Method and system for laser welding

The laser welding method addresses the issue of blowholes and cost in conductive wire joining by using a dual laser beam approach to maintain melting and prevent blowhole formation, improving joint strength and conductivity without additional materials.

JP2024157413APending Publication Date: 2024-11-07HONDA MOTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023071766
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Joining thick conductive wires or plates using a deoxidizing material increases processing costs and decreases electrical conductivity due to the formation of blowholes and insufficient strength in welded parts.

Method used

A laser welding method using a first laser beam to melt the workpiece, followed by a second laser beam to maintain the melting amount, reducing the first beam's output or using a specific wavelength and defocused laser light to prevent blowhole formation without the need for a deoxidizing material.

Benefits of technology

Reduces blowholes while preventing cost increases and maintaining electrical conductivity, enhancing joint strength without the use of deoxidizing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157413000001_ABST
    Figure 2024157413000001_ABST
Patent Text Reader

Abstract

To provide a method for laser welding that can reduce blow holes while preventing increase in processing cost and decrease in electrical conductivity.SOLUTION: A method for laser welding that performs welding by irradiating a processing object with a laser beam includes: a first step of irradiating a processing object with a first laser beam LL1 to melt the processing object; and a second step of irradiating a molten region melt in the first step with a second laser beam LL2 different from the first laser beam LL1 to maintain a molten amount in the molten region. As shown in Figure 11, for example, when a prescribed time is elapsed from the start of irradiation with the first laser beam LL1, the method decreases output of the first laser beam LL1 by a specified quantity and sets output of the second laser beam LL2 to be smaller than the output of the first laser beam LL1.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laser welding method and a laser welding system. [Background technology]

[0002] Electrical equipment such as rotating electrical machines and power conversion devices need to pass large currents with low resistance, and so thick conductor wires such as rectangular wires and conductor plates are used, which are joined together (see, for example, Patent Document 1). When tough pitch copper, which has a relatively high oxygen content, is used for such conductor wires and conductor plates, many blowholes are formed in the welded parts, causing problems such as insufficient strength and increased electrical resistance. Therefore, the welding method described in Patent Document 1 makes it possible to perform welding with reduced blowholes by adding a filler material (deoxidizer) containing phosphorus while melting the conductors to be joined. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 7162144 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the joining method using a deoxidizer increases the joining cycle time and the material cost of the deoxidizer, which increases the processing cost.The deoxidizer also reduces the electrical conductivity. [Means for solving the problem]

[0005] A laser welding method according to one embodiment of the present invention is a laser welding method for welding an object to be processed by irradiating a laser light thereto, the method including: a first step of irradiating the object to be processed with a first laser light to melt the object; and a second step of irradiating a melted area melted by the first step with a second laser light different from the first laser light to maintain a melt amount of the melted area, the method including: (A) a first laser light configuration for reducing an output of the first laser light by a predetermined amount and setting an output of the second laser light lower than an output of the first laser light after a predetermined time has elapsed from the start of irradiation of the first laser light; or (B) a second laser light configuration for the first laser light including a laser light having a first wavelength of 800 nm or more and 1200 nm or less and a first output, and the second laser light including a laser light having the first wavelength and an output lower than the first output and / or in a defocused state. A laser welding system according to one embodiment of the present invention includes a first laser light generating device that generates a first laser light, a second laser light generating device that generates a second laser light different from the first laser light, an optical device that irradiates the first laser light and the second laser light to an object to be processed, and a control device that controls operation of the first laser light generating device, the second laser light generating device, and the optical device, wherein the control device controls operation of the first laser light generating device, the second laser light generating device, and the optical device so as to irradiate the object to be processed with the first laser light to melt the object, and then irradiate the molten melt area with the second laser light to maintain the melt amount of the melt area. Effect of the Invention

