Method for producing metallurgical coke
Mechanical compaction of low-fluidity coal with high-fluidity coal using a double roll molding machine forms strong bonds, addressing the challenge of producing high-strength metallurgical coke with appropriate particle size from raw materials with poor caking properties, enhancing blast furnace performance.
Patent Information
- Application Number
- JP2023075289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing methods struggle to produce metallurgical coke with sufficient strength and appropriate particle size using raw materials with poor caking properties, particularly when incorporating large amounts of coal with low fluidity, which can lead to decreased coke strength and inadequate air permeability in blast furnaces.
A method involving mechanical compaction of raw material A with low fluidity (logMF ≤ 1.50) and raw material B with high fluidity (logMF ≥ 2.30) using a double roll molding machine to produce briquette coal, followed by carbonization with powdered coal, forming strong bonds at the interface to enhance coke strength and size.
This approach prevents significant strength loss while ensuring high-strength coke production with suitable particle size for blast furnaces, improving productivity and coke quality.
Smart Images

Figure 2024159345000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing metallurgical coke, which enables a significant increase in the amount of raw materials with poor caking properties used in a molded coal blending method, in which the amount of raw materials with poor caking properties can be increased by mechanically compacting a portion of the raw materials, compared to the conventional method. [Background technology]
[0002] Currently, in the production of pig iron using a blast furnace, coke produced by carbonizing coal in a chamber coke oven is used as a reducing agent for iron ore and to ensure good ventilation inside the blast furnace. It is known that the fluidity of coal during carbonization is important for producing high-strength metallurgical coke that can ensure gas permeability in such a blast furnace. For example, Non-Patent Document 1 reports that it is necessary for the coal to exhibit a fluidity of at least 200 ddpm (common logarithm value 2.30), and preferably 400 ddpm (common logarithm value 2.60) or more, in a fluidity measurement method using a Gieseler Plastometer.
[0003] However, as described above, raw coal with sufficient fluidity to produce high-strength coke tends to be more expensive than general coal used for fuel. In addition, the reserves of the resource are limited, and there is concern that they will be depleted in the future. Therefore, in order to reduce raw material costs and continue to operate blast furnaces using a variety of raw materials, there is a strong demand for the development of coke production technology that can use a large amount of raw materials with poor fluidity during carbonization.
[0004] In order to meet such demands, efforts have been made to increase the use of coal with poor fluidity by using techniques that utilize molded coal. For example, in Patent Document 1, the thermoplasticity and melting properties of a coal blend used in briquettes are calculated as a weighted average of the total expansion rates of the constituent coals.Then, when this value is below a certain level, a crushing operation is performed to increase the proportion of coal particles with a particle size of 3 mm or less, thereby making it possible to obtain coke with sufficient coke strength even if the briquettes contain a large amount of inferior coal.
[0005] Furthermore, Patent Document 2 describes a method for obtaining coke with sufficient coke strength by adding a caking filler when the coal blend used for molding contains a large amount of inferior coal with a small total expansion coefficient.
[0006] Recent research has shown that a method for producing high-strength agglomerates that can withstand use in blast furnaces from coal with poor fluidity involves first pulverizing the coal to 106 μm or less (approximately 3 mm or less in the normal coke manufacturing process), then compressing and molding the coal in a mold 15 mm in diameter and 20 mm deep before carbonizing it, which has been reported to produce high-strength agglomerates with an indirect tensile strength of over 10 MPa (5 MPa for normal coke) (Non-Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-117279 A [Patent Document 2] JP 2016-65111 A [Non-patent literature]
[0008] [Non-Patent Document 1] Miyazu et al., Japan Steel Pipe Engineering Report, 67 (1975), 1 [Non-Patent Document 2] M. Matoba, et Al., ISIJ international, 59(2019), 1440. [Non-Patent Document 3] K. Uchida, et Al., ISIJ international, 59(2019), 1449. Summary of the Invention [Problem to be solved by the invention]
[0009] However, when producing coke by carbonizing molded coal blended with low-quality coal together with powdered coal, even if the coal particle size is adjusted by the method described in Patent Document 1 or a caking filler is added by the method described in Patent Document 2, if the proportion of low-quality coal, i.e., coal with low fluidity, is high, the coke strength still decreases and sufficient strength may not be obtained.
