Polyvinyl alcohol film, optical film including the same, and method for manufacturing these

By controlling thickness deviation, phase difference uniformity, and moisture content uniformity, the film manufacturing process addresses uneven dyeing and breakage issues, resulting in a polyvinyl alcohol film with uniform dyeing and high tear resistance for polarizing plates.

JP2024155996AInactive Publication Date: 2024-10-31CHANG CHUN PETROCHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024145457
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-22
Filing Date
2024-08-27
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polyvinyl alcohol films face issues such as uneven dyeing, poor stretchability, and film breakage during the manufacturing process, particularly when producing thinner films, leading to staining spots and uneven thickness, which affect the quality of polarizing plates.

Method used

The film is manufactured with controlled thickness deviation, phase difference uniformity, and moisture content uniformity, defined by specific coefficients, along with a precise drying process to ensure uniform dyeing and high tear resistance.

Benefits of technology

The resulting film exhibits low unevenness in dyeing, high tear resistance, and no staining or density spots, enabling the production of wider and thinner films with improved optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155996000001_ABST
    Figure 2024155996000001_ABST
Patent Text Reader

Abstract

To provide a polyvinyl alcohol film, an optical film including the polyvinyl alcohol film, and a method for manufacturing these.SOLUTION: A polyvinyl alcohol film has a staining coefficient of 7 to 70. The staining coefficient is obtained by a product of a thickness deviation within 10 cm and a phase difference uniformity coefficient. The polyvinyl alcohol film has a modulus of rupture of less than 130. The modulus of rupture is obtained by a product of a phase difference uniformity coefficient and a moisture content uniformity coefficient. The polyvinyl alcohol film of the invention has characteristics of low heterogeneity of staining and high breakage resistance.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl alcohol (PVA) film. The PVA film is an optical film and its manufacturing method. , in particular, can be used as a polarizing film. [Background technology]

[0002] Polyvinyl alcohol (PVA) film is It is a type of hydrophilic polymer that has properties such as transparency, mechanical strength, water solubility, and good processability. It is widely used in packaging materials and optical films for electronic products. Coal film is an important component in polarizing plates, which has polarizing properties after dyeing and stretching, By polarizing light, it is possible to control brightness, and currently, various types of liquid crystal screens It is widely used in the

[0003] In recent years, as screen technology has become thinner, the quality requirements for the polarizing plate manufacturing process have also increased. During the process of thinning, the issues of stretchability and dye uniformity are also being addressed. In order to achieve this, gradual improvements have been required.

[0004] In the manufacturing process of preparing optical films from polyvinyl alcohol films, Depending on the function, functional group modification can be selectively used, followed by stretching. The dry method is performed in an inert gas atmosphere at a constant temperature and humidity. The polyvinyl alcohol film is stretched under atmospheric conditions, and then dyeing and other processes are carried out. In the wet method, the polyvinyl alcohol film is dyed and then stretched in a solution. Polyvinyl alcohol films prepared by the dry process have uneven surfaces. Polyvinyl acetate produced by the wet process often has the problem of uneven dyeing. Alcohol films have good properties (e.g. uniform color) and are now commonly used for wet Polyvinyl alcohol films are often produced using the formula method.

[0005] When producing polarizing film, the higher the stretch ratio, the better the optical performance obtained. Therefore, during stretching, the polyvinyl alcohol film is stretched to the critical point where it approaches rupture. The film is then stretched as far as possible to obtain a polyvinyl alcohol film having excellent optical properties.

[0006] A good polarizing film has characteristics such as uniform color, few color spots, and no wrinkles, and has excellent In order to improve the optical properties of the polarizing film, the conventional In this study, we changed the structure of polyvinyl alcohol or added functional groups (e.g., cationic groups). By changing the viscosity or degree of saponification, the optical properties are improved. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Chinese Patent No. 103992606 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the conventional technology, it is difficult to obtain a large-sized polarizing film using a polyvinyl alcohol film. When manufacturing the film, the dyeing may become uneven and the film may become less stretchable. For example, in Patent Document 1, a polyvinyl alcohol used in a polarizing plate is The retardation of the film in the width direction is 10 to 40 nm. It is described that if the thickness is less than 10 nm, staining spots are likely to occur. For example, the retardation of the polyvinyl alcohol film at the center in the width direction is set to 10 to 40. However, we noticed that even when the control was performed within 1 nm, there was still a problem of staining spots. In addition, when making a polyvinyl alcohol film thinner, the physical properties of the film must be the same as those of a wider film. As the conditions for the film stretching become more stringent, the film is stretched to prevent breakage. It is necessary to somehow control the crystal uniformity and moisture uniformity of the film.

