Functional material ink
Cellulose nanofibers in the functional material ink stabilize viscosity and expedite binder removal, addressing viscosity changes and production efficiency in conventional inks.
Patent Information
- Application Number
- JP2023072009
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional functional material inks experience changes in viscosity over time due to the influence of the resin (binder), affecting ejection properties, and require an inefficient binder removal process.
Incorporating cellulose nanofibers as the binder in the functional material ink, which reduces viscosity changes over time and shortens the binder removal time, using a solvent like methoxybutanol to enhance stability and ejection performance.
The use of cellulose nanofibers stabilizes viscosity and reduces binder removal time, ensuring consistent ejection properties and efficient production of multilayer ceramic electronic components.
Smart Images

Figure 2024157595000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a functional material ink. [Background technology]
[0002] Inkjet printing has attracted attention as a method for forming non-conductive layers and conductive or semiconductive layers of multilayer ceramic electronic components. JP 2021-24992 A (Patent Document 1) discloses a conventional functional material ink used in inkjet printing. In the manufacture of multilayer ceramic electronic components, degreasing (debinding) is performed to remove the resin (binder) contained in the functional material ink by thermal decomposition or combustion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-24992 Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional functional material inks have a problem in that the viscosity of the ink changes over time during storage after production due to the influence of the resin (binder) contained in the ink, which causes the ink's ejection properties to change over time. There is also room for further improvement in terms of shortening the time it takes to remove the binder from functional material inks.
[0005] The present invention has been made in consideration of the above problems, and has an object to provide a functional material ink that can suppress changes in viscosity over time and shorten the time required for binder removal. [Means for solving the problem]
[0006] The functional material ink according to the present invention includes a functional material, a solvent, and a binder. The solvent includes methoxybutanol. The binder includes cellulose nanofibers.
[0007] As described above, the binder containing cellulose nanofibers suppresses the change in viscosity of the functional material ink over time. Also, cellulose nanofibers require less heat energy for thermal decomposition than other conventional resins used as binders. Therefore, the binder containing cellulose nanofibers can shorten the time required for debinding the functional material ink. Effect of the Invention
[0008] According to the present invention, it is possible to suppress the change in viscosity over time and to shorten the time required for removing the binder. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component manufactured using a functional material ink according to an embodiment of the present invention. [Diagram 2] 2 is a perspective view showing a part of a structure produced during the manufacturing process of the multilayer ceramic capacitor of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A functional material ink according to an embodiment of the present invention will be described below. The functional material ink according to this embodiment contains (A) a functional material, (B) a solvent, and (C) a binder.
[0011] [(A) Functional materials] In this embodiment, the functional material (A) is a powdered material. Specifically, the functional material powder is an inorganic material powder, and may be a powder of a conductive material such as a metal, or a powder of a non-conductive material or a semiconductor material such as a metal oxide. The functional material powder may be a pigment.
[0012] Specific examples of the functional material powder are not particularly limited, but examples of the functional material powder include nickel (Ni), iron (Fe), copper (Cu), aluminum (Al), silver (Ag), tungsten (W), carbon (C), titanium (Ti), NiTi alloy, stainless steel, cobalt chromium (CoCr) alloy, gold (Au), tin (Sn), palladium (Pd), platinum (Pt), manganese (Mn), lithium (Li), silicon (Si), strontium titanate (SrTiO3), zirconate (ZrTiO4), and the like. The functional material powder is a powder containing at least one material selected from the group consisting of calcium (CaZrO3), magnesium oxide (MgO), silica (SiO2), alumina (Al2O3), chromium oxide (Cr2O3), manganese dioxide (MnO2), yttrium oxide (Y2O3), calcium titanate (CaTiO3), zirconia (ZrO2), strontium zirconate (SrZrO3), barium titanate (BaTiO3), and calcium carbonate (CaCO3). If the functional material powder is such a powder, the functional material ink according to this embodiment can be suitably used in the manufacture of a multilayer ceramic electronic component described below.
[0013] The content of the functional material (A) in the functional material ink is, for example, 20% by mass or more and 50% by mass or less.
[0014] [(B) Solvent] In the present embodiment, the (B) solvent is a water-soluble solvent containing methoxybutanol, which can suppress the (A) functional material from settling in the functional material ink, and can improve the long-term stability, ejection property, and printability of the functional material ink.
