Method for forming graphene films

A pulsed light irradiation process converts polymeric graphene precursors into high-quality graphene films efficiently and sustainably, addressing scalability and energy consumption issues in existing methods.

JP2024538171AActive Publication Date: 2024-10-18UNIV OF MASSACHUSETTS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024523147
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-18
Filing Date
2022-10-18
Publication Date
2024-10-18
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Existing methods for producing graphene are not scalable, energy-intensive, costly, and often operate under harsh conditions, making them inefficient and environmentally unfriendly.

Method used

A method involving coating a polymeric graphene precursor on a substrate and irradiating it with a pulsed high-intensity light source at multiple wavelengths for less than one second to convert it into a graphene film, which can be done at lower temperatures and ambient conditions, using a xenon flash lamp or similar sources.

Benefits of technology

This method allows for the production of high-quality graphene films with improved thermal, electrical, and mechanical stability, is more energy-efficient, and can be performed on a wide range of substrates, including heat-sensitive materials, with higher throughput and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538171000001_ABST
    Figure 2024538171000001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for forming a graphene film, the graphene film produced thereby, and uses thereof. The method for forming a graphene film includes coating a polymeric graphene precursor on a substrate. The method includes irradiating the polymeric graphene precursor coated on the substrate with a pulsed high-intensity light source emitting at two or more wavelengths for a pulse duration of less than one second, thereby converting the polymeric graphene precursor into a graphene film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This disclosure relates to methods of forming graphene films. This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 262,656, filed October 18, 2021, the disclosure of which is incorporated herein by reference in its entirety. [Background technology]

[0002] Graphene is sp 2 Graphene is a nanomaterial that has a two-dimensional honeycomb lattice of hybridized carbon atoms. Graphene has many unique properties such as high electrical conductivity, high thermal conductivity, good mechanical properties, large surface area, excellent chemical properties, and good biocompatibility. All these properties make it an ideal candidate for potential applications in nanoelectronics, energy storage, biosensing, catalysis, nanocomposites, and medicine, to name a few. There are three main forms of graphene material in use today: graphene oxide, reduced graphene oxide, and pristine single-layer and multilayer graphene. Of all the forms of graphene, pristine graphene has the best of the above properties.

[0003] Many graphene preparation methods have been reported in the literature. These methods can be broadly classified as top-down or bottom-up approaches. In the top-down approach, graphene is prepared by mechanical exfoliation, chemical exfoliation of graphite and graphite oxide, laser exfoliation of graphite, chemical reduction of graphene oxide, electrochemical reduction of graphene oxide, photothermal reduction of GO, and photolysis of various precursors using flash lamps. In the bottom-up approach, graphene is produced via solution-based chemical synthesis, via solvothermal synthesis, via chemical vapor deposition on various substrates such as metal catalysts such as copper, ruthenium, nickel, etc., via epitaxial growth on SiC, via laser-induced epitaxial growth, and via arc discharge.

[0004] Most of the above mentioned methods are not scalable for large scale production, except for the electrochemical reduction and CVD approaches: most of them are extremely energy consuming, operate under harsh conditions, are expensive and are very slow to perform. Summary of the Invention

[0005] The present invention provides a method of forming a graphene film. The method includes depositing a polymeric graphene precursor on a substrate. The method includes irradiating the polymeric graphene precursor deposited on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than 1 second, thereby converting the polymeric graphene precursor into a graphene film.

[0006] The present invention provides a method of forming a graphene film. The method includes coating a polymeric graphene precursor on a substrate comprising carbon fiber, carbon mesh, carbon cloth, carbon composite, graphene composite, graphene, carbon film, or a combination thereof. The polymeric graphene precursor and the substrate have different chemical compositions. The method includes converting the polymeric graphene precursor into a graphene film by irradiating the polymeric graphene precursor coated on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than one second.

[0007] The invention provides a graphene film formed by the method of the invention. The graphene film may be a patterned or unpatterned graphene film. The invention provides an electrochemical energy storage device, an electromagnetic shield, a chemical or biological sensor, a post-CMOS nanoelectronic device, a thermal shield, a structural composite, a filter, or a combination thereof, comprising the graphene film formed by the method of the invention.

[0008] Various aspects of the methods of the present invention may have advantages over other methods of forming graphene films. For example, in various aspects, the methods of the present invention may be performed at lower temperatures than other methods, allowing for the formation of graphene films on heat-sensitive materials. In various aspects, the rapid pyrolysis of the polymeric graphene precursor may reduce, minimize, or avoid oxidation of the resulting graphene film. In various aspects, the methods may form graphene films with similar or better thermal, electrical, and / or mechanical stability compared to graphene films formed by other methods. In various aspects, the methods of the present invention overcome limitations and shortcomings of conventional methods of making graphene with respect to energy budget, throughput, scalability, and / or versatility with respect to precursors.

[0009] In various embodiments, the methods of the present invention can form graphene without a catalyst or catalytic substrate. In various embodiments, the methods of the present invention can be carried out at room conditions with respect to temperature, pressure, and humidity. In various embodiments, the methods of the present invention provide much higher throughput compared to other methods of making graphene, since the entire pyrolysis process can be carried out in the microsecond time frame and can be completed in the millisecond time frame, depending on the number of pulses applied. In various embodiments, the methods of the present invention are a safer and more environmentally friendly alternative to conventional methods of making graphene, since they do not require harmful or polluting chemicals, extremely high power or mechanical forces, or excessive pressure. In various embodiments, the methods of the present invention are a simpler alternative to conventional methods of making graphene, since graphene can be synthesized in a single irradiation step. In various embodiments, the methods of the present invention are a less energy-intensive alternative to conventional methods of making graphene, since they use less energy to operate the flash lamps and their control electronics than other methods. In various embodiments, the method of the present invention is a cheaper alternative to conventional methods of making graphene because it can be carried out using simple equipment with flash lamps or other suitable radiation sources such as high intensity light emitting diodes that can be operated in ambient conditions without requiring a vacuum or extreme environment for operation. In various embodiments, the method of the present invention is a more scalable alternative to conventional methods of making graphene because it can be operated in a roll-to-roll format that allows for extremely high throughput and large areas of graphene material in a relatively short time of a few minutes, depending on the length of the substrate. In various embodiments, the method of the present invention can make graphene on a wide range of substrates, including metals (such as stainless steel, copper, nickel, aluminum, gold), semiconductors (such as silicon, silicon carbide, gallium arsenide, indium gallium arsenide, aluminum gallium arsenide wafers), plastics (such as polyimide, polyaramid, polyester, etc.), or combinations thereof. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 shows a scheme for the preparation of graphene by photothermal pyrolysis of precursor thin films at ambient conditions, according to various embodiments. [Figure 2A] FIG. 2A illustrates an example of a precursor material, according to various embodiments. [Figure 2B] FIG. 2B illustrates an example of a precursor material, according to various embodiments. [Figure 2C] FIG. 2C illustrates an example of a precursor material, according to various embodiments. [Figure 2D] FIG. 2D illustrates a method of synthesizing polybenzoxazine, according to various embodiments. [Diagram 3] FIG. 3 illustrates a processing scheme for the photothermal pyrolysis of an unpatterned precursor film and its conversion to a graphene composite, according to various embodiments. [Figure 4] FIG. 4 illustrates a method of curing benzoxazine monomer to polybenzoxazine, according to various embodiments. [Diagram 5] FIG. 5 shows a processing scheme for the cyclization of polyacrylonitrile, photothermal pyrolysis of unpatterned cyclized polyacrylonitrile precursor films, and its conversion to graphene composites, according to various embodiments. [Figure 6] FIG. 6 shows a processing scheme for the photothermal pyrolysis of pure carbon fibers and their conversion to graphene composites, according to various embodiments. [Figure 7] FIG. 7 illustrates a process sequence for photothermal pyrolysis to obtain patterned pure graphene, according to various embodiments. [Figure 8] FIG. 8 shows a process sequence for photothermal pyrolysis processing to obtain a screen-printed graphene composite, according to various embodiments. [Figure 9A] FIG. 9A shows the emission spectrum of a PulseForge® tool as a function of pulse voltage, according to various embodiments. [Figure 9B]FIG. 9B shows the absorption spectra of a glass substrate, a benzoxazine monomer, and a cured poly(benzoxazine) film according to various embodiments. [Figure 9C] FIG. 9C shows the temperature-time profile obtained from a cured poly(benzoxazine) film photothermally pyrolyzed in a low power process, according to various embodiments. [Figure 9D] FIG. 9D shows the temperature-time profile obtained from a cured poly(benzoxazine) film photothermally pyrolyzed in a high power process, according to various embodiments. [Figure 9E] FIG. 9E shows FTIR spectra of benzoxazine monomer, poly(benzoxazine), and photothermally generated graphene composites according to various embodiments. [Figure 9F] FIG. 9F shows TGA profiles of poly(benzoxazine), graphene composite, and carbon fiber, according to various embodiments. [Figure 10A] FIG. 10A shows an optical image of a cured precursor film, according to various embodiments. [Figure 10B] FIG. 10B shows an optical image of a graphene / carbon fiber composite, according to various embodiments. [Figure 10C] FIG. 10C shows an SEM image of a graphene / carbon fiber composite, according to various embodiments. [Figure 10D] FIG. 10D shows an SEM image of a graphene / carbon fiber composite, according to various embodiments. [Figure 11A] FIG. 11A shows an optical image of a 1K, plain weave, 228.6 mm thick pure fine mesh carbon fiber according to various embodiments. [Figure 11B] FIG. 11B shows an optical image of the resulting carbon fiber / graphene composite after coating and pyrolysis of one layer of polybenzoxazine precursor film on 1K, plain weave, 228.6 mm thick pure fine mesh carbon fiber, according to various embodiments. [Figure 11C]FIG. 11C shows an optical image of the resulting carbon fiber / graphene composite after coating and pyrolysis of two layers of polybenzoxazine precursor film on 1K, plain weave, 228.6 mm thick pure fine mesh carbon fiber according to various embodiments. [Figure 11D] FIG. 11D shows an SEM image of the composite shown in FIG. 11C, according to various embodiments. [Figure 12A] FIG. 12A shows Raman spectra of carbon fibers and graphene / carbon fiber composites according to various embodiments. [Figure 12B] FIG. 12B shows an X-ray diffraction pattern of a graphene / carbon fiber composite, according to various embodiments. [Figure 12C] FIG. 12C shows an XPS spectrum of a graphene / carbon fiber composite according to various embodiments. [Figure 13A] FIG. 13A shows an image of a graphene / carbon composite obtained by low-power pulse modulation processing, according to various embodiments. [Figure 13B] FIG. 13B shows an image of a graphene / carbon composite obtained by high power pulse modulation processing, according to various embodiments. [Figure 13C] FIG. 13C shows an image of a graphene / carbon composite obtained by high power pulse modulation processing, according to various embodiments. [Figure 13D] FIG. 13D shows Raman spectra of graphene / carbon composites obtained by low-power and high-power pulse modulation processing according to various embodiments. [Figure 14A] FIG. 14A shows a transmission electron micrograph of a graphene / carbon fiber composite, according to various embodiments. [Figure 14B] FIG. 14B shows a transmission electron micrograph of a graphene / carbon fiber composite, according to various embodiments. [Figure 14C] FIG. 14C shows a transmission electron micrograph of amorphous carbon according to various embodiments. [Figure 15A] FIG. 15A shows an SEM image of heat-cured imprinted features according to various embodiments. [Figure 15B]FIG. 15B shows an SEM image of graphene features obtained by photothermal pyrolysis of the features shown in FIG. 15A, according to various embodiments. [Figure 15C] FIG. 15C shows an SEM image of a magnified via of the feature shown in FIG. 15B, according to various embodiments. [Figure 15D] FIG. 15D shows an SEM image of a magnified via of the feature shown in FIG. 15B, according to various embodiments. [Figure 16] FIG. 16 shows Raman spectra of imprinted and thermally cured structures and graphene features derived therefrom upon photothermal pyrolysis in air, according to various embodiments. [Figure 17] FIG. 17 shows optical images of graphene / carbon fiber composites obtained from layer-by-layer coating followed by photothermal pyrolysis of cyclized polyacrylonitrile after two coatings and pyrolysis, according to various embodiments. [Fig. 18A-18F] 18A-18F show SEM images of graphene / carbon fiber composites obtained from layer-by-layer coating followed by photothermal pyrolysis of cyclized polyacrylonitrile after two subsequent coatings and pyrolysis, according to various embodiments. [Figure 19] FIG. 19 shows FTIR spectra of polyacrylonitrile (before cyclization) and cyclized polyacrylonitrile membranes according to various embodiments. [Figure 20A] FIG. 20A shows Raman spectra of graphene / carbon fiber composites (precursor films coated on carbon fiber substrates) obtained from layer-by-layer coatings followed by photothermal pyrolysis of cured poly(flange epoxy) after two and three coatings and pyrolysis according to various embodiments. [Figure 20B] FIG. 20B shows Raman spectra of graphene / carbon fiber composites (precursor films coated on stainless steel substrates) obtained from layer-by-layer coatings followed by photothermal pyrolysis of cured poly(flange epoxy) after two and three coatings and pyrolysis according to various embodiments. [Figure 21A]FIG. 21A shows optical images of dimensionally stable polyimide / graphene composite electrode structures obtained from photothermal pyrolysis in air of screen-printed and heat-cured cyclized polyacrylonitrile electrode structures according to various embodiments. [Figure 21B] FIG. 21B shows a Raman spectrum of a dimensionally stable polyimide / graphene composite electrode structure obtained from photothermal pyrolysis in air of a screen-printed and heat-cured cyclized polyacrylonitrile electrode structure according to various embodiments. [Figure 22A] FIG. 22A shows an optical image of a non-pyrolyzed pure carbon fiber fabric, according to various embodiments. [Figure 22B] FIG. 22B shows an optical image of a photothermally pyrolyzed carbon fiber fabric according to various embodiments. [Figure 23A] FIG. 23A shows an FTIR spectrum of a pure carbon fiber fabric, according to various embodiments. [Figure 23B] FIG. 23B shows Raman spectra of pure carbon fiber fabric and photothermally pyrolyzed pure carbon fiber fabric as a function of xenon flash lamp pulse power, according to various embodiments. [Figure 24A] FIG. 24A shows a low magnification SEM image of MnO 2 -deposited PPG according to various embodiments. [Figure 24B] FIG. 24B shows a low magnification SEM image of MnO2-deposited PPG according to various embodiments. [Figure 24C] FIG. 24C shows a high magnification SEM image of MnO 2 -deposited PPG according to various embodiments. [Figure 24D] FIG. 24D shows a comparison of Raman spectra of MnO2-deposited PPG and PPG according to various embodiments. [Figure 24E] FIG. 24E shows XRD profiles of PPG and corresponding MnO2 deposited on PPG, according to various embodiments. [Figure 24F] FIG. 24F shows an XPS analysis of MnO 2 deposited on PPG according to various embodiments. [Figure 25A]FIG. 25A shows CV curves at 50 mV / s of PPGs prepared at different output pulses and CFs according to various embodiments. [Figure 25B] FIG. 25B shows CV curves of PPG from PBz at different scan rates according to various embodiments. [Figure 25C] FIG. 25C shows the GCD profiles at different current densities of fabricated devices according to various embodiments. [Figure 25D] FIG. 25D shows a Nyquist plot of PPG at frequencies from 104 to 0.1 Hz according to various embodiments. [Figure 26A] FIG. 26A shows the CV curves at different scan rates of a symmetric device prepared using MnO 2 deposited on PPG according to various embodiments. [Figure 26B] FIG. 26B shows the GCD profiles at various current densities of symmetric devices prepared using MnO 2 deposited on PPG according to various embodiments. [Figure 26C] FIG. 26C shows the capacity (F / g) as a function of current density for symmetric devices prepared using MnO 2 deposited on PPG according to various embodiments. [Figure 27A] FIG. 27A shows the Ragone plot of a symmetric device prepared using MnO 2 deposited on PPG, according to various embodiments. [Figure 27B] FIG. 27B shows a demonstration of the device by lighting an LED using three devices connected in series, according to various embodiments. [Figure 28A] FIG. 28A shows a photograph of an experimental setup for EMI shielding measurements including a programmable network analyzer, a waveguide, and a sample holder assembly (top left), a photograph showing a close-up of the sample holder assembly according to various embodiments (bottom left), a photograph showing the proximity of the sample holder according to various embodiments (center), and a photograph showing a sample in the sample holder according to various embodiments (right). [Figure 28B]FIG. 28B shows a schematic diagram showing a front view of a sample placed in a sample holder (left) and a schematic diagram showing a side view of the sample arrangement in the sample holder (right), according to various embodiments. [Figure 29] FIG. 29 shows SE versus frequency illustrating multi-band (C-band, X-band, and Ku-band) EMI shielding effectiveness of a two-layer graphene / carbon fiber composite, according to various embodiments. [Diagram 30] FIG. 30 shows the UV absorption spectrum of Kapton, according to various embodiments. [Figure 31A] FIG. 31A shows optical images of PANI on CF (left) and PANI-derived graphene on CF (right) according to various embodiments. [Figure 31B] FIG. 31B shows the TGA profiles of PANI, PANI-derived graphene, and pure CF according to various embodiments. [Figure 31C] FIG. 31C shows Raman spectra of pure CF (top), PANI-derived graphene on CF (middle), and PANI produced by conventional carbonization at 1000° C. (bottom) according to various embodiments. [Figure 32A] FIG. 32A shows an SEM image of electrochemically deposited PANI according to various embodiments. [Figure 32B] FIG. 32B shows an SEM image of photothermally generated graphene from PANI according to various embodiments. [Figure 32C] FIG. 32C shows the C 1s spectrum of graphene photothermally generated from PANI according to various embodiments. [Figure 33A] FIG. 33A shows CV curves of PANI-derived graphene and CF in 0.5 M sodium sulfate at 50 mV / s according to various embodiments. [Figure 33B] FIG. 33B shows CV curves of PANI-derived graphene in 1 M sulfuric acid at different scan rates (10 mV / s to 100 mV / s) according to various embodiments. [Figure 33C] FIG. 33C shows the GCD curves of PANI-derived graphene at different current densities according to various embodiments. [Diagram 34]FIG. 34 shows a schematic diagram of an eyeglass side arm with energy storage capability formed from polyaniline on carbon fiber, according to various embodiments. [Figure 35A] FIG. 35A shows a screen printed LED circuit including a cPAN precursor, according to various embodiments. [Figure 35B] FIG. 35B shows an LED graphene circuit obtained from photothermal pyrolysis of a screen-printed cPAN precursor, according to various embodiments. [Figure 35C] FIG. 35C shows a demonstration of successful integration of a white light LED into the graphene circuit of FIG. 35B driven by an external power source using graphene wiring with a sheet resistance of 100-200 Ω / sq, according to various embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Reference will now be made in detail to certain aspects of the presently disclosed subject matter, examples of which are illustrated in part in the accompanying drawings. While the disclosed subject matter will be described in conjunction with the enumerated claims, the exemplified subject matter is not intended to limit the claims to the disclosed subject matter.

