Conductive carbon particles with excellent corrosion resistance

A multilayered structure on carbon-based particles with silver oxide, copper, and nickel/silver layers addresses bonding and conductivity issues, providing cost-effective and reliable conductive particles for electronic components.

JP2024538756AActive Publication Date: 2024-10-23C&C MATERIALS CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024521761
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-08
Publication Date
2024-10-23
Estimated Expiration
2041-10-08

AI Technical Summary

Technical Problem

Conductive metal particles face challenges in maintaining uniform size and sphericity, leading to non-uniform film or adhesive layers with poor contact properties, while carbon-based particles have lower electrical conductivity and bonding issues with metal layers, and conventional methods using palladium catalysts are costly.

Method used

A multilayer structure is formed on carbon-based particles, starting with a silver oxide layer, followed by copper and optionally nickel or silver layers, to enhance bonding strength, electrical conductivity, and corrosion resistance, using a method that avoids palladium catalysts.

Benefits of technology

The resulting conductive carbon-based particles offer excellent electrical conductivity, corrosion resistance, and bonding strength at a lower cost, enabling reliable and lightweight applications in electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538756000001_ABST
    Figure 2024538756000001_ABST
Patent Text Reader

Abstract

The present invention aims to provide conductive carbon-based particles having a metal layer formed on the surface thereof, which has excellent electrical conductivity, corrosion resistance, and bonding strength with carbon-based particles. In order to achieve the above-mentioned object, the present invention can provide conductive carbon-based particles including a first layer containing silver oxide formed on the surface of the carbon-based particle, a second layer containing copper formed on the first layer, and a third layer containing nickel or silver formed on the second layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to conductive carbon-based particles having a conductive metal coating layer, and in particular to conductive carbon-based particles having a multilayer structure and excellent corrosion resistance, in which a copper metal layer is formed on the surface without an expensive palladium catalyst layer, and a nickel or silver coating layer is further formed to protect the copper metal layer, and a method for producing the same. [Background technology]

[0002] Conductive particles are widely used in electronic materials. Among them, metal particles such as copper or nickel have high conductivity and are highly cost competitive, so they are used in a variety of applications that require electrical conductivity, such as films, adhesives, and coating slurries in various electronic components.

[0003] However, it is difficult to produce particles of various sizes during the synthesis process, and it is difficult to maintain uniform particle size and spherical shape between particles, so when producing a conductive film or adhesive, it is difficult to produce a film or adhesive layer of uniform thickness and to maintain uniform contact characteristics. In addition, to compensate for poor contact characteristics, metal particles are added in large volumes to the film or adhesive, but the high volume ratio of these metal particles can cause problems such as making the film or adhesive layer heavy and weakening the adhesive strength.

[0004] On the other hand, carbon-based particles, which have low density, excellent chemical resistance, and a certain level of electrical conductivity, are also widely used as conductive materials, and examples of carbon-based particles include graphite particles, graphene particles, CNT particles, etc. However, films or adhesive layers made of these carbon-based particles still have the problem of lower electrical conductivity than metal particles.

[0005] To overcome this problem, it is necessary to apply conductive carbon-based particles in which a conductive metal layer such as copper, nickel, silver, or gold is formed on the surface of carbon-based particles such as graphite, graphene, and CNTs, which have low density and excellent chemical resistance.

[0006] However, the carbon-based particles as the base material and the metal layer are different materials, and it is difficult to maintain the bonding strength. In general, in order to form a metal coating layer on the surface of a different material such as a carbon-based material or a ceramic, a method of forming a catalyst layer using palladium and then forming a metal layer is widely used, but palladium is too expensive, which increases the process cost.

[0007] Meanwhile, the metal layer coated on the surface of the carbon-based particles can be made of various metals, but copper has excellent electrical conductivity close to that of silver but has the problem of being easily oxidized, nickel has excellent corrosion resistance and is advantageous in terms of long-term reliability but has the problem of low electrical conductivity, and another metal, silver (Ag), has both excellent electrical conductivity and corrosion resistance but has the problem of being too expensive.

