Conductive paste composition
A conductive paste composition with high epoxy equivalent epoxy resin and phenolic ester curing agent addresses the challenge of achieving both thermal shock and moist heat resistance, ensuring reliable electrical performance.
Patent Information
- Application Number
- JP2023079413
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-12
AI Technical Summary
Conductive paste compositions containing epoxy resins face challenges in achieving both thermal shock resistance and moist heat resistance, with existing formulations often compromising one property to enhance the other.
A conductive paste composition comprising a conductive powder and a resin component, where the epoxy resin has an epoxy equivalent of 500 g/eq or more, and a curing agent represented by a phenolic ester compound, enhances both thermal shock resistance and moist heat resistance.
The composition achieves good thermal shock resistance and moist heat resistance while maintaining excellent electrical properties, ensuring reliability in electronic components.
Smart Images

Figure 2024163635000013 
Figure 2024163635000014 
Figure 2024163635000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting conductive paste composition, and in particular to a conductive paste composition that can be suitably used in the field of electronic components. [Background technology]
[0002] In the field of electronic components, a technique using a conductive paste composition has been widely used as one of the methods for forming an electrical connection. Various types of such conductive paste compositions are known, and an example of a thermosetting conductive paste composition is a composition in which a conductive powder and an epoxy resin as a resin component are blended.
[0003] Epoxy resins have advantages such as good adhesion to metals constituting electronic components, good heat resistance, and relatively small volumetric shrinkage upon curing, etc. Therefore, epoxy resins are widely used as the resin component of conductive paste compositions.
[0004] In recent years, electronic components are increasingly required to be smaller, lighter, more precise, and more reliable. Therefore, various studies have been conducted on conductive paste compositions to meet the requirements of such electronic components. For example, Patent Document 1 discloses a conductive adhesive that uses a liquid epoxy resin and a solid epoxy resin in combination to achieve both stress relaxation and heat resistance when mounting chip components on a substrate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-277384 A Summary of the Invention [Problem to be solved by the invention]
[0006] Here, a conductive paste composition containing an epoxy resin as a resin component is required to have both thermal shock resistance and moist heat resistance after curing. However, when the resin component is an epoxy resin, the moist heat resistance tends to decrease when an attempt is made to improve the thermal shock resistance.
[0007] In recent years, as described above, higher requirements are being placed on electronic components, and therefore the conductive paste composition is required to have a stronger balance between thermal shock resistance and moist heat resistance. However, no conductive paste composition containing an epoxy resin has been known that can balance these properties better. For example, the conductive adhesive described in Patent Document 1 aims to balance stress relaxation properties and heat resistance as described above, but no consideration has been given to thermal shock resistance or moist heat resistance.
[0008] The present invention has been made to solve such problems, and has an object to provide a conductive paste composition containing an epoxy resin as a resin component, which is capable of realizing good thermal shock resistance and good moist heat resistance after curing. [Means for solving the problem]
[0009] In order to solve the above-mentioned problems, the conductive paste composition according to the present disclosure contains (A) a conductive powder and a resin component, the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator, the (B) epoxy resin contains at least one epoxy resin having an epoxy equivalent of 500 g / eq or more, and the (C) curing agent is a compound represented by the following general formula (1):
[0010] [ka]
[0011] (In the formula (1), R is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom; X in the formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2); A in the formula (2) is an alkyl group having 1 to 6 carbon atoms;
[0012] [ka] Z in formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms, m in formula (1) is an integer of 0 to 4, n in formula (1) is a number of 0 to 2 on average, R, X, Z, and A contained in formula (1) may be the same substituent or atom or different substituents or atoms, and m in formula (1) may be the same integer or different integers.) The compound is a phenol ester compound having a structure represented by the following formula:
[0013] According to the above-mentioned configuration, the epoxy resin (B) contained as the resin component has at least one epoxy equivalent of 500 g / eq or more, and the phenol ester compound of the general formula (1) is used as the curing agent (C). This allows the cured product of the obtained conductive paste composition to have good thermal shock resistance and good moist heat resistance while maintaining good electrical properties. Therefore, it is possible to obtain a conductive paste composition containing an epoxy resin as a resin component, which can achieve good thermal shock resistance and good moist heat resistance after curing.
[0014] In the conductive paste composition having the above-mentioned configuration, the (B) epoxy resin may contain 30 mass % or more of an epoxy resin having an epoxy equivalent of 500 g / eq or more.
[0015] In the conductive paste composition having the above-mentioned configuration, the (C) curing agent may have an esterification rate of 70% or more.
[0016] In the conductive paste composition having the above-mentioned configuration, the (C) curing agent may be blended in an amount within a range of 3 to 150 parts by mass with respect to 100 parts by mass of the (B) epoxy resin.
[0017] In addition, in the conductive paste composition having the above-mentioned configuration, the (A) conductive powder may be at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder.
[0018] The conductive paste composition having the above-mentioned structure may be used by being applied onto a substrate using a printer, a dispenser, or by dipping.
[0019] The conductive paste composition having the above-mentioned configuration may be used by being applied to electrodes of electronic components. Effect of the Invention
[0020] The present invention has the above-mentioned configuration, and thus has an effect of providing a conductive paste composition containing an epoxy resin as a resin component, which can achieve good thermal shock resistance and good moist heat resistance after curing. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a plan view showing the shape of a conductive pattern for evaluating the conductor resistance of a conductive pattern (cured product) obtained by curing a conductive paste composition according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a model diagram showing a schematic configuration of an evaluation sample used for evaluating the connection resistance and adhesive strength after curing of a conductive paste composition in the examples and the like of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Representative embodiments of the present disclosure will be described below. The conductive paste composition according to the present disclosure contains (A) a conductive powder and a resin component, and the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator. The epoxy resin (B) contains at least one type of epoxy resin having an epoxy equivalent of 500 g / eq or more. Furthermore, the curing agent (C) is a compound having a structure represented by the general formula (1) described below, that is, a compound obtained by esterifying a phenolic hydroxyl group of a polyhydric phenol compound. In the present disclosure, this compound is referred to as a phenol ester compound.
[0023] [(A) Conductive powder] The specific constitution of the conductive powder (A) contained in the conductive paste composition according to the present disclosure is not particularly limited, and a conductive powder known in the field of conductive paste compositions can be suitably used. Representative examples include at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder.
[0024] In the present disclosure, in the examples described later, a flake-shaped or spherical silver powder or a spherical silver-coated copper powder is exemplified as a representative (A) conductive powder. Therefore, in the present disclosure, a powder containing at least silver is used as the (A) conductive powder. For convenience of explanation, a powder containing silver is appropriately referred to as a "silver-based powder".