[0010] Furthermore, Non-Patent Documents 2 and 3 report that high-strength agglomerates can be produced using only coal with poor melting property without using any caking filler. However, the molding method using a mold as reported in the literature is insufficient in terms of production speed to be applied to coke production using several thousand to several tens of thousands of tons of coal per day.
[0011] In addition, one of the important roles of coke in a blast furnace is to ensure gas permeability as a spacer inside the blast furnace, and therefore a certain particle size is required. Although the methods described in Non-Patent Documents 2 and 3 can produce high-strength agglomerates, it is extremely difficult to produce coke with a particle size sufficient to ensure gas permeability in the blast furnace.
[0012] The present invention has been made in consideration of the above circumstances, and aims to provide a metallurgical coke with high strength and an appropriate particle size that can contribute to ensuring the gas permeability of a blast furnace while using a larger amount of raw materials such as coal and biomass, which have poor caking properties, than conventionally. [Means for solving the problem]
[0013] That is, the gist of the present invention is as follows. 1. A method for producing metallurgical coke, comprising the steps of: forming raw material A by mechanical compaction into molded coal, using raw material A' as raw material A'; blending raw material A' with powdered raw material B (powdered coal) to produce blended coal, and carbonizing the blended coal to produce coke; wherein raw material A has a common logarithm of maximum fluidity (logMF) of 1.50 or less in a fluidity test method (Gieselaar Plastometer method) specified in JIS M 8801, raw material A has a maximum particle size of 300 μm or less, and raw material B has a common logarithm of maximum fluidity (logMF) of 2.30 or more.
[0014] 2. The method for producing metallurgical coke described in 1 above, wherein a double-roll molding machine is used for the mechanical compaction.
[0015] 3. The density of the raw material A' is 1.00 g / cm 3 3. The method for producing metallurgical coke according to 1 or 2 above.
[0016] 4. The method for producing metallurgical coke according to any one of the above items 1 to 3, wherein the mass ratio of raw material A' to the total mass of raw material A' and raw material B is 0.30 or less. Effect of the Invention
[0017] According to the present invention, even though a larger amount of raw material having poor caking properties is used than in the past, the finely pulverized raw material is compacted to prevent a significant decrease in the drum strength of the coke, which is a problem when the raw material is used as a coke raw material. In addition, by using a raw material having a certain level of fluidity for the powdered coal, a good bond can be formed at the interface between the molded coal and the powdered coal, thereby advantageously resolving issues related to productivity and coke particle size. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a diagram showing the state of filling an 'alumina crucible' used in the examples. [Diagram 2] This is a photograph of the interface between raw coal 1 (right) and molded coal 6 (left). [Diagram 3] This is a photograph of the interface between raw coal 2 (left) and molded coal 6 (right). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention relates to a method for producing metallurgical coke, which comprises carbonizing a blended coal obtained by blending a part of a raw material (referred to as raw material A in the present invention) with powdered raw material B (referred to as powdered coal in the present invention) to produce molded coal (referred to as raw material A' in the present invention), which is produced by molding a part of the raw material (referred to as raw material A in the present invention) by mechanical compaction, to produce coke. In particular, the logarithm of the maximum flowability (logMF) of the raw material A in the fluidity test method (Giesserer Plastometer method) specified in JIS M 8801 (hereinafter referred to as "JIS8801") is 1.50 or less, and the maximum particle size of the raw material A is 300 μm or less. In addition, the logarithm of the maximum flowability (logMF) of the raw material B in the fluidity test method is 2.30 or more. In the following, the maximum fluidity (MF) in the fluidity test method (Giesserler Plastometer method) specified in JIS8801 may be simply referred to as maximum fluidity or fluidity.
[0020] [The raw material A is a material having a common logarithm (logMF) of maximum fluidity of 1.50 or less in the fluidity test method (Giesserer Plastometer method) specified in JIS8801] The raw material A (raw material for molded coal) in the present invention has a common logarithm of maximum fluidity (logMF) of 1.50 or less in the fluidity test method (Gieselaar plastometer method) specified in JIS8801. The purpose of the present invention is to enable the use of a low-fluidity raw material as a coke raw material while suppressing a decrease in coke strength, when the raw material has a low fluidity and would otherwise be subject to a significant decrease in coke strength in a conventional manufacturing method. In other words, it is not economically desirable to finely grind and use highly fluid raw materials that can be used in normal coke production in accordance with the present invention, since the fine grinding is costly and the improvement in coke strength is limited. Therefore, it is essential to use raw material A having a common logarithm of the maximum fluidity of 1.50 or less, and preferably 1.30 or less.