[0008] Thus, it is difficult for the metal layer formed on the surface of the carbon-based particle to satisfy all of the desired qualities. Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide conductive carbon-based particles having a metal layer formed on the surface thereof, which metal layer has excellent electrical conductivity, corrosion resistance, and bonding strength with carbon-based particles.

[0010] Yet another object of the present invention is to provide a method for producing conductive carbon-based particles, which can inexpensively form a metal layer on the surface of the conductive carbon-based particles, the metal layer having excellent electrical conductivity, corrosion resistance, and bonding strength with the carbon-based particles. [Means for solving the problem]

[0011] In order to achieve the above object, the present invention can provide conductive carbon-based particles including a first layer containing silver oxide formed on the surface of carbon-based particles, a second layer formed on the first layer and containing copper, and a third layer formed on the second layer and containing nickel or silver.

[0012] Further, the carbon-based particles may be one or more selected from the group consisting of graphite, graphene, and CNT.

[0013] Further, the first layer further contains metallic silver, and the molar ratio (Ag x+ / Ag 0 (0 < x ≤ 3)) of silver element in the silver oxide to silver element in the metallic silver may be in the range of 1 to 20.

[0014] Further, the first layer may further contain tin.

[0015] Further, the content of silver contained in the first layer may be 10 to 1,000 ppm of the total weight of the conductive carbon-based particles.

[0016] Further, the third layer may further contain phosphorus together with the nickel.

[0017] Further, the third layer may contain 0.1 to 13.0% by weight of phosphorus.

[0018] The method for manufacturing conductive carbon-based particles according to the present invention may include: (a) a hydrophilization step of hydrophilizing the surface of carbon-based particles; (b) a first layer formation step of coating silver oxide on the hydrophilized carbon-based particles; (c) a second layer formation step of electroless plating copper on the first layer; and (d) a third layer formation step of electroless plating nickel or silver on the second layer.

[0019] Further, between the steps (a) and (b), a step of forming a tin layer may be further included.

[0020] In addition, after the step (b) and before the step (c), a post-treatment step of stirring the carbon-based particles on which the first layer has been formed in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of silver oxide may be further included. Effect of the Invention

[0021] The conductive carbon-based particles according to the present invention are inexpensive, have excellent electrical conductivity and corrosion resistance, and can be applied to various electronic components that require electrical conductivity. They also have excellent bonding strength of the surface metal layer, making it possible to achieve weight reduction and improved electrical conductivity and reliability of the components to which they are applied.

[0022] In addition, the method for producing conductive carbon-based particles provided by the present invention enables mass production of conductive carbon-based particles with excellent conductivity and reliability through a low-cost process. [Brief description of the drawings]

[0023] [Figure 1] 1 is a scanning electron microscope image of conductive carbon-based particles according to an embodiment and a comparative example of the present invention. [Diagram 2] FIG. 2 is a diagram showing an analysis result by X-ray Photoelectron Spectroscopy (XPS) for conductive carbon-based particles in one embodiment according to the present invention.

[0024] BEST MODE FOR CARRYING OUT THEINVENTION Hereinafter, the configuration and operation of the embodiment of the present invention will be described with reference to the accompanying drawings. In the following, when a specific description of a related known function or configuration is determined to make the gist of the present invention unclear, the detailed description will be omitted. In addition, when a certain part is described as "including" a certain component, this does not mean that other components are excluded, but that other components may be further included, unless otherwise specified.

[0025] Although carbon-based particles have the advantages of excellent chemical resistance and low density, they have limitations in terms of their use as conductive particles due to their low electrical conductivity. To overcome this, a conductive metal layer can be formed on the surface of carbon-based particles of various shapes and sizes to provide electrical conductivity.

[0026] However, since carbon and metal are different materials and their adhesive strength is very low, it is very difficult to form a metal layer on the surface of carbon-based particles. In order to overcome this, a method of forming an intermediate layer that facilitates adhesion between a metal layer that provides conductivity and carbon-based particles has been used, and a catalyst layer containing palladium was formed as this intermediate layer. These palladium catalyst layers led to the smooth formation of metal layers such as copper, nickel, and silver. However, as is well known, palladium is an expensive precious metal and has recently become more expensive than gold, so there is a problem that the process costs are too high to produce using palladium.

