Method for producing lithium carbonate coating for nickel-based cathodes and electrochemical cells using same

A cost-effective method using gaseous carbon dioxide and water vapor to form a lithium carbonate coating on nickel-based cathode materials addresses the complexity and cost issues of existing coating techniques, enhancing electrochemical cell stability and performance by reducing interfacial resistance and maintaining discharge capacity.

JP2024544403APending Publication Date: 2024-11-29SOLID POWER OPERATING INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024536279
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-17
Filing Date
2022-12-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Current methods for forming coatings on high energy density cathode materials to prevent reaction with electrolytes are complex and expensive, requiring specialized equipment and high temperatures, and do not effectively reduce interfacial resistance or improve cycle life and rate performance.

Method used

A method involving exposure of a nickel-based cathode material to gaseous carbon dioxide and water vapor at controlled conditions forms a lithium carbonate coating, which acts as a barrier between the cathode and electrolyte, reducing interfacial resistance and enhancing cycle life and rate performance without the need for specialized equipment.

Benefits of technology

The lithium carbonate coating significantly improves the stability and performance of electrochemical cells by maintaining discharge capacity and reducing degradation, with solid state battery cells achieving at least 85% of their initial capacity after three cycles and showing improved starting discharge capacity compared to uncoated materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544403000001_ABST
    Figure 2024544403000001_ABST
Patent Text Reader

Abstract

A method for producing a lithium carbonate coated cathode containing convertible lithium by growing lithium carbonate on the surface by exposure to carbon dioxide. An electrochemical cell including a lithium carbonate coated cathode having an outer lithium carbonate coating having a thickness in the range of about 2 nanometers to about 1 micron.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is related to and claims priority under U.S. Provisional Application No. 63 / 265,672, entitled "Method for Production of Lithium Carbonate Coating for Nickel-Based Cathodes and Electrochemical Cells Using Same," filed on December 17, 2021, the entire contents of which are hereby fully incorporated by reference into this disclosure for all purposes.

[0002] Various embodiments described in this disclosure relate to the field of primary and secondary electrochemical cells, electrodes and electrode materials including lithium carbonate coated components, and corresponding methods of making and using the same. [Background technology]

[0003] For lithium rechargeable batteries to meet increasing energy density demands, researchers have turned to high energy density oxide-based cathode materials, such as the NMC class of oxides, to power today's batteries. Unfortunately, when these high energy density materials come into direct contact with solid or liquid electrolytes, they can react and decompose, resulting in increased interfacial resistance, capacity loss, and reduced rate performance during cycling. One way to prevent this degradation has been to form a coating on the cathode material to act as a buffer between the cathode and the electrolyte used. Current methods for forming these coatings include techniques such as atomic layer deposition, described in WO 2016 / 196688 A8. However, this method requires specialized equipment and high temperature operating conditions, making the process complex and expensive. In this disclosure, methods are described that are designed to create cost-effective coatings that not only reduce interfacial resistance, increase cycle life, and improve rate performance, but also reduce the need to use multi-step reactions or specialized equipment.

SUMMARY OF THE INVENTION

[0004] Disclosed herein is a method for manufacturing a cathode for an electrochemical cell, the cathode being coated with lithium carbonate, the method comprising exposing a nickel-based cathode material containing lithium and oxygen in a molar ratio of 1:2 to gaseous carbon dioxide and water vapor, and incubating the nickel-based cathode material and carbon dioxide at a predetermined time (e.g., period), a predetermined temperature, a predetermined pressure, and / or a predetermined relative humidity level, wherein lithium carbonate is formed as a layer on the outer surface of the cathode material to form a cathode coated with lithium carbonate.

[0005] In some embodiments, the nickel-based cathode material has the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1). In another embodiment of the method, the nickel-based cathode material is NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O2), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O2), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O2), or a combination thereof. In yet another embodiment, the nickel-based cathode material is LiNiO2, LiNi 1-Y Co Y O2, LiNi 1-Y Mn Y O2 (where 0 ≤ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, and a + b + c = 2), LiMn 2-ZNi Z O4, Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1) or a combination thereof, including one or more of the coated or uncoated metal oxides. In yet other embodiments, the nickel-based cathode material is V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≤ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≤ Z ≤ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 O4, or a combination thereof, further including one or more of the coated or uncoated metal oxides. In still another embodiment, the nickel-based cathode material further includes one or more of the coated or uncoated metal sulfides including titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), nickel sulfide (Ni3S2), lithium sulfide (Li2S), or a combination thereof.

[0006] In some embodiments, the exposure step includes applying high pressure to increase the growth rate of the lithium carbonate coating. In some further embodiments, the exposure step includes applying high temperature to increase the growth rate of the lithium carbonate coating.

[0007] In some embodiments, the predetermined temperature ranges from about 20°C to about 120°C.

[0008] In some embodiments, the exposing step comprises applying a high concentration of gaseous carbon dioxide for a predetermined period of time to increase the growth rate of the lithium carbonate coating. In some further embodiments, the exposing step comprises applying a high concentration of gaseous carbon dioxide for a predetermined period of time to increase the growth rate of the lithium carbonate coating.

[0009] In some embodiments, the exposing step comprises applying a high concentration of water vapor for a predetermined period of time to increase the growth rate of the lithium carbonate coating. In some further embodiments, the exposing step comprises applying a high concentration of water vapor for a predetermined period of time to increase the growth rate of the lithium carbonate coating.

[0010] In some embodiments, the nickel-based cathode material is coated with a lithium-containing layer prior to exposure to gaseous carbon dioxide and water vapor.

[0011] In some embodiments, the lithium-containing layer comprises Li2ZrO3, Li2ZrO4, LiCl, LiF, LiOH, Li2O, lithium niobate, lithium nitride, lithium titanate, lithium silicate, or a combination thereof.

[0012] In some embodiments, the nickel-based cathode material is not treated prior to exposure to gaseous carbon dioxide and water vapor.

[0013] In some embodiments, the lithium carbonate coating has a thickness in the range of about 5 nanometers to about 1 micrometer.

[0014] In some embodiments, the method further comprises vacuum drying the lithium carbonate coated cathode to remove residual moisture.

[0015] In some embodiments, the method further comprises washing the coated cathode with lithium carbonate.

[0016] In some embodiments, the method includes combining the lithium carbonate coated cathode with one or more of a suitable binder, a solid electrolyte, and a conductive additive to form a cathode for an electrochemical cell.

[0017] In some embodiments, the method further includes combining the lithium carbonate coated cathode with an anode and a separator to form a functioning electrochemical cell.

[0018] Further provided in the present disclosure is an electrochemical cell including a lithium carbonate coated cathode having an outer lithium carbonate coating having a thickness in the range of about 2 nanometers to about 1 micron.

[0019] Further provided in the present disclosure is a method for producing a lithium carbonate uniformly coated cathode in a gas mode, the method generally comprising contacting gaseous carbon dioxide and water vapor with a nickel-based cathode material containing lithium and oxygen, and producing a lithium carbonate uniformly coated cathode in a gas mode, where the lithium carbonate is uniformly formed as a layer on an outer surface of the cathode material to form a lithium carbonate coated cathode.

[0020] In some embodiments, the method further comprises contacting the nickel-based cathode material with carbon dioxide at a predetermined relative humidity level, hi some further embodiments, the method further comprises contacting the nickel-based cathode material with carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, or at a predetermined relative humidity level.

[0021] In some embodiments, the cathode material comprises a 1:2 molar ratio of lithium and oxygen.

[0022] In some embodiments, the nickel-based cathode material includes a catalytic amount of nickel.

[0023] In some embodiments, the uniform lithium carbonate coating has a thickness in the range of about 5 nanometers to 1 micrometer. In some aspects, the uniform lithium carbonate coating has a thickness in the range of about 1 nanometer to about 100 nanometers, about 1 nanometer to about 50 nanometers, or about 10 nanometers to about 40 nanometers.

[0024] Furthermore, in the present disclosure, a solid-state battery cell comprising a nickel-based cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), wherein the nickel-based cathode material is a cathode uniformly coated with lithium carbonate, and the solid-state battery cell maintains 85% or more, 90% or more, 95% or more, 98% or more, or 99% or more of its discharge capacity after 3 cycles, is provided.

[0025] Furthermore, in the present disclosure, a solid-state battery cell comprising a nickel-based cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), wherein the nickel-based cathode material is uniformly coated with lithium carbonate, and the solid-state battery cell has a higher initial discharge capacity compared to the same nickel-based cathode material without the lithium carbonate coating, is provided.

[0026] Furthermore, in the present disclosure, a cathode composition comprising a cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1) and a lithium carbonate layer, wherein the cathode material is uniformly coated with the lithium carbonate layer, is provided. In some embodiments, the lithium carbonate layer has a thickness in the range of about 1 nanometer to about 1 micron.

[0027] In some embodiments, the cathode material is LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.4 Mn 0.3 Co 0.3 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiNi 0.85 Mn 0.05 Co 0.1 O2, and is selected from the group consisting of any combination thereof.

[0028] In some further embodiments, the cathode material further comprises a metal oxide. In some aspects, the metal oxide is LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≦ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≦ Z ≦ 2), Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), and is selected from the group consisting of any combination thereof. In other embodiments, the metal oxide is V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≦ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≦ Z ≦ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4O2, LiMn 1.5 Ni 0.5 It is selected from the group consisting of O4 and any combination thereof.

[0029] In some embodiments, the lithium carbonate layer is formed in a gas mode.

[0030] Furthermore, in the present disclosure, a cathode composition comprising a cathode material including LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≤ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≤ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≤ Z ≤ 2), or Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), and a lithium carbonate layer, and the cathode material is uniformly coated with the lithium carbonate layer, is provided. In some embodiments, the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

[0031] Furthermore, in the present disclosure, a cathode composition comprising V2O5, V6O 13、 MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≤ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≤ Z ≤ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, or LiMn 1.5 Ni 0.5There is further provided a cathode composition comprising a cathode material comprising O4 and a lithium carbonate layer, the cathode material being uniformly coated with the lithium carbonate layer, in some embodiments, the lithium carbonate layer having a thickness of about 1 nanometer to about 1 micron.

[0032] The present disclosure further provides a method for producing a lithium carbonate coated cathode for an electrochemical cell in a gaseous manner, comprising exposing a nickel-based cathode material comprising a 1:2 molar ratio of lithium and oxygen to gaseous carbon dioxide and water vapor, and incubating the nickel-based cathode material and carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, and / or at a predetermined relative humidity level, wherein lithium carbonate forms as a uniform layer on the outer surface of the cathode material to form a lithium carbonate coated cathode. [Brief description of the drawings]

[0033] The present disclosure will be understood by reference to the following detailed description in conjunction with the drawings, which are briefly described below. It should be noted that for clarity of illustration, certain elements in the drawings may not be drawn to scale.

