Low-stress-level chemical copper plating solution and preparation method thereof
By using modification accelerator and carbon nanotube technology in electroless copper plating solution, the internal stress of copper plating layer is reduced, and the problems of plating fracture and high-temperature and low-speed deposition are solved, and low-temperature and high-speed deposition and stability are improved. It is suitable for new materials copper plating process.
Patent Information
- Application Number
- CN202411145773.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The existing electroless copper plating solution causes the plating to break or peel off under high stress, and the working temperature is high, the deposition speed is slow, and the stability is insufficient, which increases the cost.
The formulation of low-stress level electroless copper plating solution, including soluble copper salts, complexing agents, stabilizers, modification accelerators, surfactants and pH regulators, is adopted to adjust the pH value through the preparation of carbon nanotube modification accelerators. Reduce the internal stress of the copper plating layer, improve stability and deposition rate.
Significantly reduce the internal stress of the copper plating layer, improve the bonding force between the copper plating layer and the substrate, achieve low temperature and high speed deposition, extend the life of the plating solution, reduce costs, and enhance the stability and quality of the plating layer.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical copper plating, and in particular relates to a low-stress level chemical copper plating solution and a preparation method thereof. Background Art
[0002] Chemical copper plating is one of the key processes in the manufacturing of printed circuit boards (PCBs) and integrated circuit (IC) substrates. In recent years, various new materials such as high-frequency and high-speed PCB materials, IC substrate materials, and flexible circuit board substrates have continued to appear on the market, and the design of circuits and through and blind vias has become more complex, which has put forward higher requirements for chemical copper plating technology.
[0003] Stress refers to the internal force formed by the interaction of various parts of a material or object due to deformation caused by force or other external factors. It is a force that resists the influence of this external factor and attempts to restore the object from the position after deformation to the position before deformation. In chemical plating and other surface treatment processes, the issue of coating stress is involved. Chemical plating stress refers to the stress that exists inside the coating when there is no external load, which is generated by the unbalanced crystallization process during chemical deposition. The internal stress of chemical plating can be divided into the following two types. The first type is the stress that causes the volume of the chemical plating to shrink, which is called tensile stress; the second type is the stress generated by the volume expansion of the chemical plating itself, which is called compressive stress. If the tensile stress is too large during the chemical plating process, the deposited coating will directly break or crack. If the compressive stress is too large, it will directly cause the deposited coating to blister.
[0004] The stress of the coating often causes deformation of the substrate surface or cracks on the coating surface, and sometimes even causes the coating to completely peel off. The internal stress of the chemical coating has a significant effect on the bonding strength between the coating and the substrate. If the internal stress of the substrate is very high, using a coating with lower internal stress will help improve the bonding strength between them. Usually, in situations where there are special requirements for mechanical properties, the smaller the internal stress of the coating, the better.
[0005] Chinese patent CN113652676A discloses a low stress chemical copper plating solution, which includes the following components in terms of concentration: 1-20 g / L soluble copper salt, 1-50 g / L main complexing agent, 1-45 g / L auxiliary complexing agent, 1-30 g / L pH adjusting agent, 1-20 g / L reducing agent, 1×10 -3 ~3×10 -2 g / L composite stabilizer, 1×10 -3 ~2×10 -1 g / L composite surfactant, 1×10 -3 ~5×10 -1g / L stress reliever and 1-20g / L reaction accelerator; wherein the stress reliever is a composite of one or more of a soluble nickel salt and an azole compound; and the reaction accelerator is an organic acid containing a hydroxyl group. This invention solves the problems of high working temperature, slow deposition rate and large internal stress of traditional chemical copper plating solution. However, the working temperature of the copper plating solution of this patent is relatively high, and the maximum deposition rate can only be achieved at 48-50°C.
[0006] Chinese patent CN103014682A discloses a low-temperature, low-stress chemical copper plating solution, which mainly adds an accelerator, an inhibitor, nickel ions and an anionic surfactant to a basic system with copper sulfate as the main salt, potassium sodium tartrate tetrahydrate as a complexing agent, and formaldehyde or acetaldehyde as a reducing agent. It can achieve rapid deposition under low temperature conditions to form a chemical copper film coating with bright appearance, low stress, good quality and high bonding strength. However, the chemical copper plating solution is not stable enough. The plating solution will decompose after about 3 consecutive plating cycles, which increases the cost of low-stress chemical copper plating.
