Silver plating solution
The electroless silver plating solution using silver carboxylate and a reducing agent addresses the limitations of cyanide-based processes by providing a stable, environmentally friendly, and high-quality silver plating suitable for diverse substrates, enhancing scalability and safety.
Patent Information
- Application Number
- JP2024547398
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-19
- Filing Date
- 2022-11-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Existing silver plating processes, particularly those using cyanide compounds, face challenges in achieving high-quality, cost-effective, and environmentally friendly plating solutions due to issues such as adhesion problems, contamination, and environmental hazards associated with cyanide waste, as well as limitations in scalability and stability of alternative cyanide-free solutions.
An electroless silver plating solution comprising a silver complex solution and a reducing agent, utilizing silver carboxylate represented by formula R1-COOAg, which allows for a stable silver mirror reaction at neutral to slightly alkaline pH, enabling high-quality silver plating on various substrates without the need for toxic cyanide compounds.
The solution provides an environmentally friendly, stable, and high-quality silver plating process suitable for a wide range of substrates, with improved storage stability and safety, allowing for the production of high-quality silver-plated products.
Smart Images

Figure 2024538434000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a silver plating solution that can be used to produce high-quality silver-plated products in an environmentally friendly and simple manner, and to a silver-plated product produced using the silver plating solution. [Background technology]
[0002] Silver belongs to the precious metal category and has been used as a material for luxury ornaments, tableware, and coins since ancient times. In recent years, silver has been used in a wide variety of applications, such as electrodes in electronic devices such as mobile phones, batteries (including solar cells), automobiles, and semiconductors, electromagnetic shielding and heat dissipation products, and machine parts, due to its electrical, thermal, optical, and frictional properties that are far superior to other metals, as well as its high antibacterial activity. Silver is also widely applied as a catalyst for electrochemical reactions, as well as medical and antibacterial products. In addition, mirrors or high-reflective luxury metallic gloss products for general household use are also manufactured by painting, plating, or depositing with highly reflective metals such as silver, aluminum, chromium, nickel, titanium, and copper. Painting, coating, and printing are generally used to manufacture products that are not very conductive or reflective. Although plating can be used to obtain films with high conductivity and reflectivity, and even thin films with high quality surface gloss, it may increase the number of defects in the product, incur significant costs, and emit harmful substances, causing air pollution and wastewater problems. Vacuum deposition and sputtering are dry processes that allow the production of thin-film electrodes or highly reflective films. However, the deposition process requires the use of expensive vacuum equipment and has limitations on the shape or size of the substrate. In addition, the deposition process is suitable for small batch production, which creates problems in the production of products on a large scale. Thus, the plating process cannot be applied to the production of desired industrial electrical and electronic products or household products, and has many environmental problems, such as wastewater treatment problems, that need to be solved.
[0003] Silver plating is broadly divided into silver electroplating and electroless silver plating. Both silver plating processes have in common the use of silver precursors or complexes, but electroless silver plating is distinguished from silver electroplating in that it deposits silver using a reducing agent instead of electricity, facilitating plating of non-electrically conductive plastic, textile, and ceramic products. In particular, silver electroplating has long been carried out with alkaline cyanide solutions (e.g., potassium cyanide and sodium cyanide solutions) containing highly toxic silver cyanide. Much research and development has been carried out over the past decades to replace silver plating using cyanide compounds with cyanide-free silver plating using silver compounds such as silver nitrate and various complexing agents and other additives. However, cyanide-free silver plating has disadvantages in terms of adhesion, difficulty in producing shiny silver-plated products, and the disadvantage that the plating solution is easily contaminated, so silver plating using cyanide compounds is still used as the main process in the production of commercial products. As examples of cyanide-free silver plating, U.S. Patent No. 5,322,553 discloses the use of silver thiosulfate or silver sulfite to provide a more stable plating solution, U.S. Patent No. 6,620,304 mentions the possibility of producing high-quality products using plating solutions containing silver methanesulfonate and amino acids such as cysteine without the need for any harmful substances, and U.S. Patent No. 8,608,932 discloses a differentiated silver electroplating method using a silver complex of 5,5-dimethylhydantoin. However, a plating solution comparable in price and quality to cyanide-containing plating solutions has not yet been developed. From the perspective of environmental protection, the development of a silver plating solution free of cyanide compounds remains an ongoing challenge. A silver ammonium complex called Tollens' reagent is reduced to form a silver mirror when reacted with a compound having an aldehyde group such as glucose. This is a type of electroless silver plating that clearly shows an oxidation-reduction reaction and is used in the manufacture of thermoses or Dewar flasks. However, since this silver plating solution is produced from a strongly alkaline aqueous solution using silver nitrate and aqueous ammonia as a complexing agent, silver nitride is formed during storage, which poses the risk of explosion.For this reason, the silver plating solution should be used immediately after preparation, and after use, it should be subjected to acid treatment and then disposed of without storage. Although the plating solution using silver nitrate and ammonia water as a complexing agent is very excellent in stability and quality during silver electroplating or electroless silver plating, its use is extremely limited due to the above-mentioned problems. Therefore, the selection of an appropriate type of complexing agent and an appropriate reducing agent corresponding thereto is a very important factor for electroless silver plating.
[0004] Under these circumstances, the inventors have continued to make efforts to solve the problems encountered during silver plating, and have finally arrived at the present invention. Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide an environmentally friendly and highly stable silver plating solution and a high-quality silver-plated product produced using the silver plating solution. [Means for solving the problem]
[0006] According to one embodiment of the present invention, there is provided an electroless silver plating solution comprising a silver complex solution and a reducing agent solution, the silver complex solution comprising a silver carboxylate represented by Formula 1: [Formula 1] R1-COOAg In the formula, R1 is hydrogen or a substituted or unsubstituted C1-C 22 Alkyl, substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted C6-C 30 Aralkyl, substituted or unsubstituted C1-C 30 Heteroalkyl, substituted or unsubstituted C2-C 30 Heterocycloalkyl or substituted or unsubstituted C5-C 30 Heteroaralkyl, and electroless silver plating is based on the silver mirror reaction between the silver complex solution and the reducing agent solution.
[0007] According to another aspect of the present invention, there is provided a silver-plated product produced by reacting with the silver plating solution at 5 to 50°C. Effect of the Invention
[0008] The silver plating solution of the present invention is environmentally friendly and has excellent storage stability and performance. Due to these advantages, a variety of high-quality silver-plated products can be provided by using the silver plating solution of the present invention. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a photograph showing the silver mirror products produced in Examples 1-7. [Diagram 2] FIG. 2 is a photograph showing the glass bottle produced in Example 3 as a silver mirror product. [Diagram 3] FIG. 3 is a photograph showing the PET bottle produced in Example 8 as a silver mirror product. [Figure 4] FIG. 4 is a photograph of the silver-plated nylon fabric product produced in Example 41 and the electrical conductivity of the product. [Diagram 5] FIG. 5 is a photograph showing the silver-plated nylon fiber product produced in Example 42 and the electrical conductivity of the product. [Figure 6] FIG. 6 is a surface scanning electron microscope (SEM) image of the silver-plated nylon fiber product produced in Example 42. [Figure 7] FIG. 7 is a photograph showing the silver-plated mirror-like polyimide film produced in Example 43. [Figure 8] FIG. 8 is a photograph showing the silver-plated polyurethane foam produced in Example 45. [Figure 9] FIG. 9 is a surface scanning electron microscope (SEM) image of the silver-plated polyurethane foam produced in Example 45. [Figure 10] FIG. 10 is a photograph showing the silver-plated copper foil produced in Example 50. [Figure 11] FIG. 11 is a photograph showing the silver-containing antimicrobial cotton fabric produced in Example 51. [Figure 12] FIG. 12 is a photograph showing the state of the silver complex solution prepared in Preparation Example 2 after storage at room temperature for six months. [Figure 13] FIG. 13 is a photograph showing the state of the reducing agent solution prepared in Preparation Example 8 after storage at room temperature for 6 months. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] As used herein, the term "alkyl" includes straight-chain, branched, and cyclic hydrocarbon radicals and combinations thereof. The term can also include one or more double bonds, triple bonds, or combinations thereof within the chain, if desired. Thus, "alkyl" is intended to include alkenyl and alkynyl.
