Plate material
The described board material, with fiber-reinforced resin plates and a foam core, addresses warping and delamination issues in wooden boards by ensuring rigidity and stability, maintaining structural integrity and wood-like texture.
Patent Information
- Application Number
- JP2023070261
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
Wooden boards face issues with warping, bending, and delamination due to external forces and uneven expansion/contraction, making it difficult to create large-area, thin laminated boards with sufficient rigidity and stability.
A board material composed of fiber-reinforced resin plates laminated on both sides of a foam core material, with a wooden board on one side, achieving a bending elastic modulus of 15 MPa or more and a total thickness of 4 mm to 30 mm, using a reactive adhesive for chemical bonding and a foam core material with a compressive strength of 0.2 MPa or more.
The solution provides a lightweight, rigid board material with the texture of wood that resists delamination even when made thin over a large area, maintaining structural integrity under various conditions.
Smart Images

Figure 2024155500000001 
Figure 2024155500000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a plate material. [Background technology]
[0002] Compared to metals, ceramics, etc., wood has a warm texture and feel, and has the unique ability to adjust the environment by absorbing moisture when the humidity is high and releasing it when the humidity is low. Furthermore, wood is used as a structural material because it has a low density and is lightweight, so it is still used in various parts of our lives today.
[0003] On the other hand, wood has a disadvantage in that it has low rigidity compared to metals, ceramics, etc., making it difficult to use as a material for parts that are subjected to external forces such as bending and twisting. Furthermore, wood, particularly large areas, has low dimensional stability and is prone to deformation, as it expands and contracts unevenly depending on the temperature and humidity conditions, causing warping and bending, due to the characteristics of natural materials that vary depending on the region and time of harvest, and even within the same material.
[0004] Therefore, for example, Patent Document 1 proposes a technology in which a synthetic resin foam material or a plastic lattice is used as a core material covered entirely with a synthetic resin or fiber-reinforced synthetic resin, and a two-layer board made by joining wooden flat boards together and bonding the upper and lower boards with the ends reversed, to the front and back of this core material, thereby producing a board material that has the appearance of wood and is highly rigid, and which can be used as a terrace deck. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Utility Model Registration No. 3049893 Summary of the Invention [Problem to be solved by the invention]
[0006] For applications where thickness is not an issue, such as terrace decks, warping and bending of the board can be suppressed by making each layer, including wood, thicker, but when large, thin boards such as table tops and shelves, or fittings, are made from laminates containing wood (wood boards), they are prone to delamination due to warping caused by external forces, bending caused by their own weight, and stress caused by differences in expansion and contraction between the layers. Therefore, the issue of simply making laminates larger or thinner remains.
[0007] The present invention has been made to solve such problems, and aims to provide a board material that is lightweight and highly rigid, has the texture and feel of wood, and is less likely to undergo delamination even when made thin and large in area. [Means for solving the problem]
[0008] As a result of intensive research by the present inventors to solve the above problems, they have completed the following embodiment of the present invention.
[0009] (1) The board material of the present invention is a board material comprising a base material in which fiber-reinforced resin plates are laminated on both sides of a foamed core material, and a wooden board is laminated on at least one side of the base material, wherein the flexural modulus of the foamed core material is 15 MPa or more and the overall thickness is 4 mm or more and 30 mm or less.
[0010] (2) In the plate material according to the present invention, the 5% compressive strength of the foamed core material may be 0.2 MPa or more.
[0011] (3) In the plate material according to the present invention, the reinforcing fibers constituting the fiber-reinforced resin plate may be carbon fibers.
[0012] (4) In the plate material according to the present invention, the reinforcing fibers constituting the fiber-reinforced resin plate may have a woven structure.
[0013] (5) Furthermore, in the plate material of the present invention, the matrix resin constituting the fiber-reinforced resin plate may have active hydrogen groups in its molecules, and the fiber-reinforced resin plate and the foamed core material may be bonded via a reactive adhesive that forms chemical bonds with the active hydrogen groups in the matrix resin.