[0025] Specific examples of silver-based powders include silver powders that are essentially composed of silver, silver-coated powders in which silver is coated on the surface of a powder (main powder) composed of a material other than silver, and silver alloy powders composed of an alloy containing silver (silver alloy).
[0026] Silver powder is a powder composed only of silver, but it goes without saying that it may contain known unavoidable impurities. In addition, even if it is a silver alloy powder, if it has a purity that is recognized as "silver" according to various known standards, it can be treated as silver powder in this disclosure.
[0027] The specific configuration of the silver-coated powder is not particularly limited, and the main powder composed of a material other than silver may be a metal or a material other than a metal. Examples of materials other than metal include known resin materials, known ceramic materials, glass, etc. When the main powder is a resin material, it is sufficient that the material has heat resistance to such an extent that the powder shape (particle shape) can be maintained even at the heating temperature when the conductive paste composition according to the present disclosure is cured.
[0028] Examples of silver-coated powders in which the main powder is a metal, i.e., silver-coated metal powders, include, but are not limited to, silver-coated copper powders, silver-coated copper alloy powders, silver-coated nickel powders, and silver-coated aluminum powders. Examples of silver-coated powders in which the main powder is glass, i.e., silver-coated glass powders, include, but are not limited to, the specific type of glass. Examples include various known glass powders coated with silver.
[0029] Examples of silver-coated powders in which the main powder is a resin, i.e., silver-coated resin powders, include, but are not limited to, silver-coated silicone resin powders, etc. Examples of silver-coated powders in which the main powder is a ceramic material, i.e., silver-coated ceramic powders, include, but are not limited to, silver-coated alumina powders, etc.
[0030] When the silver-based powder is a silver-coated powder, the amount of silver coated on the surface of the main powder, i.e., the amount of silver coating, is not particularly limited and can be set appropriately according to various conditions. The amount of silver coating can be increased or decreased depending on the volume resistivity required depending on the application (application of the cured product) of the conductive paste composition according to the present disclosure. Alternatively, the amount of silver coating can be increased or decreased depending on the material (conductivity) of the main powder. The amount of silver coating can be expressed as the ratio of the mass of coated silver to the total mass of the silver-coated powder (mass ratio, for example, percentage (mass%), etc.).
[0031] The specific shape of the silver-based powder (or other conductive powder) is not particularly limited, and may be spherical (granular) or flake-like (thin or scaly). Note that the flake-like powder may be a powder that has a shape close to a flat plate or a thin rectangular parallelepiped when viewed as a whole, even if it has some unevenness and deformation. The spherical powder may be a powder that has a three-dimensional shape closer to a cube than a rectangular parallelepiped when viewed as a whole, even if it has some unevenness and deformation.
[0032] The specific physical properties of the silver-based powder (or other conductive powder) are not particularly limited, and the average particle size, specific surface area, tap density, etc. may be within known ranges. For example, if the silver-based powder is a flake-shaped powder, the average particle size D50 may be within a range of, for example, 0.5 to 20 μm, and the BET specific surface area may be within a range of, for example, 0.1 to 2.0 m. 2 / g, and the tap density is, for example, 0.5 to 10 g / cm 3 The aspect ratio may be within a range of, for example, 5 to 15. If the silver-based powder is a spherical powder, the average particle size D50 may be within a range of 0.1 to 10 μm, and the BET specific surface area may be within a range of 0.5 to 2.0 m. 2 / g, and the tap density is, for example, 1.0 to 10 g / cm 3 Conductive powders other than silver-based powders may also be used as long as their physical properties fall within the above ranges.
[0033] The method for measuring (evaluating) the average particle diameter D50 of the conductive powder is not particularly limited, but in the present disclosure, it may be measured (evaluated) by a laser diffraction method using a microtrack particle size distribution measuring device, as in the examples described later. The method for evaluating the BET specific surface area of the conductive powder is also not particularly limited, but it may be measured and evaluated by a BET one-point method using nitrogen adsorption using a known specific surface area meter, as in the examples described later. The method for evaluating the tap density of the conductive powder is also not particularly limited, but it may be evaluated by tapping under predetermined conditions using a known tap density measuring device, and calculating the sample mass relative to the sample volume after tapping, as in the examples described later.
[0034] The various conditions in the various measurement or evaluation methods for the (A) conductive powder containing these silver-based powders can be conditions known in the field of resin-type conductive pastes (for example, the conditions described in the published patent applications of the applicant of the present application).
[0035] Regardless of whether the silver-based powder is a silver powder (or a silver alloy powder) or a silver-coated powder, or whether the silver-based powder has a flake-like or spherical shape, the method for producing the powder is not particularly limited, and any known method can be used.
[0036] When the silver powder (or silver alloy powder) is a flake powder, for example, a spherical powder produced by a known method is used as the base powder, and the base powder is subjected to a known mechanical treatment to produce the flake powder. The particle size, degree of aggregation, and other physical properties of the base powder can be appropriately selected depending on, for example, the intended use of the conductive paste composition (the type of electrode or electrical wiring, which is the cured product, or the type of electronic parts or electronic devices equipped with these electrodes or electrical wiring, etc.).
[0037] In addition, when the silver powder (or silver alloy powder) is a spherical powder, the manufacturing method is not particularly limited, and examples thereof include powder manufactured by a wet reduction method, and spherical powder manufactured by other known methods such as an electrolytic method or an atomization method. In the case of a silver-coated powder, the surface of the flake-shaped or spherical main powder manufactured as described above may be coated with silver by a known method.
[0038] In the conductive paste composition according to the present disclosure, at least a silver-based powder may be used as the (A) conductive powder, but a conductive powder other than the silver-based powder may be used in combination. Examples of such other conductive powders include, but are not limited to, gold powder, copper powder, palladium powder, nickel powder, aluminum powder, lead powder, and carbon powder. A representative example is copper powder.
[0039] When multiple types of powders are used in combination as the (A) conductive powder, the blending ratio (blending amount) is not particularly limited. For example, when a silver-based powder is used in combination with a conductive powder other than the silver-based powder, the silver-based powder may be contained in at least more than 10 mass% of all the (A) conductive powders, and may be contained in 50 mass% or more, 90 mass% or more, or 95 mass% or more. The blending amount when using other conductive powders in combination can be appropriately set according to the various conditions required for the obtained cured product.
[0040] [(B) Epoxy resin] The specific structure of the epoxy resin (B) used as one of the resin components in the present disclosure is not particularly limited, but as the epoxy resin (B), at least one type of epoxy resin having an epoxy equivalent of 500 g / eq or more is used.
[0041] For convenience of explanation, an epoxy resin having an epoxy equivalent of 500 g / eq or more is referred to as a "first epoxy resin," and an epoxy resin having an epoxy equivalent of less than 500 g / eq is referred to as a "second epoxy resin." In the present disclosure, as the (B) epoxy resin, only the first epoxy resin may be used, or the first epoxy resin and the second epoxy resin may be used in combination.