[0034] [Figure 1] FIG. 1 is a schematic cross-sectional view of an example of an uncoated and coated cathode material, according to one embodiment.

[0035] [Diagram 2] FIG. 2 is a schematic cross-sectional view of an example of a coated cathode material used in the construction of an electrochemical cell, according to one embodiment.

[0036] [Diagram 3] FIG. 3 is a flow chart of a process for growing a lithium carbonate layer on a cathode material and using the resulting material in an electrochemical cell, according to one embodiment.

[0037] [Figure 4A] 4A shows a chart demonstrating the difference between coated and uncoated cathode materials with respect to performance in an electrochemical cell according to one embodiment. FIG 4A shows the performance of an electrochemical cell including the coated cathode material of Example 1 and the uncoated cathode material of Comparative Example 1. [Figure 4B] 4B shows a chart demonstrating the difference between coated and uncoated cathode materials with respect to performance in an electrochemical cell according to one embodiment. FIG. 4B shows the performance of an electrochemical cell including the coated cathode material of Example 2 and the uncoated cathode material of Comparative Example 2.

[0038] [Diagram 5] FIG. 5 is an attenuated total reflectance Fourier transform infrared (ATR-FTIR) spectroscopy scan showing the presence of Li2CO3 on a coated NMC 622 (LiNiO.6MnO.2CoO.2O2) material compared to an uncoated NMC 622 (LiNiO.6MnO.2CoO.2O2) material, according to one embodiment.

[0039] [Figure 6] FIG. 6 is an ATR-FTIR spectroscopic scan showing the presence of Li2CO3 on a coated NMC 851005 (LiNi0.85Mn0.05Co0.1O2) material compared to an uncoated NMC 851005 (LiNi0.85Mn0.05Co0.1O2) material, according to one embodiment.

[0040] [Figure 7]FIG. 7 is an ATR-FTIR spectroscopic scan of Comparative Example 3 showing the absence of Li2CO3 on the NMC 622 (LiNiO.6MnO.2CoO.2O) material after exposure to relative humidity levels outside the range of an enablement embodiment, and Examples 3-5 showing the presence of Li2CO3 on the NMC 622 (LiNiO.6MnO.2CoO.2O) material after exposure to relative humidity within the required humidity limits, in accordance with an embodiment.

[0041] [Figure 8] FIG. 8 is an ATR-FTIR spectroscopic scan of original uncoated NMC-622 particles (Example 6-A), NMC-622 material after exposure to relative humidity within the required humidity limits according to one embodiment (Example 6-B), original uncoated LMO material (Comparative Example 4-A), LMO material after exposure to relative humidity within the required humidity limits according to one embodiment (Comparative Example 4-B), original uncoated LCO particles (Comparative Example 5-A), and LCO material after exposure to relative humidity within the required humidity limits according to one embodiment (Comparative Example 5-B).

[0042] [Figure 9] FIG. 9 is an ATR-FTIR spectroscopic scan of original uncoated NMC-622 particles (Example 6-A), NMC-622 material after exposure to relative humidity within the required humidity limits according to one embodiment (Example 6-C), original uncoated NMC 851005 particles (Example 7-A), and NMC 851005 material after exposure to relative humidity within the required humidity limits according to one embodiment (Example 7-B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] In the following description, specific details are provided to give a complete understanding of various embodiments of the present disclosure. However, after reading and understanding the specification, claims, and drawings, those skilled in the art will understand that some embodiments of the present disclosure can be implemented without following some of the specific details described in the present disclosure. Furthermore, to avoid obscuring the present disclosure, some well-known methods, processes, devices, and systems that find application in various embodiments described in the present disclosure are not disclosed in detail.

[0044] In the present disclosure, a composition for use in an electrochemical cell is provided. The composition generally includes a cathode material and a uniform lithium carbonate layer. The uniform lithium carbonate layer completely coats the cathode material. The lithium carbonate layer acts as a barrier between the cathode material and the solid electrolyte, thereby improving the stability of the electrochemical cell.

[0045] The cathode material may include a nickel-manganese-cobalt (NMC) material. The NMC material may have an average particle size of about 1 micron to about 20 microns. The NMC material can have the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1). In an exemplary embodiment, the NMC material is NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O2), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O2), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O2), NMC 851005 (LiNi 0.85 Mn 0.05 Co0.1 It may include O2), or any combination thereof.

[0046] In another embodiment, the cathode material may include a metal oxide. The metal oxide may be LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≦ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≦ Z ≦ 2), Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), or any combination thereof. In another embodiment, the metal oxide may be V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≦ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≦ Z ≦ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 O4, or any combination thereof.

[0047] The lithium carbonate layer having a uniform composition can have a thickness of about 1 nanometer to about 1 micron, for example, the thickness of the lithium carbonate layer can be about 1 nanometer to about 5 nanometers, about 1 nanometer to about 10 nanometers, about 1 nanometer to about 20 nanometers, about 1 nanometer to about 50 nanometers, about 1 nanometer to about 100 nanometers, about 1 nanometer to about 250 nanometers, about 1 nanometer to about 500 nanometers, about 1 nanometer to about 750 nanometers, about 1 nanometer to about 1 micron, about 5 nanometers to about 1 micron, about 10 nanometers to about 1 micron, about 20 nanometers to about 1 micron, about 50 nanometers to about 1 micron, about 100 nanometers to about 1 micron, about 250 nanometers to about 1 micron, about 500 nanometers to about 1 micron, or about 750 nanometers to about 1 micron. In some embodiments, the thickness can be about 5 nanometers to about 750 nanometers. In another embodiment, the thickness can be from about 10 nanometers to about 500 nanometers. In a further embodiment, the thickness can be from about 15 nanometers to about 250 nanometers. In yet another embodiment, the thickness can be from about 17 nanometers to about 100 nanometers. In another embodiment, the thickness can be from about 20 nanometers to about 50 nanometers. As used in this disclosure, the term "uniform" with respect to the lithium carbonate layer is understood to include a lithium carbonate layer that is uniformly coated, completely covering the surface of the cathode layer (i.e., there are no uncovered portions of the cathode) and / or is coated such that the resulting composition does not have uncovered surface areas that may be found with liquid deposition or spraying techniques.

[0048] Preferably, the uniform lithium carbonate coating layer is formed in a gaseous manner. A gaseous formed lithium carbonate coating layer can be formed by contacting gaseous carbon dioxide and water vapor with a cathode material comprising lithium and oxygen, as further described below.

[0049] Figure 1 is a schematic cross-sectional view of an example of an uncoated and coated cathode material. The uncoated cathode material 100 can be, for example, particles of an NMC (nickel-manganese-cobalt) material in a size range of about 1 to 20 microns in diameter. The NMC material can, stoichiometrically, be in the form of LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1). Generally, NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O2), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O2), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O2), NMC 851005 (LiNi 0.85 Mn 0.05 Co 0.1 O2), or any combination thereof. In an NMC material that does not contain excess lithium, the ratio of the molar fraction of lithium to the molar fraction of oxygen of 2 is fixed. Any lithium that exceeds this ratio can be called "excess lithium", and any lithium within the range of this ratio can be called "convertible lithium". The lithium contained in the uncoated cathode material 100 can move to the lithium carbonate layer growing on the surface of the coated cathode material 120 and be in a convertible chemical state without adversely affecting the electrochemical performance or structure of the uncoated cathode material 100. The uncoated cathode material 100 must contain nickel and may also contain lithium, manganese, oxygen, cobalt, aluminum, and other transition metals.

[0050] The coated cathode material 120 includes an inner portion 130 having a lithium content that is less than the lithium content of the uncoated cathode material 100 due to the movement of lithium to the outer grown lithium carbonate layer 140. In one embodiment, the amount of lithium is gradient in the coated cathode material, and the outer portion has an increased amount of lithium compared to the amount of lithium in the inner portion. Although shown as ideal spherical particles, the uncoated cathode material 100 and the coated cathode material 120 can be of a shape / size that allows for the growth of lithium carbonate and may have variable surface textures / roughnesses that occur either initially or after the growth of lithium carbonate. The resulting lithium carbonate layer acts as a barrier between the NMC and the contacting solid electrolyte, improving cell stability. Without the coating, the NMC cathode material can react with the solid electrolyte, potentially leading to the failure of any electrochemical cell fabricated using such an uncoated NMC cathode material.

[0051] In another embodiment, the coated cathode material 120 is LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≦ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≦ Z ≦ 2), Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), or one or more of the coated or uncoated metal oxides such as, but not limited to, these, and combinations thereof.

[0052] In yet another embodiment, the coated cathode material 120 is selected from the group consisting of VO, VO 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (wherein 0≦Y<1), LiMn 2-Z Co Z O4(0 <Z<2)、LiCoPO4、LiFePO4、CuO、LiCO 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 The nanoparticles may further comprise one or more coated or uncoated metal oxides, such as, but not limited to, O4, or any combination thereof.

[0053] In yet other embodiments, the coated cathode material may further comprise one or more coated or uncoated metal sulfides, such as, but not limited to, titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), nickel sulfide (Ni3S2), and lithium sulfide (Li2S), or combinations thereof.

[0054] The composite positive electrode material 220 may include the positive electrode active material in an amount of 20% to 99% by weight. In another embodiment, 30% to 95% by weight. In a further embodiment, 40% to 92.5% by weight. In yet another embodiment, 50% to 90% by weight. In another embodiment, 60% to 87.5% by weight. In a further embodiment, 65% to 85% by weight.

[0055] 2 is a schematic cross-sectional view of an example of a coated cathode material used in the construction of an electrochemical cell, according to one embodiment. The solid-state electrochemical cell 200 includes a positive electrode (current collector) 210, a positive electrode active material (cathode) 220, a separator (solid electrolyte layer) 230, a negative electrode active material (anode) 250, and a negative electrode (current collector) 260. The positive electrode active material 220 can be disposed between the positive electrode 210 and the separator 230. The negative electrode active material 250 can be disposed between the negative electrode 260 and the separator 230. The positive electrode 210 is in electrical contact with the composite positive electrode active material 220, and the negative electrode 260 is in electrical contact with the negative electrode active material 250.