[0014] (6) In the plate material according to the present invention, the matrix resin may be a phenoxy resin.
[0015] (7) Furthermore, in the board material according to the present invention, the thickness of the wooden board may be 0.15 mm or more and 3.0 mm or less. Effect of the Invention
[0016] According to the present invention, it is possible to provide a board material that is lightweight and highly rigid, has the texture and feel of wood, and is resistant to delamination even when made thin and large in area. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiments of the present invention will be described. Note that each of the embodiments described below shows one specific example of the present invention. Furthermore, the present invention is not limited to only the following aspects, and many modifications are possible within the spirit and scope of the present invention.
[0018] The board material in this embodiment is a board material comprising a base material in which fiber-reinforced resin plates are laminated on both sides of a foamed core material, and a wooden board is laminated on at least one side of the base material, wherein the flexural modulus of the foamed core material is 15 MPa or more, and the overall thickness is 4 mm or more and 30 mm or less.
[0019] <Foam core material> The plate material according to the present embodiment includes a foamed core material having a flexural modulus of 15 MPa or more, with a fiber-reinforced resin plate described later laminated on both sides as a base material. The foamed core material in the present invention refers to a plate-shaped core material made of a porous body (foamed body) having a large number of independent or interconnected fine bubbles with a diameter of about 0.1 μm to 1 mm inside.
[0020] The core material according to the present embodiment has a relatively high flexural modulus, and therefore plays a role in providing rigidity and thickness to the base material. In addition, by using a foam as the core material, the apparent density of the plate material is reduced, making it a lightweight plate material, and the adhesive area is secured and the adhesive has an anchor effect, improving the adhesive strength between the foam core material and the fiber-reinforced resin plate.
[0021] The material used as the foam core is not particularly limited as long as it can form a plate-shaped foam with a flexural modulus of 15 MPa or more, and examples of the material include thermoplastic resins such as (meth)acrylic resin, polyvinyl chloride, polystyrene, polyurethane resin, and novolac, thermosetting resins such as melamine and resol, and inorganic materials such as ceramics. For weight reduction, it is preferable to use an organic resin as the material for the foam core, and in particular, when shaping is performed, such as curving the plate material by hot pressing, a thermoplastic resin is preferable.
[0022] The method of foaming the material is not particularly limited, and examples of the method include mechanical foaming in which bubbles are formed in the resin by stirring the resin with a mixer or injecting gas, and chemical foaming in which bubbles are formed by gas generated during the reaction of a curing agent or a separate foaming material. In addition, a large number of the material such as beads obtained by mechanical foaming or by foaming in advance may be collected and molded into a plate, or a method in which gas generation is promoted during the process of molding into a plate and foaming is performed simultaneously with molding may be used.
[0023] The expansion ratio depends on the material selected, but is preferably 10 to 25 times. If the expansion ratio is 10 times or more, the weight of the plate material will be reduced and the anchor effect of the adhesive will be more pronounced. If the expansion ratio is 25 times or less, it is easier to obtain a foam core material with high mechanical strength in bending, compression, tension, etc.
[0024] The foam core material according to the present embodiment has a flexural modulus of 15 MPa or more. By using a foam core material having a relatively high flexural modulus of 15 MPa or more, each layer of the plate can withstand external forces such as bending and twisting, compared to a case where the flexural modulus is relatively low, and the stress that causes delamination can be dispersed, thereby suppressing the occurrence of delamination. The flexural modulus of the foam core material is preferably 25 MPa or more, more preferably 35 MPa or more, and even more preferably 55 MPa or more. The upper limit of the flexural modulus is not particularly limited, but is preferably 150 MPa or less from the viewpoint of weight reduction. The flexural modulus can be measured in accordance with JIS K7221-2 (2006).
