Electrode mixture and lithium-ion battery
The use of silicon clathrate active material particles with aluminum fluoride particles of controlled size in lithium ion batteries addresses the issue of expansion, resulting in improved battery stability and performance.
Patent Information
- Application Number
- JP2023072150
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Silicon clathrate active materials, while effective in reducing expansion during charging, still require further suppression of expansion in lithium ion batteries.
An electrode composite material comprising silicon clathrate active material particles and aluminum fluoride particles with a controlled average particle size of 3.0 μm or less, and a specific ratio of aluminum fluoride to silicon clathrate active material particles, to prevent interference with uniform charging and reduce expansion.
The electrode composite material significantly reduces expansion during charging, enhancing the performance and stability of lithium ion batteries.
Smart Images

Figure 2024157669000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrode mix and a lithium ion battery. [Background technology]
[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as an active material for batteries, particularly lithium ion batteries.
[0003] Silicon active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate active material as the silicon active material.
[0004] For example, Patent Document 1 discloses a silicon clathrate active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]
[0006] Although silicon clathrate active materials can suppress expansion during charging as compared with ordinary silicon active materials, there is a demand for further suppression of the expansion of silicon clathrate active materials during charging.
[0007] The present disclosure aims to provide an electrode mixture that exhibits small expansion during charging, and a lithium-ion battery that includes such an electrode mixture. [Means for solving the problem]
[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> An electrode mixture comprising silicon clathrate active material particles and aluminum fluoride particles, the aluminum fluoride particles having an average particle size of 3.0 μm or less. <Aspect 2> 2. The electrode mixture according to aspect 1, wherein the aluminum fluoride particles have an average particle size of 0.1 μm or more and 2.5 μm or less. <Aspect 3> 3. The electrode mixture according to aspect 2, wherein the aluminum fluoride particles have an average particle size of 0.8 μm or more and 1.8 μm or less. <Aspect 4> 4. The electrode mixture according to any one of aspects 1 to 3, wherein a ratio of an average particle size of the aluminum fluoride particles to an average particle size of the silicon clathrate active material particles is 2.5 or less. <Aspect 5> The electrode mixture according to any one of aspects 1 to 4, wherein, when a cross section of the electrode mixture is observed by SEM-EDX measurement, the ratio of the content of the aluminum fluoride particles to the content of the silicon clathrate active material particles is less than 2.0 area %. Aspect 6 An electrode active material layer is provided, and The electrode active material layer contains the electrode mixture according to any one of aspects 1 to 5. Lithium-ion battery. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide an electrode mixture that exhibits small expansion during charging, and a lithium ion battery that includes such an electrode mixture. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a graph showing the relationship between the average particle size of aluminum fluoride particles and the expansion rate of a battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0012] 《Electrode composite material》 The electrode mixture of the present disclosure contains silicon clathrate active material particles and aluminum fluoride particles, and the aluminum fluoride particles have an average particle size of 3.0 μm or less.
[0013] In the context of the present disclosure, an "electrode" may be a positive electrode or a negative electrode, and is particularly preferably a negative electrode.
[0014] In the context of this disclosure, a "composite" refers to a composition that can form an electrode active material layer as is or by further containing other components, and a "composite slurry" refers to a slurry that contains a dispersion medium in addition to a "composite" and can be applied and dried to form an electrode active material layer.
[0015] As a method for obtaining silicon clathrate active material particles, for example, a method for removing sodium from a sodium silicon (NaSi) alloy is mentioned. The present inventors have developed a technique for removing sodium from a NaSi alloy by reacting the NaSi alloy with aluminum fluoride.
[0016] In this regard, the present inventors have found that the electrode mixture obtained using this technology has room for improvement in terms of the effect of suppressing expansion during charging. Specifically, without intending to be bound by any theory, they have found that in the electrode mixture obtained using this technology, the silicon clathrate active material particles are not uniformly charged due to the presence of insulating aluminum fluoride particles remaining, which may result in large expansion.
[0017] In contrast, the electrode mixture of the present disclosure has aluminum fluoride particles with a small average particle size of 3.0 μm or less, which is thought to not interfere with uniform charging of the silicon clathrate active material particles and to be able to suppress expansion during charging.
[0018] Silicon clathrate active material particles The electrode mix of the present disclosure includes silicon clathrate active material particles.
