than 1.5mg / cm 2 It was within the following range.

[0063] Comparative Example 1 The light-transmitting member of Comparative Example 1 was the same as that of Example 1, except that the light extraction surface of the light-transmitting member was not polished.

[0064] Evaluation of light-transmitting materials Arithmetic mean roughness, maximum height of roughness curve, average length of roughness curve element The arithmetic mean roughness, maximum height of the roughness curve, and average length of the roughness curve element of the light extraction surface of each of the light-transmitting members in the examples and comparative examples before contact with the organic solvent, after polishing, and after contact with the organic solvent were measured using a shape measuring laser microscope (VK-X200, manufactured by Keyence Corporation) in accordance with JIS B0601-2001. For the light extraction surface of each light-transmitting member, the arithmetic mean roughness before contact with the organic solvent was Ra1, the maximum height of the roughness curve was Rz1, and the average length of the roughness curve element was RS1. For the light extraction surface of each light-transmitting member, the arithmetic mean roughness after contact with the organic solvent was Ra2, the maximum height of the roughness curve was Rz2, and the average length of the roughness curve element was RS2. The results are shown in Table 1.

[0065] SEM images Measurement of protrusions and particles The light-transmitting member of the embodiment was observed at any site on the light-extraction surface before and after contact with the organic solvent using a scanning electron microscope (SEM). The light-transmitting member sample of the embodiment was placed on a tilted table inclined at 20°, and an SEM photograph was taken from directly above the light-transmitting member. The light-transmitting member sample was placed on the tilted table to take the SEM photograph so that the convex parts of the light-extraction surface of the light-transmitting member could be more clearly confirmed.

[0066] Measurement of protrusions and particles In an area surrounded by a square with sides of 20 μm in an SEM photograph of the light-transmitting member of the Example, the number of protrusions having an angle in the range of more than 0° and not more than 160° in cross-sectional view and two sides with one side being in the range of 0.5 μm to 2 μm was visually counted as shown in the schematic diagram of the protrusions in Fig. 5. For each of the light-transmitting members of the Example and Comparative Example, an arbitrary site on the light extraction surface before and after contact with the organic solvent was observed using an SEM, and the number of particles with diameters in the range of 0.2 μm to 20 μm measured in plan view was visually counted in an area surrounded by a square with sides of 20 μm.

[0067] [Table 1]

[0068] In the light-transmitting member of Example 1, after polishing, the arithmetic mean roughness Ra1 of the light extraction surface before contact with the organic solvent was in the range of 0.8 μm or more and 5.0 μm or less, and the mean roughness ratio Ra2 / Ra1 of the light extraction surface before and after contact with the organic solvent was in the range of 0.2 or more and 0.8 or less. In the light-transmitting member of Example 1, after polishing, the maximum height Rz1 of the roughness curve of the light extraction surface before contact with the organic solvent was in the range of 5 μm or more and 18 μm or less, and the maximum height ratio Rz2 / Rz1 of the roughness curve of the light extraction surface before and after contact with the organic solvent was in the range of 0.1 or more and 0.9 or less. In the light-transmitting member according to Example 1, after polishing, the average length RS1 of the roughness curve element of the light extraction surface before contact with the organic solvent was in the range of 10 μm or more and 20 μm or less, and the average length ratio RS2 / RS1 of the roughness curve element of the light extraction surface before and after contact with the organic solvent was in the range of 0.1 or more and 0.9 or less. In the light-transmitting member according to Example 1, the tips of the fine protrusions formed by polishing the light extraction surface were rounded by contact with the organic solvent.

[0069] FIG. 3 is an SEM photograph taken from directly above the light-transmitting member of Example 1, where one sample before contact with an organic solvent was placed on an inclined platform inclined at an angle of 20° from the plane. It was confirmed that fine convex portions were formed on the light-extraction surface of the light-transmitting member of Example 1 by polishing. FIG. 4 is an SEM photograph taken from directly above the light-transmitting member of Example 1, where one sample after contact with an organic solvent was placed on an inclined platform inclined at an angle of 20° from the plane. The light-extraction surface of the light-transmitting member of Example 1 had the tips of the fine convex portions rounded by contacting the light-extraction surface with an organic solvent after polishing.

[0070] In the light extraction surface of the light-transmitting member according to Example 1, the number of convex portions having an angle of more than 0° and less than 160° in cross-sectional view within a region surrounded by a square with one side of 20 μm, and having two sides with one side of 1 μm, was 360 before contact with the organic solvent, and was 56 after contact with the organic solvent. In the light extraction surface of the light-transmitting member according to Example 1, the number of convex portions having an angle of more than 0° and less than 160° in cross-sectional view within a region surrounded by a square with one side of 20 μm, and having two sides with one side of 1 μm, was reduced to a range of 1 to 100 after polishing the light extraction surface compared to the number of convex portions before contact with the organic solvent. From this result, it was speculated that when the light-transmitting member according to Example 1 is used in a light-emitting device, the lens effect of the convex portions with rounded tips present on the light extraction surface increases the light distribution component in a direction perpendicular to the light extraction surface, reducing the total reflection on the light extraction surface, and improving the light extraction efficiency.

