Dialkylphosphinic acid hybrid salts and their preparation and use

A dialkyl phosphinic acid hybrid salt with a specific composition addresses the limitations of existing dialkyl phosphinates by enhancing flame retardant efficiency and thermal stability, making it suitable for diverse polymer materials, including those requiring high-temperature processing.

JP2024536906AActive Publication Date: 2024-10-08NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024521757
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-15
Publication Date
2024-10-08
Estimated Expiration
2041-10-15

AI Technical Summary

Technical Problem

Existing dialkyl phosphinates, such as aluminum diisobutylphosphinate, have low thermal stability and limited flame retardant efficiency for high-temperature processing and are not effective on all polymer materials, particularly glass fiber reinforced nylon and polyester, while aluminum diethylphosphinate has high volatility and affects the physical properties of polymers.

Method used

A dialkyl phosphinic acid hybrid salt with a specific composition (formula I) is developed, comprising paired diethylphosphinate, ethylisobutylphosphinate, and diisobutylphosphinate ions with a metal element, offering improved flame retardant efficiency and thermal stability by forming a single or overlapping double peak in XRD spectra.

Benefits of technology

The hybrid salt achieves high flame retardant efficiency with excellent thermal stability and economic efficiency, suitable for various polymer materials, including those requiring high-temperature processing, without adversely affecting physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536906000001_ABST
    Figure 2024536906000001_ABST
Patent Text Reader

Abstract

The present application discloses a dialkylphosphinic acid hybrid salt and its preparation method and use, and the dialkylphosphinic acid hybrid salt is at least one selected from compounds having the chemical formula shown in formula (I). The dialkylphosphinic acid hybrid salt having the composition of formula (I) according to the present application has a small amount of addition, a high flame retardant efficiency for various polymeric materials, and is economically excellent, which not only overcomes the disadvantages of diethylphosphinic acid salt, which is low in flame retardant efficiency for polymeric materials, but also overcomes the disadvantages of diisobutylphosphinic acid salt, which is too volatile and low in flame retardant efficiency for polyester, but can also be widely used in the flame retardancy of various polymeric materials that require high-temperature processing. JPEG2024536906000030.jpg50153
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a dialkylphosphinic acid hybrid salt and its preparation method and use, which are in the field of producing flame-retardant polymeric materials. [Background technology]

[0002] Dialkyl phosphinates, especially aluminum diethyl phosphinate, are widely used as halogen-free flame retardants for polymer materials. Dialkyl phosphinate-based flame retardant products have low density, low flame retardant usage, and good mechanical properties, but existing dialkyl phosphinates have limited flame retardant efficiency as flame retardants. For example, polydialkyl phosphinates can be used as flame retardants without glass fiber reinforced nylon, but their flame retardant efficiency is low and they can have a significant negative impact on the physical properties of flame retarded polymer materials when used. There have also been reports of the use of aluminum diisobutyl phosphinate to make nylon flame retardant. Although aluminum diisobutyl phosphinate has a very high flame retardant efficiency, it has low thermal stability and begins to decompose and volatilize in large amounts at 300°C, which is disadvantageous for engineering plastics that require high-temperature processing. In addition, aluminum diisobutyl phosphinate does not have a good flame retardant effect on polyester. In addition, its high plasticity is disadvantageous to the physical properties of flame retarded polymers. Summary of the Invention [Problem to be solved by the invention]

[0003] In order to solve the above technical problems, the present application provides a dialkylphosphinic acid hybrid salt having a composition of formula (I), which can be added in a small amount, has high flame retardancy efficiency for various polymer materials, and is economical, as well as a production method thereof and use thereof. [Means for solving the problem]

[0004] According to a first aspect of the present application, there is provided a dialkylphosphinic acid hybrid salt, which is at least one selected from compounds having a chemical formula represented by formula (I): [ka] Here, M is a central atom, and the diethylphosphinate ion, the ethylisobutylphosphinate ion, and the diisobutylphosphinate ion are all ligands. M is selected from a metal element, and the metal element is at least one selected from the group consisting of group IIA, IIIA, IVA, and VA metal elements, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; 0≦x≦0.95, 0.05≦y≦0.8, 0≦z≦0.5, and x+y+z=1, and x+z>0.

[0005] In the embodiment of the present application, in formula (I), when y is less than 0.05, the flame retardant effect is not good. When y is greater than 0.8, the production cost is high, the economic efficiency is poor, and the thermal stability of the dialkylphosphinic acid hybrid salt is reduced, which is disadvantageous to the production and physical properties of the flame retardant polymer material. When x is greater than 0.95, the flame retardant properties are not good. When z is greater than 0.5, the production cost is high, the economic efficiency is poor, and the thermal stability is reduced, which is disadvantageous to the production and physical properties of the flame retardant polymer material.

[0006] Alternatively, the lower limit of x is independently selected from 0, 0.15, 0.2, 0.25, 0.3, 0.35, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.03 and the upper limit is independently selected from 0.95, 0.9, 0.85, 0.87, 0.7.

[0007] Alternatively, the lower limit of y is independently selected from 0.05, 0.1, 0.15, 0.2, 0.13, 0.29 and the upper limit is independently selected from 0.8, 0.7, 0.6, 0.5, 0.4, 0.35, 0.3, 0.25, 0.68.

[0008] Alternatively, the lower limit of z is independently selected from 0, 0.02 and the upper limit is independently selected from 0.5, 0.45, 0.4, 0.35, 0.3, 0.25, 0.2, 0.15, 0.1, 0.05.

[0009] Optionally, the Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, Ba; The group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The lanthanide metal element is Ce.

[0010] Optionally, the metal element is at least one selected from Al, Zn, Ca, Fe.

[0011] Optionally, the metal element is Al and n=3.

[0012] Alternatively, 0.03≦x≦0.87, 0.13≦y≦0.68, and 0≦z≦0.45.

[0013] Alternatively, 0.03≦x≦0.7, 0.29≦y≦0.68, and 0.01≦z≦0.45.

[0014] Optionally, 0.5≦x≦0.7, 0.29≦y≦0.48, and 0.01≦z≦0.21.

[0015] In the examples of the present application, the larger the z value, the faster the thermal weight loss of the dialkylphosphinic acid hybrid salt.

[0016] The dialkylphosphinic acid hybrid salt in the present application is not a simple physical mixture of different dialkylphosphinic acid salts, for example, it is not a simple mixture of aluminum diethylphosphinate and aluminum ethylisobutylphosphinate, but may contain diethylphosphinic acid salt ions, ethylisobutylphosphinic acid salt ions, and diisobutylphosphinic acid ions that are paired with the same aluminum atom. The X-ray diffraction spectrum (XRD) of these hybrid salts is very different from the XRD spectrum of a simple physical mixture of dialkylphosphinic acid salts. The dialkylphosphinic acid hybrid salt having the composition of formula (I) shows a single peak or overlapping double peaks in the strongest absorption peak region in the XRD spectrum. In addition, the crystal plane spacing shown by the maximum peak is different from that of aluminum diethylphosphinate and aluminum diisobutylphosphinate. The maximum peak of aluminum diethylphosphinate has a crystal plane spacing d=9.663, and the maximum peak of aluminum diisobutylphosphinate has a crystal plane spacing d=12.084, while the value of the crystal plane spacing d of the dialkylphosphinic acid hybrid salt having formula (I) is between the above two. Even in the case of overlapping double peaks, their d values ​​indicate that they are not pure aluminum diethylphosphinate or aluminum diisobutylphosphinate. However, a physical mixed salt obtained by simply mixing aluminum diethylphosphinate and aluminum diisobutylphosphinate shows two completely independent peaks in the XRD spectrum, and their d values ​​are close to the d values ​​of aluminum diethylphosphinate and aluminum diisobutylphosphinate, respectively.