[0027] In order to solve such problems, the inventors of the present invention have investigated an intermediate layer that is less expensive than palladium and can provide sufficient bonding strength with the surface of carbon-based particles. Silver oxide is an oxide that can be smoothly adhered to the surface of carbon-based particles and is known to have excellent bonding strength with metals, so they developed a technology to form an intermediate layer and then form a metal coating layer.

[0028] As a result, it was found that when an intermediate layer of silver oxide alone or a composite of silver oxide and silver metal was formed, the metal layer formed subsequently could be strongly bonded to the carbon-based particles, exhibiting a bonding strength equal to or greater than that when a conventional layer containing palladium was used.

[0029] Meanwhile, the characteristics of the conductive carbon-based particles are determined by the type of metal layer formed on the surface of the carbon-based particles. Copper has excellent electrical conductivity, but is easily oxidized, which makes reliability a problem. Nickel, on the other hand, has excellent corrosion resistance, but has a problem of lower electrical conductivity than copper. Silver has both excellent corrosion resistance and electrical conductivity, but is expensive. As such, it is difficult to meet all of the characteristics required by industry with only one type.

[0030] In order to overcome such problems, the inventors of the present invention have invented conductive carbon-based particles having a multi-layered metal layer formed on the surface thereof by first forming a copper metal layer, and then forming a nickel or silver metal layer on the copper metal layer to protect the copper metal layer.

[0031] As a result, the present invention can provide conductive carbon-based particles comprising a first layer containing silver oxide formed on the surface of a carbon-based particle, a second layer containing copper formed on the first layer, and a third layer containing nickel or silver formed on the second layer.

[0032] The carbon-based particles constituting the core of the conductive carbon-based particle may be one or more types selected from the group consisting of graphite, graphene, and CNT.

[0033] Conductive carbon particles have low density, excellent chemical resistance, and can have various particle sizes, which is advantageous for application to various electronic components. For this reason, the carbon particles constituting the core are preferably graphite, graphene, or CNT, and since products with various properties are commercially available, it is possible to manufacture various conductive carbon particle products by using these. In particular, graphite is commercially available in various particle sizes and shapes depending on the type, such as artificial graphite and natural graphite, and has various properties and unit prices, which allows for various products and applications.

[0034] As described above, due to the characteristics of the carbon-based particles, the surface thereof is difficult to easily bond with the metal layer. In order to modify the characteristics of these surfaces, it is necessary to form a catalyst layer. In the present invention, instead of the conventional catalyst layer containing palladium, a first layer which is a catalyst layer containing silver oxide is formed first. Since silver oxide is excellent in bonding not only with carbon but also with metals, the bond between the carbon-based particles constituting the core and the surface metal layer can be strongly maintained.

[0035] In the present invention, the first layer containing silver oxide may further contain tin. Tin is an element used to guide the smooth adhesion of silver oxide to the surface of the carbon-based particles. When performing the coating operation with an aqueous solution, it imparts hydrophilicity to the surface of the carbon-based particles and helps the adhesion of silver elements to the surface of the carbon-based particles. These tins can also constitute the first layer together with silver oxide, or may be formed between the first layer containing silver oxide and the surface of the carbon-based particles.

[0036] In the present invention, the first layer containing silver oxide may further contain metallic silver together with silver oxide. When metallic silver is further contained, the bond with copper which is the metal contained in the second layer can be further strengthened. Silver oxide strengthens the bond with the carbon-based particles, and metallic silver strongly bonds with these silver oxides and provides a strong bond with copper which is the same metal. As a result, the bonding force between the second layer containing copper and the carbon-based particles is further strengthened.

[0037] At this time, the molar ratio of silver element in silver oxide to silver element in metallic silver in the first layer (Ag x+ / Ag 0 (0 < x ≦ 3)) is preferably in the range of 1 to 20.