[0015] The (B) solvent may contain other water-soluble solvents, such as glycols, ethylene glycol, polypropylene glycol, and the like; diols, such as 1,3-butanediol, pentanediol, and the like; glycol esters, such as propylene glycol laurate, ethers of diethylene glycol monoethyl and diethylene glycol monobutyl, glycol ethers, such as propylene glycol ether and dipropylene glycol ether, alcohols, such as methanol and ethanol, sulfolane, lactones, such as γ-butyrolactone, and lactams, such as N-(2-hydroxyethyl)pyrrolidone, and the like.
[0016] The (B) solvent preferably further contains at least one compound selected from the group consisting of 1,3-butanediol and ethylene glycol. When the (B) solvent is a mixed solvent containing the above compound together with methoxybutanol, sedimentation of the (A) functional material in the functional material ink can be further suppressed.
[0017] The content of the solvent (B) in the functional material ink is, for example, 50% by mass or more and 70% by mass or less.
[0018] [(C) Binder] The binder (C) contains cellulose nanofibers, which makes the change in viscosity of the functional material ink according to this embodiment relatively small over time.
[0019] Cellulose nanofibers are nanocelluloses extracted from cellulose raw materials (e.g., wood). Methods for extracting cellulose nanofibers include, for example, mechanical treatments (e.g., grinding treatments using a bead mill) and chemical treatments (e.g., TEMPO catalytic oxidation treatments, carboxymethylation treatments, and cationization treatments). As cellulose nanofibers, cellulose nanofibers extracted by mechanical treatments are preferred.
[0020] The average diameter (fiber diameter) of the cellulose nanofibers is, for example, 2 nm to 20 nm, preferably 3 nm to 10 nm, and more preferably 3 nm to 7 nm. By making the average diameter of the cellulose nanofibers 20 nm or less, the ejection properties of the functional material ink can be further improved.
[0021] The aspect ratio of the cellulose nanofibers (average fiber length / average diameter) is from 30 to 200, preferably from 100 to 200, and more preferably from 150 to 200. By setting the aspect ratio of the cellulose nanofibers to 200 or less, the ejection properties of the functional material ink can be improved.
[0022] Here, the "average fiber length" and "average diameter" of the cellulose nanofibers are values measured based on a two-dimensional projected image (for example, an SEM photograph) of the cellulose nanofibers. Specifically, in measuring the "average fiber length" and "average diameter" of the cellulose nanofibers, first, the fiber length or diameter of each of 20 cellulose nanofibers randomly selected in the two-dimensional projected image is measured. Then, the arithmetic mean value of the measured fiber length or diameter of the cellulose nanofibers is calculated, and the calculated value is regarded as the average fiber length or average diameter. Note that, if the diameter of the cellulose nanofiber to be measured is not constant, the diameter is measured at five randomly selected points on the cellulose nanofiber to be measured, and the arithmetic mean value is regarded as the diameter of the cellulose nanofiber to be measured. In addition, cellulose nanofibers in a dry state are used to measure the average fiber length and average diameter of the cellulose nanofibers.
[0023] The (C) binder may further contain other resins, such as polyvinyl resins, polyester resins, ether resins, polyamide resins, polyester resins, phenolic resins, silicone resins, fluorine-based polymer compounds, or resins made of non-nanofiber-shaped polysaccharide derivatives such as cellulose (e.g., hydroxypropyl cellulose).
[0024] The content of cellulose nanofibers in the (C) binder is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 80% by mass or more. Most preferably, the (C) binder is substantially composed of cellulose nanofibers. The higher the content of cellulose nanofibers in the (C) binder, the greater the effect of the cellulose nanofibers in suppressing the change in viscosity of the functional material ink over time.
[0025] The content of the binder (C) in the functional material ink is, for example, 0.5% by mass or more and 3.0% by mass or less. If the content of the binder (C) in the functional material ink is 3.0% by mass or less, it is possible to prevent the viscosity of the functional material ink from changing significantly over time, and also to prevent the viscosity of the functional material ink from varying significantly between production lots.
