Ultra-thin copper foil with carrier foil for easy micro-hole processing, copper foil laminate including same, and method for manufacturing same

The ultra-thin copper foil with a carrier foil, featuring a surface treatment layer and additional layers, addresses the laser reflectance issue, enabling efficient and precise via hole processing for high-density printed wiring boards.

JP2024536265AActive Publication Date: 2024-10-04LOTTE ENERGY MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024519784
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-07-12
Publication Date
2024-10-04
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

Conventional ultra-thin copper foils with carrier foils reflect a significant portion of laser beams, limiting efficient via hole processing, especially when using CO2 gas lasers for high-density printed wiring boards requiring fine line widths and pitches.

Method used

The ultra-thin copper foil with a carrier foil features a surface treatment layer with protrusions and grooves to scatter and absorb laser light, combined with a diffusion prevention and heat-resistant layer, allowing for improved laser penetration and processing.

Benefits of technology

The new structure enables precise and efficient laser hole processing, facilitating the formation of via holes with larger diameters and reduced processing time, suitable for high-density printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536265000001_ABST
    Figure 2024536265000001_ABST
Patent Text Reader

Abstract

The present invention provides an ultra-thin copper foil with a carrier foil, which is formed by sequentially laminating a carrier foil, a release layer, and an ultra-thin copper foil, and the carrier foil includes a surface treatment layer on the surface facing the release layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ultra-thin copper foil with a carrier foil and a copper foil laminate using the same. [Background technology]

[0002] An ultra-thin copper foil with a carrier foil is formed by sequentially forming a release layer and an ultra-thin copper foil by electrolytic copper plating on one side of a carrier foil, and generally, the outermost surface of the ultra-thin copper foil formed by copper plating is finished as a roughened surface.

[0003] A printed wiring board using an ultra-thin copper foil with a carrier foil may be manufactured as follows. First, the ultra-thin copper foil with a carrier foil is placed on the surface of an insulating substrate made of resin or the like, and then heated and pressed to manufacture a copper foil laminate. Next, through-holes are formed and through-hole plating is performed in order in the manufactured laminate to form plated through holes, and then the copper foil on the surface of the laminate is etched to form a wiring pattern with the required line width and line pitch, and finally, a solder resist is formed and other processes are performed.

[0004] Meanwhile, in recent years, the roughened surface of copper foil is previously bonded to an adhesive resin such as epoxy resin, and the adhesive resin is used as an insulating resin layer in a semi-cured state (B stage), and the resin-bearing copper foil is used as a copper foil for forming a surface circuit, and the insulating resin layer is thermocompressed to an insulating substrate to manufacture a printed wiring board, particularly a build-up wiring board. In such a build-up wiring board, high integration of various electronic components is required, and correspondingly, high density wiring patterns are also required, so that wiring patterns consisting of wiring with fine line widths and line pitches, that is, fine pattern printed wiring boards are required. For example, high density printed wiring boards with line widths and line pitches of about 20 μm each are required. For the formation of via holes in build-up wiring boards, the laser via method using a CO2 gas laser is mainly used for reasons such as high productivity. However, when using a CO2 gas laser on a conventional carrier foil, ultra-thin copper foil, the wavelength of the CO2 gas laser is in the infrared region of around 10,600 nm, and the copper foil surface reflects most of the light in this region, so via holes cannot be directly processed, and a conformal mask method is used in which the copper foil in the area where the via holes are to be formed is first etched and removed, and then via holes are processed in the base material. However, the conformal mask method does not cover the area where the ultra-thin copper foil is to be formed with an etching resist, but covers other areas with an etching resist, so a complex method is used in which the ultra-thin copper foil is etched in advance and then via holes are processed in the board (resin part) with a CO2 gas laser. Therefore, if via holes could be processed simultaneously in the ultra-thin copper foil and the resin part using a CO2 gas laser, it would be possible to simplify the via hole processing.

