Layered thermal element

A layered thermoelectric element using an amorphous ferroelectric and paraelectric structure on aluminum generates power at low temperatures by leveraging spontaneous polarization, addressing the limitations of high-temperature requirements in existing technologies and enabling efficient thermal energy conversion.

JP2024162933APending Publication Date: 2024-11-21小野田 浩三
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023087298
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing thermoelectric elements require high temperatures and complex cooling systems to generate power, limiting their practical application, especially for low-temperature environments where vast thermal energy sources exist, such as atmospheric and underground heat.

Method used

A layered structure comprising an amorphous ferroelectric layer and an amorphous paraelectric layer, with a conductive material on both surfaces, utilizing spontaneous polarization and internal electric fields to generate power without temperature differences, achieved by forming an electrolytic oxide film on aluminum using specific polybasic acids and removing electrolytes to stabilize polarization.

Benefits of technology

The structure enables stable power generation at low temperatures below 100°C, allowing for efficient conversion of thermal energy into electricity without requiring temperature gradients, thereby harnessing previously untapped energy sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162933000001_ABST
    Figure 2024162933000001_ABST
Patent Text Reader

Abstract

To provide a thermoelectric element that can be stacked and stably operated at low temperatures of 100°C or less, even if temperature difference is not required.SOLUTION: As an amorphous ferroelectric material, an oxide film 11 made by electrolyzing an aluminum base material 12 in a polybasic acid bath with a strong acid group with a pKa value less than 2.5 is boiled with the base material, and a residual electrolyte is removed and pseudoboehmite is formed on the surface of the oxide film as an amorphous paraelectric. Then, a counter electrode 9 with a work function that promotes spontaneous polarization in the oxide film is coated on the film surface via a synthetic resin 10 containing an ionic liquid. This configuration allows stable power without temperature differences even at low temperatures of 100°C or less. In addition, by stacking such components, power proportional to the number of layers can be obtained.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a power generating unit using an electrolytic oxidation film and a power generating method. [Background technology]

[0002] When a temperature difference of 85°C is applied to a general-purpose tellurium-bismuth Seebeck element, it produces 2.5kW / m even from a heat source of less than 100°C. 2 However, to obtain a large amount of power, it is necessary to increase the effective temperature difference, and obtaining power at low temperatures requires expensive cooling methods and equipment, so practical application has not progressed.

[0003] Therefore, in order to obtain high power even with a small temperature difference, a technology has been developed that utilizes the porosity of an aluminum anodized film and deposits a thermoelectric material on the film to make it porous, thereby lowering the thermal conductivity of the element and enhancing the Seebeck effect, as shown in Patent Document 1. In addition, thermoelectric elements that do not require cooling, i.e., temperature differences, have also been developed: thermoelectric elements that utilize orientation polarization (Patent Document 2), thermoelectric elements that utilize differences in band gap width (Patent Document 3), and thermoelectric elements that utilize the thermionic emission phenomenon (Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5964199 [Patent Document 2] Patent No. 6944168 [Patent Document 3] Patent No. 6551849 [Patent Document 4] Patent No. 6147901 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the porous thermoelectric material of Patent Document 1, the anodized film itself is not a thermoelectric material as in the present invention, but the anodized film is used as a mold for the thermoelectric material. At this time, a specific thermoelectric material must be used, and the thermoelectric material can only perform at high temperatures. The thermoelectric element of Patent Document 2 does not utilize the spontaneous polarization of ferroelectrics as in the present invention, but utilizes the orientation polarization of paraelectrics. One or both ends must be made of insulators, and it is difficult to stack and serialize the elements, so only micro-power applications are expected. The thermoelectric element of Patent Document 3 does not require a temperature difference to generate electricity, as in the present invention, but generates electricity only at high temperatures of 200 to 500°C. The thermoelectric element of Patent Document 4 uses metal nanoparticles to enable the thermionic emission phenomenon that usually occurs at high temperatures at low temperatures. Metal nanoparticles such as those used here are prone to agglomeration, and the use of a dispersant reduces the thermionic emission phenomenon, so stable power generation cannot be expected.

[0006] Most environments where thermoelectric conversion is required are below 100°C. If it can be achieved at room temperature, it will be possible to utilize the enormous amount of thermal energy present in the atmosphere, underground, water, etc., which could help curb global warming. There is a demand for thermoelectric conversion technology that can generate large amounts of electricity.

[0007] The present invention was developed in light of these problems, and aims to develop an element that does not require a temperature difference, can generate electricity stably even at low temperatures below 100°C, particularly below room temperature, and can be stacked to generate large amounts of power. [Means for solving the problem]

[0008] The inventor discovered that aluminum oxide is originally used as a paraelectric in capacitors and FETs, but the surface film obtained by electrolytically oxidizing aluminum in the presence of a specific polybasic acid becomes an amorphous ferroelectric. A crystalline ferroelectric generates stable spontaneous polarization in a certain direction when poling is performed at or above the Curie point, but an electrolytically oxidized film is poled during electrolysis, generating spontaneous polarization in the film thickness direction and creating an electric field inside. As an amorphous property, it has countless localized levels inside, and even at room temperature, electric charges transition from one localized level to another due to heat, resulting in hopping conduction. An electric field due to spontaneous polarization acts on this, and the positive and negative charges in the localized levels are separated and transported to the electrodes.

[0009] However, the charge carried to the electrodes creates an electric field in the opposite direction, blocking the electric field in the ferroelectric, and the electromotive force disappears. Therefore, by placing a paraelectric with a lower capacitance than the ferroelectric on the surface of the ferroelectric, the paraelectric side is weakly polarized by the spontaneous polarization of the ferroelectric, creating a polarization difference between the two. In this way, a reverse electric field equal to or less than the electric field caused by the polarization in the paraelectric is generated between the electrodes, and only a portion of the electric field in the ferroelectric is blocked, generating an electromotive force. If it is constructed with single-crystal or polycrystalline ferroelectrics or paraelectrics, the band gap is large, so not only is it impossible to expect an electromotive force at low temperatures, but depolarization progresses as the temperature rises, which is fatal.

[0010] This phenomenon occurs because while the configuration of the present invention has a capacitor structure, the capacitance defined by dQ / dV (Q is the charge generated by the potential difference V applied from the outside) takes a negative value, as the voltage application direction is reversed, regardless of whether it is applied externally, and it functions as a capacitor with a negative dielectric constant. Also, when a certain amount of iron element is present in the aluminum, the iron component is doped into the molecular skeleton of the film, reversing the direction of polarization and increasing polarization, and further interacting with the magnetism of the combined substance, resulting in multiferroic properties.

[0011] In order to effectively link these to power generation, the researchers considered processing conditions, configuration requirements, etc., and discovered a layered structure that can generate electricity stably at low temperatures without the need for a temperature difference, and that can obtain power proportional to the number of layers by stacking.

[0012] The layered structure is characterized in that it is a laminate having an amorphous ferroelectric layer having ferroelectricity at room temperature and an amorphous paraelectric layer having a lower absolute value of capacitance than the ferroelectric layer on one side of the laminate, with conductive materials being placed on the upper and lower surfaces of the laminate.

[0013] For example, an amorphous ferroelectric material having ferroelectricity at room temperature is an electrolyte-removed product of an electrolytic oxidation film formed on the surface of a substrate made of pure aluminum or an aluminum alloy in an acidic bath containing at least one polybasic acid having a pKa value of less than 2.5 for at least one of the acid groups, and the amorphous paraelectric material is pseudo-boehmite. Aluminum electrolytic oxidation film and pseudo-boehmite have the same dielectric constant when used alone, but in this composition, since the electrolytic oxidation film has a large negative electrostatic capacitance, the absolute value of the electrostatic capacitance of the pseudo-boehmite is naturally lower than that of the electrolytic oxidation film. For this reason, the composite capacitance C is measured by an AC application method such as the usual automatic balancing bridge method. TIFF2024162933000082.tif11170 Capacitance, C OX is the electrolytic oxide film capacitance), and only a capacitance equivalent to that of pseudo-boehmite is observed.

[0014] The electrolytic oxide film here is preferably formed in a bath of a polybasic acid such as sulfuric acid, chromic acid, phosphoric acid, or oxalic acid having an acid group with a pKa value of less than 2.5, and may be a mixed acid using a plurality of these polybasic acids.

[0015] Immediately after formation, electrolytes such as residual acid and acid radicals remain inside the electrolytic oxide film, and it is necessary to prevent internal short circuits. These are removed by methods such as long-term immersion in water, immersion in water to which ultrasonic waves are applied, and hot water immersion. Among these, hot water immersion is preferred because it removes the electrolyte and simultaneously hydrates the surface of the electrolytic oxide film to form pseudo-boehmite, which functions as an amorphous paraelectric.

[0016] Furthermore, by introducing an electrolyte such as a solution of ammonium borate or an ammonium salt of an organic acid dissolved in a polyhydric alcohol such as ethylene glycol or glycerin, or an ionic liquid, between the pseudo-boehmite and the conductive material, or by introducing a synthetic resin to which such an electrolyte has been added, or by introducing a synthetic resin with low resistivity, the electrical barrier between the pseudo-boehmite and the conductive material can be neutralized or passed through.

[0017] Among these, the substrate with an iron purity of 0.1% by weight or more and less than 1% by weight is particularly preferred because of its large spontaneous polarization. The iron atoms contained in aluminum are covalently bonded to oxygen atoms in the electrolytic film. This electrolytic film is poled during electrolysis, and spontaneous polarization occurs from the substrate interface side to the surface, and the internal electric field due to the spontaneous polarization occurs in the opposite direction. The pseudo-boehmite layer on the surface of the electrolytic film is electrostatically polarized by the spontaneous polarization, creating an internal electric field in the same direction as the inside of the electrolytic film, which is a ferroelectric. Then, the internal charge moves to the electrode, and the aluminum substrate side becomes positively charged, and the electrode on the pseudo-boehmite side tends to become negatively charged. This causes the energy band to tilt upward from the substrate side to the pseudo-boehmite side. Therefore, it is preferable to place a low work function substance on the pseudo-boehmite side, because this promotes the tilting of the energy band and stabilizes the polarization.

[0018] In addition, the field oxide film Fe x Al 2-x O 3 becomes a weakly antiferromagnetic multiferroic. Therefore, it interacts with electrodes that have ferromagnetism, diamagnetism, or antiferromagnetism, and tries to return the polarization direction from the side with smaller magnetic entropy to the side with larger magnetic entropy. If a paramagnetic material with a larger magnetic entropy than the coating is placed on the surface, the polarization will be directed toward the paramagnetic material, and it is preferable to use a paramagnetic material with a low work function because the polarization can be stabilized. On the other hand, if a ferromagnetic material, antiferromagnetic material, or diamagnetic material with a small magnetic entropy is placed, the polarization will be reversed, and even if a low work function material is used, the polarization will be small and lack stability.

[0019] When using a general-purpose substrate, it is best to use aluminum with a purity of 96% by weight or more but less than 99.85%. The limit for aluminum alloys that do not cause impurities to segregate and result in poor film formation is 96% by weight. On the other hand, aluminum alloys with a purity of around 99.85% by weight, which has a low Fe content and results in high purity, have opposing polarization directions and do not show much spontaneous polarization.

[0020] High-purity aluminum refers to aluminum with a purity of 99.99% or more. The spontaneous polarization in the electrolytic oxidation film using this as the substrate is reversed, and its direction is from the pseudo-boehmite side to the oxide film side. The film does not contain iron components, and does not interact with the magnetism of the conductive material placed on the surface. Therefore, it is preferable to combine the conductive material placed on the surface with a material that has a high work function due to the inclination of the energy band caused by polarization.

[0021] After the formation of the electrolytic oxide film, it is necessary to remove the electrolyte remaining in the film, and it is preferable to immerse the film in hot water at 75° C. or higher, which allows the electrolyte to be removed and the amorphous paraelectric pseudo-boehmite to be formed at the same time. In addition, after the electrolyte is removed by immersion in water, the surface of the electrolytic oxide film can be converted to pseudo-boehmite by exposing the film to pressurized steam, in the same way as by immersion in hot water.