[0007] Therefore, it is of great significance to develop a horizontal chemical copper plating solution with good stability and effective in reducing the internal stress of the copper plating layer in the field. Summary of the invention
[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a low-stress level chemical copper plating solution and a preparation method thereof. The copper plating solution can significantly reduce the internal stress of the copper plating layer, effectively solving the problem of excessively high internal stress of the copper plating layer. At the same time, the copper plating solution has good stability and a low operating temperature. A high deposition rate can be achieved at 30-35°C, and the solution has good application prospects.
[0009] To achieve the above object, the present invention provides the following technical solutions:
[0010] A low stress level chemical copper plating solution comprises the following raw materials per liter: 7-15g of soluble copper salt, 10-30g of complexing agent, 0.01-0.03g of stabilizer, 4-8g of reducing agent, 0.05-0.1g of modification accelerator, 0.05-0.2g of surfactant, and the balance is water, and the pH value is adjusted to 10-12 by using a pH regulator.
[0011] Preferably, a low stress level chemical copper plating solution is composed of the following raw materials per liter: 9-13g of soluble copper salt, 15-25g of complexing agent, 0.015-0.025g of stabilizer, 5-7g of reducing agent, 0.07-0.09g of modification accelerator, 0.1-0.15g of surfactant, and the balance is water, and the pH is adjusted to 10-11 with a pH regulator.
[0012] More preferably, a low stress level chemical copper plating solution, each liter of chemical copper plating solution is composed of the following raw materials: 11g of soluble copper salt, 20g of complexing agent, 0.02g of stabilizer, 6g of reducing agent, 0.08g of modification accelerator, 0.13g of surfactant, and the balance is water, and the pH is adjusted to 11 with a pH adjuster.
[0013] Preferably, the soluble copper salt is one or more of copper sulfate pentahydrate, copper nitrate, and copper chloride; the complexing agent is one or more of tetrasodium diaminetetraacetic acid, potassium sodium tartrate, tetrahydroxypropylethylenediamine, and sodium citrate.
[0014] In the present invention, the addition of the complexing agent helps to enhance the stability of the solution, and can also refine the grains of the copper layer, make the plated film bright, and improve the performance of the chemical copper plating layer.
[0015] Preferably, the stabilizer is one or more of sodium thiosulfate, p-toluenesulfonamide, and thiourea; the reducing agent is one or more of formaldehyde, glyoxylic acid, and sodium hypophosphite; the pH adjuster is one or more of ammonia water, NaOH, and KOH; and the preparation method of the surfactant is as follows: add 10-15 parts of fatty alcohol polyoxyethylene ether OS-25 and 5-8 parts of sodium stearoyl lactylate to 35-45 parts of glycerol, stir and mix evenly, and obtain the surfactant.
[0016] In the present invention, the added stabilizer can improve the stability of the copper plating solution and increase the life of the copper plating solution. The stabilizer can cover the active nuclei appearing in the copper plating solution to prevent the active nuclei from continuing to grow and causing the decomposition of the copper plating solution, thereby achieving the purpose of stabilizing the copper plating solution. The added reducing agent has the function of reducing the copper ions in the solution into metallic copper. The added pH adjusting agent is used to adjust the pH range of the copper plating solution. Since hydrogen is generated during the chemical copper plating process, the pH value of the plating solution changes, so the pH adjusting agent must be used to maintain the pH of the plating solution. The added surfactant can reduce the surface tension of the plating solution and reduce the porosity of the plating layer. Other additives synergistically fill the micropores, timely eliminate the H2 generated during the chemical copper plating process, and reduce the hydrogen embrittlement phenomenon.
[0017] Preferably, the preparation method of the modified accelerator comprises the following steps:
[0018] S1, adding carbon nanotubes to a mixed solution of KMnO4 and nitric acid, stirring and impregnating, filtering, washing and drying after the impregnation is completed, to obtain pretreated carbon nanotubes; then adding the pretreated carbon nanotubes to an ethanol aqueous solution, and then adding γ-aminopropyltrimethoxysilane, stirring and reacting, filtering, washing and drying after the reaction is completed, to obtain amino carbon nanotubes;
[0019] S2, adding the aminated carbon nanotubes in step S1 into toluene, and then adding 2-chloro-4,6-diamino-1,3,5-triazine, and reacting at a constant temperature under a nitrogen atmosphere, adding ammonia water dropwise during the reaction to adjust the pH to 7-8, and filtering, washing, and drying after the reaction to obtain modified carbon nanotubes;
[0020] S3, adding the modified carbon nanotubes in step S2 into DMF, and then adding 6-(3-thienyl)pyridine-2-carboxaldehyde and triethylamine, heating and reacting under a nitrogen atmosphere, controlling the pH at 10-11 during the reaction, filtering, washing and drying after the reaction is completed, and obtaining the modified accelerator.
