MRAM structure with enhanced magnetism through seed engineering
The MRAM structure addresses resistance and TMR penalties by using a wider seed region with sidewall shunting, improving performance and scalability.
Patent Information
- Application Number
- JP2024524400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-15
- Filing Date
- 2022-11-09
- Publication Date
- 2024-11-08
AI Technical Summary
Conventional MRAM structures using thick tunnel barrier seed layers suffer from increased resistance and tunneling magnetoresistive (TMR) penalties due to magnetic or crystalline disorder, which negatively impact memory performance.
The MRAM structure incorporates a wider seed region with a tunnel barrier seed layer below a chemical template layer, and redeposited metallic material on the sidewalls of the seed region to shunt the structure, reducing resistance while minimizing TMR loss.
This design effectively reduces resistance and maintains magnetic order, enhancing the performance of MRAM structures by minimizing TMR penalties and improving scalability.
Smart Images

Figure 2024541223000001_ABST
Abstract
Description
[Technical field]
[0001] This application relates to memory structures, and more particularly to magnetoresistive random access memory (MRAM) structures that include increased seed region through intentional shunting to overcome resistance and tunneling magnetoresistance (TMR) penalties. [Background technology]
[0002] MRAM is a non-volatile random access memory technology in which data is stored by magnetic storage elements. These elements are typically formed of two ferromagnetic plates, each capable of retaining magnetization, separated by a thin dielectric layer (i.e., tunnel barrier layer). One of the two plates (i.e., the magnetic reference layer or pinned layer) is a magnet whose magnetic moment direction is crystallized and solidified in a particular direction, while the magnetization of the other plate (i.e., the magnetic free layer) can be changed to at least two different directions to represent different digital states such as 0 and 1 for memory applications. In MRAM, such elements are sometimes called magnetic tunnel junction (MTJ) structures. In a typical MTJ structure, the magnetization of the magnetic reference layer is fixed in one direction (e.g., up), but the orientation of the magnetic free layer can be "switched" by some external force, such as a magnetic field or a charge current generated by a spin transfer torque. A smaller current (regardless of polarity) can be used to read the resistance of the device, which depends on the relative orientation of the magnetizations of the magnetic free layer and the magnetic reference layer. Resistance is usually higher when the magnetizations are antiparallel and lower when they are parallel (although this can be reversed for some materials).
[0003] One type of MRAM that can use MTJ structures is spin-transfer torque (STT) MRAM. STT MRAM has the advantages of lower power consumption and greater scalability compared to conventional MRAM, which uses a magnetic field to flip the active element. In STT MRAM, spin-transfer torque is used to flip (switch) the orientation of the magnetic free layer. In STT MRAM devices, a current passing downward through the MTJ structure is used to switch or "write" the bit state of the MTJ memory element. A current passing through the MTJ structure aligns the magnetic free layer parallel to the magnetic reference layer, and a current passing upward through the MTJ structure aligns the magnetic free layer anti-parallel to the magnetic reference layer.
[0004] In certain material systems, such as ordered magnetic alloys, growing the magnetic stack on top of a relatively thick tunnel barrier seed layer is desired for better deposition control; a thin tunnel barrier seed layer can result in magnetic or crystalline disorder, resulting in detrimental magnetic properties for memory cells incorporated therein. However, the use of a thick tunnel barrier seed layer in conventional memory structures negatively impacts TMR due to the increased resistance caused by the tunnel barrier seed layer. Thus, there is a need for memory structures that overcome the resistance and TMR penalty. Summary of the Invention
[0005] A memory structure, i.e., an MRAM structure, is provided that includes a seed region, including at least a tunnel barrier seed layer, located below the chemical template layer and wider than an MTJ structure located on the chemical template layer. A redeposited metal material is located on at least a sidewall of the tunnel barrier seed layer of the seed region to shunt the seed region of the structure. The memory structure has reduced resistance with minimal TMR loss penalty.
[0006] In one aspect of the present application, a memory structure is provided. In one embodiment of the present application, the memory structure includes a bottom electrode embedded in a first interconnect dielectric material layer. A non-magnetic pedestal structure is located on the bottom electrode and a portion of the first interconnect dielectric material layer. A seed region having a first width is located on the non-magnetic pedestal structure, the seed region including at least a tunnel barrier seed layer. A chemical template layer is located on the seed region. An MTJ structure having a second width is located on the chemical template layer, the second width being smaller than the first width. A top electrode is located on the MTJ structure, and a layer of non-oxidized metal residue is located on at least a sidewall of the tunnel barrier seed layer, intentionally shunting at least the seed region.
[0007] In an embodiment of the present application, the chemical template layer has an upper portion and a lower portion, the lower portion having a width greater than the upper portion and forming an interface with the tunnel barrier seed layer.
[0008] In an embodiment of the present application, the memory structure further includes a dielectric spacer located on a sidewall of the MTJ structure and the top electrode and having a bottom surface located on a lower portion of the chemical template layer.
[0009] In an embodiment of the present application, the memory structure further includes an encapsulation layer located laterally adjacent to the dielectric spacers, the seed region and the non-magnetic pedestal structure and having a bottom surface located on a surface of the first interconnect dielectric material layer.
[0010] In embodiments of the present application, the memory structure further includes a second interconnect dielectric material layer laterally adjacent to and above the encapsulation layer. In such embodiments, a conductive structure can be embedded in the second interconnect dielectric material layer, the conductive structure contacting the top electrode. Typically, the conductive structure has a third width greater than at least the second width of the MTJ structure.
[0011] In embodiments of the present application, the layer of non-oxidized metal residue extends on the sidewalls of the non-magnetic pedestal structure or on the sidewalls of the lower portion of the chemical template layer, and optionally on the sidewalls of the dielectric spacer, hi some embodiments of the present application, the layer of non-oxidized metal residue extends on the sidewalls of each of the non-magnetic pedestal structure, the lower portion of the chemical template layer, and the dielectric spacer.