[0022] The electrolytic oxidation film is preferably a film formed by applying an AC voltage of more than 10 V but less than 20 V, and 40 Hz to 100 Hz. Although an electrolytic oxidation film formed by DC also has spontaneous polarization, a film formed by applying a low voltage AC voltage is preferable because it can obtain a larger electric power than a film formed by applying a high voltage DC voltage of 50 V or more, which is usually performed.

[0023] By placing a synthetic resin between the pseudo-boehmite and the conductive material, the electrical barrier between the pseudo-boehmite and the conductive material can be neutralized. However, the electrical resistance increases, and the volume resistivity at room temperature is 10 8 Ωcm or more 10 12 It is preferable to use a synthetic resin with a low resistivity of Ωcm or less as a thin film having a thickness of several μm or less.

[0024] In particular, by using an electrolyte or an electrolyte-containing synthetic resin between the pseudo-boehmite and the conductive material, it is possible to obtain a high current flow rate by slipping through the electrical barrier. The former is preferable when it is used as a high current source in a wound structure by soaking it into paper or nonwoven fabric, as in electrolytic capacitors, while the latter is suitable for use as a high voltage source by laminating flat plates. In this case, it is preferable to add an ionic liquid to prevent the electrolyte or solvent from volatilizing or leaking out. By selecting a synthetic resin and adding a few percent of ionic liquid, the volume resistivity can be increased to 10 2 Ωcm to 10 4 It is possible to reduce the resistance by approximately Ωcm.

[0025] In this way, by satisfying the requirements for forming an electrolytically oxidized film that functions as a ferroelectric, the requirements for the components of the substrate, the requirements for generating pseudo-boehmite that functions as an amorphous paraelectric, the requirements for suppressing an electric barrier, and the work function and magnetic requirements of the conductive material on the surface, spontaneous polarization in the electrolytically oxidized film is promoted and stabilized, making it possible to generate electricity without the need for a temperature difference. Effect of the Invention

[0026] The present invention provides a stackable layered thermal element that can generate power at temperatures as low as 100° C. or less without the need for a temperature differential. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a front view (with the electrolytic cell shown in perspective) illustrating the power source, electrolytic cell, and temperature regulator used to electrolyze an aluminum substrate. [Diagram 2] FIG. 2 is a perspective view of an example of assembling an aluminum base material that has been subjected to electrolytic treatment and residual electrolyte removal treatment, a synthetic resin, and a counter electrode. [Diagram 3] FIG. 3 is a cross-sectional view of an example of a layered structure made of an aluminum base material that has been subjected to electrolytic treatment and residual electrolyte removal treatment, a synthetic resin, and a counter electrode. [Figure 4] FIG. 4 is a side view showing the test piece assembled into the electrode being inserted into a precision vice as a fixture having a heater with a thermocouple attached. [Diagram 5] FIG. 5 shows an example of the second and third quadrants of an IV graph obtained by measuring a test piece. [Figure 6] Figure 6 shows an example of incorporating a power graph into the second quadrant of an IV graph obtained by measuring a test piece. [Figure 7] FIG. 7 is an example of a graph plotting the relationship between peak power density and temperature from IV data obtained by measuring a test specimen. [Figure 8] Figure 8 is a cross-sectional photograph of an oxide film formed by alternating current electrolysis in an oxalic acid bath on a pure aluminum substrate with a purity of 99.5% (hereafter referred to as PA2), observed with a transmission electron microscope H-9500 (manufactured by Hitachi High-Technologies). The photograph shows the electrolytic film, the evaporated carbon on the surface of the film, and the aluminum substrate. [Figure 9]Figure 9 is a graph showing the Fe concentration (left axis) and secondary ion intensity of Al and O (right axis) measured from the surface toward the substrate while irradiating the surface of the oxide film electrolyzed by AC in the oxalic acid bath used in Figure 8 with O2 primary ions using a secondary ion mass spectrometer PHI ADEPT1010 (manufactured by ULVAC-PHI). [Figure 10] Figure 10 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring a test specimen prepared by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, followed by sputtering with pure Mg. [Figure 11] FIG. 11 shows a graph in the second and third quadrants of the IV data obtained by measuring a PA2 substrate that was subjected to AC electrolysis in an oxalic acid bath and boiled, followed by sputtering of pure Mg to prepare a test specimen. [Figure 12] Figure 12 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring a test specimen in which a PA2 substrate was subjected to AC electrolysis in an oxalic acid bath and boiled, to which an Mg alloy was bonded using only an adhesive (for comparison, a specimen in which pure Mg was sputtered is also shown). [Figure 13] FIG. 13 shows a graph in the second and third quadrants of the IV data obtained by measuring a PA2 substrate that was subjected to AC electrolysis in an oxalic acid bath and boiled, and then bonding the Mg alloy to the substrate using only an adhesive. [Figure 14] Figure 14 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring a test piece made by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and then placing an Mg alloy on paper impregnated with ionic liquid (for comparison, a sample sputtered with pure Mg is also shown). [Figure 15] Figure 15 shows a graph in the second and third quadrants of the IV data obtained by measuring a PA2 substrate that was subjected to AC electrolysis in an oxalic acid bath and boiled, and then preparing a test piece by placing a paper impregnated with an ionic liquid and an Mg alloy on top of the paper. [Figure 16]Figure 16 is a graph plotting the relationship between peak power density and temperature obtained from IV data obtained by measuring a test specimen prepared by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding an Mg alloy to the substrate using an adhesive containing added ionic liquid (for comparison, a specimen obtained by sputtering pure Mg is also shown). [Figure 17] FIG. 17 shows a graph in the second and third quadrants of the IV data obtained by measuring a test piece prepared by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding an Mg alloy to the substrate using an adhesive containing added ionic liquid. [Figure 18] Figure 18 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring a test specimen in which a PA2 substrate was subjected to AC electrolysis in an oxalic acid bath and boiled, and then bonded to the same pure aluminum as the substrate with an adhesive containing added ionic liquid (for comparison, a specimen bonded to an Mg alloy is also shown). [Figure 19] Figure 19 is a graph plotting the relationship between electromotive force and temperature from IV data obtained by measuring a test specimen in which a PA2 substrate was subjected to AC electrolysis in an oxalic acid bath and boiled, and then bonded to the same pure aluminum as the substrate with an adhesive containing added ionic liquid (for comparison, a specimen bonded to an Mg alloy is also shown). [Figure 20] Figure 20 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring test pieces prepared by bonding a commercially available oxalic acid bath coated product and a commercially available sulfuric acid bath coated product with an adhesive containing a magnesium alloy and an ionic liquid. [Figure 21] FIG. 21 is a graph plotting the relationship between the peak power density and DC voltage from the IV data at 20°C obtained by measuring a PA2 substrate that was subjected to oxalic acid bath electrolysis at various DC voltages and boiling treatment, and then directly contacting the Mg alloy with the substrate. [Figure 22] 22A and 22B are photographs taken with an optical microscope MX-61 (Olympus) of the upper surface of a coating formed by AC electrolysis in an oxalic acid bath on substrates made of PA2 and high-purity aluminum (hereafter abbreviated as HPA) with a purity of 99.999%, respectively. [Figure 23] Figure 23 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring test pieces prepared by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and AC electrolysis in a sulfuric acid bath, followed by boiling treatment, and then bonding each to an Mg alloy with an adhesive containing an ionic liquid (for comparison, a commercially available oxalic acid coated product bonded to an Mg alloy is also shown). [Figure 24] FIG. 24 is a graph plotting the relationship between the peak power density and electrolysis voltage from the IV data at 20°C obtained by measuring a PA2 substrate that was electrolyzed in an oxalic acid bath at various AC voltages using a 50 Hz square wave and then boiled, and then directly contacting the Mg alloy with the substrate. [Diagram 25] Figure 25 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring a test piece prepared by subjecting a PA2 substrate to oxalic acid bath electrolysis at 50 Hz, 15 V square wave, triangular wave, and sine wave, followed by boiling treatment, and then bonding an Mg alloy with an adhesive containing ionic liquid (for comparison, a commercially available oxalic acid coated product bonded to an Mg alloy is also shown). [Figure 26] FIG. 26 is a graph plotting the relationship between peak power density and electrolysis frequency from the IV data obtained by measuring a PA2 substrate that was electrolyzed in an oxalic acid bath at various frequencies from 0 to 500 Hz using a 15 V square wave and then boiled. The test specimen was then bonded to an Mg alloy using an adhesive containing an ionic liquid. [Figure 27] Figure 27 is a graph plotting the relationship between the peak power density from the IV data obtained by measuring the test pieces, in which a PA2 substrate was subjected to AC electrolysis in an oxalic acid bath and boiled, and an Mg alloy was bonded to the PA2 substrate using adhesives with different volume resistivities to which ionic liquid had been added, and the volume resistivity of the adhesive to which no ionic liquid had been added. [Figure 28] Figure 28 is a graph plotting the relationship between peak power density and temperature from the IV data obtained by measuring test pieces prepared by subjecting pure aluminum to AC electrolysis in an oxalic acid bath and boiling treatment, to which an Mg alloy was bonded using an adhesive containing ionic liquids of different concentrations. [Figure 29]Figure 29 is a graph plotting the relationship between the peak power density and the work function of each counter electrode from the IV data obtained by measuring each test piece at 60°C, in which a PA2 base material was subjected to AC electrolysis in an oxalic acid bath and boiled, and various paramagnetic, diamagnetic, and ferromagnetic materials were bonded as counter electrodes with an adhesive containing an ionic liquid. [Diagram 30] Figure 30 is a graph in which a total of 16 types of test specimens were prepared by subjecting four types of substrates, HPA, 99.85% pure aluminum (hereinafter abbreviated as PA1), PA2, and 99% pure aluminum (hereinafter abbreviated as PA3), to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding Mg alloy, isotropic graphite, the same Al as the substrates, and Sn as the counter electrodes with an adhesive containing added ionic liquid. The test specimens were measured, and the IV data was extracted from the data at 60°C, and the relationship between the peak power density and the work function of each counter electrode was plotted. [Diagram 31] Figure 31 shows the relationship between the peak power density from the IV data obtained by measuring each test piece at 60°C and the impurity concentration measured with a ZSX primus X-ray fluorescence spectrometer (Riken), which has been plotted and fitted with a dotted line. Test pieces were prepared by subjecting substrates of different aluminum purities to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding a Mg alloy to the test pieces using an adhesive containing added ionic liquid. [Diagram 32] FIG. 32 shows a plot of the relationship between the Fe element concentration and the impurity concentration in the substrate used in FIG. 31, fitted with a solid line (the graph in FIG. 31 is also shown for comparison). [Diagram 33] FIG. 33 shows a plot of the relationship between the Si element concentration and the impurity concentration in the substrate used in FIG. 31, fitted with a solid line (the graph in FIG. 31 is also shown for comparison). [Diagram 34] FIG. 34 shows a plot of the relationship between the Cu element concentration and the impurity concentration in the substrate used in FIG. 31, fitted with a solid line (the graph in FIG. 31 is also shown for comparison). [Diagram 35] FIG. 35 shows a plot of the relationship between the Mn element concentration and the impurity concentration in the base material used in FIG. 31, fitted with a solid line (the graph in FIG. 31 is also shown for comparison). [Diagram 36] FIG. 36 shows a plot of the relationship between the Zn element concentration and the impurity concentration in the substrate used in FIG. 31, fitted with a solid line (the graph in FIG. 31 is also shown for comparison). [Figure 37] Figure 37 shows a Sawyer-Tower circuit diagram for evaluating the dielectric properties of a test piece when a PICOSCOPE 2208B (manufactured by Picotechnology) is used as the oscilloscope device and a programmable AC / DC power supply EC750SA (manufactured by NF Circuit Design Block) is used as the power supply. [Figure 38] Figure 38 shows the hysteresis data at room temperature when a test specimen was prepared by bonding a 99% pure aluminum (hereafter referred to as PA3) substrate to an adhesive containing ionic liquid, which was prepared by subjecting the substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and using the specimen as a sample capacitor in the circuit of Figure 37. [Figure 39] Figure 39 shows the hysteresis data at room temperature when a test specimen was prepared by subjecting an HPA substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding the same HPA as the substrate with an adhesive containing added ionic liquid, and using this specimen as a sample capacitor in the circuit of Figure 37. [Diagram 40] Figure 40 shows the hysteresis data at room temperature when a test piece was prepared by subjecting a PA3 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, to which an Mg alloy was attached using an adhesive containing an ionic liquid, and the test piece was used as a sample capacitor in the circuit of Figure 37. [Diagram 41] Figure 41 shows data on the electromotive force that appears on the test pieces prepared by subjecting a PA2 substrate to AC electrolysis in an oxalic acid bath and boiling treatment, and then bonding a paramagnetic Mg plate, ferromagnetic Ni and Gd, and a diamagnetic graphite sheet with an adhesive containing ionic liquid, in a low-temperature incubator at a constant temperature using a heater that sandwiched the test pieces. The data was collected by using the substrate side as the anode. [Diagram 42]Figure 42 shows a circuit diagram for observing the charge transfer from the test piece to the electrolytic capacitor by connecting an electrolytic capacitor and a switch in parallel while keeping the test piece at 25°C in a low-temperature incubator after preparing a test piece by subjecting a PA3 base material to AC electrolysis in an oxalic acid bath and boiling treatment, and then measuring the voltage across the test piece to observe the charge transfer from the test piece to the electrolytic capacitor. [Diagram 43] Figure 43 shows a plot of the change in terminal voltage over time every minute after the switch in Figure 42 is opened, along with two fitting curves in which the parameters of the terminal voltage obtained from the equivalent circuit in Figure 44 are changed. [Diagram 44] Figure 44 shows the equivalent circuit of Figure 42, in which a capacitance component, an insulation resistance, and a series equivalent resistance component are provided for the electrolytic capacitor, and a capacitance component, an insulation resistance, a series equivalent resistance component, and a DC voltage source are provided for the test piece. [Diagram 45] FIG. 45 is a circuit diagram for measuring the insulation resistance of an electrolytic capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] <Method of creating test pieces and method of creating IV data necessary for explaining the embodiments of the present invention> A method for preparing a test piece and a method for preparing IV data, which are necessary to explain the embodiment of the present invention, will be described with reference to the drawings. The electrolytic oxidation film is the central feature of the present invention, and the method for forming the film is important for the preparation of the test piece. Therefore, the apparatus shown in FIG. 1 was adopted. An aqueous solution for electrolysis 3 and a stirrer 4 are placed in a square glass container 1 with external dimensions of 120×120×150 mm, and the four sides around the container are insulated with 10 mm thick polystyrene foam 2. Three copper pipes are passed through the container at intervals of 40 mm, and a graphite plate 7 with dimensions of 120×84×8 mm is hung on both ends of the pipes, and an aluminum base material 8 is hung on the central pipe with copper wire. The graphite plate 7 and the aluminum base material 8 are connected to the cathode terminal and the anode terminal of a programmable AC / DC power supply EC750SA (manufactured by NF Corporation) 6, respectively. The glass container 1 surrounded by the polystyrene foam 2 is placed on the electric heating surface of a cool stirrer CPS-30 (manufactured by Iuchi Seiei-do) 5, and the temperature of the aqueous solution for electrolysis 3 is controlled by rotating the stirrer 4 at a low speed. The power source 6 can output direct current and alternating current of various waveforms.

