Plated steel sheet with excellent corrosion resistance and whiteness and its manufacturing method

A Zn-Mg-Al plated steel sheet with controlled crystal phase ratios and precise manufacturing processes addresses bending issues and whiteness limitations, achieving enhanced corrosion resistance and suitability for exterior applications.

JP2024539569AActive Publication Date: 2024-10-29POHANG IRON & STEEL CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2024519262
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-09-28
Publication Date
2024-10-29
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Conventional Zn-Mg-Al zinc alloy plated steel sheets suffer from poor bending workability due to hard intermetallic compounds and inadequate whiteness, limiting their application in high-grade exterior building materials despite having sacrificial corrosion protection.

Method used

A plated steel sheet with a Zn-Mg-Al based plating layer containing specific ratios of Mg and Al, controlled through X-ray diffraction intensities of crystal peaks, is manufactured using precise hot-dip galvanizing and cooling processes to enhance corrosion resistance, bendability, and whiteness.

Benefits of technology

The solution provides a plated steel sheet with improved corrosion resistance, bendability, and enhanced whiteness, suitable for high-grade exterior applications by optimizing the crystal phase ratios and manufacturing conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539569000001_ABST
    Figure 2024539569000001_ABST
Patent Text Reader

Abstract

The present invention provides a Zn-Mg-Al plated steel sheet having excellent corrosion resistance and whiteness, and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a highly corrosion-resistant plated steel sheet having excellent corrosion resistance and whiteness, and a method for producing the same. [Background technology]

[0002] When exposed to a corrosive environment, zinc-based plated steel sheets have a sacrificial corrosion protection property in which zinc, which has a lower redox potential than iron, corrodes first, suppressing the corrosion of the steel material. In addition, as the zinc in the plated layer oxidizes, it forms a dense corrosion product on the surface of the steel material, insulating the steel material from the oxidizing atmosphere and improving the corrosion resistance of the steel material. Due to these advantageous properties, the range of applications of zinc-based plated steel sheets has recently expanded to building materials, home appliances, and automotive steel sheets.

[0003] However, the corrosive environment is gradually worsening due to increased air pollution accompanying industrial advancement, and strict regulations on resources and energy conservation are creating a growing need for the development of steel materials with superior corrosion resistance to conventional galvanized steel materials.

[0004] In order to solve these problems, various researches are being conducted on the manufacturing technology of zinc alloy-coated steel sheets that improve the corrosion resistance of steel materials by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. A representative example is Zn-Mg-Al zinc alloy-coated steel sheets, which further add Mg to the Zn-Al plating composition.

[0005] However, Zn-Mg-Al zinc alloy plated steel sheets are often used after processing, but they have the disadvantage of poor bending workability, such as causing cracks in the plating layer during bending, due to the large amount of intermetallic compounds with high hardness contained in the plating layer.In addition, Zn-Mg-Al zinc alloy plated steel sheets usually have poor whiteness, which means there are technical limitations to their application as high-end building materials for exterior use.

[0006] Therefore, the reality is that no technology has been developed to date that can meet the high demand for excellent corrosion resistance, bendability and / or whiteness. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 2010-0073819 Summary of the Invention [Problem to be solved by the invention]

[0008] According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and whiteness, and a method for producing the same.

[0009] According to another aspect of the present invention, there are provided a plated steel sheet excellent not only in corrosion resistance and whiteness but also in bendability, and a method for producing the same.

[0010] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding additional objects of the invention from the entire contents of the specification of the present invention. [Means for solving the problem]

[0011] One aspect of the present invention is Base steel sheet; and A Zn-Mg-Al-based coating layer is provided on at least one surface of the base steel sheet; The plating layer contains, by weight percent, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, A plated steel sheet is provided that satisfies the following relational expression 1. [Equation 1] 0.26≦I (110) / I (103) ≦0.65 (In the above Relational Formula 1, the above I (110)indicates the integrated X-ray diffraction intensity of the crystal peak of the (110) plane of the MgZn2 phase, and the above I (103) indicates the integrated X-ray diffraction intensity of the (103) crystal plane of the MgZn2 phase.