[0071] Two or more samples were prepared for the light-transmitting member according to Example 1. In the light extraction surface of one sample of the light-transmitting member according to Example 1, the number of particles having a diameter of 0.2 μm or more and 20 μm or less in a plan view was visually counted within an area surrounded by a square with one side of 20 μm. In the light extraction surface of one sample 1 of the light-transmitting member according to Example 1, the number of particles having a diameter of 0.2 μm or more and 20 μm or less before contact with the organic solvent was 55, and the number of particles having a diameter of 0.2 μm or more and 20 μm or less after contact with the organic solvent was 16, which was a smaller number of particles than before contact with the organic solvent. In the light extraction surface of another sample 2 of the light-transmitting member according to Example 1, the number of particles having a diameter of 0.2 μm or more and 20 μm or less before contact with the organic solvent was 41, and the number of particles having a diameter of 0.2 μm or more and 20 μm or less after contact with the organic solvent was 13, which was a smaller number of particles than before contact with the organic solvent. From these results, it was inferred that when the light-transmissive member of Example 1 is used in a light-emitting device, the number of particles present on the light extraction surface is small, which suppresses diffuse reflection due to the particles and increases the light distribution component in the direction perpendicular to the light extraction surface, thereby improving the light extraction efficiency.

[0072] FIG. 6 is a planar SEM photograph of the light extraction surface of the light-transmitting member according to Example 1 before contact with an organic solvent, and the white frame indicates a region surrounded by a square with a side length of 20 μm. FIG. 7 is a planar SEM photograph of the light extraction surface of the light-transmitting member according to Example 1 after contact with an organic solvent, and the white frame indicates a region surrounded by a square with a side length of 20 μm. The light extraction surface of the light-transmitting member according to Example 1 was polished to form fine convex portions, and the tips of the fine convex portions were rounded by contacting the light with an organic solvent after polishing. From this result, it was speculated that when the light-transmitting member according to Example 1 is used in a light-emitting device, the lens effect of the convex portions with rounded tips present on the light extraction surface can increase the light distribution component in a direction perpendicular to the light extraction surface, reduce the total reflection on the light extraction surface, and improve the light extraction efficiency.

[0073] Light emitting device manufacturing Example 2 A light emitting device similar to the embodiment shown in Figures 2A to 2C was manufactured using the obtained light-transmitting member according to Example 1. Specifically, the light emitting device was manufactured as follows. The base material 2 of the substrate 4 was a bismaleimide triazine (BT) resin composition (HL832NSF typeLCA, manufactured by Mitsubishi Gas Chemical Co., Ltd.) containing a naphthalene-based epoxy resin containing a commercially available glass cloth. The base material 2 had a rectangular parallelepiped shape without a recessed portion 25. The connection terminal 3 was made of Cu / Ni / Au (total thickness: 2 μm) laminated from the base material 2 side. The substrate 4 had a length of 1.8 mm in the longitudinal direction, a width of 0.3 mm in the lateral direction, and a thickness of 0.45 mm. The light-emitting element 5 had a nitride semiconductor laminate (thickness: about 8 to 12 μm) formed on a sapphire substrate (thickness: about 150 μm), and had a pair of positive and negative electrodes on the surface of the laminate opposite to the sapphire substrate. The light-emitting element 5 has a pair of positive and negative electrodes connected to the protruding patterns 3a of the pair of connection terminals 3 of the base 4 by a fusible bonding member 6 (thickness: 20 μm) which is Au-Sn eutectic solder, and is flip-chip mounted on the base 4. The light-emitting element 5 is a rectangular parallelepiped blue-emitting LED chip (emission peak wavelength 455 nm) with a length of 0.9 mm in the longitudinal direction, a width of 0.2 mm in the lateral direction, and a thickness of 0.15 mm. The surface roughness Ra of the side surface of the light-emitting element 5 was 1.0 μm or less. The light-transmitting member 10 according to Example 1 was disposed so that the surface 10b opposite the light extraction surface 10a was on the light-emitting element 5 side, and covered the light-emitting element 5. The light-transmitting member 10 according to Example 1 had a thickness of 20 μm. The sealing member 7 is formed in a substantially rectangular parallelepiped shape with a longitudinal length (total length) of 1.2 mm, a lateral width (total length) of 0.3 mm, and a thickness of 0.15 mm. The sealing member 7 is formed from a silicone resin containing silica with an average particle size of 14 μm (catalog value) and titanium oxide as inorganic particles with an average particle size of 0.25 μm to 0.3 μm (catalog value) in a range of 2% by mass to 2.5% by mass and 40% by mass to 50% by mass, respectively, relative to the total mass of the sealing member 7. The end face of the sealing member 7 and the end face of the light-transmitting member 10 are substantially aligned.

[0074] Comparative Example 2 A light emitting device was manufactured in the same manner as in Example 2, except that the light-transmitting member according to Comparative Example 1 was used.

