Plated material and electric wire with terminal using the same, connector, and wire harness

A silver-tin alloy plating with isotropically arranged Ag3Sn crystal grains addresses silver precipitation issues in vehicle connectors, enhancing environmental and wear resistance while reducing heat generation and contact resistance.

JP2024158864AInactive Publication Date: 2024-11-08YAZAKI CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023074447
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Charging connectors in hybrid and electric vehicles face issues with environmental resistance due to silver-tin plating prone to silver precipitation in high-temperature, high-humidity environments, and salt water exposure, despite the need for wear resistance and low heat generation.

Method used

A plating material with a silver-tin alloy layer containing isotropically arranged Ag3Sn crystal grains, with a Sn grain proportion of 2.0% to 11.0% and a Vickers hardness of 180 Hv to 310 Hv, is applied to terminals, terminals, and wire harnesses, using a specific plating process to enhance environmental resistance and wear resistance.

Benefits of technology

The solution provides improved environmental resistance and wear resistance, minimizing silver migration and contact resistance, suitable for high-current applications in vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158864000001_ABST
    Figure 2024158864000001_ABST
Patent Text Reader

Abstract

To provide a plated material with improved environmental resistance and an electric wire with a terminal using the same, a connector, and a wire harness.SOLUTION: A plated material 1 comprises a metallic substrate 2 and a silver / tin alloy plated layer 3 including a silver / tin alloy disposed on the metallic substrate 2. The silver / tin alloy layer 3 includes crystal grains 60 of Ag3Sn, with the crystal grains 60 of Ag3Sn being isotropically arranged, and the ratio of the crystal grains 70 of Sn per observed area being 2.0% or more and 11.0% or less upon observing the cross section of the silver / tin alloy plated layer 3 by an FE-SEM.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plated material, and to an electric wire with a terminal, a connector, and a wire harness each using the same. [Background technology]

[0002] In recent years, the demand for hybrid and electric vehicles has been increasing. These vehicles use high-power motors, so large currents flow through their wiring and terminals, generating a large amount of heat. For this reason, silver plating, which generates less heat, is used for the terminals used in these vehicles. Furthermore, charging connectors used in hybrid and electric vehicles are repeatedly inserted and removed, so it is desirable for them to be less prone to wear. For this reason, hard silver plating, which has improved wear resistance, is used for the terminals.

[0003] Since the Vickers hardness of hard silver plating is also about Hv140, in order to further improve wear resistance, it has been disclosed that the plating layer is made thicker or, as in Patent Document 1, silver-tin plating, which has a higher hardness than hard silver plating, is applied. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6172811 Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, charging connectors used in hybrid and electric vehicles require environmental resistance, but silver-tin plating has the problem of silver deposition on the surface (Ag migration) in high-temperature, high-humidity environments or after salt spray.

[0006] The present invention has been made in view of the problems inherent in the conventional techniques, and an object of the present invention is to provide a plated material having improved environmental resistance, and an electric wire with a terminal, a connector, and a wire harness each using the same. [Means for solving the problem]

[0007] A plating material according to an embodiment of the present invention includes a metal substrate and a silver-tin alloy plating layer disposed on the metal substrate and containing a silver-tin alloy. The silver-tin alloy plating layer is Ag. 3 Contains Sn crystal grains and Ag 3 The Sn crystal grains are isotropically arranged, and when a cross section of the silver-tin alloy plating layer is observed by FE-SEM, the ratio of the Sn crystal grains per observed area is 2.0% or more and 11.0% or less. Effect of the Invention