[0005] For this reason, there is a demand for an ultra-thin copper foil with a carrier foil or a copper foil laminate containing the same that has a low reflectivity to a CO2 gas laser when processing through holes or via holes, and that can simultaneously process via holes in the ultra-thin copper foil and resin.

[0006] Therefore, Korean Patent Publication No. 2013-82320 provides an ultra-thin copper foil with a carrier foil, in which the release layer is made of a metal alloy layer with a specific content including a first metal, a second metal that facilitates plating of the first metal, and a third metal. However, even when processing via holes in such an ultra-thin copper foil with a CO2 laser, the copper foil surface still reflects a significant portion of the laser light, limiting efficient via hole processing. Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve the above-mentioned problems of the conventional technology, the present invention aims to provide an ultra-thin copper foil with a carrier foil having a new structure that allows easy laser hole processing, and a manufacturing method thereof.

[0008] Another object of the present invention is to provide an ultra-thin copper foil with a carrier foil that has excellent penetration processability with a CO2 laser, and a method for producing the same.

[0009] Another object of the present invention is to provide a copper foil laminate including the above-mentioned ultra-thin copper foil with a carrier foil. [Means for solving the problem]

[0010] In order to achieve the above technical objectives, the present invention provides an ultra-thin copper foil with a carrier foil, in which a carrier foil, a release layer, and an ultra-thin copper foil are laminated in this order, and the carrier foil includes a surface treatment layer on the surface facing the release layer.

[0011] In the present invention, the surface treatment layer may have a surface structure in which protrusions having an average diameter of 10 μm or less are arranged. In this case, the surface treatment layer may have a surface structure in which protrusions having an average diameter of 2 μm or less are arranged.

[0012] In the present invention, the protrusions are 8,000 to 10,000 / mm 2 The surface area density may be

[0013] In the present invention, the protrusions may be formed by etching the surface of the carrier foil.

[0014] In the present invention, the ultra-thin copper foil with a carrier foil may have a surface structure formed on the S-side of the ultra-thin copper foil after peeling, in which grooves having an average diameter of 10 μm or less are arranged.

[0015] In the present invention, the ultra-thin copper foil with a carrier foil may have a surface structure in which grooves having an average diameter of 2 μm or less are arranged on the S-side of the ultra-thin copper foil after peeling.

[0016] At this time, the grooves of the surface structure are 8,000 to 10,000 / mm 2 The density may be

[0017] In the present invention, the S-side of the peeled ultra-thin copper foil may contain Ni and P.

[0018] In addition, the present invention may further include a laser absorbing layer between the release layer and the ultra-thin copper foil, the laser absorbing layer containing Cu and at least one metal selected from the group consisting of Ni, Co, Fe, Pb, and Sn, or an alloy thereof.

[0019] The ultra-thin copper foil with a carrier foil of the present invention may further include a diffusion prevention layer between the carrier foil and the release layer. Also, the ultra-thin copper foil with a carrier foil of the present invention may further include a heat-resistant layer between the release layer and the ultra-thin copper foil.

[0020] In order to achieve the above-mentioned other technical object, the present invention provides a copper foil laminate comprising the above-mentioned ultra-thin copper foil with a carrier foil laminated on a resin substrate.

[0021] In order to achieve the above-mentioned further technical object, the present invention provides a method for producing an ultra-thin copper foil with a carrier foil, comprising the steps of forming a laminated structure of a carrier foil, a release layer and an ultra-thin copper foil, the laminated layer structure comprising the steps of: providing a carrier foil; etching one side of the carrier foil to form a surface treatment layer; and sequentially forming a release layer and an ultra-thin copper foil on the surface treatment layer.