[0075] Light emitting device evaluation Chromaticity coordinates (x, y) and luminous flux of the light-emitting device For each light-emitting device of the examples and comparative examples, the chromaticity coordinates (x, y) and luminous flux in the chromaticity coordinate system of the CIE (Commission Internationale de l'Eclairage) 1931 chromaticity diagram were obtained using a light measurement system combining a spectrophotometer (PMA-11, Hamamatsu Photonics Co., Ltd.) and an integrating sphere. For each light-transmitting member of the examples and comparative examples, the chromaticity coordinates of the light-emitting device using the light-transmitting member before contact with the organic solvent were obtained as the chromaticity coordinates (x1, y1), and the luminous flux was obtained as F1. For each light-transmitting member of the examples and comparative examples, the chromaticity coordinates of the light-emitting device using the light-transmitting member after contact with the organic solvent were obtained as the chromaticity coordinates (x2, y2), and the luminous flux was obtained as F2. In addition, the difference between the chromaticity coordinates (x1, y1) and the chromaticity coordinates (x2, y2) was obtained as the change rate (Δx, Δy) of the chromaticity coordinates. The luminous flux ratio F2 / F1 between the luminous flux F1 and the luminous flux F2 was calculated as the rate of change with the luminous flux F1 being set at 100%. The results are shown in Table 2.

[0076] [Table 2]

[0077] In the light emitting device of Example 2 using the light-transmitting member of Example 1, the fine protrusions formed by polishing the light extraction surface of the light-transmitting member of Example 1 have rounded tips when exposed to an organic solvent, and the lens effect of the rounded tips of the protrusions increases the light distribution component in the direction perpendicular to the light extraction surface, reducing total reflection at the light extraction surface and improving the light extraction efficiency, with a high luminous flux ratio F2 / F1 of 100.6%.

[0078] In the light-emitting device of Comparative Example 2 using the light-transmitting member of Comparative Example 1, since the light-transmitting member of Comparative Example 1 was not polished, fine convex portions were not formed, and therefore the lens effect was not expected to be significant even when contacted with an organic solvent, resulting in a low luminous flux ratio F2 / F1. [Industrial Applicability]

[0079] In one embodiment of the present invention, the light-transmitting member can be used as a wavelength conversion member of a light-emitting device. A light-emitting device using the light-transmitting member can be used as a backlight source for a liquid crystal display, a light-emitting device for various types of illumination, a large display, a light-emitting device for a vehicle, a display device, a digital video camera, a facsimile, a copy machine, an image reading device in a scanner, a projector device, and the like. [Explanation of symbols]

[0080] 1: light-emitting device, 2: base material, 2a: first main surface (upper surface), 2b: second main surface (lower surface), 2c: first end surface, 2d: second end surface, 3: connection terminal, 3a: protruding pattern, 3b: external connection portion, 3d: metal layer, 4: base, 5: light-emitting element, 6: bonding member, 7: sealing member, 7a: side surface extending in the longitudinal direction, 7b: side surface extending in the lateral direction, 8: insulating film, 10: light-transmitting member, 10a: light extraction surface, 10b: surface facing the light extraction surface.

Claims

1. The light extraction surface includes a particulate phosphor and a resin, and the light extraction surface includes a convex portion having an angle in a cross-sectional view of more than 0° and not more than 160° within a region surrounded by a square with one side of 20 μm, and having two sides with one side being in a range of 0.5 μm to 2 μm, and the number of the convex portions is 1 to 100, A light-transmitting member, the arithmetic mean roughness Ra of a light extraction surface of the light-transmitting member after contact with an organic solvent being in the range of 0.2 μm to 4 μm, as measured in accordance with JIS B0601-2001.

2. 2. The light-transmitting member according to claim 1, wherein the maximum height Rz2 of a roughness curve of the light extraction surface, measured in accordance with JIS B0601-2001, is 15 μm or less.

3. 3. The light-transmitting member according to claim 1, wherein the light extraction surface has 30 or less particles each having a diameter in the range of 0.2 μm to 20 μm in a square region with sides of 20 μm.

4. 4. The light-transmitting member according to claim 1, wherein the phosphor has an average particle size measured by a Fisher subsieve sizer method in the range of 5 μm to 50 μm.

5. 5. The light-transmitting member according to claim 1, wherein the resin is at least one resin selected from the group consisting of a silicone resin, a silicone-modified resin, an epoxy resin, an epoxy-modified resin, a phenol resin, a polycarbonate resin, an acrylic resin, a polymethylpentene resin, a polynorbornene resin, and mixtures thereof.

6. The light-transmitting member according to claim 1 , which is a sheet-like body or a plate-like body having a surface facing the light extraction surface.

7. The light-transmitting member according to claim 1 , wherein the particulate phosphor includes a nano-sized phosphor having a particle size of 1 nm to 20 nm.

8. A light emitting device comprising: the light-transmitting member according to claim 1 ; and an excitation light source.

9. The light emitting device according to claim 8 , wherein the excitation light source is a light emitting element.

Citation Information

Patent Citations

  • Laser medium and its manufacture

    JP1997326523A

  • Multicolor luminescent device

    JP1998241860A

  • Phosphor panel manufacturing method

    JP2006300647A

  • Manufacturing method for light-emitting element

    JP2011060658A

  • Wavelength conversion member and semiconductor light-emitting device using the same

    JP2014192251A