[0012] The drawings illustrate generally, by way of example, but not by way of limitation, various aspects of the present invention. Throughout this specification, values ​​expressed in range format should be interpreted flexibly to include not only the numerical values ​​explicitly recited as the limits of the range, but also all individual numerical values ​​or subranges subsumed within the range as if each numerical value and subrange were explicitly recited. For example, the range "about 0.1% to about 5%" or "about 0.1% to 5%" should be interpreted to include not only about 0.1% to about 5%, but also the individual values ​​(e.g., 1%, 2%, 3%, and 4%) and subranges (e.g., 0.1% to 0.5%, 1.1% to 2.2%, 3.3% to 4.4%) within the indicated range. The statement "about X to Y" has the same meaning as "about X to about Y" unless otherwise indicated. Similarly, the statement "about X, Y, or about Z" has the same meaning as "about X, about Y, or about Z" unless otherwise indicated.

[0013] In this specification, the term "a" is used to include one or more, unless the context clearly indicates otherwise. The term "or" is used to refer to a non-exclusive "or" unless otherwise indicated. The statements "at least one of A and B" or "at least one of A or B" have the same meaning as "A, B, or A and B". It may also be understood that expressions or terms used herein and not otherwise defined are for descriptive purposes only and not for limiting purposes. The use of section headings is intended to aid in the reading of this specification and should not be construed as limiting, and information associated with a section heading may be present within or outside that particular section.

[0014] In the methods described herein, operations may be performed in any order without departing from the principles of the invention, unless a temporal or operational order is explicitly recited. Moreover, specified operations may be performed simultaneously unless express claim language recites that they be performed separately. For example, a claimed operation of doing X and a claimed operation of doing Y may be performed simultaneously in a single operation, whereby the process falls within the claimed process language.

[0015] The term "about" as used herein allows for some variability in a value or range, for example, within 10%, within 5%, or within 1% of the stated value or the limits of a stated range, and includes the exact stated value or range.

[0016] As used herein, the term "substantially" refers to a majority or majority, such as at least about 50%, 60%, 70%, 80%, 90%, 95%, 96%, 97%, 98%, 99%, 99.5%, 99.9%, 99.99%, or at least about 99.999% or more, or 100%. The term "substantially free" as used herein can mean having no or only such an amount of the material such that the amount of the material present does not affect the material properties of the composition including that material, such as about 0% to about 5%, about 0% to about 1%, about 5% or less, about 5% or less and about 4.5% or more, or 4%, 3.5%, 3%, 2.5%, 2, 1%.5, 1%, 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1%, 0.01%, or about 0.001% or less, or about 0% by weight of the material.

[0017] As used herein, the term "polymer" refers to a molecule having at least one repeating unit, and can include copolymers. [Graphene film formation method] Various aspects of the invention provide methods of forming a graphene film. The method includes depositing a polymeric graphene precursor on a substrate. The method also includes irradiating the polymeric graphene precursor deposited on the substrate with a pulsed high intensity light source emitting at two or more wavelengths and having a pulse duration of less than one second. The irradiation converts the polymeric graphene precursor into a graphene film. The irradiation can pyrolyze the polymeric graphene precursor to form a graphene film.

[0018] The formed graphene film may be a composite graphene film or a graphene non-composite film. The formed graphene film may include a substrate such that the formed graphene film is coated on a substrate. The substrate may be any suitable material, such as a heat-sensitive material or a heat-non-sensitive material. The substrate and the polymer-graphene precursor may have the same chemical composition. The substrate and the polymer-graphene precursor may have different chemical compositions. The substrate and the graphene film formed on the substrate may have different chemical compositions. The substrate may be a material other than a graphene film or a polymer-graphene film precursor.

[0019] The irradiating includes irradiating the polymer graphene precursor coated on a substrate. The irradiating may include irradiating the polymer graphene precursor or both the polymer graphene precursor and the substrate. The irradiating the substrate may not cause a change to the substrate or may cause a change to the substrate. In various embodiments, the irradiating the substrate may convert the substrate to a material comprising graphene. In various embodiments, the irradiating the substrate does not convert the substrate to a material comprising graphene. The irradiating the polymer graphene precursor may be performed in air, an inert gas, or any suitable gas. The irradiating the polymer graphene precursor may be performed in atmospheric air.

[0020] Irradiation can include irradiating and / or maintaining the polymeric graphene precursor at a temperature less than 100° C., e.g., between 0° C. and 99° C., between 10° C. and 50° C., between 20° C. and 30° C., less than 100° C. and greater than or equal to 0° C., 1, 2, 4, 6, 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95° C. Irradiation can include irradiating the polymeric graphene precursor at room or ambient temperature. Irradiation can include substantially maintaining the polymeric graphene precursor at a pre-irradiation temperature throughout irradiation. Irradiating may include increasing the temperature of the polymeric graphene precursor by 10° C. or less, 2° C. or less, to 0° C., or to 100° C. or less and 0.001° C., 0.005, 0.01, 0.05, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95° C. or more relative to the pre-irradiation temperature of the precursor film. The method may include localizing light absorption in the precursor film such that the temperature increase of the polymeric graphene precursor is below a desired limit. By localizing light absorption in the precursor film during photothermal treatment, the treatment can be carried out at ambient temperature, allowing for the preparation of high quality graphene and graphene composites on any substrate, including heat-sensitive substrates, without the need for a catalyst. Various aspects of the method of the present invention allow for the substrate to be left undamaged relative to its state prior to coating and irradiation. By allowing for the formation of graphene films without damaging the substrate, the method allows for the individual selection of polymer-graphene precursors and substrates, providing advantages in tailoring graphene materials on any substrate.

[0021] The light source may be any suitable light source that induces graphene formation from the polymeric graphene precursor described herein. The light source may be any suitable light source having an emission band that overlaps with an absorption band of the polymeric graphene precursor. The light source may include a xenon flash lamp, a halogen flash lamp, a light emitting diode, two or more light emitting diodes, or a combination thereof. The light source may include or be a xenon flash lamp. The light source may include an emission wavelength that overlaps with an absorption wavelength of the polymeric graphene precursor. The light source may include an emission wavelength in the range of 100 nm to 2000 nm, 300 nm to 800 nm, 400 nm to 600 nm, or less than 2000 nm and more than 100 nm, 150, 200, 250, 300, 350, 400, 410, 420, 430, 440, 450, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, 560, 570, 580, 590, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1200, 1400, 1600, or 1800 nm.

[0022] The pulse duration of the light source during irradiation can be shorter than the thermal equilibration time of the polymeric graphene precursor such that the temperature rise of the polymeric graphene precursor during irradiation is small, minimal, or zero. The pulse duration can be any suitable pulse duration, such as 1-999 ms, 200-900 ms, 400-800 ms, or less than 999 ms and 1 ms, 2 ms, 5, 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, or 950 ms or more.