[0009] Regarding the thickness of the film, the inventors have found that if the difference in thickness between the film surfaces is excessively large, The thick areas will become darker and the light areas will become lighter, resulting in an uneven appearance and poor filtering. When the deviation in film thickness is not large, the difference in phase difference between adjacent film surfaces is excessively large. When the phase difference is large, the area with a large phase difference will be darker and the area with a small phase difference will be lighter. Therefore, the appearance of the dye on the film surface is affected by the thickness of the film and the Since it is determined by a complex factor of the difference in phase difference, both deviation values ​​must be controlled within certain limits. If you use a roller, you can avoid the occurrence of dye spots and density spots. Also, the problem of film cutting can be avoided. Regarding the above, the inventors have investigated the water content uniformity of the film (which indicates the stretchability) and the phase difference uniformity (which indicates the crystallinity). If the temperature (T) is controlled within a certain range, it is possible to manufacture wider and thinner films. I noticed that this did not cause any film cutting issues. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides a polyvinyl alcohol filter. The thickness deviation of the film at 10 cm and the dyeing coefficient determined by the phase difference uniformity coefficient are and the modulus of rupture, which is determined by combining the phase difference uniformity coefficient with the moisture content uniformity. This gives the film low unevenness in dyeing and high tear resistance. is.

[0011] The present invention relates to a polyvinyl alcohol having a dye coefficient of 7 to 70 and a modulus of rupture of less than 130. The dyeing coefficient is based on the thickness deviation and phase difference within 10 cm. The modulus of rupture is the product of the phase difference uniformity coefficient and the moisture content uniformity coefficient.

[0012] In a preferred embodiment, the dye coefficient of the polyvinyl alcohol film is between 7 and 27.

[0013] In the preferred embodiment, the thickness deviation of the polyvinyl alcohol film within 10 cm is 3.0 μm. m or less.

[0014] In a preferred embodiment, the phase difference uniformity coefficient of the polyvinyl alcohol film is 4.7 to 24. Between 7.

[0015] In a preferred embodiment, the polyvinyl alcohol film further has a standard moisture content of less than 0.3%. Has deviation.

[0016] In the preferred embodiment, the thickness deviation of the polyvinyl alcohol film within 10 cm is 2.0 μm. m or less.

[0017] Another object of the present invention is to provide an optical film, which is made of the above-mentioned polyvinyl acetate. It is made of alcohol film.

[0018] In a preferred embodiment, the optical film is a polarizing film.

[0019] Another object of the present invention is to provide a method for producing the polyvinyl alcohol film. The process includes: (a) heating a polyvinyl alcohol resin at a temperature of 100° C. or higher for 1 hour; Dissolve under a pressure of at least 1000000000 atm for at least 5 hours to form a polyvinyl alcohol solution. (b) A dissolving step, and (b) a polyvinyl alcohol solution is extruded at 20 kg / cm 2 The above (c) a film is formed on multiple drying rolls. The distribution of the inlet temperature and outlet temperature of the heat source of the first drying roll is less than 4°C; (d) a moisture adjustment step in which the standard deviation of the temperature in the width direction is less than 4°C; After the film is formed, it is dried in a dryer to obtain a polyvinyl alcohol film. Including,

[0020] In a preferred embodiment, step (b) is performed with a die back pressure of 25 kg / cm 2 This will be carried out under the above . Effect of the Invention

[0021] As an effect of the present invention, the polyvinyl alcohol film provided by the present invention has a high degree of elasticity after dyeing. After that, when the polarizing plate is crossed, it is inspected and there are no staining spots or density spots, and the staining non-uniformity is low. It has been found that the film provided by the present invention has the following characteristics when stretched: It has sufficient extensibility to avoid breakage and has high tear resistance. [Brief description of the drawings]

[0022] [Figure 1]FIG. 2 is a conceptual diagram of a drying step in a moisture adjustment step in a method for producing a polyvinyl alcohol film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The following embodiments are not intended to excessively limit the present invention. Those skilled in the art may make modifications to the examples discussed herein without departing from the spirit or scope of the present invention. Modifications and variations can be made, all of which are within the scope of the present invention.