[0038] As described above, the inclusion of metallic silver strengthens the bond between the first layer containing silver oxide and the second layer containing copper, but if the proportion of silver element in metallic silver is too high compared to that of silver element in silver oxide, the bonding strength of the silver oxide with the surface of the carbon-based particle of the first layer decreases accordingly, which is not preferable. Therefore, the molar ratio of silver element in metallic silver to silver element in silver oxide is preferably 1 to 20, more preferably 1 to 10, so that the proportion of silver element in silver oxide is even higher. These molar ratios can be measured by X-ray photoelectron spectroscopy (XPS).

[0039] Here, the oxidation number of silver in silver oxide can range from +1 to +3, and since the oxidation number does not have to be a constant in the amorphous phase, the oxidation number of silver in silver oxide may be greater than 0 and less than or equal to 3.

[0040] The first layer may further contain palladium, and the inclusion of palladium can further strengthen the bond between the surface of the carbon-based particle and the silver oxide and the bond between the second layer. The amount of palladium contained in this case can be even less than that contained in conventional conductive carbon-based particles without silver oxide. For example, the amount of palladium used in the manufacturing process of conventional conductive carbon-based particles is generally in the range of 100 to 1,000 ppm based on the conductive carbon-based particles, but the conductive carbon-based particles according to the present invention can use an amount of palladium greater than 0 and less than 50 ppm.

[0041] The content of silver in the first layer may be 10 to 1,000 ppm based on the total weight of the conductive carbon-based particles.

[0042] The metallic silver or silver oxide formed in the first layer can provide a satisfactory bonding strength to the second layer only if it is at a certain content or more, and if it is too much, the process cost increases, which is not preferable. More preferably, it may be 10 to 500 ppm.

[0043] The first layer in the present invention may be in the form of islands discontinuously formed on the surface of the carbon-based particle. The first layer is a layer that strengthens the bonding force between the carbon-based particle and the second layer that imparts electrical conductivity, and even if the first layer is in the form of discontinuous islands, it can provide sufficient bonding force to the second layer.

[0044] Meanwhile, the first layer may be in the form of a continuous film, in which case the first layer occupies at least 50% or more of the surface area of ​​the carbon-based particle, because even if it is in the form of a continuous film, it must occupy at least 50% or more of the surface area of ​​the particle in order to provide sufficient binding strength to the second layer.

[0045] A second layer containing copper, a metal with excellent electrical conductivity, is formed on the first layer containing silver oxide. Copper, among metals, has particularly excellent electrical conductivity, which allows the conductive carbon particles to have excellent electrical conductivity.

[0046] The copper-containing second layer may be 5 to 40% by weight of the entire conductive carbon-based particle, but if it is less than 5% by weight, the electrical conductivity may decrease, and if it exceeds 40% by weight, the density of the entire conductive carbon-based particle increases, which is not preferable, and the risk of the second layer falling off increases. Therefore, the content of the second layer in the conductive carbon-based particle is preferably 5 to 30% by weight, more preferably 8 to 20% by weight.

[0047] On the other hand, in the present invention, the copper content in the copper-containing second layer is 90% by weight or more. If the copper content is less than 90% by weight, the electrical conductivity of the second layer decreases.

[0048] In the present invention, a third layer containing nickel or silver may be further formed on the second layer containing copper.

[0049] The third layer, containing nickel or silver, prevents the metallic copper formed in the second layer from oxidizing and has excellent electrical conductivity, ultimately enabling the conductive carbon-based particles to ensure both electrical conductivity and reliability.

[0050] When a third layer, a metal layer containing nickel, which has excellent corrosion resistance, is formed, it protects the second layer while the formation of metallic nickel ensures a certain level of electrical conductivity.

[0051] These third layers may contain not only nickel but also phosphorus, but since the inclusion of phosphorus improves chemical resistance and oxidation resistance, although the electrical conductivity is somewhat reduced, it is preferable for the third layer to contain phosphorus in addition to nickel when used in parts where reliability is important. If phosphorus is contained, the phosphorus content in the third layer is preferably 0.1 to 13.0 wt %, but if it is too low, the desired chemical resistance and oxidation resistance will not be improved, and if the phosphorus content exceeds 13 wt %, sufficient electrical conductivity cannot be obtained. More preferably, the phosphorus content is 0.5 to 6 wt %.