[0023] The light source may have any suitable intensity during irradiation, such as 100V to 2000V, 400V to 700V, or up to 2000V and 100V, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, or 1900V or more. 2 ~100J / cm 2 , 1J / cm 2 ~10J / cm 2 , 2J / cm 2 ~9J / cm 2 , or 100 J / cm 2 Less than or equal to 0.1 J / cm 2 , 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 12, 14, 16, 18, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 J / cm 2 The light source may have an energy density per pulse of 10 J / cm or more during irradiation. 2 ~1000J / cm 2 , 30J / cm 2 ~200J / cm 2 , or 1000 J / cm 2 Less than or equal to 10 J / cm 2 , 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 250, 300, 400, 500, 600, 700, 800, or 900 J / cm 2 or more.

[0024] The light source may have any suitable pulse frequency, such as between 0.001 Hz and 1000 Hz, between 0.1 Hz and 10 Hz, between 0.5 Hz and 1 Hz, or between 1000 Hz and 0.1 Hz, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 2, 2.5, 3, 4, 5, 6, 8, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 80, 100, 150, 200, 250, 300, 400, 600, 800, or 900 Hz or more. Irradiating can include between 5 and 1000 pulses of the light source, between 10 and 40 pulses of the light source, or any suitable number of pulses of the light source, such as less than 1000 pulses and up to 5 pulses, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 140, 160, 180, 200, 250, 300, 400, 500, 600, 700, 800, or 900 pulses or more.

[0025] Coating the polymeric graphene precursor on the substrate can be done by any suitable means. For example, coating the polymeric graphene precursor on the substrate can include using printing, offset printing, inkjet printing, transfer printing, aerosol jet printing, microcontact printing, embossing, nanoimprint lithography, optical lithography, electron beam lithography, ion beam lithography, or a combination thereof. The method can include curing the coating of the polymeric graphene precursor, such as by thermal curing, light or UV curing, or a combination thereof, to form a cured film of the polymeric graphene precursor. Irradiating can include irradiating the cured film. In other aspects, the method does not include curing and irradiating can include irradiating an uncured film of the polymeric graphene precursor.

[0026] The polymeric graphene precursor on the substrate may include a patterned polymeric graphene precursor. That is, the polymeric graphene precursor may be patterned. The patterning may be introduced into the coating after the coating is applied to the substrate or may be introduced into the coating at the same time the coating is applied to the substrate. The patterned coating of the polymeric graphene precursor may be formed by any suitable method, such as printing, offset printing, inkjet printing, transfer printing, aerosol jet printing, microcontact printing, or a combination thereof. The patterned coating of the polymeric graphene precursor may be formed by embossing, nanoimprint lithography, or a combination thereof. The patterned coating of the polymeric graphene precursor may be formed by optical lithography, electron beam lithography, or ion beam lithography.

[0027] The polymeric graphene precursor may be any suitable polymer precursor that forms a graphene film under the irradiation conditions described herein. For example, the polymeric graphene precursor may include a polymer containing disubstituted benzene, benzene substituted with one or more chromophores, polycyclic aromatic rings, or a combination thereof. The polymeric graphene precursor may include a polymer containing nitroaniline, aniline, nitrophenol, biphenyl (e.g., two conjugated benzene rings), nitrobenzene, benzaldehyde, acetophenone, pyrene, pentacene, anthracene, tetracene, or a combination thereof. The polymeric graphene precursor may include a polymer selected from resol, oligomers of pyrene pitch, cyclized polyacrylonitrile, polyaniline, carbon fibers, thermoset resin networks formed from blending and crosslinking polybenzoxazine with epoxy, and combinations thereof. The polymeric graphene precursor may comprise a polymer selected from poly(3-phenyl-2,4-dihydro-1,3-benzoxazine), poly(phenylbenzoxazine), poly(3-furanyl-2,4-dihydro-1,3-benzoxazine), poly(furanylbenzoxazine), poly(phenol-co-formaldehyde), resole, oligomers of pyrene pitch, cyclized polyacrylonitrile, pure carbon fiber, polyaniline, thermoset networks formed from blending and crosslinking polybenzoxazine with bis-phenol-A furfuryl diglycidyl ether, and combinations thereof. In various embodiments, the polymeric graphene precursor comprises polyaniline. In various embodiments, the polymeric graphene precursor comprises polyaniline. The polymeric graphene precursor is irradiated to form a graphene film with reduced or no requirement for high temperature crosslinking or curing. For example, such irradiation may be performed (e.g., maintained) at room temperature or at or below 30° C., 35, 40, 45, or 50° C. In various embodiments, the polymeric graphene precursor comprises polyaniline and the graphene film produced is a porous graphene film.

[0028] The polymer graphene precursor may have an absorption band that overlaps with the emission band of the pulsed light source. The polymer graphene precursor may have an absorption band in the range of 100 nm to 2000 nm, 300 nm to 800 nm, 400 nm to 600 nm, or 2000 nm or less and 100 nm, 150, 200, 250, 300, 350, 400, 410, 420, 430, 440, 450, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, 560, 570, 580, 590, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1200, 1400, 1600, or 1800 nm or more.

[0029] The substrate can be any suitable substrate. The substrate can include plastic, metal, cloth, woven cloth, carbon, or a combination thereof. The carbon-containing substrate can include carbon fiber, carbon mesh, carbon cloth, carbon composite, graphene composite, graphene, carbon film, or a combination thereof. In various embodiments, the carbon-containing substrate can form graphite, graphene, or a combination thereof during irradiation. In other embodiments, the carbon-containing substrate can remain unchanged during irradiation. Alternatively, the carbon-containing substrate can be transformed into a material other than graphite and / or graphene.

[0030] The graphene film can have a conductivity of at least 150 S / cm, e.g., 150 to 5000 S / cm, 150 S / cm to 1000 S / cm, 150 to 500 S / cm, or 5000 S / cm or less but 150 S / cm, 160, 170, 180, 190, 200, 220, 240, 260, 280, 300, 320, 340, 360, 380, 400, 420, 440, 460, 480, 500, 550, 600, 650, 700, 750, 800, 900, 1000, 1250, 1500, 1750, 2000, 2500, 3000, or 3500 S / cm or more.

[0031] The graphene film exhibits a 1350 cm -1 A characteristic disorder band (D band) with a peak near 1582 cm-1 The graphene film may have a characteristic graphitic band (G band) with a peak near 2700 cm ratio of less than 1, as determined by Raman spectroscopy. -1 A characteristic 2D band with a peak near 1582 cm that can be fitted to a single Lorentzian function -1 The ratio of the characteristic graphitic band (G band) having a peak nearby may be less than 1.

[0032] The irradiating can include pulsed power modulation. The method can include tailoring the microstructure of the graphene film using pulsed power modulation. [Graphene film] Various aspects of the invention provide graphene films formed by the methods of the invention. The graphene film may be a graphene film deposited on a substrate as described herein. The graphene film may be a patterned graphene film or an unpatterned graphene film.

[0033] [Devices containing graphene films] Various aspects of the invention provide electrochemical energy storage devices, electromagnetic shielding materials, chemical or biological sensors, post-CMOS nanoelectronic devices, heat shielding materials, structural composites, filters, or combinations thereof, comprising graphene films formed by the methods of the invention. For example, graphene films formed by the methods can find applications in electrochemical energy storage devices as electrodes in supercapacitors and batteries, electromagnetic interference and electromagnetic pulse shielding structures as shielding materials, chemical and biological sensors as electrodes, flexible electronics as electrodes and sensors, post-CMOS nanoelectronic devices as interconnects, thermal applications as heat shielding materials in hypersonic and electronics, structural composites, filtration as filters for water and biological products, eyewear such as eyeglass side arms that can store electrochemical energy and be used for laser projection applications, and the like. Various aspects of the invention provide graphene derived from photothermal pyrolysis of screen printed exemplary precursor materials such as cPAN and / or poly(BZ) coated onto flexible polyimide and targeted for printing and flexible electronics applications.

[0034] [Example] Various aspects of the present invention may be better understood by reference to the following examples, which are provided for illustrative purposes only and are not intended to limit the invention to the examples set forth herein.

[0035] A method for rapid and efficient preparation of graphene by photothermal pyrolysis of precursor thin films in millisecond time frames at ambient conditions involves photothermal pyrolysis of unpatterned, printed-patterned, and imprint-patterned graphene precursor films using high-intensity pulsed light from a xenon flash lamp operating in air at room temperature.

[0036] Figure 1 shows the processing scheme. By localizing light absorption in the precursor film during photothermal processing, the processing can be carried out at ambient temperature, making it possible to prepare high-quality graphene and graphene composites over large areas and without the need for catalysts on any substrate, including those that are heat-sensitive. The use of patterned films deposited using screen printing or additives directly results in two-dimensionally patterned graphene materials. Nanoimprint patterning of precursor films prior to photothermal processing can directly result in engineered three-dimensional surfaces with features spanning nanoscale to microscale dimensions. The processing relies on the starting precursor to produce high-quality pure graphene and graphene composites.

[0037] If the radiation source is pulsed for a duration (on the order of milliseconds) shorter than the thermal equilibration time of the preceramic polymer with the substrate, the precursor film may rapidly heat up and pyrolyze before it can transfer significant energy to the substrate. Ideal pyrolysis conditions depend on the precursor film, its absorption cross section, film thickness, type of substrate, and type / content of additives (if any). The exposure energy delivered to the sample can be adjusted by varying the discharge voltage and pulse duration. The ability to independently adjust the pulse duration and intensity provides independent control over both the power and energy delivered to the sample. The choice of photoprocessing using a xenon flash lamp source rather than a laser offers several advantages, including reduced cost and complexity, improved efficiency in converting electrical energy to light, and scalability for large area processing without rastering.

[0038] Polymer graphene precursors have an absorption profile that overlaps with a portion of the emission spectrum of a xenon flash lamp with a peak intensity at 400-600 nm. The n-π* (R band) is the most relevant electronic transition corresponding to this wavelength region, and materials with moieties excitable by radiation within a significant portion of the emission spectrum of a xenon flash lamp will necessarily pyrolyze well when irradiated with pulses of sufficient intensity and power density. Although the use of a xenon flash lamp is emphasized here, other broadband, high intensity pulse sources can also be used to photothermally pyrolyze suitable precursors. Examples of suitable precursors include disubstituted benzenes such as nitroaniline, nitrophenol, and biphenyl (where the two aromatic rings are conjugated), as well as benzenes substituted with chromophores such as nitrobenzene, benzaldehyde, acetophenone, nitrobenzene, and biphenyl, and materials containing polynuclear aromatic compounds with high aromatic content such as pyrene, pentacene, anthracene, and tetracene. Selected representative examples of precursor resins shown in Figures 2A-2C include, but are not limited to, poly(3-phenyl-2,4-dihydro-1,3-benzoxazine) or poly(phenylbenzoxazine) (I), poly(3-furanyl-2,4-dihydro-1,3-benzoxazine) or poly(furanylbenzoxazine) (II), poly(phenol-co-formaldehyde) or resole (III), oligomers of pyrene pitch (IV), cyclized polyacrylonitrile (V), polyaniline, thermoset resin networks formed from blending and crosslinking polybenzoxazine with epoxies such as furfuryl diglycidyl ether of bisphenol-A (where R2 is bisphenol-A and epoxy is the diglycidyl ether of bisphenol-A) and furfuryl epoxies (VI). Other examples include pure carbon fibers and / or polyaniline (e.g., structure -(phenyl-NH) n -, and the phenyl rings in the polymer backbone have 1,4 (para) connectivity.

[0039] Conventional methods, with the exception of electrochemical reduction and CVD approaches, are not scalable for large-scale production. Most of them are extremely energy-intensive, operated under harsh conditions, expensive, and very slow to run. Various aspects of the present invention overcome all of these drawbacks by using high-intensity pulsed xenon flash lamps in air at ambient conditions at room temperature and atmospheric pressure to pyrolyze suitable precursors in a few milliseconds. The millisecond duration of the radiation pulse is shorter than the thermal equilibrium time of the precursor, allowing for pyrolysis of the precursor and the formation of high-quality graphene before significant energy transfer to the substrate, making this process uniquely suitable for graphene preparation on or adjacent to heat-sensitive materials. The rapid precursor pyrolysis and phase transformation during the flash lamp process limits oxidation of the resulting graphene, even in air.

[0040] Example 1: Synthesis of Exemplary Precursor Materials (Benzoxazine Monomer and Polyaniline) Benzoxazine monomer can be synthesized via a one-pot chemical reaction using bisphenol A, aniline, and paraformaldehyde according to a molar ratio of 1:2:4, as shown in FIG. 2D. Bisphenol A and aniline are introduced into a two-necked round-bottom flask fitted with a reflux condenser, and the resulting solution is stirred at room temperature for 30 minutes to ensure uniform mixing. The temperature of the mixture is then reduced to 5° C. using an ice bath, after which a stoichiometric amount of a dispersion of paraformaldehyde dispersion in dioxane is added dropwise to the bisphenol A and aniline reaction mixture. The resulting reaction mixture is then heated in a silicone oil bath at 60° C. for 1 hour, followed by heating at 120° C. for an additional 5 hours with constant stirring and reflux. The conversion of the reagents to benzoxazine monomer is confirmed by a change in the color of the reaction solution from milky white to clear orange. Residual dioxane solvent can be removed from the benzoxazine monomer by heating the product mixture at 130° C. for 2 hours, after which the product is cooled to room temperature to obtain pure benzoxazine monomer. The pure benzoxazine monomer can be used as is without further treatment. The reaction yield is 90%.