[0008] According to the present invention, it is possible to provide a plated material having improved environmental resistance, and an electric wire with a terminal, a connector, and a wire harness using the same. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic diagram showing an example of a plating material according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a plating material according to the present embodiment. [Diagram 3] 1A is a field emission scanning electron microscope (FE-SEM) photograph showing an enlarged cross section of a silver-tin alloy plating layer in which (a) Ag3Sn crystal grains are arranged isotropically and (b) Ag3Sn crystal grains are arranged in a columnar shape. [Figure 4] Photographs of the surface of the silver-tin alloy plating layer of test pieces having a silver-tin alloy plating layer in which (a) Ag3Sn crystal grains are arranged isotropically and (b) Ag3Sn crystal grains are arranged columnarly, after a high-temperature, high-humidity test and a salt spray test. [Diagram 5] FIG. 2 is a perspective view showing an example of an electric wire with a terminal according to the present embodiment before the electric wire is crimped with the terminal. [Figure 6] FIG. 2 is a perspective view showing an example of an electric wire with a terminal according to the present embodiment after the electric wire is crimped with the terminal. [Figure 7] 1 is a perspective view showing an example of a wire harness according to an embodiment of the present invention. [Figure 8] 1 is an FE-SEM photograph (magnification: 25,000) showing an enlarged cross section of a silver-tin alloy plating layer in (a) Example 1, (b) Example 2, and (c) Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a plating material according to the present embodiment, a terminal using the plating material, and an electric wire, a connector, and a wire harness including the terminal will be described in detail with reference to the drawings. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0011] [Plating material 1] The plating material 1 of this embodiment includes a metal substrate 2 and a silver-tin alloy plating layer 3 containing a silver-tin alloy that is disposed on the metal substrate 2. Therefore, the plating material 1 of this embodiment has a smaller electrical resistance than conventional tin plating and is less likely to generate heat even in places where a high current flows, such as in hybrid cars and electric cars.

[0012] The silver-tin alloy plating layer 3 contains an intermetallic compound of silver and tin. The surface of the silver-tin alloy plating layer 3 in the plating material 1 preferably has a Vickers hardness of 180 Hv or more and 310 Hv or less. Therefore, the plating material 1 of this embodiment has high wear resistance, and when used as a terminal, the plating layer is not easily worn even if the terminal is repeatedly inserted and removed. Therefore, the contact resistance is small, and when used as a terminal, heat generation can be suppressed and power consumption can be reduced. Details of each configuration of this embodiment will be described below.

[0013] (Metal base material 2) The metal substrate 2 is a material to be plated with the silver-tin alloy plating layer 3. As a material for forming the metal substrate 2, a metal having high electrical conductivity, for example, at least one selected from the group consisting of copper, copper alloy, aluminum, aluminum alloy, iron, iron alloy, magnesium, and magnesium alloy, can be used. The specific shape of the metal substrate 2 is not particularly limited, and may be a shape according to the application.

[0014] (Silver-tin alloy plating layer 3) As shown in Fig. 1, the silver-tin alloy plating layer 3 is disposed on a metal substrate 2. The silver-tin alloy plating layer 3 serves to protect the metal substrate 2 from corrosion. From the viewpoints of corrosion prevention and formability, it is preferable that the silver-tin alloy plating layer 3 covers the entire metal substrate 2.

[0015] The Sn content in the silver-tin alloy plating layer 3 is preferably 26 mass % to 38 mass %. Furthermore, the silver-tin alloy plating layer 3 preferably contains at least one element selected from the group consisting of In, Zn, Ti, and Sb, in addition to silver and tin. This is because the silver-tin alloy plating layer 3 contains such an element, which generates an intermetallic compound with silver, and is expected to improve the surface hardness of the silver-tin alloy plating layer 3.

[0016] The silver-tin alloy plating layer 3 contains an intermetallic compound of silver and tin. Examples of the intermetallic compound of silver and tin include Ag 3 In the present embodiment, the silver-tin alloy plating layer 3 contains an intermetallic compound, which can improve the hardness of the silver-tin alloy plating layer 3. Such an intermetallic compound is precipitated by controlling the concentrations of silver ions and tin ions in the plating bath. Other intermetallic compounds include, in addition to silver and tin, an intermetallic compound containing at least one element selected from the group consisting of In, Zn, Ti, and Sb, such as Ag, 3 In, AgZn, AgTi, Ag 7 Examples include Sb.

