Inkjet recording method, inkjet recording device, and set of aqueous ink and aqueous reaction solution
The inkjet recording method on non-absorbent media uses specific ink and reaction liquid formulations with controlled heating to enhance scratch resistance and color development by forming a resin film and exposing wax particles, addressing the limitations of existing methods.
Patent Information
- Application Number
- JP2024051818
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing inkjet recording methods using aqueous inks on non-absorbent recording media, such as polyvinyl chloride sheets and polyethylene terephthalate sheets, fail to achieve sufficient scratch resistance and color development, despite using reaction liquids that enhance image integrity.
An inkjet recording method involving the application of an aqueous ink and reaction liquid on a recording medium, followed by heating, where the ink contains pigments, resin particles, and wax particles dispersed by anionic groups, with specific temperature and particle diameter relationships to ensure resin fusion and wax exposure, enhancing scratch resistance and color development.
The method achieves images with improved scratch resistance and color development by ensuring resin particles form a film and wax particles remain on the surface, reducing friction and promoting slipperiness.
Smart Images

Figure 2024159532000011 
Figure 2024159532000012 
Figure 2024159532000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an inkjet recording method, an inkjet recording apparatus, and a set of an aqueous ink and an aqueous reaction liquid. [Background technology]
[0002] In recent years, inkjet recording methods have been increasingly used in the field of sign and display, such as for recording posters and giant advertisements. In this field, polyvinyl chloride sheets and polyethylene terephthalate (PET) sheets are often used as recording media from the viewpoints of the durability and cost of the recording media. These recording media have no or almost no water-based ink absorbing layer on the recording surface of the recording media, and are called non-absorbent recording media (recording media that have no water-based ink absorbing properties) and low-absorbent recording media (recording media that have low water-based ink absorbing properties). Hereinafter, recording media whose surfaces have almost no ink absorbing properties will also be referred to as "non-absorbent recording media". When recording images on not only absorbent recording media but also non-absorbent recording media, solvent-based inks and curable inks have been used conventionally. However, from the viewpoints of reducing environmental loads and odors, there is an increasing need for water-based inks using water-based media.
[0003] Not only absorbent recording media, but also images recorded on non-absorbent recording media used in the field of sign and display are required to have excellent abrasion resistance and color development. In order to meet such requirements, for example, a method has been proposed in which a reaction liquid that aggregates the components of an aqueous ink is brought into contact with an aqueous ink containing acrylic resin particles and wax on a recording medium to record an image exhibiting abrasion resistance while ensuring high productivity (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-142725 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have studied the recording method proposed in Patent Document 1. As a result, it has been found that while high productivity is ensured by using a reaction liquid, the scratch resistance of the recorded image is not necessarily sufficient, and there is room for further improvement.
[0006] Therefore, an object of the present invention is to provide an inkjet recording method capable of recording an image having excellent abrasion resistance and color development using an aqueous ink and an aqueous reaction liquid. Another object of the present invention is to provide an inkjet recording apparatus used in the inkjet recording method, and a set of an aqueous ink and an aqueous reaction liquid. [Means for solving the problem]
[0007] That is, according to the present invention, there is provided an inkjet recording method for recording an image on a recording medium using an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink, the method including: a reaction liquid applying step of applying the aqueous reaction liquid to the recording medium; an ink applying step of applying the aqueous ink so as to overlap at least a part of an area of the recording medium to which the aqueous reaction liquid is applied; and a heating step of heating the recording medium to which the aqueous ink and the aqueous reaction liquid have been applied at a predetermined temperature T F (° C.), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups, and the heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (°C) satisfies the relationship of the following formula (1), and the average particle diameter D Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), and the anionic group E Pig(μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): T M >T F ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) E Wax ≦E Em <E Pig (3) Effect of the Invention
[0008] According to the present invention, it is possible to provide an inkjet recording method capable of recording an image having excellent abrasion resistance and color development properties using an aqueous ink and an aqueous reaction liquid. Also, according to the present invention, it is possible to provide an inkjet recording apparatus used in the inkjet recording method, and a set of an aqueous ink and an aqueous reaction liquid. [Brief description of the drawings]
[0009] [Figure 1] 1 is a perspective view illustrating an embodiment of an inkjet recording apparatus of the present invention. [Diagram 2] 1 is a side view diagrammatically illustrating an embodiment of an inkjet recording apparatus of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink and reaction liquid in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt". In addition, the aqueous ink and aqueous reaction liquid for inkjet printing may be simply referred to as "ink" and "reaction liquid". Physical property values are values at room temperature (25°C) unless otherwise specified. When "(meth)acrylic acid" and "(meth)acrylate" are written, they mean "acrylic acid, methacrylic acid" and "acrylate, methacrylate", respectively.
[0011] The present inventors used the ink and reaction liquid (treatment liquid) proposed in Patent Document 1, and heated a recording medium to a predetermined temperature (T F (°C)) to record an image, and the scratch resistance of the image was confirmed. F The temperature (T M (℃)) of 90℃ wax particles (particles formed from wax) and glass transition temperature (T G The toner contains urethane resin particles having a temperature (° C.) of 90° C. As a result, it was found that the scratch resistance of the recorded images was not necessarily sufficient, and the present inventors investigated the cause of this.
[0012] When the surface of the image was observed with an SEM, it was found that some of the wax particles had melted due to the heat, and the exposed wax particles on the surface of the image had decreased. It is presumed that the reduced exposed wax particles caused the friction coefficient of the image surface to not decrease sufficiently, and the scratch resistance of the image did not improve. Therefore, F (℃)) is the melting point of the wax particles (T M (℃), it was observed that the wax particles did not melt on the image surface and were fully exposed on the image surface. However, it was observed that some of the urethane resin particles were not fused and remained in particulate form, indicating that the scratch resistance of the image was not improved.
[0013] Therefore, the heating temperature at which the urethane resin particles are sufficiently fused (T F (℃) and its melting point (T M (℃)) is the heating temperature (T F (℃)), an image was recorded using wax particles with a temperature higher than that of the original. As a result, it was observed that the fusion of the urethane resin particles had progressed sufficiently on the image surface, and the wax particles were exposed on the image surface, indicating that the scratch resistance of the image had improved.
[0014] In order to further improve the scratch resistance of the image, the inventors focused on the particle sizes of the wax particles and the pigment. Specifically, they conducted further studies under the assumption that the wax particles are more easily exposed on the image surface by using wax particles having a larger particle size than the pigment. As a result, they found that the scratch resistance of the image is further improved by using wax particles having a larger particle size than the pigment.
[0015] That is, the inkjet recording method of the present invention has the following features. First, the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of a carboxylic acid group. The heating temperature T of the recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is F (° C.), the glass transition temperature T G (° C.), and the melting point T M The average particle diameter D of the pigment (°C) satisfies the relationship of the following formula (1). Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2). Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): The present inventors speculate as follows about the mechanism by which the above-mentioned configuration enables recording of images with excellent scratch resistance and color development. T M >TF ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) E Wax ≦E Em <E Pig (3)
[0016] The ink contains a pigment that is dispersed by the action of carboxylic acid groups, so that when it comes into contact with an aqueous reaction liquid that contains a reactant that reacts with the aqueous ink, the pigment reacts with the reactant in the reaction liquid through electrostatic interaction and aggregates.
[0017] In addition to the pigment, the ink contains resin particles and wax particles. The resin particles are fused to the image surface by heating or the like to form a resin film, thereby improving the scratch resistance of the image. The wax particles remain on the image surface, which can impart slipperiness to the image, leading to improved scratch resistance of the image.