[0041] Polyaniline (PANI) was electrochemically grown (electrodeposited) on conductive carbon fiber substrates using three electrodes set up as previously described in various publications, i.e., carbon fiber as working electrode, platinum wire as counter electrode, and Ag / AgCl as reference electrode. The electrodes were immersed in an aqueous solution containing 0.3 M aniline and 1 M HCl as electrolyte. A constant current of 10 mA was applied for 10 min to grow PANI uniformly on the carbon fiber. After deposition, the PANI on CF was thoroughly washed with deionized water to remove excess electrolyte and then dried at 100 °C for 1 h.

[0042] Example 2: Photothermal pyrolysis processing of exemplary unpatterned precursor film materials 3-5 are schematic diagrams of the processing sequence for the photothermal pyrolysis of two exemplary unpatterned precursor films of polybenzoxazine and cyclized polyacrylonitrile coated on carbon fibers. FIG. 6 shows the processing scheme for the photothermal pyrolysis of pure carbon fibers. Solutions of precursor materials in an appropriate solvent and appropriate concentrations are first formulated for use in the photothermal treatment. For the exemplary precursor material of benzoxazine, and blends of benzoxazine and epoxy precursor materials, solutions are made in dioxane to a concentration of 1.0 g / mL. FIG. 5 shows the photothermal treatment sequence of cyclized polyacrylonitrile, another exemplary precursor material. Solutions of polyacrylonitrile in dimethylformamide and appropriate concentrations are first formulated for use in the photothermal treatment.

[0043] The processing sequence for unpatterned films begins with coating a film of the precursor 5-8 microns thick onto both sides of a suitable substrate, e.g., a carbon fiber substrate (dimensions 10 cm x 10 cm), using a Meyer rod (#20), drying at room temperature, and then thermal curing for 24 hours in a nitrogen-filled oven maintained at 220°C. Curing crosslinks the precursor monomer, converting it to the corresponding polymer, as shown in Figure 4 for the crosslinking of benzoxazine monomers to an exemplary polybenzoxazine precursor.

[0044] The unpatterned and patterned films are then photothermally pyrolyzed using a xenon flash lamp in a PulseForge 1300 tool (PulseForge® 1300 Xenon Lamp System, Novacentrix, Austin, Texas, USA). The dried and crosslinked PCP film on the respective substrate is first loaded onto a stainless steel chuck, which is placed under the center of the xenon flash lamp of the tool. The lamp needs to be positioned 15 mm above the sample to ensure a uniform energy distribution in the irradiated PCP film. It is important to control the rate and mechanism by which the organics and solvents in the PCP film are removed as gaseous products during the pyrolytic conversion of the precursors to ensure uniform densification, prevent the retention of impurities, and / or prevent the creation of gassing defects such as pores. For this purpose, first, a 5.3 J / cm 2 The sample must then be irradiated with 20 pulses (frequency of 0.5 Hz, pulse length of 800 μs, and voltage of 540 V) with an areal energy density of 8.2 J / cm to volatilize the residual solvent and low molecular weight components of the film that still remain in the film after thermal curing in a vacuum oven. 2 The samples must be pyrolyzed by irradiating them with 20 high power pulses (1.0 Hz frequency, 800 μs pulse length, and 620 V voltage) with an areal energy density of 1.

[0045] The photothermal treatment of PANI on CF involved two steps similar to those of polybenzoxazine-based systems. PANI on CF was crosslinked during carbonization, allowing photothermal treatment without the need for high-temperature crosslinking, making the process more sustainable and lower energy consumption. The sample was initially exposed to 2.6 J / cm 2 The organic residues were removed by 10 pulses of low energy dose (400V, 800μs, 1Hz frequency) followed by 8.91J / cm 2 PANI was completely converted to graphene by irradiation with 10 pulses of high energy dose (630 V, 800 μs, 1 Hz frequency).

[0046] Example 3: Photothermal pyrolysis processing of exemplary patterned precursor film materials The processing sequence for the patterned films (Figure 7) involves soft lithographic imprint patterning of suitable polymer films coated onto suitable substrates, including silicon wafers and stainless steel foils, using a fluorinated solvent permeable patterned poly(dimethylsiloxane) stamp while simultaneously curing the film at an appropriate temperature. The cured film is then subjected to photothermal pyrolysis in air using a high intensity xenon flash lamp to obtain patterned graphene structures without the use of a catalyst. The processing conditions for photothermal pyrolysis are 5.3 J / cm for the cured samples. 2The method involved irradiating the stamp with 70 pulses (1.0 Hz frequency, 500 μs pulse length, and 540 V voltage) of areal energy density of 1000 nm. Fluorination of the stamp ensures smooth release of the stamp at the end of the imprinting process without damaging the imprinted features. Thermal curing at 220° C. in an oven supplied with nitrogen gas results in structures that are structurally stable against photothermal pyrolysis in air at temperatures up to 1500° C. Structures of various shapes, including lines, holes, trenches, etc., and length scales ranging from nanometers to millimeters, are easily realized in minutes with this technique. Suitable precursor polymers have absorption spectra with peak maxima that overlap with the emission spectrum of a xenon flash lamp, and these include polybenzoxazines, phenol-formaldehyde resins, etc.

[0047] Example 4: Photothermal pyrolysis processing of exemplary screen-printed precursor film materials FIG. 8 shows the processing sequence for screen printed films, which involves dispensing an appropriate amount of neat viscous solution of the precursor film onto a screen placed over a suitable hot substrate, such as a polyimide film, and printing an image of the screen onto the substrate by applying a force to force the solution through the screen. The film is then thermally cured for 24 hours at the appropriate temperature (220° C. for polybenzoxazine) in an oven supplied with nitrogen. For poly(acrylonitrile) precursors, the screen printed film is first cured at 150° C. in an oven supplied with air, followed by heating the sample at 250° C. overnight to cyclize the linear polyacrylonitrile. Thermal curing of the screen printed precursor film of polybenzoxazine at 220° C. and cyclization of polyacrylonitrile at 250° C. results in a structure that is structurally stable against photothermal pyrolysis in air at temperatures up to 1500° C.

[0048] The cured or cyclized precursor film is then subjected to photothermal pyrolysis in air to convert it into graphene structures without the use of a catalyst. 2The photothermal pyrolysis using such low power pulses allows for the maintenance of the structural integrity of the screen-printed features, which could otherwise be damaged.

[0049] Example 5. Materials characterization of exemplary unpatterned precursor polybenzoxazine and graphene / carbon fiber composites derived from photothermal pyrolysis Polybenzoxazine is a moderate char yield polymer with an absorbance spectrum that overlaps with the maximum intensity of the xenon lamp emission spectrum (Figures 9A and 9B). UV / Vis / NIR absorption spectra of polybenzoxazine films coated on stainless steel substrates were collected in reflectance mode over the wavelength range of 200 nm to 1200 nm using a Lambda-1050 UV / Vis / NIR spectrophotometer (Perkin-Elmer, Boston, MA, USA). Samples were spin-coated on glass substrates for measurements. Upon photothermal pyrolysis, the films can reach temperatures in excess of 1530 °C and 2040 °C depending on the pulsed power modulation (Figures 9C and 9D). IR spectroscopy was used to monitor the structural changes of the films in response to treatment. Infrared absorption spectra of the samples were measured from 3200 to 500 cm using a Frontier 1300 attenuated total reflectance Fourier transform infrared spectrometer (Perkin-Elmer, Boston, MA, USA). -1 The samples consisted of composite powders scraped off from carbon fiber substrates after pyrolysis. -1 and 1491 cm -1The disappearance of the monomer oxazine ring and trisubstituted benzoxazine in the peaks confirmed the complete conversion of the benzoxazine monomer to polymer and the thermal curing of the polymer (Figure 9E). The lack of structure in the composite spectrum confirmed the complete pyrolysis of the precursor material and its conversion to a carbonaceous composite (Figure 9E). Thermogravimetric analysis was performed in a nitrogen atmosphere at 10 °C / min in the temperature range of 25-700 °C on a Q50TA instrument. Thermogravimetric analysis confirmed the conversion of polybenzoxazine to a carbonaceous composite (Figure 9F).

[0050] The surface morphology of the samples was analyzed using field emission scanning electron microscopes (FEI Magellan 400 XHR SEM, and FEI Helios Dual Beam FIB SEM). High-resolution transmission electron microscopy (HRTEM) analysis of the samples was performed by a JEOL JEM-2200 OFS energy-filtered transmission electron microscope using a 200 kV accelerating voltage. The samples consisted of graphene composite powders scraped off from carbon fiber substrates after pyrolysis. Raman spectroscopy was used to investigate the phase order and phase transformation of the composites. Raman spectra of the samples were recorded at room temperature with a ThermoScientific DXR Smart Raman spectrometer (ThermoFisher Scientific, Waltham, MA, USA) using an excitation laser wavelength of 633 nm and a laser power of 5 mW, a spot diameter of 3.1 μm, and a sample exposure of 5 s. 10A-10D show optical images of cured poly(benzoxazine) on carbon fiber cloth (FIG. 10A) and SEM images of composites obtained from photothermal pyrolysis of cured poly(benzoxazine) (FIG. 10C, FIG. 10D). FIG. 11A-11C show optical images of pure carbon fiber fabric (FIG. 11A), carbon fiber / graphene composite obtained after coating and pyrolysis of one layer of precursor film (FIG. 11B), and carbon fiber / graphene composite with a thickness of 1093 μm obtained after coating and pyrolysis of two layers of precursor film (FIG. 11C). FIG. 11D shows an SEM image of the composite of FIG. 11C. The composite has a microporous surface morphology. The Raman spectrum obtained for the photothermal pyrolyzed sample shows a peak at 1582 cm-1 (graphite, G band) and 1350 cm -1 (disorder, D band) (Figure 12A). The ratio of the intensity of the D band to the intensity of the G band (I D / I G The I ratio is a good measure of the quality of graphitic carbon in a sample. D / I G The ratio is 0.46. Since this ratio is less than 1, the sample has a high degree of ordering and is highly graphitic. -1 The peak near (the 2D band) is an overtone of the D band, which is also characteristic of graphite, specifically the graphitic ordering of free carbon along the free axis. The ability to fit this peak to a single Lorentzian peak indicates the presence of high quality graphene in the sample. Also, the size of this peak relative to the G peak is a good measure of the number of graphene layers present in the sample. I 2D / I G The ratio is 0.64, suggesting the presence of few layers of graphene in the sample.

[0051] X-ray diffraction patterns reveal that the composites are highly ordered (FIG. 12B). The crystallinity of the photothermally induced graphene composites was determined using an X-ray diffractometer (PANanalytical X´Pert X-ray diffractometer) with CuKαα radiation of wavelength 1.54 Å at a voltage of 45 kV and a current of 40 mA. X-ray photoelectron spectroscopy (XPS) of the graphene composites was carried out using a Physical Electronics Versa Probe II instrument equipped with a monochromated Alkα X-ray source (hν=1486.6 eV) and a concentric hemispherical analyzer. All peaks were corrected using the reference C1s spectrum at 284.5 eV. The XPS spectrum showed the presence of C1s at a binding energy of 284.5 eV, which is characteristic of the graphene and graphite structures, sp 2 XPS also shows that the atomic composition of the composite is 99.1% C and 0.9% O, suggesting a pure carbonaceous composite.

[0052] Figures 13A-D show the pulse power modulation and phase ordering of the graphene / carbon composite microstructure. Low power treatment results in complete carbonization, leading to a low quality graphene composite with significant defects and high porosity. High power treatment is associated with fewer defects, less porosity, and higher quality graphene. The I of the spectra obtained with high power pulse treatment D / I G is 0.46, and the I 2D / I G is 0.65, and the I D / I G is 1.29, and the I 2D / I G was 0.57. For low power pulse treatment, 106 J / cm 2 5.3 J / cm per pulse, corresponding to a total areal energy density of 2 Twenty pulses (0.5 Hz, 800 μs pulse length, and 540 V voltage) with an areal energy density of 164 J / cm were used. 2 8.2 J / cm per pulse, corresponding to a total areal energy density of 2 20 pulses of areal energy density of 1.0 Hz, 800 μs pulse length, and 620 V voltage were used.

[0053] Transmission electron microscopy was used to study the microstructure of the composites. A hexagonal lattice with a D spacing of about 0.33 nm obtained by Fourier transformation further confirmed the presence of graphene in the composites (Figures 14A-C). In contrast, the TEM of amorphous carbon (Figure 14C) does not show any kind of structure.