[0017] As shown in Fig. 3(a), the silver-tin alloy plating layer 3 contains Sn crystal grains in addition to the intermetallic compounds. When the cross section of the silver-tin alloy plating layer is observed by FE-SEM, the ratio of Sn crystal grains per observed area is 2.0% or more and 11.0% or less. In this state, the silver-tin alloy plating layer 3 contains Sn crystal grains, which results in Ag 3 The Sn crystal grains are prevented from growing columnarly (as shown in Fig. 3(b)). As a result, the Ag grains are prevented from growing columnarly (as shown in Fig. 3(a)). 3 The Sn crystal grains are aligned isotropically. In addition, the reference numeral 60 in FIG. 3(a) and (b) represents Ag. 3 The reference numeral 70 in FIG. 3(a) denotes a Sn crystal grain.

[0018] Furthermore, Ag of the silver-tin alloy plating layer 3 3 Since the Sn crystal grains are isotropically arranged, the occurrence of Ag migration in a high temperature and high humidity environment or after salt water spray (example shown in Fig. 4(b)) is suppressed, and as a result, no Ag migration is observed as shown in Fig. 4(a). Note that reference numeral 80 in Fig. 4(b) indicates the location on the surface of the silver-tin alloy plating layer 3 where Ag migration has occurred.

[0019] From the viewpoint of wear resistance, the Vickers hardness of the surface of the silver-tin alloy plating layer 3 in the plated material 1 is preferably 180 Hv or more and 310 Hv or less. The Vickers hardness can be measured in accordance with Japanese Industrial Standard JIS Z2244:2009 (Vickers hardness test - Test method).

[0020] From the viewpoint of corrosion resistance, the thickness of the silver-tin alloy plating layer 3 is preferably 0.1 μm or more, and more preferably 1 μm or more. From the viewpoint of productivity and cost reduction, the thickness of the silver-tin alloy plating layer 3 is preferably 30 μm or less, and more preferably 20 μm or less.

[0021] The silver-tin alloy plating layer 3 can be formed, for example, by mixing a tin salt into a silver plating bath to prepare a silver-tin alloy plating bath, and immersing the metal substrate 2 in the silver-tin alloy plating bath for plating. The plating process is preferably constant current electrolysis, since it is easy to control the film thickness.

[0022] The silver-tin plating bath used for the silver-tin alloy plating layer 3 may contain, for example, silver salt, tin salt, conductive salt, brightener, etc. Examples of materials used for the silver salt include at least one salt selected from the group consisting of silver cyanide, silver iodide, silver oxide, silver sulfate, silver nitrate, silver methanesulfonate, and silver chloride. Examples of the conductive salt include at least one salt selected from the group consisting of potassium cyanide, sodium cyanide, potassium pyrophosphate, silver methanesulfonate, potassium iodide, and sodium thiosulfate. Examples of the brightener include metal brighteners such as antimony, selenium, and tellurium, and organic brighteners such as benzenesulfonic acid and mercaptan. The silver ion concentration in the plating bath is preferably, for example, 30 g / L to 45 g / L.

[0023] Materials used for the tin salt of the silver-tin alloy plating layer 3 include at least one salt selected from the group consisting of stannous salts such as stannous methanesulfonate and other organic sulfonates, stannous pyrophosphate, stannous chloride, stannous sulfate, stannous acetate, stannous sulfamate, stannous gluconate, stannous tartrate, stannous oxide, stannous borofluoride, stannous succinate, stannous lactate, stannous citrate, stannous phosphate, stannous iodide, stannous formate, and stannous silicofluoride, and stannous salts such as sodium stannate and potassium stannate. The tin ion concentration in the plating bath is preferably, for example, 5 g / L to 9 g / L.

[0024] Ag in the silver-tin alloy plating layer 3 3 In order to arrange the Sn crystal grains isotropically, the current density in electrolytic plating of the silver-tin alloy plating layer 3 is 2.0 A / dm 2 ~7.0A / dm 2It is preferable that the current density is set to 100%. If the current density is increased, the silver-tin alloy plating can be performed in a shorter time, and the productivity is improved, but if the current density is increased, the surface tends to become rough. Therefore, the upper limit of the current density is set so as to satisfy the surface roughness conditions in consideration of various factors such as productivity, plating bath composition, ion concentration, and the shape of the plated object.