[0021] In coke production, raw materials with different fluidities are generally blended to prepare raw material A. In such a case, in the present invention, the raw materials are blended so that the weighted average value calculated from the common logarithm of the maximum fluidity of each raw material that is the raw material of raw material A and the mass proportion of each raw material is 1.50 or less, and the blended raw material can be used as raw material A used in the present invention.
[0022] Here, for raw materials that do not exhibit any fluidity at all, i.e., raw materials with a maximum fluidity (MF) of 0 ddpm in the fluidity test method (Giesserer Plastometer method) specified in JIS8801, the common logarithm of the maximum fluidity (logMF) is set to 0 in the calculation.
[0023] Since the inside of the molded coal is bonded between particles by a solid-phase sintering-like phenomenon, not by the conventional liquid-phase sintering-like phenomenon, there is no particular lower limit for the maximum fluidity of raw material A. Therefore, even raw materials that do not exhibit any fluidity at all can be used as coke raw materials in the present invention. Therefore, the lower limit of the logMF is not particularly limited and may be 0.00.
[0024] Furthermore, in the present invention, the carbonaceous material to be the raw material A is not particularly limited as long as it is a raw material having low fluidity and mainly composed of carbon, but in addition to coal, biomass, precipitated carbon, etc. can be used, and carbides obtained by heat treating these, as well as mixtures thereof, can be suitably used. When using a large amount of raw materials with a high volatile content, such as inferior coal or biomass, it is preferable to heat treat the raw materials in advance to reduce the volatile content to 30 mass% or less. This can increase the yield as coke and prevent the solid-phase sintering phenomenon from being inhibited by gas expansion. On the other hand, if the volatile content is too low, the aromatization and polycyclization reactions, which are the driving forces of the solid-phase sintering phenomenon, are difficult to occur, so the volatile content is preferably 1 mass% or more, and more preferably 6 mass% or more. The adjustment of the volatile content may be performed by heat treatment in an atmosphere where the supply of oxygen is blocked, for example, by storing the raw material in a container that forms a space where the inflow of air is blocked and an inert gas flows. The container that stores the raw material may be heated and the adjustment may be performed by heat transfer from the container. The heat treatment temperature may be, for example, 400°C or higher.
[0025] [Raw material A, maximum particle size 300μm or less] In the present invention, raw material A is pulverized so that the maximum particle size is 300 μm or less. If raw material A contains more than 5% coarse particles with a particle size of over 300 μm, these coarse particles will remain in the molded coal even after carbonization, reducing its strength. This is because the smaller the particle size, the more accelerated the solid-phase sintering phenomenon that bonds particles together, so the remaining coarse particles will inhibit the bonding between particles and cause a decrease in strength.
[0026] The maximum particle size of the raw material A is preferably 100 μm or less. When the particle size of the carbonaceous material is appropriately small, the physical structure in the molded coal becomes dense and uniform, which contributes to increasing the coke strength. The finer the particle size of the carbonaceous material, the higher the bonding strength in the molded coal, which is preferable. Therefore, the lower limit of the maximum particle size of the raw material A is not limited. However, considering the productivity, even if the particle size of the raw material A is made small, making the maximum particle size of the raw material A less than 20 μm increases the cost of fine pulverization, while the improvement in the coke strength is limited. Therefore, it is preferable that the maximum particle size is about 20 μm or more.
[0027] In the present invention, the particle size refers to the maximum particle size unless otherwise specified. When the measurement is performed using a particle size distribution measuring device, the maximum particle size can be measured as follows. That is, in the present invention, the particle size and particle size distribution may be values measured using a commercially available particle size distribution measuring device. Specifically, the particle size and particle size distribution (volume basis) measured using a laser diffraction / scattering particle size distribution measuring device "Laser Micronsizer LMS-3000" (hereinafter simply referred to as particle size distribution measuring device) manufactured by Malvern Panalytical is used.