[0011] The term "heteroalkyl," by itself or in combination with another term, means, unless otherwise stated, a stable linear, branched, or cyclic hydrocarbon radical, or combination thereof, consisting of one or more carbon atoms and one or more heteroatoms selected from the group consisting of O, N, P, Si, and S, wherein the nitrogen, phosphorus, and sulfur atoms may optionally be oxidized, and the nitrogen heteroatom may optionally be quaternized.
[0012] The terms "cycloalkyl" and "heterocycloalkyl", by themselves or in combination with other terms, represent, unless otherwise stated, cyclic versions of "alkyl" and "heteroalkyl", respectively.
[0013] The term "aryl", unless otherwise specified, means a polyunsaturated aromatic hydrocarbon substituent which may be a single ring or multiple rings (1 to 3 rings) fused together or covalently linked.
[0014] The term "heteroaryl" refers to an aryl group (or ring) containing from 1 to 4 heteroatoms (in separate rings in the case of multiple rings) selected from N, O, and S, wherein the nitrogen and sulfur atoms are optionally oxidized and the nitrogen atom is optionally quaternized. The heteroaryl group may be attached to the remainder of the molecule through a carbon or heteroatom.
[0015] The term "aralkyl" refers to an alkyl group substituted with an aryl, where the alkyl and aryl portions independently are optionally substituted.
[0016] The term "heteroaralkyl" refers to an alkyl group substituted with a heteroaryl, where the alkyl and heteroaryl portions independently are optionally substituted.
[0017] The term "substituted" in the phrase "substituted or unsubstituted" as used herein means that one or more hydrogen atoms in the hydrocarbon are each independently replaced with the same or different substituents. Suitable substituents include, but are not limited to, -F; -Cl; -Br; -CN; -NO2; -OH; =O; C1-C unsubstituted or substituted with -F, -Cl, -Br, -CN, -NO2, -OH, or =O. 20 Alkyl; C1-C unsubstituted or substituted with -F, -Cl, -Br, -CN, -NO2, -OH, or =O 20 Alkoxy; unsubstituted or C1-C 20 Alkyl, C1-C 20 C6-C substituted with alkoxy, -F, -Cl, -Br, -CN, -NO2, -OH, or =O 30 Aryl; unsubstituted or C1-C 20 Alkyl, C1-C 20 C6-C substituted with alkoxy, -F, -Cl, -Br, -CN, -NO2, -OH, or =O 30 Heteroaryl; unsubstituted or C1-C 20 Alkyl, C1-C 20 C5-C substituted with alkoxy, -F, -Cl, -Br, -CN, -NO2, -OH, or =O20 Cycloalkyl; unsubstituted or C1-C 20 Alkyl, C1-C 20 C5-C substituted with alkoxy, -F, -Cl, -Br, -CN, -NO2, -OH, or =O 30 Heterocycloalkyl; C1-C unsubstituted or substituted with F, -Cl, -Br, -CN, -NO2, -OH, or =O 20 Alkoxysilane; and a group represented by -N(G1)(G2) (wherein G1 and G2 are each independently hydrogen, C1 to C 10 Alkyl, unsubstituted or C1-C 10 Alkyl-substituted C6-C 30 aryl).
[0018] The term "derivative" of a specific substance described herein means a compound prepared by replacing some of the hydrogen atoms in the specific substance with the above-mentioned substituents.
[0019] The present invention provides an electroless silver plating solution comprising a silver complex solution and a reducing agent solution, the silver complex solution comprising a silver carboxylate represented by Formula 1: [Formula 1] R1-COOAg In the formula, R1 is hydrogen or a substituted or unsubstituted C1-C 22 Alkyl, substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted C6-C 30 Aralkyl, substituted or unsubstituted C1-C 30 Heteroalkyl, substituted or unsubstituted C2-C 30 Heterocycloalkyl or substituted or unsubstituted C5-C 30 Heteroaralkyl, and electroless silver plating is based on the silver mirror reaction between the silver complex solution and the reducing agent solution.
[0020] Specifically, the silver plating solution of the present invention contains, as a main component, a silver carboxylate represented by the formula 1: [Formula 1] R1-COOAg In the formula, R1 is hydrogen or a substituted or unsubstituted C1-C 22 Alkyl, substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted C6-C 30 Aralkyl, substituted or unsubstituted C1-C 30 Heteroalkyl, substituted or unsubstituted C2-C 30 Heterocycloalkyl or substituted or unsubstituted C5-C 30 Includes silver carboxylates and nitrogen-containing complexing agents that are heteroaralkyl.
[0021] The present invention also provides various conductive products and silver mirror products manufactured using the silver plating solution.
[0022] R1 in Formula 1 can be, for example, hydrogen, methyl, ethyl, n-propyl, iso-propyl, n-butyl, iso-butyl, t-butyl, n-pentyl, iso-amyl, t-amyl, n-hexyl, 2-ethylhexyl, n-heptyl, octyl, iso-octyl, nonyl, decyl, neodecyl, dodecyl, tetradecyl, hexadecyl, octadecyl, docosanyl, oleyl, linoleyl, cyclopropyl, cyclopentyl, or cyclohexyl.
[0023] The silver carboxylate of formula 1 is a silver precursor, and specific examples thereof include silver acetate, silver propionate, silver trifluoroacetate, silver lactate, silver malonate, silver maleate, silver fumarate, silver pyruvate, silver succinate, silver picrate, silver citrate, silver 2-ethylhexanoate, silver neodecanoate, silver stearate, silver docosanoate, silver oleate, silver linoleate, and silver cyclohexanecarboxylate. From a comprehensive viewpoint including economic efficiency, stability, and solubility characteristics required in the present invention, silver acetate and silver alkanoates such as silver propionate and silver neodecanoate are most preferred.
[0024] The amount of silver used is not particularly limited as long as it does not impair the object of the present invention, and is typically 0.05 to 5.0% by weight, preferably 0.1 to 3.0% by weight, and more preferably 0.2 to 2.0% by weight, based on the weight of the final plating solution. If the amount of silver is less than the lower limit or exceeds the upper limit, the economic efficiency and stability of the plating solution may be deteriorated, or the quality of the final product may be deteriorated.
[0025] The complexing agent combines with the silver ions in the silver plating solution to form stable complex ions, which are easily dissolved in a solvent at high concentration. The complexing agent acts mainly as an electron donor. The complexing agent is preferably a compound containing at least one nitrogen, phosphorus, or sulfur atom. From the viewpoint of stability and economic efficiency, nitrogen-containing compounds are more preferred.