[0006] According to the present invention, it is possible to reduce blowholes while preventing an increase in processing costs and a decrease in electrical conductivity. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a block diagram showing a schematic configuration of a laser welding system according to the present embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of an object to be processed by laser welding. [Diagram 3] FIG. 3 is a flowchart illustrating control of laser welding in the embodiment. [Figure 4] FIG. 4 is a schematic diagram showing the first scanning mode. [Diagram 5] FIG. 5 is a view of the end portion where the molten region is formed, viewed from the side of the conductor. [Figure 6] FIG. 6 is a schematic diagram showing the second scanning mode. [Figure 7] FIG. 7 is a view of the end portion where the merged fusion region is formed, viewed from the side of the conductor. [Figure 8] FIG. 8 is a graph qualitatively illustrating the relationship between the laser light irradiation and the amount of melting and the amount of blowholes. [Figure 9] FIG. 9 is a diagram illustrating the release of a blowhole into the atmosphere. [Figure 10] FIG. 10 is a diagram illustrating the first modified example. [Figure 11] FIG. 11 is a diagram illustrating the second modification. [Figure 12] FIG. 12 is a diagram showing an example of reducing the output in multiple stages. [Figure 13] FIG. 13 is a diagram showing an example of continuously decreasing the output. [Figure 14] FIG. 14 is a diagram illustrating the third modified example. [Figure 15] FIG. 15 is a flowchart illustrating the fourth modification. [Figure 16] FIG. 16 is a diagram showing a case where plate materials are overlapped and welded. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiment of the present invention will be described with reference to the drawings. The following description and drawings are examples for explaining the present invention, and appropriate omissions and simplifications have been made for clarity of explanation. In addition, in the following description, the same or similar elements and processes are given the same reference numerals, and duplicate explanations may be omitted. Note that the contents described below are merely examples of the embodiment of the present invention, and the present invention is not limited to the following embodiment, and can be implemented in various other forms.

[0009] FIG. 1 is a block diagram showing a schematic configuration of a laser welding system 1 according to the present embodiment. The laser welding system 1 includes a first laser beam generating device 10, a second laser beam generating device 11, an optical device 12, a control device 13, and an optical fiber 14. Each of the laser beam generating devices 10 and 11 includes a laser oscillator. The laser beam generating device 10 generates a first-wavelength laser beam having a wavelength of 800 nm or more and 1200 nm or less. The laser beam generating device 11 generates a second-wavelength laser beam having a wavelength of 400 nm or more and 500 nm or less.

[0010] The optical fiber 14 guides the laser light output from the laser light generating devices 10, 11 to the optical device 12. The optical device 12 is an optical system for irradiating the laser light input from the laser light generating devices 10, 11 toward the processing object 15. Although not shown, the optical device 12 includes a collimating lens, a condensing lens, a mirror, a filter, etc. The optical device 12 is configured to be able to scan the laser light on the processing object 15.

[0011] The control device 13 controls the operations of the laser light generating devices 10, 11 and the optical device 12. The control device 13 includes a CPU, memory (RAM, ROM, etc.), and controls the laser welding system 1 by executing a program stored in the memory with the CPU. The control device 13 controls the output of laser light from the laser light generating devices 10, 11. The control device 13 controls the focal position of the laser light from the optical device 12 and the scanning trajectory.

[0012] The above-mentioned first-wavelength laser light having a wavelength of 800 [nm] or more and 1200 [nm] or less is a laser light in a wavelength region generally called IR laser light. The second-wavelength laser light having a wavelength of 400 [nm] or more and 500 [nm] or less is a laser light in a wavelength region generally called BLUE laser light. When comparing the first-wavelength laser light and the second-wavelength laser light, the first-wavelength laser light has a small spot diameter and a high power density, but a low absorption rate in the processing object 15. On the other hand, the second-wavelength laser light has a large spot diameter and a low power density, but a high absorption rate in the processing object 15.

[0013] Therefore, when the workpiece is scanned with a laser beam including a first-wavelength laser beam and a second-wavelength laser beam, the area on the scanning path is irradiated with the second-wavelength laser beam having a larger spot diameter, and then with the first-wavelength laser beam. That is, the first-wavelength laser beam having a higher output density is irradiated after the second-wavelength laser beam having a lower output density but a higher absorption rate, thereby improving the occurrence of spatters and blowholes. In this embodiment, the workpiece 15 is melted using a laser beam including a first-wavelength laser beam and a second-wavelength laser beam, and the occurrence of blowholes is further reduced by employing a welding method as described later.

[0014] FIG. 2 is a diagram showing an example of a workpiece 15 to be processed by laser welding. FIG. 2 is a diagram showing a part of a stator coil 21 provided in a stator core 20 of a motor. The stator core 20 is formed by laminating electromagnetic steel sheets. A plurality of slots 200 are formed in the stator core 20. A stator coil 21 is disposed in each slot 200. The stator coil 21 is formed by connecting a plurality of segment coils. In the example shown in FIG. 2, a pair of segment coils 21A, 21B connected to each other among the plurality of segment coils that constitute the stator coil 21 is shown.