[0022] In the present invention, the etching solution for the etching treatment may be prepared using one or more organic agents selected from sulfuric acid, hydrogen peroxide, sodium hydroxide, a nitrogen-containing organic compound, and a sulfur-containing organic compound. As the nitrogen-containing organic compound, 1,2,3-benzotriazole, carboxybenzotriazole, etc. can be used, and as the sulfur-containing organic compound, mercaptobenzothiazole, thiocyanuric acid, etc. can be used. Effect of the Invention

[0023] According to the present invention, it is possible to provide an ultra-thin copper foil with a carrier foil having a new structure that allows easy laser hole processing. Also, it is possible to provide an ultra-thin copper foil with a carrier foil that has precise and excellent penetration processability with a CO2 laser, and a copper foil laminate including the same. [Brief description of the drawings]

[0024] [Figure 1A] FIG. 1 is a diagram showing a laminated structure of an ultra-thin copper foil with a carrier foil according to an embodiment of the present invention. [Figure 1B] FIG. 1 is a diagram showing a laminated structure of an ultra-thin copper foil with a carrier foil according to an embodiment of the present invention.

[0025] [Figure 2A] 1 is an electron microscope photograph of the surface of a carrier foil according to an embodiment of the present invention. [Figure 2B] 1 is an electron microscope photograph of the surface of a carrier foil according to an embodiment of the present invention.

[0026] [Figure 3A] 1 is an electron microscope photograph of a surface of a copper foil after peeling off a carrier foil from a very thin copper foil specimen with a carrier foil manufactured according to an embodiment of the present invention. [Figure 3B] 1 is an electron microscope photograph of a surface of a copper foil after peeling off a carrier foil from a very thin copper foil specimen with a carrier foil manufactured according to an embodiment of the present invention.

[0027] [Figure 4A] 1 is an electron microscope image taken after laser through-hole processing of a carrier foil-attached ultra-thin copper foil specimen manufactured according to an embodiment of the present invention. [Figure 4B] 1 is an electron microscope image taken after laser through-hole processing of a carrier foil-attached ultra-thin copper foil specimen manufactured according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention, so it should be understood that there are various equivalents and modifications that can be substituted therefor. Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0029] In the present specification, the term "lamination" means bonding at least two or more layers together. For example, the lamination of a first layer and a second layer includes not only the direct contact between the first layer and the second layer, but also bonding the first layer and the second layer with an additional third layer sandwiched between them. In addition, in the laminate structure of the present invention, the presence of the third layer between the first layer and the second layer includes a state in which the third layer is in direct contact with the first layer and the second layer, and a state in which the third layer is not in direct contact with the first layer or the second layer.

[0030] 1A and 1B are schematic diagrams showing the laminated structure of an ultra-thin copper foil with a carrier foil according to one embodiment of the present invention.

[0031] First, referring to FIG. 1A, the ultra-thin copper foil with a carrier foil has a structure in which a carrier foil 100, a surface treatment layer 110, a diffusion prevention layer 120, a release layer 130, a heat-resistant layer 140, and an ultra-thin copper foil 150 are laminated in this order.

[0032] The carrier foil 100 serves as a support (carrier) until the ultra-thin copper foil is bonded to an insulating substrate. The carrier foil may be an aluminum foil, a stainless steel foil, a titanium foil, a copper foil, or a copper alloy foil. For example, an electrolytic copper foil, an electrolytic copper alloy foil, a rolled copper foil, or a rolled copper alloy foil may be used. Preferably, the carrier foil may be an electrolytic copper foil, and the upper surface 100B of the carrier foil may be either a glossy surface or a matte surface. In addition, a roughening treatment layer may be formed on the lower surface 100A of the carrier foil.

[0033] The carrier foil may have a thickness of 1 mm or less. For example, the carrier foil may have a thickness of 7 to 70 μm. For example, the carrier foil may have a thickness of 12 to 18 μm. If the thickness of the carrier foil is less than 7 μm, it is difficult for the carrier foil to function as a carrier. If the thickness of the carrier foil is more than 1 mm, there is no problem in functioning as a carrier, but when continuously plating to form a release layer and an ultra-thin copper foil, it is necessary to increase the tension of the foil in the continuous plating line, which may require large-scale equipment.

[0034] In the present invention, a surface treatment layer 110 is added between the carrier foil 100 and the diffusion prevention layer 120 or on the boundary surface between the carrier foil 100 and the diffusion prevention layer 120. In the present invention, the surface treatment layer 110 has a structure in which fine protrusions having an average diameter of 10 μm or less, 5 μm or less, 2 μm or less, or 1 μm or less are arranged. In the present invention, the average diameter of the fine protrusions is preferably 0.5 μm or more.