[0026] For example, the nitrogen-containing compound may be selected from the group consisting of ammonia, amines (including primary, secondary, and tertiary amines), quaternary ammonium salts, polyamines, and mixtures thereof. 20 An alkyl group, an aryl group, or an aralkyl group may be bonded to the nitrogen atom of the nitrogen-containing compound.
[0027] The alkyl group may be of any type, such as linear, branched, comb, star, dendritic, or cyclic, etc. The nitrogen-containing compound may have a functional group, such as a hydroxyl group, an alkoxy group, an ester group, an amide group, or a urethane group.
[0028] In one embodiment, the nitrogen-containing compound is ammonia, an amine compound represented by formula 2: [Formula 2] (R2R3R4)N In the formula, R2 to R4 are the same or different and each independently represents hydrogen or a substituted or unsubstituted C1 to C 20 Alkyl, substituted or unsubstituted C6-C 30 Aryl, substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted C6-C30 Aralkyl, substituted or unsubstituted C1-C 30 Heteroalkyl, substituted or unsubstituted C2-C 30 Heterocycloalkyl, substituted or unsubstituted C5-C 30 Heteroaryl or substituted or unsubstituted C5-C 30 a heteroaralkyl, amine compound or a quaternary ammonium salt compound represented by formula 3: [Formula 3] (R5R6R7R8)N + X wherein R5 to R8 are as defined for R2 to R4 in formula 2, and X is F - , Cl - , Br - , I - , O.H. - , hydrogen sulfate, hydrogen carbonate, carbamate, or perchlorate.
[0029] Specifically, the nitrogen-containing compound is ammonia, methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, tert-butylamine, n-pentylamine, iso-pentylamine, tert-amylamine, n-hexylamine, diethylamine, triethylamine, 2-ethylhexylamine, cyclohexylamine, allylamine, propargylamine, ethylenediamine, 1,3-propylenediamine, hexamethylenediamine, triethylenediamine, 1,2-diaminopropane, monoethanolamine, diethanolamine, 1-amino-2-propanol, 3-amino-1-propanol, 1,4-butanediamine, spermine, spermidine, diethylenetriamine, triethylenediamine, ... The amine may be selected from ammonium tetramine, tris(2-aminoethyl)amine, 1,1,1-tris(aminomethyl)ethane, N,N-diethylhydroxyamine, methoxyethylamine, N,N-diethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, pyridine, piperidine, piperazine, morpholine, imidazole, pyrrole, quinuclidine, benzylamine, phenethylamine, ammonium carbamate, ammonium carbonate, tetraethylammonium bicarbonate, tetraethylammonium bromide, tetrabutylammonium hydroxide, aminopropyltriethoxysilane, polyethyleneimine (PEI), poly(propyleneimine), polyvinylamine (PVAm), poly(amidoamine) (PAMAM), and derivatives thereof. In one embodiment, the plating solution may be an alkaline aqueous solution containing ethylenediaminetetraacetic acid (EDTA) or nitrilotriacetic acid (NTA) compounds, such as disodium EDTA, trisodium EDTA, tetrasodium EDTA, sodium NTA, or trisodium NTA, succinimide, maleimide, phthalimide, ethylenediamine, hexamethylenetetramine, saccharin, imidazole, oxazoline, hydantoin, 5,5-dimethylhydantoin, or mixtures thereof. The nitrogen-containing compound is most preferably ammonia or an alkylamine, such as methylamine or ethylamine, from the viewpoint of economic efficiency and properties required in the present invention.
[0030] The amount of the complexing agent used is not particularly limited as long as it does not impair the object of the present invention. The complexing agent is typically used in a molar ratio of 0.1 to 10.0, preferably 0.3 to 7.0, more preferably 0.5 to 5.0, to the silver carboxylate. If the amount of the complexing agent is less than the lower limit or exceeds the upper limit, the stability of the plating solution may be insufficient, or the reaction may not be completed, resulting in a deterioration in quality.
[0031] The silver plating solution of the present invention may use water, ethanol, ethylene glycol, glycerin, or a mixture thereof as a solvent. That is, the silver plating solution may be an aqueous solution containing alcohol or glycol, and may have very high wettability. Therefore, the silver plating solution can be used to easily plate various types of substrates, such as metals and metal alloys such as copper, nickel, zinc, tin, antimony, molybdenum, platinum, bronze, and brass, oxides and sulfides of these metals, ceramics such as silica, alumina, titanium oxide, mica, clay, and glass, plastics such as polyester, nylon, polyimide, polyurethane, and acrylic, various carbon compounds such as carbon, carbon nanotubes, graphite, and graphene, rubber, nonwoven fabric, and paper, as well as particles, flakes, beads, sheets, foils, films, and fibers thereof, regardless of their form and shape.
[0032] The silver mirror reaction test using the Tollens' reagent is inconvenient in that a new silver solution must be prepared and used for each silver mirror reaction. In contrast, the silver plating solution of the present invention can be prepared in advance and stored so that it can be used whenever necessary. The silver plating solution of the present invention is not necessarily limited to a specific hydrogen ion concentration (pH). A typical silver plating process (including electroless silver plating) is carried out in a relatively strongly acidic (pH≦3.0) or alkaline (pH≧10.0) range. In contrast, the present invention is characterized in that silver plating is well performed even in a neutral to weakly alkaline range (pH 7.0-9.0) except in special cases. That is, the silver plating solution of the present invention is environmentally friendly and has good storage stability, so that it can be stored before use and can be conveniently used in experiments whenever desired. Another feature of the silver plating solution according to the present invention is that when it is intended to carry out an exemplary oxidation-reduction reaction experiment in school or to manufacture a silver mirror souvenir or ornament, the silver plating solution is very useful for anyone because of its simplicity and safety. In addition, since the silver plating solution of the present invention does not use tin chloride, it can be used to produce silver mirrors with small surface roughness. In particular, the silver plating solution of the present invention is highly suitable for use in producing high-quality optical mirrors such as telephoto lenses.
[0033] The above-mentioned features of the present invention can be more effectively realized when the silver plating solution containing the silver carboxylate as the silver precursor and the complexing agent further contains a stabilizer, a solvent, and an additive. In particular, a reducing agent is essential for electroless silver plating or silver mirror reaction.