[0017] In the examples of the present application, when the dialkylphosphinic acid hybrid salt having the composition of formula (I) and aluminum diethylphosphinate are simply physically mixed, two independent peaks appear in the XRD spectrum. These results strongly indicate that the dialkylphosphinic acid hybrid salt having the composition of formula (I) obtained by the present invention is not a simple mixture of aluminum diethylphosphinate, aluminum ethylisobutylphosphinate, and aluminum diisobutylphosphinate, but contains a structure in which diethylphosphinate, ethylisobutylphosphinate, and diisobutylphosphinate are paired with the same aluminum atom.

[0018] In the examples of the present application, the flame retardant effect of pure diethylphosphinate or diisobutylphosphinate is much inferior to that of the hybrid salt containing both diethylphosphinate and ethylisobutylphosphinate at the same usage amount.The flame retardant property is also related to the content of ethylisobutylphosphinate, and only the composition in which y is within a certain range has excellent flame retardant property, thermal property and excellent economical efficiency.

[0019] According to a second aspect of the present application, there is provided a method for producing the above-mentioned dialkylphosphinic acid hybrid salt, the method comprising the steps of: A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylisobutylphosphinic acid and / or an alkali metal salt thereof, and diisobutylphosphinic acid and / or an alkali metal salt thereof.

[0020] Alternatively, the molar ratio of diethylphosphinic acid and / or its alkali metal salt, ethylisobutylphosphinic acid and / or its alkali metal salt, diisobutylphosphinic acid and / or its alkali metal salt, and metal element source M is close to x:y:z:q; Here, q = 1 / n.

[0021] The solubility of the hybrid salt in water varies depending on the M. In the case of a hybrid salt with high solubility, the values ​​of x, y, and z of diethylphosphinic acid and / or its alkali metal salt, ethylisobutylphosphinic acid and / or its alkali metal salt, and diisobutylphosphinic acid and / or its alkali metal salt in the solution differ from the values ​​of x, y, and z in the hybrid salt, so the molar ratio with the M source also changes. In addition, in order to obtain a larger amount of M-containing precipitate, the molar ratio of x, y, and z of the reactants to M may exceed the theoretically calculated value.

[0022] During actual operation, the actual values ​​of x, y, z, and q can be determined by phosphorus nuclear magnetism.

[0023] Alternatively, the molar ratio of diethylphosphinic acid and / or an alkali metal salt thereof, ethylisobutylphosphinic acid and / or an alkali metal salt thereof, and diisobutylphosphinic acid and / or an alkali metal salt thereof in the mixture A is the same or substantially the same as the ratio of x, y, and z in formula (I).

[0024] Alternatively, the conditions for the reaction I are a temperature of 0 to 250° C., a pressure of 0.1 to 10 MPa, and a time of 0.1 to 20 hours.

[0025] Optionally, obtaining the mixture A comprises: The method includes a step of introducing ethylene and isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and carrying out reaction II to obtain the mixture A.

[0026] Alternatively, the molar ratio of the phosphinic acid and / or its alkali metal salt, ethylene, and isobutene is 1:0.05-1.95:0.5-1.5.

[0027] In actual reactions, the amount of olefin consumed is higher than the theoretical ratio due to side reactions such as the formation of long-chain dialkylphosphinate salts by polymerization of ethylene.

[0028] Optionally, the molar ratio of the phosphinic acid and / or its alkali metal salt to ethylene and isobutene is the same as or close to the ratio of x, y and z in formula (I). Optionally, in the reaction II, the reaction rate depends on the ratio of x, y and z. The larger the z value is, the slower the reaction rate is, so the z value needs to be controlled to obtain economic efficiency. In addition, during the reaction of the phosphinic acid or its alkali metal salt with ethylene or isobutene, the value of y has a maximum value less than 1, and after reaching this maximum value, x or z increases, so that y does not reach 1. If it is necessary to make y=1, it is necessary to separate and purify the reaction intermediate product to remove diethylphosphinic acid and / or diisobutylphosphinic acid or their salts, which is economically disadvantageous.

[0029] Specifically, in reaction II, the order of addition of ethylene and isobutene may be reversed, they may be added simultaneously, or a portion of them may be added first.

[0030] Alternatively, in reaction II, phosphinic acid and / or its alkali metal salt is reacted with isobutene to obtain the corresponding values ​​of y and z, followed by substantially complete or complete reaction with ethylene. By "substantially complete," it is meant that the total phosphorus contained in the ethylphosphinate, isobutylphosphinate, and phosphinate salts in the reaction mixture is less than 5% molar of the total phosphorus in the reaction mixture.

[0031] Specifically, after completion of reaction I, the next reaction may be carried out without separating diethylphosphinic acid, ethylisobutylphosphinic acid, diisobutylphosphinic acid, or a mixture of alkali metals thereof.

[0032] Optionally, the mass of the water in the aqueous solution is 10 to 99% of the total mass of the radical initiator and the phosphinic acid and / or the alkali metal salt thereof.

[0033] Specifically, if the aqueous solution contains too little water, the solubility of the olefin in water decreases due to a salting-out effect, slowing down the reaction rate, whereas if the aqueous solution contains too much water, the utilization rate of the reaction vessel decreases.

[0034] Optionally, the mass of the water in the aqueous solution is 20 to 95% of the total mass of the radical initiator and the phosphinic acid and / or its alkali metal salt.

[0035] Optionally, the mass of the water in the aqueous solution is 45 to 92% of the total mass of the radical initiator and the phosphinic acid and / or its alkali metal salt.

[0036] Optionally, the mass of the water in the aqueous solution is 50 to 90% of the total mass of the radical initiator and the phosphinic acid and / or its alkali metal salt.

[0037] Optionally, the mass of the water in the aqueous solution is 55 to 90% of the total mass of the radical initiator and the phosphinic acid and / or its alkali metal salt.

[0038] Alternatively, the conditions for the reaction II are a temperature of 0 to 250° C., a time of 0.01 to 50 h, and a pressure of 0 to 3 MPa.

[0039] Specifically, if the temperature of the reaction II is too low, the reaction rate is slow, whereas if the temperature is too high, the phosphinate is likely to decompose.

[0040] Optionally, the temperature of the reaction II is 10 to 200°C.

[0041] Specifically, the pressure of the reaction II is higher than 3 MPa, and the pressure required for the reaction apparatus is high, making the operation difficult.

[0042] Optionally, the pressure of the reaction II is 0.2 to 1.5 MPa.

[0043] Alternatively, the molar ratio of the radical initiator to the phosphinic acid and / or its alkali metal salt is 0.001-0.1:1.

[0044] Optionally, the radical initiator is at least one selected from azo-based initiators, peroxide-based initiators, and photoinitiators, wherein the amount of the radical initiator added can be determined according to practical needs.

[0045] Optionally, the azo initiator is selected from cationic and / or non-cationic azo initiators, including one or more of azodiisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-amidinopropane) dichloride, 2,2'-azodiisobutylamidino dihydrochloride.

[0046] Alternatively, the peroxide-based initiator is preferably an inorganic peroxide and an organic peroxide radical initiator, and particularly preferably one or more of hydrogen peroxide, ammonium persulfate, potassium persulfate, sodium persulfate, sodium percarbonate, benzoyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, and peracetic acid.

[0047] Preferably, the radical initiator is a peroxide-based initiator, and more preferably, the radical initiator is one selected from ammonium persulfate, potassium persulfate, and sodium persulfate.

[0048] Alternatively, the molar ratio of the radical initiator to the phosphinic acid and / or its alkali metal salt is 0.003-0.05:1.

[0049] Optionally, obtaining the mixture A comprises: The method includes a step of introducing isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator to react with each other, and after the molar ratio of the introduced isobutene to the total phosphorus of the phosphinic acid and / or the alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of ethylene to react with each other to obtain the mixture A.

[0050] Optionally, obtaining the mixture A comprises: The method includes a step of introducing isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and after the isobutene reaction is complete or nearly complete, introducing ethylene to continue the reaction, thereby obtaining the mixture A.