[0029] The electrolytic oxide film made by the device in Figure 1 contains residual electrolyte and acid radicals, and in order to remove these, the film is immersed in pure water for a long period of time or in boiled pure water. When the film is boiled or exposed to pressurized steam after removing the electrolyte, the surface of the electrolytic oxide film opposite the substrate 11 is hydrated and changes to pseudo-boehmite. In other words, a composite film of amorphous ferroelectric and amorphous paraelectric is formed. The product that has undergone this process is the composite film 12 in Figures 2 and 3, which is Al. The electrode is formed on the surface of a miniature substrate 11. This is then covered with a resin 10 and a counter electrode 9.

[0030] However, Fig. 2 and Fig. 3 are representative examples of test pieces for obtaining data of the present invention, and the embodiments are not limited to these examples. Examples of the embodiments include a case where the one shown in Fig. 3 is laminated, a case where the composite film 12 is applied to both sides of an aluminum substrate and both sides are covered with the resin 10 or the counter electrode 9, a case where the resin 10 is wound with electrolyte-containing paper, a case where the counter electrode 9 is a thin film such as a vapor deposition film or a sputtering film, a case where the substrate 12 is a molded product or an extruded material, a case where the resin 10 or the counter electrode 9 is a part of the surface, a method that does not use an electrolytic oxidation film, for example, a case where an amorphous ferroelectric is formed on an electrode by sputtering or the like, and an electrode is further formed on the amorphous ferroelectric.

[0031] As shown in FIG. 4, a single specimen 13 of the present invention thus obtained is sandwiched between an aluminum electrode 14 and a heat insulating material 15 to produce a specimen 16, which is then inserted between a heater WALN-3 (manufactured by WAELOW) 21 with a thermocouple attached to a precision vice VMV-20 (manufactured by VERTEX) 17, and the clamping bolt 18 is lightly tightened to fix the specimen to the vice 17. Furthermore, the heater 21 and the side of the inserted specimen 16 are insulated with a 10 mm thick foamed polypropylene. This is placed in a low-temperature incubator SB01 (manufactured by ETAC), and the temperature controller Model 335 (manufactured by Lake Shore) connected to the heater 21 and the low-temperature incubator are used to control both sides and the side of the specimen to the same temperature. Then, IV data is taken while applying a voltage with an electrometer 8252 (manufactured by ADC) so that the aluminum substrate side becomes the anode and the counter electrode side becomes the cathode.

[0032] The IV data are only taken in the second and third quadrants, i.e., when the applied voltage is negative. This is because when the aluminum substrate side appears as the anode in the electromotive force of the test piece, the power and electromotive force data can only be obtained in these quadrants. Conversely, when the substrate side is the cathode, the connection between the electrometer and the test piece is reversed to obtain the data required for the second and third quadrants. Curve 24 in Figures 5 and 6 is an example of IV data, and the intersection point 25 with the x-axis represents the release voltage, i.e., the electromotive force. Furthermore, by calculating and plotting the IV product from IV curve 24, power curve 26 is obtained, from which peak power 27 is obtained. Furthermore, by plotting the relationship between the peak power divided by the joint area of ​​the counter electrode of the test piece, i.e., the peak power density value, and the measurement temperature, the temperature dependence curve 28 in Figure 7 is obtained. The IV data acquisition conditions are shown in Table 1.

[0033] [Table 1]

[0034] <How the present invention is achieved> The process leading to the embodiment of the present invention will be described in detail with reference to the drawings. First, the present invention is a method for manufacturing a composite film made of an electrolytic oxidation film and pseudo-boehmite, and a counter electrode, with a synthetic resin or the like interposed therebetween. A test piece was prepared by sputtering pure Mg (work function 3.66 eV) to a thickness of 0.1 μm on the surface of a composite coating obtained from a PA2 substrate under the conditions shown in Table 2 below.

[0035]

Table 2

[0036] The IV characteristics of this test piece were examined under the conditions in Table 1, and the data at 60°C was extracted as shown in FIG. 11. The peak power density obtained from this data is plotted for each measurement temperature as shown in FIG. 10. The temperature dependence curve 43 in FIG. 10 shows that the peak power density is 1 nW / cm even in the range of 60 to 100°C. 2 11, from the intersection 45 of the curve 44 and the x-axis to around −2 V, the curve 44 appears as a rectifying curve that asymptotically approaches the x-axis, and it was confirmed that there is an electrical barrier.

[0037] However, it was found that the power increases when the counter electrode is joined via a synthetic resin. This is shown in Figures 12 and 13. Figures 12 and 13 show a composite film obtained by bonding a PA2 substrate under the conditions in Table 2 to the surface of the composite film, on which an Mg alloy AZ31 (work function 3.7 eV), which has a work function equivalent to that of pure Mg, is bonded with an epoxy resin adhesive (volume resistivity 4.1×10 11 The test pieces were prepared by bonding at room temperature (1 MPa) with adhesive A) (Hexagonal strength Ωcm, glass transition temperature -65°C, hereafter abbreviated as adhesive A).

[0038] Figure 12 shows a comparison with the temperature dependency curve 43 of a pure Mg sputtering test piece, and the temperature dependency curve 46 of adhesive A shows a higher power. Also, Figure 13 shows the IV characteristics at 60°C under the conditions in Table 1, and the IV curve 47 is linear, showing no rectification and no electrical barrier.

[0039] In this situation, we discovered that when an electrolyte such as an ionic liquid is used, high power can be generated regardless of the electrical barrier. We used methyltributylammonium bis(trifluoromethylsulfonyl)imide (electrical conductivity 2.2 mS / cm, window potential 5.7 V, hereafter abbreviated as "N 1444 ][NTf 2 When a 40 μm thick glassine paper soaked in the sol-gel coating solution was placed between the composite film obtained under the conditions in Table 2 on a PA2 substrate and an AZ31 plate, a large amount of electricity was generated.

[0040] This is shown in Figures 14 and 15. Figure 14 compares the temperature dependence curve 43 of the pure Mg sputtering test piece, and the temperature dependence curve 49 of the ionic liquid shows power three orders of magnitude higher. Although it generates an extraordinary amount of power compared to the adhesive in Figure 12, in Figure 15, the IV curve 50 approaches the x-axis from the intersection point 51 to around -2.3 V, and a rectification curve due to the electrical barrier appears. This shows that the ionic liquid obtains a large amount of power without being affected by the electrical barrier.

[0041] This phenomenon is not caused by a chemical reaction between the ionic liquid as an electrolyte, the substrate as an anode (reduction electrode), and the counter electrode as a cathode (oxidation electrode).The electrons in the composite film move to the cathode side and behave as if they are reducing the cathode, so no chemical reaction (oxidation reaction at the cathode) occurs.

[0042] On the other hand, because this ionic liquid is not a solid, it is not possible to fix or deposit bulk materials, and only a weak current can be expected with only the synthetic resin, which is an insulator. Unlike surfactants, ionic liquids exhibit electrical conductivity on their own without water, but adding ionic liquids to synthetic resins is equivalent to introducing a localized level into the insulator, similar to an electrolyte in water, and promotes hopping conduction between the band gaps of the composite film and the synthetic resin, making it unaffected by electrical barriers.

[0043] This is shown in Figures 16 and 17. Figures 16 and 17 show the results of the adhesive A used in Figures 12 and 13 applied to the surface of the composite film obtained under the conditions shown in Table 2 using a PA2 substrate. 1444 ][NTf 2 ]The test specimens were prepared by bonding AZ31 sheets at room temperature (1 MPa) with a material containing 5 wt% ionic liquid, curing for more than one week, and then curing at 100°C for 12 hours.

[0044] In comparison with the temperature dependence curve 43 of a pure Mg sputtering specimen in Figure 16, the temperature dependence curve 52 shows power two orders of magnitude higher. Also, in Figure 17, the IV curve 53 approaches the x-axis asymptotically from the intersection point 54 to around -3 V, revealing a rectification curve due to an electrical barrier. Figures 16 and 17 show that the power can be increased without being affected by the electrical barrier by adding a small amount of ionic liquid.

[0045] Up to this point, we have shown examples where the counter electrode of the aluminum substrate is made of a material with a lower work function than the substrate in order to explain the necessity of using synthetic resins, etc., but here we will show examples that serve as an opportunity to show that the generation of electricity is due to physical factors that occur within the composite film. These are Figures 18 and 19. These are examples where the surface of a composite film obtained under the conditions in Table 2 using a PA2 substrate was coated with adhesive A [N 1444 ][NTf 2 ]The test specimen was made by adding 5 wt% ionic liquid and bonding the same aluminum as the base material at room temperature (1 MPa), leaving it to cure for more than a week, and then curing it at 100°C for 12 hours.