[0018] Heating temperature T of the recording medium to which the aqueous ink and aqueous reaction liquid are applied F (° C.), the glass transition temperature T G (° C.), and the melting point T M (°C) satisfies the relationship of the following formula (1). In other words, the heating temperature of the recording medium is lower than the melting point of the wax particles and 10°C or more higher than the glass transition temperature of the resin particles. As a result, the resin particles are sufficiently fused to the image surface to form a resin film. Then, the wax particles are exposed to the image surface without melting, improving the scratch resistance of the image. T M >T F ≧(T G -10) ···(1)
[0019] If the heating temperature of the recording medium is equal to or higher than the melting point of the wax particles, the molten wax will run off, making it impossible to leave a sufficient amount of wax on the surface of the image, and it will be difficult to reduce the coefficient of friction of the image surface. As a result, the image will not have abrasion resistance. F <(T G In the case of -10), the resin particles are not sufficiently fused to the image surface, and a resin film is not formed, resulting in the image not being resistant to abrasion.
[0020] Average pigment particle size D Pig (nm) and the average particle size of the wax particles D Wax (nm) satisfies the following formula (2). D Pig (nm) and D Wax When (nm) satisfies the relationship of the following formula (2), the toner has excellent abrasion resistance and color development, and an image having both of these properties can be recorded. 4.00≧(D Wax / D Pig ) ≧ 0.70 (2)
[0021] "D Wax / D Pig If the value of "D" exceeds 4.00, the wax particles unevenly distributed on the image surface cause strong surface scattering, and the image cannot be colored. Wax / D Pig If the value of " is less than 0.70, the pigment is more likely to be exposed on the image surface than the wax particles, and the image will not have abrasion resistance.
[0022] In recording using a reaction liquid, in order to further improve the scratch resistance of an image, it is necessary to satisfy the following relationship: Pig (μmol / g), anionic group E of resin particles Em (μmol / g), and anionic group E of wax particles Wax (μmol / g) must satisfy the relationship of the following formula (3). Pig (μmol / g), E Em (μmol / g), and E WaxWhen the density (μmol / g) satisfies the relationship of the following formula (3), the wax particles in the ink can be more effectively distributed in the outermost layer of the image. This value represents the density (in micromoles) of the anionic groups present in each component per unit mass of each component. The amount of anionic groups can be measured by colloid titration using potential difference. For convenience, the value of the anionic groups can also be expressed as the value of the charge amount or the value of density. E Wax ≦E Em <E Pig (3)
[0023] The inventors consider the reason why the above effect can be obtained by satisfying formula (3) as follows. Among the particulate components in the ink, the component with a smaller amount of anionic groups has a lower reactivity with the reaction liquid, and therefore is more likely to be unevenly distributed on the surface of the image. Therefore, the anionic group E of the pigment Pig (μmol / g) of the anionic group E of the resin particles Em (μmol / g) is preferable from the viewpoint of improving the scratch resistance of the image. By satisfying this relationship, when the ink and the reaction liquid contact on the recording medium, the pigment having a larger amount of anionic groups strongly aggregates, and then the resin particles weakly aggregate. As a result, the aggregated pigment is covered with the resin particles, and the resin particles having a relatively low friction coefficient tend to be unevenly distributed on the surface of the image, which is thought to further improve the scratch resistance of the image.
[0024] Similarly, the anionic groups E of the wax particles Wax (μmol / g) of the anionic group E of the pigment Pig (μmol / g) and anionic group E of resin particles Em By setting the content of the wax particles to 0.01 μmol / g or less, the wax particles tend to be unevenly distributed on the surface of the image. In order to further increase the scratch resistance of the image, it is preferable to unevenly distribute the wax particles on the surface of the image to an extent equal to or greater than that of the resin particles. For this reason, the anionic group E Wax (μmol / g) is the anionic group E of the resin particles EmIf the above formula (3) is not satisfied, the components unevenly distributed on the surface of the image will change, and the image will not have sufficient scratch resistance.
[0025] <Inkjet recording method, inkjet recording apparatus, and set of aqueous ink and aqueous reaction liquid> The inkjet recording method of the present invention is a method in which an aqueous ink and an aqueous reaction liquid are ejected from an inkjet recording head by the action of thermal energy and applied to a recording medium to record an image. The inkjet recording method of the present invention has a reaction liquid application step, an ink application step, and a heating step. The reaction liquid application step is a step of applying the aqueous reaction liquid to the recording medium. The ink application step is a step of applying the aqueous ink so as to overlap at least a part of the area of the recording medium to which the aqueous reaction liquid is applied. The heating step is a step of heating the recording medium to which the aqueous ink and the aqueous reaction liquid have been applied at a predetermined heating temperature T F (°C). The aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups. The aqueous reaction liquid contains a reactant that reacts with the aqueous ink. The heating temperature T F (℃), glass transition temperature T G (℃), and the melting point T M (℃) satisfies the relationship of the following formula (1). Pig (nm) and the average particle size of the wax particles D Wax (nm) satisfies the relationship of the following formula (2). Pig (μmol / g), anionic group E of resin particles Em (μmol / g), and anionic group E of wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): It is not necessary to cure the image by irradiating it with active energy rays or the like. T M >T F ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) EWax ≦E Em <E Pig (3)
[0026] The inkjet recording apparatus of the present invention is an apparatus used in an inkjet recording method in which an aqueous ink and an aqueous reaction liquid are ejected from an inkjet recording head by the action of thermal energy and applied to a recording medium to record an image. The inkjet recording apparatus of the present invention is an apparatus that is suitably used in the above-mentioned recording method.
[0027] The set of aqueous ink and aqueous reaction liquid of the present invention is a set used in an inkjet recording method in which an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink are ejected from a recording head to record an image on a recording medium. The set is preferably used in the above-mentioned recording method. The form of the set includes a set of multiple ink cartridges each containing multiple inks (reaction liquids) independently, and an ink cartridge formed integrally by combining multiple ink containing parts each containing multiple inks (reaction liquids). The set of the present invention is not limited to the above form and may be in any form as long as it is configured so that the inks and reaction liquids can be used in combination.
[0028] The inkjet recording method and inkjet recording apparatus (hereinafter, also simply referred to as "recording method and recording apparatus") of the present invention will be described in detail below.
[0029] FIG. 1 is a perspective view showing an embodiment of an inkjet recording apparatus of the present invention. FIG. 2 is a side view showing an embodiment of an inkjet recording apparatus of the present invention. The recording apparatus of the embodiment shown in FIGS. 1 and 2 includes an inkjet recording head 22 that ejects ink (reaction liquid). The recording head 22 is a recording head that ejects ink by the action of thermal energy. The recording head that ejects ink by the action of thermal energy is a thermal recording head that applies thermal energy to the ink by applying an electric pulse to an electrothermal conversion element, and ejects the ink from the ejection port. Here, a recording head that ejects ink by the action of thermal energy is taken as an example, but a recording head that ejects ink by the action of mechanical energy may also be adopted. Since the recording head 22 can eject ink and reaction liquid, it can be said to be equipped with an ink applying means and a reaction liquid applying means. The recording head may include a mechanism (temperature control mechanism) that heats the aqueous ink ejected from the recording head. When the temperature control mechanism is included, the temperature of the ink ejected from the recording head is preferably 35° C. or higher and 70° C. or lower.
[0030] (Heating process) In the recording method of the present invention, the recording medium to which the ink and the reaction liquid have been applied is heated to a predetermined temperature T F The method includes a heating step of heating (heat treatment) the recording medium to (°C). Heating the recording medium to which the ink and reaction liquid have been applied not only promotes drying, but also promotes film formation of the resin particles, making it possible to record an image with excellent abrasion resistance.
[0031] The means for heating the recording medium is not particularly limited, and examples of the heating means include known heating means such as a heater, a blowing means using a blower such as a dryer, and a combination of these. That is, the inkjet recording apparatus heats the recording medium on which the ink has been applied to a temperature T F(°C). The heating means may be the above-mentioned warming means, air blowing means, or a combination of these. Examples of the heat treatment method include a method of applying heat from the opposite side (back side) of the recording surface (ink application surface) of the recording medium using a heater, a method of applying warm or hot air to the recording surface of the recording medium, and a method of heating from the recording surface or back side using an infrared heater. A combination of these methods may also be used. In order to improve the scratch resistance of the image, it is preferable to dry the image by blowing air onto the surface of the recording medium to heat the recording medium. In other words, it is preferable that the heating step includes a step of blowing air onto the surface of the recording medium to heat it. This promotes evaporation of moisture from the image surface, causing wax particles to be unevenly distributed on the image surface, and the friction coefficient of the image surface is reduced, which is believed to further improve the scratch resistance of the image.
