Optical element having cooling passage and optical device

By controlling OH content and using protective coatings or material removal, the optical element minimizes thermal deformation in EUV lithography mirrors, improving imaging quality by maintaining uniform thermal expansion and reducing image defects.

JP2024535801APending Publication Date: 2024-10-02CARL ZEISS SMT GMBH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024515858
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-13
Filing Date
2022-08-16
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

EUV lithography mirrors experience image defects due to thermal deformation caused by gradients in OH content resulting from thermal bonding, which affects the coefficient of thermal expansion and zero-crossing temperature.

Method used

The optical element features cooling channels with channel walls adjacent to lands, maintaining a zero-crossing temperature deviation of less than 3.0 K from the land's center, achieved by controlling OH content and using protective coatings or material removal to minimize OH gradients.

Benefits of technology

This approach significantly reduces image defects by ensuring uniform thermal expansion, maintaining mirror surface integrity under high radiation power, and enhancing imaging quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535801000001_ABST
    Figure 2024535801000001_ABST
Patent Text Reader

Abstract

The invention relates to an optical element (M2) for reflecting radiation, in particular EUV radiation (16), comprising a substrate (31) made of quartz glass, in particular titanium-doped quartz glass or of glass ceramic, comprising a first partial body (26a) and a second partial body (26b) joined to one another along a bonding surface (27) by thermal bonding, a plurality of cooling channels (25) extending into the substrate (31) in the region of the bonding surface (27) and separated from one another by lands (35), and a reflective coating (33) applied to a surface (32) of the first partial body (26a). In the substrate, each cooling channel (25) is located at at least one position (P) adjacent to each land (35). S ) at the center (M) of the land (35) over the entire sidewall portion (36c, 36d) adjacent to each land (35), ZC,M ) deviating from the zero cross temperature (T ZC,S The invention also relates to an optical device, in particular an EUV lithography system (1), comprising at least one optical element (M2) designed as described above.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [Reference to Related Applications] This application claims priority from German Patent Application No. 10 2021 210 093.7, filed on September 13, 2021, the entire disclosure content of which is incorporated herein by reference.

[0002] The invention relates to an optical element for reflecting radiation, in particular EUV radiation, comprising a substrate made of quartz glass, in particular titanium-doped quartz glass or of a glass ceramic, a first partial body and a second partial body joined along a bonding surface by thermal bonding, a plurality of cooling channels extending into the substrate in the region of the bonding surfaces and separated from one another by lands, and a reflective coating applied to the surface of the first partial body. The invention also relates to an optical device, in particular an EUV lithography system, comprising at least one such reflective optical element. [Background technology]

[0003] In EUV lithography systems in the form of EUV lithography apparatus, reflective optical elements in the form of mirrors, in particular mirrors of the projection system, are subjected to high radiant powers, which leads to heating of the mirrors and thus of the mirror substrate. Heating of the substrate leads to deformation of the surface of the substrate provided with a reflective coating (i.e. of the mirror surface). The deformation leads to image defects that impair the imaging quality of the projection system. To address this problem, the substrates used for EUV mirrors usually consist of materials with a low coefficient of thermal expansion. Titanium-doped quartz glass, for example sold under the trademark ULE® by Corning, and certain glass ceramics, such as Zerodur®, have a particularly low coefficient of thermal expansion and are therefore suitable for the manufacture of substrates for EUV mirrors.

[0004] A known method of reducing the temperature of the mirror is to introduce cooling channels in the substrate through which a cooling fluid flows. The production of the cooling channels usually requires the introduction of through channels in the substrate, the through channels having a geometric shape depending on the respective mirror. The processing of the substrate for the production of the cooling channels may cause stresses in the glass material, which may also have an undesirable effect on the shape of the mirror surface during the final formation of the mirror, since these stresses may lead to unexpected shape changes during, for example, milling or polishing of the mirror surface.

[0005] Patent document 1 describes a method for manufacturing a glass body having a plurality of cooling channels, which includes the steps of providing a first and a second partial body of a glass body, forming at least one cooling channel by processing, in particular machining, a glass material on a surface of the first partial body and / or the second partial body, and manufacturing the glass body by joining the first partial body to the second partial body at the processing surface by high-temperature bonding.

[0006] In the high-temperature or thermal bonding described in US Pat. No. 5,999,222, two halves are joined along the bonding surface and generally heated to a temperature of at least about 1000° C. or higher. The two halves are here bonded along the bonding surface without the use of a bonding agent. At lower heating temperatures, the required adhesive strength of the halves or adherends is generally not achieved. In the case of bonding by high-temperature bonding, the two halves are first pressed against each other along the subsequent bonding surface and then heated to the temperature required for high-temperature bonding. Alternatively, the two halves can be heated separately and only brought into contact with each other along the bonding surface at high temperature.

[0007] For example, as is known from Non-Patent Document 1 (hereinafter "Bruckner II"), when a quartz glass body is subjected to high-temperature treatment at temperatures of about 700 ° C or higher, OH groups diffuse out of the quartz glass body. As a result, the OH content of the quartz glass is reduced in a depletion zone starting from the surface of the quartz glass body and extending into a volumetric region near the surface. The near-surface volume forming the depletion zone may extend several millimeters or centimeters into the volume of the quartz glass body during prolonged heat treatment, with one effect being a higher refractive index of the volumetric region near the surface relative to the volumetric region closer to the center of the quartz glass body.

[0008] It is also known that the lower the OH content in a quartz glass, the higher the viscosity at a given temperature in general. As a consequence, the glass matrix in quartz glasses with low OH content does not anneal well with conventional tempering programs and therefore the fictive temperature cannot be set to as low a level as is possible for OH-rich quartz glasses. For example, it is known from the company brochure, Non-Patent Document 2, that dry quartz glasses with glass codes 7979 or 8655, which have an OH content of less than 1 ppm, have a refractive index at a wavelength of 194 nm that is about 65 ppm higher than glasses with a higher OH content, which is a result of the higher fictive temperature and lower OH content.

[0009] This is also the case for titanium-doped quartz glass, with the result that for a comparable titanium content and a comparable tempering program, the zero-cross temperature of the quartz glass material and the slope of the thermal expansion coefficient as a function of temperature remain at a higher level for OH-poor quartz glass compared to OH-rich quartz glass. Furthermore, there is a direct dependence between the OH content of the (titanium-doped) quartz glass and the thermal expansion coefficient and the zero-cross temperature, which dependence usually dominates.

[0010] The effect of the OH content on the properties of quartz glass has been investigated in particular in Non-Patent Document 3 and Non-Patent Document 4. In particular, the diffusion constants for the diffusion of OH groups in quartz glass have been reported in Non-Patent Document 5 (hereinafter "Bruckner I") and in the paper "Bruckner II".

[0011] US Pat. No. 5,399,633 describes a substrate for an EUV mirror with a zero-cross temperature profile that deviates from the statistical distribution. The zero-cross temperature profile is adapted to the operating temperature of the mirror. The substrate material is titanium-doped quartz glass produced by the soot method. The zero-cross temperature profile and the OH content profile are mutually dependent and correspond. In one example, the zero-cross temperature changes by an order of magnitude of about 1 K when the OH content is reduced from 200 ppm by weight to 170 ppm by weight. The fictive temperature also changes depending on the OH content and is about 970° C. for a temperature process with a cooling rate of 4 K / h when the OH content in the bulk of the quartz glass is 180 ppm by volume.

[0012] Patent Document 3 discloses a method for annealing or tempering silicon dioxide-titanium dioxide glass. The tempering method is for enabling independent adjustment of the zero cross temperature and the slope of the temperature dependence curve of the thermal expansion coefficient. According to Patent Document 3, when the OH content in the bulk of the quartz glass is about 850 ppm by weight and the cooling rate of the tempering process is about 3 K / h, the fictive temperature is less than about 950° C.

[0013] US Patent No. 4,363,336 describes a method for forming a zero cross temperature gradient in a silicon dioxide-titanium dioxide glass article, in which a temperature gradient is formed through the glass article and the glass article is cooled at a predetermined cooling rate to form a zero cross temperature gradient across the thickness of the glass article.

[0014] As mentioned above, in the high-temperature treatment or tempering process, the OH content in the depletion zone formed at the edge of the (titanium-doped) quartz glass body is less than in the bulk, where a (maximum) OH content of about 850 ppm by weight is usually obtained for directly deposited glasses (see Patent Document 3), or about 180 ppm by weight for glasses produced by the soot process (see Patent Document 2). The thickness of the depletion zone at the edge of the quartz glass can be expressed, for example, by the distance from the edge or from the outer surface at which the OH content drops to a certain percentage of the maximum OH content, for example 50%, or the distance at which the OH content deviates from the maximum OH content by a certain absolute value. The thickness of the depletion zone depends on factors including the holding temperature, holding time, and heating and cooling ramps in the tempering process, as well as the atmosphere of the tempering furnace and the composition of the workpiece, and can be tens of micrometers to several millimeters, as mentioned above.

[0015] If the substrate material contains hydrogen, as is generally the case in the case of direct deposition and homogenization processes in hydrogen / oxygen gas flames, hydrogen depletion will also occur in the depleted zones and will proceed more rapidly than the depletion of OH groups. If the tempering process is carried out in a reducing atmosphere, this will also result in the formation of oxygen deficiency defects (=Si or Si-Ti bonds) or TI 4+ From Ti 3+ In addition, sodium from the treatment agent may diffuse into the quartz glass, which may affect the coefficient of thermal expansion. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] International Publication No. 2020 / 207741 [Patent Document 2] U.S. Pat. No. 10,732,519 [Patent Document 3] European Patent No. 3 044 174 [Patent Document 4] European Patent No. 3 110 766 [Non-patent literature]

[0017] [Non-Patent Document 1] “Properties and Structure of Vitreous Silica. II” by R. Bruckner, Journal of Non-Crystalline Solids 5 (1971) 177-216 [Non-Patent Document 2] internet <URL: https: / / www.corning.com / media / worldwide / csm / documents / HPFS_Product_Brochure_All_Grades_2015_07_21.pdf> [Non-Patent Document 3] “Der strukturmodifizierende Einfluss des Hydroxylgehaltes in Kieselglasern” [The Structure Modifying Effect of Hydroxyl Content in Silica Glasses] by Rolf Bruckner, Glastechn. Berichte, page 8ff., 1970 [Non-Patent Document 4] “Der Einfluss des Hydroxylgehaltes auf die Dichte und auf den Diffusionsmechanismus in Kieselglasern” [The Effect of Hydroxyl Content on Density and on the Mechanism of Diffusion in Silica Glasses] by Rolf Bruckner, Glastechn. Berichte, page193ff., April 1965 [Patent Document 5] “Properties and Structure of Vitreous Silica. I” by R. Bruckner, Journal of Non-Crystalline Solids 5 (1970) 123-175 Summary of the Invention [Problem to be solved by the invention]

[0018] An object of the present invention is to reduce image defects during operation of an optical element that are caused by gradients in OH content induced by thermal bonding. [Means for solving the problem]

[0019] This object is achieved by an optical element of the aforementioned type, in which each cooling channel has a channel wall which, at at least one location adjacent each land, and in particular over the entire side wall portion adjacent each land, has a zero cross temperature which deviates from the zero cross temperature in the centre of the land by less than 3.0 K, preferably less than 2.0 K, in particular less than 1.0 K.

[0020] The comparison of the zero cross temperature at the location on the channel wall adjacent to each land with the zero cross temperature at the center of the land is performed in a plane extending laterally, i.e. perpendicular to the thickness direction of the substrate. It will be clear that the channel side walls adjacent to the lands will usually have a zero cross temperature that deviates from the zero cross temperature at the center of the land by less than the above value, and not only at a single location adjacent to each land. In particular, the above condition may be satisfied along the entire side wall, i.e. at all locations on the side wall. However, for the reduction of image defects, it may be sufficient if the above condition is satisfied only along a part of the side wall. In particular, the above condition of the zero cross temperature does not necessarily have to be satisfied in the corner areas where the side wall adjoins the upper and lower wall parts of the channel wall.

[0021] In one embodiment, the flow path wall, at least at one location facing the reflectively coated surface, in particular over the entire upper wall portion facing the surface, has a zero cross temperature that deviates from the zero cross temperature of the surface by less than 3.0 K, preferably less than 2.0 K, in particular less than 1.0 K.