[0015] The segment coil 21A is inserted into the slot 200a, and the segment coil 21B is inserted into the slot 200b. The end 211a of the segment coil 21A is juxtaposed adjacent to the end 211b of the segment coil 21B. The end 211a and the end 211b are joined to each other by laser welding. The laser light is irradiated to the end faces of the end 211a and the end 211b.

[0016] The stator coil 21 is generally made of oxygen-free copper having a low oxygen content. When tough pitch copper is used instead of oxygen-free copper to reduce costs, as described in Patent Document 1, there is a problem that many blowholes are formed in the welded portion. Tough pitch copper has a higher oxygen content than oxygen-free copper. For example, oxygen-free copper contains 10 ppm or less, while tough pitch copper contains about 300 to 500 ppm of oxygen. When tough pitch copper melts, the oxygen contained therein combines with hydrogen to generate water vapor, which is considered to be the cause of the generation of blowholes. In this embodiment, the generation of blowholes is suppressed by performing laser welding by the method described below.

[0017] FIG. 3 is a flow chart for explaining the control of laser welding by the control device 13. In step S101, the control device 13 sets the irradiation conditions of the laser light to be irradiated to the processing object 15 to the first irradiation conditions. In the first irradiation conditions in the embodiment, the first-wavelength laser light of the laser light generating device 10 and the second-wavelength laser light of the laser light generating device 11 are irradiated simultaneously. Furthermore, the output of the second-wavelength laser light is set to an output that maintains the melting amount M of the combined melting region S3 at a predetermined melting amount Mth, as described later. On the other hand, the output of the first-wavelength laser light is set to an output that can melt the processing object 15 (coil conductor) when the first-wavelength laser light and the second-wavelength laser light of the above-mentioned output are irradiated. For example, it is set to an output that can melt the coil conductor only with the first-wavelength laser light. Hereinafter, the laser light under the first irradiation conditions will be referred to as the first laser light LL1.

[0018] In step S102, the first laser light LL1 is irradiated onto the end faces of the ends 211a and 211b of the segment coils 21A and 21B in a first scanning mode as shown in Fig. 4. Fig. 4 is a schematic diagram showing the first scanning mode, showing the end faces of the ends 211a and 211b as viewed from above (top view). Arrows R1 and R2 indicate the scanning trajectory of the first laser light LL1.

[0019] In the first scanning mode, first, a spot of the first laser light LL1 is moved back and forth over the end face of one end 211a as shown by the scanning trajectories R1 and R2. This melts the conductor of the end 211a to form a melted region S1. Next, a spot of the first laser light LL1 is moved back and forth over the end face of the other end 211b as shown by the scanning trajectories R1 and R2. This melts the conductor of the end 211b to form another melted region S2 on the end face of the end 211b.

[0020] As a pattern for alternately scanning the ends 211a and 211b, the ends 211a and 211b may be alternately scanned back and forth once each, such as 211a → 211b → 211a → 211b..., or the ends 211a and 211b may be alternately scanned back and forth multiple times, such as 211a → 211a → 211b → 211b → 211a → 211a → 211b → 211b.... Also, a combination of once and multiple times may be used.

[0021] 5 is a view of the ends 211a and 211b in which the melted regions S1 and S2 are formed, viewed from the conductor side. By scanning the end face of the end 211a back and forth with the first laser light LL1, a part of the end 211a melts to form the melted region S1. Next, by scanning the end face of the end 211b back and forth with the first laser light LL1, a part of the end 211b melts to form the melted region S2. Each time the laser light irradiation to each of the ends 211a and 211b is repeated, the melting amount of the melted regions S1 and S2 increases. As the ends 211a and 211b melt, blowholes BH are generated. In this embodiment, bubbles generated in the melted region and pores generated in the welded part are unified and referred to as blowholes.

[0022] Returning to FIG. 3, in step S103, the control device 13 judges whether the number of reciprocating scans N1 in the first scanning mode (reciprocating scan) for each end 211a, 211b has reached a preset number N1th. The melting amount of each melted region S1, S2 shown in FIG. 5 increases with an increase in the number of scans N1, and the melted regions S1, S2 that were separated from each other merge into one. The melted region S3 indicated by the two-dot chain line indicates the melted region after the merger, and will be referred to as the merged melted region S3 below. The merged melted region S3 is formed across the end face of the end 211a and the end face of the end 211b.