[0026] [(D) Dispersant] In this embodiment, the functional material ink may further contain a dispersant (D). Examples of the dispersant (D) include polycarboxylic acid copolymers and nonionic dispersants such as acetylene glycol surfactants. The content of the dispersant (D) in the functional material ink is, for example, 0.1% by mass or more and 1.0% by mass or less.
[0027] [Functional material ink] The functional material ink according to this embodiment can be used, for example, as an ink for ink jet printing.
[0028] In the functional material ink, the ratio of the volume of the (A) functional material to the total volume of the (A) functional material, the (C) binder, and the (D) dispersant is preferably 80 vol% or more and 90 vol% or less. If the above volume ratio is 80 vol% or more, the density of the (A) functional material can be increased after the (B) solvent is dried and the (C) binder is vaporized (de-bindered) together with the (C) dispersant in the printed layer formed by printing the functional material ink. Also, if the above volume ratio is 90 vol% or less, the viscosity can be prevented from becoming too high.
[0029] The viscosity of the functional material ink is preferably 10 mPa·S or more and 35 mPa·S or less. If the viscosity of the functional material ink is 10 mPa·S or more and 35 mPa·S or less, the functional material ink can be suitably used as an ink for inkjet printing. The above viscosity is measured, for example, using a cone-type rheometer ("MCR301" manufactured by Anton Paar) with a cone diameter of 50 mm (CP50) and a temperature condition of 25°C ± 2°C, at a shear rate of 1000 sec -1 The viscosity after 3 seconds at
[0030] [Multilayer ceramic electronic components] Next, a multilayer ceramic electronic component manufactured using a functional material ink according to an embodiment of the present invention will be described with reference to the drawings. In the following description of the multilayer ceramic electronic component, the same or corresponding parts in the drawings are given the same reference numerals, and the description thereof will not be repeated.
[0031] FIG. 1 is a cross-sectional view showing a multilayer ceramic capacitor as an example of a multilayer ceramic electronic component manufactured using a functional material ink according to an embodiment of the present invention.
[0032] As shown in Fig. 1, the multilayer ceramic capacitor 1 includes a ceramic body 3 having a laminated structure made of ceramic layers 2 as multiple laminated non-conductive layers, and first internal electrodes 4 and second internal electrodes 5 as multiple conductor layers formed along multiple interfaces between the ceramic layers 2. In the multilayer ceramic capacitor 1, the ceramic layers 2 are made of dielectric ceramic. The first internal electrodes 4 and the second internal electrodes 5 face each other via the ceramic layers 2 so as to form a capacitance, and are arranged alternately when viewed in the lamination direction.
[0033] A first external electrode 6 serving as a conductor layer is formed on one end face of the ceramic body 3. The first external electrode 6 is electrically connected to the first internal electrode 4. A second external electrode 7 serving as a conductor layer is formed on the other end face of the ceramic body 3. The second external electrode 7 is electrically connected to the second internal electrode 5.
[0034] Fig. 2 is a perspective view showing a part of a structure produced in the course of producing the multilayer ceramic capacitor of Fig. 1. As shown in Fig. 2, a structure 10 is produced in order to produce the multilayer ceramic capacitor 1 described above. The structure 10 includes ceramic green sheets 11 which correspond to the ceramic layers 2 of the multilayer ceramic capacitor 1.
[0035] An internal electrode printed layer 12 which will become the first internal electrode 4 or the second internal electrode 5 is formed on one main surface of the ceramic green sheet 11. The internal electrode printed layer 12 has a predetermined thickness, and therefore, a step is generated on the ceramic green sheet 11 due to this thickness.
[0036] On the other hand, a step absorption printed layer 13 is formed in an area on the main surface of the ceramic green sheet 11 where the internal electrode printed layer 12 is not formed. The step absorption printed layer 13 serves as a step absorption layer as a non-conductive layer for absorbing steps due to the thickness of the internal electrode printed layer 12 described above. The step absorption printed layer 13 may be formed after or before the step of forming the internal electrode printed layer 12. Although the step absorption layer is not particularly shown in FIG. 1, it is formed in the ceramic body 3 so as to extend on the same plane as each of the first internal electrode 4 and the second internal electrode 5.