[0032] The heating temperature of the recording medium to which the ink and the reaction liquid have been applied may satisfy the above-mentioned formula (1) and formula (2). In particular, the heating temperature of the recording medium to which the ink and the reaction liquid have been applied is preferably 50° C. or more and 90° C. or less, since the scratch resistance of the image can be increased. Here, the heating temperature of the recording medium to which the ink and the reaction liquid have been applied can be rephrased as the surface temperature of the recorded image or the temperature reached by heating the recording medium to which the ink and the reaction liquid have been applied. For example, the heating temperature of the recording medium can be determined as the heating setting temperature of the inkjet recording device. The heating temperature of the recording medium to which the ink and the reaction liquid have been applied may be read by a sensor incorporated at a position corresponding to the heating means of the recording device, or may be determined from the relationship between the amount of heat determined according to the type of ink and recording medium and the temperature of the recording medium.
[0033] In the recording device shown in FIGS. 1 and 2, a heater 25 supported by a frame (not shown) is disposed downstream in the sub-scanning direction A from the position where the recording head 22 reciprocates in the main scanning direction B. The recording medium 1 to which ink has been applied can be heated by the heater 25. Specific examples of the heater 25 include a sheath heater and a halogen heater. The heater 25 is covered by a heater cover 26. The heater cover 26 is a member for efficiently irradiating the heat generated by the heater 25 to the recording medium 1. Furthermore, the heater cover 26 is also a member for protecting the heater 25. The recording medium 1 to which ink has been applied ejected from the recording head 22 is wound by a take-up spool 27 to form a roll-shaped wound medium 24.
[0034] (Recording medium) In the recording method and recording device of the present invention, inkjet-specific paper having an ink receiving layer (glossy paper, matte paper, etc.), "absorbent recording medium" such as plain paper having no coating layer, and non-absorbent recording medium (low to non-absorbent recording medium) can be used as recording media. Non-absorbent recording media are those that are measured after 30 msec from the start of contact in the Bristow method described in JAPAN TAPPI Paper and Pulp Test Method No. 51 "Liquid Absorbency Test Method for Paper and Paperboard". 1 / 2 Water absorption up to 10mL / m 2 In the present invention, a recording medium that satisfies the above-mentioned condition of water absorption amount is defined as a "low to non-absorbent recording medium". A recording medium for inkjet recording having an ink receiving layer formed of inorganic particles (glossy paper, matte paper, etc.) and plain paper having no coating layer have a water absorption amount of 10 mL / m or less. 2 It is an "absorbent recording medium" that exceeds this.
[0035] The use of a non-absorbent recording medium is preferable because it allows an image with further improved abrasion resistance to be recorded. When the ink and the reaction liquid are brought into contact with each other on a non-absorbent recording medium, it is considered that the time for the wax particles to be unevenly distributed on the image surface is extended, making it possible to unevenly distribute a sufficient amount of wax particles on the image surface, thereby further improving the abrasion resistance of the image.
[0036] Examples of low to non-absorbent recording media that can be used include plastic films, recording media in which a plastic film is bonded to the recording surface of a substrate, and recording media in which an organic resin coating layer is provided on the recording surface of a substrate containing cellulose pulp. Among these, plastic films are preferred, and recording media in which an organic resin coating layer is provided as an organic resin layer on the recording surface of a substrate containing cellulose pulp are also preferred.
[0037] When the ink used in the recording method and recording apparatus of the present invention is applied to a non-absorbent recording medium, components such as water and water-soluble organic solvents evaporate and the resin particles are concentrated. This promotes fusion between the concentrated resin particles, and the scratch resistance of the recorded image is further improved. In contrast, when the ink is applied to a recording medium that has high absorbency of liquid components, the fusion between the resin particles is not promoted, so the effect of improving the scratch resistance of the image may not be sufficiently obtained. Note that the recording medium in this specification does not mean a transfer body, but means a recording medium on which an image as a recorded matter is recorded.
[0038] (Reaction solution) The recording method of the present invention has a reaction liquid applying step of applying an aqueous reaction liquid containing a reactant that reacts with an aqueous ink to a recording medium. In particular, it is preferable to have a reaction liquid applying step before the ink applying step, or to perform the ink applying step and the reaction liquid applying step in parallel. Each component used in the reaction liquid will be described in detail below.
[0039] [Reactants] The reaction liquid reacts with the ink when it comes into contact with the ink, coagulating the components in the ink (resins and components having anionic groups such as self-dispersing pigments), and contains a reactant, such as an organic acid, a polyvalent metal salt, or a cationic resin.
[0040] The reactant preferably contains at least one of an organic acid and a polyvalent metal salt, and a cationic resin, because it is possible to record an image with further improved abrasion resistance. The polyvalent metal salt and the organic acid have a smaller atomic size or molecular size than the cationic resin, and therefore have a high diffusion rate into the ink. Therefore, when the reactant comes into contact with an ink containing a pigment, resin particles, and wax particles with different amounts of anionic groups, the polyvalent metal salt and the organic acid with a high diffusion rate react quickly with the pigment with a large amount of anionic groups. Then, the cationic resin with a low diffusion rate reacts with the wax particles with a small amount of anionic groups, so that the wax particles are more likely to be unevenly distributed on the image surface, and the abrasion resistance of the image is further improved.
[0041] [Organic acid] The reaction liquid containing an organic acid has a buffering ability in the acidic range (less than pH 7.0, preferably pH 2.0 to 5.0), and thus efficiently converts the anionic groups of the components present in the ink into an acid form and causes them to aggregate. Examples of the organic acid include monocarboxylic acids and salts thereof, such as formic acid, acetic acid, propionic acid, butyric acid, benzoic acid, glycolic acid, lactic acid, salicylic acid, pyrrole carboxylic acid, furan carboxylic acid, picolinic acid, nicotinic acid, thiophene carboxylic acid, levulinic acid, and coumaric acid; dicarboxylic acids and salts thereof, such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, itaconic acid, sebacic acid, phthalic acid, malic acid, and tartaric acid; tricarboxylic acids and salts thereof, such as citric acid and trimellitic acid; and tetracarboxylic acids and salts thereof, such as pyromellitic acid. The content (mass %) of the organic acid in the reaction liquid is preferably 1.0 mass % or more and 50.0 mass % or less based on the total mass of the reaction liquid.
[0042] [Polyvalent metal salt] Polyvalent metal salts are compounds that consist of divalent or higher metal ions (polyvalent metal ions) and anions. Polyvalent metal salts dissociate in the reaction solution to become polyvalent metal ions, which cause the pigments dispersed in the ink to flocculate due to the action of the anionic groups in the ink. Examples of polyvalent metal ions include Ca2+ , Cu 2+ , Ni 2+ , Mg 2+ , Sr 2+ , B.A. 2+ , and Zn 2+ Divalent metal ions such as Fe 3+ , Cr 3+ , Y 3+ , and Al 3+ Examples of the anions constituting the polyvalent metal salt include Cl. - , Br - , I - , ClO - , ClO2 - , ClO3 - , ClO4 - , NO2 - , NO3 - , SO4 2- , CO3 2- , HCO3 - , PO4 3- , HPO4 2- , and H2PO4 - Inorganic anions such as HCOO - , (COO - )2, COOH(COO - ), CH3COO - , C2H5COO - , CH3CH(OH)COO - , C2H4(COO - )2, C6H5COO - , C6H4(COO - )2, and CH3SO3 - and the like organic anions.