[0056] The positive electrode 210 can be formed from materials including, but not limited to, aluminum (Al), nickel (Ni), titanium (Ti), stainless steel, magnesium (Mg), iron (Fe), zinc (Zn), indium (In), germanium (Ge), silver (Ag), platinum (Pt), gold (Au), lithium (Li), or alloys thereof. In some embodiments, the positive electrode layer 210 can be formed from one or more carbon-containing materials, such as carbon fiber, graphite, graphene, carbon black, conductive carbon, amorphous carbon, VGCF, and carbon nanotubes. Similarly, the negative electrode 260 can be formed from materials including, but not limited to, aluminum (Al), nickel (Ni), titanium (Ti), stainless steel, magnesium (Mg), iron (Fe), zinc (Zn), indium (In), germanium (Ge), silver (Ag), platinum (Pt), gold (Au), lithium (Li), or alloys thereof. In some embodiments, the anode layer 260 can be formed from one or more carbon-containing materials, such as carbon fiber, graphite, graphene, carbon black, conductive carbon, amorphous carbon, VGCF, and carbon nanotubes.

[0057] The composite positive electrode active material 220 can include a coated cathode material 120, such as, but not limited to, a lithium carbonate coated NMC (nickel-manganese-cobalt) material as described in this disclosure, which has a Li(Ni a Co bMn c )O₂(0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), or, for example, NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O₂), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O₂), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O₂), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O₂), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O₂) or combinations thereof.

[0058] The composite active cathode material 220 may further include one or more polymers or binders, such as, but not limited to, fluororesins containing vinylidene fluoride (VdF), hexafluoropropylene (HFP), tetrafluoroethylene (TFE), and derivatives thereof as structural units, including homopolymers such as polyvinylidene fluoride (PVdF), polyhexafluoropropylene (PHFP), polytetrafluoroethylene (PTFE), and binary copolymers such as copolymers of VdF and HFP, such as poly(vinylene difluoride-hexafluoropropylene) copolymer (PVdF-HFP). In another embodiment, the polymer or binder can be one or more of thermoplastic elastomers, such as, but not limited to, styrene-butadiene rubber (SBR), styrene-butadiene-styrene copolymer (SBS), styrene-isoprene block copolymer (SIS), styrene-ethylene-butylene-styrene (SEBS), polyacrylonitrile (PAN), nitrile-butylene rubber (NBR), polybutadiene, polyisoprene, poly(methacrylate)nitrile-butadiene rubber (PMMA-NBR), etc. In a further embodiment, the polymer or binder can be one or more of acrylic resins, such as, but not limited to, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polyisopropyl (meth)acrylate, polyisobutyl (meth)acrylate, polybutyl (meth)acrylate, etc. In yet another embodiment, the polymer or binder can be one or more of polycondensation polymers, such as, but not limited to, polyurea, polyamide paper, polyimide, polyester, etc. In yet another embodiment, the polymer or binder can be one or more of nitrile rubbers, such as, but not limited to, acrylonitrile-butadiene rubber (ABR), polystyrene nitrile-butadiene rubber (PS-NBR), and mixtures thereof. The one or more of the binders or polymers may be added in an amount of 1% to 80% by weight. In another embodiment, 3% to 70% by weight. In a further embodiment, 5% to 60% by weight. In yet another embodiment, 8% to 50% by weight.In another embodiment, it is 11% to 40% by mass. In a further embodiment, it is 14% to 30% by mass.

[0059] The composite cathode active material 220 includes one or more solid electrolyte materials, such as Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-S-SiS2-LiCl, Li2S-S-SiS2-B2S3-LiI, Li2S-S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers, and Z is Ge, Zn or Ga), Li2S-GeS2, Li 2- S-S-SiS2-Li3PO4, and Li2S-S-SiS2-Li x MO y (where x and y are positive numbers, and M is P, Si, Ge, B, Al, Ga or In) and one or more of them. In another embodiment, one or more of the solid electrolyte materials are Li3PS4, Li4P2S6, Li7P3S 11 、Li 10 GeP2S 12 、Li 10 SnP2S 12 can be. In a further embodiment, one or more of the solid electrolyte materials may be Li6PS5Cl, Li6PS5Br, Li6PS5I, or may be represented by the formula Li 7-y PS 6-y X y where "X" represents at least one halogen element and / or pseudohalogen, 0 < y ≦ 2.0, the halogen can be one or more of F, Cl, Br, I, and the pseudohalogen can be one of N, NH, NH2, NO, NO2, BF4, BH4, AlH4, CN, and SCN. In yet another embodiment, one or more of the solid electrolyte materials are of the formula Li 8-y-z P2S 9-y-z X y Wz where "X" and "W" represent at least one halogen element and / or pseudo halogen, with 0≦y≦1 and 0≦z≦1, and the halogen can be one or more of F, Cl, Br, I, and the pseudo halogen can be one of N, NH, NH2, NO, NO2, BF4, BH4, AlH4, CN, and SCN. The solid electrolyte composition can be added in an amount of 5% to 80% by weight. In another embodiment, 7.5% to 70% by weight. In a further embodiment, 10% to 60% by weight. In yet another embodiment, 12.5% ​​to 50% by weight. In another embodiment, 15% to 40% by weight. In a further embodiment, 17.5% to 30% by weight.

[0060] The composite positive electrode active material 220 has a conductivity of 1 mS / cm 2 The composite cathode active material 220 may further include one or more carbon-containing species having an electronic conductivity of 0.1 to 1.0% by weight or more. The carbon-containing species may be, but is not limited to, carbon black, graphite, graphene, carbon nanotubes, carbon fibers, VGCF, carbon black, or amorphous carbon. In another embodiment, the composite cathode active material 220 may further include one or more metal particles, filaments, or other structures. The carbon-containing species may be added in an amount of about 2% to about 50% by weight. In another embodiment, the carbon-containing species may be added in an amount of about 4% to about 40%. In a further embodiment, the carbon-containing species may be added in an amount of about 6% to about 30%. In yet another embodiment, the carbon-containing species may be added in an amount of about 8% to about 25%. In another embodiment, the carbon-containing species may be added in an amount of about 10% to about 20%. In a further embodiment, the carbon-containing species may be added in an amount of about 12% to about 18%.

[0061] The layer thickness of the composite positive electrode active material 220 can be, for example, in the range of 1 μm to 1000 μm. In another embodiment, the thickness can be in the range of 2 μm to 900 μm. In yet another embodiment, the thickness can be in the range of 5 μm to 750 μm. In a further embodiment, the thickness can be in the range of 10 μm to 500 μm. In yet another embodiment, the thickness can be in the range of 15 μm to 350 μm. In another embodiment, the thickness can be in the range of 20 μm to 200 μm. In a further embodiment, the thickness can be in the range of 25 μm to 100 μm.

[0062] The anode active material 250 may include, but is not limited to, an alkali metal, such as lithium metal, lithium alloy, sodium metal, sodium alloy, potassium metal, and potassium alloy. In other embodiments, the anode active material 250 may include one or more of an alkaline earth metal, such as magnesium metal, magnesium alloy, calcium metal, and calcium alloy. In further embodiments, the anode active material 250 may include one or more of carbon-containing species having an electronic conductivity of 1 mS / cm or more, the carbon-containing species being, but not limited to, graphitic carbon, hard carbon, amorphous carbon, carbon black, vapor grown carbon fiber (VGCF), carbon nanotubes, graphene, or combinations thereof. In yet another embodiment, the anode active material 250 may include one or more species containing silicon (Si), tin (Sn), iron (Fe), germanium (Ge), or indium (In), zinc (Zn).

[0063] The thickness of the negative electrode active material 250 can be within the range of 0.1 μm to 1000 μm, for example.

[0064] The solid electrolyte material contained within the separator 230 is preferably Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-GeS2, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-LiI-LiBr, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-S-SiS2-LiCl, Li2S-S-SiS2-B2S3-LiI, Li2S-S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (wherein m and n are positive numbers, and Z is Ge, Zn, or Ga), Li2S-GeS2, Li 2- SS-SiS2-Li3PO4 and Li2S-S-SiS2-Li x MO y In another embodiment, one or more of the solid electrolyte materials is Li3PS4, Li4P2S6, Li7P3S, Li4P2S6, Li5P3S, Li6P3S, Li7P3S, Li8P3S, Li9P3S, Li10P3S, Li11P3S, Li12P3S, Li13P3S, Li14P3S, Li15P3S, Li16P3S, Li17P3S, Li18P3S, Li19 ... 11 , Li 10 GeP2S 12 , Li 10 SnP2S 12 In further embodiments, one or more of the solid electrolyte materials can be Li6PS5Cl, Li6PS5Br, Li6PS5I, or a compound of the formula Li 7-y P.S. 6-y X y wherein "X" represents at least one halogen element and / or pseudohalogen, 0≦y≦2.0, the halogen can be one or more of F, Cl, Br, I, and the pseudohalogen can be N, NH, NH2, NO, NO 2、 BF 4、 BH 4、 AlH 4、 In yet another embodiment, one or more of the solid electrolyte materials can be one of the formula Li 8-y-z P2S 9-y-z X y W zwherein "X" and "W" represent at least one halogen element and / or pseudo halogen, with 0≦y≦1 and 0≦z≦1, and the halogen can be one or more of F, Cl, Br, I, and the pseudo halogen can be one of N, NH, NH2, NO, NO2, BF4, BH4, AlH4, CN, and SCN. The solid electrolyte composition can be added in an amount of 5% to 80% by weight. In another embodiment, 7.5% to 70% by weight. In a further embodiment, 10% to 60% by weight. In yet another embodiment, 12.5% ​​to 50% by weight. In another embodiment, 15% to 40% by weight. In a further embodiment, 17.5% to 30% by weight.

[0065] Separator 230 may additionally or alternatively include one or more binders or polymers, such as, but not limited to, fluororesins containing vinylidene fluoride (VdF), hexafluoropropylene (HFP), tetrafluoroethylene (TFE), and derivatives thereof as structural units, such as homopolymers, such as polyvinylidene fluoride (PVdF), polyhexafluoropropylene (PHFP), and polytetrafluoroethylene (PTFE), and binary copolymers of VdF and HFP, such as poly(vinylene difluoride-hexafluoropropylene) copolymer (PVdF-HFP). In another embodiment, the polymer or binder can be one or more of thermoplastic elastomers, such as, but not limited to, styrene-butadiene rubber (SBR), styrene-butadiene-styrene copolymer (SBS), styrene-isoprene block copolymer (SIS), styrene-ethylene-butylene-styrene (SEBS), polyacrylonitrile (PAN), nitrile-butylene rubber (NBR), polybutadiene, polyisoprene, poly(methacrylate)nitrile-butadiene rubber (PMMA-NBR), etc. In a further embodiment, the polymer or binder can be one or more of acrylic resins, such as, but not limited to, polymethyl (meth)acrylate, polyethyl (meth)acrylate, polyisopropyl (meth)acrylate, polyisobutyl (meth)acrylate, polybutyl (meth)acrylate, etc. In yet another embodiment, the polymer or binder can be one or more of polycondensation polymers, such as, but not limited to, polyurea, polyamide paper, polyimide, polyester, etc. In yet another embodiment, the polymer or binder can be one or more of nitrile rubbers, such as, but not limited to, acrylonitrile-butadiene rubber (ABR), polystyrene nitrile-butadiene rubber (PS-NBR), and mixtures thereof. The one or more of the binders or polymers may be added in an amount of 1% to 80% by weight. In another embodiment, 3% to 70% by weight. In a further embodiment, 5% to 60% by weight. In yet another embodiment, 8% to 50% by weight.In another embodiment, between 11% and 40% by weight. In a further embodiment, between 14% and 30% by weight. Separator 230 may additionally or alternatively include one or more of elemental sulfur, sodium sulfide, magnesium sulfide, and non-reactive oxides such as ZrO2 and Al2O3.