[0052] Meanwhile, the third layer may contain metallic silver other than nickel, but silver is an ideal metal in terms of properties, as it is both corrosion-resistant and has excellent electrical conductivity, but it has the disadvantage of being expensive. Therefore, in terms of electrical conductivity, if the second layer is made of copper, which has the same level of electrical conductivity as silver, and the third layer is made of silver, which protects the copper and has excellent electrical conductivity, it is possible to minimize the amount of silver used, ensure reliability, and maximize the electrical conductivity of the conductive carbon-based particles.

[0053] The present invention can also provide a method for producing conductive carbon-based particles, the method including: (a) a hydrophilization step of hydrophilizing the surfaces of carbon-based particles; (b) a first layer formation step of coating the hydrophilized surfaces of the carbon-based particles with silver oxide; (c) a second layer formation step of electrolessly plating copper onto the first layer; and (d) a third layer formation step of electrolessly plating nickel or silver onto the second layer.

[0054] To produce conductive carbon-based particles, a hydrophilization step is first required to introduce chemical functional groups to the surface of the carbon-based particles to make them hydrophilic. This hydrophilization step may consist of a strong acid solution of pH 3 or less. This is because the strong acid solution can partially cleave the carbon bonds on the surface of the carbon-based particles, facilitating the attachment of chemical functional groups to the surface of the carbon-based particles. Therefore, in order to treat the surface of a stable carbon-based particle, a strong acid atmosphere of pH 3 or less made by an inorganic acid such as sulfuric acid, nitric acid, or hydrochloric acid is preferred.

[0055] On the other hand, the hydrophilization treatment of carbon-based particles can be carried out in a strong acid aqueous solution as described above, but the hydrophilization can also be carried out in a dry manner by modifying the surface of the carbon-based particles by plasma treatment.

[0056] After the hydrophilization treatment, a first layer containing silver oxide is formed, and tin can be coated together with the silver oxide. Tin can increase the binding force of silver oxide on the surface of the hydrophilized carbon-based particles.

[0057] For more precise control, a tin layer can be formed first on the surface of the hydrophilized carbon-based particles, followed by the formation of a first layer containing silver oxide.

[0058] The first layer containing silver oxide can be formed using an alkaline aqueous solution having a pH of 8 or higher. This is because silver oxide is well formed in an alkaline atmosphere having a pH of 8 or higher. More preferably, the first layer can be formed using an aqueous solution having a pH in the range of 9 to 11.

[0059] In addition, the method for producing conductive carbon-based particles may further include, after step (b) and before step (c), a post-treatment step of stirring the carbon-based particles on which the first layer has been formed in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of silver oxide.

[0060] When the first layer is formed in an aqueous solution, silver ions in the aqueous solution may be reduced and attached to the surface of the carbon-based particles as metallic silver, not silver oxide. If the proportion of metallic silver becomes too high, the binding strength between the carbon-based particles and the first layer may be reduced, which is not preferable. Therefore, in order to increase the content of silver oxide to a desired level, the amount of silver oxide can be adjusted by treating with an alkaline aqueous solution at an appropriate temperature.

[0061] In this way, by adjusting the amount of silver oxide and then forming a second layer containing conductive copper, it is possible to provide conductive carbon-based particles that have excellent bonding strength between the metal coating layer that imparts conductivity and the carbon-based particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0062] In order to fully understand the present invention, preferred embodiments of the present invention will now be described with reference to the accompanying drawings.

[0063] The examples of the present invention are provided to more completely explain the present invention to those skilled in the art, and the following examples can be modified in various different forms, and the scope of the present invention is not limited to the following examples. Rather, these examples are provided to make the present disclosure more complete and complete, and to fully convey the idea of ​​the present invention to those skilled in the art.

[0064] [Example 1] 3 g of hydrochloric acid (35% solution) was added to 100 g of deionized water and heated to 60°C. 50 10 g of graphite with a particle size of 20 μm was added and stirred for 10 hours to hydrophilize the surface of the graphite powder. The hydrophilized graphite powder was then collected, stirred with 100 g of deionized water, washed three times, and then collected.