[0022] Since the thickness of the first portion typically varies laterally between the top wall of the cooling passage and the surface, a comparison of the zero cross temperature at each location on the top wall of the passage wall to the zero cross temperature at the surface is made at the same lateral location.

[0023] It will be clear that the top wall of the channel will usually have a zero cross temperature that deviates from the zero cross temperature of the reflectively coated surface by less than the above value, and not only at a single location. In particular, the above condition may be fulfilled along the entire top wall, i.e. at all locations on the top wall. However, for the reduction of image defects, it may be sufficient if the above condition is fulfilled only along a part of the top wall. In particular, the above condition of the zero cross temperature does not necessarily have to be fulfilled in the corner regions where the top wall adjoins each side wall of the channel wall.

[0024] As mentioned above, thermal bonding results in OH depletion of the glass material of the substrate near all outer surfaces of the glass bodies joined in the thermal bonding operation, and therefore also at the channel walls of each cooling channel. The inventors recognized that the concentration gradient near the channel walls that occurs during outward diffusion of OH groups affects the zero cross temperature of the thermal expansion coefficient of the substrate to such an extent that the mirror surface deforms and image defects occur during operation of the optical element.

[0025] Due to the OH concentration gradient, it may be possible that the tempering program will affect whether the substrate generates a zero cross temperature that is higher or lower than the undisturbed glass in the glass body. Because of the concentration gradient, it is virtually impossible to select a temperature program that results in the same behavior of the thermal expansion coefficient and zero cross temperature for the undisturbed glass and all the OH concentrations that occur.

[0026] Another effect of OH deficiency is that, for the same tempering program, the fictive temperature is higher and therefore the slope of the thermal expansion coefficient as a function of temperature at or near the channel wall is larger. Thus, when the mirror is heated by a localized thermal load in its region, the difference in expansion between the low-OH region and the surrounding material increases with the heating intensity. This nonlinear behavior as a function of the heat input can pose special challenges to the compensation of the resulting image defects, especially since it increases proportionally to the temperature difference or the square of the heating. It should be noted here that the effect of OH deficiency generally increases with the operating temperature, since conventional polishing and measurement methods are performed at room temperature (22° C.). Thus, ridges or grooves above the cooling channels are compensated at room temperature and only reappear at operating temperatures that are significantly different from room temperature.

[0027] Depending on the tempering program used and the local temperature relative to the mean zero cross temperature of the substrate, the OH deficiency leads to circumferential tensile or compressive stresses. Here we assume that compressive stresses arise. The unconstrained depleted zone becomes less dense than the surrounding material. This firstly leads to an expansion of the glass material into the cooling channels, which has no significant negative effects, and secondly leads to a protuberance of the reflectively coated surface above the cooling channels. This is particularly problematic, since machining of this surface is generally not possible at the subsequent operating temperatures of the mirror (see above), and corrections cannot completely remove these protuberances. In terms of strength, low drift of the joint, and controllability of the zero cross temperature, a higher bonding temperature and / or a longer hold time is preferred, the effect being even more pronounced at higher bonding temperatures, since the diffusion constant of OH groups increases with temperature (see figure 36 in "Bruckner II").

[0028] The substrate of the mirror described herein has a relatively small lateral gradient in zero cross temperature and a relatively small gradient through the thickness of the substrate above the cooling channels, so that the prominence of the above-mentioned reflectively coated surface is relatively small. At the lower channel wall, the effect of the zero cross temperature gradient on the surface is relatively small, so there is generally no need to follow the constraint on the zero cross temperature there.

[0029] In principle, however, it is preferred that the cooling channels have a zero cross temperature along the entire channel wall that deviates from the average zero cross temperature of the bulk of the substrate by less than 3.0 K, preferably less than 2.0 K, in particular less than 1.0 K. In this case, the zero cross temperature is averaged over all positions in the bulk of the substrate at a distance of less than 1 cm from the surface provided with the reflective coating. In the lateral direction, the averaging is performed over all positions in the bulk of the substrate up to a lateral distance of 1 cm below the optically utilized area of ​​the reflective coating in the thickness direction. The optically utilized area refers here to a sub-area of ​​the reflective coating that makes the imaging light further usable after reflection.

[0030] As mentioned above, the zero cross temperature is strongly influenced by the OH content of the substrate, but may also be influenced by other effects. For example, hydrogen or oxygen deficiency would produce a similar concentration profile, or the inward diffusion of metals, e.g., sodium, would produce an inverse profile. Sodium in particular diffuses particularly rapidly. See, e.g., U.S. Pat. No. 9,382,151.

[0031] In yet another aspect of the invention, which can in particular be combined with the above aspects, each cooling channel has a channel wall, at at least one location adjacent each land, in particular over the entire sidewall adjacent each land, which has an OH content that deviates by 60 ppm by weight or less, preferably 30 ppm by weight or less, in particular 20 ppm by weight or less, from the OH content in the center of each land.

[0032] In one embodiment of this aspect of the invention, the flow channel wall, at at least one location facing the reflectively coated surface, in particular over the entire upper wall portion facing the surface, has an OH content that deviates from the OH content of the surface by no more than 60 ppm by weight, preferably no more than 30 ppm by weight, in particular no more than 20 ppm by weight.

[0033] As mentioned above, the OH content of the glass has a large influence on the zero cross temperature and therefore on the deformations occurring on the surface of the mirror at the operating temperature. By complying with the conditions stated here for the OH content in the lateral or thickness direction, it is usually possible to comply with the above conditions for the zero cross temperature of the substrate in the lateral and thickness directions, and thus to significantly reduce image defects during operation of the optical element.

[0034] It has been found that even a small difference in the OH content of the quartz glass, for example 30 ppm, can cause a change in the zero cross temperature of about 1 K, i.e., the effect of small variations in the OH content on the zero cross temperature is quite large. Thus, a significant reduction in the OH content, for example from a maximum value of 180 ppm or 850 ppm by weight to 0 ppm by weight, has a serious effect on the zero cross temperature, even if the thickness of the depletion zone is only a few micrometers.

[0035] If the two parts are heated separately in a thermal bonding process and only bonded at high temperatures, there is usually also an OH deficiency of the substrate material on either side of the bonding surface where the two parts are joined, since the surfaces of the two parts along which the subsequent bonding surface extends lose OH groups before bonding. However, the OH deficiency along the bonding surface is not very detrimental, since any OH inhomogeneity there or any inhomogeneity in the thermal expansion coefficient leads essentially to a constant lateral variation in the thickness of the substrate. Moreover, this inhomogeneity after bonding is largely compensated for by the diffusion of OH groups from the substrate to the depleted area.

[0036] In contrast, in a thermal bonding process where the two sections are pressed together before heating, an increased concentration of OH groups and HO linked via hydrogen bonds is expected, which can diffuse into the material during subsequent hot processing. It is also expected to result in layers with different thermal expansion coefficients, which are relatively small in effect except at the edges close to the cooling channels, where lateral OH gradients are also possible.

[0037] In one embodiment, the flow channel wall has an OH content of greater than 0 ppm by weight, preferably greater than 60 ppm by weight, in particular greater than 120 ppm by weight at at least one location adjacent the land, in particular across the side wall, and / or at least one location opposite the surface, in particular across the top wall.

[0038] The furnaces in which the thermal bonding process is usually carried out are operated with vacuum, air or inert gas with sufficient circulation, so that the environment of the glass body formed during the joining of the two parts in the furnace is at zero water vapor pressure. Therefore, due to the above-mentioned outward diffusion of OH groups without the barrier action according to "Bruckner II", the OH content of the channel walls is 0 ppm by weight, i.e. the channel walls have a negligible OH content. There are various ways to increase the OH content of the channel walls and thus reduce the gradient of the OH content compared to the average OH content in the bulk of the substrate, some of which are described below.

[0039] To reduce the OH gradient, for example, substrate material can be removed from the channel walls of the cooling channels. The thickness of the removed region depends on the thickness of the depletion region and the OH gradient that can be tolerated in the material of the substrate with respect to image defects. Since the gradient of OH content increases with the maximum OH content of the substrate, the thickness of the removed region depends in particular on the magnitude of the average or maximum OH content of the substrate.

[0040] There are various options for removing material.

[0041] The cooling channels can be treated after bonding, for example with an abrasive emulsion or an etchant. The emulsion must in any case be rinsed under pressure. In the case of the etchant, periodic replacement or stepwise rinsing is also desirable to avoid over-etching at the inlet and outlet of each cooling channel. However, both methods result in roughening of the channel walls on the inside, leading to uneven removal, for example in curved regions of the channel. For depletion areas with large thicknesses, requiring removal of more than 1 mm, this method becomes impractical.

[0042] It is also possible to use hot phosphoric acid as etchant instead of standard hydrofluoric acid, which is much less toxic and has a slower etching rate. This has the advantage that the cooling channels with hoses attached by flange connections can be purged for longer periods, which is not possible with hydrofluoric acid for work safety reasons. It is also possible to spatially control the etching effect by suitable pre-damage, for example with a short-pulse laser. Pre-damage can be performed in the open cooling channels or in the machined recesses before joining the two parts, or on the surface that will be provided with a reflective coating at a later stage before thermal bonding. It is also possible to control the etching operation in situ by ultrasonic treatment. The subsequent exposure or sonication through the mirror surface improves the removal, preferably in the upper side and upper regions of the channel side walls of the cooling channels. As mentioned above, these are precisely the areas where non-uniformities in the thermal expansion coefficient or zero cross temperature are particularly problematic. The heat load removed at the mirror surface during operation of the mirror results in the largest temperature increase at the top surface or upper channel wall of the channel and continues to decrease with increasing depth, so that there is still little temperature increase at the bottom surface or lower channel wall of the channel.

[0043] It is also possible to use alkalis as etchants, especially with pre-damage. It is known that for quartz glass, short-pulse laser pre-damage with 8 molar KOH at 80 °C with ultrasound can achieve an etch rate of 300 μm / h. The etching selectivity is 1:1400, i.e. without pre-damage only 0.2 μm / h is achieved in the worst case. For 100 μm of material removal, that means 3 weeks, a tolerable time for material removal, especially since the etch rate of titanium-doped quartz glass may be slightly higher. Alternatively, it is possible to increase the temperature and concentration of the alkali somewhat, since the boiling point of a particularly concentrated alkali should be well above 100 °C (the boiling point of a 50% sodium hydroxide solution is 143 °C, and that of a 45% potassium hydroxide solution is 136 °C). Exceeding the boiling point would require a pressure vessel, which would only increase the complexity of the equipment. Of course, since there is no intention to achieve etching selectivity, it is possible to go more aggressive with regard to the etching parameters without pre-damage.

[0044] Moreover, OH-deficient quartz glass is much more likely to have a higher etch rate than non-deficient quartz glass, since OH acts as a matrix stopper, i.e., it increases the freedom of the glass matrix since bridging at the tetrahedral vertices with neighboring tetrahedra according to bond angles is not necessary. In the case of OH outdiffusion, it is unlikely that two defects will combine to form a covalent bond, i.e., these defects can be considered as preliminary damage. In that case, the depleted zone is removed almost autonomously, i.e., regardless of the flow conditions in the case of active purging with the etchant. In this case, an acid may be more effective than an alkali, since the alkali replenishes the missing OH. On the other hand, the acid donates protons, which can also act as a matrix stopper.

[0045] Generally, the use of slow etchants (phosphoric or alkaline) is advantageous for material removal because the relatively low etch rates can handle very low flow rates and therefore do not suffer from the problem of maximum etch removal occurring at high flow sites.

[0046] It is also possible to use gaseous etching media, for example the evaporated gases from concentrated hydrofluoric acid or fluorinated organic substances such as those used in the fluorine doping of soot glass.

[0047] It will be clear that during the production of the substrate from the glass body formed by thermal bonding, the deficient zone is usually removed on the surface with the reflective coating and also on the opposite side at the bottom of the glass body or the second part. The surface of the first part with the reflective coating and the bottom of the second part are easily accessible, which allows for a simpler removal of the deficient zone. However, the material of the first part in particular must be of very high quality in terms of homogeneity and bubble-freeness. Removal of a few millimeters or centimeters quickly reaches a limit both in terms of costs and in terms of the possibility of producing a high-quality glass block of suitable weight.