[0034] The reducing agent acts to deposit silver on the surface of the object by transferring electrons released during its oxidation to silver ions. Specific examples of reducing agents suitable for use in the silver plating solution of the present invention include acetol, acetoin, hydroxyacetone, hydroxylamine, diethylhydroxylamine, methylethylketoxime, Rochelle salt, sodium erythorbate, alkylaminoboranes such as ammonia borane, methylaminoborane, and diethylaminoborane, hydrazine, hydrazine hydrate, hydrazine sulfate, sodium hypophosphite, sodium sulfite, sodium thiosulfate, sodium borohydride, lithium aluminum hydride, sodium citrate, and alkylamines such as butylamine, ethanolamine, ethylenediamine, and dodecylamine, ethylene glycol, thiodiglycol, diethylene glycol, formaldehyde, glucose, sorbitol, sugars, formic acid, ammonium formate, triethylammonium formate, tetramethylammonium formate, citric acid, ascorbic acid, tartaric acid, phenidone, 2-((4-amino-3-methylphenyl)ethylamino)ethyl sulfate, N-( Hydroquinone compounds such as 2-((4-amino-3-methylphenyl)ethylamino)ethyl)methanesulfonamide, 4-(N-ethyl-N-2-hydroxyethyl)-2-methylphenylenediamine sulfate, methylhydroquinone, methoxyhydroquinone, t-butylhydroquinone, 2,5-di-t-butylhydroquinone, 2,5-bis(1,1-dimethylbutyl)hydroquinone, and 2,5-bis(1,1,3,3-tetramethylbutyl)hydroquinone, as well as 4-methoxyphenol, 2 phenolic and polyphenolic compounds such as, for example, 6-di-t-butyl-4-methylphenol, quinhydrone, p-methylaminophenol sulfate, p-aminophenol, diaminophenol, 2-naphthol, catechol, t-butylcatechol, resorcinol, phloroglucinol, hydroxyquinol, pyrogallol, tannin, tannic acid, dopamine, cardanol, urushiol, gallic acid and its derivatives, flavonoids, isoflavones, and anthocyanins. These reducing agents may be used alone or as a mixture of two or more thereof.Representative examples of these reducing agents include glucose, hydrazine, hydroquinone, and derivatives thereof. Glucose reacts slowly, and hydrazine reacts quickly but is harmful to the human body. Therefore, hydroquinone is most preferred from various viewpoints including the reaction rate required in the present invention, environmental friendliness, and safety. Apart from these reducing agents, treatments using heat, light, plasma, infrared (IR), ultraviolet (UV), electron beam, photon, laser, microwave, electricity, and magnetism also act as reducing agents. Therefore, these treatments are performed alone or in combination with the reducing agent for faster reduction. The amount of the reducing agent used is not particularly limited as long as it does not impair the object of the present invention, and is typically a molar ratio of 0.1 to 5.0, preferably 0.3 to 3.0, and more preferably 0.5 to 2.0, relative to the silver carboxylate. If the amount of the reducing agent is less than the lower limit or more than the upper limit, problems may occur in the stability of the plating solution, or the reaction may proceed too slowly or too quickly, making it difficult to control the reaction, and the quality of the product may be reduced.
[0035] The reaction temperature during silver plating is not particularly limited as long as it does not impair the object of the present invention, and is typically 5 to 50° C., preferably 10 to 40° C., and more preferably 15 to 30° C. If the reaction temperature is below the lower limit or higher than the upper limit, the stability of the plating solution may decrease, or the reaction may proceed too slowly or too quickly, making it difficult to control the reaction, and the quality of the product may decrease.
[0036] The stabilizer may be selected from long-chain mercaptans such as dodecanethiol, fatty acids such as oleic acid, amines such as oleylamine, polymers and copolymers thereof such as polyvinylpyrrolidone, poly(2-ethyl-2-oxazoline), polyvinyl alcohol, polyethylene glycol, and polystyrene sulfonic acid, as well as synthetic and natural polymers such as carboxymethylcellulose, alginic acid, chitosan, dopamine, starch, polysaccharides, and gums. The stabilizer is expected to effectively prevent deterioration over time or improve adhesion. The additive may be a surfactant and a discoloration inhibitor. The surfactant is preferably a nonionic surfactant such as polyoxyethylene alkyl ether or ester, fatty acid sorbitan ester, or alkyl monoglyceryl ether. The discoloration inhibitor may be selected from the group consisting of benzotriazole and its derivatives. One or more other additives selected from the group consisting of metal compounds such as ammonium molybdate, bismuth nitrate, selenic acid, and thallium nitrate, and mixtures thereof, may also be used in the present invention.
[0037] In electroless silver plating based on the silver mirror reaction, the silver plating solution of the present invention may use an ammonium salt as an additive. In this case, the ammonium salt may be ammonium formate, ammonium acetate, ammonium nitrate, ammonium sulfate, ammonium sulfite, ammonium carbonate, ammonium bicarbonate, ammonium carbamate, or ammonium phosphate. Appropriate use of the ammonium salt allows control over the reaction rate, ensuring uniform plating, improved mirror properties, and high conductivity. The amount of the ammonium salt used is not particularly limited as long as it does not impair the object of the present invention, and is typically 0.01 to 10.0% by weight, preferably 0.05 to 5.0%, and more preferably 0.1 to 3.0% based on the weight of the final plating solution. If the amount of the ammonium salt is less than the lower limit or exceeds the upper limit, the stability of the plating solution may be deteriorated, or the quality of the final product may be deteriorated.
[0038] The solvent is not necessarily limited as long as it does not impair the object of the present invention, and may be selected from the group consisting of polar solvents, for example, deionized water, alcohols such as methanol, ethanol, n-propanol, iso-propanol, n-butanol, iso-butanol, 1-methoxy-2-propanol, diacetone alcohol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol, glycols and glycol ethers such as ethylene glycol, diethylene glycol, propylene glycol, glycerin, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, and diethylene glycol monoethyl ether, ionic liquids such as ethylammonium nitrate and 1-ethyl-3-methylimidazolium dicyanamide, and mixtures thereof. Water, ethanol, ethylene glycol, glycerin, or mixtures thereof, especially a mixed solvent of water and ethanol, is most suitable for use in the present invention. Using a minimum amount of water in silver electroplating ensures high plating quality. If the water content increases during electroless plating based on the silver mirror reaction, the reaction rate increases and the life of the plating solution decreases. If the water content is too high, the stability of the plating solution may decrease, and the quality of the final product may become non-uniform. Therefore, the water content is preferably limited to 1 to 80% by weight, more preferably 20 to 50% by weight, based on the total weight of the solvent.
[0039] Nonconductors such as glass, ceramics, or plastics may be cleaned with nitric acid, surfactants, or alcohols prior to electroless silver plating. After cleaning, adhesion may be improved using a suitable process selected from mechanical polishing such as vapor blasting or grinding with silicon carbide, etching with chromic acid, sulfuric acid, or hydrofluoric acid, and sensitization and activation with tin chloride (SnCl2) and palladium chloride (PdCl2). In contrast, the silver plating solution of the present invention mainly uses an alcohol solution, and the autocatalytic plating of silver ions occurs, so that electroless plating based on the silver mirror reaction proceeds well while maintaining some adhesion without even the need for the pretreatment process mentioned above. Then, electroplating may be performed with the electroless plated material as the cathode to increase the plating thickness or to achieve better appearance and physical properties.
[0040] Copper substrates are susceptible to displacement plating without the use of a reducing agent solution. Thus, the silver complex solution may be used alone to perform electroless plating. In the case of electroplating, the silver complex solution may be used as an electrolyte. In this case, electricity is used instead of a reducing agent to perform silver plating.
[0041] After completion of silver plating, silver and silver alloys are generally protected from tarnishing by the use of commercially available tarnish inhibitors such as Tarniban®, surface coating with sulfur compounds such as thiols or sulfides, immersion in chromic anhydride solutions, or cathodic treatment in alkaline chromic acid solutions. Depending on the type of final product, a heat treatment at 50-150°C may be further performed for quality stabilization and impurity removal. The heat-treated product may be immersed in polymeric compounds such as water-based polyurethanes, water-based acrylic polymers, polyesters, silicone polymers, or fluorinated polymers, coated by wet processes such as spray coating, spin coating, bar coating, slit die coating, or gravure coating, or vacuum deposited or sputtered with inorganic compounds such as silica or titanium dioxide, depending on the type of said final product.
[0042] The present invention will now be described in more detail with reference to the following examples, which are provided for illustrative purposes and are not intended to limit the scope of the present invention. EXAMPLES
[0043] In the following examples, including Preparation Examples 1-13, unless otherwise noted, all experiments were performed at room temperature, 25° C. All percentages are by weight unless otherwise noted.