[0012] Another aspect of the present invention is The base steel sheet was immersed in a plating bath containing, by weight, 4.0-6.3% Mg, 11.0-19.5% Al, and the balance Zn and other unavoidable impurities. B +10℃~T B +40℃(T B : A step of immersing the workpiece in a drawing temperature (galvanizing bath temperature) to perform hot-dip galvanizing; supplying nitrogen gas heated at 25 to 100°C to the hot-dip galvanized steel sheet to perform air wiping; cooling the air-wiped steel sheet to 420° C. at an average cooling rate of 1.0 to 3.0° C. / s; and Secondarily cooling the primarily cooled steel sheet at a temperature range of 300°C or more but less than 420°C at an average cooling rate of 3.5 to 5.0°C / s; The present invention provides a method for producing a plated steel sheet, which satisfies the following relational expression 2. [Equation 2] 0.005≦P air / (W air ×T) (In the above Relational Formula 2, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied nitrogen in °C. Effect of the Invention

[0013] According to one aspect of the present invention, there is provided a plated steel sheet having excellent corrosion resistance and whiteness, and a method for producing the same.

[0014] According to another aspect of the present invention, it is possible to provide a plated steel sheet that is excellent not only in corrosion resistance and whiteness but also in bendability, and a method for producing the same.

[0015] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]

[0016] [Figure 1] 1 is a graph showing X-ray diffraction peaks versus X-ray diffraction angle (2θ) measured by X-ray diffraction (hereinafter, referred to as "XRD") on the surface of the plating layer for the plated steel sheets obtained in Example 8 and Comparative Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The terms used in this specification are for the purpose of describing specific embodiments and are not intended to limit the present invention. Furthermore, the singular forms used in this specification also include the plural forms unless the related definition clearly indicates otherwise.

[0018] The meaning of "comprise" as used in the specification is to specify a feature and does not exclude the presence or addition of other features.

[0019] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this invention belongs. Dictionary-defined terms are to be interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content.

[0020] Hereinafter, a "plated steel sheet" according to one aspect of the present invention will be described in detail. In the present invention, the content of each element is expressed in percent by weight unless otherwise specified.

[0021] In conventional Zn-Mg-Al zinc alloy plated steel sheet related technologies, magnesium is added to improve corrosion resistance. However, if too much magnesium is added, there is a problem that more dross is generated floating in the plating bath, and the dross must be removed frequently. Therefore, the upper limit of magnesium addition was limited to 3%.

[0022] Therefore, research was conducted to further improve corrosion resistance by increasing the amount of Mg added beyond 3%, but as the amount of Mg added increases, the plating layer contains large amounts of intermetallic compounds with high hardness, which causes problems such as cracks in the plating layer during bending, resulting in a deterioration of bendability (or bending workability).

[0023] In addition to the bendability problem, the conventional technology had a problem of insufficient whiteness of Zn-Mg-Al zinc alloy plated steel sheets due to the absence of diffuse reflection caused by an inappropriate ratio of the crystal phase of the MgZn2-based intermetallic compound. Therefore, there was a limit to the application of conventional Zn-Mg-Al zinc alloy plated steel sheets to high-end building materials for exterior use.

[0024] For this reason, it has been technically difficult with conventional techniques to provide a plated steel sheet that not only ensures corrosion resistance but also has excellent bendability and whiteness.

[0025] Therefore, the present inventors conducted extensive research in order to solve the above-mentioned problems and at the same time provide a plated steel sheet that is excellent not only in corrosion resistance but also in bendability and / or whiteness. As a result, they found that an important factor is not only the composition of the plating layer but also controlling within a specific range the ratio of the X-ray diffraction integrated intensity of the crystal peak of the (110) plane of the MgZn2 phase, obtained by analyzing the surface of the plating layer by XRD, to the X-ray diffraction integrated intensity of the crystal of the (103) plane of the MgZn2 phase, and thus completed the present invention.

[0026] The configuration of a plated steel sheet that is excellent in corrosion resistance and also excellent in bendability and / or whiteness will be specifically described below.

[0027] First, the plated steel sheet according to the present invention includes a base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet.

[0028] In the present invention, the type of base steel sheet is not particularly limited. For example, the base steel sheet may be an Fe-based base steel sheet used as a base steel sheet for ordinary zinc-based plated steel sheets, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. Alternatively, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, or automobiles.

[0029] However, as an example, the above-mentioned base steel sheet has, by weight%, C: more than 0% (more preferably, 0.001% or more) and 0.18% or less, Si: more than 0% (more preferably, 0.001% or more) and 1.5% or less, Mn: 0.01 to 2.7%, P: more than 0% (more preferably, 0.001% or more) and 0.07% or less, S: more than 0% (more preferably, 0.001% or more) and 0.015% or less, Al: more than 0% (more preferably, It may have a composition including: Nb: more than 0% (more preferably, 0.001% or more) and 0.06% or less, Cr: more than 0% (more preferably, 0.001% or more) and 1.1% or less, Ti: more than 0% (more preferably, 0.001% or more) and 0.06% or less, B: more than 0% (more preferably, 0.001% or more) and 0.03% or less, and the balance being Fe and other unavoidable impurities.