[0028] In the present invention, the maximum particle size (maximum value) is defined as the particle size that is 95% of the smaller particle size (detection limit particle size) of the particle size distribution of the particles contained in the mixed powder measured by a particle size distribution measuring device. Hereinafter, when simply referring to particle size or particle size distribution, it means the value measured by the above particle size distribution measuring device.
[0029] In the present invention, the pulverizing method and the pulverizing device are not particularly limited. The pulverizing method may be a conventional method, and the pulverizing device may be a media mill such as a cutter mill, a hammer mill, a pin mill, a jet mill, or a ball mill. In addition, the pulverizing device is not limited to a device that performs only pulverization, and may be, for example, a pulverizer with a built-in classifier.
[0030] [Raw material B has a common logarithm of the maximum fluidity (logMF) of 2.30 or more] In the present invention, by using a raw material B (powdered raw material or powdered coal) that has a certain level of fluidity when heated, a strong adhesive joint is formed at the interface between the molded coal and the powdered coal during carbonization, and the entire raw material is agglomerated, making it possible to produce coke with high strength and a particle size suitable for use in a blast furnace. Therefore, the fluidity of the powdered coal needs to be the same as or higher than that of raw coal normally used in coke production. Specifically, raw material B must have a common logarithm of maximum fluidity of 2.30 or more in the fluidity test method (Gieselaar Plastometer method) specified in the above-mentioned JIS 8801. From the viewpoint of producing stronger coke, it is preferable that the common logarithm is 2.40 or more, and more preferably 2.60 or more. If the fluidity of raw material B is too high, the bond at the interface between the molded coal and the powdered coal will be strong, but the coke strength may decrease due to excessive expansion of raw material B and a decrease in coke density. Therefore, the common logarithm (logMF) of the maximum fluidity of raw material B is preferably 3.00 or less.
[0031] In coke production, raw materials with different fluidities are generally blended and used as raw material B. In this case, the raw materials are blended so that the weighted average value calculated from the common logarithm of the maximum fluidity of each raw material that is to be the raw material of raw material B and the mass proportion of each raw material is 2.30 or more, and the blended material can be used as raw material B used in the present invention.
[0032] [Manufacturing method of molded coal (raw material A')] From the viewpoint of ensuring the strength of the coke, the method for producing the molded coal is not particularly limited. However, it is preferable to use a double-roll molder in order to increase the production rate of the molded coal and achieve productivity suitable for the production amount of the coke.
[0033] In general, when producing molded coal, a binder may be used to improve the handling properties of the molded coal. In the present invention, a binder can be added as necessary to the raw material A that satisfies the above-mentioned fluidity and particle size. As such a binder, a coal-based binder (coal tar pitch, solvent refined coal, tar, tar slag, etc.), a petroleum-based binder (asphalt, asphalt pitch, propane deasphalted asphalt, etc.), and an organic binder (starch, molasses, resin, etc.) may be used.
[0034] In addition, as a method for improving the handleability of molded coal without using a binder, a method of molding while pushing raw material A between double rolls with a screw can also be used. The closer the distance between particles in raw material A, the more the solid-phase sintering phenomenon is promoted and the stronger the bond between particles is formed during carbonization. Therefore, the density of the molded coal (raw material A') is 1.00 g / cm 3 More preferably, from the viewpoint of producing stronger coke, the content is 1.05 g / cm 3 More preferably, it is 1.10 g / cm or more. 3 Although there is no particular upper limit to the density of the molded coal (raw material A'), if the molding pressure is too high in order to increase the density, rebound cracks will occur in the molded coal, and the yield will decrease, resulting in a decrease in productivity. Therefore, the target value for the density of the molded coal is 1.30 g / cm 3 The following is preferred:
[0035] In the present invention, there is no need to restrict the size of the briquettes, and for example, briquettes having a volume of 6 to 120 (cc) may be used. In consideration of the strength of the briquettes, the size of the briquettes is preferably in the range of 6 to 80 (cc), and more preferably in the range of 6 to 50 (cc).
[0036] In the present invention, the production rate is preferably 45 tons / day or more in terms of processing capacity, since the present invention is applied to coke production using several thousand to several tens of thousands of tons of coal per day. On the other hand, the upper limit is not particularly limited, but is industrially about 4500 tons / day.