[0025] In addition, Ag in the silver-tin alloy plating layer 3 3 In order to arrange the Sn crystal grains isotropically, the plating bath temperature when electrolytically plating the silver-tin alloy plating layer 3 is preferably 0° C. to 50° C., and more preferably 20° C. to 36° C. By setting the plating bath temperature within this range, the silver-tin alloy plating layer 3 can be effectively formed by the complex effect.

[0026] (base layer 4) 2, the plating material 1 of this embodiment may further include an underlayer 4 in order to impart various functions. In this embodiment, the underlayer 4 is disposed between the metal substrate 2 and the silver-tin alloy plating layer 3.

[0027] The underlayer 4 preferably contains at least one metal selected from the group consisting of nickel, copper, and silver. Specifically, the underlayer 4 preferably contains at least one metal selected from the group consisting of nickel, a nickel alloy, copper, a copper alloy, silver, and a silver alloy.

[0028] When the underlayer 4 contains nickel or a nickel alloy, for example, the underlayer 4 can suppress the diffusion of elements constituting the metal base material into the silver-tin alloy plating layer 3, thereby improving contact reliability and heat resistance. That is, the underlayer 4 functions as a barrier layer. When the underlayer 4 contains either nickel or a nickel alloy, the layer thickness is not particularly limited as long as it functions as a barrier layer, but is preferably more than 0 μm and 3 μm or less, and more preferably 0.1 μm to 1.0 μm.

[0029] When the underlayer 4 contains at least one metal selected from the group consisting of copper, copper alloy, silver, and silver alloy, for example, the adhesion between the metal substrate 2 and the silver-tin alloy plating layer 3 can be improved. That is, the underlayer 4 functions as a strike plating layer. When the underlayer 4 contains at least one metal selected from the group consisting of copper, copper alloy, silver, and silver alloy, the layer thickness is not particularly limited as long as the adhesion is improved, and even a very thin layer thickness may improve the adhesion. Therefore, in this case, the layer thickness is preferably, for example, more than 0 μm and 3 μm or less, and more preferably 0.1 μm to 1.0 μm.

[0030] The underlayer 4 may be a single layer or multiple layers. For example, the underlayer 4 may include a lower layer and an upper layer disposed on the lower layer. For example, the lower layer of the underlayer 4 may include either nickel or a nickel alloy, and the upper layer of the underlayer 4 may include at least one metal selected from the group consisting of copper, a copper alloy, silver, and a silver alloy. Thus, for example, a nickel plating layer may be formed on the lower layer of the underlayer 4, and a silver strike plating layer may be formed on the upper layer of the underlayer 4. The combination of these layers may be appropriately changed depending on the purpose.

[0031] The method for forming the underlayer 4 is not particularly limited, but for example, the material to be plated, that is, the metal base material 2, can be placed in a plating bath and plated by a known plating method.

[0032] The plating material 1 of this embodiment includes a metal substrate 2 and a silver-tin alloy plating layer 3 that is disposed on the metal substrate 2 and contains a silver-tin alloy. The silver-tin alloy plating layer 3 contains Ag 3 Contains Sn crystal grains and Ag 3 The Sn crystal grains are isotropically arranged, and when the cross section of the silver-tin alloy plating layer is observed by FE-SEM, the ratio of the Sn crystal grains per observation area is 2.0% to 11.0%. Therefore, the plating material 1 of this embodiment has excellent environmental resistance when used as a terminal.

[0033] [Terminal 10] The terminal 10 of this embodiment is formed from a plating material 1. Therefore, the terminal 10 of this embodiment has high wear resistance while minimizing an increase in contact resistance, compared to a conventional terminal plated with silver or a silver alloy. From the viewpoints of corrosion prevention and formability, it is preferable that the silver-tin alloy plating layer 3 of the terminal 10 entirely covers the metal substrate 2 of the terminal 10.

[0034] [Terminal Wire 20] As shown in Fig. 5 and Fig. 6, the electric wire with terminal 20 of this embodiment includes a terminal 10. Specifically, the electric wire with terminal 20 of this embodiment includes an electric wire 30 having a conductor 31 and a wire coating material 32 that covers the conductor 31, and a terminal 10 that is connected to the conductor 31 of the electric wire 30 and is formed from a plating material. Note that Fig. 5 shows a state before the electric wire is crimped with the terminal, and Fig. 6 shows a state after the electric wire is crimped with the terminal.

