Residual expansion amount measuring method
The simulated energization test method effectively predicts residual expansion in concrete with delayed-reactive aggregates, enabling precise repair strategies by measuring alkali-silica reaction progression.
Patent Information
- Application Number
- JP2023074529
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional accelerated expansion tests, such as the Canadian and Danish methods, are ineffective for concrete containing delayed-reactive aggregates, as they fail to predict the actual ASR expansion that occurs in such structures.
A simulated energization test method involving a core specimen from concrete structures, where a steel material is inserted into a hole, immersed in an electrolytic solution, and subjected to electricity for a period, followed by curing to measure residual expansion, using electrolytes like alkali metal solutions and specific conditions to promote the alkali-silica reaction.
Enables accurate prediction of residual expansion in concrete with delayed-reactive aggregates, allowing for appropriate repair methods, including the selection of effective electrolytes for electrochemical corrosion protection.
Smart Images

Figure 2024158905000002 
Figure 2024158905000003 
Figure 2024158905000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for measuring the residual expansion of a concrete structure. [Background technology]
[0002] The causes of deterioration of concrete structures include alkali-silica reaction, carbonation of concrete, and salt damage. Repair methods that apply electrochemical techniques are used to remove carbonation and salt damage of concrete. Specifically, this is a desalination method in which chloride ions in the concrete are extracted outside the concrete surface by passing a direct current between the reinforcing bars (steel) inside the concrete and an anode on the surface of the concrete, via an alkaline electrolyte solution. It is also a method of re-alkalinizing neutralized concrete by electrically penetrating an alkaline substance, such as an aqueous solution of an alkali metal, into the concrete.
[0003] However, aqueous solutions of alkali metals can promote alkali-silica reaction (ASR), a phenomenon in which alkali-reactive aggregates in concrete react with alkali from cement, producing expansive ASR gel inside the aggregate, which leads to expansion cracks in the concrete. Therefore, predicting the progression of ASR in concrete structures is important for the maintenance and management of concrete structures, and for concrete structures in which ASR has occurred, it is extremely important to predict whether or not further expansion will occur in the future.
[0004] The commonly used method for predicting whether or not future expansion will occur is to conduct accelerated expansion tests on concrete core specimens (hereinafter referred to as "core specimens" or simply "specimens") taken from a concrete structure to measure the amount of remaining expansion (future expansion). Accelerated expansion test methods include the Canadian method, the Danish method, the JCI-DD2 method, etc. All of these methods involve storing the product under certain conditions and measuring the degree of expansion according to their respective criteria. For example, in the Canadian method, a test specimen is immersed in a 1 mol / L NaOH solution at 80±2°C, and the amount of expansion after 14 days from the start of the test is judged according to the following criteria (ASTM C1260-94). Below 0.10%: Harmless 0.10-0.20%: Contains both harmful and non-harmful aggregates. Over 0.20%: Potentially harmful expansion Based on the above evaluation results, if the amount of expansion is 0.10% or less, a repair method applying electrochemical methods is used, whereas if it is 0.20% or more, methods other than electrochemical methods have been used. For example, in the case of cracked or missing concrete, cross-sectional repair is carried out by chipping off the concrete in that area and then filling it with new concrete or mortar.
[0005] Methods for predicting the above-mentioned amount of expansion (expansion rate) include, for example, Patent Documents 1 and 2 below. Patent Document 1 discloses a method for predicting future expansion rates by taking a first concrete specimen from a healthy part of a concrete structure and a second concrete specimen from a deteriorated part, conducting an accelerated expansion test on each concrete specimen, and obtaining changes in the accelerated expansion rate over time. Furthermore, Patent Document 2 discloses a method for predicting the progression of deterioration of a concrete structure due to alkali-silica reaction, which predicts the progression of deterioration of a concrete structure deteriorated by alkali-silica reaction based on the correlation between the expansion rate of concrete in an accelerated expansion test of concrete sampled from the concrete structure and the alkali hydroxide concentration of concrete sampled from the concrete structure.