[0046] In Fig. 18, temperature dependence curve 55 shows a composite coating made of an electrolytic oxidation film and pseudo-boehmite sandwiched between a PA2 substrate and the same material, and is compared with temperature dependence curve 52 showing a composite coating sandwiched between a PA2 substrate and AZ31. Meanwhile, Fig. 19 shows the temperature dependence of electromotive force, with curve 57 showing a composite coating sandwiched between PA2 substrates, and is compared with curve 56 showing a composite coating sandwiched between PA2 and AZ31.

[0047] From FIG. 18, the data shown by the temperature dependence curve 55 is generated between the same aluminum, that is, between electrodes with no work function difference, and indicates that it is due to a physical phenomenon in the composite film rather than a chemical reaction. On the other hand, the temperature dependence curve 52 shows a power density one order of magnitude higher than that of the temperature dependence curve 55, which is the effect of the low work function of AZ31. The difference between the curves 57 and 56 in FIG. 19 is a constant value of 0.56 V at 60° C. or higher, and the energy to move the elementary charge against this electromotive force difference is 0.56 eV, which is almost the same as the work function difference between aluminum and AZ31, 0.58 eV. This suggests that the work function difference affects the power density.

[0048] From these results, it was believed that the electromotive force and electric power obtained were generated by a physical phenomenon occurring in the composite film. Therefore, we investigated what was happening in the composite film. The electrolytic oxidation film on the aluminum substrate mainly consists of amorphous aluminum oxide. However, pure aluminum contains impurities such as Si, Fe, Cu, Mn, Zn, and Ti as shown in Table 3, and aluminum alloys further contain Si, Cu, Mn, Mg, etc. as additives. Here, components other than aluminum in aluminum alloys will be called impurities.

[0049]

Table 3

[0050] FIG. 31 shows the results of the composite coating obtained by the method shown in Table 2 using high-purity aluminum, pure aluminum, and aluminum alloys shown in Table 3 as substrates, and the ionic liquid [N 1444 ][NTf 2 The Mg alloy AZ31 was bonded at room temperature (1 MPa) with adhesive A containing 5 wt% of ZnO, and after curing for more than one week, it was cured at 100°C for 12 hours to prepare the test specimens. The data at 60°C was extracted from the IV data collected for each test specimen using the method described in Table 1, and the peak power density was calculated from it. The correlation with the amount of impurities in the substrate was plotted to draw a fitting curve 89.

[0051] The composition of the aluminum material listed in Table 3 was calculated by excluding element data other than Al, Si, Fe, Cu, Mn, Mg, Cr, Zn, and Ti from the measurement data using a fluorescent X-ray spectrometer ZSX primus (manufactured by Riken), and standardizing and recalculating the data using these nine elements. The amount of impurities was calculated from this. Furthermore, in Figures 32 to 36, the relationship between the concentration of Fe, Si, Cu, Mn, and Zn elements in the impurities of each substrate and the total amount of impurities is plotted to draw fitting curves 90 to 94, which are compared with fitting curve 89 in Figure 31, which is a correlation with power density. As a result, only fitting curve 90 of Fe element concentration is approximated to fitting curve 89 of power density, and a correlation was only observed between the power obtained from the test piece and Fe.

[0052] From this correlation, it was speculated that the origin of the electromotive force was due to Fe being doped into the aluminum oxide skeleton, which is the electrolytic oxidation film. It is known that Si is physically incorporated into the electrolytic oxidation film and forms voids, and Cu is said to concentrate at the interface between the aluminum and the electrolytic oxidation film. Since Mn, Mg, Zn, etc. have no correlation with the electric power, it is thought that they are not doped into the film. Therefore, we decided to investigate the distribution of Fe components in the electrolytic oxidation film. Figure 8 shows a cross section of a small piece of PA2 substrate taken from the surface of the electrolytic oxidation film made under the conditions in Figure 2 (but without boiling) and carbon-deposited, observed with a transmission electron microscope H-9500 (Hitachi High-Tech). The thickness of the film 29 was 2.3 μm.

[0053] The surface of this film was analyzed using a secondary ion mass spectrometer, PHI ADEPT1010 (manufactured by ULVAC-PHI). 2 Primary ions (accelerating voltage 6 kV) were irradiated to an area of ​​18 × 18 μm, and secondary ions generated during sputtering were detected to calculate the Fe concentration (calculation standard was Al 2 O 3 ).that This is curve 34 in Figure 9. Line 35 indicates the interface between the substrate and the electrolytic oxide film. Since Fe is distributed almost uniformly in proportion to the secondary ion strength of Al and O in the internal region of the electrolytic oxide film and no concentrated areas are observed, it is believed that Fe is doped into the molecular framework without any physical phenomena such as void formation or concentration at the film interface.

[0054] From this point, we considered the case where Fe is doped into aluminum oxide. 2 O 3 In the case of Al, when the Fe atom is replaced by the host cation Al ion, the Fe atom tends to adopt the same valence triad as the host cation due to covalent bonding. At the same time, the Fe electron configuration prefers the half-filled triad for the exchange correlation energy, because the exchange splitting and exchange correlation energy are maximized when the Fe electron configuration is half-filled. As a result, the Fe atom forms a hybrid state with the ligand anion O, resulting in Fe x Al 2-x O 3 The crystals of this material exhibit multiferroic properties, possessing both ferroelectricity and antiferromagnetism even at room temperature. Multiferroic properties are a property in which a material possesses ferroelectricity and (anti)ferromagnetism simultaneously, with each property interacting with the other. It was suspected that this interaction also occurs in amorphous electrolytic oxide films.

[0055] So, Fe x Al 2-x O 3 The dielectric properties of the electrolytic oxidation film on the substrate, which is expected to form a PA3 substrate, were investigated. 1444 ][NTf 2 ]5wt% of the adhesive was used to bond the same aluminum as the substrate at room temperature (1MPa), and after curing for more than one week, the specimen was cured at 100℃ for 12 hours to prepare a test piece. The specimen was connected with the positive and negative poles reversed using an impedance analyzer IM3570 (HIOKI), and 1V was applied in reverse to measure the capacitance at room temperature at 100Hz, which was 22.7nF. A film capacitor with a capacitance of 1μF, which is much larger than this capacitance, was used as the reference capacitor to measure the dielectric properties using the Sawyer-Tower circuit in Figure 37. A 3.3kΩ compensation resistor was used for the compensation resistor 97, and a sine wave effective voltage of 50V was supplied to the power supply 99 from an EC750SA (NF Circuit Design Block).

[0056] As a result, hysteresis appeared as shown in Figure 38, and the residual polarization was ±0.47μC / cm when the applied electric field was 0V / cm. 2 (Film thickness 2μm, area 4.2cm 2 When this was applied to an HPA substrate, a small hysteresis appeared as shown in Figure 39, and the residual polarization was 0.20 μC / cm 2 (Film thickness 2.9μm, area 4.2cm 2 In other words, it was found that the composite film formed by the electrolytic process can have ferroelectricity even if it is amorphous or does not contain Fe components.

[0057] At the same time, it was found that the remanent polarization increases due to the inclusion of Fe. Furthermore, when AZ31 was bonded to a composite film of PA3 substrate in the same manner, hysteresis appeared as shown in Figure 40. The remanent polarization was 0.57μC / cm 2 (Film thickness 2μm, area 4.2cm 2 It was confirmed that the polarization varies depending on the type of counter electrode. This is consistent with the results in Figure 18, and means that the polarization varies by creating a work function difference between the substrate and the counter electrode.

[0058] Since the pseudo-boehmite layer in the composite film is not formed by electrolysis, i.e., application of an electric field, it does not become a ferroelectric but acts as a paraelectric. The spontaneous polarization of the electrolytic oxidation film, which is a ferroelectric, dielectrically polarizes the pseudo-boehmite layer, so that the composite film appears to have ferroelectric properties.

[0059] The magnetic properties were also confirmed. The PA2 substrate was coated with a composite film obtained by the method described in Table 2, and each of the magnetic materials Mg, a paramagnetic material, Ni, a ferromagnetic material Gd, a ferromagnetic material that changes to a paramagnetic material at 18°C, and diamagnetic expanded graphite HT-715 (manufactured by eGRAF) was soaked in ionic liquid [N1444 ][NTf 2 5wt% of adhesive A was used for room temperature bonding (1MPa), and after curing for more than one week, it was heated at 100°C for 1 The specimens were cured for 2 hours.

[0060] As shown in Figure 4, the test piece was sandwiched between two heaters 21 and fixed in a precision vice 17, then cooled to -11°C in a low-temperature incubator SB01 (ETAC), and the heater was heated from -10 to 100°C at a rate of 1°C / min using a temperature controller Model 335 (Lake Shore), while the electromotive force was measured with an electrometer 8252 (ADC). The results are shown in Figure 41.

[0061] The reference is connected so that the substrate side is the anode and the magnetic material side of the counter electrode is the cathode, and the paramagnetic material (curve 103) that does not have magnetic order has a large positive electromotive force, while the ferromagnetic material (curve 105) and diamagnetic material (curve 106) that have magnetic order have relatively small negative electromotive forces. Therefore, when the ferromagnetic material Gd (curve 104) with a Curie point 107 at 18°C ​​is used as the counter electrode, the direction of the electromotive force suddenly changes near the Curie point and rapidly changes to a positive electromotive force.

[0062] This phenomenon indicates that the spontaneous polarization of the ferroelectric material is reversed, and suggests that the electrolytic oxidation film, which is an amorphous ferroelectric material, is the source of the electromotive force. x Al 2-x O 3 Since the electrolytic oxidation film containing the component is considered to be a weak antiferromagnetic material, it interacts with the magnetic material at the opposite pole, reversing the polarization and reversing the electromotive force. In other words, it determines the direction of polarization from the side with smaller magnetic entropy to the side with larger magnetic entropy. This phenomenon means that in the case of an electrolytic oxidation film of HPA that does not contain Fe, the polarization is not affected regardless of what kind of magnetic material is placed at the opposite pole.

[0063] In this way, the electrolytic oxide film formed on the aluminum substrate in a strong polybasic acid bath exhibits ferroelectricity and spontaneously polarizes in the thickness direction, while the adjacent low-capacity paraelectric is influenced by the ferroelectric and dielectrically polarized, forming a smaller polarization than the ferroelectric. As a result, only an electric field dependent on the polarization of the paraelectric is generated between the electrodes, so the internal electric field in the electrolytic oxide film is not shielded and an electromotive force is generated between the electrodes. This polarization also creates a tilt in the energy band, which is in the opposite direction to the internal polarization and the electric field between the electrodes.

[0064] When polarization occurs from the substrate to the counter electrode, the substrate becomes the positive electrode and the counter electrode becomes the negative electrode, and the energy band slopes downward from the negative electrode side to the positive electrode side. Therefore, in this case, by using a low work function material for the counter electrode, the slope of the energy band is increased, promoting polarization and stabilizing it. On the other hand, when polarization occurs in the opposite direction, polarization is promoted by using a high work function material for the counter electrode.

[0066] However, when an electrolytically oxidized film containing Fe is used, the energy band slopes downward from the paraelectric side to the electrolytically oxidized film side, and an electrical barrier appears between the pseudo-boehmite layer surface and low work function materials such as p-type semiconductors. When an electrolytically oxidized film made of high purity aluminum is used, a barrier appears between the pseudo-boehmite layer surface and high work function materials such as n-type semiconductors. Therefore, it is necessary to insert an electrolyte, synthetic resin, or a synthetic resin containing an electrolyte between the pseudo-boehmite layer and the electrode in order to break the electrical barrier.

[0067] The phenomenon discovered as a result of the accumulation of such various verifications is the basis of this invention. From here, we will explain in detail with reference to the figures the composite film formation conditions, synthetic resin conditions, and ionic liquid conditions in Table 2, which are part of the requirements of this invention.