[0024] As used herein, the terms "a" and "one" refer to one or more of the objects of the grammar. It refers to the presence of at least one of the following:

[0025] The present invention relates to a polyvinyl alcohol having a dye coefficient of 7 to 70 and a modulus of rupture of less than 130. The dyeing coefficient is based on the thickness deviation and phase difference within 10 cm. The modulus of rupture is the product of the phase difference uniformity coefficient and the moisture content uniformity coefficient.

[0026] The thickness deviation of the polyvinyl alcohol film is in the range of 100 to 2000 mm to avoid color difference. The difference in thickness in the direction is controlled within a limited range. The "thickness deviation within 10 cm" is the thickness deviation of t mm in the width direction and 50 mm in the machine direction. A polyvinyl alcohol film sample was taken, and the t value was set to the width of the polyvinyl alcohol film sample. The obtained polyvinyl alcohol film sample was measured using a Swing-Albert meter. Thwing-Albert Instrument Company Place it on the oGage thickness gauge, record the thickness value across the width every 1 cm, and then measure the thickness value. The range is in 10cm increments (e.g. 0~10cm, 1~11cm, ..., 270~280cm, etc. (e.g., subtract the maximum value M and the minimum value m of the thickness difference of the obtained polyvinyl alcohol film sample. The thickness deviation within 10 cm was calculated by the above formula. In a preferred embodiment, 10 cm of polyvinyl alcohol film is The thickness deviation within the range is 3.0 μm or less. Specifically, for example, 3 μm or less, 2.5 μm or less In a more preferred embodiment, the polyimide of the present invention is The thickness deviation of the vinyl alcohol film within 10 cm is less than 2.0 μm.

[0027] The retardation of the polyvinyl alcohol film is due to the complex crystals of the polyvinyl alcohol itself. This is due to the refraction, and the refraction phenomenon is affected by the crystallinity of polyvinyl alcohol. After staining and color development, the difference in refraction causes the color to have different shades. The deviation of the phase difference uniform coefficient must be controlled within a certain range. " is a polyvinyl alcohol film sample taken with a width of t mm and a machine direction of 50 mm. The t value is determined by the width of the polyvinyl alcohol film sample. The vinyl alcohol film sample was placed on the X-stage, a phase difference measuring instrument manufactured by Photoron. The width of the measurement range was set to 20 cm and the flow direction to 30 cm. The phase difference uniformity coefficient is calculated by obtaining the difference average value x and the standard deviation y. The coefficient of difference (%) is y / x*100%. In a preferred embodiment, polyvinyl alcohol is The phase difference uniformity coefficient of the film is between 4.7 and 24.7. .7, 6.7, 8.7, 10.7, 12.7, 14.7, 16.7, 18.7, 20.7 , 22.7 or 24.7.

[0028] The "dyeing coefficient" described in this specification is the thickness deviation within 10 cm and the phase difference uniformity described above. The inventors control the thickness deviation and phase difference uniformity within a specific range. By doing so, the appearance of the film surface is adjusted to within a certain limit, and the occurrence of dye spots and density spots is prevented. In a preferred embodiment, the staining factor is between 7 and 70. Specifically, for example, 7, 10, 13, 16, 19, 21, 24, 27, 30, 33, 36 , 39, 41, 44, 47, 50, 53, 56, 59, 61, 64, 67 or 70 In a more preferred embodiment, the polyvinyl chloride of the present invention is a copolymer of The dyeing coefficient of the alcohol film is between 7 and 27.