[0021] Preferably, the mass concentration of nitric acid in the mixed solution in step S1 is 10-20%, the mass fraction of KMnO4 is 3-6%, the temperature of the stirring and impregnation is 40-50°C, and the time is 1-2h; the mass ratio of the pretreated carbon nanotubes and γ-aminopropyltrimethoxysilane is 10:0.3-0.6, the temperature of the stirring reaction is 60-70°C, and the time is 2-4h.
[0022] In the present invention, carbon nanotubes are used as raw material carriers of accelerators. Carbon nanotubes have a large surface area and a special electronic structure that can provide active sites, which are helpful for adsorbing copper ions and promoting copper deposition of the coating. The carbon nanotubes are first oxidized in an acidification process to increase the active sites on their surfaces, and then reacted with γ-aminopropyltrimethoxysilane. On the one hand, the dispersibility of the carbon nanotubes can be improved, and on the other hand, amino groups can be introduced, which is beneficial to the subsequent reactions.
[0023] Preferably, in step S2, the mass ratio of the aminated carbon nanotubes to 2-chloro-4,6-diamino-1,3,5-triazine is 10:0.5-0.9, the temperature of the isothermal reaction is 105-120° C., and the time is 4-7 hours.
[0024] In the present invention, the amino groups on the carbon nanotubes react with the chlorine groups in 2-chloro-4,6-diamino-1,3,5-triazine to introduce triazine groups and amino groups into the carbon nanotubes, which can improve the bonding strength between the substrate and the chemically deposited copper film, and the heterocyclic groups in 2-chloro-4,6-diamino-1,3,5-triazine can improve the deposition rate of chemical copper plating, so that the copper plating solution has a higher copper plating rate even at low temperatures, thereby improving the reaction efficiency of the copper plating solution.
[0025] Preferably, in step S3, the mass ratio of the modified carbon nanotubes, 6-(3-thienyl)pyridine-2-carboxaldehyde and triethylamine is 10:0.1-0.3:3-4, and the heating reaction temperature is 70-50° C. and the reaction time is 3-6 h.
[0026] In the present invention, the modified carbon nanotubes are reacted with 6-(3-thienyl)pyridine-2-carboxaldehyde, and a Schiff base reaction occurs between the amino group and the aldehyde group, thereby introducing a thiophene group and a pyridine group on the carbon nanotubes. Both thiophene and pyridine have the ability to form a complex with copper ions, which can help stabilize the dissolved state of copper ions in the plating solution, and is beneficial to the transmission and deposition of copper ions; in the copper plating process, it can also promote the uniform growth of the copper plating layer, improve the quality of the plating layer, and thus reduce the internal stress of the plating layer.
[0027] The present invention also protects a method for preparing the low stress level chemical copper plating solution as described above, characterized in that it comprises the following steps:
[0028] The raw materials are weighed according to the formula, a complexing agent and a soluble copper salt are added into water, a surfactant and a stabilizer are added after stirring evenly, an accelerator and a reducing agent are modified after stirring evenly, a pH adjuster is added after stirring evenly, and the pH is adjusted to 10-12 to obtain the low stress level chemical copper plating solution.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The low stress level chemical copper plating solution provided by the present invention is prepared by specifically modifying carbon nanotubes to obtain a modified accelerator, which is then compounded with a complexing agent, a stabilizer, a reducing agent, and a surfactant in specific amounts, and finally the pH value of the copper plating solution is adjusted with a pH regulator, so that the prepared copper plating solution has good stability, a low operating temperature, and a high deposition rate, and at the same time significantly reduces the internal stress of the copper plating layer, and the copper plating layer has a high bonding force with the substrate, effectively solving the problem of the copper plating layer falling off due to excessive internal stress of the copper plating layer, thereby increasing the service life of the PCB board and having good application prospects.