[0048] In mechanical removal methods, rotating brushes or sponges can also be introduced into the cooling channels, as can purging with an abrasive emulsion. Dry grinding particles or grinding fluids with maximum density difference between the fluid and the particles can also be introduced. The particles can be agitated by ultrasound or by vibration of the entire glass body by a shaker. It is also possible to use ferromagnetic particles and an external magnetic field. The external field can be an alternating magnetic field to vibrate the particles. Alternatively, the field can be a quasi-static moving magnetic field, in which case the vibration is additionally generated by a shaker. This has the advantage that the location and direction of material removal can be controlled, i.e. for example, unwanted increases in removal in areas of high moving speed can be suppressed.

[0049] Furthermore, material removal can occur, for example, by the generation of cavitation bubbles in the liquid, which can be generated, for example, by focused ultrasound, electrical discharges or laser pulses. If the liquid simultaneously has an etching effect, locally controllable material removal is thus possible.

[0050] In yet another embodiment, the depletion region adjacent the channel wall, where the OH content of the substrate is at least 5 ppm by weight less than the OH content of the center and / or surface of each land, has a thickness of less than 50 μm, preferably less than 30 μm, especially less than 1 μm. As discussed above, the thickness of the depletion region can be reduced by removing material from the channel wall. The thickness of material removed and the thickness of the depletion region will vary depending on factors including the steepness of the gradient in the OH content of the substrate.

[0051] As mentioned above, it can be said that generally, the greater the difference between the operating temperature of the mirror and the polishing temperature at which the ridges or grooves above the cooling channels are corrected (usually 22°C), the greater the degree of OH deficiency that is problematic. Therefore, the higher the operating temperature, the greater the material removal required. The tolerable residual OH content of the depleted area is therefore inversely proportional to the difference between the polishing temperature and the operating temperature. For a polishing temperature of 22°C and an operating temperature of 25°C, it may be sufficient to remove the depleted area by 0% to 20% of the average OH content in the bulk of the substrate. For an operating temperature of 35°C, removal of 0% to 90% of the average OH content in the bulk of the substrate may be required. Thus, in the first case, the thickness of the depleted area remaining after material removal will be greater than in the second case. The thickness of the removed material also depends on the absolute value of the OH content in the substrate. For an operating temperature of 25°C and a maximum OH content of the substrate of about 200 ppm by weight, it is generally sufficient to remove material within the range of 0% to 20% of the maximum OH content. For a maximum OH content of 800 ppm by weight, typically material having an OH content between 0% and 50% by weight of the maximum OH content needs to be removed at the channel walls, i.e., correspondingly more material needs to be removed.

[0052] In yet another embodiment, the OH content of the channel walls deviates from the average OH content in the bulk of the substrate (i.e. outside the channel walls) by less than 10%, preferably less than 5%, in particular less than 1%.

[0053] In the above-mentioned embodiment, OH deficiency occurs in the volume region adjacent to the channel wall, i.e. the OH content is reduced compared to the OH content in the bulk of the substrate. Alternatively, it is possible in principle for the average OH content of the substrate in the region adjacent to the channel wall to be higher than the average OH content of the substrate. This may be the case if the thermal bonding is carried out under suitable ambient conditions, in particular in saturated water vapor, and / or if a post-treatment of the substrate or glass body formed by thermal bonding is carried out. It should be noted here that an increase in the OH content over the average OH content also leads to an undesirable OH gradient, which should be avoided.

[0054] The average OH content of the substrate or substrate material can be determined, for example, by FTIR or IR spectroscopy or Raman spectroscopy. The ideal OH content for the thermal bonding process or post-treatment can be calculated if the diffusion coefficient is known, and the water vapor partial pressure can be adjusted accordingly. For the device, the correct partial pressure can be achieved by limiting the water injection, adding dry air, or by appropriate suction resulting in reduced pressure. Since the diffusion ratio decreases at low temperatures, it is usually necessary to track and reduce the water vapor partial pressure during the cooling stage of the thermal bonding process, possibly according to a pre-calculation. Thermal bonding or post-treatment with water vapor can have the effect that, especially in the case of soot-deposited (titanium-doped) quartz glass, the OH content of the channel walls or of the areas adjacent to the channel walls deviates from the average OH content in the bulk of the substrate by only about 10%, 5%, or possibly 1%.

[0055] One factor that is fundamentally opposed to thermal bonding with water vapor is that when the hydrogen-bonded SiOH groups are converted to Si-O-Si matrix bonds, surface water and condensed water cannot easily diffuse outward, even laterally, from the bonding surface.

[0056] A factor opposing post-treatment by subsequent replenishment of OH groups in the form of heat treatment with saturated steam or water is that the post-treatment process takes at least as long as the original thermal bonding, during which other material properties may change, for example the coefficient of thermal expansion. Moreover, it is generally not possible to directly compensate for the deficiency profile of the OH content, since it is not easily detectable by measurements, especially on the micrometer scale. A further factor is that such a process, which generally must be carried out at a lower temperature than bonding, is very time-consuming, since according to FIG. 36 and section 5.1.3.2 of the paper "Bruckner II", outward diffusion has a diffusion constant significantly larger than inward diffusion (see above). In either case, the maximum partial pressure of water or water vapor should be used at any temperature, since the solubility increases proportionally to the square of the vapor pressure.

[0057] It has been found that a combination of replenishment of OH groups with a time-delayed supply of water vapor with thermal bonding is preferred. In this case, thermal bonding is first started under dry conditions, a holding step for several hours or days at 120°C-250°C is carried out for the outward diffusion of surface water, and possibly a further holding step for several hours at 500°C-600°C is carried out for the outward diffusion of concentrated water, after which water vapor is added. According to "Bruckner II", the rate of outward diffusion at low temperatures is still moderate, so that replenishment can be carried out efficiently during the holding step of thermal bonding, which is required in any case. Thus, the outward diffusion of OH groups can usually be significantly reduced, especially if the tempering step at the highest temperature in thermal bonding is carried out with maximum saturated water vapor.

[0058] If this is not practical, at least an oxidizing atmosphere should be used in the thermal bonding operation. At the surface of the part where the bonding surface is to be formed, there are unsaturated Si and Ti bonds, as well as unsaturated Si-O and Ti-O bonds, and also the saturated forms SiH and TiH and Si-OH and Ti-OH, where in particular OH groups predominate in standard atmosphere. Therefore, if the surface is previously exposed to atmosphere, OH groups predominate. OH groups can only become water if hydrogen is supplied, which diffuses from the substrate or glass body or leaves the furnace. In an oxidizing atmosphere, such hydrogen is directly oxidized to water vapor and therefore cannot bind to OH groups. In a reducing atmosphere, the residual water can react with auxiliary materials such as the furnace wall or mold (often made of graphite), which releases hydrogen. The oxidizing atmosphere therefore forms an artificial exit barrier for OH groups at the surface. As a result, the concentration profile is no longer determined only by the volume diffusion coefficient, but a non-zero concentration is established at the surface.

[0059] Regarding the question of which parameters are necessary for bonding or post-treatment in saturated water vapor, the solubility of OH groups is important. According to "Glass Science" by RH Doremus (2nd ed., Wiley, New York 1994, pages 198-199), the solubility of quartz glass in the range of 700 °C to 1200 °C is 3 × 10 per SiO2 group at a vapor pressure of 700 mmHg. -3 The SiOH group. This, and also the paper "Water in Silica Glass" (AJ Moulson and JP Roberts, Trans. Faraday Soc., 1961, 57, 1208-1216) state that the solubility increases as the square of the vapor pressure. Converting to mass numbers (OH is 17, SiO2 is 60), the solubility of OH is 850 ppm, which corresponds to the typical OH content of direct deposition silica glass or titanium-doped silica glass. In the production of these glasses, the growth rate of new glass is faster than the rate of outward diffusion of OH groups, so the outward diffusion of OH groups does not need to be considered.

[0060] However, in the thermal bonding operation, no new glass is deposited. In other words, outward diffusion must be considered. A partial pressure of water vapor close to 100% for direct deposition glass and about 25% for soot glass with 200 ppm OH content allows for replenishment of OH groups or prevention of outward diffusion. With regard to the equipment, the appropriate vapor pressure can be achieved by using an evaporation dish or water injection and by closed-loop control of the fresh gas purge and the ratio of air inlet to air outlet pressure. At a partial pressure of about 100%, it is possible to eliminate the purge or reduce the purge level and use a pressure relief valve. The actual bonding can also be performed in a humid atmosphere.

[0061] In carrying out the thermal bonding process, in both cases, i.e. in the case of directly deposited quartz glass and in the case of quartz glass deposited by the soot method, only a small and tolerable decrease in the OH content occurs, so that it is possible to eliminate material removal from the channel walls.

[0062] In yet another embodiment, the channel walls are preferably at least partially, in particular completely, covered with a metallic protective coating to prevent the outward diffusion of OH groups. Usually, any kind of metallic layer or coating significantly inhibits the outward diffusion of OH groups. A suitable metal should have a melting point above the highest process temperature of the thermal bonding operation. In particular, chromium has good applicability and structure forming properties and a sufficiently high melting point.

[0063] It should be noted that in the case of a protective coating in the form of one or more layers applied to the unbonded parts, a cleaning operation is still necessary before bonding, especially in the case of crimping. Materials and / or cleaning processes should therefore be selected in such a way that the protective coating or its layers are not attacked.

[0064] Ideally, each cooling channel is metallized over the entire extent of the channel wall, possibly over the subsequent mirror area, or over the entire surface of the glass body or parts exposed to the atmosphere during thermal bonding. A sufficient number of methods are known for metallizing nonconductors, but the requirement of an internal coating of the cooling channels somewhat limits the options. Possible methods include sputtering deposition, initial deposition from the gas phase or from a liquid after an initial etching. As soon as a so-called primer layer is applied, a thicker layer of another metal is also electrolytically deposited. It is possible that the primer layer is applied before thermal bonding and the thick layer is applied only after thermal bonding.

[0065] In principle, the protective layer could remain in each cooling channel after thermal bonding, but it could also be removed again by etching or electrolysis after thermal bonding, for example due to its effect on the thermal expansion coefficient.

[0066] As mentioned above, the entire channel walls of the cooling channels can be covered with the protective coating, but it is also possible that only the top and side walls of the cooling channels are covered completely, or optionally only partially (see below), with the protective layer. Such a protective coating can be applied particularly simply if the first section is recessed and the second section is not, so that the cross section of the cooling channels is entirely within the first section. The first section can then be completely covered on the surface that will form the subsequent bonding surface, including the cooling channels or recesses that remain open. A grinding or polishing step removes the metal layer so that at the subsequent bonding surface, open cooling channels remain that are three-sidedly covered. In this case, the second section can remain uncoated or only covered in the areas that will later become the cooling channels.

[0067] As mentioned above, the layer applied before bonding, which may be masked or of different structure, may be very thin and may only serve as a primer for electroplating or chemical deposition from a solution after thermal bonding. This causes the layer to grow in thickness, but also laterally along the covered surface(s). If the metallization in the area where the cooling channels are not provided (the second part in this example) is only a few tens of micrometers narrower than the channel width, this lateral growth may be sufficient to close the gap and provide a metallic protective coating on the entire channel wall.

[0068] For ground and possibly etched cooling channels, the surface roughness Ra at the channel walls may be expected to be 5 μm to 10 μm. In particular, when metallization is applied by evaporation or sputtering, it may be expected that the valleys of the rough topography will not be completely filled. Again, subsequent electroplating or chemical deposition may be effective in filling these gaps.

[0069] The seamless metallization method can of course also be used if the channels are integrated into the second section and the first section acts as a lid closing the cooling channels.

[0070] As mentioned above, in the thermal bonding process, there may also be an inward diffusion of sodium and other metals. This undesirable inward diffusion can be reduced by measures known from quartz glass for 193 nm applications, such as acidifying the workpiece, using especially high purity or halogen-free auxiliary materials, suitable furnace linings, and cooling of the metal surface. Furthermore, the above-mentioned metal protective coatings, especially the use of chromium or with the above-mentioned material removal after thermal bonding, act against high concentration gradients of metals close to the surface.

[0071] It may be advantageous if the metallization or metal protective layer has well-defined interruptions (e.g. slots), since the metal layer has a different coefficient of thermal expansion than the glass and therefore stresses are introduced into the surrounding glass during tempering and are frozen in, only partially relieved upon removal of the metal layer. These stresses are constant over the life of the mirror and vary only slightly with temperature, but this may lead to stress effects at the mirror surface, for example in the form of selective material removal, if they cause birefringence locally in the range of a few tens of nm / cm.