[0044] Preparation of silver complex solution for silver plating Preparation Example 1 40g of ammonia water (28-30%) was slowly added to 100g of silver neodecanoate, and then completely dissolved. 70g of ethanol (95%) was added to this solution. The silver neodecanoate-ammonia complex solution was obtained by filtration (final silver content: about 18.0%).
[0045] Preparation Example 2 A mixed solution of 280 g of ethanol and 70 g of deionized water (hereinafter simply referred to as "water") was added to 10 g of the silver neodecanoate-ammonia complex solution prepared in Preparation Example 1 to prepare a colorless and transparent silver neodecanoate-ammonia complex solution (final silver content: 0.5%).
[0046] Preparation Example 3 To 10 g of the silver neodecanoate-ammonia complex solution prepared in Preparation Example 1, 350 g of ethanol was added to prepare a silver neodecanoate-ammonia complex solution (final silver content: 0.5%).
[0047] Preparation Example 4 To 100 g of the silver neodecanoate-ammonia complex solution prepared in Preparation Example 2, 2.0 g of ammonia water was added to prepare a silver complex solution.
[0048] Preparation of reducing agent solution Preparation Example 5 A reducing agent solution was prepared by adding 1.5 g of hydroquinone to a mixed solution of 100 g of ethanol and 400 g of water.
[0049] Preparation Example 6 A reducing agent solution was prepared by adding 1.5 g of hydroquinone to a mixed solution of 100 g of glycerin and 400 g of water.
[0050] Preparation Example 7 A reducing agent solution was prepared by adding 1.5 g of hydroquinone to a mixed solution of 400 g of ethanol and 100 g of water.
[0051] Preparation Example 8 A reducing agent solution was prepared by adding 3.0 g of 2,5-di-tert-butylhydroquinone to a mixed solution of 250 g of ethanol and 250 g of water.
[0052] Preparation Example 9 A reducing agent solution was prepared by adding 0.5 g of ammonium formate to 100 g of the reducing agent solution prepared in Preparation Example 5.
[0053] Preparation Example 10 A reducing agent solution was prepared by adding 0.5 g of 80% hydrazine hydrate to 100 g of water.
[0054] Preparation Example 11 A reducing agent solution was prepared by adding 5.0 g of glucose to 100 g of water.
[0055] Preparation Example 12 0.5 g of 80% hydrazine hydrate was added to a mixed solution of 50 g of water and 50 g of ethanol, and 0.5 g of ammonium nitrate was added thereto to prepare a reducing agent solution.
[0056] Preparation Example 13 A reducing agent solution was prepared by adding 0.5 g of 80% hydrazine hydrate to 100 g of water, to which was added 0.5 g of ammonium formate.
[0057] Manufacturing of silver mirror products Example 1 First, about half of a pre-washed transparent glass container with a lid was filled with the silver complex solution of Preparation Example 2. The container was thoroughly shaken to sensitize and activate its inner surface. The remaining half of the container was then filled with the reducing agent solution of Preparation Example 5. The container was thoroughly shaken and allowed to stand for about 30 minutes. The contents of the container were drained and then thoroughly washed with ethanol. As a result, a light gold mirror was formed on the inner surface of the container and a clean silver mirror was formed on the outer surface of the container. The inner surface of the container was coated with water-based polyurethane to prevent tarnishing. A photograph of the obtained sample is shown in Figure 1.
[0058] Example 2 The procedure of Example 1 was repeated, except that the reducing agent solution of Preparation Example 6 was used instead of the reducing agent solution of Preparation Example 5. As a result, the reaction was slightly slower than in Example 1, and a thin black mirror was successfully formed on the inner surface of the container, and a clean silver mirror was successfully formed on the outer surface of the container. The inner surface of the container was coated with a water-based acrylic polymer to prevent discoloration. A photograph of the obtained sample is shown in Figure 1.
[0059] Example 3 The procedure of Example 1 was repeated, except that the reducing agent solution of Preparation Example 7 was used instead of the reducing agent solution of Preparation Example 5. As a result, the reaction was slightly slower than in Example 1, and clean silver mirrors were successfully formed on both the inner and outer surfaces of the container. A photograph of the obtained sample is shown in Figure 1.
[0060] Example 4 The procedure of Example 1 was repeated, except that the reducing agent solution of Preparation Example 8 was used instead of the reducing agent solution of Preparation Example 5. As a result, a clean silver mirror was successfully formed on each of the inner and outer surfaces of the container. A photograph of the obtained sample is shown in Figure 1.
[0061] Example 5 First, about half of the capacity of a pre-washed transparent glass container with a lid was filled with the silver complex solution of Preparation Example 3. The container was thoroughly shaken to sensitize and activate its inner surface. The remaining half of the container was then filled with the reducing agent solution of Preparation Example 6. The container was thoroughly shaken and left to stand for about 1 hour. The contents of the container were drained and then thoroughly washed with ethanol. As a result, a gold mirror was well formed on the inner surface of the container, and a clean silver mirror was well formed on the outer surface of the container. The inner surface of the container was coated with a silicone-based polymer to prevent discoloration. A photograph of the obtained sample is shown in Figure 1.
[0062] Example 6 First, about half of a pre-cleaned transparent glass container with a lid was filled with the silver complex solution of Preparation Example 2. The container was thoroughly shaken to sensitize and activate its inner surface. The remaining half of the container was then filled with the reducing agent solution of Preparation Example 9. The container was thoroughly shaken and allowed to stand for about 1 hour. The contents of the container were drained and then thoroughly washed with ethanol. As a result, a black mirror was well formed on the inner surface of the container, and a clean silver mirror was well formed on the outer surface of the container. A photograph of the obtained sample is shown in Figure 1.
[0063] Example 7 The procedure of Example 6 was repeated, except that the silver complex solution of Preparation Example 4 was used instead of the silver complex solution of Preparation Example 2. As a result, a light gold silver mirror was well formed on the inner surface of the container, and a clean silver mirror was well formed on the outer surface of the container. A photograph of the obtained sample is shown in Figure 1.
[0064] Example 8 The procedure of Example 1 was repeated, except that a transparent polyester container (PET bottle) was used instead of the pre-cleaned transparent glass container with lid. As a result, a light gold mirror was formed on the inner surface of the container, and a clean silver mirror was formed on the outer surface of the container. A photograph of the obtained sample is shown in Figure 3.
[0065] Example 9 First, about half of a pre-cleaned transparent glass container with a lid was filled with the silver complex solution of Preparation Example 3. The container was thoroughly shaken to sensitize and activate its inner surface. The remaining half of the container was then filled with the reducing agent solution of Preparation Example 10. The container was thoroughly shaken and allowed to stand for about 10 minutes. The contents of the container were drained and then thoroughly washed with water. As a result, shiny light gold and silver mirrors were formed on the inner and outer surfaces of the container, respectively. The mirrors were thinner than those formed when the hydroquinone reducing agent was used.
[0066] Example 10 First, about half of a pre-cleaned transparent glass container with a lid was filled with the silver complex solution of Preparation Example 3. The container was thoroughly shaken to sensitize and activate its inner surface. The remaining half of the container was then filled with the reducing agent solution of Preparation Example 11. The container was thoroughly shaken and allowed to stand for about 6 hours. The contents of the container were drained and then thoroughly washed with water and ethanol in turn. As a result, shiny gold and silver mirrors were formed on the inner and outer surfaces of the container, respectively. The mirrors were thinner than those formed when the hydroquinone reducing agent was used.