[0023] The predetermined number of times N1 in step S103 is set in consideration of the timing when the melting amounts of the melted regions S1, S2 formed at the ends 211a, 211b increase and the melted regions S1, S2 merge to form a merged melted region S3. That is, the predetermined number of times N1th is set to a number of times at which the merged melted region S3 is always formed when the reciprocating scan is performed the predetermined number of times N1th.

[0024] The process of step S103 is repeated until the number of scans for each end 211a, 211b reaches a predetermined number N1th, and if it is determined in step S103 that N1≧N1th, the process proceeds to step S104. In step S104, the first laser light LL1 is irradiated to the entire merged melting region S3 in a second scanning form as shown in FIG. 6. In the second scanning form, the first laser light LL1 is irradiated to each end 211a, 211b in a circular scanning trajectory as shown by the dashed line R3 so as to straddle the boundary between the adjacent ends 211a, 211b. With the irradiation of the first laser light LL1, the melting amount of the merged melting region S3 increases. FIG. 7 is a view of the end 211a, 211b in which the merged melting region S3 is formed, viewed from the conductor side. With the increase in the melting amount M of the merged melting region S3, the amount of blowholes BH that are generated also increases.

[0025] In step S105 in Fig. 3, the control device 13 judges whether the number of scans N2 in the second scanning mode has reached a predetermined number N2th. In this case, the predetermined number N2th is set to the number of times at which the melting amount M of the merged melting region S3 reaches a predetermined melting amount Mth. The process of step S105 is repeated until the number of scans N2 reaches the predetermined number N2th, and if it is judged in step S105 that N2 ≥ N2th, the process proceeds to step S106.

[0026] In step S106, the control device 13 changes the setting of the irradiation conditions of the irradiated laser light from the first irradiation conditions to the second irradiation conditions. The second scanning form is continued. In the second irradiation condition in the embodiment, the first wavelength laser light of the laser light generating device 10 is stopped, and only the second wavelength laser light of the laser light generating device 11 is irradiated. The output of the second wavelength laser light is set to the same as that in the first irradiation condition (output that maintains the melt amount M of the merged melt region S3 at a predetermined melt amount Mth). Hereinafter, the laser light under the second irradiation condition will be referred to as the second laser light LL2.

[0027] Here, the output power for maintaining the merged melt region S3 corresponds to the output power for maintaining the melt amount M of the merged melt region S3 without increasing it when the merged melt region S3 is irradiated with the second laser beam LL2 in the second scanning pattern shown in Fig. 6. In this case, no new melting of the ends 211a and 211b occurs, and the melt amount M of the merged melt region S3 is maintained at a predetermined melt amount Mth.

[0028] In step S107, the control device 13 judges whether the number of scans N3 by the second laser light LL2 has reached a predetermined number N3th. The process of step S107 is repeated until the number of scans N3 reaches the predetermined number N3th, and if it is judged in step S107 that N3≧N3th, the process proceeds to step S108. In step S108, the irradiation of the second laser light LL2 is stopped, and a process of ending the laser welding is performed, and a series of laser welding processes is ended.

[0029] 8 is a graph qualitatively explaining the relationship between the laser light irradiation and the melting amount and the blowhole amount. The upper graph in the figure shows the time transition of the melting amount M and the blowhole amount Vb, and the lower graph in the figure shows the time transition of the laser light output W. Irradiation with the first laser light LL1 is performed from time t=0 to time t2, and irradiation with the second laser light LL2 is performed from time t2 to time t3. The first laser light LL1 includes the first-wavelength laser light IR with output W1 and the second-wavelength laser light Bu with output W2. On the other hand, the second laser light LL2 includes only the second-wavelength laser light Bu with output W2.

[0030] Line L1 indicates the melt amount M, and line L2 indicates the estimated blowhole amount Vb. The slope of line L1 indicating the melt amount M changes (increases) at time t1. This is believed to be due to the fact that the melted region spreads over almost the entire end faces of the ends 211a and 211b, and the laser light absorption rate of the processing target increases. When the irradiated laser light is switched from the first laser light LL1 to the second laser light LL2 at time t2, the increase in the melt amount M stops and is maintained at a predetermined melt amount Mth.