[0029] If the moisture distribution in the polyvinyl alcohol film is not uniform, brittle fracture may occur during the stretching process. The moisture content uniformity coefficient described in this specification is likely to occur, and the stretchability of the film is also deteriorated. " is a measurement of the weight of a polyvinyl alcohol film 100 mm long and 100 mm wide taken and weighed on a balance. Weigh out the weight of Sg, place the polyvinyl alcohol film in a dryer at 83 °C and dry it for 20 min. After that, take it out and put it in a drying dish to cool for 5 minutes, weigh Wg, and then measure its moisture content. Calculate. That is, moisture content (%) = (SW) / S * 100%. Divide the alcohol film into 5 equal parts widthwise and take samples in order, measure the moisture content, and then average the number Calculate m and standard deviation n, then calculate the moisture content uniformity coefficient. That is, the moisture content uniformity coefficient (% )=n / m*100%. In a preferred embodiment, the polyvinyl alcohol film The standard deviation of the moisture content is less than 0.3%. Specifically, for example, less than 0.3%, 0.25%, less than, less than 0.2%, less than 0.15% or less than 0.1%.

[0030] In the stretching process of polarizing plates, in order to avoid breakage during stretching, in addition to the phase difference uniformity, the moisture content Uniformity is also an important control index. The "modulus of rupture" described in this specification is the above-mentioned phase The product of the difference uniformity factor and the moisture content uniformity factor described above. The modulus of rupture of the alcohol film is less than 130. Specifically, for example, less than 130, 12 Less than 0, Less than 110, Less than 100, Less than 90, Less than 80, Less than 70, Less than 60, Less than 50 , less than 40, less than 30, less than 20, and less than 10.

[0031] In another aspect, the present invention also provides a method for producing the polyvinyl alcohol film. The process includes: (a) subjecting a polyvinyl alcohol resin to a temperature of 100° C. or higher and a pressure of 1 atm. Dissolve the mixture under the above pressure for at least 5 hours to form a polyvinyl alcohol solution. (b) A polyvinyl alcohol solution is extruded at 20 kg / cm 2 Under back pressure of (c) forming a film on a plurality of drying rolls; The distribution of the inlet and outlet temperatures of the first drying roll heat source is less than 4°C, and the (d) forming a film by the drying roll described above; and then drying in a dryer to obtain a polyvinyl alcohol film. include.

[0032] The dissolving process involves dissolving the polyvinyl alcohol resin at a temperature of 100°C or higher and a pressure of 1 atm or higher. Dissolve under pressure for at least 5 hours to form a polyvinyl alcohol solution for later preparation. The polyvinyl alcohol film is made from the stock solution. For example, the temperature at which the polyvinyl alcohol resin is dissolved is preferably 100° C. or higher. , for example, 100°C, 115°C, 120°C, 125°C or 130°C. The pressure for dissolving the alcohol-based resin is preferably 1 atm or more. m, 1.51 atm, 2 atm, 2.5 atm, or 3 atm. The dissolution time for dissolving the coal resin is preferably at least 5 hours. For example, at least 5 hours, at least 6 hours, at least 7 hours, at least 8 hours, or At least 9 hours.

[0033] The above-mentioned polyvinyl alcohol resin is produced by polymerization of vinyl ester resin monomers. The vinyl ester resin is formed and then saponified. Ester resin monomers include vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, These include vinyl esters such as vinyl pentanoate or vinyl octanoate, but the present invention is not limited to these. The vinyl acetate is preferably vinyl acetate. Copolymers formed by copolymerizing vinyl ester derivatives with the vinyl ester resin monomers described above may also be used. The olefin compounds include ethylene, propylene, butylene, etc. However, the present invention is not limited thereto. The acrylate derivatives include acrylic acid, methyl acrylate, etc. , ethyl acrylate, n-propyl acrylate, isopropyl acrylate or acrylic acid n-butyl, but the present invention is not limited thereto.

[0034] The saponification degree / alkalinization degree of the above-mentioned polyvinyl alcohol resin is 98.00% or more. It is preferable that the content of the fluorine-containing polymer is 98.00%, which provides good optical properties. , 98.50%, 99.00%, 99.50%, 100.00%, preferably 98. 00%~99.00%.

[0035] The degree of polymerization of the above-mentioned polyvinyl alcohol is between 1500 and 5000. Specifically, For example, 1500, 2000, 2500, 3000, 3500, 4000, 4500 or 5 The range is between any two values ​​between 1,000 and 1,500. However, if the degree of polymerization exceeds 5000, it becomes difficult to dissolve.

