Plated steel sheet for hot press forming with excellent surface quality and manufacturing method thereof
A plated steel sheet with controlled Zn, Si, and Fe composition, along with specific cooling and heat treatment, addresses issues of oxidation, low productivity, and peeling in hot press forming, achieving excellent surface quality and corrosion resistance for complex shape molding.
Patent Information
- Application Number
- JP2024533301
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-02-03
- Publication Date
- 2024-12-06
AI Technical Summary
High-strength steel used in hot press forming faces challenges with complex shape molding due to material breakage and springback, and plated steel sheets suffer from oxidation, low productivity, poor corrosion resistance, and plating layer peeling during hot forming.
A plated steel sheet with a specific composition of Zn: 21 to 34%, Si: 6.3 to 15%, Fe: 3 to 13%, and Al, along with controlled cooling rates and heat treatment, to ensure corrosion resistance, productivity, and adhesion of the plating layer during hot press forming.
The solution provides a plated steel sheet with excellent surface quality, corrosion resistance, and prevents peeling of the plating layer, enhancing productivity and adhesion, suitable for complex shape hot press forming applications.
Smart Images

Figure 2024545452000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a plated steel sheet for hot press forming having excellent surface quality and a method for producing the same. [Background technology]
[0002] The use of high-strength steel is increasing to reduce the weight of automobiles. However, high-strength steel has problems in that it is difficult to form products with complex and precise shapes due to the occurrence of material breakage during processing and springback phenomenon after processing. Hot Press Forming (HPF) is a method to solve these problems, and its application has been expanding recently.
[0003] The steel sheet for hot press forming is advantageous in that it is easy to form by performing press working in a state where it is usually heated to 800 to 950 ° C., and the strength of the formed product can be increased by quenching through a mold. However, when the steel material is heated at a high temperature, oxidation occurs on the surface of the steel material, which necessitates an additional process of removing the oxide on the surface of the steel sheet after press forming. To prevent this, plated steel sheets in which an aluminum plating layer, a zinc plating layer, or a mixture of both is formed on the surface of the steel sheet are used as materials for hot press forming.
[0004] However, aluminum-plated steel sheets have a very poor productivity because the melting point of the aluminum plating bath is high and the sink roll used in the plating bath has a lifespan of only 3 to 4 days, so production must be stopped periodically to replace the sink roll. Since the lifespan of such sink rolls is inversely proportional to the temperature of the plating bath, it is important to lower the temperature of the plating bath. In addition, the aluminum plating layer has a problem of poor corrosion resistance after hot press forming because the plating layer does not have sacrificial corrosion protection.
[0005] To solve these problems, attempts have been made to use galvalume, a mixture of zinc and aluminum, in the hot press process to lower the temperature of the plating bath, thereby increasing the number of cycles of use of the sink roll and increasing productivity, while improving the corrosion resistance of the plating layer. The addition of zinc lowers the temperature of the plating bath, increasing the productivity of plated steel sheets, and the zinc contained in the plating layer after plating improves the corrosion resistance of the plating layer even after hot press forming, compared to aluminum.
[0006] However, aluminum plating layers containing added zinc have the problem that the plating layer easily peels off from the base material at curved areas of the die after hot press forming, and have not been able to meet the demand for high-end steel materials, which have required strict quality standards.
[0007] Therefore, there is a need to develop technology that ensures corrosion resistance and productivity while also preventing the plating layer from peeling off from the base material during hot forming, and that provides excellent surface quality. However, to date, no technology has been developed that can meet the high-end demand for good surface quality in addition to corrosion resistance and productivity. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] U.S. Patent Publication No. 6,296,805 Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a plated steel sheet for hot press forming having excellent surface quality and a method for producing the same.
[0010] Another object of the present invention is to provide a plated steel sheet for hot press forming, which has excellent productivity and corrosion resistance, while also having excellent surface quality in which a plating layer does not peel off from a base material even after hot forming, and a manufacturing method thereof.
[0011] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding further object of the present invention from the entire content of the specification of the present invention. [Means for solving the problem]
[0012] One embodiment of the present invention comprises: Plain steel; and a coating layer provided on at least one surface of the base steel, the coating layer containing, by weight, 21 to 34% Zn, 6.3 to 15% Si, 3 to 13% Fe, the balance being Al and other unavoidable impurities; Including, Provided is a plated steel sheet for hot press forming which satisfies the following Relational Expressions 1 and 2. [Equation 1] 0.09≦[Zn] / [Si]≦4.8 [Equation 2] 3.6≦[Al] / [Si]≦8.5 (In the above Relational Formulas 1 and 2, the [Zn] represents the average Zn content by weight in the plating layer, the [Si] represents the average Si content by weight in the plating layer, and the [Al] represents the average Al content by weight in the plating layer.)
[0013] Furthermore, another embodiment of the present invention is a plating step of immersing the base steel in a plating bath containing, by weight, 21 to 34% Zn, 6.3 to 15% Si, 2% or less (including 0%) Fe, the balance being Al and other unavoidable impurities, and satisfying the following relational expressions 1 and 2, to obtain a steel sheet having a hot-dip plating layer formed on the surface thereof; and cooling the steel sheet such that an average cooling rate Vc1 is 25-90°C / s in a first section of 630-530°C and an average cooling rate Vc2 is 3-15°C / s in a second section of 529-350°C based on the surface temperature of the hot-dip coating layer; The present invention provides a method for producing a plated steel sheet for hot press forming, comprising the steps of: [Equation 1] 0.09≦[Zn] / [Si]≦4.8 [Equation 2] 3.6≦[Al] / [Si]≦8.5 (In the above Relational Formulas 1 and 2, the [Zn] indicates the average Zn content by weight in the hot-dip plated layer, the [Si] indicates the average Si content by weight in the hot-dip plated layer, and the [Al] indicates the average Al content by weight in the hot-dip plated layer.)