[0031] It is believed that the amount of blowholes BH contained in the molten region (blowhole amount Vb) increases depending on the amount M of newly melted conductor. Therefore, from the start of welding until approximately time t2 when the melting amount M is increasing, the blowhole amount Vb increases with time. On the other hand, when the irradiated laser light is switched from the first laser light LL1 to the second laser light LL2, only the second-wavelength laser light Bu with output W2 is irradiated to the molten region (combined molten region S3). Since the spot diameter of the second-wavelength laser light Bu is large and the power density is low, no new melting of the conductor occurs, and the molten state of the molten region is maintained.

[0032] In a state where no new melting of the conductor occurs and the melting amount M is maintained constant, no new blowholes BH are generated. On the other hand, the blowholes BH already present in the melting region (combined melting region S3) move toward the surface of the combined melting region S3 due to buoyancy as shown in FIG. 9. Then, the blowholes BH that reach the surface of the combined melting region S3 are released into the atmosphere from the surface of the combined melting region S3. In a state where the melting amount M is maintained constant, the blowhole amount Vb of the combined melting region S3 decreases as shown by line L2 in FIG. 8 due to the release of the blowholes BH into the atmosphere. The irradiation time of the second laser light LL2, i.e., the time during which the melting amount M is maintained constant (Mth), is set according to the release speed of the blowholes BH.

[0033] As described above, in this embodiment, the second laser beam LL2 is irradiated to the melting region to maintain the melting amount M and promote the release of the blowholes BH into the atmosphere, thereby reducing the blowholes BH in the combined melting region S3. As a result, the amount of blowholes BH remaining in the welded portion of the ends 211a and 211b (blowhole amount Vb) can be reduced more than ever before, and the joining strength of the welded portion can be improved. In addition, since a deoxidizing material is not used as in the technology described in Patent Document 1, an increase in processing costs and a decrease in electrical conductivity can be prevented.

[0034] In the above-described embodiment, the first laser light LL1 includes the first-wavelength laser light IR having a wavelength of 800 [nm] or more and 1200 [nm] or less, and the second-wavelength laser light Bu having a wavelength of 400 [nm] or more and 500 [nm] or less, and the second laser light LL2 is a laser light composed only of the second-wavelength laser light Bu. However, the configurations of the first laser light LL1 and the second laser light LL2 are not limited to these. Below, other examples (Modifications 1 to 4) will be described. In addition, in Modifications 1 to 3, the flow chart related to the control as shown in FIG. 3 is omitted, but the irradiation conditions and the like may be appropriately changed according to the contents of the modification.

[0035] (Variation 1) FIG. 10 is a diagram for explaining the first laser beam LL1 and the second laser beam LL2 in the first modification. In the first modification, the second laser beam LL2 also has a configuration including the first wavelength laser beam IR and the second wavelength laser beam Bu. In the first laser beam LL1, the output of the first wavelength laser beam IR is W1, and in the second laser beam LL2, the output of the first wavelength laser beam IR is W11 (<W1). Further, since the second laser beam LL2 includes the first wavelength laser beam IR with the output W11, the output of the second wavelength laser beam Bu is set to W21 (<W2). By setting in this way, the total output of the second laser beam LL2 can be set to an output that maintains the melting amount M of the combined melting region S3 at a predetermined melting amount Mth. When blowholes are generated at a deep position in the melting region, with only the second wavelength laser beam Bu, the heat input to the deep part of the melting region is insufficient, and the blowholes solidify before being released. Therefore, by reducing the output of the first wavelength laser beam IR to such an extent that new blowholes are not generated (output W11) and irradiating, the melting state at a deep position can be maintained and the blowholes can be released.

[0036] Further, instead of reducing the output of the first wavelength laser beam IR in the second laser beam LL2, the first wavelength laser beam IR may be irradiated in a defocused state. By being in a defocused state, the spot diameter of the first wavelength laser beam IR expands and the output density decreases. Therefore, energy can be input while preventing new melting of the conductor by the first wavelength laser beam IR. Note that not only the first wavelength laser beam IR but also the second wavelength laser beam Bu may be defocused simultaneously.

[0037] Further, in the second laser beam LL2, the output of the first wavelength laser beam IR may be reduced and it may be in a defocused state. Furthermore, regarding the output of the second wavelength laser beam Bu included in the second laser beam LL2, it may also be made lower than the output of the second wavelength laser beam Bu included in the first laser beam LL1.