[0030] Although not particularly limited, according to one embodiment of the present invention, at least one surface of the base steel sheet may be provided with a Zn-Mg-Al-based plating layer made of a Zn-Mg-Al-based alloy. The plating layer may be formed on only one surface of the base steel sheet, or may be formed on both surfaces of the base steel sheet. In this case, the Zn-Mg-Al-based plating layer refers to a plating layer that contains Mg and Al and mainly contains Zn (i.e., contains 50% or more Zn).

[0031] Although not particularly limited, according to one embodiment of the present invention, the thickness of the Zn-Mg-Al-based coating layer may be 5 to 100 μm, and more preferably 7 to 90 μm. If the thickness of the coating layer is less than 5 μm, the coating layer may become very thin locally due to an error caused by the thickness deviation of the coating layer, and the corrosion resistance may be poor. If the thickness of the coating layer exceeds 100 μm, the cooling of the hot-dip coating layer may be delayed, and there may be a possibility of solidification defects occurring on the surface of the coating layer, such as a sagging shape, and the productivity of the steel sheet may decrease due to solidification of the coating layer.

[0032] Meanwhile, although not particularly limited, according to an embodiment of the present invention, an Fe-Al-based inhibition layer may be further included between the base steel sheet and the Zn-Mg-Al-based coating layer. The Fe-Al-based inhibition layer is a layer mainly containing (for example, 60% or more) an intermetallic compound of Fe and Al, and examples of the intermetallic compound of Fe and Al include FeAl, FeAl3, Fe2Al5, etc. In addition, a component derived from the coating layer such as Zn, Mg, etc. may be further included, for example, 40% or less. The inhibition layer is a layer formed by alloying Fe diffused from the initial coating base steel sheet and coating bath components. The inhibition layer can play a role in improving the adhesion between the base steel sheet and the coating layer, and at the same time, can play a role in preventing Fe diffusion from the base steel sheet to the coating layer. In this case, the inhibition layer can be formed continuously or discontinuously between the base steel sheet and the Zn-Mg-Al-based coating layer. With respect to the inhibition layer, except for the above description, contents commonly known in the art can be similarly applied.

[0033] Although not particularly limited, according to one embodiment of the present invention, the thickness of the inhibition layer may be selectively 0.1 to 1 μm. The inhibition layer plays a role in preventing alloying and ensuring corrosion resistance, but since it is brittle, it may affect workability, and in the present invention, the thickness of the inhibition layer may be 1 μm or less. However, in order to function as an inhibition layer, the thickness may be 0.1 μm or more. From the viewpoint of further improving the above-mentioned effects, preferably, the upper limit of the thickness of the inhibition layer may be 1.00 μm, or the lower limit of the thickness of the inhibition layer may be 0.15 μm.

[0034] In this case, the thickness of the inhibition layer may refer to the minimum thickness of the inhibition layer in the thickness direction when a cross-sectional specimen is prepared by cutting the plated steel sheet in the thickness direction (i.e., the direction perpendicular to the rolling direction) and then photographing the cross-section with a scanning electron microscope (hereinafter referred to as "SEM").

[0035] According to the present invention, the plating layer contains, by weight, 4.0-6.3% Mg, 11.0-19.5% Al, and the balance being Zn and other inevitable impurities. The reasons for adding each component and limiting the content thereof will be specifically described below.

[0036] Mg: 4.0% or more and 6.3% or less Mg is an element that plays a role in improving the corrosion resistance of plated steel materials, and in the present invention, the Mg content in the plating layer is controlled to 4.0% or more in order to ensure the desired excellent corrosion resistance. On the other hand, if Mg is added excessively, not only may dross be generated, but also intermetallic compounds with high hardness may be excessively formed in the plating layer, weakening the bendability, so the Mg content can be controlled to 6.3% or less.

[0037] Al: 11.0% or more and 19.5% or less Generally, when Mg is added at 1% or more, it is effective in improving corrosion resistance, but when Mg is added at 2% or more, there is a problem that the generation of floating dross in the plating bath increases due to oxidation of Mg in the plating bath, and the dross must be removed frequently. Due to this problem, in the conventional technology, Mg is added at 1.0% or more in Zn-Mg-Al zinc alloy plating to ensure corrosion resistance, but the upper limit of Mg content was set at 3.0% for general use.