[0037] Furthermore, in the present invention, the type of raw material for the powdered coal is not particularly limited, and raw materials mainly consisting of raw coal generally used in coke production may be used. As the raw material for the powdered coal, in addition to coal, charcoal obtained by heat treatment of coal or biomass, or a mixture thereof may be used. In addition, pitches such as coal tar pitch and asphalt pitch may be partially used as the raw material for the powdered coal in order to improve the strength of the coke. In addition, even if a material does not fall under Raw Material A' (molded coal) or Raw Material B (powdered coal) (such as plastic lumps added for the purpose of recovering gas from waste), it is permitted without any problems as long as it has the components and amounts used in conventionally known blended coal for coke production.
[0038] The particle size of the powdered coal is not particularly limited, and the powdered coal may be pulverized so that the proportion of particles having a diameter of 3 mm or less is 70 to 100 mass %, following a general coke manufacturing process. Regarding the blending ratio of briquettes and powdered coal, the mass ratio of briquettes to the total raw material including briquettes and powdered coal is desirably 30 mass% or less. In the present invention, a bond is formed inside the briquettes by a phenomenon similar to solid phase sintering. Meanwhile, a bond is formed at the interface between the powdered coal and the briquettes by a phenomenon similar to liquid phase sintering using the fluidity of coal during carbonization. As a result, the entire raw material is agglomerated, and coke with a large particle size suitable for use in a blast furnace can be produced.
[0039] Therefore, if the proportion of powdered coal is too low, the adhesive strength between the molded coal and the powdered coal is insufficient, and coke with a large particle size cannot be produced. Therefore, the mass proportion of molded coal in the entire raw material is preferably 30 mass% or less, and more preferably 25 mass% or less. In addition, from the viewpoint of the above adhesion, the lower limit of the mass proportion of molded coal is not particularly limited, but in light of the purpose of using a large amount of low-fluidity raw material that has been difficult to use in the past, the mass proportion of molded coal is preferably 3 mass% or more, and more preferably 5 mass% or more.
[0040] The pretreatment process of the raw material in the present invention may include some or all of the steps of crushing, classifying, mixing, kneading, drying, adding water, and preheating, etc. The carbonization conditions may be performed in a general chamber-type coke oven at a temperature of about 900° C. or higher.
[0041] In the method for producing metallurgical coke according to the present invention, any item not described in this specification can be performed by a conventional method. EXAMPLES
[0042] The present invention will be described below based on examples, but the present invention is not limited to the following examples. Example 1 The coals listed in Table 1 were used as raw material A. Note that the maximum fluidity of coals 2 and 4 was 0 ddpm, and since the common logarithm of the maximum fluidity could not be calculated, they were described as having "no melting ability." Furthermore, the molded coal produced by molding the raw material A was designated as raw material A'.
[0043] The molded coals (raw material A') 1 to 6 shown in Table 2 were produced by the following procedure. The coals listed in Table 1 were used as raw material A. First, each raw material was crushed to particle sizes of 3 mm or less, 106 μm or less, and 74 μm or less (hereinafter and in the table, "less than" is represented by a "-" (minus)). Note that an ultracentrifugal crusher (manufacturer: Verder Scientific, model: ZM200) was used to crush to -106 μm and -74 μm. Molded coal (raw material A') 1 to 4 were prepared by adding 6 mass% tar and 6 mass% tar pitch (both outer frames) as binders to 100 mass% of the crushed coal 1 or 2, raw material A, and thoroughly kneading the mixture in a kneader to obtain a kneaded product. The kneaded product was then molded in a small double-roll molding machine equipped with a mold. In addition, molded coal (raw material A') 5 to 6 was molded using a small double-roll molding machine equipped with a screw in front of the rolls and a mold, by compressing the crushed coal 3 or 4 with the double rolls while pushing it with the screw.
[0044] In the conventional examples, comparative examples, and invention examples below, the raw coal shown in Table 3 was used as the pulverized coal (raw material B). In the present invention, the fluidity of the briquettes is extremely low compared to the conventional method, and the briquettes are produced by grinding the briquettes finer than the conventional method, and the briquettes are carbonized together with the powdered coal. This leads to a decrease in the strength of the coke. In order to investigate the effect of the fluidity of the powdered coal on the adhesion at the interface, the following experiment was carried out. Raw coals 1 and 2 shown in Table 3 were crushed to 1 mm 100% and used as powdered coal. Each raw coal shown in Table 3 and molded coal 6 shown in Table 2 were packed in an alumina crucible as shown in Figure 1. At this time, the density of the powdered coal was 750 kg-dry / m 3 The alumina crucible filled with the powdered coal and other materials was covered with a lid and heated in an electric furnace from room temperature to 1000°C at a heating rate of 3°C / min. After cooling, the obtained coke sample was embedded in resin and cut, and the interface between the powdered coal and the molded coal was observed under a microscope.