[0038] (Second modification) 11 is a diagram illustrating the first laser light LL1 and the second laser light LL2 in Modification 2. In Modification 2, the output of the first wavelength laser light IR included in the first laser light LL1 of Modification 1 (FIG. 10) described above is reduced by a predetermined amount ΔW from output W1 to W12 (W1>W12>W11) at time t1. The other configurations are the same as those of Modification 1 described above.

[0039] It is known that the absorptivity of the laser light increases as the temperature of copper, which is the processing target, increases, and that the absorptivity increases stepwise when copper changes from a solid state to a molten state. Time t1 is a timing set in accordance with the increase in the absorptivity of the laser light, and the output of the first-wavelength laser light IR contained in the first laser light LL1 is reduced from W1 to W12 in accordance with this timing. When the absorptivity of the laser light increases, melting by the first laser light LL1 increases rapidly. Therefore, in the second modification, in order to suppress a sudden increase in blowholes due to such a sudden increase in melting, the output of the first laser light LL1 is reduced by a predetermined amount ΔW.

[0040] In FIG. 11, the output of the first laser light LL1 is reduced by a predetermined amount ΔW in one step, but as shown in FIG. 12, it may be reduced in two steps, each step being ΔW / 2. Of course, it may be reduced in three or more steps. Furthermore, as shown in FIG. 13, the output of the first laser light LL1 may be reduced continuously and smoothly by a predetermined amount ΔW. As a result, it is possible to more appropriately cause the output of the first laser light LL1 to follow the change in the absorptance, and it is possible to more effectively suppress the occurrence of blowholes.

[0041] 11 and 12, one period of irradiation combining the irradiation of the end 211a with a reciprocating movement (reciprocating scanning) and the irradiation of the end 211b with a reciprocating movement (reciprocating scanning) is defined as one unit, and the output is reduced every n units (n=1, 2, 3, . . .) In this manner, by reducing the output in cycle units, the melted state of each end can be made uniform.

[0042] In addition, with regard to Figure 8 of the embodiment, similar to the cases of Figures 11 to 13 for Figure 10, at time t1, the output of the first wavelength laser light IR contained in the first laser light LL1 may be reduced stepwise or continuously from W1 to W12.

[0043] (Variation 3) 14 is a diagram illustrating the first laser light LL1 and the second laser light LL2 in Modification 3. In Modification 3, each of the first laser light LL1 and the second laser light LL2 is composed of only the first-wavelength laser light IR. The output of the first-wavelength laser light IR in the first laser light LL1 is set to W13. The output W13 may be the same as the output W1 shown in FIG. 8, or may be set to be slightly higher. The output of the first-wavelength laser light IR in the second laser light LL2 is set to W14. In addition, the first-wavelength laser light IR is defocused to increase the spot diameter, thereby reducing the output density of the first-wavelength laser light IR.

[0044] In this manner, in the third modification, the second laser light LL2 is composed of only the first-wavelength laser light IR, but the output is reduced and the output density is also reduced by defocusing, so that the melting amount M of the merged melted region S3 is maintained constant. The first-wavelength laser light IR of the second laser light LL2 may be configured to only have its output reduced, or may simply be in a defocused state. Also, in the third modification of FIG. 14, similarly to the cases of FIG. 11 to FIG. 13 with respect to FIG. 10, the output of the first-wavelength laser light IR included in the first laser light LL1 may be reduced from W1 to W12 in a stepwise or continuous manner at time t1.

[0045] (Variation 4) Fig. 15 is a flowchart for explaining the modified example 4. The flowchart in Fig. 15 is obtained by deleting steps S103, S104, and S105 from the flowchart in Fig. 3 and adding step S113. The processing of the steps other than step S113 is the same as the processing of the steps with the same reference numerals in Fig. 3. The following mainly describes the steps after step S113.

[0046] In step S102, as described above, irradiation of the first laser light LL1 by the first scanning pattern is started on the end faces of the ends 211a and 211b of the segment coils 21A and 21B. The melting amounts of the melted regions S1 and S2 shown in FIG. 5 increase with an increase in the number of scans N1. Then, the melted regions S1 and S2 that were separated from each other merge into one, forming a merged melted region S3 that spans the end faces of the ends 211a and 211b.