[0037] 2 is to become the first internal electrode 4 shown in FIG. 1, the external electrode printed layer 14 to become the first external electrode 6 is formed so as to be connected to an edge of the internal electrode printed layer 12. The external electrode printed layer 14 is formed so as to have a thickness equivalent to the total thickness of the ceramic green sheet 11 and the internal electrode printed layer 12 or the step absorption printed layer 13. Similarly, the external electrode printed layer 15 to become the second external electrode 7 is formed so as to be connected to an edge of the internal electrode printed layer to become the second internal electrode 5 (not shown).
[0038] The functional material ink according to this embodiment can be used to form the structure 10 including the above-mentioned ceramic green sheet 11, the internal electrode printed layer 12, the step absorption printed layer 13, and the external electrode printed layers 14 and 15. That is, functional material inks having compositions suitable for the ceramic green sheet 11, the internal electrode printed layer 12, the step absorption printed layer 13, and the external electrode printed layers 14 and 15 are used. Simply put, functional material inks containing ceramic (metal oxide) powder as inorganic material powder that serves as the functional material are used to form the ceramic green sheet 11 and the step absorption printed layer 13, and functional material inks containing metal powder as inorganic material powder that serves as the functional material are used to form the internal electrode printed layer 12 and the external electrode printed layers 14 and 15.
[0039] Preferably, a three-dimensional inkjet printing method may be performed in which separate inkjet heads are sequentially operated to sequentially form the ceramic green sheet 11, the internal electrode printed layer 12, the step absorption printed layer 13, and the external electrode printed layers 14 and 15. The three-dimensional inkjet printing method is repeated a required number of times to obtain a green laminate that will become the multilayer ceramic capacitor 1.
[0040] Next, the green laminate is debindered and fired. As a result of this debindering and firing, a multilayer ceramic capacitor 1 is manufactured, which includes a ceramic body 3 having a first internal electrode 4 and a second internal electrode 5 built therein and a first external electrode 6 and a second external electrode 7 formed thereon, as shown in FIG. 1. The firing conditions are not particularly limited, but for example, firing can be performed by increasing the temperature to 1200°C at 5°C / min in an air atmosphere, keeping it at 1200°C for 2 hours, and then decreasing the temperature to 20°C at 1°C / min.
[0041] In addition, a two-dimensional inkjet printing method may be used instead of a three-dimensional inkjet printing method to obtain a green laminate that will become the multilayer ceramic capacitor 1. In this case, a ceramic green sheet 11 is formed by a sheet forming method such as a doctor blade method, and an internal electrode print layer 12 and a step absorption print layer 13 are formed thereon by a two-dimensional inkjet printing method. Then, a plurality of ceramic green sheets 11 are laminated to obtain a green laminate. This green laminate is fired to obtain a ceramic body 3 incorporating a first internal electrode 4 and a second internal electrode 5. Then, a first external electrode 6 and a second external electrode 7 are formed on the ends of the ceramic body 3 by, for example, applying and baking a conductive paste, thereby completing the multilayer ceramic capacitor 1.
[0042] As described above, the functional material ink according to this embodiment can be used to form a non-conductive layer (dielectric layer), a conductive layer, or a semiconductor layer in a multilayer ceramic electronic component by inkjet printing. EXAMPLES
[0043] The functional material ink according to the present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0044] [Example 1] The functional material ink according to Example 1 was manufactured as follows. First, Ni powder as the functional material powder, polycarboxylic acid copolymer as the dispersant, and methoxybutanol as the solvent were mixed and stirred in a ball mill at a rotation speed of 150 rpm for 16 hours to attach the dispersant to the inorganic material powder, thereby obtaining a first mixture. Next, only cellulose nanofiber (CNF) to which hydrophobicity was imparted by introducing an alkanoyl group or the like was added as a binder to the first mixture, and the mixture was again mixed and stirred in a ball mill at a rotation speed of 150 rpm for 4 hours to obtain a second mixture. Then, the second mixture was filtered once with a filter having a pore size of 1 μm to remove the functional material powder and impurities having a particle size exceeding 1 μm, thereby obtaining the functional material ink according to Example 1. In Example 1, the materials were mixed so that the contents of the functional material powder, binder, and dispersant contained in the functional material ink were 37.0 mass%, 0.7 mass%, and 0.6 mass%, respectively. Furthermore, the functional material powder, binder, and dispersant were mixed together such that the ratio of the volume of the functional material powder to the total volume of the functional material powder, binder, and dispersant was 90 vol %.