[0043] Specific examples of polyvalent metal salts include calcium carbonate such as heavy calcium carbonate and light calcium carbonate, calcium nitrate, calcium chloride, calcium sulfate, magnesium sulfate, calcium hydroxide, magnesium chloride, magnesium carbonate, barium sulfate, barium chloride, zinc carbonate, zinc sulfide, aluminum silicate, calcium silicate, magnesium silicate, copper nitrate, calcium acetate, magnesium acetate, aluminum acetate, aluminum sulfate, calcium methanesulfonate, calcium lactate, magnesium lactate, calcium propionate, calcium acetate, calcium pantothenate, and calcium gluconate. These polyvalent metal salts may have water of hydration. The content (mass%) of the polyvalent metal salt in the reaction solution is preferably 1.0 mass% or more and 20.0 mass% or less based on the total mass of the reaction solution. In this specification, when the polyvalent metal salt is a hydrate, the "content (mass%) of the polyvalent metal salt in the reaction solution means the "content (mass%) of the anhydrous polyvalent metal salt" excluding water as the hydrate.
[0044] [Cationic Resin] The cationic resin has a cationic site in the resin structure, and aggregates pigments dispersed by the action of carboxylic acid groups in the ink. Examples of the cationic resin include resins having a structure of primary to tertiary amines and resins having a structure of quaternary ammonium salts. Specific examples include resins having a structure of vinylamine, allylamine, vinylimidazole, vinylpyridine, dimethylaminoethyl methacrylate, ethyleneimine, guanidine, diallyldimethylammonium chloride, and alkylamine-epichlorohydrin condensate. In order to increase the solubility in the reaction liquid, the cationic resin may be used in combination with an acidic compound, or the cationic resin may be subjected to a quaternary treatment. The content (mass%) of the cationic resin in the reaction liquid is preferably 0.1% by mass or more and 10.0% by mass or less based on the total mass of the reaction liquid.
[0045] [Aqueous medium] The reaction liquid is an aqueous reaction liquid containing at least water as an aqueous medium. Examples of the aqueous medium used in the reaction liquid include the same aqueous media as those that can be contained in the ink, which will be described later.
[0046] [Other ingredients] The reaction liquid may contain various other components as necessary. Examples of the other components include the same components as those that can be contained in the ink, which will be described later.
[0047] [Physical properties of reaction solution] The reaction liquid that can be suitably used in the recording method of the present invention is an aqueous reaction liquid applied to the inkjet method. Therefore, from the viewpoint of reliability, it is preferable to appropriately control the physical property values. Specifically, the surface tension of the reaction liquid at 25°C is preferably 20 mN / m or more and 60 mN / m or less. In addition, the viscosity of the reaction liquid at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the reaction liquid at 25°C is preferably 5.0 or more and 9.5 or less, more preferably 6.0 or more and 9.0 or less.
[0048] <Ink> The ink used in the recording method of the present invention is a water-based ink for ink-jet recording, which contains a pigment dispersed by the action of an anionic group, resin particles, and wax particles. Each component constituting the ink will be described in detail below.
[0049] [Pigment] The ink contains a pigment as a coloring material. The pigment is dispersed by the action of an anionic group, and is aggregated by the reactant in the reaction liquid. The content (mass %) of the pigment in the ink is preferably 0.1 mass % or more and 15.0 mass % or less, and more preferably 1.0 mass % or more and 10.0 mass % or less, based on the total mass of the ink.
[0050] Specific examples of pigments include inorganic pigments such as carbon black and titanium oxide; and organic pigments such as azo, phthalocyanine, quinacridone, isoindolinone, imidazolone, diketopyrrolopyrrole, and dioxazine.
[0051] As a method for dispersing pigments, resin-dispersed pigments using a resin (resin dispersant) as a dispersant, self-dispersed pigments in which hydrophilic groups are bonded to the pigment particle surface, etc. can be used. In addition, resin-bonded pigments in which organic groups containing a resin are chemically bonded to the pigment particle surface, and microcapsule pigments in which the pigment particle surface is coated with a resin, etc. can be used. Among them, it is preferable to use resin-dispersed pigments in which a resin as a dispersant is physically adsorbed onto the pigment particle surface, rather than resin-bonded pigments or microcapsule pigments. In other words, it is preferable that the pigment is a pigment that is dispersed by the action of a resin dispersant.
[0052] As the resin dispersant for dispersing the pigment in the aqueous medium, it is preferable to use one that can disperse the pigment in the aqueous medium by the action of anionic groups. As the resin dispersant, a resin described below, particularly a water-soluble resin, can be used. The content (mass%) of the pigment in the ink is preferably 0.3 to 10.0 times the mass ratio of the content of the resin dispersant.
[0053] As the self-dispersing pigment, an anionic group such as a carboxylic acid group, a sulfonic acid group, or a phosphonic acid group can be used, which is bonded to the particle surface of the pigment directly or via another atomic group (-R-). The anionic group may be either an acid type or a salt type, and when it is a salt type, it may be either a partially dissociated state or a completely dissociated state. When the anionic group is a salt type, examples of the cation that serves as the counter ion include an alkali metal cation, ammonium, and organic ammonium. Specific examples of the other atomic group (-R-) include a linear or branched alkylene group having 1 to 12 carbon atoms; an arylene group such as a phenylene group or a naphthylene group; a carbonyl group; an imino group; an amide group; a sulfonyl group; an ester group; and an ether group. In addition, it may be a group that is a combination of these groups.
[0054] [Resin particles] The ink contains resin particles. From the viewpoint of recording an image having excellent abrasion resistance, the heating temperature T F (℃) and the glass transition temperature T G (℃) must satisfy the following formula (6): F (℃) and T G When the glass transition temperature T (°C) of the resin particles satisfies the relationship of the following formula (6), the resin particles can be sufficiently coated, and the scratch resistance of the image can be improved. G The glass transition temperature (°C) is preferably from 40°C to 120°C, and more preferably from 50°C to 100°C. The glass transition temperature (°C) of the resin particles can be measured using a differential scanning calorimeter (DSC). T F ≧(T G -10) (6)
[0055] The anionic groups (μmol / g) of the pigment, resin particles, and wax particles described later can all be determined by colloid titration. In the examples described later, an automatic potentiometric titrator (AT-510; manufactured by Kyoto Electronics Manufacturing Co., Ltd.) equipped with a streaming potential titration unit (PCD-500) was used to measure the anionic groups (μmol / g) by colloid titration utilizing potential difference. During the measurement, the pH of the pigment dispersion, the aqueous dispersion of resin particles, and the aqueous dispersion of wax particles were all adjusted to 8 to 9. In addition, methyl glycol chitosan was used as the titration reagent.
[0056] The content (mass%) of the resin particles in the ink is preferably 0.1% by mass or more and 15.0% by mass or less, and more preferably 1.0% by mass or more and 10.0% by mass or less, based on the total mass of the ink. The content (mass%) of the resin particles in the ink is preferably 0.5 times or more, more preferably 1.5 times or more, and particularly preferably 1.7 times or more, in terms of mass ratio to the pigment content (mass%). The above mass ratio is preferably 10.0 times or less. The resin particles are present in the ink in a dispersed state, i.e., in the form of a resin emulsion.
[0057] In this specification, "resin particles" refers to a resin that exists in a state in which it is not dissolved in the aqueous medium of the ink, and more specifically, refers to a resin that can exist in the aqueous medium in the form of particles whose particle size can be measured by dynamic light scattering. In contrast, "water-soluble resin" refers to a resin that exists in a state in which it is dissolved in the aqueous medium of the ink.
[0058] Whether or not a certain resin corresponds to a "resin particle" can be judged according to the method shown below. First, a liquid containing the resin to be judged is prepared, and a sample is prepared by diluting with pure water so that the resin content is about 1.0%. Then, when the particle size of the resin in the sample is measured by dynamic light scattering, if particles having a particle size are measured, the resin is judged to be a "resin particle" (i.e., a "water-dispersible resin"). On the other hand, if particles having a particle size are not measured, the resin is judged not to be a "resin particle" (i.e., a "water-soluble resin"). The measurement conditions at this time can be, for example, SetZero: 30 seconds, number of measurements: 10, measurement time: 120 seconds, shape: spherical, refractive index: 1.5, and density: 1.0.