[0012] In embodiments of the present application, the MTJ structure is a top pinned MTJ structure including, from bottom to top, a magnetic free layer, a tunnel barrier layer, and a magnetic reference layer. In some embodiments, the magnetic free layer of the top pinned MTJ structure includes an ordered magnetic alloy, such as a Heusler alloy or an L10 alloy. In some embodiments, the magnetic reference layer of the top pinned MTJ structure is a single magnetic reference layer, and in other embodiments, the magnetic reference layer of the top pinned MTJ structure includes a bottom magnetic reference layer, a synthetic antiferromagnetic coupling layer, and a top magnetic reference layer.
[0013] In an embodiment of the present application, the non-magnetic pedestal structure has a width greater than at least the second width of the MTJ structure, and the top electrode has a width equal to the second width of the MTJ structure.
[0014] In an embodiment of the present application, the layer of non-oxidized metal residue includes at least one metal, such as Ta, present in the non-magnetic pedestal structure. In an embodiment of the present application, the chemical template layer is a crystallized solidification layer for the magnetic free layer of the MTJ structure. In an embodiment of the present application, the bottom electrode and the first interconnect dielectric material layer provide one interconnect level of a multilevel interconnect structure.
[0015] In an embodiment, the tunnel barrier seed layer has a thickness sufficient to induce magnetic or crystalline order in the magnetic free layer of the MTJ structure. "Magnetic order" means that the magnetic free layer has an electron system that forms localized or itinerant magnetic moments and that there is an interaction between these moments. "Crystalline order" means that the magnetic free layer has a particular crystal structure, for example, face-centered cubic (FCC) or body-centered cubic (BCC).
[0016] In another aspect of the present application, a method for forming a memory structure is provided. In one embodiment of the present application, the method includes forming a non-magnetic pedestal region on an interconnect level, the interconnect level including a bottom electrode embedded in a first interconnect dielectric material layer. Then, a layer of seed metal, a layer of tunnel barrier seed material, a layer of chemical template material, an MTJ stack, and a top electrode layer are formed on the non-magnetic pedestal region. The top electrode layer, the MTJ stack, and the top portion of the layer of chemical template material are subjected to a first patterning process to provide the top electrode, the MTJ structure, and the top portion of the chemical template layer, respectively, the first patterning process including an etch that stops on a surface of the bottom portion of the layer of chemical template material. Then, a dielectric spacer is formed on the bottom portion of the layer of chemical template material and laterally adjacent to the top electrode, the MTJ structure, and the top portion of the chemical template layer. The lower portion of the layer of chemical template material, the layer of tunnel barrier seed material, the layer of seed metal, and the non-magnetic pedestal region are then subjected to a second patterning process using the dielectric spacer as an etch mask to provide a lower portion of the chemical template layer, a tunnel barrier seed layer, a seed metal layer, and a non-magnetic pedestal structure, respectively, the second patterning process including an etch to sputter non-oxidized metal particles from the non-magnetic pedestal region and redeposit the non-oxidized metal particles on at least a sidewall of the tunnel barrier seed layer.
[0017] In embodiments of the present application, the method may further include forming an encapsulation layer laterally adjacent to the dielectric spacer, the lower portion of the chemical template layer, the tunnel barrier seed layer, the seed metal layer, and the non-magnetic pedestal structure. In embodiments of the present application, the method may further include forming a second interconnect dielectric material layer on the encapsulation layer, the second interconnect dielectric material layer including a conductive structure embedded in the second interconnect dielectric material layer and contacting a top surface of the top electrode.
[0018] In an embodiment of the present application, the etch employed in the second patterning process is an ion beam etch, and the angle of the ion beam etch is between 0° and 45° with respect to the plane of the interconnect level.
[0019] These and other aspects of the present application will become more apparent from the drawings and detailed description of the present application which follow. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a cross-sectional view on an exemplary structure that may be used in accordance with one embodiment of the present application, the exemplary structure including an interconnect level including at least one bottom electrode embedded in a first interconnect dielectric material layer. [Diagram 2] 2 is a cross-sectional view of the exemplary structure shown in FIG. 1 after forming a non-magnetic pedestal region on an interconnect level. [Diagram 3] FIG. 3 is a cross-sectional view of the example structure shown in FIG. 2 after forming a layer of seed metal, a layer of tunnel barrier seed material, a layer of chemical template material, an MTJ stack, and a top electrode layer on the non-magnetic pedestal region. [Figure 4] FIG. 4 is a cross-sectional view of the exemplary structure shown in FIG. 3 after a first patterning is performed on the top electrode, the MTJ stack, and an upper portion of the layer of chemical template material to provide the top electrode, the MTJ structure, and an upper portion of the chemical template layer, respectively, where the first patterning includes an etch that terminates on, and thus physically exposes, a lower portion of the layer of chemical template material. [Diagram 5] FIG. 5 is a cross-sectional view of the exemplary structure shown in FIG. 4 after forming a dielectric spacer on the physically exposed lower portion of the layer of chemical template material and laterally adjacent to the top electrode, the MTJ structure, and the upper portion of the chemical template layer. [Figure 6]FIG. 6 is a cross-sectional view of the exemplary structure shown in FIG. 5 after the layer of chemical template material, the layer of tunnel barrier seed material, the layer of seed metal, and the non-magnetic pedestal region are second patterned using the dielectric spacer as an etch mask to provide a lower portion of the chemical template layer, the tunnel barrier seed layer, the seed metal layer, and the non-magnetic pedestal region, respectively, followed by forming an encapsulation layer. [Figure 7] FIG. 7 is a cross-sectional view of the example structure shown in FIG. 6 after forming a second interconnect dielectric material layer and forming a conductive structure in the second interconnect dielectric material layer and contacting the top surface of the MTJ structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present application will now be described in more detail with reference to the following description and the drawings accompanying the present application. It should be noted that the drawings in the present application are provided for illustrative purposes only and therefore the drawings are not drawn to scale. It should also be noted that like and corresponding elements are indicated with like reference numerals.
[0022] In the following description, numerous specific details are set forth, such as particular structures, components, materials, dimensions, processing steps, and techniques, to provide an understanding of various embodiments of the present application. However, those skilled in the art will understand that various embodiments of the present application may be practiced without these specific details. In other instances, well-known structures or processing steps have not been described in detail to avoid obscuring the present application.