[0038] However, in the present invention, in order to further improve the corrosion resistance, it is necessary to increase the Mg content to 4% or more. However, if the coating layer contains Mg at 4% or more, there is a problem of dross being generated due to oxidation of Mg in the coating bath, so it is necessary to add Al at 11.0% or more. However, if excessive Al is added to suppress dross, the melting point of the coating bath becomes high, and the accompanying operating temperature becomes too high, which can cause problems due to high-temperature work such as erosion of the coating bath structure and denaturation of the steel material. Therefore, it is preferable to control the upper limit of the Al content in the coating layer to 19.5%.

[0039] The balance is Zn and other unavoidable impurities. In addition to the above-mentioned composition of the coating layer, the balance may be Zn and other inevitable impurities. The inevitable impurities may include any impurities that can be unintentionally mixed in the normal manufacturing process of a hot-dip galvanized steel sheet, and the meaning of the inevitable impurities can be easily understood by a person skilled in the art.

[0040] On the other hand, according to the present invention, the above-mentioned plated steel sheet preferably satisfies the following relational expression 1 in order to ensure corrosion resistance and at the same time a desired level of excellent bendability and / or whiteness. [Equation 1] 0.26≦I (110) / I (103) ≦0.65 (In the above Relational Formula 1, the above I (110) indicates the integrated X-ray diffraction intensity of the crystal peak of the (110) plane of the MgZn2 phase, and the above I (103) indicates the integrated X-ray diffraction intensity of the (103) crystal plane of the MgZn2 phase.

[0041] The present inventors have found that the ratio of MgZn2 phase (110) crystals and MgZn2 phase (103) crystals present in the coating layer is an important factor in improving the bendability and whiteness of the coating layer. That is, by controlling the ratio of the X-ray diffraction integrated intensity of the crystal peak of the MgZn2 phase (110) crystal plane obtained by XRD analysis on the surface of the coating layer to the X-ray diffraction integrated intensity of the MgZn2 phase (103) crystal plane, it is possible to ensure not only excellent corrosion resistance but also to improve bendability and whiteness.

[0042] In the present invention, an increase in the (110) crystal plane of the MgZn2 phase reduces the lattice mismatch between the crystalline phase formed parallel to the surface of the coating layer and the Zn phase, thereby reducing the occurrence of cracks in the MgZn2 phase and improving the bendability. On the other hand, an increase in the (103) crystal plane of the MgZn2 phase has the disadvantage that the crystalline phase is formed in a direction perpendicular to the surface of the coating layer, which may increase the occurrence of cracks. Therefore, in order to improve the bendability, it is necessary to appropriately harmonize the two crystal planes of the MgZn2 phase described above. Furthermore, since the combination ratio of the (110) crystal plane of the MgZn2 phase and the (103) crystal plane of the MgZn2 phase affects the diffuse reflection on the surface of the coated steel sheet, the (110) crystal plane of the MgZn2 phase and the (103) crystal plane of the MgZn2 phase can be controlled at an appropriate ratio to induce an increase in diffuse reflection and improve the whiteness.

[0043] Therefore, I defined by the above relation 1 (110) / I (103) If the value is less than 0.26, the ratio of the (103) crystal plane of the MgZn2 phase to the (110) crystal plane of the MgZn2 phase is excessive, and the bendability and whiteness may be insufficient. (110) / I (103) If the value exceeds 0.65, the ratio of the (110) crystal plane of the MgZn2 phase to the (103) crystal plane of the MgZn2 phase is extremely excessive, making it impossible to induce an increase in diffuse reflection, which may result in insufficient whiteness.

[0044] According to the present invention, by mixing the above-mentioned (110) crystal plane of the MgZn2 phase and the (103) crystal plane of the MgZn2 phase so as to satisfy the above-mentioned relational expression 1, not only is excellent bendability ensured, but the surface shines due to diffuse reflection, and excellent whiteness properties are obtained. Furthermore, by the ratio of the above-mentioned (110) crystal plane of the MgZn2 phase and the (103) crystal plane of the MgZn2 phase satisfying the relational expression 1, and at the same time, the coexistence of the (002) crystal plane of the Zn phase, which is the main crystal, can further increase the diffuse reflection.

[0045] On the other hand, although not particularly limited, according to one embodiment of the present invention, from the viewpoint of further maximizing the above-mentioned effects, it is more preferable that I defined by the above Relational Formula 1 be used. (110) / I (103) The lower limit of the value can be 0.55, or the above I (110) / I (103) The upper limit of the value can be 0.64.