[0067] Example 11 In Preparation Example 1, 60 g of methylamine aqueous solution (40%) was used as a complexing agent instead of aqueous ammonia. Silver neodecanoate was completely dissolved, and 80 g of ethanol was added thereto. A purple silver neodecanoate-methylamine complex solution was obtained by filtration. 300 g of ethanol was added to 10 g of the complex solution to prepare a colorless complex solution (final silver content: about 0.5%). This complex solution was placed in a transparent glass container with a lid that had been washed in advance. The container was thoroughly shaken to sensitize and activate its inner surface. The container was then filled with the same amount of the reducing agent solution of Preparation Example 13 on a weight ratio basis. The container was thoroughly shaken and allowed to stand for about 10 minutes. The contents of the container were drained, and then thoroughly washed with water and ethanol in turn. As a result, a black dark gold mirror was well formed on the inner surface of the container, and a shiny silver mirror was well formed on the outer surface of the container.
[0068] Example 12 The procedure of Example 11 was repeated, except that the reducing agent solution of Preparation Example 11 was used instead of the reducing agent solution of Preparation Example 13. After 1 hour, a shiny silver mirror was well formed on the inner surface of the container, and a shiny silver mirror was well formed on the outer surface of the container.
[0069] Comparative Example 1 A colorless alcoholic ammonia complex solution (final silver content: 0.5%) was prepared in the same manner as in Preparation Example 1, except that silver neodecanoate was dissolved in alcoholic ammonia instead of aqueous ammonia, and absolute ethanol was used as the diluent. The colorless alcoholic ammonia complex solution was thoroughly shaken in a pre-cleaned transparent glass container with a lid to sensitize and activate the inside surface of the container. The container was then filled with an equal amount of reducing agent solution on a weight ratio basis, which had been previously prepared by dissolving 0.3% hydroquinone in absolute ethanol. The reaction was allowed to proceed for 30 minutes. As a result, a darker silver mirror was formed, which was of lower quality than the silver mirror formed when 95% ethanol was used.
[0070] Comparative Example 2 Except for continuously adding water instead of ethanol, an aqueous solution of silver neodecanoate-ammonia complex (final silver content: 0.5%) was prepared in the same manner as in Preparation Example 1. However, a white solid precipitated, and it was impossible to further proceed with the silver mirror reaction.
[0071] Examples 13 to 19 An experiment was conducted to determine whether plating would be performed well depending on the silver content. A silver mirror product was manufactured in the same manner as in Example 1, except that the amount of ethanol mixed with the complex solution was adjusted so that the final silver content would be as shown in Table 1. The water content was fixed at 70 g, the same as in Preparation Example 2. [Table 1]
[0072] The complex solution was placed in a previously cleaned transparent glass container with a lid. The container was thoroughly shaken to sensitize and activate its inner surface. The container was then filled with the same amount of the reducing agent solution of Preparation Example 5 on a weight ratio basis. The container was thoroughly shaken and allowed to stand for about 10 minutes. The contents of the container were drained and then thoroughly washed with water and ethanol in turn. The final silver content was used to determine whether the silver mirror reaction had proceeded.
[0073] From the experiments, it was found that the silver mirror reaction was most stable and produced clean plating in Example 16, and silver mirrors were formed despite the low silver content in Examples 14 and 15. In Example 13, the silver mirror reaction occurred even when the silver content was as low as 0.01%, but the silver mirror was translucent with poor mirror properties.
[0074] In contrast, the higher silver content silver mirrors formed in Examples 17 and 18 darkened in color as the silver content increased, and the 7.5% silver mirror formed in Example 19 was dark in color with silver precipitated on the bottom of the container.
[0075] Example 20 In Preparation Example 1, 15 g of ammonia water was slowly added to 20 g of silver acetate instead of silver neodecanoate. The silver acetate was completely dissolved, and 15 g of ethanol was added thereto. A colorless silver acetate-ammonia complex solution was obtained by filtration. 500 g of ethanol was added to 10 g of the complex solution to prepare a colorless complex solution (final silver content: about 0.5%). The silver acetate solution was placed in a transparent glass container with a lid that had been washed in advance. The container was thoroughly shaken to sensitize and activate its inner surface. The container was then filled with the same amount of the reducing agent solution of Preparation Example 13 on a weight ratio basis. The container was continuously shaken. As a result, a shiny silver mirror was well formed within 5 minutes. The contents of the container were drained, and then thoroughly washed with water and ethanol in turn. As a result, a golden mirror was well formed on the inner surface of the container, and a shiny silver mirror was well formed on the outer surface of the container.
[0076] Examples 21 to 26 To determine whether the silver mirror reaction occurs in response to the silver carboxylates shown in Table 2, an experiment similar to that of Example 20 was carried out. [Table 2]
[0077] As can be seen from the results in Table 2, when silver propionate or silver 2-ethylhexanoate was used, the silver mirror reaction proceeded relatively smoothly under appropriate reaction conditions, as in the cases of using silver neodecanoate and silver acetate in Examples 1 to 20. The silver mirror reaction also occurred when different types of silver carboxylates were used. However, due to their low reactivity, a weak silver mirror reaction occurred under general conditions. In other words, the silver mirror reaction could be caused to proceed with the different types of silver carboxylates at a level equal to or higher than that achieved by silver nitrate, which has been widely used for this purpose.
[0078] Examples 27 to 33 In order to determine whether plating is performed well depending on the content of the complexing agent, an experiment similar to that of Example 20 was carried out. A silver mirror product was manufactured in the same manner as in Preparation Example 1 and Example 1, except that the amount of the complexing agent (ammonia water) mixed with the silver carboxylate (silver neodecanoate) in the complex solution was adjusted as shown in Table 3. [Table 3]
[0079] The silver mirror reaction was carried out in the same manner as in Example 1, except that the silver carboxylate and the complexing agent were mixed in the same ratio as shown in Table 3. In Examples 27 and 28, which had a low content of the complexing agent, there was a problem with solubility, and the silver mirror reaction hardly occurred. In Examples 29 to 32, the silver mirror reaction was carried out normally. The best silver mirror was formed in Example 30.
[0080] In Example 33, in which an excess amount of the complexing agent was used, the storage stability of the complex solution of the complexing agent and the silver carboxylate was low, making it difficult to obtain a clean silver mirror.
[0081] Examples 34 to 40 In order to determine whether plating is performed well depending on the content of the reducing agent, the silver complex and the reducing agent were mixed in the amounts shown in Table 4, and an experiment was performed in the same manner as in Example 1, except that the same amount of the mixture (10 g) was placed in the container. [Table 4]
[0082] A mixture of a silver complex solution and a reducing agent solution in the ratio shown in Table 4 was poured into each container. In Examples 35 to 39, the desired silver mirror reaction was normally carried out. The rate of the silver mirror reaction increased with an increase in the content of the reducing agent. In Example 34, in which the content of the reducing agent was low, the silver mirror reaction took a long time (about 50 to 80 minutes), making it difficult to use the silver mirror for industrial purposes. In Example 40, in which the reducing agent was used in excess, silver precipitated, and the silver content was relatively low, so the silver mirror was translucent with poor mirror properties.