[0047] In step S113, the control device 13 judges whether the number of scans N1 in the first scanning mode has reached a predetermined number of scans Nth1. This predetermined number of scans Nth1 is set to the number of scans at which the melting amount M of the merged melting region S3 reaches a predetermined melting amount Mth. The process of step S113 is repeated until the number of scans N1 reaches the predetermined number of scans Nth1, and if it is judged in step S113 that N1≧Nth1, the process proceeds to step S106.

[0048] In step S106, the control device 13 changes the setting of the irradiation condition of the irradiated laser light from the first irradiation condition (first laser light LL1) to the second irradiation condition (second laser light LL2). The first scanning form is continued as the scanning form. In step S107, it is determined whether the number of scans N3 by the second laser light LL2 has reached a predetermined number of scans N3th, and if it is determined that N3≧N3th, the process proceeds to step S108. In step S108, the irradiation of the second laser light LL2 is stopped, and a process of ending the laser welding is performed, and a series of laser welding processes is ended.

[0049] In the laser beam scanning control shown in Fig. 3, when the melted region becomes the merged melted region S3, the scanning is switched from the reciprocating scanning (first scanning form) to the circular orbit scanning (second scanning form). On the other hand, in the modified example 4, since the switching of the scanning form is not required, the scanning control becomes simpler.

[0050] In the above embodiment, the laser welding is described by taking the case of joining a stator coil of a motor as an example, but the laser welding method of the present invention can be applied to welding of various processing objects, not limited to joining of a stator coil. For example, it can be applied to the case of welding overlapping plate materials 30a and 30b as shown in FIG. 16. First, a first laser beam LL1 is irradiated to form a melting region S4 spanning the plate materials 30a and 30b. Next, a second laser beam LL2 is irradiated to the melting region S4 to maintain a constant melting amount. During the period in which this melting amount is maintained, blowholes BH in the melting region S4 are released into the atmosphere, and blowholes in the welded portion can be reduced.

[0051] According to the embodiment and modified examples of the present invention described above, the following advantageous effects are achieved.

[0052] (1) As shown in Figures 5, 7, 11 to 14, etc., the laser welding method includes a first step of irradiating the ends 211a, 211b, which are the objects to be processed, with a first laser beam LL1 to melt the ends 211a, 211b, and a second step of irradiating the melted region (combined melted region S3) melted by the first step with a second laser beam LL2 having irradiation conditions different from those of the first laser beam LL1 to maintain the melting amount of the combined melted region S3.

[0053] The laser light configuration includes a first laser light configuration (A) or a second laser light configuration (B) described below. In the first laser light configuration (A), when a predetermined time has elapsed from the start of irradiation of the first laser light LL1, as shown in, for example, Figs. 11 to 13, the output of the first laser light LL1 is reduced by a predetermined amount, and the output of the second laser light LL2 is set to be smaller than the output of the first laser light LL1. In the second laser light configuration (B), as shown in Fig. 14, the first laser light LL1 has a first wavelength of 800 nm or more and 1200 nm or less, and includes first-wavelength laser light IR with an output W13, and the second laser light LL2 has a first wavelength, and includes first-wavelength laser light IR with an output smaller than the output W13 and / or in a defocused state.

[0054] In this way, in the second process, the amount of melt in the merged fusion zone S3 is maintained, so that the generation of new blowholes that occur with melting can be stopped. Then, the blowholes in the fusion zone move toward the surface of the fusion zone due to buoyancy, and are released from the surface of the fusion zone into the atmosphere. As a result, the number of blowholes in the fusion zone is reduced, and residual blowholes in the welded zone are reduced, and the joining strength of the welded zone can be improved. In addition, since no deoxidizing agent is used, it is possible to suppress increases in costs and decreases in electrical conductivity.

[0055] (2) Furthermore, as shown in Figures 4 to 7, the objects to be processed are the conductor ends (ends 211a, 211b) of multiple conductors (segment coils 21A, 21B) arranged side by side, and until the molten regions S1, S2 formed at each end 211a, 211b merge to form a single merged molten region S3, the laser light is scanned individually over the ends 211a, 211b as shown in Figure 4, and after the merged molten region S3 is formed, the laser light is scanned so as to straddle each of the ends 211a, 211b as shown in Figure 6.