[0035] The terminal 10 shown in FIG. 5 is a female crimp terminal. The terminal 10 has an electrical connection portion 11 that is connected to a mating terminal (not shown). The electrical connection portion 11 has a box-like shape and incorporates a spring piece that engages with the mating terminal. Furthermore, on the opposite side of the terminal 10 to the electrical connection portion 11, an electric wire connection portion 12 is provided that is connected to an end portion of the electric wire 30 by crimping. The electrical connection portion 11 and the electric wire connection portion 12 are connected via a connecting portion 13. Note that the electrical connection portion 11, the electric wire connection portion 12, and the connecting portion 13 are made of the same material and integrally constitute the terminal 10, but for convenience, names are given to each portion.

[0036] The electric wire connection portion 12 includes a conductor crimping portion 14 that crimps a conductor 31 of the electric wire 30 , and a covering material crimping portion 15 that crimps a wire covering material 32 of the electric wire 30 .

[0037] The conductor crimping portion 14 comes into direct contact with the conductor 31 exposed by removing the wire coating material 32 at the end portion of the electric wire 30, and has a bottom plate portion 16 and a pair of conductor clamping pieces 17. The pair of conductor clamping pieces 17 extend upward from both side edges of the bottom plate portion 16. The pair of conductor clamping pieces 17 are bent inward so as to wrap around the conductor 31 of the electric wire 30, thereby enabling the conductor 31 to be clamped so as to be in close contact with the upper surface of the bottom plate portion 16. The conductor crimping portion 14 is formed into a generally U-shaped cross section by the bottom plate portion 16 and the pair of conductor clamping pieces 17.

[0038] The covering material clamping portion 15 is in direct contact with the wire covering material 32 at the end portion of the electric wire 30, and has a bottom plate portion 18 and a pair of covering material clamping pieces 19. The pair of covering material clamping pieces 19 extend upward from both side edges of the bottom plate portion 18. The pair of covering material clamping pieces 19 are bent inward to wrap around the portion to which the wire covering material 32 is attached, so that the wire covering material 32 can be clamped in a state in which it is in close contact with the upper surface of the bottom plate portion 18. The covering material clamping portion 15 is formed into a generally U-shaped cross section by the bottom plate portion 18 and the pair of covering material clamping pieces 19. The bottom plate portion 16 of the conductor crimping portion 14 to the bottom plate portion 18 of the covering material clamping portion 15 are continuously formed as a common bottom plate portion.

[0039] The electric wire 30 has a conductor 31 and an electric wire covering material 32 that covers the conductor 31. The material of the conductor 31 may be a metal having high electrical conductivity. For example, copper, a copper alloy, aluminum, an aluminum alloy, or the like may be used. Note that in recent years, there has been a demand for lighter electric wires. For this reason, the conductor 31 is preferably made of lightweight aluminum or an aluminum alloy.

[0040] The material of the wire coating material 32 that covers the conductor 31 can be a resin that can ensure electrical insulation. For example, an olefin-based resin can be used as the material of the wire coating material 32. Specifically, the material of the wire coating material 32 can be mainly composed of at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), an ethylene copolymer, and a propylene copolymer. Also, the material of the wire coating material 32 can be mainly composed of polyvinyl chloride (PVC). Among these, it is preferable that the material of the wire coating material 32 contains polypropylene or polyvinyl chloride as the main component because of its high flexibility and durability. Here, the main component refers to a component that accounts for 50% by mass or more of the entire wire coating material 32.