[0068] <Embodiments that constitute the requirements of the present invention> The amorphous ferroelectric of the present invention is, for example, an electrolytic oxidation film of aluminum. Regardless of the electrolytic method such as direct current, alternating current, or orthogonal superposition, aluminum is electrolytically oxidized with various acids having at least one acid group with a pKa value of less than 2.5, such as sulfuric acid, phosphoric acid, chromic acid, and oxalic acid. This refers to a film formed by electrolytic oxidation in an aqueous solution containing at least one basic acid, with any electrolyte remaining inside removed.

[0069] Electrolytic oxidation coatings using direct current have a structure in which a thin barrier film is formed in the area in contact with aluminum, and then a honeycomb-like porous film is formed on top of that, with pores several tens of nanometers in diameter facing the surface. Commercially available electrolytic oxidation coatings are anodic oxidation coatings made with direct current (or a superposition of direct current and alternating current) in a sulfuric acid bath or oxalic acid bath, and electricity can also be obtained from these commercially available electrolytic oxidation coatings (however, they are composite coatings that form pseudo-boehmite).

[0070] Figure 20 shows the results of the measurements of [N 1444 ][NTf 2 ]The test specimens were made by bonding AZ31 sheets at room temperature with adhesive A containing 5 wt% ionic liquid, curing for more than one week, and then curing at 100°C for 12 hours. The temperature dependence curve for the former is 59 and that for the latter is 58, and both anodized coating products generated electricity, with the latter oxalic acid bath showing higher electricity despite the thicker coating.

[0071] Electrolytic oxidation films consisting only of a barrier film can be obtained by using weakly acidic to alkaline aqueous solutions such as those used in electrolytic capacitors, such as boric acid, ammonium borate, ammonium tartrate, and sodium borate, as electrolytes, but they do not become ferroelectric and do not generate electricity. The thickness of the barrier film in electrolytic oxidation films made from a direct current bath of a polybasic acid with strong acid groups is proportional to the electrolytic voltage, and the thickness decreases in the order of chromic acid > phosphoric acid > oxalic acid > sulfuric acid, with thinner being preferable. On the other hand, the density of pores formed in electrolytic oxidation films made from a direct current bath of a polybasic acid with strong acid groups is inversely proportional to the electrolytic voltage, and the pore walls become smaller and thicker in the order of sulfuric acid > phosphoric acid > oxalic acid, resulting in higher film density. Chromic acid produces a rough film with uneven pores.

[0072] From these trends, it is preferable to perform low-voltage electrolysis in an oxalic acid bath with a high film density in order to increase the internal current density caused by the electromotive force of the ferroelectricity and to thin the barrier film thickness that is not related to the appearance of ferroelectricity. The fact that it is preferable to form the film in an oxalic acid bath is consistent with the results of the commercially available product. FIG. 21 shows a test piece in which an anodic oxide film was formed on a PA2 substrate under the conditions shown in Table 4 using a direct current of 20 to 70 V electrolysis voltage under which pseudo-boehmite was formed by boiling, and AZ31 was directly contacted with the film, and the peak power density obtained from the IV data at 20°C is plotted. From this result, the maximum power was obtained from the oxide film electrolyzed at a relatively low voltage of 40 V in direct current.

[0073]

Table 4

[0074] On the other hand, when AC is used for electrolysis at a voltage of 30 V or more, like DC, a layered structure of many overlapping thin layers appears, which acts as a current barrier, and high current density cannot be expected. However, when electrolysis is performed at an effective voltage of 20 V or less, the layered structure does not appear, and the pores are shallow, small pores are formed, and the density is high. This is shown in the optical microscope photographs of the top surface of the film in Figures 22(A) and (B), and the transmission electron microscope photograph of the cross section of the film in Figure 8.

[0075] These photographs show electrolytic oxidation films formed on a PA2 substrate under the conditions shown in Table 2. Figure 22(A) and Figure 8 show the PA2 substrate, and Figure 22(B) shows the HPA substrate. Shallow pores of a few microns in size are formed randomly at low density, and no fine pores are seen inside the film between the pores, as seen with DC electrolysis. Furthermore, no pores are seen in HPA. For this reason, AC electrolysis at a low voltage is preferable to DC electrolysis.

[0076] FIG. 23 shows a composite coating of oxalic acid bath electrolytic oxidation film and pseudo-boehmite formed under the conditions shown in Tables 2 and 5 on a PA2 substrate, and a composite coating of sulfuric acid bath electrolytic oxidation film and pseudo-boehmite formed under the conditions shown in Tables 2 and 5. 1444 ][NTf 2 ]The test specimen was prepared by bonding AZ31 at room temperature under 1 MPa using adhesive A containing 5 wt% ionic liquid, curing for one week, and then curing at 100°C for 12 hours.

[0077] [Table 5]

[0078] In Figure 23, temperature dependency curve 52 is an AC electrolytic composite coating product using an oxalic acid bath, and temperature dependency curve 61 is a sulfuric acid bath, and they are compared with a commercially available oxalic acid bath composite coating product 56 (DC electrolytic product). From this result, in the electrolytic oxidation coating of oxalic acid baths, AC shows higher power. Also, similar to the tendency of the commercially available products, in the electrolytic oxidation composite coating of oxalic acid bath and sulfuric acid bath, the power obtained from the oxalic acid bath is higher. In other words, a composite coating electrolyzed by AC in an oxalic acid bath is particularly preferable.

[0079] In Figure 24, the test specimen is made by directly contacting AZ31 with an electrolytic oxidation composite coating formed on a PA2 substrate under the conditions in Table 6. However, the electrolysis effective voltage was 10V, 13V, 15V, 17V, 19V, 21V, and 25V. The IV data at 20°C was taken from this test specimen, and the peak power density was plotted to produce curve 62 in Figure 24. From this result, it is preferable that the electrolysis voltage by AC is a low voltage greater than 10V and less than 19V in effective value.

[0080] [Table 6]

[0081] FIG. 25 shows the electrolytic oxidation composite coating formed on the PA2 substrate under the conditions shown in Table 7. 1444 ][NTf 2 ] The test pieces were made by bonding AZ31 at room temperature at 1 MPa with adhesive A containing 5 wt% ionic liquid, aging for one week or more, and then curing for 12 hours at 100°C. Here, however, electrolysis was performed on electrolytic oxide films formed with two types of waveforms, a sine wave and a triangular wave, and the square wave was based on the previous example (embodiment of temperature dependency curve 52 in Figure 16).

[0082] [Table 7] TIFF2024162933000090.tif3196

[0083] In Figure 25, temperature dependency curve 63 is a sine wave, and temperature dependency curve 64 is a triangular wave. A comparison is also made with a commercially available oxalic acid bath composite coating product 56 (DC electrolysis product). As a result, although the AC waveforms have the same effective value and the obtained power differs depending on the waveform, all of them show larger values ​​than the DC electrolysis product, indicating that the AC product is superior. Among them, the square wave, which shows the maximum value in all temperature ranges, is particularly preferable.

[0084] In Fig. 26, the test piece is an electrolytic oxidation composite coating formed on a PA2 substrate under the conditions shown in Table 8, which is directly contacted with AZ31. In Table 7, the electrolysis time is changed according to the electrolysis frequency, and the amount of electrolysis power is adjusted so that it is the same based on the power value obtained during electrolysis, with the amount of electrolysis power at 50 Hz as the reference. However, for DC (0 Hz), the electrolysis voltage and the electrolysis voltage are set based on the previous example (the embodiment shown in Fig. 21).

[0085] [Table 8]

[0086] From the IV data obtained from such a test piece, data at 60°C, 80°C, and 100°C were extracted, and the peak power density was plotted in FIG. 26. Curves 65, 66, and 67 are for 100°C, 80°C, and 60°C, respectively. From FIG. 26 and Table 8, in the low frequency range of electrolysis frequencies of 20 Hz or less and in the high frequency range of frequencies higher than 100 Hz, the growth of the electrolytic oxide film is slow, long electrolysis times are required, and the obtained power is low. Therefore, a frequency of 40 to 100 Hz is preferable because it can obtain high power, and among these, a commercial frequency of 50 to 60 Hz is particularly preferable.

[0087] The bath temperature during electrolysis is preferably in the range in which a film grows most easily with direct current, even with alternating current. The acid concentration is preferably 3 to 5% for oxalic acid. If it is less than 1%, a high voltage is required to maintain the current density, and the available power also decreases. As for the electrolysis time, at an effective voltage of 20 V or less, an electrolytic oxide film formed in 30 minutes or less will not provide power. A film of 1 μm or more will be formed and power can be obtained by spontaneous polarization with an electrolysis time of 60 minutes or more, which is preferable.

[0088] The present invention An example of an amorphous ferroelectricElectrolytic oxidation film In forming an electrolytic oxidation film, it is necessary to remove the electrolyte from within the film. After the film is formed, the acid from the electrolytic bath and the acid radicals from the by-product remain inside the film. If these are not removed, even if an electric field is generated inside the film, a short circuit will occur and no electromotive force will be generated. A suitable method for removing this electrolyte is immersion in pure water to which ultrasonic waves are applied, or immersion in hot water where pure water is heated. Hot water treatment or steaming treatment, which involves exposure to pressurized steam, converts the material into an amorphous paraelectric material. The surface of the electrolytic oxide film is hydrated to form pseudo-boehmite, which functions as a catalyst. In particular, the hot water treatment is preferred because it can simultaneously remove the electrolyte. In addition, the steam treatment is less effective at removing the electrolyte, so it is preferred to remove the electrolyte in advance.

[0089] Commercially available anodized films produced in sulfuric acid baths or oxalic acid baths have their surface pores sealed with pseudo-boehmite formed by hot water treatment or steaming treatment to enhance corrosion resistance, but the purpose of the present invention is different. This is to form an amorphous paraelectric substance using the electrolytically oxidized film by the hot water treatment or steaming treatment. If this paraelectric substance is not formed, no electromotive force will be generated.

[0090] When the hot water treatment is performed, the treatment is preferably performed at 75 to 100°C at which pseudo-boehmite is formed under normal pressure, but it is also possible to perform treatment for a short time with hot water at a higher temperature under pressure. 6 It is preferable to use pure water or purified water with a resistance of Ωcm or more. The treatment time depends on the thickness of the electrolytic oxide film, but is about 5 to 30 minutes, and for a film with a thickness of about 1 to 3 μm, a few minutes to about 10 minutes will suffice.

[0091] In addition, in the steam treatment in which the film is exposed to pressurized steam, although the effect of removing the electrolyte inside the film is low, an amorphous paraelectric substance can be generated on the surface by utilizing the electrolytic oxidation film. Pseudo-boehmite begins to form under saturated steam with a gauge pressure of 2 atmospheres or more, and exposure to low-pressure heated steam of 5 atmospheres or less, where crystallinity does not increase, is preferable. In addition, like the hot water treatment, the treatment time depends on the film thickness, and is preferably about several minutes to 30 minutes.

[0092] In the configuration of the present invention, an important element when using an electrolytic oxidation film for an amorphous ferroelectric is a synthetic resin or electrolyte interposed between the amorphous paraelectric and the electrode. The importance of this is that it can nullify or slip through the electrical barrier that appears between the paraelectric and the electrode. A synthetic resin alone can nullify the barrier, but the electrical resistance is likely to be high. By adding an electrolyte such as an ionic liquid to the synthetic resin or by interposing the electrolyte itself, it is possible to slip through the electrical barrier. As a result, it becomes possible to arrange a work function material that promotes the energy band tilt in the composite film as an electrode. This can increase and stabilize polarization, leading to increased power generation.

[0093] Here, this synthetic resin is also an insulator, and it is preferable that the synthetic resin has a low volume resistivity that promotes charge transfer. 1444 [NTf2] The test pieces were bonded to AZ31 at room temperature at 1 MPa using various epoxy resin adhesives shown in Table 9 (values ​​published by the manufacturer are shown) containing 5 wt% ionic liquid, and then cured at 100°C for 12 hours after curing for more than one week.