[0006] The prediction methods disclosed in Patent Documents 1 and 2 are both methods in which an accelerated expansion test is performed, and the expansion rate due to ASR is predicted from the change in the expansion rate due to the accelerated expansion test. Patent Document 1 states that the accelerated expansion test may be performed by selecting from among publicly known test methods as appropriate, such as by extending the test period of the Canadian method, the Danish method, or the method specified in JIS A 1804 (see paragraph 0025 of Patent Document 1). Furthermore, Patent Document 2 states that examples of accelerated expansion tests include a saturated sodium chloride solution immersion method at 50°C (corresponding to the Danish method) and an accelerated test in a 1N sodium hydroxide solution at 80°C (NBRI test, corresponding to the Canadian method), with the NBRI test being preferred (Patent Document 2, paragraph 0010). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2010-243397 A [Patent Document 2] JP 2001-99833 A Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, Patent Documents 1 and 2 use conventionally known accelerated expansion tests such as the Canadian method and the Danish method. However, while these accelerated expansion tests are effective for normal reactive aggregates, it has been found that concrete specimens containing delayed-reactive aggregates may not expand under the conditions of the Canadian method, etc. Therefore, in concrete containing delayed-reactive aggregates, the results of accelerated expansion tests such as the Canadian method may not reflect the ASR that actually occurs. Therefore, an object of the present invention is to provide an accelerated expansion test method that is effective for concrete containing delayed-reactive aggregate as a preliminary investigation for electrochemical corrosion protection methods, as an alternative to conventional accelerated expansion tests. [Means for solving the problem]
[0009] As a result of intensive research to solve the above problems, it has been found that by taking a core specimen from a concrete structure and conducting a simulated current test using an electrochemical method such as a desalination method or a re-alkalization method, it is possible to effectively predict the residual expansion amount, thereby solving the above problems. That is, the present invention is as follows. [1] A method for measuring the amount of residual expansion using a simulated current test, which involves taking a core specimen from a concrete structure, drilling a hole in the core specimen, inserting a steel material into the hole, immersing a portion of the core specimen in an electrolyte, passing a current between the steel material, which is the cathode, and the anode in the electrolyte for a certain period of time, then curing the core specimen to promote the alkali-silica reaction, and then measuring the expansion rate. [2] The method for measuring the residual expansion amount by a simulated current test according to the above [1], wherein the electrolyte is an aqueous alkali metal solution. [3] The current density per surface area of concrete is 0 to 5 A / m 2 The method for measuring residual expansion amount by a simulated current test according to the above [1] or [2]. [4] The method for measuring residual expansion by a simulated electric current test according to any one of the above [1] to [3], wherein the gap between the steel material and the hole is filled with cement paste or a saturated calcium hydroxide aqueous solution. [5] The method for measuring a residual expansion amount by a simulated current test according to any one of the above [2] to [4], wherein the alkali metal is at least one selected from the group consisting of lithium, sodium and potassium. [6] The method for measuring residual expansion amount by a simulated current test according to the above item [5], wherein the alkali metal is lithium or potassium. [7] The method for measuring a residual expansion amount by a simulated current test according to any one of the above [1] to [6], wherein the electrolyte is a carbonate. [8] The method for measuring residual expansion amount by a simulated current test according to any one of the above [1] to [7], wherein the current-flow period is 7 to 80 days. [9] The method for measuring a residual expansion amount by a simulated current test according to any one of the above [1] to [8], wherein the curing is carried out under any one of the following conditions (1) to (3): (1) Keep the container in an atmosphere of 20 to 40°C and a relative humidity of 95% or more. (2) Immerse in a 1 mol / L NaOH solution at 80°C. (3) Immerse in a saturated NaCl aqueous solution at 50°C.
[10] The method for measuring the amount of residual expansion by a simulated current test according to the above [9], wherein the curing period is 7 to 365 days.
[11] The method for measuring residual expansion by a simulated electric current test according to any one of the above [1] to
[10] , wherein the core specimen is cylindrical, has a diameter of 40 to 120 mm, and a height of 120 to 320 mm.
[12] The method for measuring residual expansion by a simulated current test according to any one of the above [1] to
[11] , wherein the steel material is a cathode and titanium is an anode.
[13] The method for measuring a residual expansion amount by a simulated electric current test according to any one of the above [1] to
[12] , wherein at least one of a pH in the electrolyte, a chloride ion concentration, and an inter-electrode potential difference is measured during the electric current. Effect of the Invention
[0010] According to the present invention, it is possible to provide an accelerated expansion test method which is effective even for concrete containing delayed-reactive aggregate. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing a core specimen used in the method of the present invention. [Diagram 2] 1 is a photograph showing a simulated current test device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Method of measuring residual expansion amount by simulated current test] The method for measuring residual expansion of the present invention (hereinafter sometimes referred to as "the method of the present invention") is characterized in that a core specimen is taken from a concrete structure, a hole is formed in the core specimen, a steel material is inserted into the hole, a part of the core specimen is immersed in an electrolyte, a current is passed between the steel material and an anode in the electrolyte for a certain period of time, the core specimen is then cured to promote the alkali-silica reaction, and the expansion rate is then measured. The concrete structure to which the method of the present invention is applied is not particularly limited, but a suitable example is a concrete structure containing delayed-reactive aggregate, the difference of which cannot be detected by conventional accelerated expansion tests. Examples of delayed-reactive aggregate include chert, which has good physical properties as an aggregate, such as particle size and strength. The method of the present invention will now be described in detail.