[0023] When an element, such as a layer, region, or substrate, is described as being "on" or "over" another element, it will be understood that it can be directly on the other element, or there may be intervening elements. On the other hand, when an element is described as being "directly on" or "directly over" another element, there are no intervening elements. Also, when an element is described as being "beneath" or "under" another element, it will be understood that the element can be directly beneath or under the other element, or there may be intervening elements. On the other hand, when an element is described as being "directly beneath" or "directly under" another element, there are no intervening elements.
[0024] It should be noted that the figures of the present application illustrate memory device regions in which memory structures, such as, for example, MRAM structures, are formed. Non-memory device regions may be located laterally adjacent to the memory device regions illustrated in the figures of the present application. In the present application, the memory structures are formed on the back end. The memory structures of the present application may be used in a variety of memory applications, including, for example, STT MRAM devices.
[0025] Referring first to Figure 1, an exemplary structure that may be used in accordance with one embodiment of the present application is illustrated. The exemplary structure illustrated in Figure 1 includes an interconnect level that includes at least one bottom electrode 12 embedded in a first interconnect dielectric material layer 10. Although not shown, the bottom electrode 12 contacts a surface of a conductive structure (e.g., Cu lines and / or vias) that may also be embedded in the first interconnect dielectric material layer 10 or another interconnect dielectric material layer located below the first interconnect dielectric material layer 10.
[0026] Although this application illustrates a single bottom electrode embedded in the first interconnect dielectric material 10, this application is not limited to only a single bottom electrode embedded in the first interconnect dielectric material 10. Instead, this application works when multiple spaced apart bottom electrodes are embedded in the first interconnect dielectric material 10.
[0027] The interconnect level illustrated in FIG. 1 may be located above at least one underlying metal level (not shown) and a front-end-of-the-level (FEOL), also not shown. In some embodiments, the metal level may be a middle-of-the-line (MOL) level. In other embodiments, the metal level may be at least one lower interconnect level of a multi-level interconnect structure. In further embodiments, the metal level may be a combination of a MOL level and at least one lower interconnect level of a multi-level interconnect structure. The metal level may include conductive structures embedded in a layer of dielectric material. The FEOL may include a semiconductor substrate having one or more semiconductor devices (e.g., transistors, etc.) formed thereon. The metal level and the FEOL may be formed utilizing materials and techniques well known to those skilled in the art. As such, the materials and techniques used in providing the metal level and the FEOL are not described herein so as not to obscure the memory structures herein.
[0028] The first interconnect dielectric material layer 10 can be composed of any interconnect dielectric material including, for example, silicon dioxide, silsesquioxane, C-doped oxides (i.e., organosilicates) containing atoms of Si, C, O, and H, thermosetting polyarylene ethers, or multilayers thereof. The term "polyarylene" is used herein to describe aryl or inertly substituted aryl moieties linked by bonds, fused rings, or inert linking groups such as oxygen, sulfur, sulfone, sulfoxide, carbonyl, etc. The first interconnect dielectric material layer 10 can be formed using a deposition process such as, for example, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), or spin-on coating.
[0029] The bottom electrode 12 is comprised of a conductive material such as, for example, Ta, TaN, Ti, TiN, Ru, RuN, RuTa, RuTaN, Co, CoWP, CoN, W, WN, or any combination thereof. The bottom electrode 12 can have a thickness of 5 nm to 25 nm, although other thicknesses are possible and may be used herein as the thickness of the bottom electrode 12. The conductive material providing the bottom electrode 12 can be formed by a deposition process such as, for example, sputtering, CVD, PECVD, atomic layer deposition (ALD), physical vapor deposition (PVD), etc.
[0030] In some embodiments where the conductive structures are also embedded in the first interconnect dielectric material layer 10, the bottom electrode 12 can be formed by first recessing the conductive structures embedded in the first interconnect dielectric material layer 10, and then the conductive material providing the bottom electrode 12 is deposited on the recessed surface of the conductive structures embedded in the first interconnect dielectric material layer 10. A planarization process, such as chemical mechanical polishing (CMP), may be performed after deposition of the conductive material. In yet other embodiments where the conductive structures are not embedded in the first interconnect dielectric material layer 10, the bottom electrode 12 can be formed in one of two ways: In the first method, the first interconnect dielectric material layer 10 is deposited, openings are formed in the first interconnect dielectric material layer 10 by lithography and etching, then the conductive material providing the bottom electrode 12 is deposited in the opening, and then an optional planarization process may be employed. In the second method, a layer of conductive material is first deposited, then the layer of conductive material is patterned by lithography and etching to provide the bottom electrode 12, after which a first interconnect dielectric material layer 10 is deposited and planarized to provide the structure shown in FIG.
[0031] The bottom electrode 12 has a top surface that is substantially coplanar (within a few angstroms) with the top surface of the first interconnect dielectric material layer 10. The bottom electrode 12 may penetrate partially through the first interconnect dielectric material layer 10, or the bottom electrode 12 may penetrate completely through the first interconnect dielectric material layer 10. Note again that the bottom electrode 12 is in contact with the underlying conductive structure.
[0032] 2, there is shown the exemplary structure shown in FIG. 1 after forming a non-magnetic pedestal region 14 on the interconnect level. Notably, the non-magnetic pedestal region 14 is formed on the first interconnect dielectric material layer 10 and the bottom electrode 12. The non-magnetic pedestal region 14 has a smooth top surface, which is used herein to minimize roughness in subsequently formed layers in the exemplary structure.