[0045] [Example 2] A functional material ink according to Example 2 was obtained in the same manner as in Example 1, except that a mixed solvent containing 50 vol % of methoxybutanol and 50 vol % of 1-3-butanediol was used as the solvent.
[0046] [Example 3] A functional material ink according to Example 3 was obtained in the same manner as in Example 1, except that a mixed solvent containing 50 vol % of methoxybutanol and 50 vol % of ethylene glycol was used as the solvent.
[0047] [Example 4] In Example 4, the functional material ink was mixed so that the contents of the functional material powder, binder, and dispersant in the functional material ink were 34.6 mass%, 1.6 mass%, and 0.6 mass%, respectively. The materials were also mixed so that the ratio of the volume of the functional material powder to the total volume of the functional material powder, binder, and dispersant was 85 vol%. Other than these, the functional material ink of Example 4 was obtained in the same manner as Example 1.
[0048] [Examples 5 to 8] Functional material inks according to Examples 5 to 8 were obtained in the same manner as in Examples 1 to 4, except that Cu powder was used as the functional material powder.
[0049] [Examples 9 to 12] Functional material inks according to Examples 9 to 12 were obtained in the same manner as in Examples 1 to 4, except that C powder was used as the functional material powder.
[0050] [Examples 13 to 16] Functional material inks according to Examples 13 to 16 were obtained in the same manner as in Examples 1 to 4, respectively, except that Ag powder was used as the functional material powder.
[0051] [Examples 17 to 20] Functional material inks according to Examples 17 to 20 were obtained in the same manner as in Examples 1 to 4, except that Ti powder was used as the functional material powder.
[0052] [Examples 21 to 24] Functional material inks according to Examples 21 to 24 were obtained in the same manner as in Examples 1 to 4, except that NiTi alloy powder was used as the functional material powder.
[0053] [Example 25] In Example 25, cellulose nanofibers to which hydrophobicity was imparted by introducing an alkanoyl group or the like and hydroxypropyl cellulose (HPC) were used as the binder in a mass ratio of 1:1. In addition, the contents of the functional material powder, binder, and dispersant in the functional material ink were 30.4 mass%, 2.6 mass%, and 0.6 mass%, respectively, and the materials were mixed. In addition, the ratio of the volume of the functional material powder to the total volume of the functional material powder, binder, and dispersant was 80 vol.%. Apart from the above, the functional material ink of Example 25 was obtained in the same manner as in Example 24.
[0054] [Examples 26 to 29] Functional material inks according to Examples 26 to 29 were obtained in the same manner as in Examples 1 to 4, except that CaZrO3 powder was used as the functional material powder.
[0055] [Examples 30 to 33] Functional material inks according to Examples 30 to 33 were obtained in the same manner as in Examples 1 to 4, except that BaTiO3 powder was used as the functional material powder.
[0056] [Examples 34 to 37] Functional material inks according to Examples 34 to 37 were obtained in the same manner as in Examples 1 to 4, except that Al2O3 powder was used as the functional material powder.
[0057] [Example 38] A functional material ink according to Example 38 was obtained in the same manner as in Example 25, except that CaZrO3 powder was used as the functional material powder.
[0058] [Comparative Example 1 to Comparative Example 36] Functional material inks according to Comparative Examples 1 to 36 were obtained in the same manner as in Examples 1 to 24 and Examples 26 to 37, respectively, except that only hydroxypropyl cellulose was used as the binder.
[0059] [Viscosity measurement] The viscosity of the functional material ink according to each of the examples and comparative examples was measured. The viscosity of the functional material ink was measured using a cone rheometer ("MCR301" manufactured by Anton Paar) with a cone diameter of 50 mm (CP50) and a temperature condition of 25°C ± 2°C at a shear rate of 1000 [sec -1 The viscosity after 3 seconds was measured. For each of the functional material inks according to the examples and comparative examples, the viscosity (first viscosity) was measured 5 hours after preparation by the above-mentioned method, and the viscosity (second viscosity) was measured 30 days after preparation by the above-mentioned method. In addition, for each of the examples and comparative examples, the value obtained by dividing the second viscosity by the first viscosity was calculated as the viscosity change rate.