[0019] The average particle size of the silicon clathrate active material particles may be 0.4 μm or more, 0.6 μm or more, 0.8 μm or more, 0.9 μm or more, 1.0 μm or more, or 1.1 μm or more, and may be 2.0 μm or less, 1.8 μm or less, 1.6 μm or less, 1.5 μm or less, 1.4 μm or less, or 1.3 μm or less.
[0020] The average particle size of the silicon clathrate active material particles can be obtained by observation with an electron microscope such as SEM, and is obtained, for example, as the average value of the equivalent circle diameters (equivalent circle area diameters) of a plurality of silicon clathrate active material particles. The number of samples is preferably large, for example, 20 or more, or may be 50 or more, or may be 100 or more.
[0021] <Aluminum Fluoride Particles> The electrode mix of the present disclosure includes aluminum fluoride particles.
[0022] The average particle size of the aluminum fluoride particles is 3.0 μm or less. The average particle size of the aluminum fluoride particles may be 0.1 μm or more, 0.3 μm or more, 0.5 μm or more, 0.6 μm or more, 0.7 μm or more, 0.8 μm or more, or 0.9 μm or more, or may be 2.7 μm or less, 2.5 μm or less, 2.3 μm or less, 2.1 μm or less, 2.0 μm or less, 1.9 μm or less, 1.8 μm or less, 1.7 μm or less, 1.6 μm or less, or 1.5 μm or less.
[0023] The average particle size of the aluminum fluoride particles can be determined by observation with an electron microscope such as SEM, and is determined, for example, as the average value of the equivalent circle diameters of a plurality of aluminum fluoride particles. The number of samples is preferably large, for example, 20 or more, or may be 50 or more, or may be 100 or more.
[0024] The ratio of the average particle size of the aluminum fluoride particles to the average particle size of the silicon clathrate active material particles (AlF3 / Si(particle size)) may be 2.5 or less. This ratio may be 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more, or may be 2.3 or less, 2.1 or less, 1.9 or less, 1.7 or less, 1.5 or less, 1.4 or less, or 1.3 or less.
[0025] The ratio of the content of the aluminum fluoride particles to the content of the silicon clathrate active material particles (AlF3 / Si (area)) may be less than 2.0 area %, and may be 0.1 area % or more, 0.5 area % or more, or 1.0 area % or more, and may be 1.9 area % or less, 1.8 area % or less, or 1.7 area % or less.
[0026] AlF3 / Si (area) can be calculated by observing the cross section of the electrode composite by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) measurement, and expressing the ratio of the area of the range showing aluminum fluoride particles to the area of the range showing silicon clathrate active material particles.
[0027] The silicon clathrate active material particles of the present disclosure can be obtained by any method, exemplified by a method of removing sodium from a sodium silicon (NaSi) alloy.
[0028] Specifically, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy, and then the thus prepared NaSi alloy is reacted with aluminum fluoride particles as a sodium trapping agent to prepare silicon clathrate active material particles.
[0029] The unreacted aluminum fluoride particles in the above reaction can be used as the aluminum fluoride particles of the present disclosure. In addition, commercially available aluminum fluoride particles or aluminum fluoride particles prepared by a conventional method can be used as the aluminum fluoride particles of the present disclosure.
[0030] The aluminum fluoride particles may be subjected to a particle size adjustment process so that the average particle size falls within the range of the present disclosure. Examples of particle size adjustment processes include, but are not limited to, sieving.
[0031] The electrode mixture of the present disclosure can be prepared by mixing the thus obtained silicon clathrate active material particles and a material containing aluminum fluoride particles by any method.
[0032] Lithium-ion battery The lithium ion battery of the present disclosure may be a liquid battery or a solid-state battery. In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.
[0033] The lithium ion battery of the present disclosure has an electrode active material layer, and the electrode active material layer contains the electrode mixture of the present disclosure. In particular, the lithium ion battery of the present disclosure may have a negative electrode mixture which is the electrode mixture of the present disclosure, and in this case, may include, in this order, a negative electrode current collector layer, a negative electrode active material layer containing the electrode mixture of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.
[0034] The lithium ion battery of the present disclosure can be restrained from both sides of the stacking direction of each of the layers by restraining members such as end plates. Examples of the restraining method include, but are not limited to, a method that utilizes the restraining torque of a bolt.
[0035] Hereinafter, a method for producing a battery in which the negative electrode mixture is the electrode mixture of the present disclosure will be described.