[0033] The non-magnetic pedestal region 14 includes at least one non-magnetic metal-containing layer that is composed of a non-magnetic metal having a high sticking coefficient that has a low etch coefficient during the etching process that is performed after the deposition of the tunnel barrier seed material. As known to those skilled in the art, the term sticking coefficient is a term used to describe the ratio of the number of adatoms (or molecules) that adsorb or "stick" to a surface to the total number of atoms that strike that surface in the same time. The symbol SC is sometimes used to denote this coefficient, which has a value between 1 (all the striking atoms stick) and 0 (no atoms stick). This coefficient is a function of the surface temperature, surface coverage (θ), structural details, and kinetic energy of the striking particles. In this application, the term "high sticking coefficient" indicates that the non-magnetic metal that provides the non-magnetic metal pedestal region has a sticking coefficient SC of 0.5 to 1. The etch rate of a material refers to how quickly the material is removed when exposed to an etchant. The etch rate is usually expressed as a ratio of thickness to time (e.g., Å / min), but may also be expressed in terms of cycles. The etch rate may depend on the geometry, such as feature size or exposed area. In this application, the term "low etch rate" indicates that the non-magnetic metal has an etch rate of less than 10 Å / min.
[0034] Exemplary non-magnetic metals that can be used to provide the non-magnetic pedestal region 14 include, but are not limited to, Ta, TaN, Ti, TiN, or multi-layer combinations thereof. The non-magnetic metals providing the non-magnetic pedestal region 14 may be compositionally the same as the conductive materials described above for the bottom electrode 12, compositionally different, or both. In one example, the figures in this application illustrate the non-magnetic pedestal region 14 as a multi-layer structure including a first non-magnetic metal-containing layer 16L and a second non-magnetic metal-containing layer 18L. The first non-magnetic metal-containing layer 16L can be comprised of a first non-magnetic metal layer, and the second non-magnetic metal-containing layer 18L can be comprised of a second non-magnetic metal that is compositionally different from the first non-magnetic metal. In one example, the first non-magnetic metal-containing layer 16L can be comprised of Ti or Ta, and the second non-magnetic metal-containing layer 18L can be comprised of TaN or TiN.
[0035] The non-magnetic pedestal region 14 may be formed utilizing at least one deposition process, including but not limited to CVD, PECVD, ALD, PVD, sputtering, and the like. A planarization process follows the at least one deposition process to provide the non-magnetic pedestal region 14 with a smooth top surface, i.e., uppermost surface. The non-magnetic pedestal region 14 may have a thickness between 2 nm and 50 nm, although other thicknesses of the non-magnetic pedestal region 14 are contemplated and may be used as the thickness of the non-magnetic pedestal region 14. It should be noted that the individual non-magnetic metal-containing layers (16L, 18L) that provide the non-magnetic pedestal region 14 have a thickness less than the thickness of the non-magnetic pedestal region 14, but the thicknesses of the individual non-magnetic metal-containing layers (16L, 18L) add up to the thickness of the non-magnetic pedestal region 14.
[0036] 3, the exemplary structure shown in FIG. 2 is illustrated after forming a layer of seed metal 20L, a layer of tunnel barrier seed material 22L, a layer of chemical template material 24L, an MTJ stack S1, and a top electrode layer 32L on the non-magnetic pedestal region 14. The layer of seed metal 20L and the layer of tunnel barrier seed material 22L together provide the seed region of the exemplary structure. The MTJ stack S1 includes a top fixed MTJ stack including, from bottom to top, a layer of magnetic free material 26L, a layer of tunnel barrier material 28L, and a layer of magnetic reference material 30L. This top fixed MTJ stack is then patterned into a top fixed MTJ structure.
[0037] Each of the layer of seed metal 20L, the layer of tunnel barrier seed material 22L, the layer of chemical template material 24L, the MTJ stack S1, and the top electrode layer 32L can be formed by a deposition process, including, but not limited to, CVD, PECVD, PVD, ALD, or sputtering.
[0038] The layer of seed metal 20L formed on the top surface of the non-magnetic pedestal region 14 comprises a non-magnetic metal that promotes the growth of a layer of tunnel barrier seed material 22L. Exemplary non-magnetic metals that may be employed as the seed metal include, but are not limited to, Ta, Ti, or Mn3N. The seed metal 20L typically has a thickness of 1 nm to 10 nm, although other thicknesses of the layer of seed metal 20L are contemplated and may be used herein.
[0039] The layer of tunnel barrier seed material 22L formed on top of the layer of seed metal 20L has a thickness sufficient to induce magnetic or crystalline order in the layer of magnetic free material 26L of the MTJ stack S1. The tunnel barrier seed material includes, but is not limited to, magnesium oxide, aluminum oxide, titanium oxide, and the like. Typically, the layer of tunnel barrier seed material 22L has a thickness of 0.5 nm to 2 nm. It is noted that the layer of tunnel barrier seed material 22L is a thick seed layer that provides deposition control to the exemplary structure and helps to facilitate the growth of the subsequently formed layer of chemical template material 24L.
[0040] The layer of chemical template material 24L formed on the top surface of the layer of tunnel barrier seed material 22L is a crystallized solidification layer for the layer of magnetic free material 26L of the MTJ stack S1. That is, the layer of chemical template material 24L provides a desired crystal structure, e.g., FCC or BCC, for the subsequently formed layer of magnetic free material 26L of the MTJ stack S1. The layer of chemical template material 24L may be comprised of a metal alloy, e.g., CoAl, CoGe, CoGa, or CoSn. The layer of chemical template material 24L typically has a thickness of 1 nm to 10 nm, although other thicknesses of the layer of chemical template material 24L are contemplated and may be used herein.
[0041] The layer of magnetic free material 26L of the MTJ stack S1 that forms an interface with the underlying layer of chemical template material 24L has a magnetization that can be changed in orientation relative to the magnetization orientation of the layer of magnetic reference material 30L. The layer of magnetic free material 26L has magnetic and / or crystalline order, as defined above. The layer of magnetic free material 26L may have a thickness of 0.3 nm to 3 nm, although other thicknesses are possible and may be used as the thickness of the layer of magnetic free material 26L. The layer of magnetic free material 26L may be composed of a magnetic material or a stack of magnetic materials that are well known to those skilled in the art.
[0042] In some embodiments, the layer of magnetic free material 26L includes alloys and / or multilayers of cobalt, iron, cobalt-iron alloys, nickel, nickel-iron alloys, and cobalt-iron-boron alloys.