[0051] Alternatively, the method includes reacting a phosphinic acid and / or an alkali metal salt thereof with isobutene to obtain monoisobutylphosphinic acid or an alkali metal salt thereof equal to or close to the value of y, controlling z to be equal to or less than 0.5, stopping the addition of isobutene, adding ethylene instead, continuing the reaction in the presence of an initiator, and then reacting with the required metal salt to obtain a flame retardant having the formula (I).

[0052] Optionally, obtaining the mixture A comprises: The method includes a step of introducing a part of isobutene and ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the ethylene and the ethylene with each other so that the molar ratio of the ethylene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof is smaller than (2x+y) / 1 in formula (I) and, after the molar ratio of the isobutene to the total phosphorus of the phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of the remaining ethylene to react the ethylene and obtain the mixture A.

[0053] Optionally, obtaining the mixture A comprises: The method includes the steps of introducing a portion of isobutene and ethylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and after the portion of the isobutene and ethylene has reacted completely or almost completely, introducing the remaining ethylene and continuing the reaction to obtain the mixture A, The molar ratio of the total amount of the ethylene to the isobutene is 0.33 to 39:1.

[0054] Optionally, obtaining the mixture A comprises: The method includes the steps of: introducing a portion of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator; making the molar ratio of the portion of ethylene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof smaller than (2x+y) / 1 in formula (I); after the portion of ethylene has completely reacted, continuing the introduction of isobutene for reaction; and, after the molar ratio of the introduced isobutene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of the remaining ethylene for reaction, thereby obtaining the mixture A.

[0055] Optionally, obtaining the mixture A comprises: The method includes the steps of introducing a part of ethylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and after the part of the ethylene is completely or almost completely reacted, introducing isobutene to continue the reaction, and after the isobutene is completely or almost completely reacted, introducing the remaining ethylene to continue the reaction, thereby obtaining the mixture A; The molar ratio of the total amount of the ethylene to the isobutene is 0.33 to 39:1.

[0056] Optionally, the metal element source M is at least one selected from metal element M salts.

[0057] Optionally, the metal element M salt is at least one selected from the group consisting of a nitrate, a sulfate, a hydrochloride, an acetate, and an oxide of the metal element M.

[0058] Alternatively, phosphinic acid and / or its alkali metal salt are reacted simultaneously with a portion of isobutene and ethylene in the presence of a radical initiator, the amount of isobutene and ethylene is controlled, and after the mole % of isobutylphosphinic acid or its alkali metal salt in the reaction system is close to the value of y, the mole % of diisobutylphosphinic acid or its alkali metal salt is close to the value of z, and z is less than or equal to 0.5, the addition of isobutene is stopped, the remaining ethylene is added, and the reaction is continued until completion in the presence of an initiator, and then reacted with the required metal salt to obtain a dialkylphosphinic acid hybrid salt having the formula (I).

[0059] According to a third aspect of the present application, there is further provided a flame retardant comprising at least one of the above dialkylphosphinic acid hybrid salts.

[0060] Optionally, the flame retardant further contains at least one selected from the group consisting of phosphate ions, phosphite ions, alkylphosphonate ions, and alkylphosphinate ions, the molar content of these phosphorus-containing acid salt ions in the flame retardant being 10 mol % or less, and the number of moles of the flame retardant being calculated in terms of the number of moles of phosphorus element contained therein.

[0061] According to a fourth aspect of the present application, there is provided a flame retardant material comprising a flame retardant P and a thermoplastic polymeric material, The flame retardant P is used in at least one flame retardant selected from the above dialkylphosphinic acid hybrid salts and the above flame retardants.

[0062] Optionally, the content of the flame retardant P in the flame-retardant material is 1 to 35% by mass.

[0063] Optionally, the flame retardant material comprises 1-35 wt% of flame retardant P and 65-99 wt% of thermoplastic polymeric material.

[0064] The thermoplastic polymer material in this application refers to a plastic that has the property of softening when heated and hardening when cooled.

[0065] Specifically, the amount of the flame retardant P used depends on the thermoplastic polymer material.

[0066] Optionally, the content of the flame retardant P in the flame retardant material is 3 to 20% by mass.

[0067] Optionally, the flame retardant material further comprises a functional additive; The functional additive is at least one selected from a reinforcing agent, an anti-drip agent, a stabilizer, a pigment, a dye, a carbonization catalyst, a dispersant, a nucleating agent, an inorganic filler, and an antioxidant.

[0068] Optionally, the reinforcing agent is selected from glass fibers.

[0069] Optionally, the anti-drip agent is selected from Teflon.

[0070] Optionally, the inorganic filler is at least one selected from mica, calcium carbonate, calcium oxide, and silica.

[0071] Optionally, the content of the functional additive in the flame retardant material is 5 to 40% by mass.

[0072] Optionally, the flame retardant material further comprises a flame retardant Q; The flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.

[0073] Optionally, the nitrogen-based flame retardant is at least one selected from melamine cyanurate, melamine polyphosphate, and ammonium polyphosphate. The boron-based flame retardant is selected from zinc borates.

[0074] Optionally, the content of the flame retardant Q in the flame-retardant material is 0.5 to 20% by mass.

[0075] Optionally, the thermoplastic polymeric material is at least one selected from polyamide and polyester.

[0076] Optionally, the polyamide is at least one selected from an aliphatic polyamide, an aromatic polyamide, a semi-aromatic polyamide, and a copolymer of a semi-aromatic polyamide and an aliphatic polyamide.

[0077] Those skilled in the art can add other flame retardants B to the flame retardant material according to specific needs, such as nitrogen-based flame retardants including melamine cyanurate, phosphorus-nitrogen-based flame retardants including melamine polyphosphate, ammonium polyphosphate, and the like, and boron-based flame retardants including zinc borate.

[0078] Optionally, the flame retardant material includes reinforcing glass fiber in an amount of 5-40% by mass, and other auxiliary agents include, for example, stabilizers, anti-drip agents, pigments, dyes, carbonization catalysts, dispersants, flame retardants, nucleating agents, and inorganic fillers or mixtures thereof, such as mica, calcium carbonate, calcium oxide, and silica, with the total of all components being 100% by mass.

[0079] According to common knowledge in the art, polyamide, also called polyamide fiber or nylon, is a general term for polymers having -NH-C(O)-amide as a structural unit, and is synthesized by condensation or ring-opening reaction of one or more dicarboxylic acids with one or more diamines, and / or one or more amino acids, and / or one or more lactams. Polyamides are generally classified into aliphatic polyamides, aromatic polyamides, and semi-aromatic polyamides according to the main chain components. Semi-aromatic polyamides refer to those having an aromatic group in at least one monomer structure in the synthetic monomer.

[0080] Optionally, the aliphatic polyamide is a mixture of any one or more selected from a copolymer of polyamide 6 and polyamide 66, polyamide 6, and polyamide 66.

[0081] Alternatively, the semi-aromatic polyamide can be produced from any one or more aromatic dicarboxylic acids and any one or more aliphatic diamines, or from any one or more aromatic diamines and any one or more aliphatic dicarboxylic acids. Furthermore, one or more selected from dicarboxylic acids, diamines, lactams and amino acids can be added to the system to produce polyamide copolymers with corresponding properties. The added dicarboxylic acids are aromatic dicarboxylic acids and / or aliphatic dicarboxylic acids. The added diamines are aromatic diamines and / or aliphatic diamines. The added lactams can be aliphatic lactams or aromatic lactams. The added amino acids can be aromatic amino acids or aliphatic amino acids.

[0082] Optionally, the semi-aromatic polyamide is prepared from any one or more aromatic dicarboxylic acids selected from terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and one or more aliphatic diamines selected from butylenediamine, hexadiamine, octanediamine, decanediamine, and 2-methylpentanediamine.

[0083] Optionally, the semi-aromatic polyamide is prepared from an aliphatic diamine, an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid.