[0054] Example 6: Material characterization of exemplary patterned precursor polybenzoxazine and graphene / carbon fiber composites derived from photothermal pyrolysis Figures 15A-15D show SEM images of the imprinted and thermally cured structure and the graphene features obtained from the structure upon photothermal pyrolysis in air. Figures 15B-15D show dimensionally stable graphene features including lines, square holes, and trenches with patterned features decorated with graphene flakes and platelets (grey). When the feature size is smaller than the graphene flakes and platelets, some of the imprinted features are covered by the graphene flakes and platelets.

[0055] Figure 16 shows the results for 175 J / cm 2 2.5 J / cm per pulse, corresponding to a total areal energy density of 2 70 pulses (1.0 Hz, 500 μs pulse length, and 520 V voltage) with an areal energy density of 210 J / cm 2 3 J / cm per pulse, corresponding to a total areal energy density of 2 FIG. 1 shows Raman spectra of imprinted and thermoset structures and graphene features obtained from the structures upon photothermal pyrolysis in air as a function of irradiation pulse energy density using 70 pulses (1.0 Hz, 500 μs pulse length, and 560 V voltage) with an areal energy density of 1.0 Hz. Non-thermolyzed samples were not photothermally treated. The spectra obtained for the photothermally pyrolyzed samples show a peak at 1582 cm -1 (graphite, G band) and 1350 cm -1 (disorder, D band). The intensity ratio of the D band to the G band is 210 J / cm 2 The ratio of the D-band intensity to the G-band intensity is less than 1 for the sample pyrolyzed at a total pulse energy density of 170 J / cm, indicating that the sample has a high degree of structural order and high graphitic phase quality. 2 The photothermally pyrolyzed samples showed a high degree of structural disorder and low graphitic phase quality. -1The graphene has a 2D peak near 210 J / cm, which is also characteristic of graphite, specifically the graphitic ordering of free carbon along the free axis. The ability to fit this peak to a single Lorentzian peak indicates the presence of high quality graphene in these samples. 2 In samples photothermally pyrolyzed with pulses of 10000 Hz, the ratio of the 2D peak to the G peak is less than 1, suggesting the presence of few layers of graphene in the samples. The quality of the graphene obtained improves with the pulse power density used to pyrolyze the precursor film. In contrast, the non-pyrolyzed samples lack a 2D peak and have a very broad D peak and a poorly defined G peak.

[0056] Example 7: Material properties of graphene / carbon fiber composites derived from photothermal pyrolysis of an exemplary unpatterned precursor (cyclized polyacrylonitrile) Cyclized polyacrylonitrile has an absorbance spectrum that overlaps with the maximum intensity of the xenon lamp emission spectrum, whereas linear polyacrylonitrile does not. This explains why cyclized polyacrylonitrile is easily pyrolyzed with a xenon flash, whereas its linear form is not. Figure 17 shows optical images of graphene / carbon fiber composites obtained from photothermal pyrolysis of cyclized polyacrylonitrile films after layer-by-layer coating followed by one coating and pyrolysis. The surface morphology of the composites was investigated by scanning electron microscopy. Figures 18A-18F show SEM images of graphene / carbon fiber composites obtained from photothermal pyrolysis of cyclized polyacrylonitrile films after layer-by-layer coating followed by one coating and pyrolysis. The composites have a microporous surface morphology. IR spectroscopy was used to observe the structural changes of the membrane during the cyclization process (Figure 19). From the FTIR spectrum, the 2245 cm -1 Disappearance of the nitrile group C≡N peak at 1596 cm -1 The appearance of a C=N peak at 1257 cm -1The completion of the cyclization reaction of polyacrylonitrile is confirmed as indicated by the appearance of a C-N single bond peak at 1000 nm. The absence of structure in the spectrum of the composite obtained from pyrolysis confirmed the complete pyrolysis of the precursor material and conversion to the carbonaceous composite.

[0057] Raman spectroscopy was used to investigate the phase ordering and phase transformation of the composites as a function of the substrate type (carbon fiber and stainless steel). The Raman spectra of the composites obtained for both carbon fiber and stainless steel substrates (Figures 20A and 20B) show a peak at 2650 cm -1 The presence of a 2D peak at 1350 cm -1 Disorder band at 1550cm -1 The intensity ratio of the graphite band at I is slightly lower than 1, especially after a single layer-by-layer coating on the carbon fiber substrate and after pyrolysis. D / I G Considering the fact that the ratio is 1350 cm, it is confirmed that the composite contains graphene of fairly good quality. -1 Disorder band at 1550cm -1 The ratio of the intensity of the 2D peak to the graphite band at 2D is slightly greater than 1.0, suggesting that perhaps the stainless steel substrate is not as efficient as the carbon fiber in forming high quality graphene. The ability to fit the 2D peak obtained for both substrates to a single Lorentzian peak indicates the presence of high quality graphene in the samples. Also, the size of this peak relative to the G peak is a good measure of the number of graphene layers present in the sample. The ratio of the 2D peak to the G peak is slightly less than 1 for the samples obtained for the two substrates, suggesting the presence of few layers of graphene in the samples.

[0058] Example 8: Material properties of exemplary screen-printed precursor cyclized polyacrylonitrile and graphene / carbon fiber composites derived from its photothermal pyrolysis 21A and 21B show optical images (FIG. 21A) and Raman spectra (FIG. 21B) of dimensionally stable polyimide / graphene composite electrode structures obtained from photothermal pyrolysis in air of screen-printed and heat-cured cyclized polyacrylonitrile electrode structures. D / I G is 0.63, and the I 2D / I G The photothermal treatment was 50 J / cm 2 2.5J / cm per pulse, corresponding to a total areal energy density of 2 A Raman spectrum of 20 pulses (1.0 Hz, 500 μs pulse length, and 490 V voltage) with an areal energy density of 1.0 Hz was used. The Raman spectrum obtained for this sample showed a peak at 1582 cm -1 (graphite, G band) and 1350 cm -1 (disorder, D band) (Figure 21B). The ratio of the intensity of the D band to the intensity of the G band (I D / I G The I ratio is a good measure of the quality of graphitic carbon in a sample. D / I G The ratio is 0.63. Since this ratio is less than 1, the sample has a high degree of ordering and is highly graphitic. -1 The peak near (the 2D band) is an overtone of the D band, which is also characteristic of graphite, specifically the graphitic ordering of free carbon along the free axis. The ability to fit this peak to a single Lorentzian peak indicates the presence of high quality graphene in the sample. Also, the size of this peak relative to the G peak is a good measure of the number of graphene layers present in the sample. I 2D / I G The ratio of 0.71 suggests the presence of few layers of graphene in the sample. The sheet resistance of the graphene composite is 0.25 Ω cm.

[0059] Example 9: Material properties of graphene / carbon fiber composites obtained from photothermal pyrolysis of exemplary precursors (carbon fiber and polyaniline) Pure carbon fibers consist of graphite and have an absorption spectrum that overlaps well with the emission spectrum of a xenon flash lamp. It has a fairly short radiation decay length. Therefore, it can be exfoliated into graphene layers by irradiating it with a high-intensity flash lamp. The surface morphology of the graphene / carbon fiber composites thus obtained was investigated by scanning electron microscopy. Figures 22A and 22B show SEM images of a pure carbon fiber that has not been pyrolyzed (A) and a carbon fiber that has been photothermally pyrolyzed (B). Figure 23A shows the FTIR spectrum of a pure carbon fiber. The absence of structure in the spectrum of the pure carbon fiber cloth confirmed that the precursor material consisted only of pure carbon. Raman spectroscopy was used to investigate the phase order and phase transformation of the carbon fibers upon photothermal pyrolysis.

[0060] FIG. 23B shows Raman spectra of pure carbon fiber fabric and photothermally pyrolyzed pure carbon fiber fabric as a function of the pulse output of a xenon flash lamp. The photothermal treatment was carried out under the following conditions (1) to (3). (1) 540 to 640 V: 106 J / cm 2 5.3 J / cm per pulse, corresponding to a total areal energy density of 2 (0.5 Hz, 800 μs pulse length, and 540 V voltage) with an areal energy density of 170 J / cm 2 8.5 J / cm per pulse, corresponding to a total areal energy density of 2 (2) 20 pulses (1.0 Hz, 800 μs pulse length, and 640 V voltage) with an areal energy density of 106 J / cm 2 5.3 J / cm per pulse, corresponding to a total areal energy density of 2 (0.5 Hz, 800 μs pulse length, and 540 V voltage) with an areal energy density of 164 J / cm 2 8.2 J / cm per pulse, corresponding to a total areal energy density of 2 (3) 20 pulses (1.0 Hz, 800 μs pulse length, and 620 V voltage) with an areal energy density of 106 J / cm 2 5.3 J / cm per pulse, corresponding to a total areal energy density of 2(0.5Hz, 800μs pulse length, and 540V voltage) with an areal energy density of 158J / cm 2 7.9 J / cm per pulse, corresponding to a total areal energy density of 2 20 pulses (1.0 Hz, 800 μs pulse length, and 600 V voltage) with an areal energy density of 1582 cm -1 (graphite, G band) and 1350 cm -1 (disorder, D band) and the characteristic graphite band around 2650 cm -1 Considering the presence of the 2D band near I, the formation of high-quality graphene from the photothermal pyrolysis of pure carbon fibers is confirmed. D / I G The ratio of I to I of the photothermal pyrolyzed samples at 540–620 V is less than 1, indicating a high structural order in the graphene samples. D / I G The ratio is 2.02. This treatment uses 106 J / cm 2 5.3 J / cm per pulse, corresponding to a total areal energy density of 2 (0.5Hz repetition rate, 800μs pulse length, and 540V voltage) with an areal energy density of 164J / cm 2 8.2 J / cm per pulse, corresponding to a total areal energy density of 2This was done by irradiating the samples with 20 pulses (1.0 Hz, 800 μs pulse length, and 620 V voltage) of areal energy density of 1.0 Hz. Furthermore, the 2D peak in the photothermally pyrolyzed samples could be fitted to a single Lorentzian peak, indicating the presence of high-quality graphene in these samples. Also, the size of this peak relative to the G peak is a good measure of the number of graphene layers present in the samples. The ratio of the 2D peak to the G peak of 0.62 indicates the presence of few layers of graphene in these photothermally pyrolyzed samples. In contrast, the pure samples that were not pyrolyzed lack a 2D peak and rather have broad, ill-defined D and G peaks, suggesting the absence of graphene in the samples and the lack of structural order. The sheet resistance of the samples photothermally pyrolyzed at 540–620 V was 0.02 Ω·cm, indicating that this composite has good electrical conductivity.

[0061] Polyaniline has an absorbance spectrum in the 500 nm-700 nm region that matches well with the emission spectrum of a xenon flash lamp. This enabled the photothermal conversion of PANI to graphene. Figure 31A shows optical images of PANI and derived graphene. The green color of the precursor film was indicative of the emeraldine morphology of PANI, while the gray color of the photothermally treated film was indicative of the conversion of PANI to carbonaceous material. The conversion of PANI to carbon was confirmed by TGA, as no mass loss was observed as shown in Figure 31B.

[0062] The quality of the carbon was investigated using Raman spectroscopy. The presence of D, G and 2D bands as shown in FIG. 31C is representative of a graphitic structure as described above. 2The ratio of D band to G band at an input energy of 1000 Å is about 0.35, which indicates the presence of graphite with fewer defects in its structure. The 2D band indicates the ordering of graphite along the free axis. In the case of PANI-derived graphene, the presence of 2D band, together with the ratio of 2D band to G band less than 1, indicates the formation of few-layer graphene like polybenzoxazine-derived graphene. Interestingly, conventionally carbonized PANI at 1000°C shows diffuse D and G bands representative of amorphous carbon. Therefore, it can be said that the temperature accessed during the millisecond photothermal treatment was higher than 1000°C, resulting in the formation of high-quality graphene. Morphological investigation of the obtained graphene was carried out using SEM. The electrochemically deposited PANI exhibited a rod-like morphology as shown in Figure 32A. The photothermal treatment of PANI led to the formation of a porous network of graphene (Figure 32B). This macroporous morphology is highly beneficial for the transport of electrolytes allowing the access of the bulk material. The fibrous structure of graphene also enhances the interaction between the electrode and the electrolyte, which leads to superior electrochemical performance. XPS was performed to determine the chemical composition of PANI-derived graphene. As shown in Figure 32C, the asymmetric peak centered at 284.5 eV indicates sp 2 The presence of hybrid graphitic carbon is confirmed. Furthermore, the percentages of carbon and oxygen atoms are estimated to be 98% and 2%, respectively, suggesting that graphene is composed mostly of carbon, even if the processing was carried out in air.

[0063] Example 10: Application in electrochemical energy storage Electrochemical energy applications of graphene / carbon fiber composites obtained via photothermal pyrolysis of exemplary precursor materials of polybenzoxazine were demonstrated on the above samples coated with MnO2. MnO2 is an attractive candidate for supercapacitor electrodes due to its abundant abundance, low cost, high electrochemical performance, and environmental inertness. Unfortunately, its low electrical conductivity leads to poor cyclability and low rate capability of electrochemical energy storage devices prepared with it. Combining MnO2 with carbonaceous materials such as graphene is a viable strategy to overcome the above-mentioned limitations. However, the production of high-quality graphene in a scalable manner entails many challenges. Various aspects of the present invention overcome these challenges and can produce high-quality graphene in a scalable manner in milliseconds at ambient conditions.