[0072] In one embodiment, the channel wall has a number of corner regions, and only the outside of the corner regions are covered with the protective coating. The cooling channel generally has a substantially rectangular cross-section with a channel upper portion, a channel lower portion, and two channel sides, each adjacent to a corner region. However, in principle, different cross-sectional shapes are possible, with more or fewer corners, or even no corners, as for example in the case of cooling channels with a circular cross-section.

[0073] The protective coating can cover each channel cross section except the corners. In that case, there will be local OH deficiencies in the corner regions. However, these corner regions will be insulated, so that in this case, unlike the case of annular or tubular deficiencies, it is possible to generate much smaller temperature-dependent forces that lead to bending of the glass above the cooling channels.

[0074] In yet another development, the channel walls are not covered with the protective coating along slots that run in the longitudinal direction of the cooling channel, preferably obliquely to the longitudinal direction. For example, the channel sides or side walls of the cooling channel can have oblique slots in the protective coating. This reduces the forces due to the protective coating in the longitudinal direction of the cooling channel. The slots can also continue, for example, in a spiral or other form, over all the walls of the cooling channel.

[0075] After the bonding of hydrophilic glass surfaces, one or more water monolayers remain on the subsequent bonding surface, which prevents the formation of the desired covalent bonds in the bonding operation. Normally, water molecules can diffuse along the bonding or bonding surface during the heating process. However, if a continuous metallization of the bonding surface, including the open side of the bonding surface, is formed before the bonding operation, this outward diffusion is suppressed and only a very slow diffusion of water remains in the substrate. In order to drive the water out of the gaps, it can be advantageous to bake the bonded parts that are not yet metallized or are not yet seamlessly metallized at 100° C. to 400° C. for several hours to weeks. Only afterwards is it possible to metallize the inside of the channels or thicken the masked partial metallization, including closing the notches.

[0076] In yet another embodiment, the first partial body, preferably the entire substrate, has a maximum OH content of less than 10 ppm by weight. The smaller the absolute value of the OH content, the smaller the gradient of the OH content obtained after thermal bonding. The gradient of the zero cross temperature in the substrate is therefore also reduced, and thus the deformation of the surface with the reflective coating or the image defects occurring during operation of the optical element at the operating temperature are also reduced. To achieve such a low OH content, the OH content of the quartz glass can be reduced by suitable thermal drying or chemical drying (e.g. by halogen). Chemical drying can only be carried out before sintering in the soot method, while thermal drying can be carried out before sintering or after sintering, but thermal drying after sintering is much more time-consuming. In the course of thermal drying, the two partial bodies can be tempered individually or collectively at temperatures above 1400 ° C, preferably above 1600 ° C, for several days or weeks before joining by thermal bonding. Since the recesses forming the cooling channels at a later stage change shape at the temperature at which the thermal drying is carried out, it is not necessary or less preferred that these are already introduced into each part for drying. By the above-mentioned chemical or thermal drying, it is possible to produce quartz glass with an OH content of less than 1 ppm by weight.

[0077] In yet another aspect of the invention, which can be combined in particular with the above-mentioned aspects of the invention, the channel wall of each cooling channel has at least one slot-like recess, preferably with a depth at least equal to the thickness of the depletion region, more preferably at least twice the thickness of the depletion region. The slot-like recess(es) have a width of less than 100 μm and are introduced in at least one of the halves before thermal bonding. The depth of the slot-like recess should be 1, 2 or 5 times, but generally not more than 5 times, the thickness of the depletion region, where the depletion region is defined as an area with an OH content at least 5 ppm by weight less than the OH content of the center or surface of each land, as described above. The OH depletion during thermal bonding spreads to the slot-like recess, but the ring formed by the depletion region (based on the cross section of the cooling channel) or the tube (based on the entire cooling channel) is weakened, reducing the temperature-dependent bowing or indentation above the cooling channel. If the slot-like recesses are flow unfavorable ("flow induced vibration"), the recesses may be coated with, for example, a soft organic material after thermal bonding, or an inliner (hose) may be introduced into each cooling channel before operation of the mirror.

[0078] In one development, the channel wall has a number of corner regions and at least one slot-shaped recess is formed in one of the corner regions. As mentioned above, the cooling channel has a polygonal, in particular rectangular, cross section, in which the channel upper wall and the channel lower wall adjoin two channel side walls in the corner regions. The slot-shaped recess is preferably formed in the corner region, in which the channel lower wall adjoins two channel side walls. The slot-shaped recess here preferably extends in the thickness direction of the substrate or transversely to the thickness direction. The slot-shaped recess does not have to be introduced in the corner region, but may for example be introduced in the center of the channel side wall or may be formed in the wall of the channel wall in a spiral or in sections obliquely.

[0079] In yet another embodiment, the first sub-body, in particular the entire substrate, is 1×10 15 molecule / cm 3 Less than or equal to 1 x 10 14 molecule / cm 3 It has a maximum hydrogen content of:

[0080] The study of the diffusion constants of OH groups in the paper "Bruckner II" was carried out on semi-synthetic glasses with an OH content comparable to that of soot glasses and lower than that of directly deposited glasses. Nothing is known about the H content of the quartz glasses examined in the paper, probably because Raman measurements were not widely used at the time. Based on the production by melting in a water-oxygen gas flame described in the paper, a diffusion constant of 1×10 15 molecule / cm 3 ~5×10 16 molecule / cm 3 Titanium-doped quartz glass from the soot process is inherently hydrogen-free, but glasses used in mirrors of projection systems for EUV lithography must generally be homogenized, which results in an OH content of 1×10 15 molecule / cm 3 ~5×10 15 molecule / cm 3 Directly deposited titanium doped silica glass typically has a thickness of about 1×10 17 molecule / cm 3 Direct deposition quartz glass has a H content of approximately 1×10 20 molecule / cm 3 This should also be expected for titanium doped glasses with the corresponding process scheme, since the H content reaches up to 1000 ppm.

[0081] The paper "Bruckner II" does not address the cause of the asymmetry between the outward and inward diffusion of OH groups. Part of the explanation could be the activation energy required for the decomposition of H2O. However, it can be assumed that the glasses used in these studies contained hydrogen. The diffusion of hydrogen depends on the solubility and partial pressure. In high purity quartz glass, at 1 atm in 100% hydrogen at about 400 °C, the saturation of dissolved hydrogen is about 5 × 10 17 molecule / cm 3 At lower temperatures the solubility is higher but the diffusion constant is smaller. Since the surrounding atmosphere is nearly hydrogen-free, it follows that hydrogen-containing quartz glass will lose hydrogen from the bulk through the surface at all temperatures from room temperature to the process temperature during thermal bonding.

[0082] Hydrogen must be available so that OH groups in the form of Si-OH can desorb from the surface or near-surface regions of the glass body and evaporate in the form of water vapor.

[0083] The easiest way to do this is to use the formula SiOH+H2→SiH+H2O provided that molecular hydrogen is available.

[0084] If molecular hydrogen is not available, the hydrogen must come from another OH group. 2 SiOH → H2O + Si + SiO

[0085] Both species are already energetically unfavorable in the bulk of the glass (E' or NBOH centers). They must either recombine at the surface, which is highly unlikely at temperatures below 1000°C, or reincorporate water, which effectively stops out-diffusion. Thus, the use of a very low hydrogen glass creates an exit barrier for OH groups, similar to the use of an oxidizing atmosphere.

[0086] Therefore, in the embodiments described here, it is proposed to use hydrogen-free or low-hydrogen glasses for the production of the substrates. Standard glasses for EUV mirrors contain hydrogen for process-related reasons, which can be diffused in a controlled manner. As shown in FIG. 36 of the paper "Bruckner II", the diffusion constant of hydrogen at a temperature of about 400° C. is about five orders of magnitude larger than that of OH. It is therefore possible to temper the hydrogen without significantly affecting the OH distribution. At a temperature of about 800° C., the difference is still three orders of magnitude and can be sufficiently distinguished.

[0087] In one development of this embodiment, the second partial body has a hydrogen content that is less than 50% of the average hydrogen content of the second partial body at a distance from the lower wall of the cooling flow passage that corresponds to at least the land width, preferably less than 10 times the land width of each land and / or less than 10 times the thickness of the first partial body and the thickness of the first partial body between the upper wall of the flow passage wall and the surface carrying the reflective coating.

[0088] Since non-uniformity in the thermal expansion of the glass is a problem, especially between the reflective coated surface and the cooling channels, possibly up to half the channel height, the critical thickness used for hydrogen outdiffusion should be the thickness of the glass above the cooling channels or the land width between the channels. The hydrogen concentration in the center of the cover or the center of the land is preferably less than 1×10 14 molecule / cm 3 It should be less than or equal to:

[0089] In the direction of the second part below the lower wall, it is generally sufficient if the hydrogen content in the substrate of the second part at a distance of 1 to 10 times the cover thickness or land width falls to 50% of its maximum value. As a result, there is still a slight OH deficiency in the bottom or lower wall of the cooling channel and in the lower region of the side walls, but as mentioned above, this is no longer a significant factor.

[0090] Hydrogen content is usually detected by Raman spectroscopy, but spatial resolution below 1 mm is rarely achievable (except in the case of micro-Raman spectroscopy), and the detection limit for OH-rich silica glass is typically 1–5 × 10 15 molecule / cm 3 The appropriate hydrogen distribution can be determined by a measurement point in the center of the cover or land and a series of measurement points from the bottom of the channel further into the substrate, and / or by corresponding diffusion calculations.

[0091] Yet another aspect of the invention relates to an optical device, in particular an EUV lithography system, comprising at least one optical element formed as described above and a cooling device designed to direct a cooling liquid through a number of cooling channels. The EUV lithography system may be an EUV lithography device for exposing wafers or any other optical device using EUV radiation, for example an EUV inspection system for, for example, inspecting masks, wafers, etc. used in EUV lithography. The reflective optical element may in particular be a mirror of a projection system of an EUV lithography device. The cooling device may be designed to direct a cooling liquid, for example in the form of cooling water, through at least one cooling channel. For this purpose, the cooling device may comprise a pump and suitable supply and discharge conduits.

[0092] Further features and advantages of the invention emerge from the following description of an exemplary embodiment of the invention, with reference to the figures of the drawing which show the essential details of the invention, and from the claims. Each of the individual features can be realized alone or in any combination of several in one variant of the invention.

[0093] Exemplary embodiments are shown in the schematic drawings and explained in the following description. [Brief description of the drawings]

[0094] [Figure 1] 1 is a schematic meridian section of a projection exposure apparatus for EUV projection lithography. [Figure 2a] FIG. 2 is a schematic diagram of a blank of titanium-doped quartz glass having two part bodies bonded to one another by thermal bonding along the bonding surface in the region of a number of cooling channels. [Figure 2b] FIG. 2 is a schematic diagram of a blank of titanium-doped quartz glass having two part bodies bonded to one another by thermal bonding along the bonding surface in the region of a number of cooling channels. [Figure 3a] FIG. 2b is a schematic diagram of an optical element manufactured from the quartz glass blank from FIG. 2a during an exposure operation. [Figure 3b] FIG. 3b is a schematic view similar to FIG. 3a with material removed from the channel walls of the cooling channels. [Figure 4a] FIG. 1 is a schematic diagram of a metallic protective coating applied to the channel walls to prevent the formation of OH depleted regions during the thermal bonding operation. [Figure 4b] FIG. 1 is a schematic diagram of a metallic protective coating applied to the channel walls to prevent the formation of OH depleted regions during the thermal bonding operation. [Figure 4c] FIG. 1 is a schematic diagram of a metallic protective coating applied to the channel walls to prevent the formation of OH depleted regions during the thermal bonding operation. [Figure 4d] FIG. 1 is a schematic diagram of a metallic protective coating applied to the channel walls to prevent the formation of OH depleted regions during the thermal bonding operation. [Figure 5a] FIG. 13 is a schematic diagram of a cooling channel wall where slot-like recesses have been introduced to reduce stress caused by OH depletion regions. [Figure 5b] FIG. 13 is a schematic diagram of a cooling channel wall where slot-like recesses have been introduced to reduce stress caused by OH depletion regions. [Figure 5c] FIG. 13 is a schematic diagram of a cooling channel wall where slot-like recesses have been introduced to reduce stress caused by OH depletion regions. [Figure 6] FIG. 2 is a schematic diagram of the distribution of the hydrogen content of a blank made of titanium-doped quartz glass upon tempering. [Figure 7a] FIG. 1 is a schematic diagram of the temperature progression of a tempering process for a blank made of titanium-doped quartz glass at a holding temperature of 1080° C. [Figure 7b] FIG. 7a is a schematic diagram of the distribution of the OH content of a blank made of titanium-doped quartz glass after the tempering process; [Figure 8a] FIG. 7b is a schematic diagram similar to FIG. 7a of the tempering process at a holding temperature of 650° C. [Figure 8b] FIG. 7b is a schematic diagram similar to FIG. 7b of the tempering process at a holding temperature of 650° C. [Figure 9a] FIG. 7b is a schematic diagram similar to FIG. 7a of the tempering process at a holding temperature of 1200° C. [Figure 9b] FIG. 7b is a schematic diagram similar to FIG. 7b of the tempering process at a holding temperature of 1200° C. [Figure 10a]FIG. 2 is a schematic diagram of the OH content of blanks made of directly deposited quartz glass during thermal bonding in saturated water vapor. [Figure 10b] FIG. 2 is a schematic diagram of the OH content of a blank made of directly deposited quartz glass with subsequent increasing OH content. [Figure 11a] 10a , a schematic view similar to FIG. 10 a of a blank made of quartz glass produced by the soot method. [Figure 11b] 10b : A schematic view similar to FIG. 10b of a blank made of quartz glass produced by the soot method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0095] In the following description of the drawings, the same reference numbers are used for components that are the same or have the same functionality.