[0084] Optionally, the semi-aromatic polyamide is prepared from an aliphatic diamine and an aromatic dicarboxylic acid, and optionally an aliphatic dicarboxylic acid may be added, and the molar percentage of the aliphatic dicarboxylic acid is 0-45% of the total dicarboxylic acid, i.e., the number of moles of aliphatic dicarboxylic acid / (the number of moles of aliphatic dicarboxylic acid+the number of moles of aromatic dicarboxylic acid)=0-45%.

[0085] Optionally, the aromatic dicarboxylic acid is any one or more selected from terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, the aliphatic diamine is any one or more selected from butylenediamine, hexadiamine, octanediamine, decanediamine, and 2-methylpentanediamine, and the aliphatic dicarboxylic acid is any one or more selected from adipic acid, succinic acid, sebacic acid, and octanoic acid.

[0086] Optionally, the polyamide is selected from the group consisting of poly(hexamethylene terephthalate) (abbreviated as PA6T), polyhexamethylene isophthalamide (abbreviated as PA6I), terephthalic acid / hexadiamine / caprolactam copolymer (abbreviated as PA6T / 6), terephthalic acid / hexadiamine / adipic acid copolymer (abbreviated as PA6T / 66), terephthalic acid / hexadiamine / adipic acid / isophthalic acid copolymer (abbreviated as PA6T / 6I / 66), polynonamethylene terephthalamide (abbreviated as PA9T), polydecamethylene terephthalate (abbreviated as PA6T), polyhexamethylene isophthalamide (abbreviated as PA6I ... and any one or more selected from poly(dodecamethylene terephthalamide) (abbreviated as PA10T), poly(dodecamethylene terephthalamide) (abbreviated as PA12T), terephthalic acid / hexadiamine / laurolactam copolymer (abbreviated as PA6T / 12), polymetaxylylene adipamide (abbreviated as MXD6), terephthalic acid / hexadiamine / 2-methylpentanediamine copolymer (abbreviated as PA6T / 2-MPMDT), and terephthalic acid / 2,2,4-trimethylhexanediamine / 2,4,4-trimethylhexanediamine copolymer.

[0087] Optionally, the aliphatic polyamide is at least one selected from polyamide 6, polyamide 66, and a copolymer of polyamide 6 and polyamide 66.

[0088] Optionally, the semi-aromatic polyamide is selected from polyphthalamide (PPA).

[0089] Optionally, the polyester is selected from polybutylene terephthalate (PBT).

[0090] In the embodiment of the present application, the values ​​of x, y and z in formula (I) are x+y+z=1 and x+z>0, without considering the amount of other phosphorus-containing impurities. The flame retardant having the composition of formula (I) may contain trace amounts of other phosphorus-containing ions. Due to impurities in the raw materials or impurities generated during the synthesis process, some trace amounts of phosphate ions, phosphite ions, alkyl phosphonate ions, and alkyl phosphinate ions may exist in the flame retardant. Oligomeric products of ethylene polymerization, such as ethyl n-butyl phosphinate ions, ethylhexyl phosphinate ions, butyl butyl phosphinate ions, and butylhexyl phosphinate ions, also exist as impurities in the flame retardant having the composition of formula (I). However, as long as the total amount of these other phosphorus-containing acid salt ions does not exceed 10% mole of the total phosphorus, it will not affect the normal operation of the flame retardant having the composition of formula (I).

[0091] In the examples of the present application, the ratio of x, y and z in formula (I) is determined as follows after the flame retardant is decomposed by alkali or acid: 31 It can be determined by P-NMR (nuclear magnetism). Diethylphosphinate, ethyl isobutylphosphinate, and diisobutylphosphinate are different 31 P chemical shift, 31 The P-NMR spectrum showed three independent peaks, and the peak areas of these three peaks corresponded to the molar concentrations of the three phosphinates, respectively. Therefore, the values ​​of x, y, and z could be easily calculated from the ratios of the peak areas. Effect of the Invention

[0092] The beneficial effects that the present invention can achieve are as follows:

[0093] (1) The dialkylphosphinic acid hybrid salt having the composition of formula (I) according to the present invention has a small amount of addition, a high flame retardant efficiency for various polymeric materials, and is economically advantageous. It overcomes not only the drawback of diethylphosphinic acid salt, which is low in flame retardant efficiency for polymeric materials, but also the drawback of diisobutylphosphinic acid salt, which is too volatile and low in flame retardant efficiency for polyester, and can be widely applied to the flame retardancy of various polymeric materials that require high-temperature processing.

[0094] (2) The method for producing a dialkylphosphinic acid hybrid salt according to the present invention avoids the disadvantage of having to produce dialkylphosphinic acid independently, and uses water as a reaction solvent, which is environmentally friendly. The raw materials are easily available, and the cost is high. [Brief description of the drawings]

[0095] [Figure 1] FIG. 1 is a graph showing the thermal weight loss curves of a dialkylphosphinic acid hybrid salt, aluminum diethylphosphinate, and aluminum diisobutylphosphinate having different values ​​of x, y, and z (for convenience of display, the numerical values ​​shown in the headers are 100 times x, y, and z). [Diagram 2] FIG. 2 shows XRD curves of dialkylphosphinic acid hybrid salts, aluminum diethylphosphinate, and aluminum diisobutylphosphinate having different values ​​of x, y, and z (for ease of display, the numerical values ​​shown in the headers are 100 times x, y, and z, and the physical mixture is a mixture of aluminum diethylphosphinate and aluminum diisobutylphosphinate). [Diagram 3] FIG. 3 is a 31P-NMR spectrum of the dialkylphosphinic acid hybrid salt of Example 3 after alkaline decomposition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0096] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0097] Unless otherwise stated, all materials in the examples herein were obtained commercially.

[0098] The raw materials used in the examples are as follows:

[0099] PA66 (also called polyamide 66 or nylon 66): Zytel 70G35 HSL NC010 from DuPont, USA, with a glass fiber content of 35% by mass.

[0100] PA6 (also called polyamide 6 or nylon 6): Zytel 73G30L NC010 from DuPont, USA, with a glass fiber content of 30% by mass.

[0101] PPA (high temperature nylon): HTN 51G35 HSL NC010 from DuPont, USA, with a glass fiber content of 35% by mass.

[0102] PBT (polybutylene terephthalate): Crastin SK605 NC010 from DuPont, USA, with a glass fiber content of 30% by mass.

[0103] ADP: aluminum diethylphosphinate, Exolit OP1230 from Clariant, Germany.

[0104] ABP: Aluminum diisobutylphosphinate prepared according to US Patent 7,807,737.

[0105] MPP: Melamine polyphosphate, Suzhou Kaima Chemical Technology Co., Ltd.

[0106] Antioxidant 1010: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], Shanghai MACKLIN Co., Ltd.

[0107] Antioxidant 168: Tris(2,4-di-tert-butylphenyl)phosphite, Strem Corporation, USA.

[0108] Composite antioxidant: Antioxidant 1010 (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]) and Antioxidant 168 (tris(2,4-di-tert-butylphenyl)phosphite) mixed in a 1:1 mass ratio.

[0109] Flame test standard: GB / T 2408-2008 standard.

[0110] Nuclear magnetic resonance (NMR) test: The model number of the equipment used was AVANCE III 400MHz, Bruker, Germany.

[0111] Nuclear magnetic resonance phosphorus spectrum ( 31 P-NMR) test method: the chemical shift of 85% phosphoric acid is 0, the pre-delay is D1=10 seconds, 32 scans are performed, and the peak area ratio is the molar ratio of diethylphosphinic acid salt ion, ethylisobutylphosphinic acid salt ion, and diisobutylphosphinic acid salt ion.

[0112] X-ray diffraction (XRD) test: The model of the equipment used was D8 ADVANCED AVINCI, Bruker, Germany.

[0113] TGA thermogravimetric analysis: The instrument used was model Q500, manufactured by TA, USA.