[0042] When a first epoxy resin is used as the (B) epoxy resin, and a phenol ester compound is used as the (C) curing agent, as described below, the cured product of the obtained conductive paste composition can have good thermal shock resistance and good moist heat resistance while maintaining good electrical properties.
[0043] When the first epoxy resin and the second epoxy resin are used in combination, the content of the first epoxy resin in all the (B) epoxy resins is not particularly limited, but typically may be 30% by mass or more. If the content of the first epoxy resin is 30% by mass or more, it is possible to more satisfactorily achieve both thermal shock resistance and moist heat resistance.
[0044] In the present disclosure, as the (B) epoxy resin, the first epoxy resin may be used alone or in a suitable combination of two or more kinds. Also, when the (B) epoxy resin is used in combination with a second epoxy resin, the second epoxy resin may be used alone or in a suitable combination of two or more kinds.
[0045] In the present disclosure, regardless of the first epoxy resin and the second epoxy resin, the specific type of epoxy resin used as the (B) epoxy resin is not particularly limited. A representative example is a polyfunctional epoxy resin having two or more oxirane rings (epoxy groups) in one molecule.
[0046] Examples of such polyhydric epoxy resins include glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type. The glycidyl ether type is obtained by reacting epichlorohydrin with novolac, polyhydric phenol, polyhydric alcohol, etc. Examples of novolac include phenol novolac and cresol novolac, examples of polyhydric phenol include bisphenol A, hydrogenated bisphenol A, bisphenol F, bisphenol AD, and resorcin, and examples of polyhydric alcohol include ethylene glycol, neopentyl glycol, glycerin, trimethylolpropane, pentaerythritol, triethylene glycol, and polypropylene glycol. Examples of monofunctional glycidyl ether type epoxy resins include phenyl glycidyl ether. The glycidyl amine type is obtained by reacting epichlorohydrin with a polyamino compound such as ethylenediamine, triethylenetetramine, and aniline. The glycidyl ester type is obtained by reacting epichlorohydrin with a polyvalent carboxyl compound such as adipic acid, phthalic acid, isophthalic acid, etc. The alicyclic type is synthesized by oxidation of olefin, etc. These epoxy resins may be used alone or in combination of two or more.
[0047] In the examples described later, a commercially available bisphenol A type epoxy resin is used as the first epoxy resin (epoxy equivalent: 500 g / eq or more), and a commercially available bisphenol A type epoxy resin, bisphenol F type epoxy resin, or phenol novolac type epoxy resin is used as the second epoxy resin (epoxy equivalent: less than 500 g / eq).
[0048] [(C) Hardener] In the present disclosure, the (C) curing agent used as one of the resin components together with the (B) epoxy resin is a compound obtained by esterifying the phenolic hydroxyl group of a polyhydric phenol compound with an organic acid. More specifically, the (C) curing agent according to the present disclosure may be a phenol ester compound having a structure represented by the following general formula (1).
[0049] [ka]
[0050] R in the general formula (1) is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom. X in the general formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2). A in the general formula (2) is an alkyl group having 1 to 6 carbon atoms. Z in the general formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms.
[0051] [ka]
[0052] The R, X, Z, and A contained in the general formula (1) may each independently be the aforementioned substituent or atom. That is, in the general formula (1), the R, X, Z, and A may each be the same substituent or atom, or may each be different substituents or atoms (including the case where some of the R, X, Z, and A in the molecule are the same, and the other parts are different substituents or atoms).
[0053] Furthermore, m in general formula (1) is an integer of 0 to 4, and n in general formula (1) is an average value of 0 to 2. All of the m's in formula (1) may be the same integer, or may be different integers (including the case where some of the m's in a molecule are the same integer, and other parts are different integers).
[0054] By using such a phenol ester compound as a curing agent (C) for the epoxy resin (B) containing the first epoxy resin, the resulting cured product of the conductive paste composition can achieve good electrical properties as well as good thermal shock resistance and good moist heat resistance.
[0055] The esterification rate of the phenol ester compound as the (C) curing agent is not particularly limited, but typically, it can be 70% or more, may be 80% or more, or may be 90% or more. When the esterification rate of the phenol ester compound is 70% or more, when the (B) epoxy resin is used as the (C) curing agent for the (B) epoxy resin containing at least one kind of first epoxy resin, the cured product of the obtained conductive paste composition can easily achieve good thermal shock resistance and good moist heat resistance.
[0056] The synthesis method (production method) of the phenol ester compound represented by the general formula (1) is not particularly limited, and a known method can be suitably used. For example, in the examples described later, a phenol ester compound is synthesized by reacting a commercially available phenolic resin (e.g., phenol novolac resin or cresol novolac resin) with a carboxylic anhydride (e.g., acetic anhydride or propionic anhydride) by a known method. The esterification rate of the phenol ester compound used in the examples described later is 90% or more (95% or 93%).
[0057] In the present disclosure, the amount of the (C) curing agent used (the amount of the (C) curing agent blended in the conductive paste composition) is not particularly limited. Typically, the amount of the (C) curing agent blended may be within the range of 3 to 150 parts by mass when the total amount of the (B) epoxy resin contained in the conductive paste composition is 100 parts by mass. In the examples described later, the amount of the (C) curing agent used relative to 100 parts by mass of the (B) epoxy resin is exemplified as 4.1 to 33.3 parts by mass.
[0058] In the present disclosure, the phenol compound before esterification used in the synthesis of the phenol ester compound as the curing agent (C) is not particularly limited.Specific examples thereof include known polyhydric phenol compounds such as phenol novolac resin, cresol novolac resin, aromatic hydrocarbon formaldehyde resin modified phenol resin, dicyclopentadiene phenol addition type resin, phenol aralkyl resin (Zylok resin), naphthol aralkyl resin, triphenylol methane resin, tetraphenylol ethane resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol co-condensed novolac resin, and terpene phenol resin.
[0059] The organic acid for esterifying these phenolic compounds is not particularly limited. Representative examples include acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, succinic acid, maleic acid, phthalic acid, benzoic acid, etc. These organic acids may be anhydrides as described above.
[0060] The phenol ester compound (C) may be used as a curing agent either alone or in combination of two or more. In addition, a known curing agent other than the phenol ester compound may be used in combination as long as it does not affect the physical properties of the resulting conductive paste composition or the cured product thereof.
[0061] [(D) Curing accelerator] In the present disclosure, a curing accelerator (D) is used as a resin component together with the epoxy resin (B) and the curing agent (C). The specific curing accelerator (D) is not particularly limited, and may be a known compound used to cure the first epoxy resin used as the epoxy resin (B) or the first and second epoxy resins.