[0094] [Table 9]

[0095] The curves in Fig. 27 are plots of the relationship between the volume resistivity at room temperature of adhesives A to F that do not contain ionic liquid, and the peak power density based on the IV data obtained from test pieces A to F to which ionic liquid was added. Here, curves 68, 69, and 70 are fittings of plots obtained by measurements at temperatures of 20°C, 60°C, and 100°C, respectively.

[0096] This result shows that the relationship between the peak power density of the test piece to which the ionic liquid was added and the volume resistivity at room temperature before the addition of the ionic liquid is no longer proportional. In other words, this shows that the effect of the ionic liquid differs depending on the resin components even within the epoxy resin. In particular, when the volume resistivity is 10 15 The values ​​in the Ωcm range clearly show low values ​​over the entire temperature range, indicating that the effect of the ionic liquid decreases when the volume resistivity increases to this level.

[0097] Synthetic resins are 10 8 Therefore, when no ionic liquid is added, the temperature dependence curve 46 in FIG. 8 Ωcm or more 10 12 It is preferable that the volume resistivity at room temperature is 10 Ωcm or less. When adding an ionic liquid, 8 Ωcm or more 10 14 The preferred synthetic resin is Ωcm or less. Suitable synthetic resins include epoxy resins and polyurethane resins, as well as polyamide resins, polyvinyl acetate resins, polyvinylphenol resins, polyacrylonitrile resins, cellulose acetate resins, cellulose propionate resins, and nitrocellulose resins.

[0098] In the present invention, bulk materials made of metals, semi-metals, semiconductors, alloys, eutectics, conductive compounds, etc. are bonded with synthetic resin or electrolyte-containing synthetic resin, or these substances may be applied as thin films or ultrafine particles with diameters of several nm to 100 nm by PVD methods such as vacuum deposition, sputtering, and ion plating on synthetic resin or electrolyte-containing synthetic resin. Also, thin films by PVD, CVD, or epitaxial methods may be deposited on conductive bulk materials, and then bonded with synthetic resin or electrolyte-containing synthetic resin. The thickness of the synthetic resin or electrolyte-containing synthetic resin is preferably about 1 to 4 μm. When synthetic resin or electrolyte-containing synthetic resin is used for bonding, the amount of resin is 3 to 5 g / m. 2 It is preferable to do so.

[0099] As shown in the above embodiments, adding an electrolyte to a synthetic resin can slip through the electrical barrier, increasing electrical conductivity and thus the amount of power that can be obtained. In particular, using an ionic liquid as the electrolyte is preferable because it eliminates the need for a solvent and prevents volatilization and leakage. An ionic liquid refers to an organic salt consisting of a cation and an anion that is liquid at room temperature.

[0100] Examples of the cationic species include a dialkylimidazolium ion, an alkylhydroxymethylimidazolium ion, a dialkylpyrrolidinium ion, a tetraalkylammonium ion, a diethyl(methoxyethyl)methylammonium ion, a choline ion, a methyltrihydroxymethylammonium ion, a dialkylpiperidinium ion, a tetraalkylphosphonium ion, and a trialkylsulfonium ion, which are stable and suitable.

[0101] In addition, examples of the anion species that are stable and suitable include a bis(trifluoromethanesulfonyl)imide ion, a bis(fluorosulfonyl)imide ion, a trifluoromethanesulfonate ion, a tetrafluoroborate ion, a hexafluorophosphate ion, a trifluoroacetate ion, a methoxyacetate ion, a dicyanoamide ion, a thiocyanate ion, and a dicyanamide ion.

[0102] The combination of a cation species having low Lewis acidity and an anion species having low Lewis basicity is preferable because it provides a compound having high ionicity, excellent heat resistance, low vapor pressure, high potential window, and excellent ionic conductivity.

[0103] In order to increase the electrical conductivity of the synthetic resin, it is preferable that the electrical conductivity of the ionic liquid is high, preferably 1 mS / cm or more. The potential window is preferably 2 V or more, since the electromotive force of the present invention reaches 1 V or more. In addition, the effect differs depending on the synthetic resin used, and high It is preferable to use a synthetic resin other than a volume resistivity resin, a silicone resin, an acrylic resin, or a cellulose resin, and more preferably a resin having no functional group that is involved in a reaction with the synthetic resin.

[0104] In epoxy resin, by adding 1 to 30% of an ionic liquid with an electrical conductivity of about 1 mS / cm, the power can be increased without significantly reducing the cohesive force of the resin. This is shown in Figure 28.

[0105] FIG. 28 shows the composite coating formed on the PA2 substrate under the conditions shown in Table 2. 1444 ][NTf 2 ]The test pieces were made by bonding AZ31 at room temperature under 1 MPa using adhesive A containing various amounts of ionic liquid added at 0 to 30 wt%, and then curing at 100°C for 12 hours after curing for more than one week.

[0106] Each curve in Figure 28 is a plot of the relationship between the peak power density obtained from the IV data and the power density versus temperature. Curve 71 is for bonding with adhesive A that does not contain ionic liquid, while curves 72, 73, 74, and 75 are for bonding with 1 wt%, 5 wt%, 10 wt%, and 30 wt% [N 1444 ][NTf 2 ] Ionic liquid was added to adhesive A to form the bond. As a result, an improvement in power was observed at about 1 wt% compared to adhesive A alone, and an addition of 5 wt% produced power equivalent to that of adding 30 wt%. Addition of more than 30 wt% is not expected to result in an increase in power unless the cohesive strength is sacrificed. For this reason, an addition of about 1 to 5 wt% is particularly preferable. 。

[0107] In the layered thermal element thus constructed, when an aluminum electrolytic oxide film is used for the amorphous ferroelectric of the present invention, a characteristic phenomenon appears. This will be explained with reference to the drawings.

[0108] <Features of the embodiment of the present invention in which an electrolytic oxidation film is used for the amorphous ferroelectric material> First, when aluminum containing Fe is used as the substrate for the electrolytic oxide film, if a paramagnetic material is used for the counter electrode, the substrate side becomes the anode and the counter electrode side becomes the cathode, and high power can be obtained by placing a material with a lower work function than aluminum on the counter electrode. Also, if a ferromagnetic or diamagnetic material is used for the counter electrode, the polarity is basically reversed and high power cannot be obtained. This is shown in Figure 29.

[0109] FIG. 29 shows the composite coating formed on the PA2 substrate under the conditions shown in Table 2. 1444 ][NTf 2 ]The metals, metalloids, semiconductors and alloys in Table 10 were bonded at room temperature at 1 MPa using adhesive A containing 5 wt% ionic liquid, and after curing for more than one week, cured at 100°C for 12 hours to prepare the test pieces. Here, single crystal p-type Si was used, expanded graphite HT-715 (manufactured by eGRAF) and isotropic graphite were used for the graphite, cast products were used for Bi, Sb and Se, and rolled products were used for the others.

[0110] The dashed and dotted line 76 in Figure 29 is a fitting of the 60°C data extracted from the IV data when a paramagnetic material in Table 10 is used as the counter electrode, and the peak power density plotted as white circles. High power can be obtained by using a material with a lower work function than aluminum as the counter electrode. The dashed line 77 is a straight line approximation of the 60°C data extracted from the IV data when a diamagnetic material in Table 10 is used as the counter electrode, and the peak power density plotted as black circles.

[0111] Reference numbers 77 and 78 are graphite poles, the former being unpressurized expanded graphite, and the latter being pressurized isotropic graphite. Among diamagnetic materials, graphite has a high absolute value of magnetic susceptibility, far exceeding that of Bi, especially in the direction parallel to the crystal axis. For this reason, isotropic graphite, whose crystals are oriented by pressure, can generate more power than unpressurized expanded graphite. Cast products Bi (reference number 80) and Sb (reference number 81) do not have oriented crystal grains, so not only do they not generate large values, but in the case of Sb, the polarity does not even reverse.

[0112] Other diamagnetic materials are rolled, but the rolling method can be cold rolling or hot rolling, and the orientation of the crystal grains changes depending on whether annealing is performed or not. In and Sn, which have low melting points, recrystallize during the curing of the test piece or during the data creation cycle, causing the orientation to become distorted. Due to these reasons, diamagnetic materials that do not reverse polarity, like Sb, also appear. On the other hand, the triangles in the figure show ferromagnetic materials as the counter pole. The peak power density is shown by extracting data at 60°C from the IV data. Reference number 82 shows Gd, and reference number 83 shows Ni. Gd has a Curie point near 18°C, and at 60°C it becomes a paramagnetic material and does not reverse polarity. However, even when it becomes a paramagnetic material, its magnetic susceptibility is large and it does not show a large power.

[0113] In this way, a stable and high power can be obtained by placing a paramagnetic material with a low work function on the counter electrode. Paramagnetic materials with a low work function include metals such as Ca, Mg, Li, La, Ce, Pr, Nd, Eu, Sm, Yb, Lu, and Th, eutectics and intermetallic compounds mainly made of these elements, alloys such as magnesium aluminum zinc alloy, magnesium lithium zinc alloy, magnesium aluminum calcium alloy, magnesium lithium alloy, aluminum lithium alloy, and aluminum calcium alloy, 12CaO 7Al 2 O 3 Preferred examples of the compound include the above-mentioned electride compounds.

[0114] Among these, the work functions other than LZ91, AZ31, and p-type Si are cited from "Dictionary of Physical Data" edited by the Physical Society of Japan, p321 (2006), and the work function of p-type Si is cited from "Electrostatics Handbook" edited by the Electrostatics Society of Japan, p1239 (1998). For LZ91 and Z31, data obtained by measurement with an ultraviolet photoelectron spectrometer Versa Probe (manufactured by ULVAC-PHI, Inc.) are used.

[0115] [Table 10]

[0116] Second, as the purity of the base material increases, the power obtained tends to decrease, and when a high-purity base material is used, the polarity is reversed. When a high-purity base material is used, the power is proportional to the work function of the counter electrode, contrary to the case of using a base material containing an Fe component. This is shown in Fig. 30.

[0117] Fig. 30 shows composite film products formed from HPA, PA1, PA2, and PA3 base materials under the conditions shown in Table 2 using [N 1444 [NTf 2 ionic liquid added at 5 wt% as an adhesive A as the counter electrode material and bonded to the diamagnetic and paramagnetic materials in Table 11 at 1 MPa at room temperature, cured at 100 °C for 12 hours after curing for one week or more, and used as test pieces. For Al, the same type of aluminum as the base material is used.

[0118] [Table 11]

[0119] The four groups enclosed by the broken line in Fig. 30 are: the group with code 84 uses AZ31 alloy as the counter electrode, the group with code 85 uses isotropic graphite as the counter electrode, the group with code 86 uses the same aluminum as the base material, and the group with code 87 uses Sn as the counter electrode. Each group is composed of four types of plots using composite films made from HPA (squares), PA1 (triangles), PA2 (black circles), and PA3 (white circles) base materials.

[0120] As shown by the group with code 84, in the order of HPA < PA1 < PA2 < PA3, that is, the power increases inversely proportional to the base material purity. Focusing on HPA plotted as squares among the four groups, it has a power near 0 or with reversed polarity in any group. However, in all four types of composite films, the one that shows inversion is the group of isotropic graphite of the diamagnetic material, and a synergistic effect can be obtained by combining it with materials that originally have reversed polarity, such as diamagnetic or ferromagnetic materials.