[0114] [Example 1: Preparation of a hybrid salt having the composition of formula (I), where x=0.87, y=0.13, z=0, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.3 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h to continuously introduce isobutene into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 0.3 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 9.0 hours, the introduction of ethylene was stopped, but the introduction of the initiator was continued, and after half an hour, the pressure in the vessel no longer decreased, indicating that the reaction was completed, and the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0115] Sampling was performed during the reaction and nuclear magnetic analysis was performed. 31 The P-NMR results are shown in Table 1.

[0116] [Table 1] *Long chain alkyl phosphinates included ethyl n-butyl phosphinate, ethylhexyl phosphinate, and butyl butyl phosphinate.

[0117] A portion of the above solution (690 g) was slowly added to an aqueous solution containing 89.97 g of aluminum sulfate octadecahydrate at a concentration of 20% by weight, and the reaction temperature was controlled at 70°C, and the pH value was adjusted to 3.0 or less, resulting in a large amount of precipitate. After 1 hour, the dropwise addition was completed. The mixture was filtered while still hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C, yielding 106.75 g, with a yield of 92.9%. The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed that diethyl phosphinate was 85.79%, ethyl isobutyl phosphinate was 12.36%, diisobutyl phosphinate was 0.45%, and the remainder was long-chain alkyl phosphinate, ethyl phosphonate, and phosphite impurities, and normalized to x=0.87, y=0.13, and z=0.

[0118] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 9.787 Å (100%) and 10.039 Å (66.1%), respectively, and the results are shown in Table 2.

[0119] [Table 2]

[0120] [Example 2a: Preparation of a hybrid salt having the composition of formula (I), where x=0.83, y=0.16, z=0.01, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated 0.3 MPa, and then a 4% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 1.0 hours, the introduction of isobutene was stopped, and the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 9.0 hours, the introduction of ethylene was stopped, but the introduction of the initiator was continued, and after half an hour, the pressure of the vessel no longer decreased, indicating that the reaction was completed, and the temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0121] The reaction solution is sampled and subjected to nuclear magnetic measurement. 31 The P-NMR results are shown in Table 3.

[0122] [Table 3]

[0123] A portion of the above solution (766 g) was slowly added to a 20% aqueous solution containing 89.97 g of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to 3.0 or less, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. The mixture was filtered while hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 95.2 g of a white powder product, with a yield of 90.7%.

[0124] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed that the content was 80.35% diethylphosphinate, 16.05% ethyl isobutylphosphinate, 0.70% diisobutylphosphinate, and the remainder was long-chain alkylphosphinate, ethylphosphonate, and phosphite impurities, and the normalized values ​​were x=0.83, y=0.16, and z=0.01.

[0125] XRD tests were performed on the samples, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 9.812 Å (100%) and 10.237 Å (86.7%), respectively, and the results are shown in Table 4.

[0126] [Table 4]

[0127] [Example 2b: Preparation of a hybrid salt having the composition of formula (I), where x=0.83, y=0.16, z=0.01, M=Cu, and n=2] Following the method of Example 2a, copper sulfate was used instead of aluminum sulfate to obtain a hybrid salt of copper with x=0.83, y=0.16, z=0.01. XRD test was performed on the sample and the XRD results are shown in Table 5.

[0128] [Table 5]

[0129] [Example 3: Preparation of a hybrid salt having the composition of formula (I), where x=0.70, y=0.29, z=0.01, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated 0.3 MPa, and then a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h to continuously introduce isobutene into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 1.5 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 10.5 hours, the introduction of ethylene was stopped, but the introduction of the initiator was continued, and after half an hour, the pressure of the vessel no longer decreased, indicating that the reaction was completed. The temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0130] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 6.

[0131] [Table 6]

[0132] 724 grams of the above solution was slowly added to a 20% by weight aqueous solution containing 104.79 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 3.0, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. The mixture was filtered while hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 117.5 grams, with a yield of 90.2%.

[0133] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed that the content was 69.15% diethylphosphinate, 28.57% ethylisobutylphosphinate, 1.12% diisobutylphosphinate, and the remainder was a long-chain alkylphosphinate impurity, which was normalized to x = 0.70, y = 0.29, and z = 0.01.

[0134] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 10.407 Å (100%) and 9.902 Å (47.4%), respectively, and the results are shown in Table 7.

[0135] [Table 7]

[0136] The hybrid salt obtained in this example was subjected to alkaline decomposition, 31 The P-NMR (nuclear magnetic) spectrum is shown in FIG. 3. The peak areas of the three peaks correspond to the molar concentrations of the three phosphinates, respectively, and therefore the values ​​of x, y, and z could be easily calculated from the ratio of the peak areas.

[0137] [Example 4a: Preparation of a hybrid salt having the composition of formula (I), where x=0.60, y=0.38, z=0.02, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure vessel, the vessel was replaced twice with nitrogen gas, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated 0.3 MPa, and then a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h to continuously introduce isobutene into the vessel, and the amount of olefin introduced was measured with a gas flow meter. After 2.0 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 15.5 hours, the introduction of ethylene was stopped, but the introduction of the initiator was continued, and after half an hour, the pressure of the vessel no longer decreased, indicating that the reaction was completed. The temperature was lowered to release the pressure, and the vessel was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0138] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 8.

[0139] [Table 8]

[0140] 847 g of the above solution was slowly added to a 20% by weight aqueous solution containing 104.79 g of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to 3.0 or less, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. The mixture was filtered while hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 126.1 g, with a yield of 94.9%.

[0141] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed that the content was 60.29% diethylphosphinate, 38.24% ethylisobutylphosphinate, and 1.47% diisobutylphosphinate, i.e., x=0.60, y=0.38, and z=0.02.

[0142] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 10.455 Å (100%) and 4.436 Å (14.2%), respectively, and the results are shown in Table 9.

[0143] [Table 9]

[0144] [Example 4b: Preparation of a hybrid salt having the composition of formula (I), where x=0.63, y=0.36, z=0.01, M=Fe, and n=3] According to Example 4a, 49.46 grams of the reaction solution was slowly added to a 15% aqueous solution containing 5.41 grams of ferric chloride hexahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.0, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was > 4.0. Then, the filter cake was dried at 120°C, and 8.40 grams were obtained, with a yield of 93.7%.

[0145] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed that the content was 63.26% diethylphosphinate, 35.82% ethylisobutylphosphinate, and 0.92% diisobutylphosphinate, i.e., x=0.63, y=0.36, and z=0.01.

[0146] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 10.407 Å (100%) and 4.502 Å (8.0%), respectively, and the results are shown in Table 10.

[0147] [Table 10]

[0148] [Example 4c: Preparation of a hybrid salt having the composition of formula (I), where x=0.62, y=0.37, z=0.01, M=Zn, and n=2] According to Example 4a, 197.85 g of the reaction solution was slowly added to a 15% aqueous solution containing 34.51 g of zinc sulfate heptahydrate, the reaction temperature was controlled at 70° C., and after the dropwise addition was completed, the solution was cooled and dried to obtain a white solid. The sample was dissolved in an aqueous solution of sodium hydroxide, and the phosphorus nuclear magnetic analysis showed that the content of diethylphosphinate was 62.0%, the content of ethylisobutylphosphinate was 36.7%, and the content of diisobutylphosphinate was 1.3%, i.e., x=0.62, y=0.37, and z=0.01.

[0149] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 8.741 Å (100%) and 9.044 Å (57.6%), respectively, and the results are shown in Table 11.

[0150] [Table 11]

[0151] [Example 5a: Preparation of a hybrid salt having the composition of formula (I), where x=0.45, y=0.52, z=0.03, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.3 MPa. Next, a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the reactor. After 5.5 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 17 hours, the reaction was complete, the introduction of ethylene was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0152] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 12.

[0153] [Table 12] *Long chain alkyls included ethyl n-butylphosphinate and butyl butylphosphinate.