[0062] Specific examples of the (D) curing accelerator include acid anhydrides such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, and succinic anhydride; imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1-benzyl-2-methylimidazole, 2-methyl-4 ... imidazoles such as ethyl imidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-aminoethyl-2-methylimidazole, 1-methylimidazole, and 2-ethylimidazole; dimethyloctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dimethylbehenylamine, dilaurylmonoethylamine, methylimidazole ... Tertiary amines such as ethyldidecylamine, methyldioleylamine, triallylamine, triisopropanolamine, triethylamine, 3-(dibutylamino)propylamine, tri-n-octylamine, 2,4,6-trisdimethylaminomethylphenol, triethanolamine, methyldiethanolamine, and diazabicycloundecene; Lewis acids or compounds thereof containing boron fluoride such as boron trifluoride ethyl ether, boron trifluoride phenol, boron trifluoride piperidine, boron trifluoride acetate, boron trifluoride monoethylamine, boron trifluoride triethanolamine, and boron trifluoride monoethanolamine; amine adducts such as Amicure Series PN-23 or MY-24 available from Ajinomoto Fine-Techno Co., Ltd. and Fujicure Series FXR-1020 or FXR-1030 available from Fuji Chemical Industry Co., Ltd.; dicyandiamide; and the like.
[0063] These (D) curing accelerators may be used alone or in combination of two or more. The amount or conditions of use of the (D) curing accelerator are not particularly limited, and it may be used in a known amount or under known conditions.
[0064] In the examples described later, in all of Examples 1 to 14 and Comparative Examples 1 to 7, 2-ethyl-4-methylimidazole was used as the hardening accelerator (D).
[0065] [Method of producing conductive paste composition and its use] The method for producing the conductive paste composition according to the present disclosure is not particularly limited, and known methods can be suitably used. As a representative example, the above-mentioned components (A) to (D) and other components added or mixed as necessary are mixed in a predetermined mixing ratio (based on mass), and a paste is formed using a known kneading device. As the kneading device, for example, a three-roll mill or the like can be mentioned.
[0066] The amount (content) of each of the components (A) to (D) in the conductive paste composition according to the present disclosure is not particularly limited. When the total amount of the conductive powder (A) and the resin component is taken as 100 mass%, the amount of the conductive powder (A) may be within a range of 70 to 99 mass%, or may be within a range of 80 to 98 mass%, or may be within a range of 85 to 95 mass%.
[0067] If the amount of the (A) conductive powder is less than 70% by mass, the contact density between the (A) conductive powder particles in the cured conductive paste composition (cured product) will be small, and poor contact between the (A) conductive powder particles may result in insufficient conductivity, leading to an increase in volume resistivity. On the other hand, if the content of the (A) conductive powder is more than 99% by mass, the amount of the resin component may be reduced, and the (A) conductive powder may not be uniformly dispersed.
[0068] In addition, the conductive paste composition according to the present disclosure may contain, as necessary, a solvent known in the field of conductive paste compositions, as well as various additives, in addition to the above-mentioned (A) conductive powder and resin components ((B) epoxy resin, (C) curing agent, (D) curing accelerator). The additives are not particularly limited, but specific examples include leveling agents, antioxidants, ultraviolet absorbers, silane coupling agents, defoamers, viscosity adjusters, and the like. These additives may be added within a range that does not impair the effects of the present invention.
[0069] The solvent is added to adjust the physical properties, such as the viscosity or fluidity, of the conductive paste composition according to the present disclosure. The physical properties of the conductive paste composition according to the present disclosure are not particularly limited, but the viscosity may be, for example, within a range of 75 to 100 Pa·s from the viewpoint of convenience in forming a pattern of an electrode or an electric wiring, particularly efficiency of screen printing. If the viscosity of the conductive paste composition is within this range, pattern formation by screen printing can be performed well.
[0070] The specific type of the solvent is not particularly limited, and examples thereof include saturated hydrocarbons such as hexane; aromatic hydrocarbons such as toluene; glycol ethers (cellosolves) such as ethyl cellosolve, butyl cellosolve, and butyl cellosolve acetate; glycol ethers such as diethylene glycol diethyl ether and butyl diglycol (butyl carbitol, diethylene glycol monobutyl ether); acetate esters of glycol ethers such as butyl diglycol acetate and butyl carbitol acetate; alcohols such as diacetone alcohol, terpineol, and benzyl alcohol; ketones such as cyclohexanone and methyl ethyl ketone; esters such as DBE, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and 2,2,4-trimethyl-1,3-pentanediol diisobutyrate; etc. Only one of these solvents may be used, or two or more of them may be used in appropriate combination.
[0071] The amount of the solvent is not particularly limited, and can be added to an extent that the viscosity or fluidity of the conductive paste composition according to the present disclosure can be adjusted within a suitable range. If the content of the solvent exceeds 40 mass% relative to the entire conductive paste composition, depending on the types of other components or the composition of the conductive paste composition, a fluidity suitable for printing cannot be obtained, and printability may be reduced.
[0072] The method for forming a predetermined pattern on a substrate using the conductive paste composition according to the present disclosure is not particularly limited, and various known forming methods can be suitably used. A representative example is a method using a printer using a screen printing method, but other printing methods such as gravure printing, offset printing, inkjet printing, dispenser method, and dip method (dipping) can also be applied.
[0073] In addition, the method of forming a pattern that becomes a cured product by the conductive paste composition according to the present disclosure is not particularly limited, and various known forming methods can be suitably used. Representative examples include printing methods such as screen printing, gravure printing, offset printing, inkjet printing, dispenser method, and dip method. Therefore, the conductive paste composition according to the present disclosure may be any one that can be applied to a substrate by a printer, a dispenser, or dipping.
[0074] The method for curing the conductive paste composition according to the present disclosure is not particularly limited, and a known heating method can be suitably used depending on the type of (B) epoxy resin and (C) curing agent constituting the resin component. In the examples described below, when preparing an evaluation sample, the conductive paste composition is applied onto a substrate and heated in a hot air dryer at 200°C for 60 minutes, but it goes without saying that the present disclosure is not limited to this heating method. In the present disclosure, the method for measuring or evaluating various physical properties of the cured product of the conductive paste composition is not particularly limited, and the methods exemplified in the examples described below can be suitably used.
[0075] The conductive paste composition according to the present disclosure can be suitably used in a wide range of applications in which the conductive cured product is formed by curing the composition by heating. A representative example is the application of forming a patterned electrode or electrical wiring on a substrate. Specifically, the conductive paste composition can be suitably used in applications such as external electrodes of chip-type electronic components; electrodes or electrical wiring of components used in RFID (Radio Frequency IDentification), electromagnetic shielding, vibrator bonding, membrane switches, or electroluminescence; current collecting electrodes of solar cells; and the like. In particular, the conductive paste composition according to the present disclosure can be suitably used in applications in which the conductive paste composition is applied to electrodes of electronic components.