[0121] In the case of Sn, which has a low melting point and crystal orientation disorder occurs during curing, even if it is a diamagnetic material, there is no reversal in all four types of composite films, but since the composite film made from HPA does not contain Fe components, it does not interact with the magnetism of the counter electrode, and the power increases in proportion to the work function except for the group of isotropic graphite that interacts. Therefore, it is preferable to use materials such as Be, n-type Si, Co, Ni, Ru, Rh, Te, Re, Os, Ir, Pt, Au, Se, etc., which have a work function higher than C, or alloys, eutectics, and intermetallic compounds with high work functions centered on these elements, for the counter electrode. EXAMPLES

[0122] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. EXAMPLES

[0123] <Preparation of aluminum substrate> A PA2 base plate (0.3 mm thick) is prepared, and a square plate measuring 50 (W) x 60 (L) mm is cut out from it. It is then soaked in acetone for 1 minute to degrease, and one side is coated with acrylic paint, which is then dried and baked at 120°C for 30 minutes and then at 140°C for 5 minutes. This is then soaked in a mixed aqueous solution of 2.3 wt% sodium hydroxide and 1.5 wt% potassium hydroxide for 5 minutes, washed with tap water, and the aluminum surface is lightly rubbed with a cloth to remove the oxide film. It is then soaked in pure water, stirred and washed, and the water on the surface is wiped off with a cloth to obtain the substrate.

[0124] <Creation of amorphous ferroelectric and amorphous paraelectric materials on a substrate> A 3 wt% oxalic acid solution was prepared from 30 g of commercially available anhydrous oxalic acid and 970 g of pure water, and placed in a square glass electrolytic cell (120 x 120 x 150 mm) 1 shown in Figure 1 and kept at 30°C using a cool stirrer 5. A 40 (W) x 100 (L) mm pure aluminum alloy tube was attached to the central anode copper pipe. A 28 (W) x 100 (L) mm pure aluminum plate is suspended by copper wire from the cathode side copper pipes on both sides of the aluminum plate, and a direct current of 30 V is applied from power source 6 for 90 minutes to dissolve aluminum ions in the aqueous solution.

[0125] The aluminum plate is removed from the solution, and the aluminum substrate prepared on the anode side is suspended so that it is immersed about 35 mm into the solution, and a carbon plate of 84 (W) x 120 (L) is suspended on the cathode side. In this state, the solution is stirred with a stirrer 4 while maintaining the temperature at 30°C, and a square wave AC voltage of 15 V effective voltage is applied from a power source 6 for 90 minutes to form an amorphous ferroelectric electrolytic oxide film on the surface of the substrate.

[0126] After the electrolytic oxidation treatment, the sample washed with pure water is immersed in boiling hot water of 500 cc for 10 minutes to form pseudo-boehmite of amorphous dielectric on the surface of the electrolytic oxidation film. After the hot water immersion, it is washed with tap water and dried at 60 °C for 1 hour.

[0127] <Fabrication of Composite Film Forming Substrate Chip and Counter Electrode Chip> Remove the coating film on the back surface of the substrate dried after the hot water treatment with acetone and extract a small piece (17 (W) × 30 (L) mm). On the other hand, for the counter electrode, a small piece (15 (W) × 28 (L) mm) is extracted from magnesium-lithium-zinc alloy LZ91 with a thickness of 0.2 mm. Both sides are polished on a stone surface plate with #1000 emery paper, and only the surface to be overlapped with the substrate small piece is further polished with #8000 film and then polished with a cloth.

[0128] <Mixing and Bonding of Resin> [N 1444 [NTf 2 Weigh about 15 mg of the ionic liquid, and weigh the main agent and curing agent of adhesive A in an amount 10 times that of the ionic liquid respectively and mix them to obtain an adhesive containing about 5 wt% of the ionic liquid. Apply the mixed adhesive to the polished surface of the counter electrode chip and bond it to the film surface of the substrate chip. This is sandwiched between a reinforced polyethylene film and inserted between the surface plates of a press machine whose pressing force can be controlled by a load cell, and left at room temperature for 1 hour with a load of 410 N for bonding. After bonding, remove the adhesive protruding from the counter electrode with acetone and cure it at room temperature for 7 days to obtain a test piece.

[0129] <Curing of Test Piece> The test piece is sandwiched between the electrode 14 and the heat insulating material 15 as shown in Figure 4, inserted between the heaters 21 with thermocouples of the precision vice 17, and the side surface of the test piece is further surrounded by a heat insulating material. Then, the entire precision vice 17 is placed in a low-temperature thermostat, and the power cord 22 and thermocouple 23 of the heater 21 are connected to a temperature controller. To complete the curing of the adhesive of the test piece, in this state, the temperature of the heater 21 is raised to 100 °C and cured for 12 hours.

[0130] <Obtaining I-V Data> First, cool the test piece in the low-temperature thermostat to -11 °C and control it to -10 °C with the heater 21. In this state, measure the current flowing through the test piece while gradually decreasing the applied voltage to -0.001 V, -0.01 V to 0.07 V (at 0.02 V intervals), -0.1 V to -0.8 (at 0.05 V intervals), -0.9 to -5 V (at 0.1 V intervals) with an electrometer with the aluminum substrate on the anode side and the counter electrode on the cathode side, and obtain I-V data.

[0131] At this time, the same measurement is repeated 12 or 6 times at each applied voltage with a measurement interval of 3.5 seconds, and the latter half of the data is used. After taking the IV data at -10°C, the temperature is immediately raised, the temperature inside the low-temperature incubator is set to 16°C, the heater 21 is set to 20°C, and after about 30 minutes, IV data is obtained in the same way as at -10°C. The same procedure is repeated at 40°C, 60°C, 80°C, and 100°C. However, the applied voltage interval settings are different at each temperature.

[0132] The IV product is calculated from the obtained IV data, a PV diagram is drawn, and the peak power is calculated from it. Since the adhesive surface is the surface through which current passes, the peak power density is calculated by dividing the peak power by the area of ​​the opposing electrode. This cycle of -10 to 100°C is repeated five times, and the final data is the average of the four data sets excluding the first data.

[0133] <Data evaluation> The final data obtained is shown in Table 12. Nanowatt-level power density was obtained even at around 20°C, and increased exponentially with increasing temperature, reaching a level more than 70 times higher at 100°C. Here, it was demonstrated that power can be obtained in a low-temperature environment of 100°C or less, even though there is no temperature difference between the substrate side and the counter electrode side of the test piece.

[0134] [Table 12]

[0135] Comparative Example 1 A test piece without the electrolytic oxidation treatment and pseudo-boehmite layer of Example 1 was prepared. First, a small piece of 17 (W) x 30 (L) mm was cut out from the same pure aluminum base plate as in Example 1 and degreased by immersing in acetone for 1 minute. A small counter electrode piece was prepared in the same manner as in Example 1. The mixed adhesive used, the bonding method, and the curing were similar to those in Example 1, and a test piece in which an aluminum base material without an electrolytic oxidation film and a counter electrode were bonded was obtained.

[0136] <Evaluation of comparison test pieces> After curing, the test piece was cured, but no electromotive force was detected on the electrometer even at 100℃, and we gave up on obtaining IV data. In other words, it can be concluded that no electric power can be obtained from this comparative test piece. EXAMPLES

[0137] Here, magnesium aluminum zinc alloy AZ31 (0.2 mm thick) was used as the counter electrode of Example 1, and two test pieces were connected in series for measurement. The test piece preparation method was the same as in Example 1. The test pieces were stacked in series in two pieces and cured at 100°C for 12 hours. The procedures for obtaining IV data and calculating the peak power density were also similar to those in Example 1.

[0138] <Data evaluation> The obtained data is shown in Table 13. The embodiment of the temperature dependency curve 52 in FIG. 16 is data obtained using the same test piece alone, but the peak power density is almost the same, and it is found that the series connection provides twice the power. In addition, the possibility of series connection suggests the advantage of being able to easily obtain a high voltage.

[0139] [Table 13] TIFF2024162933000097.tif40126 EXAMPLES

[0140] Here, the alloy AZ31 (0.2 mm thick) was used as the counter electrode as in Example 2, and two test pieces were placed in parallel for measurement. The procedure for preparing the test pieces was the same as in Example 1. The test pieces were cured by placing the aluminum substrates of the two test pieces together, placing aluminum plates on both sides and in the middle of the test pieces between heaters, and performing the curing at 100°C for 12 hours. The electrode in the middle of the two test pieces was used as the anode, and the electrodes on both ends were used as the cathode for measurement, and the procedure for obtaining IV data and calculating the peak power density was also similar to Example 1.

[0141] [Table 14]

[0142] <Data evaluation> The obtained data is shown in Table 14. As in Example 2, when comparing with the data of the temperature dependency curve 52 in FIG. 16 obtained by using a single test piece, the peak power density is almost the same, and it was found that the power obtained by parallel connection is twice as much as that obtained by serial connection. In addition, the fact that parallel connection is possible suggests that high output is possible over a large area. EXAMPLES

[0143] A test piece was prepared in the same manner as in Example 1, using PA3 (0.5 mm thick) as the aluminum substrate and AZ31 (0.2 mm thick) as the counter electrode. As in Example 1, the test piece was clamped and fixed between two heaters 21 using a precision vice 17, and placed in a low-temperature incubator SB01 (manufactured by ETAC). A simplified version of this is shown in the area enclosed by the dashed line in FIG. 42. In the figure, 115 indicates the low-temperature incubator, and 114 indicates the test piece. This was connected in parallel with a 1000 μF electrolytic capacitor 111, an electrometer 8252 (manufactured by ADC) as a voltage measuring device 113, and a switch 112 as shown in FIG. 42. At this time, the switch 112 is open.

[0144] In this state, the low-temperature incubator 115 was kept at 21° C., and the heater was controlled to 25° C. with a temperature controller Model 335 (manufactured by Lake Shore) to keep both sides of the test piece 114 at 25.0±0.1° C. In this state, the switch 112 was closed and left for 30 minutes to completely discharge the electric charges in the electrolytic capacitor 111 and the test piece 114. At the same time that the switch 112 was opened, the voltage between the terminals of the electrolytic capacitor 111 and the test piece 114 was measured by the voltage measuring device 113 every minute for 24 hours.

[0145] <Data evaluation> Curve 118 in the graph of Figure 43 is the measurement result. At a temperature of 25°C, which is approximately room temperature, the voltage begins to rise immediately after the start of measurement. Since the charge in the circuit of Figure 42 has been pre-discharged, no charge exists in electrolytic capacitor 120 or test piece 123 at the start of measurement. It shows that charge gradually accumulates in the electrolytic capacitor and test piece from there. Since electrolytic capacitors do not have the ability to generate electricity, this suggests that the test piece has that ability.

[0146] Therefore, we decided to add the equivalent circuit of Figure 44 to the circuit of Figure 42 and consider it by simulation. In the electrolytic capacitor part, the capacitance 120, the insulation resistance 119, and the equivalent series resistance 121 are applied, and C C (C)、r C (Ω), R C In the test piece, there are a capacitance 123, an insulation resistance 125, an equivalent series resistance 122, and a DC power supply 124 in series with the insulation resistance. E (C)、r E (Ω), R E (Ω), E(V). The voltage V(V) between points 126 and 127 of the equivalent circuit consisting of these can be calculated from the circuit equation as follows: where t (seconds) is the elapsed time.

[0147]

number

[0148]

number

[0149] Here, the insulation resistance r of the electrolytic capacitor C was obtained from the circuit shown in Figure 45. The electrolytic capacitor is set to 128, and the shunt resistance R DC Known resistance 130 (Ω) and voltage EDC A DC power supply 129 (DC voltage current power supply 6156 (manufactured by ADC)) that supplies (V) is connected in series, and the voltage V across the known resistor 130 is DC When (V) is measured using an Electrometer 8252 (made by ADC), it can be calculated using the following formula.

[0150]

number

[0151] In addition, the equivalent series resistance R C and R E The impedance Z and reactance X at 100 Hz were measured using an impedance analyzer IM3570 (manufactured by HIOKI) and calculated using the following formula.

[0152]

number

[0153] Furthermore, the capacitance at 100 Hz was measured using an impedance analyzer. The electrolytic capacitor was measured with the same polarity as the analyzer, while the test piece had an electromotive force, so the polarity was reversed and a DC current of 1 V was applied in reverse to measure. E = 82.7 (kΩ), R C = 0.145 (Ω), r C =10.0(MΩ), C C = 937 (μF), C E = 22.7 (nF). However, the capacitance of the test piece is the combined capacitance of a ferroelectric and a paraelectric connected in series, and the value is closer to the dielectric with the smaller capacitance. Also, the insulation resistance of the test piece r E is proportional to the reciprocal of the voltage across the electrolytic capacitor in this circuit, and does not show a constant value. E and r E was used as a parameter.