[0059] As the particle size distribution measuring device, a particle size analyzer using a dynamic light scattering method (for example, the product name "Nanotrac WAVEII-Q" manufactured by Microtrac Bell) can be used. Of course, the particle size distribution measuring device and the measurement conditions to be used are not limited to those described above.
[0060] The acid value of the resin constituting the resin particles is preferably 5 mgKOH / g or more and 100 mgKOH / g or less. The weight average molecular weight of the resin constituting the resin particles is preferably 1,000 or more and 3,000,000 or less, more preferably 100,000 or more and 3,000,000 or less. The average particle diameter of the resin particles measured by dynamic light scattering is preferably 50 nm or more and 500 nm or less. The resin particles do not need to contain a coloring material.
[0061] [Wax particles] The ink contains particles (wax particles) formed of wax. By using an ink containing wax particles, an image with further improved abrasion resistance can be recorded. The wax may be a composition containing components other than wax, or may be the wax itself. The wax particles may be dispersed by a dispersant such as a surfactant or a water-soluble resin. The wax may be used alone or in combination of two or more kinds. The content (mass %) of the wax particles in the ink is preferably 0.1 mass % or more and 10.0 mass % or less, and more preferably 1.0 mass % or more and 5.0 mass % or less, based on the total mass of the ink.
[0062] In the narrow sense, wax is an ester of a water-insoluble higher monohydric or dihydric alcohol and a fatty acid, and includes animal waxes and vegetable waxes, but does not include oils and fats. In the broad sense, wax includes high-melting-point fats, mineral waxes, petroleum waxes, and blends and modified products of various waxes. In the recording method of the present invention, any wax in the broad sense can be used without particular restrictions. Wax in the broad sense can be classified into natural waxes, synthetic waxes, blends thereof (blended waxes), and modified products thereof (modified waxes).
[0063] Examples of natural waxes include animal waxes, vegetable waxes, mineral waxes, and petroleum waxes. Examples of animal waxes include beeswax, spermaceti, and wool wax (lanolin). Examples of vegetable waxes include palm wax, carnauba wax, candelilla wax, rice wax, Japan wax, olicury wax, and sugarcane wax. Examples of mineral waxes include montan wax, ozokerite, ceresin, and lignite wax. Examples of petroleum waxes include paraffin, microcrystalline, and petrolatum.
[0064] Examples of synthetic waxes include hydrocarbon waxes such as Fischer-Tropsch wax and polyolefin wax (e.g., polyethylene wax, polypropylene wax). Compounded waxes are mixtures of the above waxes. Modified waxes are waxes that have been modified by oxidation, hydrogenation, alcohol modification, acrylic modification, urethane modification, or other such modification treatments. Examples of modified waxes include paraffin wax derivatives, montan wax derivatives, and microcrystalline wax derivatives. Examples of hydrogenated waxes include castor wax and opal wax.
[0065] The material constituting the wax particles is preferably Fischer-Tropsch wax. In other words, the wax is preferably Fischer-Tropsch wax. By using wax particles formed from Fischer-Tropsch wax, an image with further improved scratch resistance can be recorded. Fischer-Tropsch wax is rich in saturated linear hydrocarbons, and therefore has less steric hindrance than other waxes. For this reason, when the surface of an image recorded using an ink containing wax particles formed from Fischer-Tropsch wax is rubbed, the wax particles are easily stretched. Therefore, when the image surface is rubbed multiple times, it is possible to more efficiently reduce the friction coefficient of the image surface, and it is considered that the scratch resistance of the image is further improved.
[0066] From the viewpoint of recording an image having excellent abrasion resistance, the heating temperature T of the recording medium to which the ink and the reaction liquid are applied is F (℃) and the melting point T of the wax particles M (℃) must satisfy the following formula (7): F (℃) and T M (℃) satisfies the relationship of the following formula (7), FThe wax particles do not melt even at temperatures below 100° C., and the wax can be present in the form of particles in the image. The melting point (° C.) of the wax is preferably 40° C. or higher and 120° C. or lower, and more preferably 50° C. or higher and 100° C. or lower. The melting point T M (°C) is the top temperature of the endothermic peak in the heating process of a differential scanning calorimeter (DSC). As a differential scanning calorimeter (DSC), for example, a product name "DSC-60" (manufactured by Shimadzu Corporation) can be used. The melting point of wax is easily affected by properties such as molecular weight (the larger the molecular weight, the higher the melting point), molecular structure (the higher the melting point if it is linear, and the lower the melting point if it is branched), crystallinity (the higher the crystallinity, the higher the melting point), and density (the higher the crystallinity, the higher the melting point). For this reason, by controlling these properties, a wax having a desired melting point can be obtained. T M >T F (7)
[0067] Anionic group E of wax particles Wax (μmol / g) is preferably 50 μmol / g or more and 90 μmol / g or less. Wax By making the anionic group E of the wax particles 90 μmol / g or less, it is possible to make the wax particles more easily exposed on the image surface, and the scratch resistance of the image can be further improved. Wax If the ratio (μmol / g) is too small, the reactant in the reaction solution and the wax particles may not react easily. This may cause the wax particles to gather on the image surface when heated, forming large clusters of wax particles, which may result in insufficient color development of the image. For this reason, in order to improve the color development of the image, it is necessary to increase the anionic group E Wax The amount of anionic groups in the wax particles can be adjusted, for example, by changing the type and amount of a dispersant that disperses the wax, and by subjecting the wax itself to an oxidation treatment.
[0068] Average pigment particle size D Pig(nm) and the average particle size of the wax particles D Wax (nm) must satisfy the following formula (2): D Pig (nm) and D Wax When (nm) satisfies the relationship of the following formula (2), the toner has excellent abrasion resistance and color development, and an image having both of these properties can be recorded. 4.00≧(D Wax / D Pig ) ≧ 0.70 (2)
[0069] In order to further improve the color reproduction of images, Wax / D Em " is preferably 3.00 or less. In order to further improve the scratch resistance of the image, "D Wax / D Em The value of " is preferably 1.00 or more. That is, the average particle diameter D Em (nm) and the average particle size of the wax particles D Wax It is preferable that (nm) satisfies the relationship of the following formula (4). 3.00≧(D Wax / D Em )≧1.00 (4)
[0070] Average wax particle size D Wax The average particle diameter D of the wax particles is preferably 100 nm or more and 200 nm or less. Wax When the average particle diameter D (nm) is 100 nm or more, the wax particles are more easily exposed on the surface of the image, and the scratch resistance of the image can be further improved. Wax When the thickness (nm) is 200 nm or less, surface scattering is suppressed, and the color development of the image can be further improved.
[0071] In this specification, the term "average particle size" refers to the cumulative 50% particle size (D 50The volume-based cumulative 50% particle diameter of pigments, resin particles, and wax particles is the diameter of the particle that is 50% of the total volume of the measured particles when integrated from the small particle diameter side on the particle diameter integration curve. This "volume-based cumulative 50% particle diameter (D 50 ) can be measured using a particle size distribution measuring device using dynamic light scattering (for example, the trade name "Nanotrac WAVEII-Q", manufactured by Microtrac Bell).
[0072] Content of wax particles in ink W Wax (mass%) and the content of resin particles in the ink W Em It is preferable that W (mass%) satisfies the following formula (5). Wax (mass%) and W Em When the ratio (mass %) satisfies the relationship of the following formula (5), it becomes possible to cause the wax particles to be distributed more unevenly on the image surface than the pigment, and the scratch resistance of the image can be further improved. 1.3≦(W Em / W Wax )≦10.0 (5)
[0073] "W Em / W Wax If the value of "W" is less than 1.3, the wax particles may be excessively exposed on the image surface, which may cause surface scattering and result in insufficient color development of the image. Em / W Wax If the value of "exceeds 10.0", the amount of wax particles exposed on the image surface tends to be insufficient, and the effect of improving the scratch resistance of the image may not be sufficiently obtained.