[0096] The essential components of an optical apparatus for EUV lithography in the form of a projection exposure apparatus 1 for microlithography are explained below by way of example with reference to Figure 1. The description here of the basic construction of the projection exposure apparatus 1 and its components should not be considered limiting.

[0097] An embodiment of the illumination system 2 of the projection exposure apparatus 1 comprises, in addition to the light source or radiation source 3, an illumination optical unit 4, which illuminates an object field 5 in an object plane 6. In an alternative embodiment, the light source 3 can also be provided in the form of a module that is separate from the rest of the illumination system. In this case, the illumination system does not include the light source 3.

[0098] A reticle 7 arranged in the object field 5 is exposed. The reticle 7 is held by a reticle holder 8. The reticle holder 8 is displaceable in particular in the scanning direction by a reticle displacement drive 9.

[0099] For the purposes of illustration, Fig. 1 shows a Cartesian xyz coordinate system. The x direction extends perpendicular to the plane of the drawing. The y direction extends horizontally and the z direction extends vertically. In Fig. 1, the scanning direction extends in the y direction. The z direction extends perpendicular to the object plane 6.

[0100] The projection exposure apparatus 1 comprises a projection system 10, by means of which the object field 5 is imaged into an image field 11 in an image plane 12. A structure on a reticle 7 is imaged onto a photosensitive layer of a wafer 13, which is arranged in the region of the image field 11 in the image plane 12. The wafer 13 is held by a wafer holder 14, which is displaceable in particular in the y-direction by a wafer displacement drive 15. Both the displacement of the reticle 7, firstly by the reticle displacement drive 9 and the displacement of the wafer 13, secondly by the wafer displacement drive 15, can be synchronized with each other.

[0101] The radiation source 3 is an EUV radiation source. The radiation source 3 in particular emits EUV radiation 16, also referred to in the following as working radiation, illumination radiation or illumination light. In particular, the working radiation has a wavelength in the range of 5 nm to 30 nm. The radiation source 3 can be a plasma source, for example an LPP source (Laser Produced Plasma) or a GDPP source (Gas Discharge Plasma). It can also be a synchrotron-based radiation source. The radiation source 3 can be a Free Electron Laser (FEL).

[0102] The illumination radiation 16 leaving the radiation source 3 is focused by a collector mirror 17. The collector mirror 17 may be a collector mirror with one or more ellipsoidal and / or hyperbolic reflecting surfaces. The illumination radiation 16 may be incident on at least one reflecting surface of the collector mirror 17 at grazing incidence (GI), i.e. at an angle of incidence greater than 45°, or at normal incidence (NI), i.e. at an angle of incidence smaller than 45°. The collector mirror 17 may be structured and / or coated, firstly to optimize its reflectivity for the radiation used and secondly to suppress extraneous light.

[0103] Downstream of the collector mirror 17, the illumination radiation 16 propagates through an intermediate focus in an intermediate focal plane 18. The intermediate focal plane 18 may form a separation between a source module, which includes the radiation source 3 and the collector mirror 17, and the illumination optical unit 4.

[0104] The illumination optical unit 4 comprises a deflection mirror 19 and, downstream of it in the beam path, a first facet mirror 20. The deflection mirror 19 can be a plane deflection mirror or a mirror with a beam-influencing effect beyond a pure deflection effect. Alternatively or additionally, the deflection mirror 19 can be in the form of a spectral filter, which separates the used light wavelengths of the illumination radiation 16 from extraneous light of different wavelengths. The first facet mirror 20 comprises a number of individual first facets 21, also referred to as field facets in the following. FIG. 1 shows only some of said facets 21 by way of example. A second facet mirror 22 is arranged downstream of the first facet mirror 20 in the beam path of the illumination optical unit 4. The second facet mirror 22 comprises a number of second facets 23.

[0105] The illumination optical unit 4 therefore forms a double-facet system. This basic principle is also called a fly's eye integrator. By means of a second facet mirror 22, the individual first facets 21 are imaged into the object field 5. The second facet mirror 22 is the last beam-shaping mirror in the beam path upstream of the object field 5 or indeed the final mirror for the illumination radiation 16.

[0106] The projection system 10 comprises a number of mirrors Mi, which are consecutively numbered according to their position in the beam path of the projection exposure apparatus 1 .

[0107] In the example shown in Fig. 1, the projection system 10 comprises six mirrors M1-M6. Four, eight, ten, twelve or any other number of mirrors Mi are equally possible. The penultimate mirror M5 and the final mirror M6 each have a passing aperture for the illumination radiation 16. The projection system 10 is a double-shielded optical unit. The projection optical unit 10 has an image-side numerical aperture which may be greater than 0.4 or 0.5, may be greater than 0.6, and may for example be 0.7 or 0.75.

[0108] Like the mirrors of the illumination optical unit 4 , the mirror Mi may have a highly reflective coating for the illumination radiation 16 .

[0109] Each mirror Mi is manufactured using a glass body 24 made of titanium-doped quartz glass having a number of cooling channels 25, as shown in Figures 2a and 2b. The glass body 24 has a first upper partial body 26a and a second lower partial body 26b that are joined by thermal bonding along a bonding surface 27, which is planar in the illustrated example. The two partial bodies 26a, 26b are formed from a solid glass body (without cooling channels) by cutting them open along a parting surface, which is planar in the illustrated example.

[0110] For the manufacture of the glass body 24 shown in Figures 2a, 2b, the lower body 26b is first machined. In the machining, a number of recesses are machined into the quartz glass material of the lower body 26b, which have an essentially square or rectangular cross section as shown. It will be clear that the recesses can alternatively be machined into the first body 26a. There is also the possibility that recesses are machined into both bodies 26a, 26b, which form the cross section of each cooling channel 25 after joining.

[0111] In the example shown in Fig. 2a, the first partial body 26a is placed on and pressed against the second partial body 26b at room temperature on a work surface which subsequently forms a bonding surface 27. The two partial bodies 26a, 26b are then subjected together to a thermal bonding process, in which the two partial bodies 26a, 26b are bonded to one another along the bonding surface 27. In contrast, in the example shown in Fig. 2b, the first partial body 26a and the second partial body 26b are first heated separately to an elevated temperature before they are bonded to one another to form the glass body 24.

[0112] 7a shows an example of the temperature course of a tempering process of a glass body made of titanium-doped quartz glass according to the example of the patent document 2, which can also be used in principle for the above-mentioned thermal bonding operation to join the two partial bodies 26a, 26b. In the tempering process, the glass body is first heated to a holding temperature of 1080° C. for 3 hours and, after a holding time of 8 hours at the holding temperature, is cooled controlled to a temperature of 950° C. at a cooling rate of 4 K / h. After a holding time of 4 hours at a temperature of 950° C., the glass body is cooled to a temperature of 300° C. at a high cooling rate of 50 K / h.

[0113] FIG. 7b shows the one-dimensional (simulated) progression of the OH content of a glass body (without cooling channels) having a thickness of 2 mm in the thickness direction (z direction) of the glass body after completion of the tempering process of FIG. 7a. For the simulation, a constant OH concentration of 180 ppm was assumed in the glass body in the thickness direction before the start of the tempering process. Furthermore, it was assumed that the glass contains sufficient hydrogen, i.e. there is no exit barrier for OH groups. As is evident in FIG. 7b, the OH content (ppm by weight) in the center of the glass body (i.e. Z=1 mm) is still 180 ppm by weight after the tempering process. However, the OH content decreases towards the edges of the glass body (Z=0 cm and Z=2 mm) to a value of 0 ppm by weight. The decrease in the OH content at the edges of the glass body is due to the diffusion of OH groups from the quartz glass.

[0114] In the simulations, the furnace in which the tempering process is carried out is operated in vacuum, air or with sufficient circulation of inert gas, so that the environment of the glass body formed during the joining of the two parts in the furnace is at zero water vapor pressure. In the simulations, the diffusion coefficients used as a function of temperature are given in the abovementioned papers "Bruckner I" or "Bruckner II", see in particular Figure 36 of the latter paper. Quartz glass referred to as type II in Figure 36 of the paper "Bruckner II" is a quartz glass obtained by melting powdered silicon dioxide under a water-oxygen gas flame. The OH content of such quartz glass is comparable to that of quartz glass produced by the soot method and somewhat lower than that of directly deposited quartz glass, so the values ​​given in the paper "Bruckner II" can be used for the simulations. The diffusion of OH groups from Ti-doped quartz glass proceeds with approximately the same temperature-dependent diffusion constant as in the case of undoped quartz glass, so the diffusion constant of undoped fused quartz glass can also be used for titanium-doped quartz glass.

[0115] The distance from the edge of the glass body at which the OH content drops to 50% of its maximum value is d in Fig. 7a. Mand form a guide value for the thickness of the depleted zone or depleted zone in the quartz glass. In the example shown in FIG. 7b, the maximum OH content is 180 ppm by weight, and the thickness d M The value is approximately 220 μm.

[0116] Thickness of the depletion area d M depends not only on the maximum OH content of the quartz glass but also on the tempering process, in particular on the values ​​of the holding temperature and holding time. As will be explained below with reference to Figures 8a, 8b and 9a, 9b, for high holding temperatures, the thickness d M increases.

[0117] Figure 8a shows the temperature progression of the tempering process with a holding temperature of 650°C and a holding time of 24 hours. Figure 8b shows the simulated progression of the OH content, which drops from a maximum OH content of 850 ppm by weight in the center of the glass body to 0 ppm by weight at the edge of the glass body. Again, it was assumed that there is no prerequisite for an exit barrier for OH groups. The OH content in the center of the glass body corresponds to a constant initial value over the thickness of the glass body, which was defined for the simulation. The thickness d of the depletion zone in this example is M is only 48 μm.

[0118] Figure 9a shows the temperature progression of the tempering process at a holding temperature of 1200 °C and a holding time of 24 h. Again, it was assumed that there was no prerequisite for an exit barrier for OH groups. Figure 9b shows the simulated progression of the OH content, which drops from a maximum OH content of about 800 ppm by weight in the center of the glass body to 0 ppm by weight at the edge of the glass body. The thickness d of the depletion zone in this example is M 290 μm. For the OH content progression shown in Fig. 9b, a constant OH content value of 850 wt ppm was assumed across the thickness of the glass body, as in the simulation examples shown in Figs. 8a and 8b. Thus, OH deficiency occurred even in the center of the glass body after the tempering process shown in Fig. 9a.