[0014] Furthermore, another embodiment of the present invention is The present invention provides a hot press-formed member obtained by hot press forming the above-mentioned plated steel sheet for hot press forming.
[0015] Furthermore, another embodiment of the present invention is A step of heat treating the above-mentioned plated steel sheet for hot press forming at a temperature in the range of Ac3 to 950°C for 1 to 1000 seconds; and The present invention provides a method for producing a hot press-formed member, which comprises hot press forming the heat-treated plated steel sheet for hot press forming using a die.
[0016] Furthermore, another embodiment of the present invention is A step of subjecting the plated steel sheet for hot press forming obtained by the above-mentioned method for producing a plated steel sheet for hot press forming to a heat treatment at a temperature in the range of Ac3 to 950°C for 1 to 1000 seconds; and The present invention provides a method for producing a hot press-formed member, which comprises hot press forming the heat-treated plated steel sheet for hot press forming using a die. Effect of the Invention
[0017] According to one embodiment of the present invention, it is possible to provide a plated steel sheet for hot press forming having excellent surface quality and a manufacturing method thereof.
[0018] According to another embodiment of the present invention, it is possible to provide a plated steel sheet for hot press forming, which has excellent productivity and corrosion resistance, while also having excellent surface quality in which the plating layer does not peel off from the base material even after hot forming, and a manufacturing method thereof.
[0019] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0020] [Figure 1] 1 shows a photograph of Example 11 of the present invention observed with a scanning electron microscope (SEM). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The terms used herein are for the purpose of describing particular embodiments and are not intended to limit the present invention. Furthermore, the singular forms used herein include the plural forms unless the related definition clearly indicates otherwise.
[0022] The meaning of "comprise" as used in the specification is to specify features and does not exclude the presence or addition of other features.
[0023] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Dictionary-defined terms are to be interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content.
[0024] In order to improve the problem of insufficient corrosion resistance and reduced productivity of aluminum-plated steel sheets, which were mainly used as plated steel sheets for conventional hot press forming, Zn-Al-plated steel sheets, to which zinc and aluminum are added, have been developed.
[0025] However, although Zn-Al-plated steel sheets have excellent corrosion resistance and productivity, the addition of Zn causes a material failure phenomenon called liquid metal embrittlement (LME), and there is also the problem that the plating layer easily peels off from the base material at curved areas of the die during hot forming, deteriorating adhesion.
[0026] Therefore, as a result of intensive investigations, the present inventors have found that in the production of plated steel sheet having a plating layer whose composition system includes Zn, Al, and Si, peeling of the plating layer becomes a major problem when primary aluminum crystals occur. They have also found that precise control of the Zn, Al, and Si compositions has the effects of preventing LME and improving plating layer adhesion, in addition to improving corrosion resistance and productivity, and have completed the present invention.
[0027] Hereinafter, a plated steel sheet for hot press forming according to one embodiment of the present invention will be described in detail.
[0028] The plated steel sheet for hot press forming according to the present invention includes a base iron; and a plated layer provided on at least one surface of the base iron. In this case, the type of the base iron is not limited and can be applied to any steel sheet for hot press forming. Therefore, the base iron furnace is sufficient as long as it starts austenitic transformation at a temperature of 800°C or higher and can be transformed into martensitic transformation by rapid cooling performed simultaneously with forming. As a representative example, a base iron having, in weight percent, C: 0.15 to 0.39%, Mn: 0.5 to 3%, B: 0.01% or less (including 0%), Ti: 0.1% or less (including 0%), the balance Fe and other inevitable impurities, such as 22MnB5, can be used.
[0029] In the present invention, the plating layer has a composition containing, in weight percent, Zn: 21-34%, Si: 6.3-15%, Fe: 3-13%, and the balance being Al and other unavoidable impurities. The reasons for adding each component and the reasons for limiting the content will be specifically explained below. In this case, the content of each element is expressed in weight percent unless otherwise specified.
[0030] [Zn: 21-34%] Zinc (Zn) is an element added to improve corrosion resistance. Since aluminum-plated steel sheets usually do not have sacrificial corrosion protection, the addition of zinc can ensure corrosion resistance. In addition, zinc is added to improve productivity by lowering the melting point of the plating bath and improving the life of the sink roll. Therefore, in the present invention, 21% or more of Zn is added to ensure the desired level of corrosion resistance and productivity. However, if Zn is added excessively, liquid metal embrittlement (LME) may occur during hot press forming, so the Zn content is limited to 34% or less in the present invention. However, from the viewpoint of further improving the intended effect of the present invention, the lower limit of the Zn content may be preferably 23%, more preferably 25%, and the upper limit of the Zn content may be 31.2%.