[0041] The terminal 10 can be manufactured, for example, as follows. First, as shown in FIG. 5, the end portion of the electric wire 30 is inserted into the electric wire connection portion 12 of the terminal 10. As a result, the conductor 31 of the electric wire 30 is placed on the upper surface of the bottom plate portion 16 of the conductor crimping portion 14, and the portion of the electric wire 30 to which the electric wire coating material 32 is attached is placed on the upper surface of the bottom plate portion 18 of the coating material crimping portion 15. Next, the electric wire connection portion 12 and the end portion of the electric wire 30 are pressed to deform the conductor crimping portion 14 and the coating material crimping portion 15. Specifically, the pair of conductor crimping pieces 17 of the conductor crimping portion 14 are bent inward to encase the conductor 31, thereby crimping the conductor 31 so as to be in close contact with the upper surface of the bottom plate portion 16. Furthermore, the pair of coating material clamping pieces 19 of the coating material clamping portion 15 are bent inward to enclose the portion with the wire coating material 32 attached, thereby clamping the wire coating material 32 so that it is in close contact with the upper surface of the bottom plate portion 18. In this manner, the terminal 10 and the wire 30 can be crimped and connected, as shown in FIG.

[0042] The electric wire with terminal 20 of this embodiment includes a terminal 10. Therefore, the electric wire with terminal 20 of this embodiment has high wear resistance at the terminal 10 portion compared to conventional terminals plated with silver or silver alloy, and an increase in contact resistance can be minimized. Therefore, the electric wire with terminal 20 of this embodiment can be suitably used in places such as hybrid cars and electric cars.

[0043] [Wire harness] The wire harness 40 of this embodiment includes the electric wires with terminals 20. Specifically, the wire harness of this embodiment includes a connector 50 and the electric wires with terminals 20, as shown in FIG.

[0044] 7, a rear side of the connector 50 is provided with a plurality of mating terminal mounting portions (not shown) in which mating terminals (not shown) are mounted. A front side of the connector 50 is provided with a plurality of cavities 51 in which the terminals 10 of the electric wire with terminal 20 are mounted. Each cavity 51 is provided with a substantially rectangular opening so that the terminals 10 of the electric wire with terminal 20 are mounted. Furthermore, the opening of each cavity 51 is formed to be slightly larger than the cross section of the terminals 10 of the electric wire with terminal 20. When the terminals 10 of the electric wire with terminal 20 are mounted in the cavities 51 of the connector 50, the electric wire 30 is drawn out from the rear side of the connector 50.

[0045] The wire harness 40 of this embodiment includes the electric wires with terminals 20. Therefore, the wire harness 40 of this embodiment has high wear resistance at the terminals 10 compared to conventional terminals plated with silver or silver alloy, and can minimize an increase in contact resistance. Therefore, the wire harness 40 of this embodiment can be suitably used in places such as hybrid cars and electric cars.

[0046] The terminal 10, the electric wire with terminal 20, and the wire harness 40 according to the present embodiment have been described above, but the present embodiment is not limited to the above embodiment and may be used, for example, as a charging cable including the terminal 10. Such a charging cable is repeatedly inserted and removed in, for example, an electric vehicle, and the electric wire is crimped, so that the provision of the terminal 10 makes it suitable for use as a charging cable. EXAMPLES

[0047] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0048] First, the metal substrate to be plated was pretreated. Specifically, the metal substrate was washed with an alkaline degrease, pickled by immersing in 10% sulfuric acid for 1 minute, and then rinsed with water. The metal substrate used was a C1020-1 / 2H copper plate with a thickness of 0.25 mm, as specified in JIS H3100:2012 (copper and copper alloy plates and strips). For the evaluation of the muddy saltwater sliding test, a test piece in which the metal substrate was embossed to a radius of 1 mm was used.

[0049] Next, a nickel plating layer was formed on the metal substrate. The nickel plating layer was the lower layer of the undercoat layer. Specifically, the metal substrate pretreated as described above was immersed in a plating bath for the nickel plating layer, and a current density of 10 A / dm was applied using a DC stabilized power source. 2 The electrolysis was carried out at a constant current under the conditions of an electrolysis time of 2 minutes and a plating bath temperature of 45°C.