[0036] Extrusion molding is done by extruding a polyvinyl alcohol solution at 20 kg / cm 2 More than 10 ... The mixture is discharged through a mold below to form a preformed polyvinyl alcohol film. According to at least one embodiment, the back pressure of the mold is 20 kg / cm 2 That's all. For example, 20kg / cm 2 More than 25kg / cm 2 More than 30kg / cm 2 That's all, 35kg / cm 2 or more than 40kg / cm 2 or more, preferably 23 kg / cm 2 End , more preferably 25 kg / cm 2 The inventors have found that the polyvinyl alcohol film It was discovered that the thickness deviation of the mold is determined by the pressure at which the material is discharged from the mold. In order to make the discharge uniform in the width direction, it is common to increase the discharge pressure. In this example, the discharge pressure is 25kg / cm 2 Increase to above.

[0037] The moisture adjustment is performed by drying the mixture under back pressure through a mold 110 as shown in the drying process 100 of FIG. The discharged polyvinyl alcohol solution is dried by a plurality of drying rolls (120 is a first drying roll, 30 is the second drying roll, 140 is the third drying roll, and 150 is the Nth drying roll), The film is heated and formed. The phase difference uniformity and moisture content uniformity are determined by the drying process during film formation. The temperature is determined by the uniformity of the heat received by the polymer, so the polyvinyl alcohol molecular chains under tension are completely If the material is not completely stretched and the heat is not uniform across the width, the crystallinity will vary. However, the birefringence decreases, which affects the subsequent dyeing and the coloring of the crosslinking between the iodine solution and the dye. To avoid this problem, it is necessary to stabilize the supply of heat source as well as the drying roll for film formation. The path is also precisely designed, from the drying roll heat source inlet 210 to the drying roll heat source outlet 220. The temperature of the entire width of the drying roll was measured by measuring the temperature along the drying roll path every 20 cm up to the It is necessary to make the temperature of the drying roll as uniform as possible. In addition, the standard deviation of the temperature in the width direction of the first drying roll 120 is controlled within a certain range. It is also necessary to control the drying. The "first drying roll" described in this specification refers to a roll that This refers to the drying roll that the polyvinyl alcohol solution discharged under back pressure first comes into contact with. According to at least one embodiment, in order to obtain a film with good phase difference uniformity, multiple drying steps are performed. The difference between the inlet and outlet temperatures of the roll heating source should be less than 4°C, and the standard deviation in the width direction should be According to at least one embodiment, the temperature of the first drying roll in the cross-machine direction is less than 4° C. The standard deviation is less than 4°C, preferably less than 3°C, more preferably less than 2°C.

[0038] The drying process is carried out by drying the polyvinyl alcohol film after the heating and film formation by the drying roll. The film is dried in a dryer to produce polyvinyl acetate with low dyeing uniformity and high tear resistance. This results in an alcohol film.

[0039] The polyvinyl alcohol film of the present invention can also be produced as an optical film. The term "optical film" used in this specification includes polarizing films and blue light blocking films. , filter lenses, etc., but the present invention is not limited to these. The polyvinyl alcohol film is considered to be a polarizing film.

[0040] In a preferred embodiment, the method for producing a polarizing film (also called a polarizing plate) includes the following steps: Polyvinyl alcohol film is swelled, dyed, stretched, color-complemented, dried and triacetylated. A polarizing film can be obtained by laminating a polyethylene terephthalate (TAC) film.

[0041] When the polyvinyl alcohol film is further used for the production of an optical film, it is stretched and For example, in the manufacturing process of polarizing film, 3 - , I 5 - Polyvinyl alcohol film is dyed with an aqueous solution of boric acid containing iodide ions. In order to achieve this, boric acid crosslinks with the amorphous areas of polyvinyl alcohol. After the binding action occurs, the iodide ions are fixed and the elution of the iodide ions can be prevented. Cut. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples. The examples are intended to help make the invention more readily understandable and are not intended to limit the scope of the invention. Please understand that this is not a guarantee.