[0031] [Si:6.3~15%] Silicon (Si) is an element added to adjust the alloying of Al contained in the coating layer and Fe contained in the base steel, and the addition of Si can prevent excessive alloying. In addition, Si is an element that induces a decrease in the melting point of Al, lowers the temperature of the coating bath, and thus effectively suppresses the generation of ash in the coating bath. Therefore, in the present invention, 6.3% or more of Si is added to appropriately control the degree of alloying between Al and Fe. If the Si content in the coating layer is less than 6.3%, the Fe-Al-based interface alloy layer, which is highly brittle, is formed very thick due to excessive alloying, which may cause the coating layer to fall off due to the emergence of brittleness during processing. In addition, if the Si content exceeds 15%, the melting point of the coating bath becomes excessively higher than the melting point of pure aluminum, which may cause problems such as deterioration of the coating equipment in the coating bath and poor operability, so the Si content is limited to 15% or less in the present invention. However, from the viewpoint of further improving the intended effects of the present invention, the lower limit of the Si content may more preferably be 7.0% and the upper limit of the Si content may more preferably be 13.1%.
[0032] [Fe: 3-13%] The (Fe) content in the coating layer is preferably 3 to 13%. If the Fe content in the coating layer is less than 3%, the Al in the coating bath and the Fe in the base iron form a non-uniform Al-Fe alloy phase on the surface of the base iron, rather than a uniform alloy phase, which may cause a problem that the coating surface becomes rough and plating defects increase. If the Fe content in the coating layer exceeds 13%, an excessive Fe-Al-based interface alloy layer is formed, and the coating layer may fall off during processing due to the brittle Fe-Al-based interface alloy layer. Furthermore, since the excessive Fe-Al-based interface alloy layer formed during plating plays a role in suppressing the diffusion of Fe in the heat treatment process performed during hot press forming, the coating layer remains in a liquid state for a long time, which may cause a problem of adhesion in a heating furnace. Therefore, in the present invention, the Fe content in the coating layer is controlled to 3 to 13%. However, from the viewpoint of further improving the effect of the present invention, more preferably, the lower limit of the Fe content may be 3.8% and the upper limit of the Fe content may be 11.2%. On the other hand, the above-mentioned Fe may be contained in a small amount in the plating bath, but this may be due to a small amount of Fe flowing into the plating bath from the base steel during the manufacturing process.
[0033] [Remainder: Al and other unavoidable impurities] In addition to the above-mentioned composition of the plating layer, the balance may be Al and other inevitable impurities. The inevitable impurities may include all impurities that are unintentionally mixed in during the manufacturing process of a normal aluminum- or aluminum alloy-plated steel sheet. Such impurities are not particularly limited in the present invention because the meanings of these impurities can be easily understood by those skilled in the art.
[0034] [Mg:1.4% or less] Although not particularly limited, the plating layer may further include 1.4% or less of Mg to selectively improve corrosion resistance. The Mg acts as a buffer to suppress the decomposition of zinc oxide in a corrosive environment, thereby further improving corrosion resistance. Therefore, Mg may be selectively added in an amount of 1.4% or less. However, since Mg is a selective element, the lower limit of its content is not particularly limited, and as an example, the lower limit of the Mg content may be 0.05%.
[0035] Meanwhile, although Zn-Al-plated steel sheets have excellent corrosion resistance and productivity, there is a problem in that the addition of Zn causes a material failure phenomenon called liquid metal embrittlement (LME). The liquid metal embrittlement is a phenomenon in which zinc in the plating layer diffuses into the base steel during the plating process or hot forming process, causing brittle fracture due to grain boundary cracks. When such plated steel sheets with cracks connecting the plating layer to the base steel are used for automotive components, there is a risk of fatigue fracture due to accumulated stress generated during vehicle operation or weakening the rigidity of the vehicle body in the event of a vehicle collision, so it is necessary to suppress the LME phenomenon in hot press formed parts.
[0036] Generally, the LME phenomenon does not occur in aluminum plating layers, but it easily occurs when zinc is added. As a result of extensive research, the inventors of the present invention have confirmed that the tendency for LME to occur varies depending on the combination of Al and Zn components.
[0037] Furthermore, when Si is added to prevent alloying in addition to Al and Zn, a ternary composition is formed. During the process of solidification to form a coating layer after continuous plating, the combination of Al, Zn, and Si components changes and primary aluminum crystals occur. This has further been discovered to be a major problem with the adhesion of the coating layer.
[0038] That is, in order to simultaneously secure the corrosion resistance and productivity, as well as the prevention of LME development and the adhesion of the plating layer, it was confirmed that it is extremely important to precisely control the relationships among the three components including Al, Zn, and Si as shown in the following Relational Formulas 1 and 2.
[0039] Therefore, it is preferable that the plated steel sheet for hot press forming according to the present invention satisfies the following Relational Expressions 1 and 2. [Equation 1] 0.09≦[Zn] / [Si]≦4.8 [Equation 2] 3.6≦[Al] / [Si]≦8.5 (In the above Relational Formulas 1 and 2, the [Zn] represents the average Zn content by weight in the plating layer, the [Si] represents the average Si content by weight in the plating layer, and the [Al] represents the average Al content by weight in the plating layer.)
[0040] Specifically, if the value of [Zn] / [Si] defined by the above Relational Formula 1 is less than 0.09, it may be difficult to ensure the desired level of corrosion resistance. Also, if the value of [Zn] / [Si] exceeds 4.8, even if the corrosion resistance of the plating layer is ensured, the adhesion of the plating layer may decrease or the LME phenomenon may occur.