[0083] Manufacturing of conductive products Example 41 The silver neodecanoate-ammonia complex solution (silver content: 18.0%) prepared in Preparation Example 1 was diluted with a mixed solution of ethanol and water in a weight ratio of 4:1 to a final silver content of 1.0%. 0.5% ammonium formate was dissolved in the diluted silver neodecanoate-ammonia complex solution to prepare an electroless silver plating solution. 3.0 g of hydroquinone was added to a mixed solution of 100 g of glycerin and 400 g of water to prepare a reducing agent solution. A nylon fabric was immersed in the silver plating solution for 1 hour to thoroughly wet it, and then the reducing agent solution was added thereto in a weight ratio of 1:1 to the silver plating solution. The reaction was allowed to proceed for 3 hours. After the reaction was completed, the nylon fabric was filtered, washed with water and ethanol in that order, and dried at 120°C for 12 hours to produce a highly conductive silver-coated nylon fabric (see FIG. 4).
[0084] Example 42 Highly conductive silver coated nylon fibers were produced in the same manner as in Example 41, except that nylon fibers were used instead of nylon fabric. Figure 5 shows a photograph of the resulting sample and its measured conductivity. Figure 6 shows a surface scanning electron microscope (SEM) image of the fiber.
[0085] Example 43 A silver-coated mirror-like polyimide film was prepared in the same manner as in Example 41, except that a 25 micron polyimide film was used instead of the nylon fabric. A photograph of the resulting sample is shown in Figure 7. The reflectance and sheet resistance of the sample were measured to be 97.5% and 120 mΩ / □ at 550 nm, respectively.
[0086] Example 44 A silver-coated mirror-like nylon film was produced in the same manner as in Example 43, except that a 12 micron nylon film was used instead of the 25 micron polyimide film. The sheet resistance of the film was measured to be 130 mΩ / □.
[0087] Example 45 The silver neodecanoate-ammonia complex solution (silver content: 18.0%) prepared in Preparation Example 1 was diluted with a mixed solution of ethanol and water in a weight ratio of 1:1 to prepare an electroless silver plating solution (final silver content: 0.5%). A polyurethane foam was immersed in the silver plating solution for 1 hour to thoroughly wet it, and then the reducing agent solution of Preparation Example 12 was added thereto in a weight ratio of 1:1 to the silver plating solution. The reaction was allowed to proceed for 2 hours while stirring. After the reaction was completed, the polyurethane foam was filtered, washed with water and ethanol in that order, and dried at 120°C for 30 minutes to produce a silver-coated polyurethane foam whose surface resistance was measured to be 0.3 Ω / cm. A photograph and a surface scanning electron microscope (SEM) image of the silver-coated sample are shown in Figures 8 and 9, respectively.
[0088] Example 46 Silica beads having an average particle size of 12 μm and surface-treated with 3-aminotriethoxysilane were added to the silver complex solution of Preparation Example 3 with stirring, thoroughly wetted, filtered, washed with ethanol, and dried. The pretreated silica beads were added to an electroless silver plating solution composed of the silver complex solution of Preparation Example 4 and the reducing agent solution of Preparation Example 9 in a 1:1 weight ratio. The reaction was allowed to proceed for 1 hour with stirring. After completion of the reaction, the silica beads were filtered, washed with water and ethanol in turn, and dried at 100° C. for 24 hours to produce silver-coated silica beads.
[0089] Example 47 Silver-coated copper particles were produced in the same manner as in Example 46, except that copper particles having an average particle size of 4 μm were used instead of the silica beads having an average particle size of 12 μm.
[0090] Example 48 The silver complex solution of Preparation Example 3 (silver concentration: 0.5%) was placed in a polypropylene plating bath. A silver plate and a copper foil with a smooth surface were used as the anode and cathode, respectively. A 4.5 V power supply was connected between the anode and the cathode. The power supply consisted of three 1.5 V dry batteries connected in series. Electroplating was performed for 1 minute and 30 seconds. After plating was completed, the plated product was thoroughly washed with water and ethanol and thoroughly dried at 80°C to produce a shiny, mirror-like copper product with silver plated on the copper surface.
[0091] Example 49 The procedure of Example 48 was repeated, except that a silver-coated PET film having a resistivity of 1.5 Ω / cm was used as the cathode instead of the copper foil. After electroplating, the sample was measured to have a surface resistivity of 0.4 Ω / cm, indicating improved electrical conductivity.
[0092] Example 50 100 g of the complex solution (silver concentration: 0.5%) prepared in Preparation Example 4 was placed in a beaker, and copper foil was placed in it. In this example, no reducing agent solution was used. Substitution plating was carried out at room temperature for 15 minutes to produce a shiny silver-coated mirror-like copper foil (see FIG. 10).
[0093] Manufacturing of antibacterial products Example 51 100g of the complex solution of Preparation Example 2 (silver concentration: 0.5%) was diluted with 4.9kg of a mixed solution of 80% ethanol and 20% water to prepare a silver-containing mixed solution with a final concentration of 100ppm. 100ppm of ammonium sulfate and a white cotton fabric were added to the silver solution, and the fabric was thoroughly wetted with the silver solution while stirring for 3 hours. The wet fabric was squeezed to thoroughly remove the solvent, and exposed to sunlight for a long time to reduce the silver ions. The color of the fabric changed to brown depending on the degree of reduction. The fabric was washed and dried using a washing machine, and its antibacterial properties were tested. As a result, the fabric showed 99.9% antibacterial activity against E. coli (see Figure 11).
[0094] Example 52 The silver complex solution (silver concentration: 0.5%) of Preparation Example 3 was diluted with ethanol to prepare a solution (final silver concentration: 50 ppm). A polyester microfiber insert, which is widely used as an insulating material for blankets and pillows, was added to the silver solution so that it was immersed in the silver solution. The polyester microfiber insert was thoroughly wetted with the silver solution while stirring for 1 hour. The reducing agent solution of Preparation Example 6 was then diluted with ethanol to prepare a hydroquinone solution with a final concentration of 60 ppm. The wet polyester microfiber insert was added to the hydroquinone solution. The reaction was allowed to proceed for 1 hour while stirring. After the reaction was completed, the polyester microfiber insert was filtered, washed with water and ethanol in turn, and dried at 80°C for 6 hours to produce a silver-treated polyester microfiber insert. The antibacterial properties of the microfiber insert were tested. The microfiber insert showed 99.9% antibacterial activity against E. coli.
[0095] Experimental Example 1 A comparison was made with existing one-component electroless silver plating chemicals. Commercially available electroless silver plating chemicals, AG-10 manufactured by HANBIT Chemical and MS-AG100 manufactured by MSC, were used as Comparative Example 3 and Comparative Example 4, respectively.
[0096] The surface of the copper-plated substrate of Example 50 was silver-plated using each of the silver plating solutions of Comparative Examples 3 and 4. The copper-plated substrate of Example 50 was placed in a container, and the same silver complex solution as that used in Example 50 was supplied to the container. After plating was completed, the plated surface was etched to remove the silver plating formed in areas other than the copper-plated area.
[0097] Each of the silver plating solutions of Comparative Examples 3 and 4 was poured into a container, and the copper-plated substrate was then immersed in the silver plating solution and silver plating was then carried out.
[0098] As a result, even when the commercially available silver plating solutions of Comparative Examples 3 and 4 were used, the same silver plating as in Example 1 could be performed. The silver plating of Example 1 could be performed simply by removing excess silver by etching. This is because when the silver plating of Example 1 was performed, a large amount of silver was deposited on the copper surface, as in the case of a conventional plating process, and although the silver layer was made to the same thickness by etching, the silver was formed thicker on the copper than on the insulator. The same silver plating was also performed when the commercially available silver plating solutions of Comparative Examples 3 and 4 were used. That is, the silver plating solution of the present invention can be used by making slight changes to the conventional product manufacturing process.