[0066] The thickness of the separator layer 230 is preferably in the range of 500 nm to 1000 μm. In another embodiment, the thickness can be in the range of 1 μm to 750 μm. In yet another embodiment, the thickness can be in the range of 5 μm to 500 μm. In a further embodiment, the thickness can be in the range of 6 μm to 250 μm. In yet another embodiment, the thickness can be in the range of 7 μm to 100 μm. In another embodiment, the thickness can be in the range of 8 μm to 50 μm. In a further embodiment, the thickness can be in the range of 10 μm to 30 μm.

[0067]

[0068] 3 is a flow chart of a process for growing a lithium carbonate layer on an uncoated cathode material and using the resulting coated material in an electrochemical cell. Process 300 begins with step 310, where the uncoated NMC cathode material is prepared for further processing. In one embodiment, excess lithium is not incorporated into the NMC cathode material and the material is not first coated with a lithium-containing compound. Preparation may include processes such as grinding and sieving to remove agglomerates. It is noted that special surface treatments such as washing or rinsing of the NMC cathode material may not be required.

[0069] Next, during step 320, the uncoated NMC cathode material is exposed to humidity and carbon dioxide in an atmosphere-controlled enclosure, room, or environment. The uncoated NMC cathode material is exposed at ambient temperature (room temperature, typically 20° C.) or at elevated temperatures up to 120° C. for a period of time ranging from minutes to days to allow the lithium in the uncoated NMC cathode material to diffuse near the surface of the material particles, where it reacts with water in the humid atmosphere to produce LiOH. This LiOH can further interact with water in the humid atmosphere and convert to a hydrate, such as lithium hydroxide hydrate. The LiOH and lithium hydroxide hydrate can be converted during step 330 into a grown lithium carbonate layer that coats the material particles. Ambient pressure may be used, but the pressure may be increased to accelerate the growth of the lithium carbonate coating. Under ambient conditions (STP), the cathode material may be exposed for up to 30 days to advance the growth of the lithium carbonate layer. Growing the lithium carbonate layer in this manner results in fewer coating irregularities, such as agglomerations, than occur in conventional coating processes, such as sol-gel processes.

[0070] Generally, higher concentrations of CO2, higher pressure, elevated temperature, and / or elevated humidity increase the growth rate of the lithium carbonate layer. In some embodiments, the pressure can be between 0.1 atm and 73 atm. In another embodiment, the pressure can be between 0.5 atm and 50 atm. In yet another embodiment, the pressure can be between 0.75 atm and 25 atm. In further embodiments, the pressure can be between 1 atm and 10 atm. The concentration of CO2 can be between 0.03% and 99.5% of atmospheric air. The growth conditions and growth rate of the lithium carbonate film can also result in changes in the density and porosity of the lithium carbonate layer and the performance of any cathode made from such coated materials. The humidity, relative humidity (RH), of the environment can also be controlled in the range of just above 0 percent to 100%, or just below the saturated condition of water vapor in the environment. In some embodiments, the relative humidity level can be about 0% to about 5%, about 0% to about 10%, about 0% to about 20%, about 0% to about 30%, about 0% to about 40%, about 0% to about 50%, about 0% to about 60%, about 0% to about 70%, about 0% to about 80%, about 0% to about 90%, about 0% to about 95%, about 0% to about 100%, about 5% to about 100%, about 10% to about 100%, about 20% to about 100%, about 30% to about 100%, about 40% to about 100%, about 50% to about 100%, about 60% to about 100%, about 70% to about 100%, about 80% to about 100%, about 90% to about 100%, or about 95% to about 100%. Preferably, the relative humidity level is from about 5% to about 100%, from about 10% to about 100%, from about 30% to about 100%, or from about 40% to about 100%.

[0071] The thickness of the resulting lithium carbonate layer can be in the range of 1 nanometer to about 1 micron, for example, the thickness of the resulting lithium carbonate layer can be about 1 nanometer to about 5 nanometers, about 1 nanometer to about 10 nanometers, about 1 nanometer to about 20 nanometers, about 1 nanometer to about 50 nanometers, about 1 nanometer to about 100 nanometers, about 1 nanometer to about 250 nanometers, about 1 nanometer to about 500 nanometers, about 1 nanometer to about 750 nanometers, about 1 nanometer to about 1 micron, about 5 nanometers to about 1 micron, about 10 nanometers to about 1 micron, about 20 nanometers to about 1 micron, about 50 nanometers to about 1 micron, about 100 nanometers to about 1 micron, about 250 nanometers to about 1 micron, about 500 nanometers to about 1 micron, or about 750 nanometers to about 1 micron. In some embodiments, the thickness can be about 5 nanometers to about 750 nanometers. In another embodiment, the thickness can be from about 10 nanometers to about 500 nanometers. In yet another embodiment, the thickness can be from about 15 nanometers to about 250 nanometers. In yet another embodiment, the thickness can be from about 17 nanometers to about 100 nanometers. In another embodiment, the thickness can be from about 20 nanometers to about 50 nanometers.

[0072] As the thickness of the lithium carbonate layer increases, the total lithium contained in the cathode material decreases. The formation of lithium carbonate may reduce the lithium contained in the cathode material by 0.1% to 3%. In some embodiments, the formation of lithium carbonate may reduce the lithium contained in the cathode material by 0.2% to 2.5%. In another embodiment, the formation of lithium carbonate may reduce the lithium contained in the cathode material by 0.25% to 1.5%. In a further embodiment, the formation of lithium carbonate may reduce the lithium contained in the cathode material by 0.3% to 0.5%. Furthermore, as the lithium carbonate layer grows, the porosity of the layer may range on the order of 1% to 50%. In some embodiments, the porosity may range from 3% to 40%. In another embodiment, the porosity may range from 5% to 30%. The nickel-based NMC cathode material may also include a lithium-containing and lithium-ion-bearing coating layer after the growth of the lithium carbonate layer. The lithium-containing layer may include Li2ZrO3, Li2ZrO4, LiCl, LiF, LiOH, Li2O, lithium niobate, lithium nitride, lithium titanate, and lithium silicate.

[0073] Following exposure and growth of the lithium carbonate layer, the nickel-based cathode material may be vacuum dried at ambient or elevated temperatures (up to 500° C.) during step 340 to remove residual moisture. When the lithium carbonate growth step is performed at elevated temperatures, vacuum drying may not be required. An optional washing process may also be included before or after vacuum drying. The coated NMC cathode material may then be combined with a suitable binder, solid electrolyte, and conductive additives to form a cathode for an electrochemical cell in step 350. The cathode can then be integrated with an anode and separator to form a functioning electrochemical cell in step 360.

[0074] In some exemplary embodiments, a catalytic amount of nickel may be used in the NMC cathode material. As used in this disclosure, a "catalytic amount of nickel" refers to an amount of nickel that increases the rate of lithium carbonate formation without itself undergoing permanent chemical change.

[0075] Further provided in the present disclosure is a method for producing a cathode uniformly coated with lithium carbonate in a gaseous manner. As used in the present disclosure, gaseous production of lithium carbonate coating refers to a method for producing lithium carbonate via a chemical reaction in which at least one reactant is in the gas phase. The method generally includes contacting gaseous carbon dioxide and water vapor with a nickel-based cathode material containing lithium and oxygen, and producing a cathode uniformly coated with lithium carbonate in a gaseous manner. The lithium carbonate can be uniformly formed as a layer on the outer surface of the cathode material to form a cathode coated with lithium carbonate.

[0076] The lithium carbonate layer having a uniform composition can have a thickness of about 1 nanometer to about 1 micron, for example, the thickness of the lithium carbonate layer can be about 1 nanometer to about 5 nanometers, about 1 nanometer to about 10 nanometers, about 1 nanometer to about 20 nanometers, about 1 nanometer to about 50 nanometers, about 1 nanometer to about 100 nanometers, about 1 nanometer to about 250 nanometers, about 1 nanometer to about 500 nanometers, about 1 nanometer to about 750 nanometers, about 1 nanometer to about 1 micron, about 5 nanometers to about 1 micron, about 10 nanometers to about 1 micron, about 20 nanometers to about 1 micron, about 50 nanometers to about 1 micron, about 100 nanometers to about 1 micron, about 250 nanometers to about 1 micron, about 500 nanometers to about 1 micron, or about 750 nanometers to about 1 micron. In some embodiments, the thickness can be about 5 nanometers to about 750 nanometers. In another embodiment, the thickness can be from about 10 nanometers to about 500 nanometers. In yet another embodiment, the thickness can be from about 15 nanometers to about 250 nanometers. In yet another embodiment, the thickness can be from about 17 nanometers to about 100 nanometers. In another embodiment, the thickness can be from about 20 nanometers to about 50 nanometers. In another embodiment, the thickness can be from about 10 nanometers to about 40 nanometers.

[0077] The method may further include contacting the nickel-based cathode material with carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, and / or at a predetermined relative humidity level.

[0078] The method can further include contacting the nickel-based cathode material with carbon dioxide for a predetermined period of time. The predetermined period of time can range from a few minutes to a few days. For example, the predetermined period of time can be about 5 minutes, about 15 minutes, about 30 minutes, about 1 hour, about 2 hours, about 4 hours, about 8 hours, about 16 hours, about 24 hours, about 48 hours, about 3 days, about 5 days, about 7 days, about 10 days, about 14 days, about 20 days, about 30 days, or more. In some embodiments, the predetermined time period can be from about 5 minutes to about 1 hour, from about 5 minutes to about 8 hours, from about 5 minutes to about 24 hours, from about 5 minutes to about 48 hours, from about 5 minutes to about 5 days, from about 5 minutes to about 7 days, from about 5 minutes to about 14 days, from about 5 minutes to about 20 days, from about 5 minutes to about 30 days, from about 1 hour to about 30 days, from about 8 hours to about 30 days, from about 24 hours to about 30 days, from about 48 hours to about 30 days, from about 5 days to about 30 days, from about 7 days to about 30 days, from about 14 days to about 30 days, from about 20 days to about 30 days, from about 8 hours to about 24 hours, from about 24 hours to about 10 days, or from about 5 days to about 20 days.