[0043] In another embodiment, the layer of magnetic free material 26L is composed of an ordered magnetic alloy. By "ordered magnetic alloy" is meant a magnetic alloy having a lattice structure in which atoms of one element occupy certain sites and atoms of at least one other element occupy other sites. In one embodiment, the ordered magnetic alloy providing the layer of magnetic free material 26L is a Heusler alloy. The term "Heusler alloy" is used herein to denote an intermetallic ternary compound of formula X2YX that possesses a Heusler half-Heusler crystal structure. Exemplary Heusler alloys that can be used herein include, but are not limited to, Mn3Ge, Mn3Ga, Co2MnSi, Mn3Sn, or Mn3Sb. In another embodiment, the ordered magnetic alloy providing the layer of magnetic free material 26L is an L10 alloy. The term "L10 alloy" refers to an intermetallic compound having a tetragonally centered body with one element occupying the corners of the lattice cells and the other element occupying the body portion of the lattice. Exemplary L10 alloys that may be used herein include, but are not limited to, MnAl or CoFe.
[0044] The layer of tunnel barrier material 28L is composed of an insulating material and is formed with a thickness sufficient to provide a suitable tunnel resistance. Exemplary insulating materials for the layer of tunnel barrier material 28L include, but are not limited to, magnesium oxide, aluminum oxide, titanium oxide, or materials with higher electrical tunnel conductivity, such as semiconductors or low band gap insulators. The thickness of the layer of tunnel barrier material 28L varies depending on the material selected. In one example, the layer of tunnel barrier material 28L may have a thickness of 0.5 nm to 1.5 nm, although other thicknesses are possible as long as the thickness of the layer of tunnel barrier material 28L provides a suitable tunnel resistance.
[0045] The layer of magnetic reference material 30L has a fixed magnetization. The layer of magnetic reference material 30L can be composed of a magnetic metal or magnetic metal alloy (or stack thereof) including one or more magnetic metals exhibiting high spin polarization at the tunnel barrier interface. In an alternative embodiment, exemplary magnetic metals for forming the layer of magnetic reference material 30L include iron, nickel, cobalt, chromium, boron, or manganese. Exemplary magnetic metal alloys can include the magnetic metals exemplified above for the layer of magnetic reference material 30L. In another embodiment, the layer of magnetic reference material 30L can be a multi-layer arrangement having (1) regions of high spin polarization formed of metals and metal alloys using the metals mentioned above or combinations thereof, and (2) regions composed of materials exhibiting strong perpendicular magnetic anisotropy (strong PMA). Exemplary materials with strong PMA that can be used include metals such as cobalt, nickel, platinum, palladium, iridium, or ruthenium, and can be arranged as alternating stacks. The strong PMA regions may also include alloys that exhibit strong intrinsic or bulk (as opposed to interfacial) PMA, with example alloys including cobalt-iron-terbium, cobalt-iron-gadolinium, cobalt-chromium-platinum, cobalt-platinum, cobalt-palladium, iron-platinum, or iron-palladium, or combinations thereof. The alloys may be arranged as alternating stacks. In one embodiment, combinations of these materials and regions may also be employed as layers of the magnetic reference material 30L.
[0046] In some embodiments, the layer of magnetic reference material 30L includes a multi-layer configuration including a lower magnetic reference layer, a synthetic antiferromagnetic coupling layer, and an upper magnetic reference layer. The lower magnetic reference layer can be composed of one of the magnetic materials described above for the layer of magnetic reference material 30L. The synthetic antiferromagnetic coupling layer can be composed of a non-magnetic material that can be coupled antiparallel to the lower and upper magnetic layers of this multi-layer structure that can be employed as the layer of magnetic reference material 30L. Exemplary non-magnetic materials that can be used as the synthetic antiferromagnetic coupling layer include, but are not limited to, ruthenium (Ru), iridium (Ir), or rhodium (Rh). In one embodiment, the synthetic antiferromagnetic coupling layer can have a thickness of 0.2 nm to 1.2 nm, although other thicknesses are possible and can be used as the thickness of the synthetic antiferromagnetic coupling layer. The upper magnetic reference layer can be composed of one of the magnetic materials described above for the magnetic reference layer 30L. Typically, in this multi-layer configuration embodiment, the upper magnetic reference layer is compositionally different from the lower magnetic reference layer.
[0047] In some embodiments (not shown), a layer of MTJ capping material can be formed between the layer of magnetic reference material 30L and the top electrode layer 32. If present, the MTJ capping material can include, but is not limited to, Nb, NbN, W, WN, Ta, TaN, Ti, TiN, Ru, Mo, Cr, V, Pd, Pt, Rh, Sc, Al, or other refractory metals or conductive metal nitrides. In some embodiments, no separate MTJ capping is formed, and the lower portion of the top electrode layer 32L can function as the capping layer. The layer of MTJ capping material can have a thickness of 2 nm to 25 nm, although other thicknesses are possible and may be used herein as the thickness of the layer of MTJ capping material.
[0048] The top electrode layer 32L includes one of the conductive materials described above for the bottom electrode 12. In one embodiment, the conductive material providing the top electrode layer 32L is compositionally the same as the conductive material providing the bottom electrode 12. In another embodiment, the conductive material providing the top electrode layer 32L is compositionally different from the conductive material providing the bottom electrode 12. The top electrode layer 32L can have a thickness of 5 nm to 100 nm, although other thicknesses are possible and may be used herein as the thickness of the top electrode layer 32L.
[0049] Referring now to FIG. 4, there is shown the example structure shown in FIG. 3 after a first patterning has been performed on the top electrode layer 32L, the MTJ stack S1, and the upper portion of the layer of chemical template material 24L, respectively, to provide the top electrode 32, the MTJ structure S2, and the upper portion of the chemical template layer (the upper portion of the chemical template layer is shown in the drawings of the present application as element 24u), where the first patterning includes an etch that stops on the surface of the lower portion of the layer of chemical template material 24L.