[0046] In this case, the crystal peak of the (110) plane of the MgZn2 phase and the crystal peak of the (103) plane of the MgZn2 phase can be distinguished from the crystal peak of the (110) plane and the crystal peak of the (103) plane by a method known in the art from the X-ray diffraction integrated intensity obtained by analyzing the surface of the coating layer by XRD, and therefore will not be separately defined in this specification.

[0047] Meanwhile, the method for measuring the X-ray diffraction integrated intensity is not particularly limited, and any method known in the art can be applied. For example, the surface of the plating layer can be analyzed by XRD to measure the X-ray diffraction integrated intensity. A RINT2000 diffractometer can be used as an apparatus for measuring the X-ray diffraction integrated intensity. The measurement conditions for the X-ray diffraction integrated intensity are a Cu target, voltage: 40 kV, current: 200 mA, and the X-ray diffraction angle (2θ) can be measured from 10 to 100°. As a representative example, when a Cu target is used, the above I (110)can be defined as the integrated intensity of the peak between 2θ = 34.0° and 34.6°, and the above I (103) can be defined as the integrated intensity of the peak between 2θ=37.0° and 37.5°. However, when the target material is different, such as Mo, the value of 2θ varies depending on the type of target material, and therefore the range of 2θ is not particularly limited in the present invention.

[0048] In this specification, the MgZn2 crystal having the (110) plane means a structure in which the (110) plane is present in the hexagonal crystal of the MgZn2 phase on the steel sheet surface. The MgZn2 crystal having the (103) plane means a structure in which the (103) plane is present in the hexagonal crystal of the MgZn2 phase on the steel sheet surface.

[0049] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the plated steel sheet may be selectively subjected to the above-mentioned I (110) The value of can be in the range of 120 to 200. (110) By ensuring that the value of satisfies the range of 120 to 200, the abundance ratio of (110) crystals of the MgZn2 phase is increased within the range satisfying the above relational expression 1, thereby not only further improving the bendability of the plated steel sheet but also further improving the whiteness.

[0050] Alternatively, although not particularly limited, according to one embodiment of the present invention, the plated steel sheet may be selectively (103) The value of can be in the range of 240 to 300. (103) By making the value of I satisfy the range of 240 to 300, the abundance ratio of the (110) crystals of the MgZn2 phase, which reduces the occurrence of cracks, is increased within the range satisfying the above-mentioned relational expression 1, while the abundance ratio of the (103) crystals of the MgZn2 phase, which reduces the occurrence of cracks, is decreased, thereby improving the bendability of the plated steel sheet and further improving the whiteness. (110) The value of I (103)The values ​​are those measured using a RINT2000 diffractometer with a Cu target under the conditions of a voltage of 40 kV and a current of 200 mA.

[0051] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the surface roughness of the plated steel sheet may selectively satisfy the ranges of Ra: 1.0 to 1.7 μm and Rpc: 10 to 30 ( / 10 mm). By making the surface roughness of the plated steel sheet satisfy the above-mentioned ranges, diffuse reflection is uniformly formed in space, and the whiteness of the plated steel sheet can be further improved.

[0052] Next, a "method for producing a plated steel sheet" according to another aspect of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet of the present invention must be produced by the following method.

[0053] According to an embodiment of the present invention, the method may further include a step of preparing a base steel sheet, and the type of the base steel sheet is not particularly limited. The base steel sheet may be, but is not limited to, an Fe-based base steel sheet used as a base steel sheet for a typical hot-dip galvanized steel sheet, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet. In addition, the base steel sheet may be, but is not limited to, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, and automobiles. In this case, the above description may be similarly applied to the base steel sheet.

[0054] Next, the base steel sheet is immersed in a plating bath containing, by weight, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, to perform hot-dip galvanization.

[0055] In this case, the reasons for adding the components in the coating bath and the reasons for limiting the contents thereof can be similarly applied to the explanation for the components of the coating layer described above, except for the small amount of Fe content that can flow in from the base steel sheet.

[0056] Meanwhile, in order to prepare the coating bath having the above composition, a composite ingot containing the desired Zn, Al, and Mg or a Zn-Mg or Zn-Al ingot containing individual components can be used. In order to replenish the coating bath consumed in hot dip coating, the ingot is melted and supplied. In this case, a method of directly immersing the ingot in the coating bath and melting it can be selected, or a method of melting the ingot in a separate port and then replenishing the molten metal to the coating bath can be selected.