[0064] The processing scheme for depositing MnO2pm-graphene composites involves first UV-ozone treatment of both sides of the graphene composite formed on the carbon fiber substrate for 5 min to oxidize the surface, thereby increasing its hydrophilicity. Then, MnO2 is deposited on the graphene composite using a three-electrode configuration, where the graphene on carbon fiber is used as the working electrode, and Pt wire and Ag / AgCl are used as the counter and reference electrodes, respectively. MnO2 is deposited on the graphene composite by immersing the three electrodes in an electrolyte containing an aqueous solution of 50 mM manganese II acetate and 100 mM sodium sulfate, and performing cyclic voltammetry measurements in the potential range of 0-1.4 V at a scan rate of 50 mV / s. To investigate the effect of the amount of MnO2 on the electrochemical performance, the number of deposition cycles is varied between 5 and 15 cycles. Following MnO2 deposition, the electrode surface is thoroughly washed using DI water and then dried in a vacuum oven at 100 °C for 2 h. Calculate the mass of the deposited MnO2 using a weighing balance with a precision of 0.01 mg.

[0065] Figure 24A, Figure 24B, and Figure 24C show SEM images of MnO2 deposited on graphene composites at various magnifications. Figure 24A confirms conformal deposition of MnO2 on graphene composites, and Figure 24C shows the flower-like structure of the deposited MnO2. This flower-like structure enhances the interaction of electrolyte with MnO2 due to its high surface area. Also, the macropores in the composites provide an easy path for the transport of electrolyte to the bulk of the material, thus making these MnO2 / graphene composites promising candidates for electrochemical energy storage applications. The deposited MnO2 structure was further investigated using Raman, XRD, and XPS, as shown in Figure 24D-F. The Raman spectrum shown in Figure 24D shows the characteristic peaks of Mn-O lattice, along with the graphene peaks at 570 and 650 cm. -1 The XRD peak at 36.9° confirmed the formation of partially crystallized alpha MnO resulting from electrochemical deposition. Elemental analysis performed using XPS is shown in FIG. 24F and shows Mn (Mn 2p , Mn 2s , Mn 3s ), O 1s and C 1s This indicates the presence of MnO2, confirming the successful deposition of MnO2.

[0066] All electrochemical characterization and electrochemical performance testing of the graphene composites derived from the photothermal pyrolysis of the exemplary precursors of polybenzoxazine were performed using a CHI660E electrochemical workstation (CH instruments, Austin, TX) at ambient conditions. Cyclic voltammetry, charge-discharge testing, and electrochemical impedance spectroscopy were performed using a three-electrode system. Here, the photothermally generated graphene composites coated with MnO2 were used as the working electrode, a Pt wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode. These measurements were performed in an electrolyte containing an aqueous solution of 0.5 M Na2SO4. The performance of a symmetric device using MnO2-deposited graphene on both electrodes, along with a separator made of cellulose filter paper presoaked in 0.5 M Na2SO4, was also investigated.

[0067] The high porosity, high electrical conductivity of graphene, together with the lack of binders in the graphene composites, make the latter an ideal supercapacitor electrode. Thus, photothermally produced graphene on MnO2-coated carbon fiber cloth was evaluated as a supercapacitor electrode using cyclic voltammetry (CV) and galvanostatic charge-discharge (GCD) studies. CV was performed in the potential range of 0-1.0 V using 0.5 M aqueous Na2SO4 solution. Graphene photothermally derived from the exemplary precursor of polybenzoxazine as well as bare graphitic carbon fibers exhibited pseudo-rectangular CV curves at 50 mV / s (Figures 25A-D), indicating EDLC behavior. The capacitance obtained from the area under the CV curves was 3.6 mF / cm for graphene produced with high-power and low-power pulses, respectively. 2 and 1.5 mF / cm 2The superior performance of the high-power pulse treated samples compared to the low-power ones can be attributed to the higher porosity, higher degree of graphitization along with the superior conductivity, all of which promoted the adsorption of ions on its surface and facilitated the charge transport. Thus, all other electrochemical analyses were performed on the graphene prepared using high-power pulses. CVs at various scan rates were performed to determine the charge transfer capability of the graphene. The charge transfer capability retained a pseudo-rectangular shape up to 2 V / s, indicating excellent charge propagation through the bulk of the material. This was further verified using GCD, where the samples maintained an isosceles triangular charge-discharge profile even at very high current densities. Also, even after increasing the current density by 8 times, the capacitance value only decreased by 9%, thus demonstrating the good rate capability of the graphene-based supercapacitor. 3.6 mF / cm 2 The obtained areal capacitance of is one of the highest values ​​reported for a graphene-based micro-supercapacitor. Collectively, these results demonstrate the potential utility of photothermally generated graphene for carbon fiber woven EDLC-type micro-supercapacitor applications.

[0068] 26A-C show electrochemical performance test results obtained at various scan rates for symmetric devices prepared using MnO2 deposited on graphene composites derived from photothermal pyrolysis of an exemplary precursor of polybenzoxazine (FIG. 26A), as well as the GCD profiles of the devices at different current densities (FIG. 26B), and the capacity (F / g) as a function of current density (FIG. 26C).

[0069] Figure 27A shows the Ragone plot of a symmetric device prepared using MnO2 deposited on a graphene composite obtained from photothermal pyrolysis of an exemplary precursor of polybenzoxazine. Figure 27B shows a demonstration of three supercapacitor devices connected in series and lighting an LED. The supercapacitors were fabricated using electrodes prepared using MnO2 deposited on a graphene composite derived from photothermal pyrolysis of an exemplary precursor of polybenzoxazine.

[0070] The electrochemical performance of the photothermally derived graphene from PANI was determined considering its macroporosity, high conductivity, and fibrous structure. Cyclic voltammetry (CV) and galvanostatic charge-discharge (GCD) tests similar to those employed for the exemplary polybenzoxazine-derived graphene were carried out using a three-electrode system. Graphene from PANI on CF was used as the working electrode, Pt as the counter electrode, and Ag / AgCl as the reference electrode. Electrochemical measurements were carried out in an aqueous salt solution of 0.5 M Na2SO4 (sodium sulfate) and in 1 M H2SO4 (sulfuric acid) electrolyte. CVs of both CF and PANI-derived graphene on CF were performed in the potential range of 0-0.8 V at 50 mV / s. Both exhibited a pseudo-rectangular shape indicating an ideal EDLC-type behavior (Figure 33A). The capacitance obtained from the area under the curve was 22.4 mF / cm for PANI-derived graphene and CF, respectively. 2 and 1.5 mF / cm 2 The capacitance of PANI-derived graphene was superior to that of polybenzoxazine-derived graphene. The superior performance of PANI-derived graphene is mainly due to its high porosity, fibrous structure, and excellent electrical conductivity, which facilitate the adsorption and transport of ions across the bulk of the material. Interestingly, the capacitance of PANI-derived graphene was 100 mF / cm at 10 mV / s when the capacitance was evaluated in acidic electrolyte (1 M H2SO4). 2 (Figure 33B). The large increase in capacitance in acidic electrolyte may have arisen from the pseudocapacitive effect of oxygen functional groups present in graphene. To substantiate the findings from cyclic voltammetry, GCD was also performed in the potential range of 0–0.8 V at various current densities, as shown in Figure 33C. The sample maintained its isosceles triangular shape even at a very high current density of 40 mA. For this sample, the capacitance was 185 mF / cm at 5 mA. 2A capacitance of 1000 nm was obtained, which is one of the highest capacitance values ​​reported for a graphene-based supercapacitor. Moreover, the device retained more than 60% of its capacity at a current density of 40 mA, suggesting good interfacial contact between graphene and CF, excellent electrical conductivity, and easy access to the bulk of the material. These findings indicate that controlling the morphology can significantly improve the performance of the devices as demonstrated, which is an area that has not been explored previously.

[0071] An exemplary application of photothermally produced graphene from polyaniline on carbon fibers is an eyeglass side arm that can store electrochemical energy and be used for laser projection applications. The very high energy storage capacity and mechanical stability enabled by the carbon fiber / graphene composite gives great advantages for custom applications. Figure 34 shows a schematic image of the frame of an eyeglass side arm with the proposed dimensions. Fabrication of the device involves generating a large area graphene membrane over an area as large as 15 cm x 15 cm, appropriately laser cutting the graphene membrane, and assembling the membrane in a series or parallel configuration with a solid electrolyte between the positive and negative plates of each cell to achieve the desired energy output.

[0072] (Example 11) Application in electromagnetic interference shielding Graphene / carbon fiber composites derived from photothermal pyrolysis of an exemplary precursor material, polybenzoxazine, were evaluated for electromagnetic interference (EMI) shielding applications.

[0073] Electromagnetic parameter characterization and EMI shielding performance testing of graphene composites derived from photothermal pyrolysis of an exemplary precursor, polybenzoxazine. EMI shielding effectiveness measurements of graphene / carbon fiber composites were performed according to ASTM D4935-99 using an Agilent Technologies Vector Network Analyzer (VNA) Series E5061B. Samples were cut to fit the required shape and dimensions of the analyzer sample holder. Thickness measurements were performed using a digital micrometer.

[0074] The sample density was calculated from the experimental measurements of volume and mass. The material parameters of the composites (permittivity, conductivity, and permeability) were extracted from the EMI shielding measurements of the composites across the three investigated frequency bands, i.e., C-band, X-band, and Ku-band, covering the frequency range from 5 GHz to 18 GHz.

[0075] The measurement of the electromagnetic properties of the composites involved a four-step process. After loading the sample into the sample holder, calibration of the experimental apparatus setup, including the VNA and the waveguide, was performed, and then the scattering parameters of the sample were measured. The experimentally measured scattering parameters were then modeled and simulated. By fitting the model to the measured S-parameters, the permittivity (ε), permeability (μ), and conductivity (σ) of the composites were easily extracted.

[0076] FIG. 28A shows a photograph of an experimental setup for EMI shielding measurements, including a programmable network analyzer, a waveguide, and a sample holder assembly (top left), a photograph showing a close-up of the sample holder assembly according to various embodiments (bottom left), a photograph showing the proximity of the sample holder according to various embodiments (center), and a photograph showing a sample in the sample holder according to various embodiments (right). The setup includes an Agilent Technologies programmable VNA (Vector Network Analyzer) Series E5061B, its cables, and three different sets of waveguides (WR137, WR90, and WR62) with operating frequency ranges of 5-8 GHz, 8-12 GHz, and 12-18 GHz. Each of these setups was calibrated and used according to the Transmission-Reflection-Length (TRL) method. The sample holders were configured to enable EMI shielding measurements for each operating frequency band. The sample holders were designed to minimize the sensitivity of the measurements to variations in the size of the sample. Figure 28B shows a schematic diagram showing a front view of the sample placed in the sample holder (left) and a schematic diagram showing a side view of the sample arrangement in the sample holder (right). This setup was able to measure EMI shielding effectiveness up to 120 dB.

[0077] A sample of the composite was inserted into the center of a rectangular waveguide, and the complex reflection and transmission coefficients of the waveguide with and without the sample were measured using a VNA. The measurement results of the waveguide without the sample were used as a calibration to remove the effect of the coaxial to rectangular waveguide adapter. The effective material parameters of the composite (permittivity (ε), permeability (μ), and conductivity (σ)) were extracted by simulating the reflection and transmission of the waveguide with the sample, fitting the simulation results to the measurement results, and using the material parameters as fitting parameters. Measurements and simulations were performed for two different polarizations of the incident wave (i.e., TE and TM modes of the waveguide) for the sample with potential anisotropic parameters. The shielding properties (i.e., shielding effectiveness, absorption, and reflection) for different thicknesses of the composite were then calculated from the extracted material parameters. The material model of the composite was refined using the measured material parameters, and potential approaches to increase the shielding effectiveness were identified.

[0078] Figure 29 shows the EMI shielding performance of a 400 μm thick bi-layer graphene / carbon fiber composite. The results show that the graphene / carbon fiber composite provided an EMI shielding effectiveness of over 80 dB across multi-band, i.e., C-band, X-band, and Ku-band frequencies. Recognizing that decibels are logarithmic, an EMI shielding effectiveness of 80 dB indicates that more than 99.99999% of the incident radiation is attenuated by the composite.

[0079] Example 12: Application of various aspects of the present invention in printed flexible electronic devices Graphene derived from photothermal pyrolysis of exemplary precursor materials, cPAN and poly(BZ) coatings, screen-printed onto flexible polyimide films was evaluated for printed flexible electronic device applications.

[0080] Demonstration of graphene LED circuitry used in illuminating a white light LED device is shown in Figures 35A-C. Figure 35A shows screen printed traces of an exemplary precursor, cPAN, on a flexible polyimide substrate. Figure 35B shows graphene traces of the LED circuitry realized from photothermal pyrolysis of the screen printed cPAN precursor of Figure 35A. Figure 35C shows successful integration of a white light LED device onto the graphene traces and demonstration of actual illumination of the LED device driven by an external power source.