[0025] The foam core material according to the present embodiment may further have a 5% compressive strength of 0.2 MPa or more. When the 5% compressive strength of the foam core material is 0.2 MPa or more, the plate material is less likely to be dented even when an impact such as a blow is applied to the plate material. The 5% compressive strength of the foam core material is preferably 0.3 MPa or more, more preferably 0.5 MPa or more, and even more preferably 1.0 MPa or more. The upper limit of the 5% compressive strength of the foam core material is not particularly limited, but is preferably 3.0 MPa or less from the viewpoint of weight reduction. The 5% compressive strength of the foam core material can be determined by performing a compression test in accordance with JIS K7220 (2006) and dividing the maximum load at the time when the deformation rate of the test piece reaches 5% by the initial cross-sectional area of the test piece.
[0026] <Fiber-reinforced resin plate> The plate material according to the present embodiment includes a base material in which a fiber-reinforced resin plate is laminated on both sides of the foam core material. The fiber-reinforced resin plate includes reinforcing fibers and a matrix resin impregnated in the reinforcing fibers, and serves to impart high rigidity to the base material.
[0027] Materials used as reinforcing fibers constituting a fiber-reinforced resin plate include inorganic fibers such as carbon fibers, graphite fibers, silicon carbide fibers, alumina fibers, tungsten carbide fibers, boron fibers, glass fibers, and basalt fibers, organic fibers such as aramid fibers, ultra-high molecular weight polyethylene fibers, polyarylate fibers, polyparaphenylene benzoxazole fibers, polyphenylene sulfide fibers, polyimide fibers, fluorine fibers, and polyvinyl alcohol fibers, and metal fibers such as aluminum fibers, iron fibers, copper fibers, nickel fibers, titanium fibers, and stainless steel fibers. Among these, it is preferable to use carbon fibers as reinforcing fibers, which have a low specific gravity, a low linear expansion coefficient, and low hygroscopicity, and exhibit little dimensional change due to temperature and humidity conditions.
[0028] The reinforcing fibers constituting the fiber-reinforced resin plate may be short fibers or long fibers (continuous fibers). The structure of the reinforcing fibers is not particularly limited, and examples include a form in which a resin containing short fibers is dispersed in a matrix resin described later, a nonwoven fabric obtained by papermaking short fibers, a unidirectional material in which long fibers are simply aligned, a woven fabric in which aligned long fibers are woven, or a knitted fabric in which aligned long fibers are knitted. From the viewpoint that it is easy to give the plate material impact resistance by conducting and releasing the impact applied to the plate material to the entire surface, it is preferable that the reinforcing fibers are long fibers. In addition, a woven fabric in which reinforcing fiber threads cross warp and weft is less likely to cause thickness variations in the process of impregnating with the matrix resin, and a flatter plate can be obtained, compared with a unidirectional material that is simply aligned and a knitted fabric in which the threads have room to move between loops. Since the occurrence of delamination can be suppressed by the flatness of the fiber-reinforced resin plate, it is more preferable that the structure of the reinforcing fibers is a woven fabric. Furthermore, unlike a unidirectional material, a woven fabric made of reinforcing fibers does not have anisotropy of strength in the plane. When using unidirectional material as the reinforcing fiber structure, it is necessary to stack multiple sheets with changing axial directions to eliminate the anisotropy of in-plane strength. When bending or twisting forces are applied, the directions of strain differ between the layers, which can lead to delamination. However, when woven fabric is used as the reinforcing fiber structure, delamination is less likely to occur even when multiple sheets are stacked.
[0029] The yarn constituting the reinforcing fiber fabric is made of 1,000 to 500,000 reinforcing fibers that have been aligned and bundled together. In addition, the fiber-reinforced resin plate is preferably impregnated with the matrix resin up to the inside of the reinforcing fiber bundle. In this case, the reinforcing fiber bundle is preferably opened to facilitate impregnation of the matrix resin into the reinforcing fiber bundle, but when a matrix resin with a sufficiently low viscosity is used, the reinforcing fiber bundle does not need to be opened.