[0041] Furthermore, if the value of [Al] / [Si] defined by the above Relational Formula 2 is less than 3.6, the formation of smooth aluminum oxide on the surface after heat treatment is insufficient, which may result in a rough surface shape. Furthermore, if the value of [Al] / [Si] exceeds 8.5, a highly brittle-resistant Fe-Al alloy phase is formed in the coating layer after hot press forming, which may cause the coating to peel off due to the Fe-Al alloy phase when the coated steel sheet is blanked to fit the part before hot press forming, or when the steel sheet is transported due to impact.
[0042] Meanwhile, according to an embodiment of the present invention, the plating layer may include an Al-Zn-based plating layer; and an Fe-Al-based interfacial alloy layer provided between the Al-Zn-based plating layer and the base steel.
[0043] The Fe-Al-based interfacial alloy layer is a layer provided on and in contact with the base steel, and contains an intermetallic compound of Fe and Al formed by an alloying reaction between Fe and Al. Examples of the intermetallic compound of Fe and Al include FeAl, FeAl3, and Fe2Al5. In this case, the Fe-Al-based interfacial alloy layer can be similarly applied to the matters generally known in the art. Thus, the Fe-Al-based interfacial alloy layer can contain, by weight %, Fe: 30 to 50% and Al: 35 to 55%, and can further contain a portion of components that can be contained in the plating layer, such as Zn, Si, etc., in addition to Fe and Al (e.g., Si 27% or less).
[0044] In other words, the Fe-Al-based interface alloy layer can contain, by weight, 30-50% Fe, 35-55% Al, 5-27% Si, 4% or less (including 0%) Zn, and the balance being other impurities.
[0045] The Al-Zn-based coating layer may refer to a layer other than the Fe-Al-based inhibiting layer among the above-mentioned coating layers. In other words, it may refer to a layer that is provided on the Fe-Al-based inhibiting layer among the coating layers formed while the hot-dip coating layer described below is solidified, and is differentiated from the Fe-Al-based inhibiting layer by content. Specifically, the Al-Zn-based coating layer may contain, by weight, 1531% Zn, 2-12% Si, 10% or less Fe, and the balance Al and other inevitable impurities.
[0046] As an example, when analyzing a coating layer with GDS, the point where the Fe content is 50% is determined to be the interface between the base steel and the coating layer, and since the thickness of an Fe-Al system is less than 30% of that of an Al-Zn system, the GDS value measured at the midpoint between the surface of the coating layer and the depth where the Fe content is 50% is determined to be the composition value of the Al-Zn system. The composition of the Fe-Al system can be determined as the average value of the values obtained by EDS analysis of the Fe-Al alloy layer three or more times at a magnification of 1500x or more using an electron scanning microscope.
[0047] According to one embodiment of the present invention, the weight ratio (Sb / Sa) of the average Si content (Sb) in the Fe-Al alloy layer to the average Si content (Sa) in the Al-Zn plating layer may be 1 to 3.1. If the value of Sb / Sa is less than 1, an excessive Si phase is formed in the Al-Zn phase during solidification of the plating layer, and the hard Si phase may cause surface defects on the surface of the plating layer. On the other hand, if the value of Sb / Sa is 3.1 or more, the Si content of the Fe-Al alloy layer becomes excessive, and Si penetrates into the Fe-Al crystal structure, inhibiting the Fe diffusion coefficient of the Fe-Al system, inhibiting the alloying of the initial plating layer during hot press forming, causing problems such as burning, which may inhibit the adhesion of the plating layer.
[0048] That is, plated steel sheets for hot press forming are usually used in automobiles after electrocoating. However, if there is a significant hue difference on the surface during the heat treatment process or if non-uniform oxides are generated, it becomes difficult to use them as parts. Such surface defects occur when the components present in the plating layer are not uniformly alloyed during the heat treatment process and different components are locally gathered. However, the present inventors have confirmed through extensive research that the above-mentioned uniform alloying can be achieved by controlling the Sb / Sa value.
[0049] According to an embodiment of the present invention, the Al-Zn-based plating layer is provided with a unit area of 100 μm2 based on a cross section in the thickness direction of the plating layer. 2 The Al-Zn-based coating layer may include a region in which the Si content is enriched by 40% or more relative to the average Si content of the Al-Zn-based coating layer per unit area. By including a region in which Si is enriched in this way, the Si phase concentrated at the interface at the initial stage of heat treatment and the enriched Si phase in the coating layer simultaneously dissolve in the molten aluminum, thereby maintaining a uniform Si content throughout the coating layer, thereby making it possible to further improve the coating adhesion after hot press forming.
[0050] According to one embodiment of the present invention, the Al-Zn-based plating layer may contain a Si phase at an area fraction of 3 to 30% based on a cross section in the thickness direction of the layer, where the Si phase means a phase containing 40 to 99.9% Si by weight.
[0051] In the present invention, by controlling the content of the Si phase to about 3 to 30%, it is possible to prevent the falling-off phenomenon caused by the highly brittle Fe-Al interfacial alloy layer at the interface between the base steel and the coating layer before hot forming, and at the same time, it is possible to prevent the peeling phenomenon of the coating layer that easily occurs during hot forming due to the inclusion of zinc. Therefore, even if a coated steel sheet having a coating layer of a component system containing Zn and Al is used for hot press forming, it is possible to further improve the adhesion of the coating layer as well as the corrosion resistance, productivity, and prevention of LME.