[0076] In this manner, the conductive paste composition according to the present disclosure may be configured so that it contains (A) a conductive powder and a resin component, the resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator, the (B) epoxy resin contains at least one type of epoxy resin having an epoxy equivalent of 500 g / eq or more, and the (C) curing agent is a phenol ester compound having a structure represented by the general formula (1) described above.
[0077] According to the above-mentioned configuration, the epoxy resin (B) contained as the resin component has at least one epoxy equivalent of 500 g / eq or more, and the phenol ester compound of the general formula (1) is used as the curing agent (C). This allows the cured product of the obtained conductive paste composition to have good thermal shock resistance and good moist heat resistance while maintaining good electrical properties. Therefore, it is possible to obtain a conductive paste composition containing an epoxy resin as a resin component, which can achieve good thermal shock resistance and good moist heat resistance after curing. EXAMPLES
[0078] The present disclosure will be described in more detail based on examples and comparative examples, but the present invention is not limited thereto. Those skilled in the art can make various changes, modifications, and alterations without departing from the scope of the present invention. In the following examples, (A) the evaluation method of the conductive powder, (C) the synthesis method of the phenol ester compound as the curing agent, and the evaluation method of the cured product were performed as follows.
[0079] [(A) Evaluation method for conductive powder] (1) Average particle size D50 The average particle size D50 of the conductive powder (A) shown in Table 1 was evaluated by laser diffraction. 0.3 g of the conductive powder (A) sample was weighed into a 50 ml beaker, 30 ml of isopropyl alcohol was added, and the powder was dispersed by treating with an ultrasonic cleaner (manufactured by AS ONE Corporation, product name: USM-1) for 5 minutes, and the average particle size D50 was measured and evaluated using a Microtrack particle size distribution analyzer (manufactured by Nikkiso Co., Ltd., product name: Microtrack particle size distribution analyzer 9320-HRA X-100).
[0080] (2) Evaluation of BET specific surface area The BET specific surface area of the conductive powder (A) shown in Table 1 was evaluated using a surface area analyzer (manufactured by Quanta Chrome, product name: Monosorb). 1 g of the conductive powder (A) sample was subjected to the surface area analyzer, and the specific surface area was measured and evaluated by the BET single point method using nitrogen adsorption. In the measurement of the BET specific surface area, the degassing condition before the measurement was 60°C for 10 minutes.
[0081] (3) Evaluation of tap density The tap density of the (A) conductive powder shown in Table 1 was evaluated using a tap density measuring device (manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd., product name: bulk specific gravity measuring device SS-DA-2) according to the following calculation formula (3). A 15 g sample of the (A) conductive powder was weighed and placed in a 20 ml test tube, tapped 1,000 times with a drop of 20 mm, and the sample volume after tapping (cm3) was measured using the tap density measuring device. 3 ) was measured, and the tap density was calculated and evaluated using the following calculation formula (3). Tap density = sample mass / sample volume after tapping (3)
[0082] [Evaluation method of the cured product] (1) Conductor resistance evaluation A conductive pattern 11 shown in FIG. 1 was screen-printed on the surface of an alumina substrate, which was a base material, using a conductive paste composition according to the embodiment or comparative example. As shown in FIG. 1, the conductive pattern 11 has rectangular terminals 11a and 11b located at both ends, and a zigzag wiring portion 11c connecting the terminals 11a and 11b. The alumina substrate on which the conductive pattern 11 was formed was heated in a hot air dryer at 200° C. for 60 minutes to harden the conductive pattern 11 (conductive paste composition). In this way, a sample for evaluating the conductor resistance was produced.
[0083] For the evaluation samples of each Example or Comparative Example, the film thickness of the cured conductive pattern 11 (cured product) was measured using a surface roughness meter (manufactured by Tokyo Seimitsu Co., Ltd., product name Surfcom 480A), and the electrical resistance was measured using a digital multimeter (manufactured by Advantest Corporation, product name R6551). Based on the measured film thickness and electrical resistance and the aspect ratio of the conductive pattern 11, the volume resistivity (μΩ·cm) of the cured product of the conductive paste composition of each Example, Comparative Example, or Reference Example was calculated and evaluated.
[0084] (2) Evaluation method for connection resistance As shown in FIG. 2, the conductive paste composition of the example or comparative example was applied to a tin (Sn)-plated substrate 21 using a dispenser to a diameter of 2.5 mm to form a paste layer 22. Then, a gold-plated rivet 23 having a circular fixing surface with a diameter of 5 mm was laminated on the paste layer 22. At this time, the thickness of the adhesive layer 22 was set to 200 μm by using a polyimide film with a thickness of 200 μm as a spacer. Next, the tin-plated substrate 21 was heated in a hot air dryer at 200° C. for 60 minutes to harden the paste layer 22 to form a hardened layer. In this way, a sample 20 for evaluating the connection resistance was produced.
[0085] The electrical resistance between the tin-plated substrate 21 and the gold-plated rivet 23 in the evaluation sample 20 was measured with an electrical resistance meter 24 (digital multimeter, manufactured by Advantest Corporation, product name: R6551) and was taken as the connection resistance of the cured layer. The measured connection resistance was rated as "A" when it was less than 0.05 Ω, and "B" when it was 0.05 Ω or more.
[0086] (3) Evaluation method for moisture and heat resistance The aforementioned connection resistance evaluation sample was stored for 1000 hours in a thermohygrostat (manufactured by Espec Corporation, product name: SH-262) set at a temperature of 85°C and a humidity of 85% RH. The connection resistance of the connection resistance evaluation specimen before and after storage was measured in the same manner as in the connection resistance evaluation described above. A change in resistance value after storage from the initial resistance value before storage of less than 10% was rated as "A", a change in resistance value of 10% or more but less than 20% was rated as "B", and a change in resistance value of 20% or more was rated as "C".
[0087] (4) Thermal shock resistance evaluation method The aforementioned connection resistance evaluation sample was subjected to 1000 heat cycles of holding temperatures of -55°C and +125°C for 30 minutes each using a thermal shock device (manufactured by Espec Corporation, product name: TSE-11-A). The connection resistance of the connection resistance evaluation specimen before and after the heat cycle was measured in the same manner as the aforementioned connection resistance evaluation. If the rate of change in resistance after storage compared to the initial resistance before storage was less than 10%, it was rated as "A", if it was 10% or more but less than 20%, it was rated as "B", and if it was 20% or more, it was rated as "C".
[0088] [(A) Conductive powder] In the conductive paste compositions according to the Examples and Comparative Examples, the (A) conductive powder was used in appropriate combination with three types of powder shown in Table 1. In each Example or Comparative Example, each (A) conductive powder is represented by the abbreviations shown in Table 1.