[0030] The weave of the fabric is not particularly limited and may be plain weave, twill weave, satin weave, etc. If it is desired to improve the strength and abrasion resistance of the resulting plate material, a plain weave may be selected, and if the plate material is to be shaped, a twill weave may be selected which is less prone to wrinkles.
[0031] The fiber-reinforced resin plate according to this embodiment is obtained by impregnating the reinforcing fibers with a matrix resin.
[0032] The material used as the matrix resin is not particularly limited, and examples thereof include polyamide, (meth)acrylic resin, polyphenylene sulfide, polyvinyl chloride, (cyclic) polyolefins such as polyethylene and polypropylene, rubbers such as polyacetal, polycarbonate, thermoplastic polyurethane resin, polyester resin, and ABS resin, thermoplastic resins such as polyphenylene ether, polysulfone, polyethersulfone, polyetherketone, polyetheretherketone, polyetherimide, novolac, and phenoxy resin, and thermosetting resins such as unsaturated polyester resin, urea resin, melamine, thermosetting polyurethane resin, resol, and epoxy resin, and these may be further chemically modified.
[0033] Among them, if a matrix resin having an active hydrogen group in the molecule is used, the fiber-reinforced resin plate and the adhesive that forms a chemical bond with the active hydrogen group in the matrix resin can form a chemical bond and can be firmly bonded. The matrix resin having an active hydrogen group in the molecule is not particularly limited as long as it has a plurality of functional groups having active hydrogen, such as hydroxyl groups, amino groups, imino groups, carboxyl groups, urethane groups, ureido groups, and thiol groups, in the molecule, and examples thereof include thermosetting resins such as melamine, thermosetting polyurethane resins, resols, and epoxy resins, (meth)acrylic resins having active hydrogen groups such as 2-hydroxy(meth)acrylate, novolac, and phenoxy resins. In particular, if the matrix resin is a thermoplastic resin, the active hydrogen groups are not consumed during polymerization and exist in large numbers as side chains, which increases the number of bonding sites with the adhesive and improves the adhesive strength, so that the matrix resin is more preferably a thermoplastic resin. In particular, the matrix resin is most preferably a phenoxy resin, which has excellent weather resistance and abrasion resistance. When a thermoplastic resin is used not only for the matrix resin but also for the foamed core material, it is possible to shape the plate material by hot pressing.
[0034] The method of impregnating the reinforcing fibers with the matrix resin is not particularly limited, and examples thereof include an in-situ polymerization method in which the reinforcing fibers are impregnated with a low-viscosity monomer and then polymerized and cured, and a hot melt method in which the matrix resin is heated and melted to impregnate the reinforcing fibers, etc. In general, monomers have low viscosity or are easy to reduce the viscosity, so it is preferable to use the in-situ polymerization method from the viewpoint that the resin can be easily impregnated into the inside of the bundle of reinforcing fibers without opening the reinforcing fibers.
[0035] The volume fraction (Vf value) of the reinforcing fibers in the fiber reinforced resin is preferably 20% to 80%, more preferably 40% to 70%. Within this range, the moldability is excellent and the obtained plate material has an excellent balance of rigidity, toughness, and strength.
[0036] The thickness of the fiber reinforced resin plate is not particularly limited, but is about 0.2 mm to 4.0 mm. If the thickness of the fiber reinforced resin plate is 0.2 mm or more, a substrate having high rigidity is easily obtained. On the other hand, if the thickness of the fiber reinforced resin plate exceeds 4.0 mm, the rigidity becomes higher than necessary, and it is likely to be economically disadvantageous. The thickness of the fiber reinforced resin plate can be adjusted by the thickness, number, Vf value, etc. of the reinforcing fibers, and a plurality of fiber reinforced resin plates may be laminated.
[0037] <Base material> The plate material according to the present embodiment includes a base material in which the fiber-reinforced resin plates are laminated on both sides of the foam core material. By laminating the fiber-reinforced resin plates on both sides of the foam core material, a base material that is lightweight and has high rigidity is obtained, and the symmetrical configuration in the thickness direction can suppress warping and bending.