[0074] [resin] The ink may contain a resin. The content (mass %) of the resin in the ink is preferably from 0.1% to 20.0% by mass, and more preferably from 0.5% to 15.0% by mass, based on the total mass of the ink.
[0075] The resin can be added to the ink (i) to stabilize the dispersion state of the pigment, that is, as a resin dispersant or its auxiliary. Also, the resin can be added to the ink (ii) to improve various properties of the recorded image. Examples of the form of the resin include block copolymer, random copolymer, graft copolymer, and combinations thereof. Also, the resin may be a water-soluble resin that can be dissolved in an aqueous medium, or may be resin particles that are dispersed in an aqueous medium. The resin may be used alone or in combination of two or more kinds.
[0076] [Resin Composition] Examples of the resin include acrylic resins, urethane resins, and olefin resins. Among them, acrylic resins and urethane resins are preferred, and acrylic resins composed of units derived from (meth)acrylic acid or (meth)acrylate are more preferred.
[0077] The acrylic resin preferably has a hydrophilic unit and a hydrophobic unit as constituent units. Among them, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of a monomer having an aromatic ring and a (meth)acrylic acid ester monomer is preferred. In particular, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one monomer selected from the group consisting of styrene and α-methylstyrene is preferred. These resins are likely to interact with pigments, and therefore can be suitably used as a resin dispersant for dispersing pigments.
[0078] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group. The hydrophilic unit can be formed, for example, by polymerizing a hydrophilic monomer having a hydrophilic group. Specific examples of the hydrophilic monomer having a hydrophilic group include acidic monomers having a carboxylic acid group such as (meth)acrylic acid, itaconic acid, maleic acid, and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. Examples of cations constituting the salts of acidic monomers include ions of lithium, sodium, potassium, ammonium, and organic ammonium. The hydrophobic unit is a unit not having a hydrophilic group such as an anionic group. The hydrophobic unit can be formed, for example, by polymerizing a hydrophobic monomer not having a hydrophilic group such as an anionic group. Specific examples of the hydrophobic monomer include monomers having an aromatic ring such as styrene, α-methylstyrene, and benzyl (meth)acrylate; and (meth)acrylic acid ester monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0079] The urethane resin can be obtained by reacting, for example, polyisocyanate with a polyol. In addition, a chain extender may be further reacted with the urethane resin. Examples of the olefin resin include polyethylene and polypropylene.
[0080] [Resin properties] The acid value of the water-soluble resin is preferably 100 mgKOH / g or more and 250 mgKOH / g or less, and the weight average molecular weight of the water-soluble resin is preferably 3,000 or more and 15,000 or less.
[0081] [Aqueous medium] The ink used in the recording method of the present invention is an aqueous ink containing at least water as an aqueous medium. The ink may contain water or an aqueous medium that is a mixed solvent of water and a water-soluble organic solvent. As the water, deionized water or ion-exchanged water is preferably used. The content (mass%) of water in the ink is preferably 50.0 mass% or more and 95.0 mass% or less based on the total mass of the ink. The content (mass%) of water-soluble organic solvent in the ink is preferably 3.0 mass% or more and 50.0 mass% or less based on the total mass of the ink. As the water-soluble organic solvent, any of those usable for inkjet inks, such as alcohols, (poly)alkylene glycols, glycol ethers, nitrogen-containing solvents, and sulfur-containing solvents, can be used. The water-soluble organic solvent may be used alone or in combination of two or more.
[0082] [Other ingredients] The ink may contain various other components as necessary. Examples of other components include various additives such as defoamers, surfactants, pH adjusters, viscosity adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, and reduction inhibitors. However, it is preferable that the ink does not contain a reactant to be contained in the reaction liquid.
[0083] [Ink properties] The ink is a water-based ink applied to the inkjet method. Therefore, from the viewpoint of reliability, it is preferable to appropriately control the physical property values. Specifically, the surface tension of the ink at 25°C is preferably 20 mN / m or more and 60 mN / m or less. In addition, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.5 or less, and more preferably 8.0 or more and 9.5 or less. EXAMPLES
[0084] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples without departing from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified.
[0085] <Method of measuring physical properties> (Glass transition temperature of resin particles) A liquid containing resin particles was dried at 60°C, and 2 mg of resin particles were placed in an aluminum container and sealed to prepare a sample for measurement. The prepared sample was thermally analyzed using a differential scanning calorimeter (trade name "DSC-2500", manufactured by TA instruments) according to the temperature program shown below. In this specification, the glass transition temperature of a resin is defined as follows. That is, in the heating curve (horizontal axis: temperature, vertical axis: amount of heat) of the following temperature program (3), the temperature is determined at the intersection of a straight line extended from the low-temperature side curve to the high-temperature side through two points on the curve, and a tangent drawn at the point where the gradient of the step-like change in the curve is maximum. The temperature thus determined is defined as the "glass transition temperature (T G )". [Temperature Program]: (1) Heat from 20°C to 200°C at 10°C / min (2) Decrease temperature from 200°C to -50°C at 5°C / min. (3) Heat from -50°C to 200°C at 10°C / min
[0086] (Melting point of wax particles) A liquid containing wax particles was dried at 60°C to obtain 2 mg of wax particles, which were then placed in an aluminum container and sealed to prepare a sample for measurement. The prepared sample was subjected to thermal analysis using the above-mentioned differential scanning calorimeter according to the temperature program shown below. The melting point T M (° C.) is the top temperature of the endothermic peak in the heating process of the temperature program (3) below. [Temperature Program]: (1) Heat from 20°C to 150°C at 10°C / min (2) Decrease temperature from 150°C to 20°C at 10°C / min. (3) Heat from 20°C to 150°C at 10°C / min.
[0087] (Determination of whether the resin is a resin particle or not, average particle size of resin particles and wax particles) The liquid containing the resin was diluted with ion-exchanged water to prepare a sample with a resin content of about 1.0%. The average particle diameter D of the resin particles in this sample was measured using a particle size distribution analyzer that uses the dynamic light scattering method under the following measurement conditions: Em (Cumulative 50% particle size on a volume basis) was measured. The particle size distribution meter used was a Nanotrac WAVEII-Q (manufactured by Microtrac Bell). When particles with a particle size were measured using this measurement method, the resin was determined to be a "resin particle" (a "water-dispersible resin"). On the other hand, when particles with a particle size were not measured using this measurement method, the resin was determined not to be a "resin particle" (a "water-soluble resin"). When measuring the particle size of wax particles, the same procedure as above was carried out except that a liquid containing wax particles was used instead of a liquid containing resin, and the average particle size D of the wax particles was obtained. Wax The measurement conditions were as follows: SetZero: 30 s, number of measurements: 3, measurement time: 120 s, shape: spherical, refractive index: 1.6, density: 1.0.
[0088] (average pigment particle size) The pigment dispersion was diluted with ion-exchanged water to prepare a sample with a pigment content of about 0.01%. The average particle diameter D of the pigment was measured for this sample using the particle size distribution meter described above under the following measurement conditions. Pig (50% cumulative particle size on a volume basis) was measured. The measurement conditions were: SetZero: 30s, number of measurements: 3, measurement time: 120 seconds, shape: aspheric, refractive index: 1.5, density: 1.0. However, when measuring the average particle size of carbon black, the refractive index was 1.8.
[0089] <Preparation of reaction solution> Each reaction solution was prepared by mixing the components (unit: %) shown in Table 1, thoroughly stirring, and then filtering under pressure with a cellulose acetate filter (Advantec) with a pore size of 3.0 μm. In Table 1, "Catiomaster PD-7" is the trade name of an amine-epichlorohydrin condensation polymer aqueous solution (cationic resin content: 50.0%) manufactured by Kawaken Fine Chemicals. Also, "BYK349" is the trade name of a silicone surfactant manufactured by BYK Japan.