[0035] In the present invention, the area density of the fine protrusions is 8,000 to 10,000 / mm 2 It is preferable that:

[0036] Thus, in the present invention, the surface treatment layer has fine protrusions having a wavelength of CO2 laser or less (e.g., 10,600 nm), and as described below, the fine grooves formed after peeling in correspondence with these fine protrusions can scatter the laser light and promote absorption of the laser light.

[0037] In addition, in the present invention, the surface treatment layer 110 may be regarded as a smooth surface with low roughness, and the pole foil 150 formed thereon in sequence may also have a surface with low roughness. In the present invention, the surface treatment layer 110 preferably has a surface roughness of 0.5 to 1.5 μm.

[0038] Preferably, in the present invention, the surface treatment layer 110 may be formed by etching the surface of the carrier foil 100. For example, the surface treatment layer 110 may be formed by treating the surface of the carrier foil 100 with an etching solution containing sulfuric acid, hydrogen peroxide, sodium hydroxide, and at least one type of BTA (benzotriazole).

[0039] In the present invention, the diffusion prevention layer 120 and the heat-resistant layer 140 may contain one or more elements selected from the group consisting of Ni, Co, Fe, Cr, Mo, W, Al, and P. For example, the diffusion prevention layer and the heat-resistant layer may be a single metal layer, an alloy layer of two or more metals, or a layer of one or more metal oxides.

[0040] For example, plating for forming a single metal layer may be nickel plating, cobalt plating, iron plating, aluminum plating, etc. Plating for forming a binary alloy layer may be nickel-cobalt plating, nickel-iron plating, nickel-chromium plating, nickel-molybdenum plating, nickel-tungsten plating, nickel-copper plating, nickel-phosphorus plating, cobalt-iron plating, cobalt-chromium plating, cobalt-molybdenum plating, cobalt-tungsten plating, cobalt-copper plating, cobalt-phosphorus plating, etc. The plating that forms a ternary alloy layer is nickel-cobalt-iron plating, nickel-cobalt-chromium plating, nickel-cobalt-molybdenum plating, nickel-cobalt-tungsten plating, nickel-cobalt-copper plating, nickel-cobalt-phosphorus plating, nickel-iron-chromium plating, nickel-iron-molybdenum plating, nickel-iron-tungsten plating, nickel-iron-copper plating, nickel-iron-phosphorus plating, nickel-chromium-molybdenum plating, nickel-chromium-tungsten plating, nickel-chromium-copper plating, nickel-chromium-phosphorus plating, nickel-molybdenum-tungsten plating, nickel-molybdenum-copper plating, nickel-molybdenum Cobalt-iron-chromium plating, nickel-tungsten-copper plating, nickel-tungsten-phosphorus plating, nickel-copper-phosphorus plating, cobalt-iron-chromium plating, cobalt-iron-molybdenum plating, cobalt-iron-tungsten plating, cobalt-iron-copper plating, cobalt-iron-phosphorus plating, cobalt-chromium-molybdenum plating, cobalt-chromium-tungsten plating, cobalt-chromium-copper plating, cobalt-chromium-phosphorus plating, cobalt-molybdenum-phosphorus plating, cobalt-tungsten-copper plating, cobalt-molybdenum-phosphorus plating, cobalt-tungsten-copper plating, cobalt-tungsten-phosphorus plating, cobalt-copper-phosphorus plating, and cobalt-copper-phosphorus plating may be used.

[0041] Preferably, the diffusion prevention layer 120 and the heat-resistant layer 140 may contain Ni and P.

[0042] The diffusion prevention layer 120 prevents copper from diffusing into the release layer when the carrier foil-attached ultra-thin copper foil is pressed against an insulating substrate at high temperature. The diffusion of copper into the release layer may generate metallic bonds between the carrier foil and the ultra-thin copper foil, and the strong bonding force of these bonds may make it difficult to peel off the carrier foil. The diffusion prevention layer 120 can prevent such a reaction.