[0119] The above-mentioned thermal bonding process, in which the two partial bodies 26a, 26b are bonded to one another along the bonding surface 27, also results in OH depletion of the quartz glass. FIG. 2a shows, by way of example, a depletion region 28 at the outside or outer edge of the glass body 24, which extends in particular along the upper and lower surfaces 29a, 29b of the glass body 24. As is also evident in FIG. 2a, a depletion region 30 adjacent to the cooling channels 25 is also present in the material of the glass body 24. In the glass body 24 shown in FIG. 2b, the two partial bodies 26a, 26b are heated separately, so that a depletion region 30' is present which extends along the bonding surface 27 between the cooling channels 25. The depletion regions 28, 30, 30' of the glass body 24 are shown with exaggerated widths or thicknesses in FIG. 2a, 2b.

[0120] FIG. 3a shows a mirror M2 having a substrate 31 made from the glass body 24 shown in FIG. 2a. In the manufacture of the substrate 31, the glass body 24 is ground to remove the depleted regions 28 on the upper surface 29a and the lower surface 29b of the glass body 24. In addition, the edges of the glass body 24 are trimmed during the manufacture of the substrate 31. In the grinding and subsequent polishing steps, a surface 32 is formed on the upper surface 29a of the substrate 31, on which a reflective coating 33 is applied after the grinding and subsequent polishing steps. In the illustrated example where the mirror M2 is an EUV mirror, the reflective coating 33 is designed to reflect EUV radiation at an operating wavelength in the EUV wavelength range of about 5 nm to about 30 nm, and for that purpose has multiple alternating layers of high and low refractive index materials. In this example, at an operating wavelength of 13.5 nm, the materials of the alternating layers of the reflective coating 33 are Si and Mo. The EUV radiation is incident only on a portion of the reflective coating 33, also referred to as the optically utilized area 32a, the outer edge of which is shown by a dashed dotted line in Fig. 3b. The area of ​​the optically utilized area 32a may possibly be much smaller than the area covered by the reflective coating 33. The optically utilized area 32a makes the imaging light passing through the projection system 10 further usable after reflection from mirror M2.

[0121] 3, a depletion region 30 in each cooling channel 25 remains in the substrate 31. The OH gradient in the depletion region 30 around each cooling channel 25 leads to a change in the zero cross temperature of the thermal expansion coefficient of the titanium doped silica glass. The gradient in the zero cross temperature at a given temperature leads to a circumferential compressive stress or a circumferential tensile stress in the depletion region 30 adjacent to the cooling channel 25.

[0122] In the example shown in Fig. 3a, it is assumed that there are compressive stresses which firstly cause a not very significant (not shown) expansion of the quartz glass material in each cooling channel 25 and secondly cause a curvature of the surface 32 with the reflective coating 33 above each cooling channel 25, the curvature being shown in exaggerated form in Fig. 3a. During manufacture of the mirror M2, the surface 32 is polished, but the smoothing or polishing is carried out at room temperature and not at the operating temperature of the mirror. Complete removal of the bumps shown in Fig. 3a is therefore not possible, which leads to image defects during operation of the mirror M2 at operating temperatures other than room temperature. The extent of the effect on the image defects of the mirror M2 is greater the greater the difference between room temperature and the operating temperature.

[0123] In order to avoid bumps or gross deformations at the surface 32 of the mirror M2 as shown in FIG. 3 a due to OH deficiency in the glass material of the substrate 31 during thermal bonding, it is preferred that the substrate 31 has a minimum gradient in OH content or zero cross temperature in both the lateral direction (X direction) and thickness direction (Z direction) in the volumetric region adjacent to the cooling channels 25.

[0124] As can be seen in Figures 3a and 3b, two adjacent cooling channels 25 are separated from each other by a land 35. Each cooling channel 25 in the illustrated example has a rectangular cross-section with a channel wall 36 having four portions 36a-36d: an upper wall portion 36a forming the roof of the cooling channel 25 and located adjacent the surface 32 having the reflective coating 33, a lower wall portion 36b forming the bottom of the cooling channel 25 and remote from the surface 32 having the reflective coating 33, and two side walls 36c, 36d adjacent the upper and lower walls 36a, 36b.

[0125] FIG. 3b shows the center position P of the right side wall portion 36d (in the Z direction). S and the central position P of the upper wall portion 36a (in the X direction) D In the example shown in FIG. 3b, material has been removed along the entire thickness d of the depletion region 30 along the channel wall 36 shown in FIG. 3a. The central location P S In this case, the zero cross temperature T ZC,S is the zero cross temperature T at the center M of land 35 due to material removal. ZC,M The difference between the two zero-cross temperatures T ZC,S , T ZC,M The comparison between the side walls 36d and 36c is performed at the center position P S In the example shown in FIG. 3b, where the entire depletion region 30 has been removed, the above condition is satisfied at a position P S The sidewall 36d is filled along its entirety, not just the sidewall 36c.

[0126] Unlike the case shown in FIG. 3b, if the entire depletion region 30 is not removed, the zero cross temperature T ZC,S is the zero cross temperature T at the center of land 35 ZC,M The difference between the two may be larger and may be less than 3.0K or less than 2.0K. ZC,M -T ZC,S The sign of varies depending on the temperature program, but generally the lower the OH content the lower the zero cross temperature.

[0127] Zero cross temperature T ZC,S , T ZC,M In order to satisfy the above condition, generally, the center position P of the side wall portion 36d is S The OH content of the substrate 31 at or along the entire sidewall portion 36d must differ from the OH content at the center M of each land 35 by 60 ppm by weight or less, 30 ppm by weight or less, or 20 ppm by weight or less, which can also be achieved by material removal as described above.

[0128] Similar to the lateral gradient of the OH content, the gradient of the OH content in the thickness direction Z of the substrate 31 also influences the zero cross temperature and thus the deformation of the surface 32 provided with the reflective coating 33. In the example shown in FIG. 3b, at the position P D At the center position P D Position P on surface 32 at distance A from O Zero cross temperature T ZC,O The difference between the zero cross temperature T and ZC,D The distance A is measured from the center position P of the upper wall portion 36a. D Measured in the thickness direction Z from the position P O is the position P D The complete elimination of the depletion region 30 reduces the zero cross temperature T ZC,D , T ZC,O The above conditions are met.

[0129] As explained in relation to the lateral gradient of the zero cross temperature, if the entire depletion region 30 is not removed, the zero cross temperature T ZC,D is the zero cross temperature T of the upper surface 32 of the channel wall 36 ZC,O The difference may be greater and may be less than 3.0K or less than 2.0K.

[0130] Zero cross temperature T ZC,D , T ZC,O In order to satisfy the above condition, generally, the central position P of the upper wall portion 36a D The OH content of the substrate 31 along the entire upper wall 36a of the cooling channel 25 is measured at a position P D At a position P on the surface 32 at a position A above O should differ from the OH content by 60 ppm or less, 30 ppm or less, or 20 ppm or less by weight, which can be achieved by material removal.

[0131] The zero cross temperature or OH content conditions satisfied by the upper wall 36a of the channel walls 36 generally do not have to be observed by the lower wall 36b, since the lower wall 36b of the channel walls 36 does not curve inwardly into the respective cooling channel 25 and therefore does not directly lead to deformation of the surface 32 provided with the reflective coating 33. Furthermore, the temperature rise due to the heat input during irradiation of the surface 32 of the mirror M2 in the lower wall 36b of the channel walls 36 of each cooling channel 25 is relatively small.

[0132] During operation of the mirror M2 or during heating of the mirror M2 to its operating temperature, there is little, if any, deformation of the surface 32 of the mirror M2, provided that the above conditions are observed. To cool the mirror M2 during operation, a cooling fluid, e.g. cooling water, can be flowed through the cooling channels 25 by means of a cooling device 37, shown in Fig. 3b. For this purpose, the cooling device 37 can comprise, for example, a pump or the like.

[0133] Due to the material removal from the channel walls 36 shown in FIG. 3a, the substrate 31 has a non-zero OH content along the entire channel walls 36 shown in FIG. 3b. Depending on the depth of material removal, the OH content of the channel walls 36 can be more than 60 ppm by weight, more than 120 ppm by weight, or even much more. The depth to which material should be removed from the channel walls 36 depends on factors including the maximum and average OH content of the substrate 31. If the glass is produced by direct deposition, it usually has a relatively high maximum OH content of about 850 ppm by weight, see for example FIG. 8b and FIG. 9b. The OH content is reduced to 0 ppm by out-diffusion, so a larger removal is generally required in this case than for glasses produced by the soot process, which have a maximum and average OH content on the order of about 200 ppm by weight.

[0134] Depending on the nature of the material removal method, it may be difficult to remove the entire depletion region 30 since the removal may take a relatively long time with a correspondingly high cost, and there may be problems with poor contour accuracy during removal. Thus, the depletion region 30, defined in this case as the region adjacent the channel wall 36 where the OH content of the substrate 31 is 5 ppm or more by weight less than the OH content of the center M of the adjacent land 35 and / or the OH content of the surface 32, should have a minimum thickness d. In particular, the thickness d should be less than 50 μm, less than 30 μm, or less than 1 μm, as the case may be after the above-mentioned material concessions.

[0135] There are various options for material removal from the channel walls 36. For example, the channel walls 36 can be treated with an abrasive emulsion or an etchant after thermal bonding. If depletion areas 30 with a thickness of more than 1 mm are to be removed, hot phosphoric acid is preferably used for removal. The etching action can also be spatially controlled with pre-damage of the glass material, for example with a short pulse laser or by ultrasonic treatment. As shown in FIG. 3b, here there can be preferential removal of the upper wall 36a and the upper regions of the side walls 36c, 36d. It is also possible to use alkali as etchant, especially in combination with pre-damage. Generally, it is preferable to use slow etchants, for example phosphoric acid or alkali, since they allow processing at low etch rates and low flow rates, which allows uniform etching removal.

[0136] As will be explained below with reference to Figs. 4a-4d, the diffusion of OH groups from the glass material of the substrate 31 or from the two halves 26a, 26b, and thus the creation of an OH gradient during thermal bonding, can be prevented by applying a protective coating 38 (possibly temporarily) to the channel walls 36. For this purpose, the protective coating 38 contains at least one material that prevents the outward diffusion of OH groups. For this purpose, the protective coating 38 usually comprises at least one metal layer, since a metal layer of any kind will significantly inhibit the outward OH diffusion. A suitable metal should have a melting point above the maximum process temperature of the thermal bonding operation. In the illustrated example, the protective coating 38 is a chromium coating. Chromium has the advantage of a high melting point as well as good applicability and structure-forming properties.

[0137] The metallic surface of the protective coating 38 of the cooling channels 25 can be protected in the thermal bonding process by carrying out the thermal bonding process in an inert gas or under reduced pressure. Alternatively, it is possible to choose a metal with a sufficiently stable oxide layer at the temperature of use, or to cover the metallic protective coating 38 with other oxide-based or non-metallic protective layers. To achieve a higher barrier effect, it is also possible to use an arrangement of different metals, metals and semimetals, or metals and oxides. Standard MoSi multilayers, which are used to make EUV optics reflective, have a virtually infinite barrier effect against hydrogen. However, due to its low melting temperature, molybdenum is only suitable for relatively low-temperature bonding processes or an additional protective layer must be applied to the Mo-Si multilayer.

[0138] Ideally, as shown in FIG. 4a, the channel walls 36 are covered with a metallic protective coating 38 over the entire channel perimeter and possibly the subsequent mirror area 32. It is also possible to provide all surfaces of the glass body 24 or of the two partial bodies 26a, 26b that are exposed to the ambient atmosphere during thermal bonding with a protective coating 38 or to metallize them. Possible methods of metallization include sputtering deposition, by initial deposition from the gas phase or from a liquid after an initial etching. Once a so-called primer layer has been applied, a thicker layer of another metal can also be electrolytically deposited.

[0139] In the example shown in Fig. 4a, the cooling channels 25 or corresponding recesses are machined into the first partial body 26a, which in this case is covered with a protective coating 38, at least over the entire area of ​​the surface that will form the subsequent bonding surface 27, including the cooling channels 25 that remain open. By means of a grinding or polishing step, the metal layer is removed in such a way that at the subsequent bonding surface 27, the first partial body 26a is left with an open cooling channel 25 coated on three sides, namely the top wall 36a and the two side walls 36c, 36d. In the example shown in Fig. 4a, the subsequent mirror surface 32 is also covered with a metallic protective coating 38', but this is not necessary.