[0052] That is, hot press formed parts are mainly used for parts with complex shapes and high strength compared to cold formed products. For this reason, deep drawing is necessary to manufacture complex shapes, and due to the characteristics of hot press forming in which dies are often used, there is a problem that peeling of the plating layer is likely to occur after applying hot press forming, in addition to the phenomenon of falling off due to excessive formation of a brittle Fe-Al based interfacial alloy layer due to friction and tolerance between the die and the plating layer.
[0053] Until now, no attention had been paid to the problem of the plating layer easily peeling off after hot press forming. However, as a result of intensive investigation, the inventors have confirmed that by precisely controlling conditions such as the above-mentioned Sb / Sa value, the presence or absence of regions with concentrated Si content (C), and the area fraction of the Si phase, it is possible to solve not only the peeling phenomenon originating from the base steel and the Fe-Al-based interface alloy layer, but also the defect problem after part forming that mainly occurs between the Al-Zn-based plating layer and the Fe-Al-based interface alloy layer.
[0054] Next, a method for producing a plated steel sheet for hot press forming according to another embodiment of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet for hot press forming according to the present invention must be produced by the following method.
[0055] The coated steel sheet for hot press forming according to the present invention includes a coating step of immersing the above-mentioned base iron in a coating bath containing, by weight, 21 to 34% Zn, 6.3 to 15% Si, 2% or less (including 0%) Fe, the balance being Al and other inevitable impurities, and satisfying the following relational expressions 1 and 2, to obtain a steel sheet having a hot-dip coating layer formed on the surface. In this case, the reasons for adding the coating bath components and the reasons for limiting the content can be similarly applied to the explanation of the coating layer described above. That is, since the composition of the coating layer contains components derived from the base iron, the components may vary slightly from those of the coating bath, but other than those derived from the base iron, the reasons for adding each component in the coating bath and the reasons for limiting the lower and upper limits of the numerical values are the same. [Equation 1] 0.09≦[Zn] / [Si]≦4.8 [Equation 2] 3.6≦[Al] / [Si]≦8.5 (In the above Relational Formulas 1 and 2, the [Zn] indicates the average Zn content by weight in the hot-dip plated layer, the [Si] indicates the average Si content by weight in the hot-dip plated layer, and the [Al] indicates the average Al content by weight in the hot-dip plated layer.)
[0056] Next, although not particularly limited, according to one embodiment of the present invention, after the plating step, cooling may be performed so that the average cooling rate Vc1 is 25-90°C / s in a first section of 630-530°C based on the surface temperature of the hot-dip plating layer on the steel sheet, and the average cooling rate Vc2 is 3-15°C / s in a second section of 529-350°C. At this time, the cooling may be controlled to satisfy the following Relation 3. [Equation 3] Vc2≦Vc1 / 7
[0057] As mentioned above, by precisely controlling the cooling rate of the hot-dip coating layer after the coating step, it is possible to exert an effect of improving the surface quality of the coating layer.
[0058] Specifically, by controlling the cooling rate to a high value of 25-90°C / s in the first section, the size of the spangles inherent to aluminum at the time of solidification of the coating layer in the first section becomes smaller and finer, making the surface roughness uniform and improving the surface quality. Also, by controlling the average cooling rate to a low value of about 3-15°C / s in the second section, the amount of air blown by the cooling tower can be reduced, thereby reducing the inclusion of foreign matter in the coating layer.
[0059] According to an embodiment of the present invention, the base steel may be heat-treated in an annealing furnace having a temperature of 650 to 850°C and a hydrogen ratio of 0.1 to 30% before the plating step. The heat treatment is performed at a temperature equal to or higher than the recrystallization temperature to prevent work hardening of the material in the continuous plating process, and the base steel sheet may be maintained at a temperature higher than the plating bath to improve the galvanizability. If the heat treatment temperature is less than 650°C, there is a disadvantage that the material may be deformed and meandered due to work hardening when passing through rolls such as in a continuous process. In addition, if the heat treatment temperature exceeds 850°C, Mn and Si present in the base steel sheet may be concentrated on the surface of the base steel sheet to form oxides, which may deteriorate the characteristics. Therefore, the temperature of the heat treatment before the plating is preferably controlled to 650 to 850°C, and more preferably, the lower limit of the heat treatment temperature may be 700°C, and the upper limit of the heat treatment temperature may be 810°C.
[0060] In addition, the heat treatment can be controlled to a reducing atmosphere in which the hydrogen ratio is 0.1 to 30% and the remainder is nitrogen gas. If high-purity nitrogen gas is not used, it may be difficult to maintain a reducing atmosphere in the heat treatment furnace, and cleaning the surface of the base steel sheet may be difficult. In this case, if hydrogen gas is added at 0.1% or more, the dew point in the heat treatment furnace can be lowered, the reducing atmosphere can be maintained, additional oxidation of the base steel can be prevented, and the base surface can be cleaned. However, if the hydrogen gas ratio exceeds 30%, there is a risk of the heat treatment furnace exploding due to contact with oxygen when the hydrogen gas leaks into the atmosphere. Therefore, in the present invention, the hydrogen ratio during the heat treatment can be controlled to 0.1 to 30%, and more preferably, the lower limit of the hydrogen ratio may be 5%, and the upper limit of the hydrogen ratio may be 25%.