[0050] The first patterning includes a lithography process in which a patterned resist (not shown) is formed on the surface of the top electrode layer 32L. The patterned resist can be formed by depositing a photoresist material, exposing the photoresist material to a desired radiation pattern, and developing the exposed photoresist material. The patterned resist protects a portion of the top electrode layer 32L while leaving other portions of the top electrode layer 32L physically exposed. The physically exposed portions of the top electrode layer 32L are removed in an initial transfer etch. After the transfer etch, the patterned resist is removed using a conventional resist removal process, such as ashing. The first patterning continues using another etch in which the remaining top electrode layer 32L (hereafter top electrode 32) serves as an etch mask for this first patterning process. This other etch stops the lower portion of the layer of chemical template material 24L on the surface. This other etch removes a portion of the MTJ stack S1 and the upper portion of the layer of chemical template material 24L that is not covered by the top electrode 32. Hereinafter, the remaining portion of the MTJ stack S1 will be referred to as the MTJ structure S2, and the remaining upper portion of the layer of chemical template material 24L will be referred to as the upper chemical template layer portion 24u.
[0051] The transfer etch and subsequent etches may include ion beam etching, reactive ion beam etching, or a combination thereof. The transfer etch may be the same as or different from the other etches used in the first patterning step. For example, the transfer etch may include a reactive ion etch and the other etches may include an ion beam etch.
[0052] In some embodiments of the present application, the exemplary structure shown in FIG. 4 can be subjected to an oxygen treatment process or any other gas treatment process to remove unwanted metal particles that may have been redeposited on the sidewalls of the MTJ structure S2 during the first patterning.
[0053] The MTJ structure S2 typically has a width equal to the width of the top electrode 32 and the width of the top chemical template layer portion 24u. In some embodiments, the MTJ structure S2, the top electrode 32, and the top chemical template layer portion 24u may have a cylindrical shape. The MTJ structure S2 includes the remaining portions of each of the layer of magnetic free material 26L (hereinafter, magnetic free layer 26), the layer of tunnel barrier material 28L (hereinafter, tunnel barrier layer 28), and the layer of magnetic reference material 30L (hereinafter, magnetic reference layer 30). In some embodiments, each of the magnetic free layer 26, the tunnel barrier layer 28, and the magnetic reference layer 30 have sidewalls that are vertically aligned with each other and with the sidewalls of the top electrode 32 and the sidewalls of the top chemical template layer portion 24u. In other embodiments, the MTJ structure S2 may have a sloped profile with an angle between 1° and 45°.
[0054] 5, the exemplary structure shown in FIG. 4 is illustrated after forming a dielectric spacer 34 on a lower portion of the layer of chemical template material 24L and laterally adjacent to the top electrode 32, the MTJ structure S2, and the upper portion of the chemical template layer (i.e., the upper chemical template layer portion 24u). As shown in FIG. 5, the dielectric spacer 34 has a bottom surface in physical contact with the physically exposed surface of the lower portion of the layer of chemical template material 24L and vertical sidewalls in physical contact with each of the top electrode 32, the MTJ structure S2, and the upper chemical template layer portion 24u. The dielectric spacer 34 need not cover the entire sidewall of the top electrode 32.
[0055] The dielectric spacer 34 may be comprised of a dielectric spacer material, such as, for example, silicon dioxide, silicon nitride, silicon oxynitride, or a low-k material. The term "low-k material" refers to a dielectric material having a dielectric constant less than 4.0 (all dielectric constants referred to herein are relative to a vacuum unless otherwise noted). One example of a low-k material that may be employed as the spacer dielectric material is a dielectric material containing atoms of Si, C, O, and H. The dielectric spacer 34 may be formed by depositing a dielectric spacer material followed by a spacer etch. The deposition of the spacer dielectric material may include, but is not limited to, PVD or PECVD. The spacer etch may include reactive ion etching or ion beam etching. The dielectric spacer 34 may have an upper portion having a first thickness and a lower portion having a second thickness greater than the first thickness.
[0056] 6, the exemplary structure shown in FIG. 5 is illustrated after a second patterning of the lower portion of the layer of chemical template material 24L, the layer of tunnel barrier seed material 22L, the layer of seed metal 20L, and the non-magnetic pedestal region 14 to provide the lower portion of the chemical template layer (hereinafter lower chemical template layer portion 24b), the tunnel barrier seed layer 22, the seed metal layer 20, and the non-magnetic pedestal structure 14S, respectively, followed by formation of an encapsulation layer 38. In an embodiment, the etch employed in the second patterning is an ion beam etch, with the angle of the ion beam etch being between 0° and 45°, more typically between 0° and 25°, relative to the plane of the interconnect level including the bottom electrode 12. In some embodiments, a portion of the first interconnect dielectric material layer 10 may be recessed during the second patterning process, as shown in FIG.
[0057] It should be noted that lower chemical template layer portion 24b and upper chemical template layer portion 24u combine to provide the chemical template layer of the present application. As shown, upper chemical template layer portion 24u of the chemical template layer has a width that is less than the width of lower chemical template layer portion 24b of the chemical template layer.
[0058] In an embodiment, the non-magnetic pedestal structure 14S may include a bilayer structure including the remaining portion of the first non-magnetic metal-containing layer 16L (hereinafter, the first non-magnetic metal-containing base layer 16) and the remaining portion of the second non-magnetic metal-containing layer 18L (hereinafter, the second non-magnetic metal-containing base layer 18). The non-magnetic pedestal portion 14S has a width greater than the width of the MTJ structure S2. The width of the non-magnetic pedestal portion 14S may be the same as or greater than the width of the seed region including the seed metal layer 20 and the tunnel barrier seed layer 22. The width of the seed region including the seed metal layer 20 and the tunnel barrier seed layer 22 is greater than the width of the MTJ structure S2. In this manner, the increased width of the seed region including the seed metal layer 20 and the tunnel barrier seed layer 22 relative to the MTJ structure S2 reduces the resistance of the memory structure of the present application. In some embodiments, when the width of the seed region is three times greater than the width of the MTJ structure S2, the resistance of the memory structure may be reduced by about an order of magnitude.