[0031] (2) The low stress level chemical copper plating solution provided by the present invention contains a modified accelerator, and uses carbon nanotubes as a raw material carrier of the accelerator. The carbon nanotubes are first pretreated to improve their dispersibility and reactivity, and then 2-chloro-4,6-diamino-1,3,5-triazine is introduced into the carbon nanotubes, thereby improving the bonding strength between the substrate and the copper plating layer and the copper deposition efficiency of the chemical copper plating. Then, 6-(3-thienyl)pyridine-2-carboxaldehyde is introduced into the carbon nanotubes through a Schiff base reaction. The thienyl group and the pyridine group can stabilize the dissolved state of copper ions in the plating solution, which is beneficial to the transmission and deposition of copper ions. In the copper plating process, the uniform growth of the copper plating layer can be promoted, the quality of the plating layer can be improved, and thus the internal stress of the plating layer can be reduced. Moreover, the heterocyclic groups (triazine groups, thienyl groups, and pyridine groups) contained in the modified accelerator have strong adsorption for copper ions, which is beneficial to the merging and deposition of island grains in the plating layer, eliminating the pore defects on the plating layer, and further reducing the internal stress of the copper plating layer. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the present invention, the carbon nanotubes are purchased from Toray New Materials (Guangdong) Co., Ltd., with a tube diameter of 10-20 nm, a tube length of 2-8 μm, and a specific surface area of 270-310 m 2 / g.
[0034] Example 1
[0035] A low stress level chemical copper plating solution, each liter of the chemical copper plating solution is composed of the following raw materials: 11g of copper sulfate pentahydrate, 20g of tetrasodium diaminetetraacetate, 0.02g of sodium thiosulfate, 6g of formaldehyde, 0.08g of a modified accelerator, 0.13g of a surfactant, and the balance is water, and the pH value is adjusted to 11 with ammonia water with a mass concentration of 10%.
[0036] The preparation method of the surfactant is as follows: add 12g fatty alcohol polyoxyethylene ether OS-25 and 7g sodium stearoyl lactylate to 40g glycerol, stir and mix evenly, and obtain;
[0037] The preparation method of the modified accelerator comprises the following steps:
[0038] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 15%, and the mass fraction of KMnO4 is 5%), and stir and immerse at 45°C for 1.5 h. After immersion, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.5 g of γ-aminopropyltrimethoxysilane, and stir and react at 65°C for 3 h. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0039] S2, adding 10g of the amino-modified carbon nanotubes in step S1 to 400g of toluene, and then adding 0.7g of 2-chloro-4,6-diamino-1,3,5-triazine, and reacting at a constant temperature of 115°C for 5h under a nitrogen atmosphere, and adding ammonia water with a mass concentration of 10% every 0.5h during the reaction to adjust the pH to 7.5. After the reaction is completed, filtering, washing, and drying to obtain modified carbon nanotubes;
[0040] S3. Add 10 g of the modified carbon nanotubes in step S2 into 400 g of DMF, then add 0.2 g of 6-(3-thienyl)pyridine-2-carboxaldehyde and 3-4 g of triethylamine, react at 73 ° C for 5 h under a nitrogen atmosphere, control the pH at 11 during the reaction, filter, wash and dry after the reaction is completed to obtain the modified accelerator.
[0041] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding tetrasodium diaminetetraacetate and copper sulfate pentahydrate into water, stirring evenly, adding a surfactant and sodium thiosulfate, stirring evenly, modifying an accelerator and formaldehyde, stirring evenly, adding ammonia water with a mass concentration of 10%, adjusting the pH to 11, and obtaining the low-stress level chemical copper plating solution.
[0042] Example 2
[0043] The invention discloses a low stress level chemical copper plating solution. Each liter of the chemical copper plating solution is composed of the following raw materials: 10g of copper nitrate, 20g of potassium sodium tartrate, 0.02g of p-toluenesulfonamide, 6g of glyoxylic acid, 0.07g of a modified accelerator, 0.12g of a surfactant, and the balance is water. The pH value is adjusted to 11 by using a NaOH solution with a mass concentration of 10%.
[0044] The preparation method of the surfactant is as follows: add 13g fatty alcohol polyoxyethylene ether OS-25 and 6g sodium stearoyl lactylate to 40g glycerol, stir and mix evenly, and obtain;
[0045] The preparation method of the modified accelerator comprises the following steps:
[0046] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 15%, and the mass fraction of KMnO4 is 4%), and stir and immerse at 45°C for 1.5 h. After immersion, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.4 g of γ-aminopropyltrimethoxysilane, and stir and react at 65°C for 3 h. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0047] S2, adding 10g of the amino-modified carbon nanotubes in step S1 to 400g of toluene, and then adding 0.7g of 2-chloro-4,6-diamino-1,3,5-triazine, reacting at a constant temperature of 110°C for 6h under a nitrogen atmosphere, adding ammonia water with a mass concentration of 10% every 0.5h during the reaction to adjust the pH to 7.5, filtering, washing and drying after the reaction is completed to obtain modified carbon nanotubes;
[0048] S3. Add 10 g of the modified carbon nanotubes in step S2 into 400 g of DMF, then add 0.2 g of 6-(3-thienyl)pyridine-2-carboxaldehyde and 3-4 g of triethylamine, react at 73° C. for 4 h under a nitrogen atmosphere, control the pH at 10 during the reaction, filter, wash and dry after the reaction is completed to obtain the modified accelerator.