[0140] As shown in Fig. 4a, the second partial body 26b can in principle remain uncoated or only be coated in the area of ​​the lower wall 36b of the subsequent cooling channel 25. The coating of the second partial body 26b at the lower wall 36b can be carried out by a complete metallization and masked etching of the subsequent bonding surface 27 or by applying a mask and selective etching. Since a perfect positioning of the first partial body 26a on the second partial body 26b is not possible, especially in a thermal bonding process using pressure, the metallization area in this case must generally be somewhat narrower than the cooling channels 25. The lower wall 26d of each cooling channel 25 is therefore left uncoated either entirely or along the side edges. The resulting depletion zone extends into the substrate 31 and therefore has a much smaller effect on the deformation of the mirror surface 32 as a function of temperature than the depletion zone 30 of the upper wall 36a of the cooling channel 31.

[0141] The protective coating 38 applied before the thermal bonding, which may be masked or may have a different structure, may be very thin and may only serve as a primer for electroplating or chemical deposition from a solution after the thermal bonding. This causes the protective coating 38 to grow in thickness, but also laterally along the covered surface. If the metallization in the area where the cooling channels 25 are not provided, in the illustrated example the second partial body 26b, is only a few tens of micrometers narrower than the width of the cooling channels 25, this lateral growth may be sufficient to close the gap and cover the cooling channels 25 with the protective coating 38 over the entire circumference of the channels. The subsequent electroplating or chemical deposition may also contribute to closing gaps in the metallization that may occur due to residual roughness of the channel walls 36 of the cooling channels 25.

[0142] Depending on the metal used, the presence or absence of cracks, the layer structure (columnar, amorphous, granular), and the process temperature and duration, a protective coating 38 with a few atomic layers may be sufficient to inhibit outward hydrogen diffusion. The protective coating 38 should not be unnecessarily thick, since the thermal expansion coefficient of the protective coating 38 is different from that of the glass, which would introduce unnecessarily high stresses into the glass during tempering. However, in particular in the case of rough glass surfaces or slots from the masking process, a final layer thickness of the protective coating 38 in the micrometer range may be necessary to achieve impermeability. However, a thin layer can be controlled pushed into valleys or corners / gaps by hot ion beam processes or glass bead blasting, so that a thinner protective coating 38 overall can be handled.

[0143] At bonding temperatures above 1200° C., it is also possible to make the metallization strip of the protective coating 38 somewhat wider than the covered cooling channels 25 of the first partial body 26, especially if the sides of the metallization run relatively obliquely as shown in FIG. 4b. In this case, the sides of the metallization or protective layer 38 result in a residual gap between the first partial body 26a and the second partial body 26b. At high temperatures, possibly assisted by the addition of contact pressure, the first partial body 26a fits between the metallization on the second partial body 26b in this case. The remaining metal residues should be etched away from the edges of these cooling channels 25 after thermal bonding, since they have a significantly different thermal expansion coefficient than the glass material of the substrate 31 that surrounds the cooling channels 25 on three sides. Any notches remaining in the glass should be rounded off by suitable machining with a rotary tool on a flexible shaft, purging with an abrasive emulsion, or by etching. To improve the flow properties, this may be further filled with a constant-elastic substance or an organic inliner may be used. The method of seamless metallization can of course also be used if the cooling channels 25 are processed in the second partial body 26b rather than in the first partial body 26a. Since the metallic material of the metallic protective coating 38 has a different thermal expansion coefficient than the glass and therefore stresses are introduced into the surrounding glass during tempering and are frozen and only partially relieved upon removal of the metallic protective layer 38, it can be advantageous if the protective coating 38 has clear interruptions (slots). Figure 4c shows an example in which the channel wall 36 is not covered with the protective coating 38 in four corner regions 39a-39d, each arranged between two adjacent wall portions 36a-36d of the channel wall 36, i.e. the channel wall 36 is covered with the protective coating 38 only outside the corner regions 39a-39d, while the corner regions 39a-39d are hollowed out. As shown in Figure 4c, this leads to local OH deficiencies in the corner regions 39a-39d. However, because the corner regions 39a-39d are insulated, the generation of temperature-dependent forces that lead to glass bulging above the cooling channel 25 can be much smaller than in the case of the annular or tubular depletion regions shown in FIG. 3a.

[0144] Fig. 4d shows yet another example of a protective coating 38 extending along a sidewall 36d of the cooling channel 25 in a top view in the longitudinal direction Y of the cooling channel 25. As can be seen in Fig. 4d, in order to reduce forces acting in the longitudinal direction Y of the cooling channel 25, the protective coating 38 has an angled slot 40, where the sidewall 36d is not covered by the protective coating 38. The slot 40 can also continue in a spiral or other form across all four walls 36a-36d of the cooling channel 25.

[0145] After the bonding of hydrophilic glass surfaces, one or more water monolayers remaining on the bonding surface prevent the formation of the desired covalent bonds in the bonding operation. Normally, water molecules can diffuse along the bonding surface 27 during heating. However, if a continuous metallization is formed, including on the open side of the bonding surface 27, before the bonding operation, this outward diffusion is suppressed and only a very slow diffusion of water remains in the glass body 24. In order to drive the water out of the gaps, it can be advantageous to bake the bonded parts 26a, 26b, which are not yet metallized or are not yet seamlessly metallized, at 100°C to 400°C for several hours to weeks. Only afterwards is the inside of the channels metallized and the masked partial metallization thickened, including closing the notches in the metal protective coating 38.

[0146] In the above examples, it has been assumed that the cooling channel 25 or its cross section is completely introduced in the first partial body 26a or in the second partial body 26b. It will be understood that the cooling channel 25 can also be introduced in both partial bodies 26a, 26b. If the cross section of the cooling channel 25 in this case consists of a notch milled in the first partial body 26a and a notch milled in the second partial body 26b, the simplest way is to apply a substantially continuous metallic protective coating 38 to the first partial body 26a and to the second partial body 26b, and only then to polish the areas to be bonded on the surfaces of the two partial bodies 26a, 26b. In this case, a metal-free bonding surface 27 remains, as well as a cooling channel 25 that is coated all around, up to the vicinity of the bonding site. The minimal uncoated areas on the sides of the channels adjacent to the bonding site, which result from the application of edge rounding or chamfering, are very limited locally and therefore usually do not matter in terms of the influence on the thermal expansion coefficient. Furthermore, this specifically allows the diffusion of water from the gap.

[0147] If the protective coating 38 is detrimental, for example due to its effect on the thermal expansion coefficient of the glass, it can be removed again by etching or electrolysis after the thermal bonding process.

[0148] Yet another way to prevent the diffusion of OH groups from the quartz glass is to fill the cooling channels with glass powder that has the same or higher OH content as the substrate glass during thermal bonding. If the filling level of the cooling channels is more than 10%, Ti-doped quartz glass with approximately the same concentration as the substrate should be used for this purpose, or the Ti content should be adjusted so that the glass powder has a lower expansion than the substrate.

[0149] Yet another way of reducing image defects of the optical element M2, which may make it possible to dispense with the removal of material or the deposition of a protective coating 38, is described below in connection with FIGS. 5a-5c, which show the first and second partial bodies 26a, 26b before bonding. In the example shown in FIG. 5a, the channel wall 36 of the first partial body 26a and in the example shown in FIGS. 5b, 5c, of the second partial body 26b, have two slot-like recesses 41a, 41b. Similarly, FIGS. 5a-5c also show a depletion area 30 adjacent to the channel wall 36, which is formed after thermal bonding of the two partial bodies 26a, 26b and has a thickness d of about 100 μm in the example shown. As is evident in FIGS. 5a-5c, the depletion area 30 formed during thermal bonding extends around the slot-like recesses 41a, 41b. The annular depletion regions 30 along the cross-section of each cooling channel 25 are attenuated by slot-like recesses 41 a, 41 b to reduce temperature-related bumps or depressions in the upper surface 32 of the cooling channel 25, which leads to reduced image defects during operation of the optical element M2.

[0150] To achieve this, the slot-like recesses 41a, 41b should have a depth T that corresponds at least to the thickness d of the depletion region 30. Preferably, the depth T is at least twice the thickness d of the depletion region 30, which corresponds to about 200 μm in the example shown, but the depth T should generally not exceed five times the thickness d of the depletion region 30. The width B of each slot-like recess 41a, 41b should be of the order of about 100 μm or more.

[0151] In all three examples shown in Fig. 5a-5c, the slot-like recesses 41a, 41b are formed in the two corner regions 39c, 39d between the respective side walls 36c, 36d and the bottom wall 36b. In the example shown in Fig. 5a, the slot-like recesses 41a, 41b are ground in the upper body 26a, through which in this example the cross section of the cooling channel 25 extends. In the example shown in Fig. 5b, the two slot-like recesses 41a, 41b are ground in the plane of the second lower body 26b. In the example shown in Fig. 5c, the cross section of the cooling channel 25 is in the second lower body 26b, and the slot-like recesses 41a, 41b extend downwards (Z direction) from the bottom wall 36b. As shown in relation to Fig. 5a, a lateral widening of the cooling channel 25 in the region of the subsequent gluing surface 27 is possibly possible in the example shown in Fig. 5c as well, but the discontinuity in this case is located close to the surface 32 of the optical element M2.

[0152] It will be clear that the slot-like recesses 41a, 41b can also be located elsewhere along the channel wall 36, for example in the middle of the side walls 36c, 36d. The slot-like recesses 41a, 41b can also be introduced into each cooling channel 25 in a spiral manner or obliquely in sections, similar to the slot 40 described in connection with Figures 4a-4c. If the slot-like recesses 41a, 41b are problematic when the cooling medium passes through the cooling channels 25, they can be coated or closed, for example with a soft organic material, or an inliner or hose can be introduced into each cooling channel 25.

[0153] Yet another way to create a minimum gradient in the OH content of the titanium-doped quartz glass in the case of the above-mentioned thermal bonding process is to reduce the maximum OH content of the substrate 31 of the optical element M2. The effect of deformation of the surface 32 covered with the reflective coating 33 shown in Figure 3a can usually be avoided if the substrate 31, but at least the upper part 26a, has a maximum OH content of less than 10 ppm by weight.

[0154] To achieve this, the OH content of the quartz glass of the body 24 can be reduced by suitable thermal or chemical drying operations (e.g. with halogens) before sintering during the manufacture of the body 24 by the soot method. Such drying operations allow the manufacture of quartz glass with an OH content of less than 1 ppm by weight, as is known for applications in the IR or DUV wavelength range. Similarly, it is possible to manufacture extremely dry titanium-doped quartz glass, as required for the substrate 31 described here for the EUV mirror M2. As dry glass is difficult to form and homogenize, one option is to perform homogenization of the Ti content at an early stage of the soot powder, and then press a grey body from the homogenized powder, from which the substrate 31 is formed by sintering or by HIP (hot isostatic pressing).

[0155] The very dry quartz glass formed in this way has a high fictive temperature and therefore a large gradient in the thermal expansion coefficient of the quartz glass, 1.8 ppb / K at 20°C. 2 For this reason, even without direct measurement of the temperature data of the quartz glass or the substrate 31, it is possible to show an OH content as low as 10 ppm by weight. The dry quartz glass of the substrate 31 is generally hydrogen free, but can also be loaded with hydrogen without incurring an increase in the OH gradient.

[0156] The above-mentioned drying can be carried out on the two halves 26a, 26b of the glass body 24 together, but it is also possible to carry out drying on each of the two halves 26a, 26b separately. It may be sufficient to dry only the top few millimeters of the upper halves 26a and also the lower halves 26b. For that purpose, each halves 26a, 26b separately or the two halves 26a, 26b together can be tempered at temperatures above 1400°C, preferably above 1600°C, for several days to weeks. At temperatures above 1450°C, there is a significant deformation of the quartz glass, so drying should be carried out in an open-top crucible or an open-top mold.

[0157] Yet another means of reducing the OH gradient in the glass by high temperature tempering is to use hydrogen-free or low hydrogen glass in the manufacture of substrate 31. Standard EUV glass contains hydrogen as a result of manufacture, so this can be diffused out of the glass in a controlled manner prior to or possibly during thermal bonding.