[0154] 445 grams of the above solution was slowly added to a 10% aqueous solution containing 59.98 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.9, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was > 4.5. Then, the filter cake was dried at 120°C, and 69.3 grams were obtained, with a yield of 89%.

[0155] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed 44.18% diethylphosphinate, 50.45% ethyl isobutylphosphinate, 3.24% diisobutylphosphinate, and the remainder was long-chain alkylphosphinate and ethylphosphonate impurities. The normalized values ​​were x=0.45, y=0.52, and z=0.03.

[0156] XRD tests were performed on the sample, and the corresponding layer spacings of the feature peaks with the highest and second highest relative intensities measured by XRD were 10.626 Å (100%) and 4.436 Å (12.7%), respectively, and the results are shown in Table 13.

[0157] [Table 13]

[0158] [Example 5b: Preparation of a hybrid salt having the composition of formula (I), where x=0.48, y=0.49, z=0.03, M=Fe, and n=3] According to Example 5a, 51.3 grams of the reaction solution was slowly added to a 15% aqueous solution containing 5.41 grams of ferric chloride hexahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.0, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was > 4.0. Then, the filter cake was dried at 120°C, and 8.70 grams were obtained, with a yield of 94.7%.

[0159] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed 47.22% diethylphosphinate, 48.25% ethyl isobutylphosphinate, 2.13% diisobutylphosphinate, and the remainder was long-chain alkylphosphinate and ethylphosphonate impurities. The normalized values ​​were x=0.48, y=0.49, and z=0.03.

[0160] XRD tests were performed on the sample, and the corresponding layer spacings of the characteristic peaks with the highest and second highest relative intensities measured by XRD were 10.603 Å (100%) and 4.524 Å (11.2%), respectively, and the results are shown in Table 14.

[0161] [Table 14]

[0162] [Example 6: Preparation of a hybrid salt having the composition of formula (I), where x=0.31, y=0.64, z=0.05, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.3 MPa. Next, a 4.0% aqueous solution of 2,2'-azobis(2-amidinopropane) dichloride was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the reactor. After 9.5 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 20 hours, the reaction was complete, the introduction of ethylene was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0163] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 15.

[0164] [Table 15]

[0165] 512 grams of the above solution was slowly added to a 10% aqueous solution containing 59.98 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.9, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was > 4.5. Then, the filter cake was dried at 120°C, and 74.46 grams were obtained, with a yield of 93.7%.

[0166] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed 30.76% diethylphosphinate, 63.27% ethyl isobutylphosphinate, 4.60% diisobutylphosphinate, and the remainder was long-chain alkylphosphinate and ethylphosphonate impurities. The normalized values ​​were x=0.31, y=0.64, and z=0.05.

[0167] XRD tests were performed on the sample, and the corresponding layer spacings of the characteristic peaks with the highest and second highest relative intensities measured by XRD were 10.965 Å (100%) and 4.463 Å (9.9%), respectively, and the results are shown in Table 16.

[0168] [Table 16]

[0169] [Example 7] Preparation of a hybrid salt having the composition of formula (I), where x=0.28, y=0.68, z=0.04, M=Al, and n=3. 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which time the pressure gauge indicated 0.3 MPa. Next, a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the reactor. After 10.5 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 21 hours, the reaction was basically completed, the introduction of ethylene was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0170] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 17.

[0171] [Table 17]

[0172] The above solution was first oxidized with enough 30% hydrogen peroxide water to form mono-addition products, and then slowly added to a 10% aqueous solution containing 104.79 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.9, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. The mixture was filtered while hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C to obtain 124.99 grams, with a yield of 91.7%.

[0173] The sample was dissolved in aqueous sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which showed 27.78% diethylphosphinate, 66.83% ethylisobutylphosphinate, 4.00% diisobutylphosphinate, and the remainder other phosphorus-containing impurities. The normalized values ​​were x=0.28, y=0.68, and z=0.04.

[0174] XRD testing was performed on the sample, and the corresponding layer spacings of the characteristic peaks with the highest and second highest relative intensities measured by XRD were 10.913 Å (100%) and 4.461 Å (12.6%), respectively, and the results are shown in Table 18.

[0175] [Table 18]

[0176] [Example 8: Preparation of a hybrid salt having the composition of formula (I), where x=0.03, y=0.58, z=0.39, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.3 MPa. Next, a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the reactor. After 13 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 25 hours, the introduction of ethylene was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0177] The above solution was first oxidized with enough 30% hydrogen peroxide water to form mono-addition products, and then 500 grams of the solution was slowly added to a 10% aqueous solution containing 13.33 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.9, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was >4.5. The filter cake was then dried at 120°C, and 19.05 grams were obtained, with a yield of 94%.

[0178] The sample was dissolved in aqueous sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which gave 2.69% diethylphosphinate, 52.89% ethylisobutylphosphinate, and 35.84% diisobutylphosphinate. The normalized values ​​are x=0.03, y=0.58, and z=0.39.

[0179] XRD testing was performed on the sample, and the corresponding layer spacings of the characteristic peaks with the highest and second highest relative intensities measured by XRD were 11.619 Å (100%) and 4.492 Å (11.7%), respectively, and the results are shown in Table 19.

[0180] [Table 19]

[0181] [Example 9: Preparation of a hybrid salt having the composition of formula (I), where x=0.03, y=0.52, z=0.45, M=Al, and n=3] 100 grams of sodium phosphinate monohydrate was dissolved in 500 grams of water and placed in a 1L stainless steel pressure cooker. The reactor was replaced with nitrogen gas twice, evacuated, and then filled with isobutene until the pressure no longer increased. The reaction liquid was heated to about 90°C, at which point the pressure gauge indicated 0.3 MPa. Next, a 3.0% by mass aqueous sodium persulfate solution was injected at a constant rate of 10 ml / h, and isobutene was continuously introduced into the reactor. After 15 hours, the introduction of isobutene was stopped, the introduction of ethylene was started, and the pressure was raised to 0.8 MPa. After 27 hours, the reaction was complete, the introduction of ethylene was stopped, the temperature was lowered to release the pressure, and the reaction liquid was purged with N2 and discharged to obtain a colorless and transparent reaction liquid.

[0182] Sampling was performed during the reaction and the results of nuclear magnetic analysis are shown in Table 20.

[0183] [Table 20]

[0184] 280 grams of the above solution was slowly added to a 10% aqueous solution containing 7.46 grams of aluminum sulfate octadecahydrate, the reaction temperature was controlled at 70°C, the pH value was adjusted to below 2.9, and a large amount of precipitate was obtained. After 1 hour, the dropping was completed. It was filtered while hot, and the filter cake was washed with clean water until the pH was > 4.5. Then, the filter cake was dried at 120°C, and 10.7 grams were obtained, with a yield of 94.3%.

[0185] The sample was dissolved in an aqueous solution of sodium hydroxide and subjected to phosphorus nuclear magnetic analysis, which gave 2.9% diethylphosphinate, 51.0% ethylisobutylphosphinate, and 43.5% diisobutylphosphinate. The normalized values ​​were x=0.03, y=0.52, and z=0.45.

[0186] The dried sample was subjected to XRD test. The X-ray diffraction (XRD) results are shown in Table 21 below. As can be seen from the characteristic peak with the highest relative intensity in Table 21, the layer spacing was mainly 11.666 Å.

[0187] [Table 21]

[0188] The results of TGA tests on the dialkylphosphinic acid hybrid salts obtained in Examples 1, 2a, 4a, 7, 8, and 9 are shown in Figure 1, which shows the thermal weight loss curves (TGA) of hybrid salts with different x, y, and z values, aluminum diethylphosphinate (ADP), and aluminum diisobutylphosphinate (ABP). As can be seen from the figure, aluminum diisobutylphosphinate had the fastest thermal weight loss and the lowest thermal stability. The larger the z value, the faster the thermal weight loss of the hybrid salt.