[0057] According to the present invention, during the hot dip galvanizing, the drawing temperature of the base steel sheet is set to be equal to or lower than the plating bath temperature (T B ) for T B +10℃~T B +40℃. B If the temperature is less than +10°C, the interface adhesion is insufficient and the problem of dross adhesion may occur. B If the temperature exceeds +40°C, the generation of zinc fumes (Zn fumes) increases and they are adsorbed on the steel sheet, which may cause problems with the quality of the plated surface. B ) may be in the range of 440 to 500°C, and more preferably in the range of 440 to 490°C.

[0058] Next, nitrogen gas heated to 25 to 100°C (more preferably, more than 25°C and 100°C or less) is supplied to the hot-dip galvanized steel sheet to perform air wiping. As a result of intensive research, the present inventors have found that, unlike conventional methods, by supplying nitrogen gas heated to a specific temperature range during air wiping, it is possible to produce a plated steel sheet with improved whiteness by ensuring appropriate surface roughness and uniforming diffuse reflection in space.

[0059] That is, if the temperature of the nitrogen gas supplied during the air wiping is less than 25° C., a problem may occur in which the steel sheet is rapidly cooled, resulting in non-uniform hue difference in the width direction of the steel sheet, whereas if the temperature of the nitrogen gas supplied during the air wiping exceeds 100° C., a problem may occur in which productivity is reduced because cooling is not easy.

[0060] From the viewpoint of maximizing the above-mentioned effect, more preferably, the lower limit of the temperature of the nitrogen gas supplied during the air wiping can be 30°C, or the upper limit of the temperature of the nitrogen gas supplied during the air wiping can be 85°C.

[0061] Meanwhile, according to the present invention, the air wiping is controlled so as to satisfy the following relational expression 2. By controlling the air wiping conditions so as to satisfy the following relational expression 2, it is possible to produce a steel sheet having excellent whiteness uniformly in the width direction. In this case, since the following relational expression 2 is an empirically obtained value, no particular unit can be specified, and the following defined W air The unit of is mm and P air It is sufficient to have the units of kPa for pressure and the units of T be °C. [Equation 2] 0.005≦P air / (W air ×T) (In the above Relational Formula 2, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied nitrogen in °C.

[0062] According to the present invention, after the air wiping step, the air wiped steel sheet is primarily cooled to 420°C (based on the surface temperature) at an average cooling rate of 1.0 to 3.0°C / s, and then the primarily cooled steel sheet is secondary cooled at an average cooling rate of 3.5 to 5.0°C / s in a temperature range of less than 420°C and not less than 300°C.

[0063] As a result of extensive investigations, the present inventors have found that uniform surface properties can be ensured in the width direction of the steel sheet by performing slow cooling in two stages while precisely controlling the cooling rate.

[0064] That is, if the average cooling rate during the primary cooling is less than 1.0°C / s, a problem of insufficient productivity may occur, and if the average cooling rate during the primary cooling exceeds 3.0°C / s, a problem of non-uniform solidification characteristics of the steel sheet may occur. Also, if the average cooling rate during the secondary cooling is less than 3.5°C / s, a problem of insufficient productivity may occur, and if the average cooling rate during the secondary cooling exceeds 5.0°C / s, the ratio of crystals on the (110) plane of the MgZn2 phase to crystals on the (103) plane of the MgZn2 phase is not appropriate, so that the desired surface structure may not be formed.

[0065] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the cooling conditions can be selectively controlled during the cooling so as to satisfy the following Relational Expression 3. By controlling the relationship between the average cooling rates during the primary cooling and secondary cooling so as to satisfy the following Relational Expression 3, the formation ratio of (110) plane crystals of the MgZn2 phase and (103) plane crystals of the MgZn2 phase is optimized, and the whiteness of the plated steel sheet can be further improved. In this case, since the following Relational Expression 3 is an empirically obtained value, no particular unit can be determined, and it is sufficient if the units of C1 and C2 defined below are satisfied. [Equation 3] 1+C1 / C2≦C2≦C1×1.6 (In the above Relational Formula 3, C1 indicates the average cooling rate [°C / s] during the first cooling, and C2 indicates the average cooling rate [°C / s] during the second cooling.)

[0066] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the surface roughness Ra of the plated steel sheet obtained by the secondary cooling can be selectively controlled to be in the range of 1.0 to 1.7 μm and 10 to 30 ( / 10 mm). By controlling the surface roughness Ra and Rpc of the plated steel sheet to satisfy the above ranges, it is possible to ensure the effect of uniformly forming diffuse reflection in space.