[0059] The second patterning includes an etch that uses the dielectric spacer 34 as an etch mask to sputter non-oxidized metal particles from the non-magnetic pedestal region 14 and redeposits the non-oxidized metal particles on at least the sidewalls of the tunnel barrier seed layer 22. That is, the etch used in the second patterning process forms a layer of non-oxidized metal residue 36 on at least the sidewalls of the tunnel barrier seed layer 22. This layer of non-oxidized metal residue 36 intentionally shunts at least the seed region, which in this application is a region of the structure including the tunnel barrier seed layer 22 and the seed metal layer 20. The layer of non-oxidized metal residue 36 forms a ring laterally adjacent to at least the seed region. The layer of non-oxidized metal residue 36 includes at least one metal, such as Ta, present in the non-magnetic pedestal structure 14S.
[0060] In addition to being present on at least the seed region, in some embodiments, the layer of non-oxidized metal residue 36 may extend onto the sidewalls of the lower portion of the chemical template layer, i.e., lower chemical template layer portion 24b. In other embodiments, the layer of non-oxidized metal residue 36 may also extend onto the sidewalls of the dielectric spacers 34. In the exemplary embodiment shown in FIG. 6, the layer of non-oxidized metal residue 36 extends onto the sidewalls of each of the non-magnetic pedestal structure 14S, the lower portion of the chemical template layer (i.e., lower chemical template layer portion 24b), and the dielectric spacers 34.
[0061] The layer of non-oxidized metal residue 36 that is formed may be a continuous layer or a discontinuous layer containing some gaps. The layer of non-oxidized metal residue 36 may have a thickness of 0.1 nm to 3 nm.
[0062] An encapsulation layer 38 laterally surrounds the top electrode 32, the MTJ structure S2, the chemical template layer (including upper chemical template layer portion 24u and lower chemical template layer portion 24b), the seed region, and the non-magnetic pedestal structure 14S. The encapsulation layer 38 is also formed on the top electrode 32 and on a surface of the first interconnect dielectric material layer 10.
[0063] The encapsulation layer 38 is comprised of a dielectric material capable of providing passivation to the top electrode 32 and the MTJ structure S2. In one embodiment, the encapsulation layer 38 is comprised of silicon nitride. In another embodiment, the encapsulation layer 38 can be comprised of a dielectric material containing atoms of silicon, carbon, and hydrogen. In some embodiments, in addition to atoms of carbon and hydrogen, the dielectric material providing the encapsulation layer 38 can include atoms of at least one of nitrogen and oxygen. In other embodiments, in addition to atoms of silicon, nitrogen, carbon, and hydrogen, the dielectric material providing the encapsulation layer 38 can include atoms of boron. In one example, the encapsulation layer 38 can be comprised of an nBLOK dielectric material containing atoms of silicon, carbon, hydrogen, nitrogen, and oxygen. In an alternative example, the encapsulation layer 38 can be comprised of a SiBCN dielectric material containing atoms of silicon, boron, carbon, hydrogen, and nitrogen.
[0064] The encapsulation layer 38 may be formed by depositing a continuous layer of a dielectric material that provides the encapsulation layer 38. The deposition may include, but is not limited to, CVD, PECVD, PVD, ALD, or spin-on coating. The encapsulation layer 38 may have a thickness of 10 nm to 200 nm. Other thicknesses are possible and may be employed for the thickness of the encapsulation layer 38.
[0065] 7, the exemplary structure shown in FIG. 6 is illustrated after forming a second interconnect dielectric material layer 40, forming a conductive structure 44 in the second interconnect dielectric material layer 40, and contacting the top electrode 32. The second interconnect dielectric material layer 40 may include one of the dielectric materials described above for the first interconnect dielectric material layer 10. The dielectric material providing the second interconnect dielectric material layer 40 may be compositionally the same as or compositionally different from the dielectric material providing the first interconnect dielectric material layer 10. The second interconnect dielectric material layer 40 may be formed utilizing one of the deposition processes described above for forming the first interconnect dielectric material layer 10. Planarization may be performed after the deposition process. As shown, the second interconnect dielectric material layer 40 is laterally adjacent to and above the encapsulation layer 38.
[0066] The conductive structure 44 is comprised of a contact metal or contact metal alloy, such as, for example, Cu, Al, W, Co, or alloys thereof. In some embodiments, the diffusion barrier liner 42 is formed along the sidewalls and bottom wall of the conductive structure 44. In some embodiments, there is no diffusion barrier liner. The diffusion barrier liner 42 is comprised of a diffusion barrier material (i.e., a material that acts as a barrier to prevent a conductive material, such as copper, from diffusing therethrough). Examples of diffusion barrier materials that can be used in providing the diffusion barrier liner include, but are not limited to, Ta, TaN, Ti, TiN, Ru, RuN, RuTa, RuTaN, W, or WN. In some embodiments, the diffusion barrier material can include a material stack of diffusion barrier materials. In one example, the diffusion barrier material can be comprised of a stack of Ta / TaN.
[0067] The conductive structure 44 and optional diffusion barrier liner 42 may be formed by first providing a contact opening in the second interconnect dielectric material layer 40, the contact opening extending downward and physically exposing at least the top surface of the top electrode 32. The contact opening may be formed by photolithography and etching. An optional diffusion barrier material layer and a contact metal-containing layer are then formed inside and outside the contact opening. A planarization process is then used to remove the optional diffusion barrier material layer and the contact metal-containing layer formed outside the contact opening, while retaining the optional diffusion barrier material layer and the contact metal-containing layer formed inside the contact opening. The retained optional diffusion barrier layer provides the optional diffusion barrier liner 42, and the retained contact metal-containing layer provides the conductive structure 44.
[0068] While the present application has been particularly shown and described with respect to preferred embodiments thereof, it will be understood by those skilled in the art that the foregoing and other changes in form and detail may be made without departing from the spirit and scope of the present application. It is therefore intended that the present application not be limited to the exact forms and details described and illustrated, but fall within the scope of the appended claims.