[0013] <Core specimen> In the method of the present invention, a core specimen is first taken from a concrete structure. The shape and size of the core specimen are not particularly limited as long as the effects of the present invention are achieved, but from the viewpoints of ease of handling and ease of taking from the site, for example, a cylindrical shape as shown in Fig. 1 is preferable. The diameter of the core specimen is preferably in the range of 40 to 120 mm, more preferably in the range of 50 to 110 mm, and even more preferably in the range of 60 to 100 mm, from the standpoint of ease of handling and the ease of making holes (hereinafter sometimes referred to as "hole drilling") as described in detail below. In addition, the height of the core specimen is preferably in the range of 120 to 320 mm, more preferably in the range of 150 to 300 mm, and even more preferably in the range of 180 to 250 mm, from the viewpoint of allowing for sufficient drilling depth.
[0014] <Drilling and steel materials> In the present invention, a drilled hole is formed in the core specimen to insert a steel material as an electrode. The shape of the drilled hole is also preferably cylindrical, and the inner diameter is not particularly limited as long as the steel material can be inserted. Specifically, it may be determined according to the diameter of the steel material. For example, the inner diameter of the drilled hole is preferably in the range of 5 to 25 mm, and more preferably in the range of 10 to 20 mm. From the viewpoint of workability of drilling, the depth of the drilling is preferably in the range of 80 / 100 to 95 / 100 of the height of the core specimen, more preferably in the range of 85 / 100 to 90 / 100. For example, when the core height is 200 mm, the depth of the drilling is preferably about 175 mm. The drilling may penetrate the core specimen, but it is necessary to insulate it so as not to come into contact with the electrolyte, which will be described later in detail.
[0015] The shape of the steel material is not particularly limited as long as it is within the range in which the effects of the present invention can be obtained, and may be, for example, round steel. The diameter of the round steel may be any diameter that allows it to be inserted into the above-mentioned drilled hole, but from the viewpoints of ease of fixing to the core and ease of current flow, it is preferable that the diameter is about 1 to 3 mm smaller than the inner diameter of the drilled hole.
[0016] It is preferable to fill the gap between the steel material and the hole with cement paste or a saturated calcium hydroxide aqueous solution (hereinafter sometimes referred to as "filler"). These fillers allow the steel material to be fixed in the hole. From the viewpoint of fixing the steel material, it is more preferable to use cement paste. There are no particular limitations on the cement paste as long as it can fix the steel material in the hole. For example, a cement paste with a water to cement ratio (water / cement) of about 30 to 60 mass%, preferably 40 to 50 mass%, can be used.
[0017] <Electrolyte> In the present invention, as described above, a hole is drilled in a core specimen taken from a concrete structure, a steel material is inserted into the hole, and a filler material is filled into the gap between the inner wall of the hole and the steel material. A part of the sample (hereinafter sometimes referred to as a "core sample") thus prepared is immersed in an electrolyte. Specifically, as shown in the photograph of FIG. 2, at least a part of the core sample is immersed in an electrolyte, and a current is passed between the steel material and the electrolyte for a certain period of time. The electrolyte constituting the electrolytic solution reduces the electrical resistance of the core sample by penetrating into the core sample, and facilitates the flow of electricity, and may be any solution in which positive and negative ions are present. Specifically, an aqueous solution in which various alkali metal salts or alkaline earth metal salts are dissolved as solutes in water as a solvent is preferably used. Examples of alkali metal salts and alkaline earth metal salts include carbonates, nitrates, nitrites, sulfates, borates, hydroxides, chlorides, etc. of lithium, sodium, potassium, magnesium, calcium, etc.