[0158] FIG. 6 shows an example of a glass block or glass blank having a thickness Z0, where the glass block is initially 1×10 14 molecule / cm 2 Assuming that H has a constant value of , several distributions of H2 concentration formed during the tempering process are shown. During the tempering process, depleted zones are first formed at the side edges of the glass block, while at the direct surface the concentration is 0 molecules / cm 2 , which rises approximately linearly inwards and plateaus in the central region. During tempering, the plateau gradually shrinks and only when a true inflection point is reached does the concentration also fall in the center of the glass block, resulting in a significantly lower H2 concentration in the center. The concentration gradient from the center concentration to the edge concentration remains the same, so the flow of hydrogen diffusing through the surface decreases only slightly as the size of the plateau decreases. Therefore, the aim is also to reduce the hydrogen concentration in the center of the glass block during tempering, for example to 1 / 10 of the initial content, in order to reduce the flow of hydrogen diffusing during thermal bonding.

[0159] One can also take advantage of the difference in the temperature dependence of H2 and OH diffusion, since most of the outward OH diffusion occurs during the hold step of the bond, e.g., at 1050°C, while the hydrogen concentration drops off, e.g., at 400°C. Relative to the diffusion rate of OH groups, the H2 profile is subcooled, i.e. does not reach high inward H2 concentrations quickly enough to provide hydrogen for the dissociation of OH groups. In that case, it is not necessarily necessary to lower the H2 concentration in the glass, since H2 depletion zones with a width of several mm or cm can form, especially in the region of the cooling channels 25.

[0160] Tempering can be performed on the usually cylindrical green glass body before separation into the two sectional bodies 26a, 26b, on the separate yet unstructured sectional bodies 26a, 26b (i.e. no recesses are introduced), on the structured sectional bodies 26a, 26b, or on the two sectional bodies 26a, 26b already in a pressed state (see also FIG. 2b). According to the paper "Wafer direct bonding: tailoring adhesion between brittle materials" (A. Plosl, G. Krauter, Materials Science and Engineering, R25 (1999) 1-88), tempering in a pressed state at 200°C to 400°C has the advantage that the water simultaneously diffuses along the bonding surface 27, which increases the bond strength, reduces its migration during heating for thermal bonding, and reduces the transverse OH gradient along the joint.

[0161] As mentioned above, if out-diffusion of hydrogen is to be allowed during thermal bonding, the tempering process must be carried out under reduced pressure or under heavy purging with air or inert gas to prevent accumulation of hydrogen in the cooling channels 25.

[0162] In the examples described herein, it has been found that the second partial body 26b preferably has a hydrogen content of 50% or less of the average hydrogen content of the second partial body 26b at a distance A' shown in Figure 3a from the lower wall 36b of the cooling channel 25 which corresponds to at least the land width b, preferably not more than 10 times the land width b of each land 25 and / or at least to the thickness D of the first partial body 26a and to the thickness D of the first partial body 26a between the channel upper wall 36a and the surface 32. The land width b is typically of the order of a few millimeters.

[0163] Yet another means of reducing the OH gradient in the titanium-doped quartz glass of the glass body 24 or substrate 31 is to at least partially perform the thermal bonding in saturated water vapor, water, or an oxidizing atmosphere, and / or to inhibit the outward diffusion of OH groups during thermal bonding by diffusing OH groups into the titanium-doped quartz glass of the glass body 24 through a post-treatment tempering process after thermal bonding.

[0164] FIG. 10a shows by way of example the progression of the OH content of a quartz glass produced by direct deposition, which has an average OH content of about 850 ppm by weight after a thermal bonding process at a holding temperature of 650 ° C and a holding time of 24 hours in the thickness direction Z in the immediate vicinity of the surface. The average OH content is in principle the maximum OH content of the quartz glass, since the thickness of the region with a lower or higher OH content than the maximum OH content is very small for diffusion-related reasons, and this region practically does not contribute much to the formation of an average in the total volume of the glass body. The solid curve shows the OH content during thermal bonding in an inert gas purged furnace, while the dashed and dotted curves show the OH content during thermal bonding in a furnace containing a partial pressure of water vapor well below 100%. The 25% partial pressure is shown as the dashed curve, and the 50% ratio as the dotted curve. The dashed and especially dotted progressions of the OH content may be acceptable, so that material removal from the channel walls 36 as described above is not necessary, or the necessary removal can at least be reduced.

[0165] 10b shows the OH content of a glass body 24 made of directly deposited quartz glass, where a post-treatment in the form of a heat treatment after thermal bonding increases the OH content after thermal bonding. The initial result of the post-treatment is the dashed curve shown in FIG. 10b, while the solid curve shown in FIG. 10b is achieved in the long term.

[0166] 11a, 11b show diagrams similar to 10a, 10b of a glass body 24 made of quartz glass deposited by the soot method with an average OH content of about 180 ppm by weight. The solid curve in 11a shows the case of a perfectly adjusted water vapor partial pressure during thermal bonding, where the OH content of the edge of the glass body 24 and thus of the channel walls 36 does not deviate practically from the average OH content of 180 ppm by weight. In 11a, the dashed curve represents the case where the selected water vapor partial pressure is too high, and the dotted curve represents the case where the selected water vapor partial pressure is too low. As is evident in 11a, the OH content of the edge of the glass body 24 and thus of the channel walls 36 also in these cases differs from the average OH content of the substrate 31 or the glass body 24 by less than 10% (corresponding to ±18 ppm by weight). The point at which the deviation from the average OH content, which may be more than 10%, depends on the bonding temperature and bonding time.

[0167] 11b shows the OH content of a completely dried and bonded quartz glass body 24 immediately after the start of the post-treatment as a dotted curve and the OH content at an ideally adjusted water vapor partial pressure after a very long time as a solid curve. As can be seen from the solid curve, the result in this case is also a distribution of OH contents that does not deviate substantially from an average OH content of about 180 ppm by weight.

[0168] In the quartz glass body 24 made of direct deposition quartz glass, when a water vapor partial pressure corresponding to approximately 100% or the solubility at each temperature is used, the curve of the distribution of the OH content is similar.

[0169] In the thermal bonding process shown in Figures 10a and 11a, it is generally desirable to begin the bonding process under dry conditions to allow surface and condensed water to diffuse out of the glass body before the addition of water vapor. Alternatively, the thermal bonding process can be carried out in water or in an oxidizing atmosphere to reduce out-diffusion.

[0170] In the above examples, the starting material was a glass body 24 in the form of titanium-doped quartz glass. However, the measures or findings described herein can also be applied or transferred to glass bodies 24 made of undoped quartz glass, which are used in the case of reflective optical elements for other wavelength ranges, for example the UV wavelength range. This is also at least partially applicable to glass bodies 24 made of glass ceramics.

Claims

1. an optical element (M2) for reflecting radiation, in particular EUV radiation (16), a substrate (31) made of quartz glass, in particular titanium-doped quartz glass or of glass ceramic, comprising a first part (26a) and a second part (26b) joined to one another along a bonding surface (27) by thermal bonding; a plurality of cooling channels (25) extending into the substrate (31) in the region of the bonding surface (27) and separated from one another by lands (35); a reflective coating (33) applied to a surface (32) of the first section body (26a); In the optical element (M2), Each cooling channel (25) has at least one location (P S ) at the center (M) of the land (35) over the entire side wall portion (36c, 36d) adjacent to each land (35), ZC,M ) deviating from the zero cross temperature (T) by less than 3.0 K, preferably less than 2.0 K, in particular less than 1.0 K. ZC,S ) adjacent to the land (35), and the flow wall (25) has a flow passage wall (36) having the at least one position (P S ), in particular over the entire side wall (36c, 36d) and / or at at least one position (P D ), in particular over the entire upper wall portion (36a), having an OH content ([OH]) of more than 0 ppm by weight, preferably more than 60 ppm by weight, in particular more than 120 ppm by weight.

2. 2. The optical element according to claim 1, wherein the flow path wall (36) is provided with at least one position (P D ) at the zero cross temperature (T) of the surface (32), particularly over the entire upper wall portion (36a) facing the surface (32). ZC,O ) deviating from the zero cross temperature (T) by less than 3.0 K, preferably less than 2.0 K, in particular less than 1.0 K. ZC,D ) an optical element having the same.

3. In an optical element according to the preamble of claim 1, in particular according to claim 1 or 2, each cooling channel (25) is arranged at at least one position (P S ), and having a flow path wall (36) having an OH content ([OH]) that deviates from the OH content ([OH]) at the center (M) of each land (35) by 60 ppm by weight or less, preferably 30 ppm by weight or less, and particularly 20 ppm by weight or less, particularly over the entire side wall portions (36c, 36d) adjacent to each land (35).

4. 4. The optical element according to claim 3, wherein the flow path wall (36) has at least one position (P) facing the surface (32) on which the reflective coating (33) is applied. D ), in particular over the entire upper wall portion (36a) facing said surface (32), having an OH content ([OH]) that deviates from the OH content ([OH]) of said surface (32) by 60 ppm by weight or less, preferably by 30 ppm by weight or less, in particular by 20 ppm by weight or less.

5. 5. An optical element according to claim 3 or 4, wherein a depletion region (30) adjacent to the flow path wall (36) in which the OH content ([OH]) of the substrate (31) is at least 5 ppm by weight lower than the OH content ([OH]) of the center (M) and / or the surface (32) of each land (35) has a thickness (d) of less than 50 μm, preferably less than 30 μm, in particular less than 1 μm.

6. An optical element according to any one of claims 1 to 5, wherein the OH content of the flow channel walls (26) deviates from the average OH content ([OH]) in the bulk of the substrate (31) by less than 10%, preferably less than 5%, in particular less than 1%.

7. Optical element according to any one of the preceding claims, wherein the channel walls (36) are at least partially, in particular completely, covered with a preferably metallic protective coating (38).

8. 8. The optical element according to claim 7, wherein the flow path wall (36) has a plurality of corner regions (39a to 39d), and the flow path wall (36) is covered with the protective coating (38) only on the outside of the corner regions (39a to 39d).

9. 9. An optical element according to claim 7 or 8, wherein the flow channel walls (36) are not covered with the protective coating (38) along slots (40) extending in the longitudinal direction (Y) of the cooling channel (25), preferably extending obliquely to said longitudinal direction (Y).

10. Optical element according to any one of the preceding claims, wherein the first part (26a), preferably the entire substrate (31), has a maximum OH content of less than 10 ppm by weight.

11. An optical element according to the preamble of claim 1, in particular according to any one of claims 1 to 10, in which the channel wall (36) of each cooling channel (25) has at least one slot-like recess (41a, 41b) preferably of a depth at least equal to the thickness (d) of the depletion region (30), more preferably at least twice the thickness (d) of the depletion region (30).

12. 12. The optical element of claim 11, wherein the flow path wall (36) has a plurality of corner regions (39a-39d), and the at least one slot-like recess (41a, 41b) is formed in one of the corner regions (39a-39d).

13. The optical element according to any one of claims 1 to 12, wherein the first part (26a), in particular the substrate (31), has a thickness of 1×10 15 molecule / cm 3 Less than or equal to 1×10 14 molecule / cm 3 The maximum hydrogen content ([H 2 ]) an optical element having the above structure.

14. 14. The optical element according to claim 13, wherein the second partial body (26b) has an average hydrogen content ([H 2 ) of at least one of the first partial body (26a) and the second partial body (26b) at a distance (A′) from the lower wall (36b) of the cooling channel (25) that corresponds at least to a land width (b), preferably at most ten times the land width (b) of each land (25) and / or at least to a thickness (D) of the first partial body (26a) and at most ten times the thickness (D) of the first partial body (26a) between the channel upper wall (36a) and the surface (32). 2 50% or less of hydrogen content ([H 2 ]) an optical element having the above structure.

15. An optical apparatus, in particular an EUV lithography system (1), comprising: At least one optical element (M2) according to any one of claims 1 to 14, A cooling device (37) designed to pass a cooling fluid through the cooling passages (25); An optical device comprising:

Citation Information

Patent Citations

  • METHOD OF MANUFACTURING SILICA GLASS CONTAINING TiO2, AND OPTICAL MEMBER FOR EUV LITHOGRAPHY EMPLOYING SILICA GLASS CONTAINING TiO2

    JP2006210404A

  • Method of manufacturing synthetic quartz glass lens having increased h2 content

    JP2007308365A

  • Titania-doped quartz glass and method for producing the same

    JP2011132086A

  • Substrate for EUV mask blanks

    JP2014033221A

  • ultra low expansion glass

    JP2016531082A