[0079] The method can further include contacting the nickel-based cathode material with carbon dioxide at a predetermined temperature. In some embodiments, the predetermined pressure can be about 20°C to about 120°C. For example, the predetermined temperature can be about 20°C to about 40°C, about 20°C to about 60°C, about 20°C to about 80°C, about 20°C to about 100°C, about 20°C to about 120°C, about 40°C to about 120°C, about 60°C to about 120°C, about 80°C to about 120°C, or about 100°C to about 120°C.

[0080] The method may further include contacting the nickel-based cathode material with carbon dioxide at a predetermined pressure. In some embodiments, the predetermined pressure can be from about 0.1 atm to about 73 atm. For example, the pressure can be from about 0.1 atm to about 1 atm, from about 0.1 atm to about 5 atm, from about 0.1 atm to about 10 atm, from about 0.1 atm to about 25 atm, from about 0.1 atm to about 50 atm, from about 0.1 atm to about 73 atm, from about 1 atm to about 73 atm, from about 5 atm to about 73 atm, from about 10 atm to about 73 atm, from about 25 atm to about 73 atm, or from about 50 atm to about 73 atm. In another embodiment, the pressure can be from 0.5 atm to 50 atm. In yet another embodiment, the pressure can be from 0.75 atm to 25 atm. In a further embodiment, the pressure can be from 1 atm to 10 atm.

[0081] The method can further include contacting the nickel-based cathode material with carbon dioxide at a predetermined relative humidity level, which can be between about 0% and about 100%, or just below the saturated condition of water vapor in the environment. For example, the predetermined relative humidity level can be about 0% to about 5%, about 0% to about 10%, about 0% to about 20%, about 0% to about 30%, about 0% to about 40%, about 0% to about 50%, about 0% to about 60%, about 0% to about 70%, about 0% to about 80%, about 0% to about 90%, about 0% to about 95%, about 0% to about 100%, about 5% to about 100%, about 10% to about 100%, about 20% to about 100%, about 30% to about 100%, about 40% to about 100%, about 50% to about 100%, about 60% to about 100%, about 70% to about 100%, about 80% to about 100%, about 90% to about 100%, or about 95% to about 100%.

[0082] The cathode material may include lithium and oxygen in a molar ratio of 1:2. The cathode material may include a catalytic amount of nickel.

[0083] Further provided in the present disclosure is a solid-state battery cell comprising the coated cathode material described in the present disclosure. The solid-state battery cell may comprise any of the compositions made by the methods described in the present disclosure. The battery cell may comprise a cathode material comprising a nickel-manganese-cobalt (NMC) material. The NMC material may have an average particle size of from about 1 micron to about 20 microns. The NMC material may be represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1). In an exemplary embodiment, the NMC material is NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O2), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O2), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O2), NMC 851005 (LiNi 0.85 Mn 0.05 Co 0.1 O2), or any combination thereof.

[0084] In another embodiment, the cathode material may comprise a metal oxide. The metal oxide is LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≤ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≤ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4, Li(Ni a Co b Alc )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), or any combination thereof may be included. In another embodiment, the metal oxide is V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≤ Y < 1), LiMn 2-Z Co Z O4 (0 ≤ Z ≤ 2), LiCoPO4, LiFePO4, CuO, LiCO 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 O4, or any combination thereof may be included.

[0085] The solid-state battery cell can maintain 85% or more, 90% or more, 95% or more, 98% or more, or 99% or more of its discharge capacity after 3 cycles.

[0086] The solid-state battery cell can have a higher initial discharge capacity than a solid-state battery cell containing the same cathode material but without the coating. The solid-state battery cell can maintain about 85% or more of its original discharge capacity after the battery cell has been cycled 3 times. For example, the battery cell can maintain about 90% or more, about 95% or more, about 98% or more, or about 99% or more of its original discharge capacity after 3 cycles.

[0087] Figure 4A is a graph of the number of cycles vs. discharge capacity of a solid lithium metal full cell using uncoated NMC 622 according to Comparative Example 1 and the same NMC 622 material with a Li2CO3-rich surface according to Example 1. Both cells are cycled at 0.1C charge and 0.1C discharge between 4.3V and 2.5V. Figure 4B is a graph of the number of cycles vs. discharge capacity of a solid lithium metal full cell using uncoated NMC 851005 according to Comparative Example 2 and the same NMC 851005 material with a Li2CO3-rich surface according to Example 2. Both cells are cycled at 0.1C charge and 0.1C discharge between 4.3V and 2.5V.

[0088] 5 is a plot of ATR-FTIR spectroscopy of NMC 622 material. The plot "Comparative Example 1" is of uncoated NMC 622 material, and the plot "Example 1" is of the same NMC 622 material after being coated with Li2CO3 as described in Example 1. The ATR-FTIR spectroscopy of Example 1 shows Li2CO3 at ν=1475 cm -1 and 1417 cm -1 Strong CO stretching band at ν=865cm -1 shows moderately strong carbonate bending modes, whereas plot "Comparative Example 1" lacks such features.

[0089] 6 is a plot of ATR-FTIR spectroscopy of NMC 851005 material. Plot "Comparative Example 2" is for uncoated NMC 851005 material, and plot "Example 2" is for the same NMC 851005 material after being coated with Li2CO3 according to Example 2. Plot "Example 2" shows a peak at ν=1475 cm -1 and 1417 cm -1 Strong CO stretching band at ν=865cm, indicating Li2CO3 -1 shows moderately strong carbonate bending modes at , whereas plot “a” lacks such features.

[0090] FIG. 7 is a plot of ATR-FTIR spectroscopy of uncoated NMC-622 particles (Counterexample 3), NMC-622 particles exposed to 0.2% relative humidity (RH) at 21° C. for 13 days (Example 3), NMC-622 particles exposed to 20% RH at 21° C. for 13 days (Example 4), and NMC-622 particles exposed to 73% RH at 21° C. for 13 days (Example 5) to form a Li2CO3 coating via atmospheric growth.

[0091] FIG. 8 is a plot of ATR-FTIR spectroscopy of initial uncoated NMC-622 particles (Example 6-A), NMC-622 particles exposed to 73.2% relative humidity (RH) at 21° C. for 4 days (Example 6-B), initial uncoated LMO particles (Comparative Example 4-A), LMO particles exposed to 73.2% relative humidity (RH) at 21° C. for 4 days (Comparative Example 4-B), initial uncoated LCO particles (Comparative Example 5-A), and LCO particles exposed to 73.2% relative humidity (RH) at 21° C. for 4 days (Comparative Example 5-B).

[0092] FIG. 9 is a plot of ATR-FTIR spectroscopy of pristine uncoated NMC-622 particles (Example 6-A), NMC-622 particles exposed to 73.2% relative humidity (RH) at 21° C. for 24 hours (Example 6-C), pristine uncoated NMC 851005 particles (Example 7-A), and NMC 851005 particles exposed to 73.2% relative humidity (RH) at 21° C. for 24 hours (Example 7-B).

[0093] It should be understood that cathode materials produced via embodiments of the present disclosure may have application in electrochemical cells, such as those having one or more of a solid electrolyte, a polymer electrolyte, a liquid electrolyte, or a solvent-in-salt electrolyte.

[0094] The above features and the features claimed below can be combined in various ways without departing from the scope of the present disclosure. Therefore, it should be noted that the matters included in the above description or shown in the accompanying drawings should be construed as illustrative and not in a limiting sense. The above-described embodiments are not to be construed as limiting the scope of the present disclosure, but rather as examples of the present disclosure. In addition to the foregoing embodiments of the disclosure, consideration of the detailed description and the accompanying drawings will show that there are other embodiments of such disclosure. Accordingly, many combinations, substitutions, variations, and modifications of the foregoing embodiments of the disclosure that are not explicitly described in the present disclosure still fall within the scope of such disclosure. The following claims are intended to encompass all descriptions of the general and specific features described in the present disclosure, as well as the scope of the method and system that may be said to fall between them as a matter of language.

[0095] Exemplary embodiments Embodiment 1: A method for producing a cathode coated with lithium carbonate for an electrochemical cell in a gas mode, the method comprising exposing a nickel-based cathode material containing lithium and oxygen in a molar ratio of 1:2 to gaseous carbon dioxide and water vapor, and incubating the nickel-based cathode material and carbon dioxide for a predetermined time at a predetermined temperature, at a predetermined pressure, and / or at a predetermined relative humidity level, wherein lithium carbonate is formed as a uniform layer on the outer surface of the cathode material to form a cathode coated with lithium carbonate.

[0096] Embodiment 2: The method according to Embodiment 1, wherein the nickel-based cathode material contains the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1).

[0097] Embodiment 3: The nickel-based cathode material is NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33O2), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O2), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O2), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O2), or a combination thereof, the method according to Embodiment 1.

[0098] Embodiment 4: The nickel-based cathode material is LiNiO2, LiNi 1-Y Co Y O2, LiNi 1-Y Mn Y O2 (0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4, Li(Ni a Co b Al c )O2 (0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), or one or more of combinations thereof, the method according to Embodiment 1.

[0099] Embodiment 5: The nickel-based cathode material is V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≦ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≦ Z ≦ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 O4, or further includes one or more of coated or uncoated metal oxides in combination thereof, the method according to Embodiment 1.

[0100] Embodiment 6: The method of embodiment 1, wherein the nickel-based cathode material further comprises one or more of coated or uncoated metal sulfides including titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS or FeS2), copper sulfide (CuS), nickel sulfide (Ni3S2), lithium sulfide (Li2S), or combinations thereof.

[0101] Embodiment 7: The method of embodiment 1, wherein the exposing comprises applying high pressure to increase the growth rate of the lithium carbonate coating.

[0102] Embodiment 8: The method of embodiment 1, wherein the exposing comprises applying an elevated temperature to increase the growth rate of the lithium carbonate coating.

[0103] Embodiment 9: The method of embodiment 1, wherein the predetermined temperature is within the range of about 20°C to about 120°C.

[0104] Embodiment 10: The method of embodiment 1, wherein the exposing step comprises applying a high concentration of gaseous carbon dioxide for a predetermined time to increase the growth rate of the lithium carbonate coating.