[0067] As described above, by precisely controlling the plating composition and manufacturing conditions, it is possible to effectively provide a plated steel sheet that is excellent not only in corrosion resistance but also in bendability and whiteness. EXAMPLES

[0068] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.

[0069] (Example) A base steel sheet having a thickness of 1.5 mm and a width of 1200 mm and having a composition of C: 0.018%, Si: 0.01%, Mn: 0.2%, P: 0.009%, S: 0.005%, Al: 0.1%, Nb: 0.02%, Cr: 0.2%, Ti: 0.02%, B: 0.015%, the balance being Fe and impurities, was prepared. The base steel sheet prepared above was immersed in a coating bath under the conditions in Table 1 below to perform hot-dip galvanizing.

[0070] Next, the hot-dip galvanized steel sheet was subjected to an air wiping treatment using nitrogen (N2) gas under the conditions shown in Table 1 below, and then subjected to primary cooling and secondary cooling under the conditions shown in Table 2 below. Thereafter, the steel sheet obtained by the secondary cooling was controlled so as to satisfy the surface roughness shown in Table 2 below.

[0071] [Table 1]

[0072] [Table 2]

[0073] Test pieces of the plated steel sheets obtained by the methods in Tables 1 and 2 above were prepared, and the plated layers were dissolved in a hydrochloric acid solution. The dissolved liquid was then analyzed by a wet analysis (ICP) method to determine the compositions of the plated layers, which are shown in Table 3 below (the remainder corresponds to Zn and impurities).

[0074] In addition, cross-sectional test pieces were prepared by cutting the steel sheet in a direction perpendicular to the rolling direction so that the interface between the coating layer and the base steel sheet could be observed, and then photographed with an SEM. It was confirmed that an Fe-Al-based inhibitory layer was formed between the base steel sheet, the Zn-Mg-Al-based coating layer, and the base steel sheet and the Zn-Mg-Al-based coating layer.

[0075] In addition, to measure the X-ray diffraction integral intensity of the plating layer, a RINT2000 diffractometer was used with a Cu target at a voltage of 40 kV and a current of 200 mA to measure the diffraction peaks MgZn2(110) and MgZn2(103) at 2θ=34.0°-38.0°, and the integral intensity of the corresponding peaks was calculated. (110) is the value obtained by integrating the peak from 34° to 34.6°, and the integrated intensity I (103) is a value obtained by integrating the peak at 37° to 37.5° (the unit is integrated intensity, which corresponds to cps*2θ), and is shown in Table 3 below.

[0076] [Table 3]

[0077] For each of the invention examples and comparative examples, the corrosion resistance, bendability and whiteness were evaluated according to the following criteria, and the evaluation results for each property are shown in Table 4 below.

[0078] <Corrosion resistance> In order to evaluate the corrosion resistance, a salt spray tester (SST) was used in accordance with the test method of ISO14993, and the evaluation was performed according to the following criteria. ○: The time it takes for red rust to appear is 30 to 40 times longer than that of Zn plating of the same thickness. △: The time it takes for red rust to appear is 20 to 30 times longer than that of Zn plating of the same thickness. ×: The time it takes for red rust to appear is less than 20 times longer than that for Zn plating of the same thickness.

[0079] <Bending property> To evaluate cracks in the bent parts, the material was cut to 30 mm x 100 mm, and the number of cracks that occurred within a length of 10 mm after 3t bending was observed using FE-SEM. ◎: Less than 3 ○: 3 or more and less than 10 △: 10 or more but less than 20 ×: 20 or more

[0080] <Whiteness> To evaluate the whiteness, the L value was measured using an X-Rite 8200 device and evaluated according to the following criteria. ◎: L value 90 or more ○: L value 85 or more and less than 90 △: L value 75 or more and less than 85 ×: L value less than 75

[0081] [Table 4]

[0082] As can be seen from the experimental results in Table 4 above, in the case of Invention Examples 1 to 9 which satisfy the plating composition and manufacturing conditions specified in the present invention, it was confirmed that the corrosion resistance, bendability and whiteness were all excellent.

[0083] In particular, it was confirmed that, among the above-mentioned invention examples, invention examples 7 to 9, which satisfy the cooling rate of the relational expression 3 defined in the present invention, are superior in bendability and whiteness to invention examples 1 to 6.

[0084] On the other hand, in the case of Comparative Examples 1 to 17, which do not satisfy all of the plating compositions and manufacturing conditions specified in the present invention, it was confirmed that one or more of the properties of corrosion resistance, bendability, and whiteness were deteriorated compared to Invention Examples 1 to 9.