[0045] [Table 1]
[0046] [Table 2]
[0047] [Table 3]
[0048] The observation results are shown in Figures 2 and 3. As shown in Figure 2, when raw coal 1 with low fluidity was used as the raw material for the powdered coal, it was observed that the inside of the briquette and the powdered coal were integrated, but the interface between the briquette and the powdered coal was not bonded at all, and gaps of about 200 μm were uniformly generated. It is believed that the low fluidity of the powdered coal prevented good adhesion at the interface between the briquette and the powdered coal, and gaps were generated at the interface due to the difference in the contraction rates of the two during carbonization.
[0049] On the other hand, when raw coal 2 with high fluidity was used as the powder coal raw material, a bond was formed at the interface between the molded coal and the powder coal, and it was observed that the molded coal part and the powder coal were integrated, as shown in Figure 3. From the results of this experiment, it was confirmed that the fluidity of the powder coal is important for forming a bond at the interface between the molded coal and the powder coal and integrating the entire coke raw material, and that by using a powder coal raw material with a certain level of fluidity or more, good adhesion can be formed at the interface between the molded coal and the powder coal.
[0050] Example 2 The effects of the present invention will be described below based on examples in which coke was produced and the coke strength was measured. First, under the blending conditions shown in Table 4, a coal blend was prepared by blending powder coal (raw material B) and molded coal (raw material A'). In Conventional Examples 1 and 2, raw coals 3 and 4 shown in Table 3 were crushed to 100% -3 mm and used as powdered coal, and only the powdered coal was used as the blended coal. In Examples 1 and 2 and Comparative Examples 1 to 6, raw coals 3 and 4 listed in Table 3 were crushed to 100% -3mm and used as powder coal (80 mass% of the total), and coals 1 to 3 listed in Table 1 were either used as unbridled coal (i.e., raw material A) or blended as briquette coal (raw material A') listed in Table 2 to make a coal blend of 20 mass% of the total. In Example 3 of the invention and Comparative Example 7, raw coal 4 listed in Table 3 was crushed to 100% -3mm and used as powder coal (90 mass% of the total), and coal 4 listed in Table 1 was used either as unbridled coal (i.e., raw material A) or as briquette coal (raw material A') listed in Table 2 to form a blended coal at 10 mass% of the total.
[0051] When the blended coal was not mixed with molded coal (Conventional Examples 1 and 2, Comparative Examples 2, 5, 6, and 7), the bulk density of the entire raw material was 750 (kg-dry / m 3 The mixture was charged into a SUS carbonization vessel shown in FIG. In addition, when the blended coal contains briquettes (Comparative Examples 1, 3, and 4, and Invention Examples 1 to 3), the bulk density of the powder coal is 750 (kg-dry / m 3 The mixture was charged into a SUS carbonization vessel shown in FIG. The SUS carbonization can containing the blended coal was heated in an electric furnace at a furnace temperature of 1050°C for 6 hours to obtain coke. The obtained coke was cooled in a nitrogen atmosphere, and then the coke strength was evaluated by the 15 mm index (DI 150 / 15) at 150 revolutions in the drum test specified in JIS K2151:2004.
[0052] Table 4 shows the blending conditions of the coke raw materials and the drum strength of the coke, and explains the effects of the present invention.
[0053] [Table 4]
[0054] [Conventional Examples 1 and 2] This is the standard for coke made from raw coal 3, 4, which is generally used in coke production. Coke for blast furnaces is required to have strength, and under the above coke production conditions, a DI 150 / 15 of 73 or more (preferably 75 or more) is required.
[0055] [Comparative Examples 1 to 3] Coal 1 is blended in different shapes with raw coal 3, and coke is produced by carbonization. In Comparative Example 2, coal 1 (-3mm 100%) is mixed with powdered coal in an unbriquette form, but the decrease in coke strength is small compared to Conventional Example 1. In Comparative Examples 1 and 3, coal 1 is crushed to different particle sizes to produce molded coal, and is mixed with powdered coal, but the change in coke strength is small. In other words, if the coal has a fluidity such that the common logarithm of the maximum fluidity is about 2.08, there is no need to pulverize it before use, and it can be used as a coke raw material by conventional methods, so there is little need to pulverize it according to the present invention.