[0036] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.
[0037] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0038] <Negative electrode active material layer> The negative electrode active material layer contains the electrode mixture of the present disclosure.
[0039] (electrode composite material) The electrode mixture includes silicon clathrate active material particles as a negative electrode active material, and aluminum fluoride particles. For the electrode mixture, reference can be made to the above description of the electrode mixture of the present disclosure.
[0040] The negative electrode active material layer optionally contains a solid electrolyte, a conductive additive, and a binder.
[0041] (solid electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0042] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.
[0043] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).
[0044] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate active material particles to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate active material particles:mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0045] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0046] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0047] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.
[0048] <Solid electrolyte layer> The solid electrolyte layer includes at least a solid electrolyte. In addition to the solid electrolyte, the solid electrolyte layer may include a binder, etc., as necessary. For the solid electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.
[0049] The thickness of the solid electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.
[0050] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.
[0051] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y Li-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.
[0052] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.
[0053] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0054] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.
[0055] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0056] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0057] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.
[0058] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred. EXAMPLES
[0059] 《Synthesis of silicon clathrate active material particles》 <Alloying> Comparative Example 1 As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, i.e., a Si powder having a porous structure.
[0060] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 400°C for 40 hours to obtain a powdered NaSi alloy. <Clathrate formation>
[0061] The obtained NaSi alloy and aluminum fluoride (AlF3) particles were weighed to a molar ratio of 1:0.35, and the weighed NaSi alloy and AlF3 particles were mixed with a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel, and reacted in a heating furnace under an argon atmosphere at 310°C for 60 hours to obtain a silicon clathrate. The obtained silicon clathrate was acid washed using a mixed solvent of HNO3 and H2O in a volume ratio of 90:10 to remove by-products in the reaction product. After washing, it was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a powdered silicon clathrate. Furthermore, the obtained silicon clathrate was washed with a 3 wt% HF solution, filtered, and then dried at 120°C for 3 hours or more to obtain silicon clathrate active material particles of Comparative Example 1. In addition, the unreacted AlF3 particles were used as the AlF3 particles of Comparative Example 1. The surface of the silicon clathrate active material particles may contain a coating or impurities containing O, C, N, or the like.
[0062] Example 1 Except for changing the alloying temperature to 500°C and changing the NaSi:AlF3 (molar ratio) in the clathrate formation to 1:0.5, the silicon clathrate active material particles and AlF3 particles of Example 1 were obtained in the same manner as in Comparative Example 1. Note that the surface of the silicon clathrate active material particles may contain a coating or impurities containing O, C, or N elements.
[0063] Example 2 Except for using AlF3 particles passed through a sieve with a mesh size of 75 μm, the silicon clathrate active material particles and AlF3 particles of Example 2 were obtained in the same manner as in Example 1. Note that the surface of the silicon clathrate active material particles may contain a coating or impurities containing O element, C element, N element, or the like.
[0064] Example 3 Except for using AlF3 particles that passed through a sieve with a mesh size of 75 μm but did not pass through a sieve with a mesh size of 32 μm, the silicon clathrate active material particles and AlF3 particles of Example 3 were obtained in the same manner as in Example 1. Note that the surface of the silicon clathrate active material particles may contain a coating or impurities containing O element, C element, N element, or the like.
[0065] Example 4 Except for using AlF3 particles passed through a sieve with a mesh size of 20 μm, the silicon clathrate active material particles and AlF3 particles of Example 4 were obtained in the same manner as in Example 1. Note that the surface of the silicon clathrate active material particles may contain a coating or impurities containing O element, C element, N element, or the like.
[0066] <<Making a lithium-ion battery>> The lithium ion batteries of each example were fabricated as follows.
[0067] <Preparation of negative electrode mixture> Butyl butyrate, 5wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, vapor grown carbon fiber (VGCF) as a conductive assistant, silicon clathrate active material particles and AlF3 particles of each example, and Li2S-P2S5 glass ceramic as a sulfide solid electrolyte were added to a polypropylene container, and stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry).
[0068] <Formation of negative electrode active material layer> The obtained negative electrode composite slurry was applied onto a copper (Cu) foil serving as a negative electrode current collector layer by the blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C to form a negative electrode active material layer on the negative electrode current collector layer.