[0038] The method of laminating the foam core material and the fiber reinforced resin plate may be, for example, by bonding the foam core material and the fiber reinforced resin plate via an adhesive, or when at least one of the matrix resins constituting the foam core material or the fiber reinforced resin plate is a thermoplastic resin, the foam core material and the fiber reinforced resin plate may be bonded and laminated by heat fusion. Here, even if the flexural modulus of the foam core material is relatively high, it is a material that is about 10 to 1000 times lower than the flexural modulus of the fiber reinforced resin plate. For this reason, when a large force is applied to the plate material, the deformation rate between the layers differs, large stress is generated, and there is a risk of causing delamination. In order to improve the adhesive strength and suppress the occurrence of delamination, it is preferable that a resin having an active hydrogen group in the molecule is used as the matrix resin constituting the fiber reinforced resin plate, and the fiber reinforced resin plate and the foam core material are bonded via a reactive adhesive that forms a chemical bond with the active hydrogen group in the matrix resin.
[0039] Examples of reactive adhesives include epoxy resin adhesives, urethane resin adhesives, formaldehyde adhesives such as urea resin, melamine resin, and phenol resin adhesives, silicone resin adhesives, and adhesives in which isocyanate is added to other base adhesives.
[0040] The method for bonding the foam core material and the fiber-reinforced resin plate is not particularly limited, and for example, when an adhesive is used, the adhesive having flowability is applied to the foam core material or the fiber-reinforced resin plate, or both, by applying a treatment such as dilution or heating as necessary, and after bonding the coated surfaces, curing may be performed while applying a means for promoting adhesive hardening, such as heating, humidification, or irradiation with active energy rays such as ultraviolet rays or electron beams, depending on the type of adhesive selected. In addition, when bonding the foam core material and the fiber-reinforced resin plate by heat fusion, the materials may be heated to a temperature at which the thermoplastic resin melts, and then bonded together while degassing as necessary, and allowed to cool.
[0041] <Wood board> The board material according to the present embodiment is a board material in which a wooden board is laminated on at least one side of the base material. The wooden board laminated on the base material plays the role of a decorative material. By using the wooden board as a decorative material, the board material can be given the texture and feel of wood.
[0042] The raw wood for the wooden boards used in this embodiment is not particularly limited, and examples thereof include coniferous trees such as cypress, pine, and cedar, and broad-leaved trees such as oak, beech, zelkova, cherry, sawtooth oak, magnolia, maple, walnut, teak, and mahogany.
[0043] The form of the wooden board is not particularly limited, and any of solid wood, width-jointed lumber, laminated lumber, etc. can be used. However, from the viewpoint of providing a strong sense of the texture and feel of wood, it is preferable to use solid wood, which is a single board cut from a log.
[0044] The thickness of the wooden board is preferably 0.15 mm or more and 3.0 mm or less. If the thickness of the wooden board is 0.15 mm or more, a board material that is resistant to surface friction can be obtained. Also, if the thickness of the wooden board is 3.0 mm or less, the stress generated by the expansion and contraction of the wooden board due to temperature and humidity conditions can be reduced, and the occurrence of delamination can be suppressed. In addition, when solid wood is used as the wooden board, thin solid wood has the advantage that it is easier to obtain and more economically advantageous than thick solid wood, which is rare. A more preferable range of the thickness of the wooden board is 0.3 mm or more and 2.0 mm or less.
[0045] <Plate material> The board material according to this embodiment is a board material in which a wooden board is laminated on at least one surface of the base material, and has an overall thickness of 4 mm or more and 30 mm or less.