[0056] [Comparative Examples 4 and 5] Coal 2 is mixed with raw coal 3 in a different shape and carbonized to produce coke. In Comparative Example 5, coal 2 (-3mm 100%) is mixed with powdered coal in an unbriquette form, but the coke strength is significantly lower than that of Conventional Example 1. In Comparative Example 4, coal 2 is crushed to -3mm 100% to produce molded coal, which is mixed with powdered coal, but the coke strength is similar to that of Comparative Example 5 and is significantly lower than that of Conventional Example 1.
[0057] [Example 1] In Example 1, coal 2 was crushed to 100% -74 mm to produce molded coal (raw material A'), which was mixed with powdered coal. Although the coke strength was lower than that of Conventional Example 1, it was clearly higher than that of Comparative Examples 4 and 5, and achieved a desirable strength (DI 150 / 15) of 75. From these results, it was confirmed that when a raw material with low melting property is used as raw material A, the decrease in coke strength can be significantly reduced by following the method of the present invention.
[0058] [Comparative Examples 6 and 7] Coals 3 and 4 in different shapes are mixed with raw coal 4 and carbonized to produce coke. In Comparative Examples 6 and 7, coals 3 and 4 pulverized to 100% -106 μm are mixed with powdered coal in an unbridled state, but the coke strength is significantly reduced compared to Conventional Example 2. In particular, the strength reduction is significant in Comparative Example 7, which uses coal 4 that does not exhibit any fluidity.
[0059] [Examples 2 and 3] In Examples 2 and 3, molded coal (raw material A') made from coals 3 and 4 pulverized to 100% -106 μm was mixed with powdered coal, and the coke strength was significantly improved compared to Comparative Examples 6 and 7 in which the same raw material A was used in an unmolded form. As a result, in Example 2, the coke strength was comparable to that of Conventional Example 2, achieving a desirable strength (DI 150 / 15) of 75. Also, in Example 3, the target strength (DI 150 / 15) of 73 was achieved. These results confirm that when using a raw material with low melting property as a coke raw material, the adverse effects on coke strength can be reduced by following the method of the present invention, which involves finely pulverizing and compacting the raw material.
[0060] The particle size of the coke produced in Examples 1 to 3 was similar to that of the coke produced in Conventional Examples 1 and 2. It was confirmed that the coke derived from the molded coal (raw material A') was integrated with the surrounding coke derived from the powdered coal, and coke with a particle size similar to that of the conventional coke production method could be produced.
Claims
1. In a method for producing metallurgical coke, a raw material A is molded by mechanical compaction to produce molded coal as raw material A', and the raw material A' is blended with a powdered raw material B (powdered coal) to produce a blended coal, and the blended coal is carbonized to produce a coke, The raw material A has a common logarithm (logMF) of maximum fluidity measured by a fluidity test method (Giesserer Plastometer method) specified in JIS M 8801 of 1.50 or less, Furthermore, the maximum particle diameter of the raw material A is 300 μm or less, Furthermore, the raw material B has a common logarithm (logMF) of the maximum fluidity of 2.30 or more. A method for producing metallurgical coke.
2. The method for producing metallurgical coke according to claim 1, wherein the mechanical compaction is performed using a double-roll molding machine.
3. The density of the raw material A' is 1.00 g / cm 3 The method for producing metallurgical coke according to claim 1 or 2.
4. 3. The method for producing metallurgical coke according to claim 1, wherein the mass ratio of raw material A' to the total mass of raw material A' and raw material B is 0.30 or less.
5. 4. The method for producing metallurgical coke according to claim 3, wherein a mass ratio of raw material A' to a total mass of raw material A' and raw material B is 0.30 or less.
Citation Information
Patent Citations
Preparation of metallurgical coke
JP1977107001A
Production of coke for blast furnace
JP1985181190A
Production of formed coke
JP1995197030A
Production of blast furnace coke
JP1996209150A
Coke production method
JP2007332233A
Cited By
Method for manufacturing bio-molded charcoal
JP7896707B1