[0105] Embodiment 11: The method of embodiment 1, wherein the exposing step comprises applying a high concentration of water vapor for a period of time to increase the growth rate of the lithium carbonate coating.

[0106] Embodiment 12: The method of any one of embodiments 1 to 11, wherein the nickel-based cathode material is coated with a lithium-containing layer upon exposure to gaseous carbon dioxide and water vapor.

[0107] Embodiment 13: The method of embodiment 12, wherein the lithium-containing layer comprises LiZrO, LiZrO, LiCl, LiF, LiOH, LiO, lithium niobate, lithium nitride, lithium titanate, lithium silicate, or a combination thereof.

[0108] Embodiment 14: The method of any one of embodiments 1-13, wherein the nickel-based cathode material is not treated prior to exposure to gaseous carbon dioxide and water vapor.

[0109] Embodiment 15: The method of any one of embodiments 1 to 14, wherein the lithium carbonate coating has a thickness in the range of about 5 nanometers to about 1 micrometer.

[0110] Embodiment 16: The method of any one of embodiments 1 to 15, further comprising vacuum drying the lithium carbonate coated cathode to remove residual moisture.

[0111] Embodiment 17: The method of any one of embodiments 1 to 16, further comprising washing the coated cathode with lithium carbonate.

[0112] Embodiment 18: The method of any one of embodiments 1 to 17, further comprising combining the lithium carbonate coated cathode with one or more of a suitable binder, a solid electrolyte, and a conductive additive to form a cathode for an electrochemical cell.

[0113] Embodiment 19: The method of any one of embodiments 1 to 18, further comprising combining the lithium carbonate coated cathode with an anode and a separator to form a functioning electrochemical cell.

[0114] Embodiment 20: An electrochemical cell comprising a cathode coated with lithium carbonate having an outer lithium carbonate coating having a thickness in the range of about 2 nanometers to about 1 micron.

[0115] Embodiment 21: A method for producing a cathode uniformly coated with lithium carbonate in a gas mode, the method comprising contacting gaseous carbon dioxide and water vapor with a nickel-based cathode material comprising lithium and oxygen, and producing a cathode uniformly coated with lithium carbonate in a gas mode, wherein the lithium carbonate is uniformly formed as a layer on an outer surface of the cathode material to form a cathode coated with lithium carbonate.

[0116] Embodiment 22: The method of embodiment 21, comprising contacting the nickel-based cathode material with carbon dioxide at a predetermined relative humidity level.

[0117] Embodiment 23: The method of embodiment 21, comprising contacting the nickel-based cathode material with carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, or at a predetermined relative humidity level.

[0118] Embodiment 24: The method of embodiment 21, wherein the cathode material comprises lithium and oxygen in a molar ratio of 1:2.

[0119] Embodiment 25: The method of embodiment 21, wherein the nickel-based cathode material comprises a catalytic amount of nickel.

[0120] Embodiment 26: The method of embodiment 21, wherein the uniform lithium carbonate coating has a thickness in the range of about 5 nanometers to 1 micrometer.

[0121] Embodiment 27: The method of embodiment 21, wherein the uniform lithium carbonate coating has a thickness in the range of about 1 nanometer to about 100 nanometers.

[0122] Embodiment 28: The method of embodiment 21, wherein the uniform lithium carbonate coating is in the range of about 1 nanometer to about 50 nanometers.

[0123] Embodiment 29: The method according to Embodiment 21, wherein the uniform lithium carbonate coating is within the range of about 10 nanometers to about 40 nanometers.

[0124] Embodiment 30: A solid-state battery cell comprising a nickel-based cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), wherein the nickel-based cathode material is a cathode uniformly coated with lithium carbonate, and the solid-state battery cell maintains 85% or more, 90% or more, 95% or more, 98% or more, or 99% or more of its discharge capacity after 3 cycles.

[0125] Embodiment 31: A solid-state battery cell comprising a nickel-based cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1), wherein the nickel-based cathode material is uniformly coated with lithium carbonate, and the solid-state battery cell has a higher initial discharge capacity compared to the same nickel-based cathode material without the lithium carbonate coating.

[0126] Embodiment 32: A cathode composition comprising a nickel-based cathode material represented by the formula LiNi a Mn b Co c O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, and a + b + c = 1) and a lithium carbonate layer, wherein the cathode material is uniformly coated with the lithium carbonate layer.

[0127] Embodiment 33: The composition according to Embodiment 32, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

[0128] Embodiment 34: The cathode material is LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi0.4 Mn 0.3 Co 0.3 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiNi 0.85 Mn 0.05 Co 0.1 02, and any combination thereof.

[0129] Embodiment 35: The cathode material is LiNi 0.33 Mn 0.33 Co 0.33 The composition of embodiment 32, comprising O2.

[0130] Embodiment 36: The cathode material is LiNi 0.4 Mn 0.3 Co 0.3 The composition of embodiment 32, comprising O2.

[0131] Embodiment 37: The cathode material is LiNi 0.5 Mn 0.3 Co 0.2 The composition of embodiment 32, comprising O2.

[0132] Embodiment 38: The cathode material is LiNi 0.6 Mn 0.2 Co 0.2 The composition of embodiment 32, comprising O2.

[0133] Embodiment 39: The cathode material is LiNi 0.8 Mn 0.1 Co 0.1 The composition of embodiment 32, comprising O2.

[0134] Embodiment 40: The cathode material is LiNi 0.85 Mn 0.05 Co 0.1The composition according to Embodiment 32, containing O2.

[0135] Embodiment 41: The composition according to Embodiment 32, wherein the lithium carbonate layer is formed in a gas mode.

[0136] Embodiment 42: The composition according to Embodiment 32, wherein the cathode material further contains a metal oxide.

[0137] Embodiment 43: The metal oxide is LiNiO2, LiNi 1-Y Co Y O2 (where 0 ≦ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≦ Z ≦ 2), Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), and the composition according to Embodiment 42, selected from the group consisting of any combination thereof.

[0138] Embodiment 44: The metal oxide is V2O5, V6O 13 , MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≦ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≦ Z ≦ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, LiMn 1.5 Ni 0.5 O4, and the composition according to Embodiment 42, selected from the group consisting of any combination thereof.

[0139] Embodiment 45: A cathode composition, LiNiO2, LiNi1-Y Co Y O2 (where 0 ≦ Y < 1), LiNi 1-Y Mn Y O2 (where 0 ≦ Y < 1), Li(Ni a Co b Mn c )O4 (where 0 < a < 2, 0 < b < 2, 0 < c < 2, a + b + c = 2), LiMn 2-Z Ni Z O4 (where 0 ≦ Z ≦ 2), or Li(Ni a Co b Al c )O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1), and a single lithium carbonate layer, wherein the cathode material is uniformly coated with a lithium carbonate layer, a cathode composition.

[0140] Embodiment 46: The composition according to Embodiment 45, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

[0141] Embodiment 47: A cathode composition comprising V2O5, V6O 13、 MoO3, LiCoO2, LiMnO2, LiMn2O4, LiCo 1-Y Mn Y O2 (where 0 ≦ Y < 1), LiMn 2-Z Co Z O4 (where 0 ≦ Z ≦ 2), LiCoPO4, LiFePO4, CuO, LiCo 0.6 Mn 0.4 O2, or LiMn 1.5 Ni 0.5 O4, and a lithium carbonate layer, wherein the cathode material is uniformly coated with a lithium carbonate layer, a cathode composition.

[0142] Embodiment 48: The composition according to Embodiment 47, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

Examples

[0143] Example 1

[0144] Formation of a coating on the cathode active material

[0145] 20 g of dry, uncoated NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 The O2) particles were exposed to air at 25 °C for 20 days, and the samples were stirred every 48 hours. Once a 20 nm Li2CO3 layer was formed on the NMC 622 particles, the material was dried in vacuum at 120 °C for 10 hours. The presence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurements in Figure 5.

[0146] Synthesis of solid electrolyte materials

[0147] The sulfide solid electrolyte (Li2S-P2S5-based glass ceramic containing LiCl) and xylene were placed in a 250 ml zirconia grinding jar with zirconia media. The loaded mill jar was then placed in a Retsch PM 100 planetary mill and milled at 400 RPM for 18 hours. The material was collected, dried at 70°C, and then heated to 200°C in an inert (argon or nitrogen) environment.

[0148] Solid-state lithium metal cell fabrication

[0149] First, the above-mentioned coated active material and the above-mentioned solid electrolyte material were mixed to produce a cathode mix. Then, a press was used to manufacture a lithium solid state battery 200 as shown in FIG. 2 above. The above-mentioned cathode mix was used as the cathode active material layer 220, a 600 micron-thick chip-shaped lithium metal anode was used as the anode active material 250 and the anode 260, and the above-mentioned solid electrolyte was used as the separator 230, respectively. The lithium solid state battery was manufactured by using the layout shown in FIG. 2.

[0150] Example 2

[0151] Formation of a coating on the cathode active material

[0152] 20 g of dry, uncoated NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 The O2) particles were exposed to air at 20 °C for 9 days, and the samples were constantly stirred using a shaking table. Once a 20 nm Li2CO3 layer was formed on the NCM 851005 particles, the material was dried in vacuum at 120 °C for 10 hours. The presence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurements in Figure 6.

[0153] Solid-state lithium metal cell fabrication

[0154] Coated NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 A solid-state lithium cell of Example 2 was prepared in the same manner as in Example 1, except that O2) particles were used as the cathode active material.

[0155] Comparative Example 1

[0156] Uncoated NMC 622(LiNi 0.6 Mn 0.2 Co 0.2 A solid-state lithium cell of Comparative Example 1 was fabricated in the same manner as in Example 1, except that Li2CO3 was used as the cathode active material. The absence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurement in FIG.

[0157] Comparative Example 2

[0158] Uncoated NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 A solid-state lithium cell of Comparative Example 2 was fabricated in the same manner as in Example 2, except that Li2CO3 particles were used as the cathode active material. The absence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurement in FIG.

[0159] Determining the humidity range required to form a Li2CO3 coating

[0160] Example 3

[0161] 20 g of dry, uncoated NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 The O2) particles were exposed to a temperature of 21 °C and a relative humidity (RH) of 0.2% for 13 days, with the samples being stirred every 48 hours. After 13 days, the NMC 622 material was vacuum dried at 120 °C for 10 hours, and the presence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurements in Figure 7.

[0162] Example 4

[0163] Example 4 was carried out in the same manner as Example 3, except that the relative humidity was 20%. The presence of Li2CO3 is shown in the ATR-FTIR spectroscopy in FIG.