[0060] [Measurement of binder removal time] The time required for binder removal was measured when the binder was removed after printing for the functional material ink according to each Example and Comparative Example. First, the functional material ink according to each Example and Comparative Example was printed by inkjet printing using a piezo inkjet printer, and then dried under conditions of 50°C and 3 minutes to obtain a printed layer. Next, the printed layer was heated to 300°C at 1°C / min in an air atmosphere and kept at 300°C. After starting to keep at 300°C, it was determined by a thermogravimetry / differential thermal analysis (TG / DTA) device that the binder had almost completely evaporated, and then the temperature was lowered to 20°C at 1°C / min. The time from the start of the temperature increase to the completion of the temperature decrease was measured as the binder removal time.
[0061] The results of the first viscosity, the second viscosity, the viscosity change rate, and the binder removal time are shown in the following Tables 1 and 2. In addition, in the (B) solvents in Tables 1 and 2, "M" represents methoxybutanol, "B" represents 1-3-butanediol, and "E" represents ethylene glycol.
[0062] [Table 1]
[0063] [Table 2]
[0064] As shown in Table 1, in Examples 1 to 38, the binder contained cellulose nanofiber, the viscosity change rate of the functional material ink was 0.9 to 1.2, and the binder removal time was 5 to 7 hours. On the other hand, as shown in Table 2, in Comparative Examples 1 to 36, the binder did not contain cellulose nanofiber, the viscosity change rate of the functional material ink was 1.3 to 1.7, and the binder removal time was 10 hours. It can therefore be seen that by including cellulose nanofiber in the binder, the change in viscosity of the functional material ink over time was suppressed, and the binder removal time was shortened.
[0065] Cellulose nanofiber requires less thermal energy for thermal decomposition compared to other resins conventionally used as binders, and it is therefore believed that by including cellulose nanofiber in the binder, the time required for thermally decomposing the binder and discharging it from the system is shortened.
[0066] In addition, in Examples 2, 3, 6, 7, 10, 11, 14, 15, 18, 19, 22, 23, 27, 28, 31, 32, 35, and 36, the solvent further contained 1,3-butanediol or ethylene glycol, and the viscosity change rate of the functional material ink was 1.0 to 1.2, and the binder removal time was 5 hours. On the other hand, as shown in Table 2, in Comparative Examples 2, 3, 6, 7, 10, 11, 14, 15, 18, 19, 22, 23, 26, 27, 30, 31, 34, and 35, the solvent further contained 1,3-butanediol or ethylene glycol, and the viscosity change rate of the functional material ink was 1.3 to 1.7, and the binder removal time was 10 hours. Thus, it can be seen that even when the solvent further contains 1,3-butanediol or ethylene glycol, the binder contains cellulose nanofiber, which suppresses the change in viscosity of the functional material ink over time and shortens the time required for binder removal.
[0067] In addition, in Examples 1 to 38 and Comparative Examples 1 to 36, the ratio of the volume of the functional material to the total volume of the functional material, binder, and dispersant was 80 vol% or more and 90 vol% or less. The functional material inks in Examples 1 to 38 had a viscosity change rate of 0.9 to 1.2 and a binder removal time of 5 to 7 hours, while the functional material inks in Comparative Examples 1 to 36 had a viscosity change rate of 1.3 to 1.7 and a binder removal time of 10 hours. Therefore, it can be seen that even when the volume ratio of the functional material is 80 vol% or more and 90 vol% or less, the inclusion of cellulose nanofibers in the binder suppresses the change in viscosity of the functional material ink over time and shortens the binder removal time.
[0068] In addition, in Examples 1 to 38 and Comparative Examples 1 to 36, powders made of nickel (Ni), copper (Cu), carbon (C), silver (Ag), titanium (Ti), NiTi alloy, calcium zirconate (CaZrO3), barium titanate (BaTiO3), or alumina (Al2O3) were used as the functional material. The viscosity change rate of the functional material inks according to Examples 1 to 38 was 0.9 to 1.2, and the binder removal time was 5 to 7 hours, while the viscosity change rate of the functional material inks according to Comparative Examples 1 to 36 was 1.3 to 1.7, and the binder removal time was 10 hours. Therefore, even when the above-mentioned powders were used as the functional material, it can be understood that the binder contains cellulose nanofibers, so that the change in viscosity of the functional material ink over time is suppressed and the binder removal time is shortened.