[0189] [Example 10 (Comparative Example) Iron diethylphosphinate] 93.82 grams of 18.4% by weight sodium diethylphosphinate aqueous solution (containing 2.1 mol% sodium ethylbutylphosphinate and 0.5 mol% sodium ethylphosphonate) was slowly added to 10.81 grams of 15% by weight aqueous solution of ferric chloride hexahydrate while maintaining the reaction temperature at 70°C and pH=2 for half an hour, and then kept warm for half an hour. Filtered while hot, the filter cake was washed with clean water until pH>4. The filter cake was then dried at 120°C to obtain 15.5 grams, with a yield of 92.5%.

[0190] The samples were subjected to XRD testing and the results are shown in Table 22.

[0191] [Table 22]

[0192] [Example 11] Polyamide PA66, the hybrid salt produced in Example 1, and the composite antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-1.

[0193] [Example 12] Polyamide PA6, the hybrid salt produced in Example 1, and the composite antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-1.

[0194] [Example 13] Polyester PBT, the hybrid salt produced in Example 1, and the composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-0.

[0195] [Examples 14 to 40] For the flame retardants of Examples 2 to 9, samples were produced and tested in accordance with the methods of Examples 11 to 13 for polyamide PA66, PA6, PPA, and PBT, respectively, and the results are shown in Tables 23 and 24.

[0196] [Example 41] Polyamide PA66, the hybrid salt prepared in Example 8, MPP and the composite antioxidant were mixed in a mass ratio of 82.6:12:5:0.4 at a temperature of 280°C set in an internal mixer with a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-0.

[0197] [Comparative Example 1] Polyamide PA66, diethyl phosphinate iron prepared in Example 10, and composite antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and then removed after 5 minutes, cooled, and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 non-rated.

[0198] [Comparative Example 2] Polyamide PA66, ADP and complex antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 unrated.

[0199] [Comparative Example 3] Polyamide PA6, ADP and complex antioxidant were mixed in a mass ratio of 79.6:20:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL-94 unrated.

[0200] [Comparative Example 4] Polyester PBT, ADP and complex antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-2.

[0201] [Comparative Example 5] Polyester PBT, aluminum diisobutylphosphinate (ABP) and composite antioxidant were mixed in a mass ratio of 84.6:15:0.4 in an internal mixer at a set temperature of 260°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 260°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-2.

[0202] [Comparative Example 6] Polyamide PA66, aluminum diisobutylphosphinate (ABP) and complex antioxidant were mixed in a mass ratio of 87.1:12.5:0.4 in an internal mixer at a set temperature of 280°C and a rotation speed of 50 rpm, and removed after 5 minutes, cooled and dried. The mixture was then filled into a mold, preheated in a press vulcanizer at 280°C for 10 minutes, maintained at 10 MPa for 5 minutes, and cold pressed. After cooling, samples were cut out and tested. The flame retardant rating of the 1.6 mm sample was UL94 V-1.

[0203] The results of the comparative examples are shown in Table 25.

[0204] [Table 23]

[0205] [Table 24]

[0206] [Table 25] *: No NG grade

[0207] Examples 11 to 41 showed that the flame retardant containing the dialkylphosphinic acid hybrid salt of the present invention has excellent flame retardant efficiency for both polyamide and polyester. Comparative Example 1 showed that pure iron diethylphosphinate had low flame retardant efficiency for polyamide and polyester. Comparative Examples 2 to 4 showed that pure aluminum diethylphosphinate had low flame retardant efficiency for polyamide and polyester. Comparative Example 5 showed that pure aluminum diisobutylphosphinate had low flame retardant efficiency for polyester. Comparative Example 6 showed that the flame retardant efficiency of pure aluminum diisobutylphosphinate for polyamide was lower than that of the hybrid salt containing ethylisobutylphosphinic acid salt at the same addition amount, and referred to Examples 20, 26, 32 and 37. In addition, according to the examples, for the hybrid salt containing diisobutylphosphinic acid salt, the higher the content, the darker the color of the flame retardant sample and the more decomposition occurred. The color of the polymer material sample obtained by flame retarding pure aluminum diisobutylphosphinic acid salt was the darkest.

[0208] The above are only some examples of the present application, and are not intended to limit the present application in any way, and the present application is disclosed in the above preferred embodiments, but they are not intended to limit the present application. Those skilled in the art can make slight changes or modifications using the technical contents disclosed above without departing from the scope of the technical proposal of the present application, which are equivalent to equivalent implementation examples and fall within the scope of the technical proposal.

[0209] (Additional Note) (Appendix 1) At least one compound selected from the group consisting of compounds having the chemical formula shown in formula (I): [ka] Here, M is a central atom, and the diethylphosphinate ion, the ethylisobutylphosphinate ion, and the diisobutylphosphinate ion are all ligands. M is selected from a metal element, and the metal element is at least one selected from the group consisting of group IIA, IIIA, IVA, and VA metal elements, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; A dialkylphosphinic acid hybrid salt, characterized in that 0≦x≦0.95, 0.05≦y≦0.8, 0≦z≦0.5, and x+y+z=1, and x+z>0.

[0210] (Appendix 2) The Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, and Ba; The group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The dialkylphosphinic acid hybrid salt according to claim 1, wherein the lanthanum-based metal element is Ce.

[0211] (Appendix 3) The dialkylphosphinic acid hybrid salt according to claim 1, wherein 0.03≦x≦0.87, 0.13≦y≦0.68, and 0≦z≦0.45.

[0212] (Appendix 4) The dialkylphosphinic acid hybrid salt according to claim 3, wherein 0.03≦x≦0.7, 0.29≦y≦0.68, and 0.01≦z≦0.45.

[0213] (Appendix 5) A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The method for producing a dialkylphosphinic acid hybrid salt according to any one of claims 1 to 4, wherein the mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylisobutylphosphinic acid and / or an alkali metal salt thereof, and diisobutylphosphinic acid and / or an alkali metal salt thereof.

[0214] (Appendix 6) The production method according to appendix 5, wherein the conditions for the reaction I are a temperature of 0 to 250° C., a pressure of 0.1 to 10 MPa, and a time of 0.1 to 20 hours.

[0215] (Appendix 7) The mixture A is obtained by The method for producing the mixture A according to claim 5, further comprising the steps of: introducing ethylene and isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator; and carrying out reaction II to obtain the mixture A.

[0216] (Appendix 8) The production method according to Appendix 7, wherein a mass of the water in the aqueous solution is 10 to 99% of a total mass of the radical initiator and the phosphinic acid and / or the alkali metal salt thereof.

[0217] (Appendix 9) 8. The production method according to claim 7, wherein the conditions for the reaction II are a temperature of 0 to 250° C., a time of 0.01 to 50 hours, and a pressure of 0 to 3 MPa.

[0218] (Appendix 10) 8. The production method according to claim 7, wherein a molar ratio of the radical initiator to the total amount of the phosphinic acid and / or the alkali metal salt thereof is 0.001 to 0.1:1.

[0219] (Appendix 11) The mixture A is obtained by The production method according to Appendix 7, comprising the steps of introducing isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the solution with the phosphinic acid and / or an alkali metal salt thereof, and stopping the introduction of isobutene and continuing the introduction of ethylene to react the solution after the molar ratio of the introduced isobutene to the total phosphorus of the phosphinic acid and / or the alkali metal salt thereof reaches (y+2z) / 1 in formula (I), thereby obtaining the mixture A.

[0220] (Appendix 12) The mixture A is obtained by The production method according to Appendix 7, comprising a step of introducing a part of isobutene and ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the part, and stopping the introduction of isobutene after a molar ratio of ethylene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes smaller than (2x+y) / 1 in formula (I) and a molar ratio of introduced isobutene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), and continuing the introduction of the remaining ethylene to react the part, thereby obtaining the mixture A.