[0069] <Formation of solid electrolyte layer> Heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li2SP2S5-based glass ceramic as a sulfide solid electrolyte were added to a polypropylene container and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.
[0070] The obtained solid electrolyte slurry was applied onto an aluminum (Al) foil as a release sheet by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100°C to form a solid electrolyte layer. Three solid electrolyte layers were produced.
[0071] Preparation of Positive Electrode Mixture A polypropylene container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and VGCF as a conductive additive were added to the container and stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT Co., Ltd.). Next, the container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.), further stirred for 30 seconds with the ultrasonic dispersion device, and shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).
[0072] <Formation of Positive Electrode Active Material Layer> The obtained positive electrode mixture slurry was applied onto an Al foil serving as a positive electrode current collector layer by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100°C, thereby forming a positive electrode active material layer on the positive electrode current collector layer.
[0073] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.
[0074] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.
[0075] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.
[0076] The positive electrode laminate and the negative electrode laminate were laminated on top of each other so that the solid electrolyte layer side of each laminate faced the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a press temperature of 120° C. Thus, an all-solid-state battery was obtained.
[0077] "evaluation" <Average particle size> The average particle diameter of the silicon clathrate active material particles and the AlF3 particles was calculated by obtaining a cross-sectional image of the negative electrode active material layer using a scanning electron microscope (SEM) and analyzing the obtained image. Specifically, the average value of the circle-equivalent diameter of the silicon clathrate active material particles and the AlF3 particles was calculated for 100 or more samples.
[0078] <AlF3 / Si (particle size)> The average particle size of the AlF3 particles was divided by the average particle size of the silicon clathrate active material particles to calculate AlF3 / Si (particle size).
[0079] <AlF3 / Si (area)> The cross section of the obtained negative electrode active material layer was observed by SEM-EDX measurement, and AlF3 / Si (area) was calculated from the ratio of the area of the area showing aluminum fluoride particles to the area of the area showing silicon clathrate active material particles.
[0080] <Expansion amount> The produced battery was restrained at a predetermined restraining pressure using a restraining jig, and was charged at a constant current and constant voltage up to 4.55 V at a 10-hour rate (1 / 10C), during which the increase in restraining pressure was measured and taken as the amount of expansion in the present disclosure. The increase in restraining pressure is the difference between the maximum and minimum values of the restraining pressure, and the values in the examples are shown as relative values when the value in Comparative Example 1 is taken as 100.
[0081] "result" The results of the above evaluations for each example are shown in Table 1. In Table 1, "Classification of AlF3" indicates the presence or absence of classification using a metal sieve and the mesh size of the metal sieve. Also, "Si" indicates silicon clathrate active material particles.
[0082] [Table 1]
[0083] As shown in Table 1, the expansion rates of the batteries of Examples 1 to 4, in which the average particle size of the AlF3 particles was within the range of the present disclosure, were small. The expansion rates of the battery of Example 3, in which the average particle size of the AlF3 particles was 1.2 μm, and the battery of Example 4, in which the average particle size of the AlF3 particles was 0.9 μm, were even smaller, and the expansion rate of the battery of Example 2, in which the average particle size of the AlF3 particles was 1.3 μm, was the smallest.
Claims
1. An electrode mixture comprising silicon clathrate active material particles and aluminum fluoride particles, the aluminum fluoride particles having an average particle size of 3.0 μm or less.
2. 2. The electrode mixture according to claim 1, wherein the aluminum fluoride particles have an average particle size of 0.1 μm or more and 2.5 μm or less.
3. The electrode mixture according to claim 2 , wherein the aluminum fluoride particles have an average particle size of 0.8 μm or more and 1.8 μm or less.
4. 2. The electrode mixture according to claim 1, wherein a ratio of an average particle size of the aluminum fluoride particles to an average particle size of the silicon clathrate active material particles is 2.5 or less.
5. 2. The electrode mixture according to claim 1, wherein when a cross section of the electrode mixture is observed by SEM-EDX measurement, the ratio of the content of the aluminum fluoride particles to the content of the silicon clathrate active material particles is less than 2.0 area%.
6. An electrode active material layer is provided, and The electrode active material layer contains the electrode mixture according to any one of claims 1 to 5. Lithium-ion battery.
Citation Information
Patent Citations
Method for manufacturing negative electrode active material
JP2023043948A
Electrode body, lithium ion battery, and method of producing active material for lithium ion battery
JP2024008702A
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158004A