Claims
1. 1. A memory structure comprising: a bottom electrode embedded in a first layer of interconnect dielectric material; a non-magnetic pedestal structure overlying the bottom electrode and a portion of the first layer of interconnect dielectric material; a seed region having a first width and located on the non-magnetic pedestal structure, the seed region including at least a tunnel barrier seed layer; a chemical template layer overlying the seed region; and a magnetic tunnel junction (MTJ) structure having a second width and located on the chemical template layer, the second width being less than the first width; a top electrode overlying the MTJ structure; a layer of non-oxidized metal residue located at least on sidewalls of said tunnel barrier seed layer and intentionally shunting at least said seed region.
2. 2. The memory structure of claim 1, wherein said chemical template layer comprises an upper portion and a lower portion, said lower portion having a width greater than said upper portion and forming an interface with said tunnel barrier seed layer.
3. The memory structure of claim 2 further comprising a dielectric spacer located on sidewalls of said MTJ structure and said top electrode and having a bottom surface located on said lower portion of said chemical template layer.
4. 4. The memory structure of claim 3 further comprising an encapsulation layer located laterally adjacent said dielectric spacers, said seed region and said non-magnetic pedestal structure and having a bottom surface located on a surface of said first interconnect dielectric material layer.
5. 5. The memory structure of claim 4 further comprising a second interconnect dielectric material layer laterally adjacent to and above said encapsulation layer.
6. 6. The memory structure of claim 5 further comprising a conductive structure embedded in said second layer of interconnect dielectric material and contacting said top electrode.
7. The memory structure of claim 6 wherein said conductive structure has a third width that is greater than at least said second width of said MTJ structure.
8. 2. The memory structure of claim 1 wherein said layer of non-oxidized metallic residue extends onto sidewalls of said non-magnetic pedestal structure.
9. 2. The memory structure of claim 1, wherein the layer of non-oxidized metal residue extends onto sidewalls of a lower portion of the chemical template layer.
10. 10. The memory structure of claim 9, wherein the layer of non-oxidized metal residue extends onto sidewalls of at least a dielectric spacer located laterally adjacent to the MTJ structure.
11. 2. The memory structure of claim 1 , wherein the layer of non-oxidized metal residue extends over sidewalls of the non-magnetic pedestal structure, the lower portion of the chemical template layer, and at least each of the dielectric spacers located laterally adjacent to the MTJ structure.
12. 2. The memory structure of claim 1, wherein said seed region further comprises a seed metal layer underlying said tunnel barrier seed layer.
13. 2. The memory structure of claim 1, wherein the MTJ structure is a top fixed MTJ structure comprising, from bottom to top, a magnetic free layer, a tunnel barrier layer, and a magnetic reference layer.
14. The memory structure of claim 13 wherein the magnetic free layer comprises an ordered magnetic alloy.
15. 15. The memory structure of claim 14, wherein said ordered magnetic alloy is a Heusler alloy or an L10 alloy.
16. The memory structure of claim 13 wherein the magnetic reference layers comprise a single magnetic reference layer.
17. 14. The memory structure of claim 13 wherein the magnetic reference layers comprise a bottom magnetic reference layer, a synthetic antiferromagnetically coupled layer, and a top magnetic reference layer.
18. 2. The memory structure of claim 1, wherein said non-magnetic pedestal structure has a width greater than at least said second width of said MTJ structure, and said top electrode has a width equal to said second width of said MTJ structure.
19. 2. The memory structure of claim 1 wherein said layer of non-oxidized metallic residue comprises at least one metal present in a non-magnetic pedestal structure.
20. The memory structure of claim 1 , wherein the chemical template layer is a crystallized solidification layer for a magnetic free layer of the MTJ structure.
21. 2. The memory structure of claim 1, wherein said tunnel barrier seed layer has a thickness sufficient to induce magnetic or crystalline order in a magnetic free layer of said MTJ structure.
22. 1. A method of forming a memory structure, comprising: forming a non-magnetic pedestal region on an interconnect level, the interconnect level including a bottom electrode embedded in a first layer of interconnect dielectric material; forming a layer of seed metal, a layer of tunnel barrier seed material, a layer of chemical template material, an MTJ stack, and a top electrode layer on the non-magnetic pedestal region; performing a first patterning on the top electrode layer, the MTJ stack, and an upper portion of the layer of chemical template material to provide a top electrode, an MTJ structure, and an upper portion of a chemical template layer, respectively, the first patterning comprising an etch that stops on a surface of a lower portion of the layer of chemical template material; forming a dielectric spacer on the lower portion of the layer of chemical template material and laterally adjacent to the top electrode, the MTJ structure, and the upper portion of the chemical template layer; and performing a second patterning on the lower portion of the layer of chemical template material, the layer of tunnel barrier seed material, the layer of seed metal, and the non-magnetic pedestal region using the dielectric spacer as an etch mask to provide a lower portion of the chemical template layer, a tunnel barrier seed layer, a seed metal layer, and a non-magnetic pedestal structure, respectively, the second patterning including an etch that sputters non-oxidized metal particles from the non-magnetic pedestal region and redeposits the non-oxidized metal particles on at least a sidewall of the tunnel barrier seed layer.
23. 23. The method of claim 22, further comprising forming an encapsulation layer laterally adjacent to the dielectric spacer, the lower portion of the chemical template layer, the tunnel barrier seed layer, the seed metal layer, and the non-magnetic pedestal structure.
24. 24. The method of claim 23, further comprising forming a second interconnect dielectric material layer over the encapsulation layer, the second interconnect dielectric material layer comprising a conductive structure embedded in the second interconnect dielectric material layer and contacting a top surface of the top electrode.
25. 23. The method of claim 22, wherein the etch employed in the second patterning is an ion beam etch, and the angle of the ion beam etch is between 0° and 45° with respect to a plane of an interconnect level.
Citation Information
Patent Citations
Method of manufacturing tunnel magnetoresistance effect element, method of manufacturing thin-film magnetic head, and method of manufacturing memory element
JP2001203408A
Magneto-resistance effect element, and magnetic memory
JP2008098523A
Method and system for providing magnetic junction having improved characteristic
JP2014120707A
Magnetoresistance effect element, method of manufacturing magnetoresistance effect element and magnetic memory
JP2015179694A
Magnetic resistance element and electronic device
JP2018032805A