[0049] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding potassium sodium tartrate and copper nitrate into water, stirring evenly, adding a surfactant and p-toluenesulfonamide, stirring evenly, modifying an accelerator and glyoxylic acid, stirring evenly, adding a NaOH solution with a mass concentration of 10%, adjusting the pH to 11, and obtaining the low-stress level chemical copper plating solution.
[0050] Example 3
[0051] The invention discloses a low stress level chemical copper plating solution. Each liter of the chemical copper plating solution is composed of the following raw materials: 7g of cupric chloride, 10g of tetrahydroxypropylethylenediamine, 0.01g of thiourea, 4g of sodium hypophosphite, 0.05g of a modified accelerator, 0.2g of a surfactant, and the balance is water. The pH value is adjusted to 10 using a NaOH solution with a mass concentration of 10%.
[0052] The preparation method of the surfactant is as follows: add 10g fatty alcohol polyoxyethylene ether OS-25 and 8g sodium stearoyl lactylate to 35g glycerol, stir and mix evenly, and obtain;
[0053] The preparation method of the modified accelerator comprises the following steps:
[0054] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 10%, and the mass fraction of KMnO4 is 6%), and stir and immerse at 40°C for 2 h. After immersion, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.3 g of γ-aminopropyltrimethoxysilane, and stir and react at 60°C for 4 h. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0055] S2, adding 10g of the amino-modified carbon nanotubes in step S1 to 400g of toluene, and then adding 0.5g of 2-chloro-4,6-diamino-1,3,5-triazine, and reacting at 105°C for 7h under a nitrogen atmosphere, adding ammonia water with a mass concentration of 10% every 0.5h during the reaction to adjust the pH to 7, filtering, washing, and drying after the reaction is completed to obtain modified carbon nanotubes;
[0056] S3, adding 10g of modified carbon nanotubes in step S2 to 400g of DMF, followed by adding 0.1g of 6-(3-thienyl)pyridine-2-carboxaldehyde and 3g of triethylamine, reacting at 70°C for 6h under a nitrogen atmosphere, controlling the pH at 10 during the reaction, filtering, washing and drying after the reaction is completed to obtain the modified accelerator.
[0057] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding tetrahydroxypropylethylenediamine and cupric chloride into water, stirring evenly, adding a surfactant and thiourea, stirring evenly, modifying an accelerator and sodium hypophosphite, stirring evenly, adding a NaOH solution with a mass concentration of 10%, adjusting the pH to 10, and obtaining the low-stress level chemical copper plating solution.
[0058] Example 4
[0059] The invention discloses a low stress level chemical copper plating solution. Each liter of the chemical copper plating solution is composed of the following raw materials: 15g of copper sulfate pentahydrate, 30g of sodium citrate, 0.03g of sodium thiosulfate, 8g of formaldehyde, 0.1g of a modified accelerator, 0.2g of a surfactant, and the balance is water. The pH value is adjusted to 12 using a KOH solution with a mass concentration of 10%.
[0060] The preparation method of the surfactant is as follows: add 15g fatty alcohol polyoxyethylene ether OS-25 and 5g sodium stearoyl lactylate to 45g glycerol, stir and mix evenly, and obtain;
[0061] The preparation method of the modified accelerator comprises the following steps:
[0062] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 20%, and the mass fraction of KMnO4 is 3%), and stir and immerse at 50°C for 1 hour. After the immersion is completed, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.6 g of γ-aminopropyltrimethoxysilane, and stir and react at 70°C for 2 hours. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0063] S2, adding 10g of the amino-modified carbon nanotubes in step S1 to 400g of toluene, and then adding 0.9g of 2-chloro-4,6-diamino-1,3,5-triazine, and reacting at a constant temperature of 120°C for 4h under a nitrogen atmosphere, and adding ammonia water with a mass concentration of 10% every 0.5h during the reaction to adjust the pH to 8. After the reaction is completed, filtering, washing, and drying to obtain modified carbon nanotubes;
[0064] S3. Add 10 g of the modified carbon nanotubes in step S2 into 400 g of DMF, then add 0.3 g of 6-(3-thienyl)pyridine-2-carboxaldehyde and 4 g of triethylamine, and react at 75° C. for 3 h under a nitrogen atmosphere. During the reaction, control the pH at 11. After the reaction is completed, filter, wash, and dry to obtain the modified accelerator.