[0065] The collected graphite particles were added to an aqueous solution of 100 g of deionized water, 1.5 g of stannous chloride (SnCl2·2H2O) and 6 ml of hydrochloric acid (35% solution), and stirred for 30 minutes to form a tin layer. The temperature of the aqueous solution was maintained at 35°C.

[0066] The graphite particles with the tin layer formed were collected by filtering, and then added to a silver nitrate solution prepared by dissolving 0.15g of silver nitrate (AgNO3) in 100g of deionized water and stirring it. At this time, 28% ammonia water was added dropwise to adjust the pH to 9.3.

[0067] The temperature was maintained at 40°C and the mixture was stirred for 1 hour to form a silver oxide layer. After 1 hour, the mixture was filtered and collected, then stirred with 200 g of deionized water, washed three times, and collected. A portion of the powder on which the silver oxide layer was formed was sampled and subjected to surface analysis by X-ray photoelectron spectroscopy (XPS).

[0068] The powder with the silver oxide layer was collected, and a copper coating layer was formed by electroless plating. A copper sulfate complex solution was prepared by adding 40g of EDTA (Ethylene-diamine-tetraacetic acid), 30g of NaOH, and 20g of copper sulfate to 300g of deionized water, and the graphite powder with the silver oxide layer was added. While stirring, a formaldehyde solution was dripped as a reducing agent to form a copper-containing coating layer.

[0069] A nickel coating layer was further formed on the graphite powder with the copper coating layer formed. For this purpose, 20g of nickel chloride (NiCl2·6H2O), 10g of sodium acetate, 5g of maleic acid, 30g of sodium hypophosphite as a reducing agent, and 3ml of lead acetate were added to 300g of deionized water to prepare a nickel plating solution, and the powder with the copper coating layer formed was added to the nickel plating solution, which was then stirred and maintained at 70~90℃ for 2 hours to perform electroless plating.

[0070] [Example 2] The process up to the formation of the copper coating layer was carried out in the same manner as in Example 1, and then a coating layer containing silver was formed by electroless plating. For this purpose, a silver coating solution was prepared by mixing 2g of EDTA (Ethylene-diamine-tetraacetic acid), 2.5ml of 28% ammonia water, and 3g of silver nitrate (AgNO3) in 300g of deionized water, and the graphite particles with the copper coating layer formed thereon were added thereto, and a reducing solution of 10g of glucose and 2g of sodium hydroxide dissolved in 50g of deionized water was dripped for 1 hour while stirring to form a third layer containing silver.

[0071] [Example 3] As in Example 1, after the first layer containing silver oxide was formed on the surface of the graphite particles, post-treatment was performed with an alkaline aqueous solution. For the post-treatment, 28% ammonia water was added to 100 g of deionized water and kept at 60° C., and then the graphite particles with the first layer were added and stirred. Before the graphite particles were added, the pH of the aqueous solution was 10.1.

[0072] Thereafter, the second layer containing copper and the third layer containing nickel were formed in the same manner as in Example 1.

[0073] [Comparative Example 1] As in Example 1, a hydrophilic treatment and a tin layer were formed. Then, without forming a silver oxide layer, electroless plating was immediately performed to successively form a second layer containing copper and a third layer containing nickel. The electroless plating of copper and nickel was performed in the same manner as in Example 1.

[0074] [Comparative Example 2] As in Example 1, a first layer containing silver oxide was formed on the surface of the graphite particles. Then, ascorbic acid was added to the aqueous solution to convert part of the silver oxide on the surface into metallic silver, and then electroless plating was performed to sequentially form a second layer containing copper and a third layer containing nickel. The electroless plating of copper and nickel was performed in the same manner as in Example 1.

[0075] [Comparative Example 3] As in Example 1, only the copper coating layer was formed, and no subsequent steps were carried out.

[0076] After forming the first layer on the conductive graphite particles thus prepared, the ratio of silver element between silver oxide and metallic silver, the content of silver element, nickel content and phosphorus content were analyzed, and the coating state was observed by a scanning electron microscope (SEM). The ratio of silver element was analyzed by XPS by taking a sample after forming the first layer. The content of silver element, nickel content and phosphorus content were analyzed by an inductively coupled plasma mass spectrometry (ICP).