[0050] Then, a silver strike plating layer was formed on the nickel plating layer. The silver strike plating layer is an upper layer of the underlayer, and can improve the adhesion between the nickel plating layer and the silver-tin alloy plating layer. Specifically, the metal substrate on which the nickel plating layer was formed was immersed in a plating bath for the silver strike plating layer, and a current density of 2.5 A / dm was applied using a DC stabilized power source. 2 Constant current electrolysis was performed under the conditions of 1 min electrolysis time and 25°C plating bath temperature. After completion of electrolysis, the metal substrate was removed from the plating bath and washed with water. As a result, a metal substrate was obtained in which a silver strike plating layer was formed over the entire surface of the metal substrate on which the nickel plating layer was formed. The composition of the plating bath for the silver strike plating layer was 4.2 g / L silver cyanide and 80 g / L potassium cyanide. The thickness of the silver strike plating layer was 0.3 μm. The DC stabilized power supply used was PA18-5B manufactured by Texio Technology Co., Ltd.

[0051] Furthermore, a silver-tin alloy plating layer was formed on the silver strike plating layer. Specifically, the metal substrate on which the silver strike plating layer was formed was immersed in a plating bath in which the silver ion concentration and tin ion concentration were adjusted as shown in Table 1, and constant current electrolysis was performed using a DC stabilized power supply. The electrolysis conditions (current density, plating bath temperature, stirring speed, stirring method) were as shown in Table 1. After the electrolysis was completed, the metal substrate was removed from the plating bath and washed with water. The electrolysis time was adjusted so that the thickness of the plating layer formed was 20 μm. The DC stabilized power supply used was PA18-5B manufactured by Texio Technology Co., Ltd.

[0052] [evaluation] The test pieces of the examples and comparative examples were evaluated by the following methods. The results are shown in Table 1.

[0053] (Sn content in silver-tin alloy plating layer) The Sn content of the silver-tin alloy plating layer was confirmed by analyzing the obtained test pieces using a scanning electron microscope (SEM)-energy dispersive X-ray spectroscopy (EDX).

[0054] (Intermetallic compounds in silver-tin alloy plating layer) Regarding the intermetallic compounds in the silver-tin alloy plating layer, the obtained test pieces were subjected to X-ray crystal structure analysis using an X-ray diffraction device (XRD) to determine the presence of Ag 3 It was confirmed to be Sn.

[0055] (Ag 3 Sn crystal grain shape) A cross section (cross-sectional area 1 cm ) cut from the obtained test piece 2 The sample was prepared by ion milling or the like, and the cross section was observed by FE-SEM (JEOL Ltd., device name: JSM-7600F). The FE-SEM observation results are shown in FIG. 8. The reference numeral 61 in FIG. 8 denotes Ag 3 The Sn crystal grains are shown in FIG. 8(a) and FIG. 8(b), and the Ag crystal grains are shown in FIG. 3 It was confirmed that the Sn crystal grains were aligned isotropically. On the other hand, no Sn crystal grains were observed in Fig. 8(c), and the Ag 3It was confirmed that the Sn crystal grains were arranged in a columnar shape.

[0056] (Sn grain ratio) The image data acquired by the FE-SEM was imported into the software (OLYMPUS Stream) of a system inverted metallurgical microscope (Olympus Corporation, device name: GX51), and the image was analyzed by binarization using the image editing function. The ratio of Sn crystal grains per observation area was calculated from the area ratio of the image.

[0057] (Check for Ag migration) The obtained test pieces were subjected to a high temperature and humidity test (temperature 80°C, humidity 90RH%, test time 100 hours) or a salt spray test (salt water concentration 5wt%, temperature 35°C, test time 100 hours). After the test, the whitened parts of the samples were analyzed with an EDS (energy dispersive X-ray spectroscope) to confirm the presence or absence of Ag migration, as shown in Figure 4.

[0058] (Vickers hardness) The Vickers hardness was evaluated by measuring the surface of the obtained test piece using a microhardness tester (manufactured by Shimadzu Corporation, device name: DUH-211) in accordance with JIS Z2244: 2009. The test temperature was 25°C and the test force was 5 gf.