[0090] TIFF2024159532000001.tif69170
[0091] <Preparation of pigment dispersion> (Pigment dispersion 1) A styrene-ethyl acrylate-acrylic acid copolymer (resin 1) with an acid value of 150 mgKOH / g and a weight average molecular weight of 8,000 was prepared. 20.0 parts of resin 1 were neutralized with potassium hydroxide in an amount equimolar to the acid value, and an appropriate amount of pure water was added to prepare an aqueous solution of resin 1 with a resin (solid content) content of 20.0%. 20.0 parts of carbon black (trade name "MCF88", manufactured by Mitsubishi Chemical), 30.0 parts of the aqueous solution of resin 1, and 50.0 parts of ion-exchanged water were mixed to obtain a mixture. The obtained mixture was subjected to a dispersion treatment at a pressure of 150 MPa using a Nanomizer (manufactured by Yoshida Machinery Co., Ltd.) with the number of passes shown in the lower part of Table 1. After centrifuging at a rotation speed of 5,000 rpm for 30 minutes to remove coarse particles, it was pressure-filtered with a cellulose acetate filter (manufactured by Advantec) with a pore size of 3.0 μm. An appropriate amount of ion-exchanged water was added to dilute the mixture, to obtain Pigment Dispersion Liquid 1 having a pigment content of 10.0% and a resin 1 (resin dispersant) content of 3.0%. The anionic group of the pigment in Pigment Dispersion Liquid 1 was 398 μmol / g.
[0092] (Pigment Dispersion 2-11) Pigment dispersions 2 to 11 were prepared in the same manner as the pigment dispersion 1 described above, except that the dispersion treatment was performed with the composition (unit: parts) shown in the upper row of Table 2 and the number of passes shown in the lower row of Table 2. In Table 2, "aqueous solution of resin 2" was prepared as follows. First, a styrene-ethyl acrylate-polyethylene glycol acrylate (product name "AE-400", NOF Corp.)-acrylic acid copolymer (resin 2) with an acid value of 25 mgKOH / g and a weight average molecular weight of 8,000 was prepared. 20.0 parts of resin 2 were neutralized with potassium hydroxide in an amount equimolar to the acid value, and an appropriate amount of pure water was added to prepare an aqueous solution of resin 2 with a resin (solid content) content of 20.0%.
[0093] TIFF2024159532000002.tif99170
[0094] <Preparation of Water Dispersion of Resin Particles> (Resin particles 1-6) 1,160 parts of ion-exchanged water were placed in a reactor and heated to the polymerization temperature shown in Table 3. In addition, 1.39 parts of potassium persulfate were dissolved in 160 parts of ion-exchanged water to prepare an initiator solution. 32 parts of the prepared initiator solution were added to the reactor and stirred. Meanwhile, 159.4 parts of ion-exchanged water, monomers of the types and amounts (parts) shown in Table 3, 1.6 parts of isooctyl thioglycolate, and 9.98 parts of an aqueous solution of an emulsifier were mixed to prepare a monomer solution. As the emulsifier, a product name "Rhodafac RS 710" (manufactured by Rhodia Novecare) was used, and an appropriate amount of ion-exchanged water was added to prepare an aqueous solution of the dispersant with a dispersant content of 30.0%. The prepared aqueous monomer solution and 129.4 parts of the initiator solution were simultaneously dropped into the reactor over 30 minutes and stirred, and then maintained at the polymerization temperature shown in Table 3 for 3 hours to obtain a reaction product. The resulting reaction product was cooled to 50°C, and then a 50% aqueous potassium hydroxide solution was added to adjust the pH to 8.5. After cooling to room temperature, the reaction product was filtered through a 200 mesh filter. An appropriate amount of ion-exchanged water was added to obtain aqueous dispersions of resin particles 1 to 6 each having a resin particle content of 30.0%. The properties of the resin particles in the aqueous dispersions obtained are shown in Table 3. The meanings of the abbreviations of the monomers in Table 3 are as follows: ·MAA: Methacrylic acid MMA: Methyl methacrylate ·HMA: Hexyl methacrylate nBMA: n-butyl methacrylate
[0095] TIFF2024159532000003.tif70170
[0096] <Preparation of aqueous dispersion of wax particles> (Wax particles 1-12) The components shown in Table 4 were mixed and the temperature and pressure were appropriately adjusted to disperse the wax. An appropriate amount of pure water was added to dilute the mixture, and aqueous dispersions of wax particles 1 to 12 each having a total wax and dispersant content of 30.0% were obtained. The properties of the wax particles in the aqueous dispersions obtained are shown in Table 4. Details of the waxes in Table 4 are shown below. Wax 1: Fischer-Tropsch wax Wax 2: Paraffin wax Wax 3: Polyethylene wax Wax 4: Fischer-Tropsch wax
[0097] TIFF2024159532000004.tif110170
[0098] (Wax particles 13) An aqueous dispersion of paraffin wax (trade name "AQUACER539", manufactured by BYK Japan) was used as the aqueous dispersion of wax particles 13. The melting point T M is 90℃, average particle diameter D Wax is 53 nm, anionic group E Wax The wax content in the aqueous dispersion was 35.0%.
[0099] <Ink Preparation> Each ink was prepared by mixing the components (unit: %) shown in Tables 5-1 to 5-3, thoroughly stirring, and then filtering under pressure with a membrane filter (manufactured by Advantec) with a pore size of 3.0 μm. In Tables 5-1 to 5-3, "BYK349" is the trade name of a silicone surfactant (manufactured by BYK Japan).
[0100] TIFF2024159532000005.tif157170
[0101] TIFF2024159532000006.tif157170
[0102] TIFF2024159532000007.tif156170
[0103] <Evaluation> (Image recording) The prepared reaction liquid and ink were filled in a cartridge, and the cartridge was set in an inkjet recording device (product name "imagePROGRAF PRO-2000", manufactured by Canon) equipped with a recording head that ejects ink by thermal energy. A heating device for drying the recording medium to which the reaction liquid and ink were applied was incorporated into this recording device at a position downstream of the recording head in the conveying direction of the recording medium. The recording environment was set to a temperature of 25°C and a relative humidity of 50%. In this example, an image recorded under the condition that one drop of 4.0 ng of ink is applied to a unit area of 1 / 1,200 inch x 1 / 1,200 inch is defined as having a recording duty of 100%. The reaction liquid and ink shown in Table 7 were applied to the recording medium in layers with a recording duty of 50% for the reaction liquid and a recording duty of 160% for the ink, and a solid image of 2 cm x 2 cm was recorded. Thereafter, the recorded image was heated and dried using a heating device by the heating method shown in Table 7. The heating temperature was measured using a radiation thermometer (product name "FT3700", manufactured by HIOKI). Details of the heating method are as shown in Table 6. In the present invention, in the evaluation criteria for each item shown below, "A" and "B" were considered to be acceptable levels, and "C" was considered to be an unacceptable level. The evaluation results are shown in Table 7. The recording media used are also shown below. Note that "Comparative Example 10" is a specific example corresponding to "Example 8" in Patent Document 1 (JP Patent Publication No. 2021-142725). Recording medium 1: Product name "Scotchcal Graphic Film IJ1220N", manufactured by 3M, material = polyvinyl chloride, 30 msec from the start of contact in the Bristow method 1 / 2 Water absorption up to = 0 mL / m 2 More than 10mL / m 2 below Recording medium 2: High-quality paper, product name "HR-101S", Canon, 30 msec from the start of contact in the Bristow method 1 / 2 Water absorption rate up to 10 mL / m 2 Super
[0104] TIFF2024159532000008.tif62170
[0105] (Abrasion resistance) A friction test was conducted by using a friction tester II (Gakushin type) abrasion resistance tester (manufactured by Tester Sangyo Co., Ltd.) conforming to JIS L0849, and a white friction cloth (cotton) specified in JIS L0803, in which the surface of the recorded image was rubbed back and forth 150 times with a load of 500 g. The image after the friction test was visually inspected, and the abrasion resistance of the image was evaluated according to the following evaluation criteria. A: No scratches were observed on the image after 150 strokes. B: Scratch marks were observed on the image after 150 reciprocal passes, but the white background of the recording medium was not visible. C: Scratch marks were observed on the image after 150 reciprocations, and the white background of the recording medium was visible.