[0085] In particular, for the plated steel sheets obtained in Example 8 and Comparative Example 8, the diffraction peaks MgZn2(110) and MgZn2(103) corresponding to the X-ray diffraction angle (2θ=34.0° to 38.0°) measured by XRD on the surface of the plated layer were measured and shown in Figure 1. From Figure 1, the peaks in the range of 2θ=34° to 34.6° were integrated to obtain the integrated intensity I (110) The peaks in the 2θ = 37° to 37.5° range were integrated to obtain the integral intensity I (103) After obtaining (110) / I (103) From this, it was confirmed that Example 8 of the present invention satisfied Relational Expression 1 and was excellent in corrosion resistance, bendability, and whiteness, whereas Comparative Example 8 did not satisfy Relational Expression 1 and, although corrosion resistance was ensured, bendability and whiteness were deteriorated compared to Example 8 of the present invention.

Claims

1. Base steel sheet; and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet; The Zn-Mg-Al-based plating layer contains, by weight, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, the balance being Zn and other inevitable impurities, A plated steel sheet satisfying the following relational expression 1. [Relationship 1] 0.26≦I (110) / I (103) ≦0.65 (See above I (110) is MgZn 2 The X-ray diffraction integrated intensity of the crystal peak of the (110) plane of the I phase is shown. (103) is MgZn 2 The X-ray diffraction integrated intensity of the (103) crystal plane of the phase is shown.

2. The plated steel sheet according to claim 1, further comprising: an Fe-Al-based inhibiting layer provided between the base steel sheet and the Zn-Mg-Al-based plating layer.

3. The plated steel sheet according to claim 2, wherein the Fe-Al-based inhibiting layer has an average thickness of 0.1 to 1 μm.

4. I (110) The plated steel sheet according to claim 1, wherein the value of is in the range of 120 to 200.

5. I (103) The plated steel sheet according to claim 1, wherein the value of satisfies the range of 240 to 300.

6. The plated steel sheet according to claim 1, wherein the surface roughness of the plated steel sheet satisfies the ranges of Ra: 1.0 to 1.7 μm and Rpc: 10 to 30 ( / 10 mm).

7. The base steel sheet was immersed in a plating bath containing, by weight, 4.0 to 6.3% Mg, 11.0 to 19.5% Al, and the balance Zn and other unavoidable impurities. B +10℃~T B +40°C (T Bdipping the workpiece at a drawing temperature of 100° C. (the temperature of the plating bath) to perform hot-dip galvanizing; supplying nitrogen gas heated to 25 to 100° C. to the hot-dip galvanized steel sheet to perform air wiping; cooling the air-wiped steel sheet to 420° C. at an average cooling rate of 1.0 to 3.0° C. / s; and Secondarily cooling the primarily cooled steel sheet at a temperature range of 300°C or more but less than 420°C at an average cooling rate of 3.5 to 5.0°C / s; A method for producing a plated steel sheet, which satisfies the following relational expression 2. [Relationship 2] 0.005≦P air / (W air ×T) (The above W air represents the distance between the air knives, and is expressed in mm. air represents the pressure of the air knife, in kPa. T represents the temperature of the supplied nitrogen, in °C.

8. The method for producing a plated steel sheet according to claim 7 , which satisfies the following relational expression 3: [Relationship 3] 1+C 1 / C 2 ≦C 2 ≦C 1 ×1.6 (C 1 indicates the average cooling rate [°C / s] during the first cooling, and 2 indicates the average cooling rate during secondary cooling [℃ / s].)

9. The method for producing a plated steel sheet according to claim 7, wherein the surface roughness of the plated steel sheet obtained by the secondary cooling is controlled in the ranges of Ra: 1.0 to 1.7 μm and Rpc: 10 to 30 ( / 10 mm).

Citation Information

Patent Citations

  • Low-aluminum low-magnesium zinc-aluminum-magnesium plated steel plate and method for producing same

    CN103361588A

  • Hot dip zinc-aluminum-magnesium plated steel sheet good in corrosion resistance and surface appearance and its production

    JP1998226865A

  • Hot dip zn-al-mg coated steel sheet excellent in corrosion resistance and external surface appearance, and its production

    JP1998306357A

  • Hot dip high al-containing zn-al-mg base metal coated steel sheet

    JP2001295015A

  • Hot dip zn-al-mg plated steel sheet and production method therefor

    JP2002285311A