[0065] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding sodium citrate and copper sulfate pentahydrate into water, stirring evenly, adding a surfactant and sodium thiosulfate, stirring evenly, modifying an accelerator and formaldehyde, stirring evenly, adding a KOH solution with a mass concentration of 10%, adjusting the pH to 12, and obtaining the low-stress level chemical copper plating solution.
[0066] Comparative Example 1
[0067] A low stress level chemical copper plating solution, each liter of the chemical copper plating solution is composed of the following raw materials: 11g of copper sulfate pentahydrate, 20g of tetrasodium diaminetetraacetate, 0.02g of sodium thiosulfate, 6g of formaldehyde, 0.08g of a modified accelerator, 0.13g of a surfactant, and the balance is water, and the pH value is adjusted to 11 with ammonia water with a mass concentration of 10%.
[0068] The preparation method of the surfactant is as follows: add 12g fatty alcohol polyoxyethylene ether OS-25 and 7g sodium stearoyl lactylate to 40g glycerol, stir and mix evenly, and obtain;
[0069] The preparation method of the modified accelerator comprises the following steps:
[0070] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 15%, and the mass fraction of KMnO4 is 5%), and stir and immerse at 45°C for 1.5 h. After immersion, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.5 g of γ-aminopropyltrimethoxysilane, and stir and react at 65°C for 3 h. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0071] S2. Add 10 g of the amino-modified carbon nanotubes in step S1 into 400 g of toluene, and then add 0.7 g of 2-chloro-4,6-diamino-1,3,5-triazine. In a nitrogen atmosphere, react at a constant temperature of 115° C. for 5 h. During the reaction, add 10% ammonia water every 0.5 h to adjust the pH to 7.5. After the reaction is completed, filter, wash and dry to obtain the modified accelerator.
[0072] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding tetrasodium diaminetetraacetate and copper sulfate pentahydrate into water, stirring evenly, adding a surfactant and sodium thiosulfate, stirring evenly, modifying an accelerator and formaldehyde, stirring evenly, adding ammonia water with a mass concentration of 10%, adjusting the pH to 11, and obtaining the low-stress level chemical copper plating solution.
[0073] Comparative Example 2
[0074] A low stress level chemical copper plating solution, each liter of the chemical copper plating solution is composed of the following raw materials: 11g of copper sulfate pentahydrate, 20g of tetrasodium diaminetetraacetate, 0.02g of sodium thiosulfate, 6g of formaldehyde, 0.08g of a modified accelerator, 0.13g of a surfactant, and the balance is water, and the pH value is adjusted to 11 with ammonia water with a mass concentration of 10%.
[0075] The preparation method of the surfactant is as follows: add 12g fatty alcohol polyoxyethylene ether OS-25 and 7g sodium stearoyl lactylate to 40g glycerol, stir and mix evenly, and obtain;
[0076] The preparation method of the modified accelerator comprises the following steps:
[0077] S1. Add 10 g of carbon nanotubes to a mixed solution of 200 g of KMnO4 and nitric acid (the mass concentration of nitric acid is 15%, and the mass fraction of KMnO4 is 5%), and stir and immerse at 45°C for 1.5 h. After immersion, filter, wash, and dry to obtain pretreated carbon nanotubes; then add 10 g of pretreated carbon nanotubes to 300 g of ethanol aqueous solution (the volume ratio of ethanol to water is 8:2), and then add 0.5 g of γ-aminopropyltrimethoxysilane, and stir and react at 65°C for 3 h. After the reaction is completed, filter, wash, and dry to obtain amino carbon nanotubes;
[0078] S2. Add 10 g of the amino-modified carbon nanotubes in step S1 to 400 g of DMF, then add 0.2 g of 6-(3-thienyl)pyridine-2-carboxaldehyde and 3-4 g of triethylamine, and react at 73° C. for 5 h under a nitrogen atmosphere. During the reaction, control the pH at 11. After the reaction is completed, filter, wash, and dry to obtain the modified accelerator.
[0079] A method for preparing a low-stress level chemical copper plating solution comprises the following steps: weighing raw materials according to a formula, adding tetrasodium diaminetetraacetate and copper sulfate pentahydrate into water, stirring evenly, adding a surfactant and sodium thiosulfate, stirring evenly, modifying an accelerator and formaldehyde, stirring evenly, adding ammonia water with a mass concentration of 10%, adjusting the pH to 11, and obtaining the low-stress level chemical copper plating solution.