[0018] The electrolyte used in the present invention is preferably an aqueous alkali metal solution. By using an electrolyte similar to that used in the electrochemical corrosion protection method, the accuracy of the method of the present invention as a preliminary simulated current test is improved. As the alkali metal, it is preferable to use at least one selected from lithium, sodium, and potassium, and lithium and potassium are particularly preferable. As the alkali metal, one type may be used alone, or two or more types of alkali metals may be used in combination. The electrolyte is preferably a carbonate. As in the above, the electrolyte used is the same as that used in the electrochemical corrosion protection method, and the accuracy of the preliminary simulated current test is improved. From the above viewpoints, the electrolyte according to the present invention is preferably an alkali metal carbonate, more preferably an aqueous solution of lithium carbonate, sodium carbonate or potassium carbonate, and particularly preferably an aqueous solution of lithium carbonate or potassium carbonate. The concentration of the electrolyte is not particularly limited, but from the viewpoints of solubility and permeability into the core sample, it is usually in the range of 0.01 to 1 mol / L, preferably in the range of 0.05 to 0.8 mol / L, and more preferably in the range of 0.1 to 0.5 mol / L.
[0019] In the method of the present invention, it is preferable to measure at least one of the pH, chloride ion concentration, and inter-electrode potential difference of the electrolyte during current application, which will be described later. Since the electrolyte properties may change over time, the electrolyte properties can be controlled by monitoring the pH, chloride ion concentration, and inter-electrode potential difference at predetermined time intervals.
[0020] <Electrode> In the method of the present invention, the steel material inserted into the core specimen is the cathode, and the anode is used by being partially or completely immersed in the electrolyte. As the anode material, it is preferable to select a material having excellent corrosion resistance, for example, titanium, titanium alloy, platinum, or metal plated with these metals. In addition, carbon materials such as carbon fiber and carbon rod, conductive polymers, etc. are also included. In the method of the present invention, it is preferable to use an electrode coated with an alloy based on titanium for the reasons of suppressing the generation of chlorine gas and stabilizing the voltage. The anode material is preferably the above-mentioned conductive material in a net, mesh or sheet form, for example, a mesh coated with a titanium-based alloy, a carbon fiber sheet, etc., and a mesh electrode coated with a titanium-based alloy is particularly preferred.
[0021] <Amount of current> In the method of the present invention, the amount of current flow between the steel material and the electrolyte is more than 0 to 5 A / m as a current density per surface area of the concrete (core sample). 2 The current density here is preferably adjusted to the conditions when the electrochemical corrosion protection method is actually performed, and is preferably within the above range. Current density is 0A / m 2 By passing a current exceeding 5 A / m, the electrolyte material can be permeated into the concrete.2 If it is below this level, alkali accumulation and OH - There is no excessive generation of ions. The voltage of the above current is also preferably adjusted to the conditions when an electrochemical corrosion protection method is actually performed, and is preferably in the range of 5 to 40V.
[0022] <Power supply period> The period for which the current is passed (current passing period) is not particularly limited as long as it is within the range in which the effects of the present invention are achieved, but within the above-mentioned current passing amount range, a period of 7 to 80 days is preferable. If it is 7 days or more, the current passing through the core sample is sufficient, and the subsequent curing can be used as an effective accelerated expansion test. On the other hand, the upper limit of 80 days is approximately the same as the current passing period in an actual electrochemical corrosion protection method. From the above viewpoints, a current passing period of 10 to 60 days is more preferable.
[0023] <Simulated current test equipment> In the method of the present invention, a simulated current test apparatus as shown in FIG. 2 is used. The simulated current test apparatus has an electrolytic cell, and the electrolytic cell is filled with an electrolyte. The material of the electrolytic cell is preferably insulating, and suitable examples include plastics, ceramics, and the like. The shape of the electrolytic cell is not particularly limited as long as it can store the electrolyte. It may be bucket-shaped as shown in FIG. 2, or may be box-shaped. The size is not particularly limited as long as the core sample can be inserted and a mesh-shaped anode can be arranged around it, and the diameter may be about 20 to 30 cm (diameter in the case of a bucket shape, diagonal length in the case of a box shape) and the depth may be about 30 to 50 cm.
[0024] <Curing> The core sample of the present invention is cured after passing an electric current to promote the alkali-silica reaction (ASR). This curing allows the degree of expansion of the core sample to be understood. The curing is performed after stopping the passage of electric current, and no electric current is passed during the curing. Curing is preferably performed under any one of the following conditions (1) to (3). Under these conditions, the degree of expansion can be adequately grasped in a system where ASR occurs. (1) Keep the container in an atmosphere of 20 to 40°C and a relative humidity of 95% or more. (2) Immerse in a 1 mol / L NaOH solution at 80°C. (3) Immerse in a saturated NaCl aqueous solution at 50°C.