[0061] At this time, although not particularly limited, the annealing may be performed in an atmosphere with a dew point temperature of −30 to −60° C. If the dew point temperature during the annealing is less than −30° C., a sufficient reducing atmosphere cannot be created, which may cause a problem in reducing Fe oxides formed on the surface, and if the dew point temperature exceeds −60° C., a problem occurs in that high purity nitrogen, etc. is used to maintain a clean atmosphere, resulting in high costs.
[0062] According to one embodiment of the present invention, the temperature of the plating bath can be controlled to be Tb+20°C to Tb+80°C based on the melting point (Tb) of the plating bath. If the temperature of the plating bath is less than Tb+20°C, the plating bath may solidify at a position in the plating pot where heat can escape to the outside, such as a sink roll, and the like, and a problem of low fluidity may occur at an overall low temperature. In addition, if the temperature of the plating bath exceeds Tb+80°C, the high temperature of the plating bath may cause a problem of shortening the roll replacement period due to deterioration of equipment, etc., and operation at high temperatures may become difficult. Therefore, in the present invention, it is preferable to control the temperature of the plating bath to be in the range of Tb+20°C to Tb+80°C.
[0063] Another embodiment of the present invention provides a hot press-formed member obtained by hot press forming the above-mentioned plated steel sheet for hot press forming.
[0064] In addition, another embodiment of the present invention relates to a method for producing a plated steel sheet for hot press forming, comprising the steps of: heat treating the plated steel sheet for hot press forming obtained by the above-mentioned method for producing a plated steel sheet for hot press forming at a temperature in the range of Ac3 to 950° C. for 1 to 1000 seconds; and The present invention provides a method for producing a hot press-formed member, which comprises hot press forming the heat-treated plated steel sheet for hot press forming using a die.
[0065] However, the hot press-formed member and the manufacturing method thereof may be applied without limitation to matters commonly known in the art, and therefore, no special limitations are imposed in the present specification. EXAMPLES
[0066] (Example) The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. This is because the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0067] (Experimental Example 1) A base iron containing, by weight, 0.23% C, 1.3% Mn, 0.002% B, 0.03% Ti, 0.25% Si, 0.15% Cr, with the balance being Fe and other impurities, was prepared. The base iron was heat-treated at 750°C in an annealing furnace with a dew point temperature of -50°C and a mixed atmosphere of 5% hydrogen and 95% nitrogen, and then immersed in a coating bath under the conditions shown in Table 1 below to form a hot-dip coating layer on the surface of the base iron. Thereafter, the base iron was treated with an air knife under the conditions shown in Table 1 below to control the coating weight per side, and then cooled to produce a coated steel sheet for hot press forming.
[0068] [Table 1]
[0069] Test pieces were prepared for each of the plated steel sheets for hot press forming obtained by the method in Table 1, and the alloy composition of the plating layer was analyzed. Specifically, the alloy composition of the plating layer was analyzed by first dissolving the plating layer in a NaOH solution for 10 minutes to remove the aluminum oxide film present on the surface, and then dissolving the plating layer for 30 minutes using an HCl solution and an inhibitor, and the two solutions thus obtained were combined and measured by ICP-OES (Inductively Coupled Plasma Optical Emission Spectroscopy), and the results are shown in Table 2 below.
[0070] [Table 2]
[0071] A test piece was taken from the plated steel sheet manufactured by the above-mentioned method, cut into a blank, and maintained in a 900°C furnace for 2 minutes after the blank test piece reached 900°C. The heated blank test piece was then transferred to a mold within 20 seconds and hot-formed using the mold, followed by cooling at a cooling rate of 20°C / s to obtain a hot-formed part.
[0072] Next, the occurrence of LME, corrosion resistance after hot press forming, whether or not peeling occurred at the interface between the base steel and the coating layer before hot forming, and coating adhesion after hot press forming were evaluated according to the following criteria, and the results are shown in Table 3 below.
[0073] [Whether or not LME occurs] The cross section of each hot press formed test piece in the thickness direction (meaning the direction perpendicular to the rolling direction) was observed with an optical microscope to measure the crack depth in the base material. Test pieces with crack depths of 30 μm or more in the base material were designated as "LME occurring" test pieces.
[0074] [Corrosion resistance after hot press forming] The test specimens were heat-treated to reach 900℃, maintained for 2 minutes, and then rapidly cooled. The test specimens were then evaluated using the salt spray test (SST), which is one of the corrosion acceleration evaluation methods. In other words, the test specimens were sprayed with salt water for 30 days in the SST, and the corrosion products were removed by shot blasting, and the maximum depth of the cracks generated by corrosion in the base steel was measured. ○: When the crack depth is 30% or less of the base material thickness ×: When the crack depth exceeds 30% of the base material thickness
[0075] [Whether or not peeling occurs at the interface between the base steel and the plating layer] To evaluate the occurrence of shedding at the interface between the base steel and the coating layer, test pieces of the coated steel sheets before hot press forming were bent 90 degrees, and then it was evaluated whether shedding occurred at the interface between the base steel and the coating layer due to the brittle Fe-Al-based interfacial alloy layer. Cases where shedding occurred were marked as "shedding".