[0221] (Appendix 13) The mixture A is obtained by 8. The production method according to claim 7, comprising the steps of: introducing a portion of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator; making a molar ratio of the portion of ethylene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof smaller than (2x+y) / 1 in formula (I); after the portion of ethylene has completely reacted, continuing the introduction of isobutene for reaction; and, after the molar ratio of the introduced isobutene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of the remaining ethylene for reaction, thereby obtaining the mixture A.

[0222] (Appendix 14) The method according to claim 5, wherein the metal element source M is at least one selected from metal element M salts.

[0223] (Appendix 15) A flame retardant selected from the dialkylphosphinic acid hybrid salts according to any one of claims 1 to 4.

[0224] (Appendix 16) A flame retardant P and a thermoplastic polymeric material are included, The flame retardant material, wherein the flame retardant P is at least one selected from the flame retardants described in Appendix 15.

[0225] (Appendix 17) 17. The flame-retardant material according to claim 16, wherein the content of the flame retardant P in the flame-retardant material is 1 to 35 mass %.

[0226] (Appendix 18) The flame retardant material further comprises a functional additive, 17. The flame-retardant material according to claim 16, wherein the functional additive is at least one selected from the group consisting of a reinforcing agent, an anti-drip agent, a stabilizer, a pigment, a dye, a carbonization catalyst, a dispersant, a nucleating agent, an inorganic filler, and an antioxidant.

[0227] (Appendix 19) 19. The flame-retardant material according to claim 18, wherein the content of the functional additive in the flame-retardant material is 5 to 40% by mass.

[0228] (Appendix 20) The flame retardant material further comprises a flame retardant Q; 19. The flame-retardant material according to claim 18, wherein the flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.

[0229] (Appendix 21) 21. The flame-retardant material according to claim 20, wherein the content of the flame retardant Q in the flame-retardant material is 0.5 to 20 mass %.

[0230] (Appendix 22) 17. The flame-retardant material according to claim 16, wherein the thermoplastic polymer material is at least one selected from polyamide and polyester.

Claims

1. At least one compound selected from the group consisting of compounds having the chemical formula shown in formula (I): 【Chemistry 1】 In the formula, M is a central atom, and the diethylphosphinate ion, the ethylisobutylphosphinate ion, and the diisobutylphosphinate ion are all ligands. M is selected from a metal element, and the metal element is at least one selected from the group consisting of metal elements of groups IIA, IIIA, IVA, and VA, transition metal elements, and lanthanide metal elements; n is the valence of the metal M, n being selected from 2, 3 or 4; A dialkylphosphinic acid hybrid salt, characterized in that 0≦x≦0.95, 0.05≦y≦0.8, 0≦z≦0.5, and x+y+z=1, and x+z>0.

2. The Group IIA metal element is at least one selected from Be, Mg, Ca, Sr, and Ba; The Group IIIA metal element is Al; The Group IVA metal element is Sn; The VA group metal element is Sb; The transition metal element is at least one selected from Fe, Zn, Cu, Ti, Zr, and Mn, The dialkylphosphinic acid hybrid salt according to claim 1, wherein the lanthanum-based metal element is Ce.

3. The dialkylphosphinic acid hybrid salt according to claim 1, characterized in that 0.03≦x≦0.87, 0.13≦y≦0.68, and 0≦z≦0.

45.

4. The dialkylphosphinic acid hybrid salt according to claim 3, characterized in that 0.03≦x≦0.7, 0.29≦y≦0.68, and 0.01≦z≦0.

45.

5. A step of causing a reaction I in an aqueous phase of a material containing a mixture A and a metal element source M to obtain the dialkylphosphinic acid hybrid salt, The method for producing a dialkylphosphinic acid hybrid salt according to any one of claims 1 to 4, characterized in that the mixture A contains diethylphosphinic acid and / or an alkali metal salt thereof, ethylisobutylphosphinic acid and / or an alkali metal salt thereof, and diisobutylphosphinic acid and / or an alkali metal salt thereof.

6. The method according to claim 5, wherein the reaction I is carried out under conditions of a temperature of 0 to 250° C., a pressure of 0.1 to 10 MPa, and a time of 0.1 to 20 hours.

7. The mixture A is obtained by The method according to claim 5, further comprising the step of: introducing ethylene and isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, and carrying out reaction II to obtain the mixture A.

8. The method according to claim 7, wherein the mass of the water in the aqueous solution is 10 to 99% of the total mass of the radical initiator and the phosphinic acid and / or the alkali metal salt thereof.

9. The method according to claim 7, wherein the reaction II is carried out under conditions of a temperature of 0 to 250° C., a time of 0.01 to 50 h, and a pressure of 0 to 3 MPa.

10. The method according to claim 7, wherein a molar ratio of the radical initiator to the total amount of the phosphinic acid and / or its alkali metal salt is 0.001-0.1:

1.

11. The mixture A is obtained by 8. The method according to claim 7, further comprising the step of: introducing isobutene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator to react with each other; and after a molar ratio of the introduced isobutene to the total phosphorus of the phosphinic acid and / or the alkali metal salt thereof reaches (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of ethylene to react with each other to obtain the mixture A.

12. The mixture A is obtained by 8. The method according to claim 7, further comprising the step of: introducing a part of isobutene and ethylene into an aqueous solution containing a phosphinic acid and / or an alkali metal salt thereof and a radical initiator, reacting the part, and stopping the introduction of isobutene after a molar ratio of ethylene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes smaller than (2x+y) / 1 in formula (I) and a molar ratio of introduced isobutene to a total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), and continuing the introduction of the remaining ethylene to react the part, thereby obtaining the mixture A.

13. The mixture A is obtained by 8. The method according to claim 7, further comprising the steps of: introducing a portion of ethylene into an aqueous solution containing phosphinic acid and / or an alkali metal salt thereof and a radical initiator; making a molar ratio of the portion of ethylene to total phosphorus of phosphinic acid and / or an alkali metal salt thereof smaller than (2x+y) / 1 in formula (I); after the portion of ethylene has completely reacted, continuing the introduction of isobutene for reaction; and, after the molar ratio of the introduced isobutene to the total phosphorus of phosphinic acid and / or an alkali metal salt thereof becomes (y+2z) / 1 in formula (I), stopping the introduction of isobutene and continuing the introduction of the remaining ethylene for reaction, thereby obtaining the mixture A.

14. 6. The method according to claim 5, wherein the metal element source M is at least one selected from metal element M salts.

15. A flame retardant selected from the dialkylphosphinic acid hybrid salts according to any one of claims 1 to 4.

16. comprising a flame retardant P and a thermoplastic polymeric material; 16. A flame-retardant material, characterized in that the flame retardant P is at least one selected from the flame retardants defined in claim 15.

17. The flame-retardant material according to claim 16, characterized in that the content of the flame retardant P in the flame-retardant material is 1 to 35 mass %.

18. The flame retardant material further comprises a functional additive, 17. The flame retardant material of claim 16, wherein the functional additive is at least one selected from the group consisting of reinforcing agents, anti-drip agents, stabilizers, pigments, dyes, carbonization catalysts, dispersants, nucleating agents, inorganic fillers, and antioxidants.

19. The flame-retardant material according to claim 18, characterized in that the content of the functional additive in the flame-retardant material is 5 to 40% by mass.

20. The flame retardant material further comprises a flame retardant Q, 19. The flame-retardant material according to claim 18, wherein the flame retardant Q is at least one selected from a nitrogen-based flame retardant and a boron-based flame retardant.

21. The flame-retardant material according to claim 20, characterized in that the content of the flame retardant Q in the flame-retardant material is 0.5 to 20 mass %.

22. 17. The flame retardant material according to claim 16, wherein the thermoplastic polymer material is at least one selected from polyamide and polyester.

Citation Information

Patent Citations

  • Polydialkyl phosphinic acid metal composite salt and / or mixture thereof, and uses thereof

    CN111825883A

  • Methods for preparing mixed substituted dialkylphosphinic acids, mixed substituted dialkylphosphinic acid esters, and mixed substituted dialkylphosphinate salts, and their uses.