[0025] The curing period is preferably within the range of 7 to 365 days, as this range promotes ASR, allows an appropriate amount of residual expansion to be measured, and is also preferable from the standpoint of cost.
[0026] <Expansion rate measurement> The expansion rate can be measured by measuring the height of the core sample before and after the accelerated test and calculating from the elongation rate. For example, as shown in Figure 1, a stainless steel band 12 is attached to a core specimen 10 with a drilled hole 11, and brass tips 13 are attached at intervals of 150 mm. The expansion rate can be calculated by measuring the distance between the brass tips after the accelerated test and dividing it by the initial distance between the tips (150 mm). The distance between the brass tips is not particularly limited as long as it is within a range that allows the expansion amount to be measured. From the viewpoint of accuracy, a long distance is preferable, but from the viewpoints of the measurement sample, measurement device, etc., a distance of about 100 to 180 mm is preferable.
[0027] [Significance of the present invention] According to the present invention, even for concrete containing delayed-reactive aggregate, which cannot be detected by the accelerated expansion test such as the Canadian method that has been conventionally used, it is possible to measure the amount of remaining expansion and estimate the amount of future expansion. In addition, it is possible to determine whether or not a repair method that applies an electrochemical method can be applied. Specifically, when an accelerated expansion test is performed by the method of the present invention, if expansion occurs regardless of which electrolyte is used, it means that an electrochemical method cannot be used. Therefore, in this case, it is suggested that repair should be performed by a method other than the electrochemical method, such as cross-section repair. On the other hand, when there are electrolytes that cause expansion and electrolytes that do not cause expansion depending on the type of electrolyte, this means that repairs can be performed by electrochemical methods by using an electrolyte that does not cause expansion, and the method of the present invention can be used as a method for selecting the optimal electrolyte. EXAMPLES
[0028] The present invention will be explained in more detail below using experimental examples. However, the present invention is not limited to the following experimental examples as long as it does not deviate from the gist of the present invention.
[0029] Experimental Example 1 (Preparation of core samples) Core specimens were taken from the concrete structure. As shown in Figure 1, the core specimen was cylindrical, with a bottom diameter of 75 mm and a height of 200 mm. A hole with an inner diameter of 15 mm and a depth of 175 mm was drilled in the center of the bottom of the core specimen. Stainless steel bands were attached 25 mm from the bottom of the top and bottom of the core specimen, and brass chips for measuring the expansion rate were attached. The distance between the brass chips was 150 mm. Next, a round bar (13 mm in diameter) of the same type as the rebar used in the concrete structure was inserted into the hole, and the gap between the hole and the round bar was filled with cement paste to create a core sample. The cement paste used here had a water / cement ratio of 45% by mass. In addition, this core specimen contained 5% by mass of cristobalite in andesite as a delayed-reactive aggregate.
[0030] (Simulated current test) The core sample was set in the simulated current test device as shown in Figure 2, and immersed in the electrolyte up to 10 mm from the top of the core sample. The electrolyte used was an aqueous solution of lithium carbonate with a concentration of 0.2 mol / L. A titanium mesh was used as the anode, and it was set in such a way that it was stretched around the core sample as shown in Figure 2. The ambient temperature is 20°C, and the resistance is 1.0 A / m per concrete surface area. 2 The current was applied continuously for 8 weeks under constant current control. The electrolytic cell in the simulated current test device used here was made of polyethylene and had a diameter of 20 cm and a depth of 40 cm.
[0031] (Curing) After 8 weeks of applying electricity, the current was stopped and the core samples were taken out. The samples were then left to stand in a thermo-hygrostat at a temperature of 40°C and a relative humidity of 95% for 125 days. The expansion rate was then measured by the method described in the specification. The expansion rate was measured 25, 60, 85, and 125 days after the start of curing. The results are shown in Table 1.
[0032] Experimental Example 2 The test was carried out in the same manner as in Experimental Example 1, except that an aqueous potassium carbonate solution was used as the electrolyte solution and the concentration was 0.3 mol / L. The results are shown in Table 1.
[0033] Reference example 1 The test was carried out in the same manner as in Experimental Example 1, except that the device was stored for 8 weeks at 20° C. and a relative humidity of 95% without applying current. The results are shown in Table 1.
[0034] Reference example 2 The core sample prepared in Experimental Example 1 was used to carry out an accelerated expansion test according to the Canadian method. Specifically, the core sample was immersed in a 1 mol / L NaOH solution at a temperature of 80±2°C for 14 days. After that, the expansion rate was measured according to the method described in the specification, and no expansion was observed according to the Canadian method.