[0099] Experimental Example 2 The procedure of Experimental Example 1 was repeated using the silver plating solution used in Example 1 and the commercially available silver plating solutions of Comparative Examples 3 and 4. It was determined whether the surface of the polymer resin was plated.
[0100] A rectangular bar having dimensions of 1 cm x 1 cm x 3 cm was placed in the plating vessel and was made of the materials shown in Table 4.
[0101] The plating solution used in Example 1 and the commercially available plating solutions of Comparative Examples 3 and 4 were each added to a plating vessel. The vessel was agitated by shaking. After 20 minutes, the rectangular bars were removed to determine whether they had been plated. [Table 5]
[0102] As can be seen from the results in Table 5, not only the surface of the metallic rectangular bar but also the surface of the polymer resin rectangular bar was uniformly plated using the plating solution used in Example 1. In contrast, when the plating solutions of Comparative Examples 3 and 4 were used, silver was plated only onto the surface of the metallic rectangular bar, and silver plating was not applied to the surface of the polymer resin rectangular bar.
[0103] Experimental Example 3 The silver complex solution prepared in Preparation Example 2 and the reducing agent prepared in Preparation Example 8 were stored at room temperature for 6 months to test their storage stability. Figures 11 and 12 show the state of the silver complex solution and the reducing agent solution, respectively, after storage at room temperature for 6 months.
[0104] As shown in Figures 12 and 13, the solution was stable without any precipitate even after 6 months of storage at room temperature, and is expected to remain stable even after several years.
[0105] In contrast, precipitation was observed during storage for the same period in the plating solutions of Comparative Examples 3 and 4, demonstrating that the stability of the two-component silver plating solution of the present invention is equal to or greater than that of existing one-component electroless plating solutions.
[0106] Experimental Example 4 An experiment was carried out to determine the amount of silver nitrate produced. The contents of silver nitrate formed in the plating solutions used in Examples 1 to 5 and the commercially available silver plating solutions of Comparative Examples 3 and 4 were measured.
[0107] There is no general method for determining the amount of silver nitrate in water, so the silver nitrate content was measured by applying the method of measuring chloride ions using silver nitrate in reverse.
[0108] A known method using 0.01N hydrochloric acid was used to measure chloride ions. However, in this method, the concentration of chloride ions was fixed instead of measured, thereby indirectly determining the content of silver nitrate. As Comparative Example 5, an experimental kit for silver mirror reaction (OfficeAhn) was used. [Table 6]
[0109] As can be seen from the results in Table 6, the amount of silver nitrate formed in the plating solutions used in Examples 1 to 5 was below the detection limit. The plating solutions used in Examples 1 to 5 were found to be very stable during long-term storage before and after use, since no explosive silver nitrate was produced. In contrast, silver nitrate was produced in the commercially available silver plating solutions of Comparative Examples 3 and 4 currently used for silver plating, indicating that the silver nitrate concentration may increase when the silver plating solution is concentrated or stored for a long period of time. Finally, a large amount of silver nitrate was detected in the experimental kit for silver mirror reaction, since the kit directly uses silver nitrate.
Claims
1. An electroless silver plating solution comprising a silver complex solution and a reducing agent solution, the silver complex solution comprising a silver carboxylate represented by Formula 1: [Formula 1] R 1 -COOAg In the formula, R 1 is hydrogen, substituted or unsubstituted C 1 ~C 22 Alkyl, substituted or unsubstituted C 3 ~C 30 Cycloalkyl, substituted or unsubstituted C 6 ~C 30 Aralkyl, substituted or unsubstituted C 1 ~C 30 Heteroalkyl, substituted or unsubstituted C 2 ~C 30 Heterocycloalkyl or substituted or unsubstituted C 5 ~C 30 and the electroless silver plating is based on the silver mirror reaction between the silver complex solution and the reducing agent solution.
2. 2. The electroless silver plating solution of claim 1, wherein the silver complex solution further comprises a nitrogen-containing compound as a complexing agent, and a solvent.
3. 3. The electroless silver plating solution of claim 2, wherein the nitrogen-containing compound is selected from the group consisting of ammonia, amines, quaternary ammonium salts, polyamines, and mixtures thereof.
4. The nitrogen-containing compound is an amine of formula 2: [Formula 2] (R 2 R 3 R 4 )N In the formula, R 2 ~R 4 are the same or different, and each independently represents hydrogen, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 6 ~C 30 Aryl, substituted or unsubstituted C 3 ~C 30 Cycloalkyl, substituted or unsubstituted C 6 ~C 30 Aralkyl, substituted or unsubstituted C 1 ~C 30 Heteroalkyl, substituted or unsubstituted C 2 ~C 30 Heterocycloalkyl, substituted or unsubstituted C 5 ~C 30 Heteroaryl, or substituted or unsubstituted C 5 ~C 30 A heteroaralkyl, amine or quaternary ammonium salt compound of formula 3: [Formula 3] (R 5 R 6 R 7 R 8 )N + X In the formula, R 5 ~R 8 is R in formula 2 2 ~R 4 and X is as defined by F - , Cl - , B - , I - , O.H. - 4. The electroless silver plating solution according to claim 3, wherein the quaternary ammonium salt compound is a quaternary ammonium salt compound selected from the group consisting of a hydrogen sulfate ion, a hydrogen carbonate ion, a carbamate ion, and a perchlorate ion.
5. 3. The electroless silver plating solution according to claim 2, wherein the nitrogen-containing compound is ammonia or an alkylamine.
6. 3. The electroless silver plating solution according to claim 2, wherein the solvent is water, ethanol, ethylene glycol, glycerin, or a mixture thereof.
7. 3. The electroless silver plating solution of claim 2, wherein the complexing agent is present in a molar ratio of 0.1 to 10.0 relative to the silver carboxylate.
8. 3. The electroless silver plating solution according to claim 2, wherein the complexing agent combines with the silver ions of the silver carboxylate to form complex ions.
9. 2. The electroless silver plating solution of claim 1, wherein the reducing agent solution comprises a reducing agent selected from the group consisting of glucose, hydrazine, hydroquinone, and derivatives thereof, and a solvent.
10. 10. The electroless silver plating solution according to claim 9, wherein the solvent is water, ethanol, ethylene glycol, glycerin, or a mixture thereof.
11. 11. The electroless silver plating solution according to claim 10, wherein the solvent is a mixed solvent containing 1 to 80% by weight of water.
12. 10. The electroless silver plating solution of claim 9, wherein the reducing agent solution further comprises one or more additives comprising an ammonium salt.
13. 13. The electroless silver plating solution of claim 12, wherein the ammonium salt is present in an amount of 0.01 to 10.0% by weight, based on the weight of the final plating solution.
14. 2. The electroless silver plating solution according to claim 1, wherein the silver carboxylate is a silver alkanoate.
15. 2. The electroless silver plating solution according to claim 1, wherein the silver content is 0.05 to 5.0% by weight based on the weight of the final plating solution.
16. 2. The electroless silver plating solution of claim 1, wherein the reducing agent is present in a molar ratio of 0.1 to 5.0 relative to the silver carboxylate.
17. A silver-plated product produced by a reaction at 5 to 50° C. using the silver plating solution according to any one of claims 1 to 16.
Citation Information
Patent Citations
Electroless plating bath and metal coating obtained by using the plating bath
JP2003268558A
Reducing type electroless silver plating solution
JP2012082444A
Method for making electrically-conductive articles
US20160333482A1