[0043] In the copper foil with carrier foil, the release layer 130 is a layer for improving the peelability when peeling the ultra-thin copper foil from the carrier foil, and is introduced to peel the carrier foil cleanly and easily. The release layer is removed together with the carrier foil.

[0044] In the present invention, the release layer 130 may include a metal or metal alloy having release properties. The release metal may include molybdenum or tungsten. The release layer 130 may also include a plating catalyst. For example, the release layer 130 may include at least one metal selected from the group consisting of Fe, Co, and Ni.

[0045] The release layer may be an organic release layer having releasability, for example, the release layer may contain at least one organic material selected from the group consisting of BTA series.

[0046] The ultra-thin copper foil 150 may have a thickness of 12 μm or less. Preferably, the ultra-thin copper foil may have a thickness of 1.5 to 5 μm.

[0047] In the present invention, the ultra-thin copper foil preferably has a surface roughness (Rz) of 0.5 to 1.5 μm.

[0048] The ultra-thin copper foil may have a roughened side and a non-roughened side depending on the application. The roughened side may be formed by a nodulation process, and the non-roughened side may be formed by adding a brightener and a suppressor when forming the copper foil.

[0049] In the present invention, the surface of the ultra-thin copper foil may be further surface-treated. For example, heat and chemical resistance treatment, chromate treatment, silane coupling treatment, or a combination thereof may be used. Which surface treatment is to be performed may be appropriately selected depending on the subsequent process.

[0050] The heat and chemical resistance treatment can be performed by forming a thin film of any one of metals such as nickel, tin, zinc, chromium, molybdenum, and cobalt, or an alloy thereof, on the metal foil by sputtering, electroplating, or electroless plating. From the viewpoint of cost, electroplating is preferred.

[0051] For the chromate treatment, an aqueous solution containing hexavalent to trivalent chromium ions can be used. The chromate treatment can be a simple immersion treatment, but is preferably performed as a cathodic treatment. For example, the cathodic treatment is performed in a solution of 0.1 to 70 g / L sodium dichromate, pH 1 to 13, bath temperature 15 to 60° C., current density 0.1 to 5 A / dm 2 It is preferable to carry out the electrolysis under the condition of 0.1 to 100 seconds. In addition, it is preferable to carry out the chromate treatment on top of the rust prevention treatment, which can further improve the moisture resistance and heat resistance.

[0052] The silane coupling agent used in the silane coupling treatment may be one or more substances or mixtures selected from the group consisting of epoxy-functional silanes such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino-functional silanes, olefin-functional silanes, acryl-functional silanes, methacryl-functional silanes, and mercapto-functional silanes. For example, the silane coupling agent is dissolved in a solvent such as water at a concentration of 0.1 to 15 g / L, and applied to a metal foil at a temperature of room temperature to 70°C or electrodeposited to be adsorbed. After the silane coupling treatment, a stable bond can be formed by heating, ultraviolet irradiation, or the like. Heating may be performed at a temperature of 100 to 200°C for 2 to 60 seconds.

[0053] Another embodiment of the present invention will now be described with reference to FIG. 1B.

[0054] The ultra-thin copper foil with carrier foil shown in FIG. 1B differs from that shown in FIG. 1A in that it further includes a laser absorbing layer 160 between the release layer 130 and the heat-resistant layer 140 .

[0055] The laser absorbing layer 160 is composed of a plating layer with low gloss and dark color. For example, the laser absorbing layer 160 may include Cu and at least one metal selected from the group consisting of Ni, Co, Fe, Pb, and Sn or an alloy thereof, for example, one, two, or three metals or an alloy thereof.

[0056] In the present invention, the thickness of the laser absorbing layer 160 is preferably 0.01 to 1 μm. More preferably, the thickness of the laser absorbing layer 160 may be 0.05 to 0.5 μm. If the thickness is 0.05 μm, the absorbing layer has almost no effect on the color change, and if the thickness is 1 μm or more, the color is too dark and defects such as penetration during laser processing may occur.