[0035] [Table 1]
[0036] From the results in Table 1, as shown in Experimental Example 2, when an aqueous potassium carbonate solution was used, the core sample expanded. Although the absolute value of the expansion rate was not large, an increase of about six times the expansion rate was observed after 125 days. On the other hand, in the case of the conventional Canadian method, the absolute value of the expansion rate was large compared to the method of the present invention, but the rate of increase in the expansion rate relative to the number of days elapsed was small, and even after 125 days the expansion rate was about twice as high (Reference Example 2). As described above, it was confirmed that the remaining amount of expansion that could not be predicted by conventional methods can be predicted by the present invention. Furthermore, as shown in Experimental Example 1, when a lithium carbonate aqueous solution was used, the core sample did not expand due to curing, whereas in Experimental Example 2, when potassium carbonate was used, the core sample expanded. In other words, it was found that for the concrete structure used in this Experimental Example, the use of an electrochemical corrosion protection method using a lithium carbonate aqueous solution is effective, whereas the use of an electrochemical corrosion protection method using a potassium carbonate aqueous solution is inappropriate. [Industrial Applicability]
[0037] According to the present invention, it is possible to determine whether or not a repair method using an electrochemical technique is possible for a concrete structure having reactive aggregate, particularly delayed-reactivity aggregate. In addition, it is possible to select an appropriate electrolyte for use in a repair method using an electrochemical technique, and thus to provide an efficient cathodic protection method. [Explanation of symbols]
[0038] 10 Core specimen 11 Drilling 12 Stainless steel band 13 Brass Tip
Claims
1. A method for measuring residual expansion by a simulated current test, comprising the steps of: taking a core specimen from a concrete structure; drilling a hole in the core specimen; inserting a steel material into the hole; immersing a portion of the core specimen in an electrolyte; passing a current between the steel material, which is the cathode, and the anode in the electrolyte for a certain period of time; curing the core specimen to promote an alkali-silica reaction; and then measuring the expansion rate.
2. 2. The method for measuring the residual expansion amount by a simulated current test according to claim 1, wherein the electrolyte is an aqueous alkali metal solution.
3. The amount of electricity is more than 0 to 5 A / m as a current density per surface area of concrete. 2 3. The method for measuring residual expansion amount by a simulated current test according to claim 1 or 2,
4. 3. The method for measuring residual expansion by a simulated current test according to claim 1 or 2, wherein a gap between the steel material and the hole is filled with cement paste or a saturated aqueous calcium hydroxide solution.
5. 3. The method for measuring the residual expansion amount by a simulated current test according to claim 2, wherein the alkali metal is at least one selected from the group consisting of lithium, sodium and potassium.
6. 6. The method for measuring the residual expansion amount by a simulated current test according to claim 5, wherein the alkali metal is lithium or potassium.
7. 3. The method for measuring the residual expansion amount by a simulated current test according to claim 1 or 2, wherein the electrolyte is a carbonate.
8. The method for measuring the residual expansion amount by a simulated current test according to claim 1 or 2, wherein the current-flow period is 7 to 80 days.
9. 3. The method for measuring residual expansion by a simulated current test according to claim 1 or 2, wherein the curing is carried out under any one of the following conditions (1) to (3): (1) Allow to stand in an atmosphere of 20 to 40°C and a relative humidity of 95% or more. (2) Immerse in a 1 mol / L NaOH solution at 80° C. (3) Immerse in a saturated NaCl aqueous solution at 50° C.
10. The method for measuring the residual expansion amount by a simulated current test according to claim 9, wherein the curing period is 7 to 365 days.
11. 3. The method for measuring residual expansion amount by a simulated current test according to claim 1 or 2, wherein the core specimen is cylindrical, has a diameter of 40 to 120 mm, and has a height of 120 to 320 mm.
12. 3. A method for measuring residual expansion by a simulated current test according to claim 1 or 2, wherein the steel material is a cathode, and a mesh electrode coated with an alloy having a titanium base is used as an anode.
13. 3. The method for measuring the residual expansion amount by a simulated current test according to claim 1 or 2, further comprising measuring at least one of a pH, a chloride ion concentration, and an inter-electrode potential difference in the electrolyte during the current flow.
Citation Information
Patent Citations
Method for predicting progress in deterioration due to alkali / silica reaction of concrete structure
JP2001099833A
Concrete expansion prediction method
JP2010243397A