[0089] [Table 1]
[0090] [Resin component] In the conductive paste compositions according to the examples and comparative examples, five types of (B) epoxy resins and four types of (C) curing agents shown in Table 2 were used in appropriate combination as the resin components. In addition, in order to cure these resins, (D) curing accelerators shown in Table 2 were used. In each of the examples and comparative examples, the respective resins, curing catalysts, and initiators are represented by the abbreviations shown in Table 2, as in the case of (A) conductive powder.
[0091] [Table 2]
[0092] [Synthesis of phenol ester compounds] Among the (C) curing agents shown in Table 2, the phenol ester compounds, acetylated phenol novolak resin designated C-01 and propionated cresol novolak resin designated C-02, were synthesized (produced) by the method described below.
[0093] (1) C-01: Synthesis of acetylated phenol novolac resin A 3-liter four-neck flask equipped with a thermometer, a cooling tube, a nitrogen inlet tube, and a stirrer was charged with 212 g of phenol novolac resin (manufactured by DIC Corporation, product name: PHENOLITE TD-2106 (abbreviation C-03 in Table 2), hydroxyl equivalent: 106 g / eq), and 500 g of methyl isobutyl ketone was added and dissolved by stirring under a nitrogen atmosphere. Furthermore, 210 g of acetic anhydride and 200 g of pyridine were added to the solution and dissolved. Then, the solution was reacted at 50° C. for 4 hours. Next, the obtained reaction solution was diluted with 500 g of methyl isobutyl ketone and cooled. Further, the cooled diluted reaction solution was thoroughly washed with distilled water and concentrated under reduced pressure to obtain an acetylated phenol novolac resin (esterification rate 95%) with the abbreviation C-01.
[0094] (2) C-02: Synthesis of propionated cresol novolac resin 238 g of cresol novolac resin (manufactured by DIC Corporation, product name: PHENOLITE KA-1165 (abbreviation C-04 in Table 2), hydroxyl equivalent: 119 g / eq) was added to a 3-liter four-neck flask equipped with a thermometer, a cooling tube, a nitrogen inlet tube, and a stirrer, and 500 g of methyl isobutyl ketone was added and dissolved by stirring under a nitrogen atmosphere. Furthermore, 267 g of propionic anhydride and 200 g of pyridine were added to the solution and dissolved. Then, the solution was reacted at 50° C. for 4 hours. Next, the obtained reaction solution was diluted with 500 g of methyl isobutyl ketone and cooled. Further, the cooled diluted reaction solution was thoroughly washed with distilled water and concentrated under reduced pressure to obtain a propionated cresol novolac resin (esterification rate 93%) with the abbreviation C-02.
[0095] Example 1 (A) As the conductive powder, a flake silver powder designated A-01 and a spherical silver powder designated A-02 in Table 1 were selected.
[0096] Of the resin components, two types of epoxy resin (B) were used: a first epoxy resin with an epoxy equivalent of 500 g / eq or more, and a second epoxy resin with an epoxy equivalent of less than 500 g / eq. As the first epoxy resin, the epoxy resin with the abbreviation B-01 (epoxy equivalent: 3,000 g / eq) in Table 2 was selected, and as the second epoxy resin, the epoxy resin with the abbreviation B-03 (epoxy equivalent: 190 g / eq) was selected.
[0097] Of the resin components, a phenol ester compound (acetylated phenol novolac resin) with the abbreviation C-01 shown in Table 2 was selected as the (C) hardener, and an imidazole with the abbreviation D-01 shown in Table 2 was used as the (D) hardener accelerator.
[0098] These components (A) to (D) were mixed in the composition (mixing ratio) shown in Table 3. In Table 3 (and Tables 4 and 5 described below), the mixing ratio of the two types of conductive powder (A) is 100 mass% in total. In Example 1, the mass ratio (A-01 / A-02) of the flaky silver powder with the abbreviation A-01 to the spherical silver powder with the abbreviation A-02 is 50 / 50.
[0099] In Table 3 (and Tables 4 and 5 described later), the composition of the resin components is such that the blending ratio of the epoxy resin (B) and the curing agent (C) is 100 mass % in total. In Example 1, the mass ratio (B-01 / B-03 / C-01) of the first epoxy resin with the abbreviation B-01, the second epoxy resin with the abbreviation B-03, and the curing agent with the abbreviation C-01 is 25 / 50 / 25.
[0100] The content of the first epoxy resin in the (B) epoxy resin is 33.3 mass% (25 / (25+75)), and the amount of the (C) curing agent used is 33.3 mass parts per 100 mass parts of the (B) epoxy resin. In Table 3 (and Tables 4 and 5 described below), the amount of the (D) curing accelerator is 1 mass part per 100 mass parts of the resin components in total.
[0101] Furthermore, in Table 3 (and Tables 4 and 5 described below), the blending ratio of (A) conductive powder to the resin component is shown as a mass ratio. In Example 1, the mass ratio of the total amount of (A) conductive powder to the total amount of (B) epoxy resin and (C) hardener, which are the resin components (solid content mass ratio (A) / (B)+(C)) is 93 / 7. The same applies to each of the following Examples and Comparative Examples.
[0102] The conductive paste composition of Example 1 was prepared (manufactured) by kneading the components (A) to (D) mixed according to the composition shown in Table 3 using a three-roll mill.
[0103] Using the obtained conductive paste composition according to Example 1, as described above, samples for evaluating conductor resistance and connection resistance (as well as moist heat resistance and thermal shock resistance) were prepared (manufactured). Using these evaluation samples, the properties (conductor resistance, connection resistance, moist heat resistance, and thermal shock resistance) of the cured product of the conductive paste composition were evaluated by the evaluation method described above. The results are shown in Table 3.
[0104] (Examples 2 and 3) A conductive paste composition according to Example 2 or Example 3 was prepared (manufactured) in the same manner as in Example 1, except that a phenol ester compound (propionated cresol novolac resin) with the abbreviation C-02 shown in Table 2 was selected as the curing agent (C) (Example 2), or an epoxy resin with the abbreviation B-02 shown in Table 2 (epoxy equivalent: 8,000 g / eq) was selected as the first epoxy resin among the epoxy resins (B) and an epoxy resin with the abbreviation B-04 shown in Table 2 (epoxy equivalent: 170 g / eq) was selected as the second epoxy resin (B) (Example 3).
[0105] Using the conductive paste compositions of Examples 2 and 3 obtained, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation method described above. The results are shown in Table 3.