[0043] Production of polyvinyl alcohol film Polyvinyl alcohol resin is heated and dissolved to form a polyvinyl alcohol solution, The polyvinyl alcohol solution is extruded and molded, and the polyvinyl alcohol solution is passed through a drying roll. The solution was used to form a film, and the moisture content was adjusted. The polyvinyl alcohol film sample was then dried in a dryer. A vinyl alcohol film is obtained.

[0044] Polarizing film manufacturing The polyvinyl alcohol film was immersed in water at 30° C. to swell it, and the film was then stretched in the machine direction (M D) uniaxially stretched to 2.0 times its original length, then 0.03 mass percent iodide was added. The polymer was immersed in an aqueous solution at 30° C. containing iodine and 3 mass percent potassium iodide. The vinyl alcohol film was stretched to 3.3 times its original length and then diluted with 3% by weight yttria. The specimen was immersed in an aqueous solution of potassium fluoride and 3 mass percent boric acid at 30°C to recover its original length. The film is then stretched further to 3.6 times its original length. % boric acid at 60°C, and then stretched to 6.0 times its original length. Then, it is immersed in a 3 mass percent potassium iodide aqueous solution for 15 seconds, and then After drying at 60°C for 4 minutes, a polarizing film can be obtained.

[0045] The following are the test control variables and the color uniformity and tear resistance measurements for Examples 1 to 4 and Comparative Examples 1 to 3. See Table 1 for the results.

[0046] [Table 1]

[0047] In this embodiment, the evaluation method for the dye uniformity of the polarizing plate includes the following:

[0048] Single piece inspection The manufactured polarizing plate was cut into a sample with a width of 30 cm and a flow direction of 30 cm, and the area The specimen was placed in a darkroom with a stage equipped with a 14,000 cd light source and a transparent A polarizing plate with a 43% polarizing efficiency is attached in advance (the person measuring is positioned on the backlight side). The person measuring the backlight side holds the sample at a height of about 1 m from the stage. The specimen surface is observed by tilting the stage at an angle of 30 to 60 degrees from the horizontal.

[0049] Two-piece inspection Place another layer of polarizing plate (transmittance 43%) on the stage and try again in the same way as above. Judge the staining of the material.

[0050] Based on the visual judgment results of single-piece and double-piece inspections, the coloring state of the polarizing plate is classified into three grades. If it passes the two-piece inspection, it is marked with "◎", and if it passes the single-piece inspection, it is marked with "○". If the single piece fails the inspection, it will be marked as "X".

[0051] In this example, the evaluation method for the cutting of the polarizing film includes the following: As a standard, a polarizing film was expanded for 2 minutes at 30°C using an in-house polarizing film production tester. The polarizing film is then stretched to 2.0 times its original length in the first stretching. Then, at 30°C of staining solution (0.5 g / L of I 2 and 20 g / L KI) for 3 minutes, then The polarizing film is stretched for the second time to 3.0 times its original length. The third stretching was performed in the stretching tank (the solution consisted of 60 g / L KI and 60 g / L boric acid). The polarizing film is stretched to 5.5 times its original length, and the polarizing film is stretched three times. Observe whether the wire is disconnected.

[0052] It is noteworthy that in the prior art, polyvinyl alcohol films used in polarizing plates It is described that the retardation at the center in the width direction is 10 to 40 nm. Furthermore, it has been pointed out that when the phase difference is less than 10 nm, staining spots are likely to occur. However, as shown in Table 1, the retardation in the width direction is 10 to 40 as in Comparative Example 1. Even if a polyvinyl alcohol film with a thickness of 100 nm is used, the problem of dye spots still exists. There is.

[0053] According to Table 1, the polarizing filter manufactured by the polyvinyl alcohol film of the present invention From the viewpoint of the dyeing coefficient, the dyeing coefficients of Examples 1 to 4 are all between 7 and 70. Among them, the dyeing coefficients of Examples 1 and 2 are between 7 and 27, and the dyeing uniformity is excellent. On the other hand, the dyeing coefficients of Comparative Examples 1 to 3 all exceeded 70, and the dyeing uniformity of the polarizing plate was excellent. In the dyeing test, all of the pieces failed the test, and the dyeing uniformity was poor.