[0046] The substrate and the wooden board are laminated by bonding via an adhesive. The adhesive used for bonding the substrate and the wooden board is not particularly limited, and examples thereof include (water) solvent type adhesives, emulsion type adhesives, hot melt type adhesives, and reactive adhesives. Here, when using wooden boards made of raw wood such as pine, maple, and teak, which are considered to be relatively difficult to bond with adhesives due to their high oil content, it is preferable to use a reactive adhesive as the adhesive for bonding the substrate and the wooden board, as in the case of bonding a foam core material and a fiber-reinforced resin board. This allows the reactive adhesive to form a chemical bond with cellulose, resulting in high adhesive strength.
[0047] When the thickness of the wooden board is thinned to 3.0 mm or less, there is a risk that the adhesive will ooze out from the grain of the wooden board. Therefore, in order to suppress the oozing out of the adhesive, a sealing layer may be laminated between the fiber-reinforced resin board and the wooden board. The sealing layer is laminated between the base material and the wooden board, integrated with the adhesive that has permeated into the layer. The material used for the sealing layer is not particularly limited as long as it prevents the adhesive from oozing out from the grain and does not interfere with the adhesion between the base material and the wooden board, and examples of the material include paper, nonwoven fabric, and woven fabric. As the sealing layer, it is particularly preferable to use Japanese paper, which has relatively long fibers that are excellent in sealing properties and are made of the same cellulose material as the wooden board and are less likely to inhibit adhesion, or long-fiber nonwoven fabric made of recycled fibers such as cellulose or rayon.
[0048] The plate material according to this embodiment can provide a plate material that is lightweight and highly rigid, has the texture and feel of wood, and is less susceptible to delamination even when it is large in area, even if it is as thin as 4 mm or more and 30 mm or less overall. From the viewpoint of easier suppression of delamination, the thickness of the plate material is preferably 6 mm or more, and more preferably 8 mm or more. Furthermore, even if the thickness of the plate material is 20 mm or less, a plate material in which delamination is suppressed can be obtained. The thickness of the plate material may be 15 mm or less.
[0049] In order to decorate the end faces of the boards, decorative stickers or the above-mentioned wooden boards cut to a narrow width may be attached to the end faces of the boards, or a separate material that will become a frame (stile) may be placed on the end of the boards. Furthermore, in order to improve the design of the end faces of the boards, the end faces may be sloped.
[0050] (Example) The plate material according to the present embodiment will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. All modifications that do not deviate from the purpose of the present invention are included in the technical scope of the present invention. In addition, the measurements, tests and evaluations of various performances in the following examples were performed by the following methods.
[0051] <Flexural modulus> The flexural modulus was measured according to JIS K7221-2 (2006). The test conditions for the foam core were as follows: the test piece size was 350 mm long x 40 mm wide x 10 mm thick, the support distance was 300 mm, and the pressure wedge speed was 20 mm / min. The test conditions for the plate material were as follows: the test piece size was 400 mm long x 30 mm wide, the support distance was 300 mm, and the pressure wedge speed was 5 mm / min.
[0052] <5% Compressive Strength> The 5% compressive strength was determined by performing a compression test in accordance with JIS K7220 (2006) and dividing the maximum load at the time when the deformation rate of the test piece reached 5% by the initial cross-sectional area of the test piece.
[0053] <Temperature and humidity cycle test> First, a rectangular plate material with a length of 280 cm and a width of 100 cm was prepared. In an environmental test room, the plate material was supported by legs installed at the four corners, and a weight of 50 kg was placed on the center of the plate material. One cycle consisted of one hour at 20°C x 60% RH, one hour at 40°C x 20% RH, one hour at 40°C x 95% RH, and one hour at 20°C x 60% RH. The presence or absence of delamination of the plate material was confirmed after each cycle. The maximum number of cycles at which no delamination occurred is listed in the table.
[0054] <Load bearing test> First, a rectangular plate material with a length of 150 cm and a width of 80 cm was prepared. The plate material was hung on a support with a distance between supports of 100 cm in an environment of 20°C and 60% RH, and a load was applied to the center of the plate material with an indenter speed of 10 kgf / sec and a maximum load of 100 kgf, and then the load was removed at the same speed. This test was counted as one cycle, and the condition was checked every 500 cycles, and the test was continued until delamination occurred.