[0106] (Examples 4 to 6) The conductive paste compositions according to Examples 4 to 6 were prepared (manufactured) in the same manner as in Example 3, except that (A) the compounding ratio of the conductive powders was A-01 / A-02=30 / 70 (Example 4), (B) the epoxy resin with the abbreviation B-03 was selected as the second epoxy resin among the epoxy resins, and the solid content mass ratio was (A) / (B)+(C)=90 / 10 (Example 5), or the epoxy resin with the abbreviation B-03 was selected as the second epoxy resin, and (C) the phenol ester compound with the abbreviation C-02 was selected as the curing agent (Example 6).
[0107] Using the obtained conductive paste compositions according to Examples 4 to 6, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 3.
[0108] Example 7 The conductive paste composition of Example 7 was prepared (manufactured) in the same manner as in Example 1, except that the epoxy resin with the abbreviation B-05 shown in Table 2 (epoxy equivalent: 190 g / eq) was selected as the second epoxy resin among the (B) epoxy resins, and the solid content mass ratio was set to (A) / (B)+(C)=95 / 5.
[0109] Using the obtained conductive paste composition according to Example 7, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 3.
[0110] [Table 3]
[0111] (Examples 8 to 10) Among the (B) epoxy resins, an epoxy resin with the abbreviation B-05 is selected as the second epoxy resin, and the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent is set to B-02 / B-05 / C-01) of 30 / 50 / 20 (Example 8), or an epoxy resin with the abbreviation B-03 is selected as the second epoxy resin, and the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent is set to B-02 / B-03 / C-01) of 25 / 55 / 20, and further, the solid content mass The ratio was (A) / (B)+(C)=85 / 15 (Example 9), or the conductive powder (A) was a flaky silver powder with the abbreviation A-01 and a spherical silver powder with the abbreviation A-02, as well as a silver-coated copper powder with the abbreviation A-03 shown in Table 1 (amount of silver coated on copper powder: 10% by mass), and the mass ratio (mixing ratio) of these conductive powders (A) was A-01 / A-02 / A-03=30 / 30 / 40 (Example 10). The conductive paste compositions of Examples 8 to 10 were prepared (manufactured) in the same manner as in Example 3.
[0112] In Example 8, the content of the first epoxy resin in the (B) epoxy resin was 37.5 mass % (30 / (30+50)), and the amount of the (C) curing agent used was 25 mass parts per 100 mass parts of the (B) epoxy resin.
[0113] Using the obtained conductive paste composition according to Example 8, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.
[0114] Example 9 A conductive paste composition according to Example 9 was prepared (manufactured) in the same manner as in Example 4, except that an epoxy resin with the abbreviation B-03 was selected as the second epoxy resin, the mass ratio of the first epoxy resin, the second epoxy resin, and the (C) curing agent was B-02 / B-03 / C-01) was 25 / 55 / 20, and the mass ratio of the solid contents was (A) / (B)+(C)=85 / 15. In Example 9, the amount of the (C) curing agent used was 26.6 parts by mass relative to 100 parts by mass of the (B) epoxy resin.
[0115] Using the obtained conductive paste composition according to Example 9, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.
[0116] Example 10 As the (A) conductive powder, in addition to the flake silver powder with the abbreviation A-01 and the spherical silver powder with the abbreviation A-02, a silver-coated copper powder with the abbreviation A-03 shown in Table 1 (amount of silver coated on copper powder: 10 mass%) was used, and the mass ratio (mixing ratio) of these (A) conductive powders was A-01 / A-02 / A-03 = 30 / 30 / 40 (Example 10). Except for this, the conductive paste compositions of Examples 8 to 10 were prepared (manufactured) in the same manner as in Example 3.
[0117] Using the obtained conductive paste composition according to Example 10, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.
[0118] Example 11 A conductive paste composition according to Example 11 was prepared (manufactured) in the same manner as in Example 1, except that only the first epoxy resin, abbreviated as B-01, was used as the (B) epoxy resin, and the mass ratio of the first epoxy resin to the (C) curing agent was B-01 / C-01=95 / 5. In Example 11, the content of the first epoxy resin in the (B) epoxy resin was 100 mass%, and the amount of the (C) curing agent used was 5.2 mass parts relative to 100 mass parts of the (B) epoxy resin.
[0119] Using the obtained conductive paste composition according to Example 11, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.
[0120] Example 12 A conductive paste composition according to Example 12 was prepared (manufactured) in the same manner as in Example 11, except that an epoxy resin having the abbreviation B-01 and an epoxy resin having the abbreviation B-02 were used in combination as the (B) epoxy resin in a mass ratio of B-01 / B-02=50 / 45. In Example 12, the content of the first epoxy resin in the (B) epoxy resin was 52.6 mass% (50 / (50+45)), and the amount of the (C) curing agent used was 5.2 mass parts relative to 100 mass parts of the (B) epoxy resin.
[0121] Using the obtained conductive paste composition according to Example 12, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 4.
[0122] (Examples 13 and 14) The conductive paste composition according to Example 13 or Example 14 was prepared (manufactured) in the same manner as in Example 11, except that the compounding ratio of the conductive powder (A) was A-01 / A-02=70 / 30, the mass ratio of the first epoxy resin was B-01 / B-02=48 / 48, and the solid content mass ratio was (A) / (B)+(C)=87 / 13 (Example 13), or the compounding ratio of the conductive powder (A) was A-01 / A-02=20 / 80, the mass ratio of the first epoxy resin was B-01 / B-02=70 / 25, and the solid content mass ratio was (A) / (B)+(C)=91 / 9 (Example 14).
[0123] In Example 13, the content of the first epoxy resin in the (B) epoxy resin was 50 mass% (48 / (48+48)), and the amount of the (C) curing agent used was 4.1 mass parts per 100 mass parts of the (B) epoxy resin. In Example 14, the content of the first epoxy resin in the (B) epoxy resin was 73.6 mass% (70 / (70+25)), and the amount of the (C) curing agent used was 5.2 mass parts per 100 mass parts of the (B) epoxy resin.
[0124] Using the conductive paste compositions of Examples 13 and 14 obtained, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation method described above. The results are shown in Table 4.
[0125] [Table 4]
[0126] (Comparative Examples 1 and 2) (C) A conductive paste composition according to Comparative Example 1 or Comparative Example 2 was prepared (manufactured) in the same manner as in Example 1, except that a phenol novolak resin (hydroxyl equivalent: 104 g / eq, Comparative Example 1) with the abbreviation C-03 shown in Table 2 or a cresol novolak resin (hydroxyl equivalent: 119 g / eq, Comparative Example 2) with the abbreviation C-04 shown in Table 2 was selected as the curing agent instead of using a phenol ester compound.
[0127] As described above, evaluation samples were prepared (manufactured) using the obtained conductive paste compositions according to Comparative Examples 1 and 2. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 5.
[0128] Comparative Example 3 (C) A conductive paste composition according to Comparative Example 3 was prepared (manufactured) in the same manner as in Example 5, except that a phenol novolac resin, abbreviated as C-03, was selected as the curing agent without using a phenol ester compound.