[0081] Example 13 Physical Properties and Device Performance Indicators The physical properties and device performance metrics of the graphene composites of the various embodiments of the present invention are summarized in Table 1. Compared to their conventionally processed counterparts, the graphene composites of the various embodiments of the present invention have D / I G The graphene composites produced by laser carbonization are of much higher quality as indicated by the ratio (<1.0), have much better properties in terms of their morphology as indicated by their much larger porosity, and have a lower sheet resistance (0.15 Ω·cm for carbon fiber / graphene composites). In contrast, graphene composites produced by laser carbonization have been reported to have sheet resistances of 21-33 Ω·cm, which is about 140-220 times greater than the sheet resistance of the various embodiments of the present invention. The polyimide / graphene composites of the various embodiments of the present invention have good electrical conductivity (150 S / m). The composites of the various embodiments of the present invention also have high areal capacitances (3 mF / cm) when used as micro-supercapacitor electrodes. 2 ) has improved performance compared to composites obtained by conventional pyrolysis, as demonstrated by a multi-band (C-band, X-band, and Ku-band) EMI shielding performance of over 80 dB.

[0082] [Table 1-1]

[0083] [Table 1-2]

[0084] Many graphene preparation methods have been reported in the literature. These methods can be broadly classified into top-down or bottom-up approaches. In the top-down approach, graphene is prepared by mechanical exfoliation, chemical exfoliation of graphite and graphite oxide, laser exfoliation of graphite, chemical reduction of graphene oxide, electrochemical reduction of graphene oxide, photothermal reduction of GO and photolysis of various precursors using flash lamps, as well as direct CO2 laser carbonization of polymer precursors that have absorption spectra that significantly overlap with the emission wavelengths of lasers in the short range of 9.4 μm to 10.6 μm that occur exclusively within the mid-infrared (IR) band. In the bottom-up approach, graphene is produced via solution-based chemical synthesis, via solvothermal synthesis, via chemical vapor deposition on various substrates such as metal catalysts (copper, ruthenium, nickel), via epitaxial growth on SiC, via laser-induced epitaxial growth, as well as via arc discharge.

[0085] Although flash lamps have been used in the past to prepare graphene, the precursors used in these preparation methods are different from the precursors of the various embodiments of the present invention. Furthermore, the low I obtained using the methods presented in the various embodiments of the present invention D / I G The quality of the graphene as shown by (see Table 1) is much better than that reported in the literature mentioned above. Also, there are clear differences in the way the radiation field is modulated and applied in the various embodiments of the present invention compared to that reported in the literature.

[0086] Of all the above methods for making graphene, direct CO2 laser carbonization based on laser flash photothermal pyrolysis is most closely related to the xenon flash lamp photothermal pyrolysis of the various embodiments of the present invention. Photonic processing using a xenon flash lamp source with an emission spectrum spanning the wavelength range of 200 nm to 1000 nm offers several advantages over CO2 lasers, namely reduced cost and complexity, improved efficiency in converting electrical energy to light, scalability to large area processing, and broadband illumination that overlaps the near ultraviolet (UV), visible, and near infrared (IR) regions of the electromagnetic spectrum, encompassing a much broader selection set of potential precursor materials with moieties that can undergo photothermal and photochemical transformations mediated by valence electronic transitions, molecular vibrations, phonons / lattice vibrations, and molecular rotations under flash photon pulse illumination. The energy of a single photon within the 300-400 nm wavelengths of the xenon flash lamp emission band, corresponding to 4.1 eV to 3.1 eV, is sufficient to directly cleave some of the bonds in the precursor polymer. The combination of photoinduced bond scission and induction of lattice vibrations in the precursor polymer ultimately leads to efficient photothermal pyrolysis, carbonization, and graphitization.

[0087] In contrast, the emission of CO2 lasers used in the carbonization of polymer precursors has an emission spectrum with wavelengths in a fairly short band of 9.4 μm to 10.6 μm, occurring exclusively within the mid-infrared (IR) band. This limits the suitable materials pool to materials that are active only in the mid-infrared (IR) range and therefore only capable of undergoing photothermal conversion mediated by molecular and phonon / lattice vibrations. The energy of a single photon within the 9.4 μm to 10.6 μm emission wavelength band of the CO2 laser, corresponding to 0.12 eV to 0.13 eV, is insufficient to directly cleave any bonds in the precursor polymer. Thus, the CO2 laser radiation induces phonons in the precursor polymer, resulting in bond dissociation, photothermal pyrolysis, carbonization, and graphitization.

[0088] A good illustration of the above-mentioned fine distinction between the photothermal and photochemical basis of xenon flash lamp photothermal pyrolysis and laser photothermal pyrolysis is illustrated in the absorption spectrum of Kapton. Kapton is a polyimide substrate commonly used for printed electronics and flexible circuit boards due to its excellent properties, i.e., high oxidative stability, high mechanical strength, high modulus of elasticity, excellent electrical and optical properties, and excellent chemical resistance. Kapton exhibits a broad UV absorption band in the UV region from 180 to 400 nm (Figure 30), which allows for effective absorption of all common excimer and exciplex laser wavelengths, including 193, 248, 308, and 351 nm, thus enabling its use in ablation studies and applications. Polyimide is not the only organic polymer with this type of absorption properties. In fact, organic polymers strongly absorb ultraviolet light, allowing efficient ablation of these materials with excimer lasers.

[0089] It is generally believed that the mechanism of laser ablation is primarily photothermal, with minor photochemical features. Kapton can be fabricated using lasers with a wavelength of 40 mJ / cm in the near ultraviolet (UV) range, which does not form graphene. 2 However, when a high-intensity continuous wave or pulsed CO2 laser is irradiated in the mid-infrared (IR) region at 9.4 μm and 10.6 μm, it is carbonized to graphene. However, under irradiation of a high-intensity xenon flash lamp on precursors such as cyclized polyacrylonitrile, the precursor is photothermally pyrolyzed to graphene, as shown in Figures 21A and 21B, because the absorption spectrum of the precursor has a peak overlapping with the emission spectrum of the xenon flash lamp in the near UV region, while Kapton is not affected at all.

[0090] Screen printed features of the precursor film in FIG. 21A and FIG. 21B show an I D / I G ratio and I of 0.71 2D / I GAs shown by the ratio, the precursor film is converted to high-quality few-layer graphene, while the open areas of the Kapton substrate that are not coated with the precursor film are not ablated or photothermally decomposed during the process, and are not turned into graphene. While there is a difference between the photothermal treatment with a high-intensity pulsed xenon flash lamp and the photothermal treatment with a high-intensity CO2 laser of the various embodiments of the present invention, there is also a difference between the photothermal treatment with a high-intensity pulsed xenon flash lamp and the photothermal treatment with an excimer laser of the various embodiments of the present invention. In other words, the photothermal treatment with a xenon flash lamp can convert a suitable precursor to high-quality graphene in the mid-ultraviolet (UV) band, while the excimer laser can only ablate the precursor film without converting it to graphene. Furthermore, CO2 laser photothermal processing can carbonize Kapton to graphene within the short wavelength band of 9.4 μm to 10.6 μm, but cannot do so outside of this narrow band of the electromagnetic spectrum, which limits its applicability to only a few precursor materials with reasonable absorption in the mid-infrared (IR) region of the spectrum. Xenon flash lamp photothermal processing, which utilizes a broad wavelength source spanning the near UV (ultraviolet), visible, and even near infrared (IR) regions of the spectrum, can carbonize a wider selection of absorbing precursors within the aforementioned bands to graphene than CO2 laser-based photothermal processing. Another drawback of CO2 laser-based photothermal processing is that the IR emission wavelength precludes its use in high resolution applications.

[0091] It should also be emphasized that photothermal graphitization of the appropriate precursor followed by coating of the precursor is an additive process where the substrate itself is not damaged and precursor and substrate can be independently selected. Independent selection of precursor offers advantages in tailoring the properties of the graphene material on any substrate. In contrast, CO2 laser graphitization of polymer films is subtractive, etching / damaging the substrate and does not allow independent selection of substrate and precursor since the substrate itself is converted to graphene.

[0092] The terms and expressions used are used as terms of description rather than limitation, and there is no intention in the use of such terms and expressions to exclude any equivalents of the features shown and described or portions thereof, and various modifications are possible within the scope of the aspects of the present invention. Thus, although the present invention has been specifically disclosed by certain embodiments and optional features, modifications and variations of the concepts disclosed herein may be employed by those skilled in the art, and such modifications and variations are also included within the scope of the aspects of the present invention.

[0093] (Exemplary embodiment) The following exemplary aspects are provided, it being noted that the numbering of the exemplary aspects should not be construed as indicating a level of importance.

[0094] Aspect 1 is a method for forming a graphene film, comprising: coating a polymeric graphene precursor onto a substrate; irradiating the polymeric graphene precursor coated on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than one second to convert the polymeric graphene precursor into the graphene film.

[0095] Example 2 provides the method of example 1, wherein the graphene film is a graphene composite film. Example 3 provides the method of example 1 or 2, wherein the graphene film is a non-graphene composite film.

[0096] Example 4 provides the method of any one of Examples 1-3, wherein the polymeric graphene precursor and the substrate have different chemical compositions. Example 5 provides the method of any one of Examples 1-4, wherein the irradiating comprises irradiating the polymeric graphene precursor and the substrate.

[0097] Example 6 provides the method of any one of Examples 1-5, wherein irradiating the polymeric graphene precursor and the substrate does not transform the substrate into a material comprising graphene.

[0098] Aspect 7 provides the method of any one of aspects 1 to 6, wherein the light source comprises an emission wavelength in the range of 100 nm to 2000 nm. Example 8 provides the method of any one of Examples 1 to 7, wherein the light source comprises an emission wavelength in the range of 300 nm to 800 nm.

[0099] Aspect 9 provides the method of any one of aspects 1 to 8, wherein the light source comprises an emission wavelength in the range of 400 nm to 600 nm. Example 10 provides the method of any one of Examples 1-9, wherein the pulse duration is shorter than a thermal equilibration time of the polymeric graphene precursor.

[0100] Example 11 provides a method according to any one of Examples 1 to 10, wherein the pulse duration is between 1 and 999 milliseconds. Example 12 provides a method according to any one of Examples 1 to 11, wherein the pulse duration is between 200 and 900 milliseconds.

[0101] Example 13 provides the method of any one of Examples 1 to 12, wherein the pulse duration is 400 to 800 milliseconds. Example 14 provides the method of any one of Examples 1 to 13, wherein the light source has an intensity of 100V to 2000V.

[0102] Example 15 provides the method of any one of Examples 1 to 14, wherein the light source has an intensity of 400V to 700V. Example 16 provides the method of any one of Examples 1 to 15, wherein the light source has a pulse frequency of 0.001 Hz to 1000 Hz.

[0103] Example 17 provides the method of any one of Examples 1 to 16, wherein the light source has a pulse frequency of 0.1 Hz to 10 Hz. Example 18 provides the method of any one of Examples 1 to 17, wherein the light source has a pulse frequency of 0.5 Hz to 1 Hz.

[0104] Aspect 19 is a method for producing an optical fiber having an irradiance of 0.1 J / cm 2 ~100J / cm 2 The method of any one of aspects 1-18 is provided, wherein the energy density per pulse is Aspect 20 is a method for producing an optical fiber having an irradiance of 1 J / cm 2 ~10J / cm 2 The method of any one of aspects 1-19 is provided, wherein the energy density per pulse is

[0105] Aspect 21 is a method for producing an optical fiber having an irradiance of 2 J / cm 2 ~9J / cm 2 The method of any one of aspects 1 to 20 is provided, wherein the energy density per pulse is Aspect 22 is a method for producing an optical fiber having an irradiance of 30 J / cm 2 ~200J / cm 2 The method of any one of embodiments 1-21 is provided, wherein the total areal density is

[0106] Example 23 provides the method of any one of Examples 1 to 22, wherein the irradiating comprises 5 to 1000 pulses of the light source. Example 24 provides the method of any one of Examples 1 to 23, wherein the irradiating comprises 10 to 40 pulses of the light source.

[0107] Example 25 provides the method of any one of Examples 1 to 24, wherein the irradiating pyrolyzes the polymeric graphene precursor. Example 26 provides the method of any one of Examples 1 to 25, wherein coating the polymeric graphene precursor on the substrate comprises using printing, offset printing, inkjet printing, transfer printing, aerosol jet printing, microcontact printing, embossing, nanoimprint lithography, optical lithography, electron beam lithography, ion beam lithography, or a combination thereof.

[0108] Example 27 provides the method of any one of Examples 1 to 26, wherein the polymeric graphene precursor on the substrate comprises a patterned polymeric graphene precursor.

[0109] Example 28 provides the method of Example 27, comprising subsequently depositing the polymer graphene precursor on the substrate, patterning the polymer graphene precursor film to form a patterned polymer graphene precursor film on the substrate.