[0057] The ultra-thin copper foil with carrier foil shown in FIG. 1B can exhibit higher laser absorption by adding the laser absorbing layer 160. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples. However, these are presented as preferred examples of the present invention and are not to be construed as limiting the present invention in any sense.

[0059] <Example 1>

[0060] A laminate structure was formed in the following order.

[0061] [A. Carrier foil]

[0062] An electrolytic copper foil having a thickness of 18 μm and a surface roughness (Rz) of 1.2 μm on the shiny side was immersed in 100 g / L sulfuric acid for 5 seconds, pickled, and then washed with pure water.

[0063] [B. Surface treatment layer]

[0064] The surface of the carrier foil was pretreated and activated with the following pretreatment solution.

[0065] a. Use one or more organic agents selected from sulfuric acid: 200-300 g / L, hydrogen peroxide: 50-150 g / L, nitrogen-containing organic compounds, and sulfur-containing organic compounds.

[0066] b.Temperature: 40℃

[0067] c. pH: 0.01 to 0.5

[0068] d. Soaking time: 5 seconds

[0069] [C. Diffusion prevention layer]

[0070] A diffusion barrier layer was formed using Ni-P plating under the following plating conditions.

[0071] a.Ni concentration: 10~20g / L, P concentration 5~15g / L

[0072] b.pH: 4.0, temperature: 30℃, current density: 1.5A / dm 2 , Plating time: 2 seconds

[0073] The amount of adhesion of the formed diffusion prevention layer is 301ug / dm 2 It was.

[0074] [D. Peeling layer]

[0075] A peeling layer was formed by plating Mo-Ni-Fe under the following plating conditions.

[0076] a. Mo concentration: 10-30g / L, Ni concentration: 3-10g / L, Fe concentration: 1-7g / L, sodium citrate: 100-200g / L, pH: 10.2 (30ml / L of ammonia water added)

[0077] b. Temperature: 30℃, current density: 10A / dm 2 , Plating time: 7 seconds

[0078] The adhesion weight of the formed peeling layer was 1.01 mg / dm 2 The composition of the peeled layer was 62.31 wt % Mo, 30.8 wt % Ni, and 6.89 wt % Fe.

[0079] [E.Heat-resistant layer]

[0080] The heat-resistant layer was formed by Ni-P plating under the following plating conditions.

[0081] a.Ni concentration: 10~20g / L, P concentration 5~15g / L, pH: 4.0

[0082] b. Temperature: 30℃, current density: 1.5A / dm 2 , Plating time: 2 seconds

[0083] The amount of adhesion of the formed diffusion prevention layer is 301ug / dm 2 It was.

[0084] [F. Copper foil]

[0085] A copper foil with a thickness of 2 μm was formed using the following plating conditions:

[0086] a.CuSO4-5H2O:300g / L, H2SO4:150g / L

[0087] b. Temperature: 35℃, current density: 20A / dm 2 , Plating time: 30 seconds

[0088] [G. Additional Processing]

[0089] The surface of the pole copper foil was further subjected to a heat and chemical resistance treatment, a chromate treatment, and a silane coupling treatment.

[0090] <Example 2>

[0091] Except for adding a laser absorbing layer between the release layer and the heat resistant layer, an ultra-thin copper foil with a carrier foil was manufactured in the same manner as in Example 1. The laser absorbing layer was formed by plating under the following conditions.

[0092] a. Copper concentration: 1-5g / L, nickel concentration: 1-5g / L, cobalt concentration: 1-10g / L, ammonium sulfate: 10-50g / L, sodium citrate: 30-70g / L

[0093] b.pH: 4.5, temperature: 30℃, current density: 20A / dm 2 , Plating time: 4 seconds

[0094] <Example 3>

[0095] Except for forming an organic release layer as the release layer, an ultra-thin copper foil with a carrier foil was manufactured in the same manner as in Example 2. The organic release layer was formed by plating under the following conditions.