[0056] Conductors such as the stator coil of a motor are coated with a coating such as enamel on their surfaces. Therefore, when welding the end faces of the ends 211a and 211b by irradiating them with a laser beam, if the laser beam is scanned across both the ends 211a and 211b, the coating will be damaged by the irradiation of the laser beam, causing adverse effects.

[0057] As described above, until the melted regions S1 and S2 formed on each end face merge, the laser light can be irradiated to the coating by irradiating the ends 211a and 211b individually as shown in Fig. 4. On the other hand, when the merged melted region S3 is formed, the coating in the boundary region between the ends 211a and 211b is covered by the merged melted region S3, so that even if the laser light is scanned so as to straddle each of the ends 211a and 211b as shown in Fig. 6, there is no risk of the laser light being irradiated to the coating. As a result, damage to the coating due to the laser light can be prevented.

[0058] The various embodiments and modifications described above are merely examples, and the present invention is not limited to these unless the characteristics of the invention are lost. Other embodiments that are conceivable within the scope of the technical idea of ​​the present invention are also included in the scope of the present invention. [Explanation of symbols]

[0059] 1...laser welding system, 10, 11...laser light generating device, 12...optical device, 13...control device, 14...optical fiber, 15...processing object, 20...stator core, 21...stator coil, 21A, 21B...segment coil, 30a, 30b...plate material, 200a, 200b...slot, 211a, 211b...end, BH...blow hole, Bu...second wavelength laser light, IR...first wavelength laser light, LL1...first laser light, LL2...second laser light, R1, R2, R3...scanning trajectory, S1, S2, S4...melted area, S3...merged melted area

Claims

1. A laser welding method for welding an object to be processed by irradiating the object with laser light, comprising the steps of: a first step of irradiating the object with a first laser light to melt the object; a second step of irradiating the melted region melted by the first step with a second laser beam different from the first laser beam to maintain a melting amount of the melted region, (A) a first laser light configuration, in which, when a predetermined time has elapsed from the start of irradiation of the first laser light, an output of the first laser light is reduced by a predetermined amount, and an output of the second laser light is set to be smaller than the output of the first laser light; or (B) a second laser light configuration, in which the first laser light includes a laser light having a first wavelength of 800 nm or more and 1200 nm or less and a first output, and the second laser light includes a laser light having the first wavelength and an output smaller than the first output and / or in a defocused state; A laser welding method comprising:

2. 2. The laser welding method according to claim 1, The laser welding method, wherein when the output of the first laser light is reduced by a predetermined amount, the output is reduced continuously and gradually with the passage of irradiation time.

3. 2. The laser welding method according to claim 1, The processing target is a conductor end portion of a plurality of conductors arranged in parallel, and the reduction in the predetermined amount is performed in a plurality of steps. A laser welding method, wherein in irradiating the laser light in each of the plurality of steps, the scanning of the laser light on each of the plurality of conductor ends is set to an integer multiple of a reciprocating scan.

4. The laser welding method according to any one of claims 1 to 3, the first laser light in the first laser light configuration includes a laser light having the first wavelength and a second output, and a laser light having a second wavelength of 400 nm or more and 500 nm or less and a third output smaller than the second output, The laser welding method, wherein the second laser light in the first laser light configuration includes laser light having the second wavelength and the third output.

5. The laser welding method according to any one of claims 1 to 4, The processing target is a conductor end portion of a plurality of conductors arranged in parallel, A laser welding method, wherein in the first step and the second step, the conductor end portion is scanned with a laser beam separately.

6. The laser welding method according to any one of claims 1 to 4, The processing target is a conductor end portion of a plurality of conductors arranged in parallel, scanning the laser beam individually over the conductor ends until the molten regions formed at each conductor end merge to form a merged molten region; After the merged molten region is formed, a laser beam is scanned across each of the conductor ends.

7. a first laser light generating device that generates a first laser light; a second laser light generating device that generates a second laser light different from the first laser light; an optical device that irradiates an object to be processed with the first laser light and the second laser light; a control device that controls operations of the first laser light generating device, the second laser light generating device, and the optical device, The control device includes: A laser welding system that controls the operation of the first laser light generating device, the second laser light generating device, and the optical device so as to irradiate the workpiece with the first laser light to melt the workpiece, and then irradiate the molten area with the second laser light to maintain the melt amount of the molten area.

Citation Information

Patent Citations

  • Laser welding method and laser welding device

    WO2022085632A1

  • Welding methods and electrical equipment

    JP7162144B2