[0154] The electromotive force of the test piece is E = 1.3 (V), and the parameter C E and r E was selected and fitted to the curve 118 in FIG. E =-939.5(μF), r E The graph for r = 15 (MΩ) is curve 117. E Since does not have a constant value, we tried to make the curve approximate the curve 118. E = 22.7 (nF), and the other conditions were the same, and the graph 116 was simulated, which did not fit the curve 118 and was different. The result was that the electromotive force V int The capacitance of a capacitor is determined by the external applied voltage V ext Using the definition of capacitance by Q, it can be expressed as the following equation, and we have proven through the examples that it has a negative value. Here, Q is the charge stored inside the capacitor.

[0155]

number

[0156] Furthermore, the absolute value of the capacitance of the test piece depends on the capacitance of the capacitor to which it is connected, and is a value that is close to the capacitance of the capacitor.

[0157] Comparative Example 2 In accordance with the test piece described in Example 4, PA3 (0.5 mm thick) was used as the aluminum substrate, and after alkaline cleaning, an electrolytic oxidation film was formed in a 3 wt% aqueous solution of oxalic acid. After that, without boiling, it was immersed in pure water for 20 days and then placed in a desiccator filled with silica gel indoors for 5 days to dry. From this point, AZ31 (0.2 mm thick) was bonded to the electrolytic oxidation film surface using an epoxy resin containing ionic liquid in the same manner as in Example 4. After curing at room temperature for 7 days, it was fixed together with a heater in a precision vice and cured at 100°C for 12 hours to obtain a test piece for comparative example.

[0158] <Evaluation of comparison test pieces> When this test piece was short-circuited for 1 minute and connected to an electrometer, no electromotive force was obtained, and we gave up on obtaining data by a connection test with the same electrolytic capacitor as in Example 4. This suggests that it is difficult to generate an electromotive force unless an amorphous paraelectric material is placed on the surface of the amorphous ferroelectric material.

[0159] From Example 1 and Comparative Example 1 and Example 4 and Comparative Example 2, it can be seen that unless a film formed by electrolytic oxidation treatment and hot water treatment of aluminum, in other words a composite film consisting of an amorphous ferroelectric and an amorphous paraelectric, is used, power cannot be obtained at low temperatures without temperature difference. Furthermore, the fact that lamination is possible as in Examples 2 and 3 means that power per unit volume is effective as a measure, rather than power per area, as in the case of Seebeck elements and solar cells. That is, in Example 1 and the like, the aluminum substrate and counter electrode material can be constructed of foil or thin film, and therefore, from the possible minimum thickness, the power density in Table 12 is 3 to 220 μW / cm at 20 to 100°C. 3 This can be converted into performance.

[0160] This lamination broadens the scope of use of the present invention, and it can play a part in the utilization of renewable energy, from micro-power generation such as IOT power sources and wearable power generation to large-scale power generation such as thermal storage power generation. In addition, it is clear from Example 4 that the generated electrical energy can be stored in a capacitor, and the storage means is also inexpensive.

[0161] Furthermore, it was revealed that the material constructed according to the present invention has negative capacitance, which has various possibilities, such as canceling parasitic capacitance in various electric circuits, signal amplification, energy saving in electric and electronic components such as lowering the voltage of FETs and memory elements, and controlling the transfer of heat (thermal conductivity) that accompanies the transfer of internal charges by turning the switch connecting the plates on and off. [Industrial Applicability]

[0162] According to the present invention, it is possible to provide a layered thermal element that can be stacked and generates power by exhibiting negative capacitance in a temperature range of 100 to -10°C even without a temperature difference. In addition, by using such a layered thermal element, it is possible to provide various power generation methods, energy saving methods for electronic circuits, and heat control methods in a temperature range of 100°C to -10°C. [Explanation of symbols]

[0163] 1...glass container, 2...styrofoam, 3...electrolyte, 4...stirring bar, 5...cool stirrer, 6...programmable AC / DC power supply, 7...graphite plate, 8...aluminum substrate, 9...counter electrode, 10...synthetic resin, 11...substrate, 12...composite coating, 13...test piece, 14aluminum electrode, 15polypropylene foam insulation, 16...combined test piece, 17...precision vice, 18...tightening bolt, 19...calcium silicate plate, 20...alumina plate, 21...heater with thermocouple, 22...heater cord, 23...thermocouple compensation cord, 24...IV data, 25...intersection, 26...I V data converted power data, 27...power peak point, 28...peak power density temperature dependency curve, 29...electrolytic oxide film cross section, 30carbon-deposited electrolytic oxide film cross section, 31...aluminum substrate cross section, 32...Al secondary ion intensity curve, 33...O secondary ion intensity curve, 34...Fe concentration curve, 35...electrolytic oxide film / substrate interface position, 36...electrolytic oxide film region, 37...substrate region, 38-42...(not used), 43, 46, 49, 52, 55, 58, 59, 61, 63, 64, 71-75...peak power density temperature dependency curve, 44, 47, 50, 53...IV data, 45, 48, 51, 54...Intersection (electromotive force point), 56, 57...Electromotive force temperature dependence curve, 60, 62...Peak power density electrolytic voltage dependence curve, 65-67...Peak power density frequency dependence curve, 68-70...Peak power density volume resistivity dependence curve, 76...Paramagnetic fitting curve, 77...Diamagnetic approximation line, 78...Data when expanded graphite is used, 79...Data when isotropic graphite is used, 80...Data when Bi is used, 81...Data when Sb is used, 82...Data when Gd is used, 83...Data when Ni is used, 84...Group using AZ31 alloy as counter electrode , 85...Group using isotropic graphite as the counter electrode, 86...Group using the same type of Al as the substrate as the counter electrode, 87...Group using Sn as the counter electrode, 88...Data using PA3 substrate, 89...Data using PA2 substrate, 90...Data when PA1 substrate was used, 91...Data when HPA substrate was used, 92...Curve fitting the relationship between the power density and the impurity concentration of the substrate obtained by combining AZ31 alloy with a composite coating consisting of an electrolytic oxidation film and a pseudo-boehmite layer made of various substrates, 93...Curve fitting the relationship between the impurity concentration of the substrate and the Fe concentration therein,94... Curve obtained by fitting the relationship between the impurity concentration of the substrate and the Si concentration therein, 95... Curve obtained by fitting the relationship between the impurity concentration of the substrate and the Cu concentration therein, 96... Curve obtained by fitting the relationship between the impurity concentration of the substrate and the Mn concentration therein, 97... Curve obtained by fitting the relationship between the impurity concentration of the substrate and the Zn concentration therein, 98... Measurement sample, 99... Reference capacitor, 100... Compensation resistor, 101... Oscilloscope, 102... AC power source, 103 to 105... Hysteresis curve, 106... Composite consisting of an electrolytic oxidation film containing an Fe component and a pseudo-boehmite layer 107...Temperature dependence curve of electromotive force obtained by combining Gd on the surface of a composite film consisting of an electrolytic oxidation film containing an Fe component and a pseudo-boehmite layer, 108...Temperature dependence curve of electromotive force obtained by combining Ni on the surface of a composite film consisting of an electrolytic oxidation film containing an Fe component and a pseudo-boehmite layer, 109...Temperature dependence curve of electromotive force obtained by combining expanded graphite on the surface of a composite film consisting of an electrolytic oxidation film containing an Fe component and a pseudo-boehmite layer, 110...Curie point of Gd, 111...electrolytic capacitor, 112...switch, 113...voltmeter, 114...test piece, 115...low-temperature incubator, 116...simulation line when applying the measured value of the impedance analyzer to the capacitance of the test piece, 117...simulation curve when applying a negative value to the capacitance of the test piece, 118...time change curve of the voltage at both ends when a test piece and an electrolytic capacitor at 25°C are connected in parallel, 119...insulation resistance in the equivalent circuit of the electrolytic capacitor, 120...capacitance in the equivalent circuit of the electrolytic capacitor, 121...series equivalent resistance in the equivalent circuit of the electrolytic capacitor, 122...series equivalent resistance in the equivalent circuit of the test piece, 123...capacitance in the equivalent circuit of the test piece, 124...DC power supply in the equivalent circuit of the test piece, 125...insulation resistance in the equivalent circuit of the test piece, 126...positive terminal in the equivalent circuit, 127 negative terminal in the equivalent circuit, 128...electrolytic capacitor, 129...DC power supply, 130...shunt resistor, 131...voltmeter

Claims

1. A layered thermal element in which an electrolytic oxidation film is formed from pure aluminum or an aluminum alloy with an aluminum purity of 96% or more but less than 99.85% in a polybasic acid bath in which the pKa value of at least one of the acid groups is less than 2.5, and the electrolytic oxidation film is then subjected to hot water treatment or steam treatment using heated steam, and a metal consisting of typical elements and having a work function equal to or lower than the work function of aluminum, or an alloy or conductive inorganic compound consisting mainly of typical elements and having a work function equal to or lower than the work function of aluminum, is disposed on the surface of the film via a synthetic resin layer.

2. A layered thermal element in which an electrolytic oxidation film is formed on high-purity aluminum in a polybasic acid bath, at least one of whose acid groups has a pKa value of less than 2.5, and then the film is subjected to hot water treatment or steam treatment using heated steam, and graphite carbon is placed on the film surface via a synthetic resin layer.

3. 3. The layered thermal element of claim 1, wherein the polybasic acid having at least one acid group with a pKa value of less than 2.5 is oxalic acid.

4. 3. The layered thermal element according to claim 1, wherein the electrolytic oxidation film is formed by an AC wave having an effective electrolytic voltage value of more than 10 V and less than 20 V.

5. The synthetic resin layer has a volume resistivity of 10 8 Ωcm or more 10 12 Synthetic resin with a volume resistivity of 10 Ωcm or less at room temperature 8 Ωcm or more 10 14 3. The layered thermal element according to claim 1, which is obtained by adding 1% to 5% of an ionic liquid to a synthetic resin having a resistance of Ωcm or less.

6. 3. The layered thermal element of claims 1 and 2, wherein the pure aluminum or aluminum alloy, or high purity aluminum is made of a plate or foil material, and an electrolytic oxide film is formed on one or both sides of the plate or foil.

7. 3. The layered thermal element according to claim 1, wherein the hot water treatment or the steam treatment with heated steam is performed by immersion in hot water of 90° C. or higher, or exposure to heated steam at a pressure of 2 to 5 atmospheres.

7. 2. The layered thermal element of claim 1, wherein the metal having a work function equal to or lower than that of aluminum and made of a typical element is magnesium.

8. 2. The layered thermal element of claim 1, wherein the alloy mainly composed of a typical element and having a work function equal to or lower than that of aluminum is at least one of a magnesium aluminum zinc alloy, a magnesium lithium zinc alloy, a magnesium aluminum calcium alloy, a magnesium lithium alloy, an aluminum lithium alloy, and an aluminum calcium alloy.

9. A conductive inorganic compound that is mainly composed of typical elements and has a work function equal to or less than that of aluminum is 12CaO.7Al. 2 O 3 2. The layered thermal element of claim 1, which is an electride of

10. 3. The layered thermal element of claim 2, wherein the graphitic carbon is at least one of isotropic graphite and graphite.

Citation Information

Patent Citations

  • FeRAM WITH LAMINATE-TYPE FERROELECTRIC FILM AND METHOD FOR FORMING THE SAME

    JP2022022192A

  • Apparatus and method for ferroelectric conversion of heat to electrical energy

    US20100289377A1

  • Negative-capacitance and ferroelectric field-effect transistor (ncfet and fe-FET) devices

    US20210296469A1

  • Primary source of electrical energy using a mixture of fuel and oxidizer

    US4863813A

  • Method for forming amorphous ferroelectric materials

    US5342648A