[0096] a. Carboxybenzotriazole concentration: 1-5g / L, copper concentration: 5-15g / L, H2SO4 concentration: 150g / L

[0097] b. Temperature: 40℃, immersion time: 30 seconds

[0098] <Comparative Example 1>

[0099] An ultra-thin copper foil with a carrier foil was produced in the same manner as in Example 1, except that the surface treatment layer was omitted.

[0100] <Comparative Example 2>

[0101] An ultra-thin copper foil with a carrier foil was produced in the same manner as in Example 2, except that the surface treatment layer was omitted.

[0102] <Experimental Example>

[0103] The surface roughness (Rz) was measured from the ultra-thin copper foil specimens with carrier foils manufactured in Examples 1 to 3 and Comparative Example 1 and Comparative Example. In addition, the manufactured specimens were peeled off, and the gloss and color of the peeled surface (S surface) were measured. The measurement conditions for surface roughness, gloss, and color were as follows.

[0104] a.Surface roughness

[0105] Measurement equipment: SURFCOM 1400D (TSK, Tokyo Seimitsu)

[0106] Measurement standard: Measured according to IPC-TM-650 standard

[0107] b. Glossiness

[0108] Measurement equipment: Gloss Metal VG7000, NIPPON DENSHOKU

[0109] Measurement standard: Gs (60°), JIS Z871-1997

[0110] c.Color

[0111] Measurement equipment: CM-2500d, KONIKA MINOLTA

[0112] Measurement standard: SCE, L* measurement

[0113] The laser processability of the ultra-thin copper foil specimens with carrier foils produced in Examples 1 to 3 and Comparative Example 1 and Comparative Example was evaluated. The laser process conditions were as follows.

[0114] d. Laser processability evaluation

[0115] After peeling off the ultra-thin copper foil with the carrier foil, the obtained ultra-thin copper foil specimen was subjected to one-shot processing of a via hole size of 30 μm using a carbon dioxide gas laser via hole processing machine, and the size of the via hole formed in the copper foil by one-shot processing was measured at laser outputs of 7 W and 5 W. At this time, the laser processing equipment used was a Laser drilling machine LC-4K series manufactured by Hitachi.

[0116] Table 1 below summarizes the evaluation results for surface roughness, gloss, color and laser processability.

[0117] [Table 1]

[0118] From Table 1, it can be seen that in Example 1, in which a surface treatment layer was formed on the surface of the carrier foil, the S-side gloss of the peeled pole foil was lower and the hole size by the CO2 laser was increased compared to Comparative Example 1, in which no surface treatment layer was formed. On the other hand, it can be seen that in Examples 2 and 3, in which both the surface treatment layer and the laser absorption layer were formed, the difference in gloss and color was more noticeable compared to Example 1, and the laser hole size was increased.

[0119] 2A and 2B are electron microscope photographs of the carrier foil surface before and after the formation of the surface treatment layer during the production process of Example 1, respectively.

[0120] This photograph shows that a protrusion structure has developed on the surface as a result of the surface treatment.

[0121] 3A and 3B are electron microscope photographs of the S-side of ultra-thin copper foils peeled from the specimens of Comparative Example 1 and Example 2, respectively.

[0122] From this photograph, it can be seen that Comparative Example 1, which does not have a surface treatment layer, shows the same state as the carrier foil surface, whereas Example 2 shows an intaglio structure with an array of multiple recessed grooves with an average diameter of 2 μm or less. It can be seen that this structure substantially corresponds to the surface relief structure in FIG. 2B.

[0123] 4A and 4B are electron microscope images of through holes after laser processing of the specimens manufactured according to Example 2 and Comparative Example 1, respectively. As shown in the figures, it can be seen that holes with a larger opening diameter are formed in the specimens of the examples compared to the comparative examples at the same laser output. This result shows that the ultra-thin copper foil with carrier foil having the laminated structure of the present invention makes it possible to form via holes or through holes with a shorter time and / or a wider diameter than conventional methods.