[0059] (Mud salt water sliding test) The mud saltwater sliding test was performed using a load-varying friction and wear tester (Shinto Scientific Co., Ltd., device name: HHS2000S) and was evaluated by the following method. First, quartz glass was used as the mating material for the test piece embossed with a radius of 1 mm. The mud saltwater was prepared by adjusting the content of special grade sodium chloride (Kishida Chemical Co., Ltd.) and AC dust (ISO12103-1 (2016), A4 (Coarse)) to 5 wt%, with the remainder being pure water. The test conditions were load: 2 N, sliding distance: 2 mm, sliding speed: 5 mm / s, and number of sliding: 300 times. The test was performed while supplying 100 μL of the adjusted mud saltwater every 10 sliding times. The wear marks on the test piece after the test were approximated by the area of ​​a circle, and the wear volume was calculated from that area. The results of the muddy saltwater sliding test were as follows: the wear volume calculated using the above method was greater than or equal to the wear volume of the Ag-2wt%Sb plating (828100μm 3 ) was rated as pass (◯), and the wear volume of the Ag-2wt%Sb plating or more was rated as fail (×).

[0060] [Table 1]

[0061] From Table 1 and Figs. 8(a) and (b), the test pieces of Examples 1 to 5 are Ag 3 The Sn crystal grains are isotropically arranged, and when the cross section of the silver-tin alloy plating layer is observed by FE-SEM, the ratio of Sn crystal grains is 2.0% or more and 11.0% or less. After the high temperature and high humidity test or the salt spray test, no Ag migration was observed. In addition, the Vickers hardness is 180Hv or more and 310Hv or less, and the result of the muddy salt water sliding test was also passed. Therefore, the wear resistance and environmental resistance are excellent.

[0062] From the results of Table 1 and FIG. 8(c), the test piece of Comparative Example 1 has Ag 3The crystal grains of Sn were arranged in a columnar shape. In the test piece of Comparative Example 1, Ag migration occurred after the high temperature and high humidity test and the salt spray test, but the Vickers hardness was 180 Hv or more and 310 Hv or less, and the result of the muddy saltwater sliding test was pass. Therefore, the wear resistance of Comparative Example 1 was good, but the environmental resistance was not sufficient. On the other hand, the test piece of Comparative Example 2 had a ratio of Sn crystal grains exceeding 11.0% when the cross section of the silver-tin alloy plating layer was observed by FE-SEM. In addition, the Vickers hardness was less than 180 Hv, and the result of the muddy saltwater sliding test was fail.

[0063] The present invention has been described above with reference to examples and comparative examples, but the present invention is not limited to these. However, various modifications are possible within the scope of the present invention. [Explanation of symbols]

[0064] 1. Plating materials 2 Metal base material 3. Silver-tin alloy plating layer 4 Base layer 10 Terminals 20 Wire with terminal 40 Wire Harness 50 Connectors 60Ag 3 Sn crystal grains 70 Sn grains

Claims

1. A metal substrate; a silver-tin alloy plating layer disposed on the metal substrate and containing a silver-tin alloy; Equipped with The silver-tin alloy plating layer is Ag 3 The Ag 3 A plated material in which Sn crystal grains are isotropically arranged, and when a cross section of a silver-tin alloy plating layer is observed by FE-SEM, the ratio of Sn crystal grains per observation area is 2.0% or more and 11.0% or less.

2. The plated material according to claim 1, wherein the Sn content in the silver-tin alloy plating layer is 26% by mass to 38% by mass.

3. 3. The plated material according to claim 1, wherein the Vickers hardness of the surface of the silver-tin alloy plating layer is 180 Hv or more and 310 Hv or less.

4. 3. The plating material according to claim 1, further comprising an underlayer disposed between the metal substrate and the silver-tin alloy plating layer, the underlayer containing at least one metal selected from the group consisting of nickel, copper, and silver.

5. A terminal formed from the plating material according to claim 1 or 2.

6. A terminal-attached electric wire comprising the terminal according to claim 5 .

7. A connector comprising the electric wire with terminal according to claim 6.

8. A wire harness comprising the connector according to claim 7.

Citation Information

Patent Citations

  • Surface treatment plating material and method for manufacturing the same, and electronic component

    JP2014077190A

  • Method for manufacturing metal laminate containing silver-tin alloy plating layer

    JP2015054979A

  • Plating material for terminal and terminal therewith, electric wire with terminal and wire harness

    JP2018120698A

  • Terminal material for connector, terminal for connector, and manufacturing method of terminal material for connector