[0080] The copper plating solutions prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, as follows:
[0081] Deposition speed: The PCB drilling panel was cut into 5 cm × 5 cm samples for horizontal copper deposition, and the process was: degreasing and adjustment (50 ° C, 5 minutes); micro-etching (room temperature, 2 minutes); pre-immersion (room temperature, 1 minute); activation (30 ° C, 10 minutes); acceleration (room temperature, 5 minutes); chemical copper deposition (33 ° C, 20 minutes, copper plating solution prepared in Example 1-4 and Comparative Example 1-2). After the copper deposition was completed, the PCB board was taken out, rinsed with distilled water, and blown dry. The deposition speed was calculated according to the following formula:
[0082] ν=
[0083] Where ν is the deposition rate in μm / hour, is the mass of the PCB board before chemical copper plating (g), is the mass of the PCB board after chemical copper plating (g), and ρ is the density of copper (8.9 g / cm 3 ), s is the area of the PCB board (m 2 ), t is the time of chemical copper plating (h).
[0084] Copper layer stress: The stress of the copper film on the copper-plated PCB board was measured by X-ray diffraction. The stress operating conditions of the X-ray diffractometer were as follows: Cu-Ka target, wavelength of 1.5406nm, tube voltage of 40kV, tube current of 40mA, graphite filter monochromator, scanning range of 40°-100°, scanning speed of 4° / min, step size of 0.1°, and stress calculation method of chemical copper layer was X-ray diffraction 2θΨ-sin 2 The Ψ method uses X-rays to irradiate the surface of chemical copper-plated PCB samples at different incident angles (Ψ) in sequence, accurately measuring the diffraction angle (2θ) corresponding to the incident angle, and obtaining the 2θ to sin 2 The present invention selects the Cu(311) crystal plane to measure the stress of the chemically plated copper film, and calculates the stress of the copper-plated layer according to the following formula:
[0085] σ=
[0086] Where σ is the stress on the surface of the tested copper film, E is the Young's modulus of copper (119×10 3 MPa), v is Poisson's ratio (0.34), θ: diffraction angle of copper layer in stress-free state, Ψ is different incident angles when testing XRD, 2θ Ψ is the corresponding diffraction angle at different incident angles.
[0087] Bonding strength: The bonding strength between the chemical copper film and the substrate is measured by the 90° bonding strength test method. This method is suitable for quantitative testing of bonding strength. Before the bonding strength test, the chemical copper film should be electroplated to thicken it, and then two parallel scratches with a spacing of 1 cm are made on the electroplated copper PCB with a knife. The scratches must be deep enough to expose the substrate. Finally, an ordinary dynamometer is used to test the bonding strength between the scratched copper layer and the substrate (unit: kN·m -1 ), the electroplating process was carried out at room temperature, and the current density was 0.03A·cm -2 , the electroplating time is 1h, and the copper layer thickness is about 20μm. The test results are shown in Table 1:
[0088] Table 1
[0089] Deposition rate (μm / h) Stressσ(MPa) <![CDATA[Bond strength (kN·m -1 )]]> Example 1 7.08 12.6 1.37 Example 2 6.94 13.1 1.32 Example 3 6.63 16.8 1.21 Example 4 6.97 14.3 1.29 Comparative Example 1 6.05 39.2 1.04 Comparative Example 2 5.36 31.8 0.96
[0090] From Table 1 above, it can be seen that the low stress level chemical copper plating solution prepared by the present invention has a low working temperature, and can achieve a high deposition rate at 30-35°C. At the same time, it can also significantly reduce the stress of the plated copper and improve the bonding strength between the plated copper and the substrate, and has good application prospects.
[0091] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A low stress level chemical copper plating solution, characterized in that: Each liter of chemical copper plating solution is composed of the following raw materials: 7-15g of soluble copper salt, 10-30g of complexing agent, 0.01-0.03g of stabilizer, 4-8g of reducing agent, 0.05-0.1g of modification accelerator, 0.05-0.2g of surfactant, and the balance is water, and the pH is adjusted to 10-12 with a pH regulator.
2. The low stress level chemical copper plating solution according to claim 1, characterized in that: Each liter of chemical copper plating solution is composed of the following raw materials: 9-13g of soluble copper salt, 15-25g of complexing agent, 0.015-0.025g of stabilizer, 5-7g of reducing agent, 0.07-0.09g of modification accelerator, 0.1-0.15g of surfactant, and the balance is water, and the pH is adjusted to 10-11 with a pH regulator.