[0164] Example 5

[0165] Example 5 was carried out in the same manner as Example 3, except that the relative humidity was 73.2%. The presence of Li2CO3 is shown in the ATR-FTIR spectroscopy in FIG.

[0166] Comparative Example 3

[0167] 20 g of dry, uncoated NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 The O2) particles were placed in an inert gas environment with 0% relative humidity at a temperature of 21 °C for 13 days, with the sample being stirred every 48 hours. After 13 days, the NMC 622 material was vacuum dried at 120 °C for 10 hours and ATR-FTIR spectroscopy measurements were taken and are shown in Figure 7.

[0168] Solid-state cell evaluation

[0169] The solid-state battery cells of Examples 1 and 2 and Comparative Examples 1 and 2 were each charged to 4.3 V at a constant current-constant voltage at a C rate of 0.1 C (1 / 10 C) at a temperature of 70° C., and then discharged to 2.5 V at a constant current-constant voltage at a C rate of 0.1 C (1 / 10 C). The discharge capacity at this time was measured. This cycle was repeated until the trend of discharge capacity decay was determined. As shown in FIG. 4A, the solid-state battery cell of Example 1 using NMC 622 coated with Li2CO3 had a higher initial discharge capacity than that of Comparative Example 1 using uncoated NMC 622 material, 123 mAh / g for Example 1 and 116 mAh / g for Comparative Example 1. Furthermore, the solid-state battery cell of Example 1 using NMC 622 coated with Li2CO3 showed a dramatically slower decline in discharge capacity compared to Comparative Example 1. The solid-state battery cell of Example 1 was cycled 85 times before its discharge capacity decreased by 85% of the starting capacity, reaching 105 mAh / g at about the 85th cycle. The solid-state battery cell of Comparative Example 1 was cycled about 22 times before its discharge capacity decreased by 85% of the starting capacity, reaching 99 mAh / g at about the 22nd cycle.

[0170] Similar results can be seen in FIG. 4B, where the solid-state battery cell of Example 2 using NCM 851005 coated with Li2CO3 had a higher initial discharge capacity than that of Comparative Example 2 using uncoated NMC 851005 material, 137 mAh / g for Example 2 vs. 120 mAh / g for Comparative Example 2. Furthermore, the solid-state battery cell of Example 2 using NMC 851005 coated with Li2CO3 showed a dramatically slower decline in discharge capacity compared to Comparative Example 2. The solid-state battery cell of Comparative Example 2 cycled only three times before its discharge capacity decreased by more than 85% of its initial capacity, reaching about 97 mAh / g by the third cycle. The solid-state battery cell of Example 2 still maintained more than 98% of its discharge capacity by the third cycle, decreasing only to about 137 mAh / g. The examples described in this disclosure show that the lithium contained in the cathode active material can be used to form a layer Li2CO3 on the surface of the cathode active material, thereby improving the initial discharge capacity and cycle life.

[0171] Evaluate the required humidity level

[0172] By examining the ATR-FTIR spectroscopy measurements in FIG. 7 for Comparative Example 3, it can be seen that at a relative humidity level of 0% and a carbon dioxide-free atmosphere, the NMC material was unable to form a Li2CO3 coating. This is due to the fact that the Li2CO3 coating was not formed at ν=1475 cm -1 and 1417 cm -1 The absence of a CO stretching band at ν = 865 cm -1 This is evident from the carbonate bending mode at ν=865 cm. -1 The carbonate bending mode at ν=1475cm -1 and 1417 cm -1The CO stretching band at ν = 1475 cm is hidden in the background. This is evidence of a very thin layer of Li2CO3, which may require more than 13 days of exposure at 0.2% relative humidity to form Li2CO3 of the desired thickness. ATR-FTIR spectroscopy in Figure 7 of Examples 4 and 5 shows that the CO stretching band at ν = 1475 cm -1 and 1417 cm -1 CO stretching band at ν=865cm -1 Both the carbonate bending modes at

[0173] Determination of cathode components required to form Li2CO3 coating

[0174] Example 6-A

[0175] Pristine, uncoated NMC 622(LiNi 0.6 Mn 0.2 Co 0.2 ATR-FTIR spectroscopy was performed on the O2 particles, and the results are shown in Figures 8 and 9.

[0176] Example 6-B

[0177] 20 g of dry, uncoated NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 The NMC 622 particles were exposed to 73.2% relative humidity (RH) for four days at a temperature of 21 °C. After four days, the NMC 622 material was vacuum dried at 120 °C for 10 hours, and the presence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurements in Figure 8.

[0178] Example 6-C

[0179] 20 g of dry, uncoated NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2The NMC 622 particles were exposed to 73.2% relative humidity (RH) for 24 hours at a temperature of 21 °C. After 24 hours, the NMC 622 material was vacuum dried at 120 °C for 10 hours, and the presence of Li2CO3 is shown in the ATR-FTIR spectroscopy measurements in Figure 9.

[0180] Example 7-A

[0181] Pristine, uncoated NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 ATR-FTIR spectroscopy was performed on the O2 particles, and the results are shown in Figure 9.

[0182] Example 7-B

[0183] Example 7-B is a dried, uncoated NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 The same method as in Example 6-C was carried out, except that Li2CO3 was used, and the presence of Li2CO3 is shown in the ATR-FTIR spectroscopy in FIG. 9.

[0184] Comparative example 4-A

[0185] Comparative Example 4-A was carried out in the same manner as Example 4-A, except that a LMO (lithium manganese oxide) cathode material was used instead of the NMC material.

[0186] Comparative example 4-B

[0187] Comparative Example 4-B was carried out in the same manner as Example 6-B, except that a LMO (lithium manganese oxide) cathode material was used instead of the NMC cathode material.

[0188] Comparative example 5-A

[0189] Comparative Example 5-A was carried out in the same manner as Example 6-A, except that LCO (lithium-cobalt-oxide) cathode material was used instead of the NMC material.

[0190] Comparative example 5-B

[0191] Comparative Example 5-B was carried out in the same manner as Example 6-B, except that LCO (lithium-cobalt-oxide) cathode material was used instead of the NMC material.

[0192] Evaluation of the cathode components required to form the Li2CO3 coating

[0193] By comparing the ATR-FTIR spectroscopy of counter example 4-A with counter example 4-B in FIG. 8, it can be seen that no appreciable amount of Li2CO3 was formed by exposing a cathode material containing manganese as its only transition metal (LMO) to 73.2% relative humidity (RH) at a temperature of 21° C. for 4 days. A similar result can be seen by comparing the ATR-FTIR spectroscopy of counter example 5-A with that of counter example 5-B in FIG. 8. In this comparison, a cathode material containing cobalt as its only transition metal (LCO) was exposed to 73.2% relative humidity (RH) at a temperature of 21° C. for 4 days. Again, no appreciable amount of Li2CO3 was formed. Only when nickel (e.g., catalytic amount of nickel) was incorporated into the cathode material was the formation of Li2CO3 confirmed. This is shown by comparing the ATR-FTIR spectroscopy of example 6-A with that of example 6-B in FIG. 8. In this comparison, a cathode material containing nickel as its transition metal (NMC) was exposed to 73.2% relative humidity (RH) at a temperature of 21° C. for 4 days. After this exposure, ATR-FTIR spectroscopy of Example 6-B showed a ν=1475 cm -1 and 1417 cm -1 CO stretching band at ν=865cm -18, indicating the presence of Li2CO3. Furthermore, ATR-FTIR spectroscopy of Example 6-C shows that the same NMC material formed a layer of Li2CO3 after only 24 hours of exposure to relative humidity (RH) at 21 °C.

[0194] FIG. 9 further illustrates the advantage of having nickel (e.g., catalytic amounts of nickel) as a component of the cathode material. FIG. 9 shows that when two cathode materials containing different amounts of nickel were exposed to the same temperature (21° C.), same level of RH (73.2%) and CO2 (atmospheric pressure) for the same time (24 hours), the cathode material containing the greater amount of nickel formed a more substantial layer of Li2CO3 on the surface of the particles. ATR-FTIR spectroscopy of Example 6-A and ATR-FTIR spectroscopy of Example 6-C show that the NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 ATR-FTIR spectroscopy of Example 7-A and ATR-FTIR spectroscopy of Example 7-B show the thermal conductivity of NCM 851005 (LiNi O2) cathode material before and after the exposures described. 0.85 Mn 0.05 Co 0.1 9 shows the ATR-FTIR spectroscopy of Example 6-C compared to that of Example 7-B. The ATR-FTIR spectroscopy of Example 7-B shows that NCM 851005 (LiNi 0.85 Mn 0.05 Co 0.1 ATR-FTIR spectroscopy of Example 6-C indicates a more abundant Li2CO3 layer on the O2 surface. -1 and ν=865cm -1 This comparison further demonstrates the role of nickel in the formation of Li2CO3 on the surface of the cathode material, such that by increasing the nickel content in the cathode material, the rate at which Li2CO3 forms also increases.

[0195] The examples and comparative examples can show that, according to embodiments, a Li2CO3 layer can be formed by exposing a lithium-containing cathode active material to a relative humidity range of greater than 0% to 100% and atmospheric CO2 for a certain time frame.

Claims

1. 1. A method for producing a lithium carbonate coated cathode for an electrochemical cell, comprising the steps of: exposing a nickel-based cathode material containing lithium and oxygen in a 1:2 molar ratio to gaseous carbon dioxide and water vapor; incubating the nickel-based cathode material and the carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, and / or at a predetermined relative humidity level; wherein lithium carbonate is formed as a layer on an outer surface of the cathode material to form a lithium carbonate coated cathode.

2. The nickel-based cathode material has the formula LiNi a Mn b Co c O 2 2. The method of claim 1 , comprising: wherein 0<a<1, 0<b<1, 0<c<1, and a+b+c=1.

3. The nickel-based cathode material is NMC 111 (LiNi 0.33 Mn 0.33 Co 0.33 O 2 ), NMC 433 (LiNi 0.4 Mn 0.3 Co 0.3 O 2 ), NMC 532 (LiNi 0.5 Mn 0.3 Co 0.2 O 2 ), NMC 622 (LiNi 0.6 Mn 0.2 Co 0.2 O 2 ), NMC 811 (LiNi 0.8 Mn 0.1 Co 0.1 O 2 ), or a combination thereof.

4. The nickel-based cathode material is LiNiO 2 , LiNi 1-Y Co Y O 2 , LiNi 1-Y Mn Y O 2 (0≦Y<1), Li(Ni a Co b Mn c ) O 4 (0<a<2, 0<b<2, 0<c<2, a+b+c=2), LiMn 2-Z Ni Z O 4 , Li(Ni a Co b A c ) O 2 13. The method of claim 1, comprising one or more of a coated or uncoated metal oxide comprising: (0<a<1, 0<b<1, 0<c<1, a+b+c=1), or combinations thereof.