[0077] The reliability was evaluated by a reflow test in which the conductive graphite particles prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were mixed with a certain amount of acrylic binder, coated on a polyimide film, dried, and then left on molten lead for 30 seconds, and the conductivity was measured.

[0078] The results are shown in Table 1 below. Here, the Cu content indicates the weight percentage of copper element based on the entire conductive graphite particles.

[0079] [Table 1]

[0080] Fig. 1 shows scanning electron microscope images of conductive graphite particles according to the examples. Fig. 1(a) is a scanning electron microscope image of a sample according to Example 1, Fig. 1(b) is a scanning electron microscope image of a sample according to Example 2, Fig. 1(c) is a scanning electron microscope image of a sample according to Comparative Example 1, and Fig. 1(d) is a scanning electron microscope image of a sample according to Comparative Example 2.

[0081] Both the samples from Examples 1 and 2 showed that a dense coating layer was formed, but in Comparative Example 1, which did not have a first layer containing silver oxide, the coating layer was not formed properly, and in Comparative Example 2, which had a high content of metallic silver in the first layer, the coating layer was not dense and the bonding was not strong.

[0082] FIG. 2 shows the results of measuring the ratio of silver element between silver oxide and metallic silver in the first layer of the sample according to Example 3. As a result of XPS, it is possible to measure it by the peak ratio of the ratio of silver in the reduced state and the ratio of silver in the oxidized state. x+ / Ag 0 ) was 7.83.

[0083] On the other hand, as shown in Table 1, the corrosion resistance was evaluated by a reflow test. In Examples 1 to 3, even after the reflow test, the resistance of the film using conductive graphite particles was good, at 50 mΩ or less. However, in Comparative Example 2, in which the formation of the coating layer was unstable, the resistance increased significantly, and in the sample of Comparative Example 3, in which the third protective layer was not formed, the resistance was too high and was not measured.

Claims

1. a first layer including silver oxide formed on a surface of the carbon-based particle; a second layer formed on the first layer and comprising copper; a third layer formed on the second layer and comprising nickel or silver; Including, Conductive carbon-based particles.

2. The carbon-based particles are one or more selected from the group consisting of graphite, graphene, and CNT. The conductive carbon-based particle according to claim 1 .

3. The first layer further contains metallic silver, and the molar ratio of silver element in the silver oxide to silver element in the metallic silver (Ag x+ / Ag 0 (0<x≦3) is in the range of 1 to 20; The conductive carbon-based particle according to claim 1 .

4. The first layer further comprises tin. The conductive carbon-based particle according to claim 1 .

5. The content of silver in the first layer is 10 to 1,000 ppm based on the total weight of the conductive carbon-based particles. The conductive carbon-based particle according to claim 1 .

6. The third layer further contains phosphorus together with the nickel. The conductive carbon-based particle according to claim 1 .

7. The third layer contains 0.1 to 13.0 wt. % phosphorus; The conductive carbon-based particle according to claim 6 .

8. (a) a hydrophilization step of hydrophilizing the surface of carbon-based particles; (b) forming a first layer by coating silver oxide on the carbon-based particles having hydrophilic surfaces; (c) forming a second layer by electrolessly plating copper on the first layer; (d) forming a third layer by electrolessly plating nickel or silver on the second layer; Including, A method for producing conductive carbon-based particles.

9. The method further includes a step of forming a tin layer between steps (a) and (b). The method for producing the conductive carbon-based particles according to claim 8 .

10. After step (b) and before step (c), the method further includes a post-treatment step of stirring the carbon-based particles on which the first layer is formed in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of the silver oxide. The method for producing the conductive carbon-based particles according to claim 8 .

Citation Information

Patent Citations

  • Method for making conductive silicone rubber

    JP1978145882A

  • The external storage medium

    JP1985116699U

  • Production of silver-tin series solder alloy powder

    JP1999293307A

  • Electroconductive fine particles, anisotropic electroconductive material and connecting structure

    JP2010103080A

  • Conductive particulate

    JP2013073919A