[0129] Using the obtained conductive paste composition according to Comparative Example 3, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 5.
[0130] Comparative Example 4 A conductive paste composition according to Comparative Example 4 was prepared (manufactured) in the same manner as in Example 1, except that, as the (B) epoxy resin, a first epoxy resin having an epoxy equivalent of 500 g / eq or more was not used, but only a second epoxy resin having the abbreviation B-03 was selected, and, as the (C) curing agent, an acetylated phenol novolac resin having the abbreviation C-01, which is a phenol ester compound, was used, and the mass ratio of the second epoxy resin to the (C) curing agent was set to B-03 / C-01=65 / 35.
[0131] Using the obtained conductive paste composition according to Comparative Example 4, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 5.
[0132] (Comparative Examples 5 and 6) A conductive paste composition according to Comparative Example 5 or Comparative Example 6 was prepared (manufactured) in the same manner as in Comparative Example 4, except that an epoxy resin with the abbreviation B-05 was selected as the second epoxy resin, and a propionated cresol novolak resin with the abbreviation C-02, which is a phenolic ester compound, was used as the (C) curing agent (Comparative Example 5), or an epoxy resin with the abbreviation B-05 was selected, and a phenolic novolak resin with the abbreviation C-03, which is not a phenolic ester compound, was selected as the (C) curing agent.
[0133] Using the conductive paste compositions according to Comparative Examples 5 and 6, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the properties of the cured products of the conductive paste compositions were evaluated by the evaluation method described above. The results are shown in Table 5.
[0134] Comparative Example 7 A conductive paste composition according to Comparative Example 7 was prepared (manufactured) in the same manner as in Example 11, except that a phenol novolak resin, abbreviated as C-03, which is not a phenol ester compound, was selected as the curing agent (C).
[0135] Using the obtained conductive paste composition according to Comparative Example 7, evaluation samples were prepared (manufactured) as described above. Using these evaluation samples, the characteristics of the cured products of the conductive paste compositions were evaluated by the evaluation methods described above. The results are shown in Table 5.
[0136] [Table 5]
[0137] (Comparison between Examples and Comparative Examples) As is clear from the results of Examples 1 to 14, by containing a first epoxy resin having an epoxy equivalent of 500 g / eq or more as the epoxy resin (B) and using a phenol ester compound represented by the general formula (1) as the curing agent (C), the obtained cured product can realize good electrical properties (conductor resistance and connection resistance) and can also have good moist heat resistance and good thermal shock resistance.
[0138] As is clear from the results of Examples 1 to 10, the electrical properties, the moist heat resistance, and the thermal shock resistance can all be improved by using the first epoxy resin together with the second epoxy resin having an epoxy equivalent of less than 500 g / eq as the epoxy resin (B). Alternatively, as is clear from the results of Examples 11 to 14, even if only the first epoxy resin is used as the epoxy resin (B), all of the electrical properties, the moist heat resistance, and the thermal shock resistance can all be improved.
[0139] In contrast, when the phenol ester compound represented by general formula (1) is not used as the curing agent (C), good thermal shock resistance cannot be achieved, as is clear from the results of Comparative Examples 1 to 3. Moreover, when the phenol ester compound represented by general formula (1) is used as the curing agent (C), good moist heat resistance cannot be achieved, as is clear from the results of Comparative Examples 4 and 5.
[0140] Furthermore, as is clear from the results of Comparative Example 6, when the phenol ester compound represented by general formula (1) is not used as the (C) curing agent and the first epoxy resin is not used, good thermal shock resistance cannot be realized. Moreover, as is clear from the results of Comparative Example 7, even if only the first epoxy resin is used, good moist heat resistance cannot be realized unless the phenol ester compound represented by general formula (1) is used as the (C) curing agent.
[0141] Based on the results of Comparative Examples 1 to 7, it is found that when the first epoxy resin is not used as the epoxy resin (B) or the phenol ester compound represented by the general formula (1) is not used as the curing agent (C), good electrical properties can be achieved, but either the moist heat resistance or the thermal shock resistance cannot be made good.
[0142] The present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments obtained by appropriately combining the technical means disclosed in different embodiments or multiple modified examples. [Industrial Applicability]
[0143] The present invention can be widely and suitably used in the fields of forming conductive cured products in the fields of electric devices and electronic devices.Typically, the present invention can be widely and suitably used in the fields of forming conductive layers on electrodes of electronic components by coating with a printer, a dispenser, or dipping. [Explanation of symbols]
[0144] 11: Conductor pattern 11a,11b:Terminal 11c: Wiring part 20: Evaluation sample 21: Tin-plated substrate 22: Paste layer (or hardened layer) 23: Gold-plated rivets 24: Electrical resistance meter
Claims
1. (A) containing a conductive powder and a resin component, The resin component contains (B) an epoxy resin, (C) a curing agent, and (D) a curing accelerator, The (B) epoxy resin contains at least one epoxy resin having an epoxy equivalent of 500 g / eq or more, The (C) curing agent is represented by the following general formula (1) 【Chemistry 1】 (In the formula (1), R is an alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted phenyl group, a substituted or unsubstituted aralkyl group, an alkoxyl group, or a halogen atom; X in the formula (1) is a hydrogen atom or an ester structure represented by the following general formula (2); A in the formula (2) is an alkyl group having 1 to 6 carbon atoms; 【Chemistry 2】 Z in formula (1) is a divalent hydrocarbon group having 1 to 15 carbon atoms, m in formula (1) is an integer of 0 to 4, n in formula (1) is a number of 0 to 2 on average, R, X, Z, and A contained in formula (1) may be the same substituent or atom or different substituents or atoms, and m in formula (1) may be the same integer or different integers.) The present invention is characterized in that the compound is a phenol ester compound having a structure represented by the formula: Conductive paste composition.
2. The (B) epoxy resin contains 30 mass% or more of an epoxy resin having an epoxy equivalent of 500 g / eq or more. The conductive paste composition according to claim 1 .
3. The esterification rate of the (C) curing agent is 70% or more. The conductive paste composition according to claim 1 .
4. The (C) curing agent is blended in an amount of 3 to 150 parts by mass relative to 100 parts by mass of the (B) epoxy resin. The conductive paste composition according to claim 1 .
5. As the (A) conductive powder, at least one selected from the group consisting of silver powder, copper powder, silver-coated copper powder, silver-coated nickel powder, silver-coated aluminum powder, and silver-coated glass powder is used. The conductive paste composition according to claim 1 .
6. It is applied to the substrate by a printer, a dispenser, or dipping. The conductive paste composition according to claim 1 .
7. Used by applying it to the electrodes of electronic components. The conductive paste composition according to claim 1 .
Citation Information
Patent Citations
Electroconductive adhesive
JP2007277384A