[0076] [Plating adhesion after hot press forming] The test pieces were heat treated to reach 900℃, and then heated for 2 minutes. The test pieces were then pressed to measure the peeling of the plating layer on the surface. The major axis length of the area that had peeled off from the part was measured and evaluated according to the following criteria. ◎: Less than 1mm along the long axis of the detached area ○: The major axis length of the detached area is 1 mm or more and less than 3 mm ×: The major axis length of the detached area is 3 mm or more.
[0077] [Table 3]
[0078] As can be seen from Table 3 above, the examples of the invention, which satisfy all of the coating layer compositions, Relational Formula 1, Relational Formula 2, and manufacturing conditions specified in the present invention, suppressed the occurrence of LME, while preventing peeling at the interface between the base steel and the coating layer, and were excellent in both corrosion resistance after hot press forming and coating adhesion after hot press forming.
[0079] On the other hand, in the case of Comparative Examples 1 to 9 which do not satisfy one or more of the composition of the coating layer, Relational Formula 1, Relational Formula 2, and manufacturing conditions specified in the present invention, it was confirmed that one or more of the properties among the LME characteristics, the occurrence of peeling at the interface between the base steel and the coating layer, the corrosion resistance after hot press forming, and the coating adhesion after hot press forming were inferior.
[0080] (Experimental Example 2) A plated steel sheet for hot press forming was produced in the same manner as in Experimental Example 1 described above, except that the base steel was heat-treated and plated at 750°C using an annealing furnace with a dew point temperature of -50°C and a mixed atmosphere of 5% hydrogen and 95% nitrogen, and then the hot-dip plated layer was cooled under the conditions shown in Table 4 below.
[0081] [Table 4] Vc1*: Average cooling rate in the range of 630 to 530°C based on the surface temperature of the hot-dip coating layer Vc2*: Average cooling rate in the range of 530 to 350°C based on the surface temperature of the hot-dip coating layer
[0082] In the same manner as in Experimental Example 1, the compositions of the plating layers of the plated steel sheets for hot press forming obtained in the respective invention examples and working examples were analyzed and are shown in Table 5 below.
[0083] [Table 5]
[0084] Next, cross-sectional test pieces were prepared by cutting each of the above-mentioned plated steel sheets in the thickness direction (meaning the direction perpendicular to the rolling direction of the steel sheets) and then observed with a scanning electron microscope (SEM). It was confirmed that a plated layer was formed on the base iron, that the plated layer was an Fe-Al-based interfacial alloy layer in contact with the base iron, and that an Al-Zn plated layer was formed on the Fe-Al-based interfacial alloy layer.
[0085] For the plating layer of each plated steel sheet, the average Si value was measured using GDS at a point that was 1 / 2t based on the total thickness t of the plating layer, and this was expressed as Sa below. Furthermore, for cross-sectional test pieces in the thickness direction of each plated steel sheet, EDS point analysis of the Fe-Al-based interface alloy layer formed adjacent to the base steel was performed three or more times by observing them with an electron microscope, and the average of the measured values was expressed as Sb below.
[0086] In addition, the cross-sectional test pieces were analyzed by SEM and EDS point analysis in the same manner as described above, and the unit area of the plating layer was 100 μm 2 The presence or absence of an area (C) where the Si content was concentrated by 40% or more relative to the average Si content of the Al-Zn-based coating layer per unit area was measured. Similarly, using SEM and EDS, a Si phase containing 40 to 99.9% Si was detected, and the area fraction (D) of the Si phase was measured based on the cross section of the coating layer. At this time, the value of D was measured in an area having an overall length of 75 μm or more in the rolling direction. Such measured values are shown in Table 6 below.
[0087] [Table 6] Sa*: Average Si content in the Al-Zn coating layer [wt%] Sb*: Average Si content in Fe-Al alloy layer [wt%] C*: 100μm2 of unit area of the plating layer based on the cross section in the thickness direction (perpendicular to the rolling direction) of the Al-Zn plating layer 2 Whether there are any areas where the Si content is concentrated by 40% or more compared to the average Si content of the plating layer [○ / ×] D*: Area fraction of the Si phase [%] based on the cross section of the Al-Zn coating layer in the thickness direction
[0088] For each of the plated steel sheets thus obtained, the properties shown in Table 7 below were evaluated in the same manner as in Experimental Example 1. Furthermore, the surface quality properties were additionally evaluated according to the following criteria and the results are shown in Table 7.
[0089] [Surface quality] The test pieces were visually observed to evaluate whether there was a difference in hue on the surface, and whether there was any overall unevenness due to zinc oxide produced excessively on the surface, and were evaluated according to the following criteria. Good: No color difference or unevenness on the surface is observed Surface hue difference: 50mm where the surface has a different hue from the surrounding area 2 There are more than two areas Surface unevenness: Unevenness is found on the surface
[0090] [Table 7]
[0091] As can be seen from Table 7 above, in the case of the examples of the invention which not only satisfy the composition of the plating layer, Relational Formula 1, and Relational Formula 2 specified in the present invention, but also satisfy one or more of the Sb / Sa value: 1 to 3.1, the presence of C, and D of 3 to 30% specified in Table 6, it was confirmed that not only the LME, corrosion resistance, plating adhesion, and surface quality but also the surface characteristics are extremely excellent.