[0054] Next, from the viewpoint of the modulus of rupture, the modulus of rupture of each of Examples 1 to 4 is less than 130. In addition, no film breakage occurred in any of the films. The film breakage occurred during the polarizing plate breakage test, and the breakage resistance was The sex was bad.

[0055] In summary, the polyvinyl alcohol film of the present invention has a dye coefficient of 7 to 70, The dyeing coefficient is calculated by multiplying the thickness deviation within 10 cm by the phase difference uniformity coefficient, and is less than 130. It has a modulus of rupture, which is calculated by multiplying the phase difference uniformity coefficient by the moisture content uniformity coefficient, and has low dyeability. It is possible to simultaneously achieve color uniformity and high tear resistance.

[0056] All ranges provided herein are to be construed as including each specific range and allocation within the assigned range. This means that combinations of subranges between the assigned ranges are included. Unless otherwise stated, all ranges provided herein are inclusive of the range endpoints. For example, the range 1 to 5 specifically includes 1, 2, 3, 4, and 5, as well as 2 to 5, 3 to 5, 2 to 3, Includes secondary ranges such as 2-4, 1-4, etc.

[0057] All publications and patent applications referenced herein are hereby incorporated by reference. and for any and all purposes, each and every publication or patent application is hereby incorporated by reference. Each of the above-referenced publications is specifically and individually incorporated herein by reference. In the event of a conflict between any publication or patent application incorporated herein, , as set forth herein.

[0058] As used herein, the terms "including," "having," and "including" are open-ended and non-exclusive. The terms "a," "an," and "the" are understood to include the plural as well as the singular. The term "one or more" refers to "at least one" and therefore to a single It may include a property or a mixture / combination of properties.

[0059] Except in the procedural examples or where otherwise indicated, all references to amounts of ingredients and / or reaction conditions are All of the numbers can be modified in all instances by the term "about." The term "essentially not included" as used herein means that the value is within ±5% of the indicated value. The terms "free" or "substantially free" mean less than about 2% of a particular characteristic. Any element or feature explicitly described in this specification may be omitted from the claims. can be quantitatively excluded. [Explanation of symbols]

[0060] 100 Drying process 110 Mold 120 First drying roll 130 Second drying roll 140 3rd drying roll 150 Nth Drying Roll 210 Drying roll heat source inlet 220 Drying roll heat source outlet

Claims

1. having a dye coefficient of 7 to 70 and a modulus of rupture of less than 130; The dyeing coefficient is the product of the thickness deviation (unit: μm) within 10 cm and the phase difference uniformity coefficient, A polyvinyl alcohol film, wherein the rupture modulus is the product of the phase difference uniformity coefficient and the moisture content uniformity coefficient.

2. 2. The polyvinyl alcohol film of claim 1, wherein the dye coefficient is between 7 and 27.

3. 2. The polyvinyl alcohol film according to claim 1, wherein the thickness deviation within 10 cm is 3.0 μm or less.

4. 2. The polyvinyl alcohol film according to claim 1, wherein the phase difference uniformity coefficient is between 4.7 and 24.

7.

5. 10. The polyvinyl alcohol film of claim 1 further having a moisture content standard deviation of less than 0.3%.

6. 2. The polyvinyl alcohol film according to claim 1, wherein the thickness deviation within 10 cm is 2.0 μm or less.

7. (a) a dissolving step of dissolving a polyvinyl alcohol-based resin at a temperature of 100° C. or higher and a pressure of 1 atm or higher for at least 5 hours to form a polyvinyl alcohol solution; (b) The polyvinyl alcohol solution is extruded at 20 kg / cm 2 an extrusion molding process in which the mixture is discharged through a die under the above back pressure; (c) a moisture adjustment step in which a film is formed on a plurality of drying rolls, among which the first drying roll has a distribution of the inlet temperature and the outlet temperature of the heat source of less than 4° C., and a temperature standard deviation in the width direction of less than 4° C.; (d) a drying step of drying the polyvinyl alcohol film in a dryer after the film formation by the drying roll to obtain the polyvinyl alcohol film.

8. In the step (b), the back pressure of the mold is 25 kg / cm 2 8. The method of claim 7, performed as above.

Citation Information

Patent Citations

  • Polyvinyl alcohol film

    CN103992606A