[0055] <Impact resistance test> The test was conducted in accordance with the impact test for horizontal surfaces described in JIS S1205 (1998). The test specimen was a rectangular plate 100 cm long x 80 cm wide, with the four corners fixed, and a 25 kg impactor was dropped 10 times from a height of 240 mm to apply impact. Those that had no dents after the test were deemed to have passed.
[0056] Example 1 <Reinforced fiber> First, glass fibers with a filament thickness of 12 μm were aligned in one direction and wound around a bobbin.
[0057] <Fiber-reinforced resin plate> The glass fiber was unwound from a bobbin, and impregnated with heat-molten polypropylene while being rolled with a hot roll to obtain a prepreg (unidirectional material) with a thickness of 0.6 mm and a Vf value of 54%. Two sheets of the prepreg were then laminated with the fiber axis direction changed by 90 degrees and thermocompression bonded to obtain a fiber-reinforced resin plate.
[0058] <Base material> An acrylic resin foam core material with a thickness of 5 mm, foaming ratio of 25 times, flexural modulus of elasticity of 26.4 MPa, and 5% compressive strength of 0.32 MPa was prepared, and a fiber-reinforced resin plate coated with a urethane resin-based adhesive was bonded to both sides of the foam core material, followed by curing to obtain a substrate.
[0059] <Plate material> A sheet of 1.0 mm thick oak solid wood was laminated on one side of the substrate so that a sheet of Japanese paper impregnated with a synthetic rubber adhesive was sandwiched between the two, and the sheet was cured to obtain a board. The evaluation results of the obtained board are shown in Table 1.
[0060] Comparative Example 1 A plate material was obtained in the same manner as in Example 1, except that an acrylic resin foamed core material having a thickness of 5 mm, an expansion ratio of 40 times, a flexural modulus of elasticity of 12.2 MPa, and a 5% compressive strength of 0.14 MPa was used as the foamed core material. The evaluation results of the obtained plate material are shown in Table 1.
[0061] Comparative Example 2 A plate material was obtained in the same manner as in Example 1, except that a paper honeycomb core having a thickness of 5 mm, a cell size of 10 mm, a flexural modulus of 27.9 MPa, and a 5% compressive strength of 0.36 MPa was used as the core material instead of the foamed core material. The evaluation results of the obtained plate material are shown in Table 1.
[0062] [Table 1]
[0063] From Table 1, it can be seen that boards using foamed cores with a flexural modulus of 15 MPa or more are less likely to develop delamination in both temperature and humidity cycle tests and load bearing tests. It was also found that boards using cores with a 5% compressive strength of 0.2 MPa or more have excellent impact resistance.
[0064] Example 2 <Reinforced fiber> A carbon fiber fabric was obtained by plain weaving a bundle of 12,000 carbon fibers with a filament thickness of 6 μm, which were aligned in one direction.
[0065] <Fiber-reinforced resin plate> The carbon fiber fabric was impregnated with a liquid containing a bifunctional epoxy monomer that becomes a phenoxy resin after curing and a curing agent, and then squeezed with a mangle roll and dried at 150° C. for 20 minutes to obtain a prepreg (fabric) with a thickness of 0.6 mm and a Vf value of 61%. Two sheets of the prepreg were then laminated and thermocompression bonded to obtain a fiber-reinforced resin plate.
[0066] <Base material> An acrylic resin foam core material with a thickness of 5 mm, foaming ratio of 25 times, flexural modulus of elasticity of 26.4 MPa, and 5% compressive strength of 0.32 MPa was prepared, and a fiber-reinforced resin plate coated with a urethane resin-based adhesive was bonded to both sides of the foam core material, followed by curing to obtain a substrate.
[0067] <Plate material> A sheet of 1.0 mm thick oak or maple solid wood was laminated on both sides of the base material so that the paper impregnated with a synthetic rubber adhesive was sandwiched between them, and the laminate was cured to obtain a board. The evaluation results of the obtained board are shown in Table 2.