3. The low stress level chemical copper plating solution according to claim 1, characterized in that: Each liter of chemical copper plating solution is composed of the following raw materials: 11g of soluble copper salt, 20g of complexing agent, 0.02g of stabilizer, 6g of reducing agent, 0.08g of modification accelerator, 0.13g of surfactant, and the balance is water, and the pH is adjusted to 11 with a pH regulator.
4. The low stress level chemical copper plating solution according to claim 1, characterized in that: The soluble copper salt is one or more of copper sulfate pentahydrate, copper nitrate, and copper chloride; the complexing agent is one or more of tetrasodium diaminetetraacetate, potassium sodium tartrate, tetrahydroxypropylethylenediamine, and sodium citrate.
5. The low stress level chemical copper plating solution according to claim 1, characterized in that: The stabilizer is one or more of sodium thiosulfate, p-toluenesulfonamide, and thiourea; the reducing agent is one or more of formaldehyde, glyoxylic acid, and sodium hypophosphite; the pH adjuster is one or more of ammonia water, NaOH, and KOH; the preparation method of the surfactant is as follows: add 10-15 parts of fatty alcohol polyoxyethylene ether OS-25 and 5-8 parts of sodium stearoyl lactylate to 35-45 parts of glycerol, stir and mix evenly, and obtain the surfactant.
6. The low stress level chemical copper plating solution according to claim 1, characterized in that: The preparation method of the modified accelerator comprises the following steps: S1, adding carbon nanotubes to a mixed solution of KMnO4 and nitric acid, stirring and impregnating, filtering, washing and drying after the impregnation is completed, to obtain pretreated carbon nanotubes; then adding the pretreated carbon nanotubes to an ethanol aqueous solution, and then adding γ-aminopropyltrimethoxysilane, stirring and reacting, filtering, washing and drying after the reaction is completed, to obtain amino carbon nanotubes; S2, adding the aminated carbon nanotubes in step S1 into toluene, and then adding 2-chloro-4,6-diamino-1,3,5-triazine, and reacting at a constant temperature under a nitrogen atmosphere, adding ammonia water dropwise during the reaction to adjust the pH to 7-8, and filtering, washing, and drying after the reaction to obtain modified carbon nanotubes; S3, adding the modified carbon nanotubes in step S2 into DMF, and then adding 6-(3-thienyl)pyridine-2-carboxaldehyde and triethylamine, heating and reacting under a nitrogen atmosphere, controlling the pH at 10-11 during the reaction, filtering, washing and drying after the reaction is completed, and obtaining the modified accelerator.
7. The low stress level chemical copper plating solution according to claim 6, characterized in that: The mass concentration of nitric acid in the mixed solution in step S1 is 10-20%, the mass fraction of KMnO4 is 3-6%, the temperature of the stirring and immersion is 40-50°C, and the time is 1-2h; the mass ratio of the pretreated carbon nanotubes and γ-aminopropyltrimethoxysilane is 10:0.3-0.6, the temperature of the stirring reaction is 60-70°C, and the time is 2-4h.
8. The low stress level chemical copper plating solution according to claim 6, characterized in that: In step S2, the mass ratio of the aminated carbon nanotubes to 2-chloro-4,6-diamino-1,3,5-triazine is 10:0.5-0.9, the temperature of the isothermal reaction is 105-120° C., and the time is 4-7 hours.
9. The low stress level chemical copper plating solution according to claim 6, characterized in that: In step S3, the mass ratio of the modified carbon nanotubes, 6-(3-thienyl)pyridine-2-carboxaldehyde and triethylamine is 10:0.1-0.3:3-4, the temperature of the heating reaction is 70-50° C., and the time is 3-6 hours.
10. A method for preparing a low stress level chemical copper plating solution according to any one of claims 1 to 9, characterized in that: The following steps are involved: The raw materials are weighed according to the formula, a complexing agent and a soluble copper salt are added into water, a surfactant and a stabilizer are added after stirring evenly, an accelerator and a reducing agent are modified after stirring evenly, a pH adjuster is added after stirring evenly, and the pH is adjusted to 10-12 to obtain the low stress level chemical copper plating solution.
Citation Information
Patent Citations
Low-temperature low-stress electroless copper plating solution
CN103014682A
Low-stress chemical copper plating solution and preparation method thereof
CN113652676A
Cited By
Chemical copper plating solution beneficial to improving surface roughness, production process and application
CN119876922A
Electroless copper plating solution, production process and application for improving surface roughness
CN119876922B