[0106] (Color development) Using the inkjet recording device described above, the reaction liquid and ink shown in Table 7 were applied to the recording medium in the order shown, and 10 types of solid images were recorded with the recording duty changed in 10% increments between 10% and 100%. The brightness (L * ) and chroma (C * ) was measured using a fluorescence spectrodensitometer (product name "FD-7", manufactured by Konica Minolta). * and C * is based on the color difference display method specified by CIE. The color development of the image was evaluated according to the evaluation criteria shown in Table 8. In this example, when the color material was carbon black, it was designated as black ink, and when the color material was CI Pigment Blue 15:3, it was designated as cyan ink. Furthermore, when the color material was CI Pigment Red 122, it was designated as magenta ink, and when the color material was CI Pigment Yellow 74, it was designated as yellow ink. In the case of black ink, the lower the lightness, the darker the image and the better the color development. In the case of color inks (cyan, magenta, and yellow inks), the higher the saturation, the more vivid the image and the better the color development.
[0107] TIFF2024159532000009.tif255155
[0108] TIFF2024159532000010.tif95170
[0109] The disclosure of this embodiment includes the following methods and configurations. (Method 1) An inkjet recording method for recording an image on a recording medium using an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink, comprising: a reaction liquid applying step of applying the aqueous reaction liquid to the recording medium; an ink applying step of applying the aqueous ink so as to overlap at least a portion of an area of the recording medium to which the aqueous reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F (°C), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (°C) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): T M >T F ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) E Wax ≦E Em <E Pig (3) (Method 2) Average particle diameter D of the resin particles Em (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the following formula (4): (D Wax / D Em )≧1.00 (4) (Method 3) Average particle diameter D of the wax particles Wax 3. The inkjet recording method according to method 1 or 2, wherein (nm) is 100 nm or more and 200 nm or less. (Method 4) Anionic group E of the wax particles Wax 4. The inkjet recording method according to any one of Methods 1 to 3, wherein (μmol / g) is 50 μmol / g or more and 90 μmol / g or less. (Method 5) The content W of the wax particles in the water-based ink Wax (mass%), and the content W of the resin particles in the water-based ink Em 5. The inkjet recording method according to any one of Methods 1 to 4, wherein (% by mass) satisfies the relationship of the following formula (5): 1.3≦(W Em / W Wax )≦10.0 (5) (Method 6) The inkjet recording method according to any one of Methods 1 to 5, wherein the reactant contains at least one of an organic acid and a polyvalent metal salt, and a cationic resin. (Method 7) The inkjet recording method according to any one of Methods 1 to 6, wherein the material forming the wax particles is a Fischer-Tropsch wax. (Method 8) 30 msec from the start of contact of the recording medium in the Bristow method 1 / 2 Water absorption up to 10mL / m 2 The inkjet recording method according to any one of Methods 1 to 7, wherein the inkjet recording method is (Method 9) The inkjet recording method according to any one of Methods 1 to 8, in which the recording medium is heated by blowing air onto the surface of the recording medium. (Configuration 1) An inkjet recording apparatus used to record an image on a recording medium using an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink, comprising: a reaction liquid applying means for applying the aqueous reaction liquid to the recording medium; an ink applying means for applying the water-based ink so as to overlap at least a portion of an area of the recording medium to which the water-based reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F (°C), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (°C) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3). T M >T F ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) E Wax ≦E Em <E Pig (3) (Configuration 2) A set of an aqueous ink and an aqueous reaction liquid used in an inkjet recording method for recording an image on a recording medium using an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink, comprising: the inkjet recording method includes a reaction liquid applying step of applying the aqueous reaction liquid to the recording medium; an ink applying step of applying the aqueous ink so as to overlap at least a portion of an area of the recording medium to which the aqueous reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F (°C), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (°C) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax A set of an aqueous ink and an aqueous reaction liquid, characterized in that (μmol / g) satisfies the relationship of the following formula (3). T M >T F ≧(T G -10) ···(1) 4.00≧(D Wax / D Pig ) ≧ 0.70 (2) E Wax ≦E Em <E Pig (3)
Claims
1. An inkjet recording method for recording an image on a recording medium using an aqueous reaction liquid containing an aqueous ink and a reactant that reacts with the aqueous ink, comprising: a reaction liquid applying step of applying the aqueous reaction liquid to the recording medium; an ink applying step of applying the aqueous ink so as to overlap at least a portion of an area of the recording medium to which the aqueous reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F and a heating step of heating to (° C.), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (° C.) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): T M >T F ≧(T G -10) ・・・(1) 4.00≧(D Wax / D Pig )≧0.70 ・・・(2) E Wax ≦E Em <E Pig ・・・(3)
2. The average particle diameter D of the resin particles Em (nm) and the average particle diameter D of the wax particles Wax The ink jet recording method according to claim 1 , wherein (nm) satisfies the following formula (4): (D Wax / D Em )≧1.00 ・・・(4)
3. The average particle diameter D of the wax particles Wax 2. The ink jet recording method according to claim 1, wherein (nm) is 100 nm or more and 200 nm or less.
4. The anionic group E of the wax particles Wax 2. The ink-jet recording method according to claim 1, wherein (μmol / g) is from 50 μmol / g to 90 μmol / g.
5. The content W of the wax particles in the water-based ink Wax (mass%), and the content W of the resin particles in the water-based ink Em The inkjet recording method according to claim 1 , wherein (% by mass) satisfies the following formula (5): 1.3≦(W Em / W Wax )≦10.0 ・・・(5)
6. The ink jet recording method according to claim 1 , wherein the reactant contains at least one of an organic acid and a polyvalent metal salt, and a cationic resin.
7. 6. The ink-jet recording method according to claim 1, wherein the material forming the wax particles is a Fischer-Tropsch wax.
8. 30 msec from the start of contact of the recording medium in the Bristow method 1/2 Water absorption up to 10 mL / m 2 The ink jet recording method according to any one of claims 1 to 5, wherein:
9. The ink jet recording method according to claim 1 , wherein the recording medium is heated by blowing air onto a surface of the recording medium.
10. An inkjet recording apparatus used to record an image on a recording medium using an aqueous reaction liquid containing an aqueous ink and a reactant that reacts with the aqueous ink, comprising: a reaction liquid applying means for applying the aqueous reaction liquid to the recording medium; an ink applying means for applying the water-based ink so as to overlap at least a portion of an area of the recording medium to which the water-based reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F (°C), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (° C.) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): T M >T F ≧(T G -10) ・・・(1) 4.00≧(D Wax / D Pig )≧0.70 ・・・(2) E Wax ≦E Em <E Pig ・・・(3)
11. A set of an aqueous ink and an aqueous reaction liquid used in an inkjet recording method for recording an image on a recording medium using an aqueous ink and an aqueous reaction liquid containing a reactant that reacts with the aqueous ink, comprising: the inkjet recording method includes a reaction liquid applying step of applying the aqueous reaction liquid to the recording medium; an ink applying step of applying the aqueous ink so as to overlap at least a portion of an area of the recording medium to which the aqueous reaction liquid is applied; The recording medium to which the aqueous ink and the aqueous reaction liquid have been applied is heated to a predetermined temperature T F and a heating step of heating to (° C.), the aqueous ink contains a pigment, resin particles, and wax particles that are dispersed by the action of anionic groups; The heating temperature T F (° C.), the glass transition temperature T G (° C.), and the melting point T M (° C.) satisfies the relationship of the following formula (1), The average particle diameter D of the pigment Pig (nm) and the average particle diameter D of the wax particles Wax (nm) satisfies the relationship of the following formula (2), The anionic group E of the pigment Pig (μmol / g), the anionic group E of the resin particles Em (μmol / g), and the anionic group E of the wax particles Wax (μmol / g) satisfies the relationship of the following formula (3): T M >T F ≧(T G -10) ・・・(1) 4.00≧(D Wax / D Pig )≧0.70 ・・・(2) E Wax ≦E Em <E Pig ・・・(3)
Citation Information
Patent Citations