[0110] Example 29 provides the method of any one of Examples 27-28, comprising depositing the patterned polymeric graphene precursor onto the substrate. Example 30 provides the method of any one of Examples 27-29, wherein coating the polymeric graphene precursor on the substrate comprises using printing, offset printing, inkjet printing, transfer printing, aerosol jet printing, microcontact printing, or a combination thereof to form the patterned polymeric graphene precursor coated on the substrate.

[0111] Example 31 provides the method of any one of Examples 27 to 30, wherein depositing the polymer graphene film on the substrate comprises using embossing, nanoimprint lithography, or a combination thereof to form the patterned polymer graphene precursor deposited on the substrate.

[0112] Example 32 provides the method of any one of Examples 27 to 31, wherein depositing the polymer graphene film on the substrate comprises forming the patterned polymer graphene precursor deposited on the substrate by using optical lithography, electron beam lithography, or ion beam lithography.

[0113] Example 33 provides the method of any one of Examples 1 to 32, wherein the polymeric graphene precursor comprises a polymer comprising a disubstituted benzene, a benzene substituted with one or more chromophores, a polycyclic aromatic ring, or a combination thereof.

[0114] Example 34 provides the method of any one of Examples 1 to 33, wherein the polymeric graphene precursor comprises a polymer comprising nitroaniline, aniline, nitrophenol, biphenyl, nitrobenzene, benzaldehyde, acetophenone, pyrene, pentacene, anthracene, tetracene, or a combination thereof.

[0115] Example 35 provides the method of any one of examples 1 to 34, wherein the polymeric graphene precursor comprises a polymer selected from resole, oligomers of pyrene pitch, cyclized polyacrylonitrile, carbon fiber, polyaniline, a thermoset network formed from blending and crosslinking polybenzoxazine with an epoxy, and combinations thereof.

[0116] Example 36 provides the method of any one of examples 1 to 35, wherein the polymeric graphene precursor comprises a polymer selected from poly(3-phenyl-2,4-dihydro-1,3-benzoxazine), poly(phenylbenzoxazine), poly(3-furanyl-2,4-dihydro-1,3-benzoxazine), poly(furanylbenzoxazine), poly(phenol-co-formaldehyde), resole, oligomers of pyrene pitch, cyclized polyacrylonitrile, pure carbon fiber, polyaniline, a thermoset network formed from blending and crosslinking polybenzoxazine with bis-phenol-A furfuryl diglycidyl ether, and combinations thereof.

[0117] Example 37 provides the method of any one of Examples 1 to 36, wherein an absorption band of the polymeric graphene precursor overlaps with an emission band of the pulsed light source. Example 38 provides the method of any one of Examples 1 to 37, wherein the polymeric graphene precursor has an absorption band in the range of 100 nm to 2000 nm.

[0118] Example 39 provides the method of any one of Examples 1 to 38, wherein the polymeric graphene precursor has an absorption band in the range of 300 nm to 800 nm. Example 40 provides the method of any one of Examples 1 to 39, wherein the polymeric graphene precursor has an absorption band in the range of 400 nm to 600 nm.

[0119] Example 41 provides the method of any one of Examples 1 to 40, wherein the substrate comprises a plastic, a metal, a fabric, a woven fabric, or a combination thereof. Example 42 provides the method of any one of Examples 1 to 41, wherein the substrate comprises carbon.

[0120] Example 43 provides the method of example 42, wherein the substrate comprises carbon fiber. Example 44 provides the method of example 42 or 43, wherein the substrate comprises a carbon mesh.

[0121] Example 45 provides the method of any one of Examples 42-44, wherein the substrate comprises carbon cloth. Example 46 provides the method of any one of Examples 42-45, wherein the substrate comprises a carbon composite.

[0122] Example 47 provides the method of any one of Examples 42-46, wherein the substrate comprises a graphene composite. Example 48 provides the method of any one of Examples 42-47, wherein the substrate comprises graphene.

[0123] Example 49 provides the method of any one of Examples 42-48, wherein the substrate comprises a carbon film. Example 50 provides the method of any one of Examples 1 to 49, wherein the light source comprises a xenon flash lamp.

[0124] Example 51 provides the method of any one of Examples 1 to 50, wherein the light source comprises a halogen flash lamp. Example 52 provides the method of any one of Examples 1 to 51, wherein the light source comprises a light emitting diode.

[0125] Example 53 provides the method of any one of Examples 1 to 52, wherein the light source comprises one or more light emitting diodes. Example 54 provides the method of any one of Examples 1 to 53, wherein the irradiating comprises irradiating the polymeric graphene precursor coated on the substrate in air.

[0126] Example 55 provides the method of any one of Examples 1 to 54, wherein the irradiating comprises irradiating the polymeric graphene precursor at a temperature less than 100 °C. Example 56 provides the method of any one of Examples 1 to 55, wherein the irradiating comprises maintaining the polymeric graphene precursor at a temperature less than 100 °C.

[0127] Example 57 provides the method of any one of Examples 1 to 56, wherein the irradiating comprises irradiating the polymeric graphene precursor at room temperature. Example 58 provides the method of any one of Examples 1 to 57, wherein the irradiating comprises substantially maintaining the polymeric graphene precursor at a pre-irradiation temperature throughout the irradiation.

[0128] Example 59 provides the method of any one of Examples 1 to 58, wherein the irradiating comprises increasing the temperature of the polymeric graphene precursor by 10 °C or less. Example 60 provides the method of any one of Examples 1 to 59, wherein the irradiating comprises increasing a temperature of the polymeric graphene precursor by 2° C. or less.

[0129] Example 61 provides the method of any one of Examples 1 to 60, wherein the graphene film has a conductivity of at least 150 S / m. In a sixth aspect, the graphene film has a refractive index of 1,350 cm as determined by Raman spectroscopy. -1 A characteristic disorder band (D band) with a peak near 1582 cm -1 The method of any one of the preceding aspects, wherein the ratio of the characteristic graphitic band (G band) having a peak near the

[0130] In a sixth aspect, the graphene film has a refractive index of 2700 cm as determined by Raman spectroscopy. -1 A characteristic 2D band with a peak near 1582 cm that can be fitted to a single Lorentzian function -1 The method of any one of the preceding aspects, wherein the ratio of the characteristic graphitic band (G band) having a peak near the

[0131] Example 64 provides the method of any one of Examples 1 to 63, wherein the irradiating includes localizing light absorption to the precursor film such that a temperature of the polymeric graphene precursor increases by 10° C. or less during the irradiation relative to a pre-irradiation temperature of the precursor film.

[0132] Example 65 provides the method of any one of Examples 1-64, wherein the method leaves the substrate undamaged relative to its state prior to the coating and irradiation. Example 66 provides the method of any one of Examples 1 to 65, wherein the irradiating comprises pulsed power modulation.

[0133] Example 67 provides the method of example 66, comprising tailoring a microstructure of the graphene film using the pulsed power modulation. Example 68 provides a graphene film formed by the method of any one of Examples 1-67.

[0134] Example 69 provides a patterned graphene film produced by the method of any one of Examples 1 to 67. Example 70 provides an electrochemical energy storage device, an electromagnetic shielding material, a chemical or biological sensor, a post-CMOS nanoelectronic device, a thermal shielding material, a structural composite, a filter, or a combination thereof, comprising a graphene film formed by the method of any one of examples 1 to 67.

[0135] Example 71 is a method for forming a graphene film, comprising: coating a polymeric graphene precursor onto a substrate comprising carbon fiber, carbon mesh, carbon cloth, carbon composite, graphene composite, graphene, carbon film, or a combination thereof, wherein the polymeric graphene precursor and the substrate have different chemical compositions; and irradiating the polymeric graphene precursor coated on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than one second to convert the polymeric graphene precursor into the graphene film.

[0136] Example 71 provides a graphene film, an electrochemical energy storage device, an electromagnetic shield, a chemical or biological sensor, a post-CMOS nanoelectronic device, a thermal shield, a structural composite, a filter, or any combination of Examples 1-70, optionally configured such that all recited elements or options are available for use or selection.

Claims

1. 1. A method of forming a graphene film, comprising: coating a polymeric graphene precursor onto a substrate; irradiating the polymeric graphene precursor coated on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than one second to convert the polymeric graphene precursor into the graphene film.

2. 10. The method of claim 1 , wherein a composition of the polymeric graphene precursor is different from a composition of the substrate.

3. The method of claim 1 , wherein the light source comprises an emission wavelength in the range of 100 nm to 2000 nm.

4. 2. The method of claim 1, wherein the pulse duration is 200-900 milliseconds, the light source has an intensity of 100 V-2000 V, the light source has a pulse frequency of 0.1 Hz-10 Hz, the light source has an energy density per pulse of 0.1 J / cm2-100 J / cm2, and the light source has a total areal density of 10 J / cm2-1000 J / cm2.

5. 10. The method of claim 1, wherein coating the polymeric graphene precursor on the substrate comprises using printing, offset printing, inkjet printing, transfer printing, aerosol jet printing, microcontact printing, embossing, nanoimprint lithography, optical lithography, electron beam lithography, ion beam lithography, or a combination thereof.

6. 10. The method of claim 1 , wherein the polymeric graphene precursor on the substrate comprises a patterned polymeric graphene precursor.

7. 10. The method of claim 1, wherein the polymeric graphene precursor comprises a polymer comprising disubstituted benzene, benzene substituted with one or more chromophores, polycyclic aromatic rings, aniline, nitroaniline, nitrophenol, biphenyl, nitrobenzene, benzaldehyde, acetophenone, pyrene, pentacene, anthracene, tetracene, or combinations thereof.

8. 2. The method of claim 1, wherein the polymeric graphene precursor comprises a polymer selected from resole, oligomers of pyrene pitch, cyclized polyacrylonitrile, carbon fiber, polyaniline, a thermoset network formed from blending and crosslinking polybenzoxazine with epoxy, poly(3-phenyl-2,4-dihydro-1,3-benzoxazine), poly(phenylbenzoxazine), poly(3-furanyl-2,4-dihydro-1,3-benzoxazine), poly(furanylbenzoxazine), poly(phenol-co-formaldehyde), resole, oligomers of pyrene pitch, a thermoset network formed from blending and crosslinking polybenzoxazine with bis-phenol-A furfuryl diglycidyl ether, and combinations thereof.

9. 2. The method of claim 1, wherein an absorption band of the polymer graphene precursor overlaps with an emission band of the pulsed light source, and the polymer graphene precursor has an absorption band in the range of 400 nm to 600 nm.

10. The method of claim 1 , wherein the substrate comprises a plastic, a metal, a fabric, a woven material, or a combination thereof.

11. The method of claim 1 , wherein the substrate comprises carbon fiber, carbon mesh, carbon cloth, carbon composite, graphene composite, graphene, carbon film, or combinations thereof.

12. The method of claim 1 , wherein the light source comprises a xenon flash lamp.

13. 10. The method of claim 1, wherein the irradiating comprises irradiating the polymeric graphene precursor coated on the substrate in air at room temperature.

14. 2. The method of claim 1, wherein said irradiating comprises irradiating and / or maintaining the polymeric graphene precursor at a temperature less than 100° C.

15. 10. The method of claim 1, wherein the polymeric graphene precursor comprises polyaniline.

16. 10. The method of claim 1, wherein the graphene film has a conductivity of at least 150 S / m.

17. The graphene film is 1350 cm as determined by Raman spectroscopy -1 A characteristic disorder band (D band) with a peak near 1582 cm -1 the ratio of the characteristic graphite band (G band) having a peak in the vicinity to that of the characteristic graphite band (G band) is less than 1; 2700 cm as determined by Raman spectroscopy -1 A characteristic 2D band with a peak near 1582 cm that can be fitted to a single Lorentzian function -1 The ratio of the characteristic graphite band (G band) having a peak near the The method of claim 1 having a combination thereof.

18. 1. A method of forming a graphene film, comprising: coating a polymeric graphene precursor onto a substrate comprising carbon fiber, carbon mesh, carbon cloth, carbon composite, graphene composite, graphene, carbon film, or a combination thereof, wherein the polymeric graphene precursor and the substrate have different chemical compositions; and irradiating the polymeric graphene precursor coated on the substrate with a pulsed high intensity light source emitting at two or more wavelengths for a pulse duration of less than one second to convert the polymeric graphene precursor into the graphene film.

19. 13. A graphene film formed by the method of claim 1.

20. 13. An electrochemical energy storage device, an electromagnetic shield, a chemical or biological sensor, a post-CMOS nanoelectronic device, a thermal shield, a structural composite, a filter, or a combination thereof, comprising a graphene film formed by the method of claim 1.

Citation Information

Patent Citations

  • Method of producing graphene from organic material using radiation and graphene produced thereby

    JP2013193953A

  • Nanoporous structures and assemblies incorporating same - Patent Application 20070122997

    JP2019534833A

  • A facile route to highly conductive porous graphene from carbon nanodots for supercapacitor applications

    JP2020527853A

  • Cooling device for air cooling type internal engine

    KR100229596B1