[0069] In the above description of the embodiment, configurations that can be combined may be combined with each other.
[0070] [Note] As described above, the present embodiment includes the following disclosure.
[0071] <1> A functional material ink comprising a functional material, a solvent, and a binder, The solvent comprises methoxybutanol; The functional material ink, wherein the binder comprises cellulose nanofiber.
[0072] <2> The solvent further comprises at least one compound selected from the group consisting of 1,3-butanediol and ethylene glycol; <1> The functional material ink according to claim 1.
[0073] <3> Further comprising a dispersant, A ratio of the volume of the functional material to the total volume of the functional material, the binder, and the dispersant is 80 vol% or more and 90 vol% or less. <1> or <2> The functional material ink according to claim 1.
[0074] <4> The functional materials include nickel (Ni), iron (Fe), copper (Cu), aluminum (Al), silver (Ag), tungsten (W), carbon (C), titanium (Ti), NiTi alloy, stainless steel, cobalt chromium (CoCr) alloy, gold (Au), tin (Sn), palladium (Pd), platinum (Pt), manganese (Mn), lithium (Li), silicon (Si), strontium titanate (SrTiO3), and calcium zirconate (CaZrO3). a powder containing at least one material selected from the group consisting of magnesium oxide (MgO), silica (SiO2), alumina (Al2O3), chromium oxide (Cr2O3), manganese dioxide (MnO2), yttrium oxide (Y2O3), calcium titanate (CaTiO3), zirconia (ZrO2), strontium zirconate (SrZrO3), barium titanate (BaTiO3), and calcium carbonate (CaCO3); <1> from <3> 2. The functional material ink according to claim 1 .
[0075] <5> Used for forming a non-conductive layer, a conductive layer, or a semiconductor layer in a multilayer ceramic electronic component by an inkjet printing method. <1> from <4> 2. The functional material ink according to claim 1 .
[0076] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0077] 1 multilayer ceramic capacitor, 2 ceramic layer, 3 ceramic body, 4 first internal electrode, 5 second internal electrode, 6 first external electrode, 7 second external electrode, 10 structure, 11 ceramic green sheet, 12 internal electrode printed layer, 13 step absorption printed layer, 14, 15 external electrode printed layers.
Claims
1. A functional material ink comprising a functional material, a solvent, and a binder, The solvent comprises methoxybutanol; The functional material ink, wherein the binder comprises cellulose nanofiber.
2. 2. The functional material ink according to claim 1, wherein the solvent further comprises at least one compound selected from the group consisting of 1,3-butanediol and ethylene glycol.
3. Further comprising a dispersant, 2. The functional material ink according to claim 1, wherein a ratio of a volume of the functional material to a total volume of the functional material, the binder, and the dispersant is 80 vol % or more and 90 vol % or less.
4. The functional materials include nickel (Ni), iron (Fe), copper (Cu), aluminum (Al), silver (Ag), tungsten (W), carbon (C), titanium (Ti), NiTi alloy, stainless steel, cobalt chromium (CoCr) alloy, gold (Au), tin (Sn), palladium (Pd), platinum (Pt), manganese (Mn), lithium (Li), silicon (Si), strontium titanate (SrTiO 3 ), calcium zirconate (CaZrO 3 ), magnesium oxide (MgO), silica (SiO 2 ), alumina (Al 2 O 3 ), chromium oxide (Cr 2 O 3 ), manganese dioxide (MnO 2 ), yttrium oxide (Y 2 O 3 ), calcium titanate (CaTiO 3 ), zirconia (ZrO 2 ), strontium zirconate (SrZrO 3 ), barium titanate (BaTiO 3 ), and calcium carbonate (CaCO 3 2. The functional material ink according to claim 1, which is a powder containing at least one material selected from the group consisting of:
5. 5. The functional material ink according to claim 1, which is used for forming a non-conductive layer, a conductive layer, or a semiconductor layer in a multilayer ceramic electronic component by an inkjet printing method.
Citation Information
Patent Citations
Functional material ink
JP2021024992A
Cited By
Titanate compound fine particle powder and method of production therefor
WO2026126902A1