[0124] Although the preferred embodiment of the present invention has been described in detail above, those skilled in the art will understand that various modifications can be made to the above-described embodiment without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the appended claims and equivalents thereto. [Industrial Applicability]

[0125] The present invention is applicable to a copper foil with a carrier foil and a copper foil laminate using the same.

Claims

1. An ultra-thin copper foil with a carrier foil, in which a carrier foil, a release layer and an ultra-thin copper foil are laminated in this order, The carrier foil includes a surface treatment layer on a surface facing the release layer.

2. The ultra-thin copper foil with a carrier foil according to claim 1 , wherein the surface treatment layer has a surface structure in which protrusions having an average diameter of 10 μm or less are arranged.

3. The ultra-thin copper foil with a carrier foil according to claim 2 , wherein the surface treatment layer has a surface structure in which protrusions having an average diameter of 2 μm or less are arranged.

4. The protrusions are 8,000 to 10,000 per mm 2 The ultra-thin copper foil with a carrier foil according to claim 2 or 3, characterized in that it has an areal density of

5. The ultra-thin copper foil with a carrier foil according to claim 2 or 3, wherein the protrusions are formed by etching a surface of the carrier foil.

6. The ultra-thin copper foil with a carrier foil according to claim 1, characterized in that after peeling, a surface structure is formed on the S-side of the ultra-thin copper foil in which grooves with an average diameter of 10 μm or less are arranged.

7. The ultra-thin copper foil with a carrier foil according to claim 1, characterized in that after peeling, a surface structure is formed on the S-side of the ultra-thin copper foil in which grooves with an average diameter of 2 μm or less are arranged.

8. The grooves are 8,000 to 10,000 per mm 2 The ultra-thin copper foil with a carrier foil according to claim 6 or 7, characterized in that it has a density of

9. The ultra-thin copper foil with a carrier foil according to claim 6 or 7, wherein the S-side of the peeled ultra-thin copper foil contains Ni and P.

10. Between the release layer and the ultra-thin copper foil, The ultra-thin copper foil with a carrier foil according to claim 1, further comprising a laser absorbing layer containing Cu and at least one metal selected from the group consisting of Ni, Co, Fe, Pb and Sn or an alloy thereof.

11. The ultra-thin copper foil with a carrier foil according to any one of claims 1 to 3, 6, 7 and 10, further comprising a diffusion prevention layer between the carrier foil and the release layer.

12. The ultra-thin copper foil with a carrier foil according to any one of claims 1 to 3, 6, 7 and 10, further comprising a heat-resistant layer between the release layer and the ultra-thin copper foil.

13. A copper foil laminate obtained by laminating the ultra-thin copper foil with a carrier foil according to any one of claims 1 to 3, 6, 7 and 10 on a resin substrate.

14. A method for producing an ultra-thin copper foil with a carrier foil, comprising forming a laminate structure of a carrier foil, a release layer and an ultra-thin copper foil, The laminate structure is providing a carrier foil; Etching one side of the carrier foil to form a surface treatment layer; and The method for producing an ultra-thin copper foil with a carrier foil, comprising the steps of sequentially forming a release layer and an ultra-thin copper foil on the surface treatment layer.

15. The method for producing an ultra-thin copper foil with a carrier foil according to claim 14, characterized in that the etching solution for the etching treatment contains one or more organic agents selected from the group consisting of sulfuric acid, hydrogen peroxide, nitrogen-containing organic compounds, and sulfur-containing organic compounds.

Citation Information

Patent Citations

  • Copper foil for high-density ultrafine wiring board

    CN1466517A

  • Ultrathin copper foil with carrier and method for manufacturing the same, and printed wiring board using ultrathin copper foil with carrier

    JP2004169181A

  • Copper foil having laser absorbing layer, copper clad laminate using copper foil and printed wiring board

    JP2013075443A

  • Copper foil with carrier, laminate, production method of copper foil with carrier, production method of laminate, production method of printed wiring board, and production method of electronic device

    JP2018168409A

  • Ultra-thin copper foil with carrier foil

    JP2020506296A