5. The nickel-based cathode material is V 2 O 5 , V 6 O 13 , MoO 3 , LiCoO 2 , LiMnO 2 , LiMn 2 O 4 , LiCo 1-Y Mn Y O 2 (Wherein, 0≦Y<1), LiMn 2-Z Co Z O 4 (Wherein, 0≦Z≦2), LiCoPO 4 , LiFePO 4 , CuO, LiCo 0.6 Mn 0.4 O 2 , LiMn 1.5 Ni 0.5 O 4 10. The method of claim 1, further comprising one or more of the following coated or uncoated metal oxides:

6. The nickel-based cathode material is titanium sulfide (TiS 2 ), molybdenum sulfide (MoS 2 ), iron sulfide (FeS or FeS 2 ), copper sulfide (CuS), nickel sulfide (Ni 3 S 2 ), lithium sulfide (Li 2 2. The method of claim 1, further comprising one or more of a coated or uncoated metal sulfide comprising:

7. 10. The method of claim 1, wherein the exposing comprises applying high pressure to increase the growth rate of the lithium carbonate coating.

8. 10. The method of claim 1, wherein the exposing comprises applying an elevated temperature to increase the growth rate of the lithium carbonate coating.

9. The method of claim 1, wherein the predetermined temperature is within a range of about 20°C to about 120°C.

10. 10. The method of claim 1, wherein the exposing step comprises applying a high concentration of gaseous carbon dioxide for a predetermined time to increase the growth rate of the lithium carbonate coating.

11. 10. The method of claim 1, wherein the exposing step comprises applying a high concentration of water vapor for a predetermined time to increase the growth rate of the lithium carbonate coating.

12. The method according to any one of claims 1 to 11, wherein the nickel-based cathode material is coated with a lithium-containing layer prior to exposure to gaseous carbon dioxide and water vapor.

13. The lithium-containing layer is 2 ZrO 3 , Li 2 ZrO 4 , LiCl, LiF, LiOH, Li 2 13. The method of claim 12, wherein the material comprises lithium oxynitride, lithium niobate, lithium nitride, lithium titanate, lithium silicate, or a combination thereof.

14. The method of any one of claims 1 to 13, wherein the nickel-based cathode material is not treated prior to exposure to gaseous carbon dioxide and water vapor.

15. 15. The method of any one of claims 1 to 14, wherein the lithium carbonate coating has a thickness in the range of about 5 nanometers to about 1 micrometer.

16. 16. The method of any one of claims 1 to 15, further comprising vacuum drying the lithium carbonate coated cathode to remove residual moisture.

17. 17. The method of any one of claims 1 to 16, further comprising washing the lithium carbonate coated cathode.

18. 18. The method of any one of claims 1 to 17, further comprising combining the lithium carbonate coated cathode with one or more of a suitable binder, a solid electrolyte, and a conductive additive to form a cathode for an electrochemical cell.

19. 19. The method of any one of claims 1 to 18, further comprising combining the lithium carbonate coated cathode with an anode and a separator to form a functioning electrochemical cell.

20. An electrochemical cell comprising a cathode coated with lithium carbonate having an outer lithium carbonate coating having a thickness within the range of about 2 nanometers to about 1 micron.

21. A method for producing a cathode uniformly coated with lithium carbonate in a gas mode, comprising the steps of: contacting gaseous carbon dioxide and water vapor with a nickel-based cathode material containing lithium and oxygen; Producing a cathode uniformly coated with lithium carbonate in a gas mode; Including, wherein lithium carbonate is uniformly formed as a layer on the exterior surface of the cathode material to form a lithium carbonate coated cathode.

22. The method further comprising:

22. The method of claim 21 comprising contacting the nickel-based cathode material with the carbon dioxide at a predetermined relative humidity level.

23. The method further comprising:

22. The method of claim 21, comprising contacting the nickel-based cathode material with the carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, or at a predetermined relative humidity level.

24. 22. The method of claim 21 , wherein the cathode material comprises lithium and oxygen in a molar ratio of 1:

2.

25. The method of claim 21 , wherein the nickel-based cathode material comprises a catalytic amount of nickel.

26. 22. The method of claim 21, wherein the uniform lithium carbonate coating has a thickness in the range of about 5 nanometers to 1 micrometer.

27. 22. The method of claim 21 , wherein the uniform lithium carbonate coating has a thickness in the range of about 1 nanometer to about 100 nanometers.

28. 22. The method of claim 21 , wherein the uniform lithium carbonate coating is in the range of about 1 nanometer to about 50 nanometers.

29. 22. The method of claim 21 , wherein the uniform lithium carbonate coating is in the range of about 10 nanometers to about 40 nanometers.

30. Formula LiNi a Mn b Co c O 2 where 0<a<1, 0<b<1, 0<c<1, and a+b+c=1, wherein the nickel-based cathode material is a cathode uniformly coated with lithium carbonate, and the solid-state battery cell maintains 85% or more, 90% or more, 95% or more, 98% or more, or 99% or more of its discharge capacity after three cycles.

31. Formula LiNi a Mn b Co c O 2 wherein 0<a<1, 0<b<1, 0<c<1, and a+b+c=1, wherein the nickel-based cathode material is uniformly coated with lithium carbonate, and the solid-state battery cell has a higher starting discharge capacity compared to the same nickel-based cathode material without the lithium carbonate coating.

32. 1. A cathode composition comprising: Formula LiNi a Mn b Co c O 2 where 0<a<1, 0<b<1, 0<c<1, and a+b+c=1; and A lithium carbonate layer; wherein the cathode material is uniformly coated with the lithium carbonate layer.

33. 33. The composition of claim 32, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

34. The cathode material is LiNi 0.33 Mn 0.33 Co 0.33 O 2 , LiNi 0.4 Mn 0.3 Co 0.3 O 2 , LiNi 0.5 Mn 0.3 Co 0.2 O 2 , LiNi 0.6 Mn 0.2 Co 0.2 O 2 , LiNi 0.8 Mn 0.1 Co 0.1 O 2 , LiNi 0.85 Mn 0.05 Co 0.1 O 2 33. The composition of claim 32, wherein the compound is selected from the group consisting of:

35. The cathode material is LiNi 0.33 Mn 0.33 Co 0.33 O 2 33. The composition of claim 32, comprising:

36. The cathode material is LiNi 0.4 Mn 0.3 Co 0.3 O 2 33. The composition of claim 32, comprising:

37. The cathode material is LiNi 0.5 Mn 0.3 Co 0.2 O 2 33. The composition of claim 32, comprising:

38. The cathode material is LiNi 0.6 Mn 0.2 Co 0.2 O 2 33. The composition of claim 32, comprising:

39. The cathode material is LiNi 0.8 Mn 0.1 Co 0.1 O 2 33. The composition of claim 32, comprising:

40. The cathode material is LiNi 0.85 Mn 0.05 Co 0.1 O 2 33. The composition of claim 32, comprising:

41. 33. The composition of claim 32, wherein the lithium carbonate layer is formed in a gaseous manner.

42. 33. The composition of claim 32, wherein the cathode material further comprises a metal oxide.

43. The metal oxide is LiNiO 2 , LiNi 1-Y Co Y O 2 (Wherein, 0≦Y<1), LiNi 1-Y Mn Y O 2 (Wherein, 0≦Y<1), Li(Ni a Co b Mn c ) O 4 (wherein, 0<a<2, 0<b<2, 0<c<2, and a+b+c=2); LiMn 2-Z Ni Z O 4 (Wherein, 0≦Z≦2), Li(Ni a Co b A c ) O 2 43. The composition of claim 42, wherein the compound is selected from the group consisting of: wherein 0<a<1, 0<b<1, 0<c<1, a+b+c=1, and any combination thereof.

44. The metal oxide is V 2 O 5 , V 6 O 13 , MoO 3 , LiCoO 2 , LiMnO 2 , LiMn 2 O 4 , LiCo 1-Y Mn Y O 2 (Wherein, 0≦Y<1), LiMn 2-Z Co Z O 4 (Wherein, 0≦Z≦2), LiCoPO 4 , LiFePO 4 , CuO, LiCo 0.6 Mn 0.4 O 2 , LiMn 1.5 Ni 0.5 O 4 43. The composition of claim 42, wherein the compound is selected from the group consisting of:

45. 1. A cathode composition comprising: LiNiO 2 , LiNi 1-Y Co Y O 2 (Wherein, 0≦Y<1), LiNi 1-Y Mn Y O 2 (Wherein, 0≦Y<1), Li(Ni a Co b Mn c ) O 4 (wherein, 0<a<2, 0<b<2, 0<c<2, and a+b+c=2); LiMn 2-Z Ni Z O 4 (wherein 0≦Z≦2), or Li(Ni a Co b A c ) O 2 where 0<a<1, 0<b<1, 0<c<1, and a+b+c=1; and A lithium carbonate layer; wherein the cathode material is uniformly coated with the lithium carbonate layer.

46. 46. ​​The composition of claim 45, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

47. 1. A cathode composition comprising: V 2 O 5 , V 6 O 13、 MoO 3 , LiCoO 2 , LiMnO 2 , LiMn 2 O 4 , LiCo 1-Y Mn Y O 2 (Wherein, 0≦Y<1), LiMn 2-Z Co Z O 4 (Wherein, 0≦Z≦2), LiCoPO 4 , LiFePO 4 , CuO, LiCo 0.6 Mn 0.4 O 2 , or LiMn 1.5 Ni 0.5 O 4 a cathode material comprising: A lithium carbonate layer; wherein the cathode material is uniformly coated with the lithium carbonate layer.

48. 48. The composition of claim 47, wherein the lithium carbonate layer has a thickness of about 1 nanometer to about 1 micron.

49. A method for producing a lithium carbonate coated cathode for an electrochemical cell in a gaseous mode, comprising: exposing a nickel-based cathode material containing lithium and oxygen in a 1:2 molar ratio to gaseous carbon dioxide and water vapor; incubating the nickel-based cathode material and the carbon dioxide for a predetermined time, at a predetermined temperature, at a predetermined pressure, and / or at a predetermined relative humidity level; wherein lithium carbonate is formed as a uniform layer on an outer surface of the cathode material to form a lithium carbonate coated cathode.

Citation Information

Patent Citations

  • All-solid battery

    JP2009272051A

  • Carbon dioxide treatment of cathodes

    US20190326591A1