[0092] In particular, a photograph taken by observing with a scanning electron microscope (SEM) a cross-sectional test piece in the thickness direction of the plated steel sheet obtained from Example 11 is shown in Figure 1. From this, it was confirmed that there was a region in the plated layer where the Si content was concentrated by 40% or more relative to the average Si content of the plated layer, and that the Si phase with a Si content of 40% or more was contained in an area fraction of 3 to 30%.
[0093] On the other hand, in the case of the comparative examples which do not satisfy one or more of the plating layer composition specified in the present invention, the Sb / Sa value specified in Relational Formulas 1 and 2 and Table 6: 1 to 3.1, the presence of C, and D of 3 to 30%, it was confirmed that one or more of the above-mentioned characteristics were deteriorated.
Claims
1. Bare iron; and a plating layer provided on at least one surface of the base steel, the plating layer containing, by weight, 21 to 34% Zn, 6.3 to 15% Si, 3 to 13% Fe, the balance being Al and other unavoidable impurities; Including, A plated steel sheet for hot press forming, which satisfies the following Relational Expressions 1 and 2. [Relationship 1] 0.09≦[Zn] / [Si]≦4.8 [Relationship 2] 3.6≦[Al] / [Si]≦8.5 (In the Relational Formulas 1 and 2, the [Zn] represents the average Zn content by weight in the plating layer, the [Si] represents the average Si content by weight in the plating layer, and the [Al] represents the average Al content by weight in the plating layer.)
2. The plated steel sheet for hot press forming according to claim 1, wherein the plating layer contains, by weight %, 25 to 34% Zn.
3. The plating layer is Al-Zn-based plating layer; and 2. The plated steel sheet for hot press forming according to claim 1, further comprising: an Fe-Al-based interfacial alloy layer provided between the Al-Zn-based plating layer and the base steel.
4. The plated steel sheet for hot press forming according to claim 3, wherein a weight ratio (Sb / Sa) of an average Si content (Sb) in the Fe-Al based alloy layer to an average Si content (Sa) in the Al-Zn based plating layer is 1 to 3.
1.
5. Based on a cross section of the Al-Zn-based plating layer in the thickness direction, the unit area of the plating layer is 100 μm 2 The plated steel sheet for hot press forming according to claim 3, comprising a region in which the Si content is concentrated by 40% or more relative to the average Si content of the Al-Zn-based plating layer per unit area.
6. The plated steel sheet for hot press forming according to claim 3, wherein the Al-Zn-based plating layer contains a Si phase in an area fraction of 3 to 30% based on a cross section in a thickness direction of the Al-Zn-based plating layer.
7. The plated steel sheet for hot press forming according to claim 6, wherein the Si phase contains, by weight %, 40 to 99.9% Si.
8. A plating step of immersing the base steel in a plating bath containing, by weight, 21 to 34% Zn, 6.5 to 15% Si, 2% or less (including 0%) Fe, the balance being Al and other inevitable impurities, and satisfying the following relational expressions 1 and 2 to obtain a steel sheet having a hot-dip plating layer formed on the surface thereof; and A method for producing a plated steel sheet for hot press forming, comprising: [Relationship 1] 0.09≦[Zn] / [Si]≦4.8 [Relationship 2] 3.6≦[Al] / [Si]≦8.5 (In the Relational Formulas 1 and 2, the [Zn] represents the average weight percent content of Zn in the hot-dip plated layer, the [Si] represents the average weight percent content of Si in the hot-dip plated layer, and the [Al] represents the average weight percent content of Al in the hot-dip plated layer.)
9. 9. The method for producing a plated steel sheet for hot press forming according to claim 8, further comprising, after the plating step, a step of cooling the steel sheet such that an average cooling rate Vc1 in a first section of 630 to 530° C. is 25 to 90° C. / s and an average cooling rate Vc2 in a second section of 529 to 350° C. is 3 to 15° C. / s based on a surface temperature of the hot-dip plated layer on the steel sheet.
10. The method for producing a plated steel sheet for hot press forming according to claim 8 , which satisfies the following relational expression 3: [Relationship 3] Vc2≦Vc1 / 7
11. 9. The method for producing a plated steel sheet for hot press forming according to claim 8, further comprising, prior to the plating step, a step of heat treating the base steel in an annealing furnace having a temperature of 650 to 850° C., a dew point temperature of −30 to −60° C., and a hydrogen ratio of 0.1 to 30%.
12. The method for producing a plated steel sheet for hot press forming according to claim 8, wherein a temperature of the plating bath is controlled to be within a range of Tb+20°C to Tb+80°C based on a melting point (Tb) of the plating bath.
13. A hot press-formed member obtained by hot press forming the plated steel sheet for hot press forming according to claim 1.
14. A step of subjecting the plated steel sheet for hot press forming according to claim 1 to a heat treatment at a temperature in the range of Ac3 to 950° C. for 1 to 1000 seconds; and The heat-treated plated steel sheet for hot press forming is hot press formed using a die.
Citation Information
Patent Citations
HOT-DIP Al-Zn PLATED STEEL SHEET, AND METHOD FOR MANUFACTURING THE SAME
JP2010070784A
Plated steel sheet for hot press forming, formed member using the same, and manufacturing method thereof
JP2021509437A
Steel for hot press forming and mmehtod for manufacturing the same
KR101639843B1
Al plated steel sheet and production method therefor
WO2019220592A1
Aluminum alloy-plated steel sheet, hot-formed member, and methods for manufacturing aluminum alloy-plated steel sheet and hot-formed member