[0068] Example 3 <Reinforced fiber> A bundle of 6,000 glass fibers with a filament thickness of 12 μm was oriented in one direction and woven into a plain weave to obtain a glass fiber fabric.
[0069] Except for using the glass fiber woven fabric as the reinforcing fiber, a plate material was obtained in the same manner as in Example 2. The evaluation results of the obtained plate material are shown in Table 2.
[0070] Example 4 <Reinforced fiber> First, carbon fibers with a filament thickness of 6 μm were aligned in one direction and wound around a bobbin.
[0071] <Fiber-reinforced resin plate> The reinforcing fiber was unwound from a bobbin, impregnated with a liquid containing a bifunctional epoxy monomer that becomes a phenoxy resin after curing and a curing agent, squeezed with a mangle roll, and dried at 150°C for 20 minutes to obtain a prepreg (unidirectional material) with a thickness of 0.5 mm to 0.6 mm and a Vf value of 56%. Next, two sheets of the prepreg were laminated with the fiber axis direction changed by 90 degrees and heat-pressed to obtain a fiber-reinforced resin plate. A plate material was obtained in the same manner as in Example 2, except that the fiber-reinforced resin plate was used. The evaluation results of the obtained plate material are shown in Table 2.
[0072] Example 5 A plate material was obtained in the same manner as in Example 2, except that polypropylene was impregnated as the matrix resin constituting the fiber-reinforced resin plate by the same hot melt method as in Example 1. The evaluation results of the obtained plate material are shown in Table 2.
[0073] Example 6 Aside from using solid oak or maple wood having a thickness of 3.5 mm as the wooden board, a board material was obtained in the same manner as in Example 2. The evaluation results of the obtained board material are shown in Table 2.
[0074] [Table 2]
[0075] From Table 2, it was found that a board material that is less likely to cause delamination in a temperature and humidity cycle test can be obtained by using carbon fiber as the reinforcing fiber and having a thickness of 3.0 mm or less for the wooden board. It was also found that a board material that is less likely to cause delamination in a load-bearing test can be obtained by using a woven structure for the reinforcing fiber that constitutes the fiber-reinforced resin board, by using a matrix resin that constitutes the fiber-reinforced resin board that has active hydrogen groups in its molecules, and by bonding the fiber-reinforced resin board and the foamed core material via a reactive adhesive that forms chemical bonds with the active hydrogen groups in the matrix resin.
Claims
1. The board material comprises a base material having a fiber-reinforced resin plate laminated on both sides of a foamed core material, and a wooden plate laminated on at least one side of the base material, the foamed core material having a flexural modulus of 15 MPa or more and an overall thickness of 4 mm or more and 30 mm or less.
2. 2. The board material according to claim 1, wherein the 5% compressive strength of the foamed core material is 0.2 MPa or more.
3. 3. The plate material according to claim 1, wherein the reinforcing fibers constituting the fiber-reinforced resin plate are carbon fibers.
4. 3. The plate material according to claim 1, wherein the reinforcing fibers constituting the fiber-reinforced resin plate have a woven structure.
5. 3. The plate material according to claim 1, wherein the matrix resin constituting the fiber-reinforced resin plate has active hydrogen groups in its molecules, and the fiber-reinforced resin plate and the foamed core material are bonded together via a reactive adhesive that forms a chemical bond with the active hydrogen groups in the matrix resin.
6. The board material according to claim 5 , wherein the matrix resin is a phenoxy resin.
7. The board material according to claim 1 or 2, wherein the thickness of the wooden board is 0.15 mm or more and 3.0 mm or less.
Citation Information
Patent Citations
Woody panel
JP1996174514A
Mat floor material
JP2000186416A
Fiber-reinforced composite body and method for producing fiber-reinforced composite body
JP2016150561A
terrace deck
JP3049893U