Holding device

The holding device addresses warping and peeling issues in electrostatic chucks by using a heat resistance layer with controlled thermal shrinkage and expansion, ensuring stability and uniform temperature distribution for improved semiconductor manufacturing.

JP7551670B2Active Publication Date: 2024-09-17NITERRA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022002699
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-12
Publication Date
2024-09-17
Estimated Expiration
2042-01-12

AI Technical Summary

Technical Problem

Existing electrostatic chucks and similar holding devices experience warping and peeling issues due to differences in thermal expansion coefficients between ceramic substrates and support parts, leading to instability and reduced performance at high temperatures.

Method used

A holding device with a ceramic substrate and a support part bonded by a heat resistance layer and a stress relaxation layer, where the heat resistance layer has a thermal shrinkage rate of 0.5% or less, an elastic modulus of 10 GPa or less, and a thermal expansion coefficient close to that of the ceramic substrate, to mitigate thermal stress and prevent warping.

Benefits of technology

The solution effectively suppresses warping and peeling of the ceramic substrate, maintaining flatness and improving the yield in semiconductor manufacturing by ensuring uniform temperature distribution and stability at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551670000006
    Figure 0007551670000006
  • Figure 0007551670000005
    Figure 0007551670000005
  • Figure 0007551670000007
    Figure 0007551670000007
Patent Text Reader

Abstract

To provide technique for suppressing warpage of a ceramic substrate in a holding device which holds an object.SOLUTION: A holding device comprises: a ceramic substrate which includes ceramic as a main component, and has a first surface and a second surface as a back surface of the first surface; a support portion which is arranged in such a manner that the support portion faces the second surface of the ceramic substrate, and which has, as a main component, material having a thermal expansion coefficient different from that of ceramic; and a joining portion which is arranged between the ceramic substrate and the support portion, and joins the ceramic substrate and the support portion together. The joining portion includes: a thermal resistance layer which is joined to the second surface of the ceramic substrate; and a stress relaxation layer which has an elastic modulus is lower than that of the thermal resistance layer, and which is joined to the support portion. The thermal resistance layer is made of a heat resistance resin having a heat resistance property higher than that of the stress relaxation layer, and which has a thermal shrinkage rate after a heating for two hours at 350°C of 0.5% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a holding device for holding an object. [Background technology]

[0002] For example, an electrostatic chuck is used as a holding device for holding an object such as a wafer when manufacturing a semiconductor. The electrostatic chuck includes a ceramic substrate on which the object is placed, a support for supporting the ceramic substrate, and a joint for joining the ceramic substrate and the support. The electrostatic chuck may be used at a temperature of the wafer surface exceeding 150°C during operation. If the thermal expansion coefficients of the ceramic substrate and the support are different, the difference in thermal expansion may cause warping of the ceramic substrate surface or peeling of the joint, so the joint is required to have high heat resistance, high thermal resistance, and high flexibility.

[0003] In response to this problem, a technology has been proposed in which a highly heat-resistant first layer is disposed on the ceramic substrate side and a highly flexible second layer is disposed on the support member side at the joint, thereby achieving a balance between heat resistance and flexibility and suppressing peeling (see, for example, Patent Document 1).In addition, a technology has been proposed in which the joint has a multi-layer structure with a recess in the center to prevent peeling (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5948513 [Patent Document 2] International Publication No. 2019 / 176544 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the electrostatic chuck described in Patent Document 1 does not mention the thermal shrinkage rate of the first layer, and there is a problem that warping occurs after cooling when the thermal shrinkage rate of the first layer is large. Similarly, the electrostatic chuck described in Patent Document 2 also has a problem that warping occurs after cooling when the thermal shrinkage rate is large.

[0006] This problem is not limited to electrostatic chucks, but is common to holding devices such as heater devices, susceptors, and mounting tables for vacuum apparatuses such as CVD (chemical vapor deposition), PVD (physical vapor deposition), and PLD (pulsed laser deposition).

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide a technique for suppressing warping of a ceramic substrate in a holding device that holds an object. [Means for solving the problem]

[0008] The present invention has been made to solve the above-mentioned problems, and can be realized in the following forms.

[0009] (1) According to one aspect of the present invention, there is provided a holding device for holding an object. The holding device includes a ceramic substrate mainly made of ceramic and having a first surface and a second surface opposite to the first surface, a support part arranged to face the second surface of the ceramic substrate and mainly made of a material having a thermal expansion coefficient different from that of the ceramic, and a support part arranged between the ceramic substrate and the support part and configured to support the ceramic substrate and the support part. and a joining portion that joins the support portion to the second surface of the ceramic substrate, the joining portion having a thermal resistance layer joined to the second surface of the ceramic substrate, and a stress relaxation layer having a lower elastic modulus than the thermal resistance layer and joined to the support portion, the thermal resistance layer being made of a heat-resistant resin having a higher heat resistance than the stress relaxation layer, and having a thermal shrinkage rate of 0.5% or less after heating at 350°C for two hours.

[0010] With this type of holding device, the thermal shrinkage rate of the thermal resistance layer after heating at 350°C for two hours is 0.5% or less, so that when the ceramic substrate of the holding device is heated, held at that temperature, and then cooled, the force that causes the thermal resistance layer to shrink from its original size can be suppressed, and changes in the flatness (warping) of the ceramic substrate can be suppressed.

[0011] (2) In the holding device of the above embodiment, the thermal resistance layer may have an elastic modulus of 10 (GPa) or less. When the thermal resistance layer has an elastic modulus of 10 (GPa) or less, the force pulling the ceramic substrate can be suppressed when the thermal resistance layer thermally shrinks as the temperature of the holding device increases or decreases, and warping of the first surface of the ceramic substrate can be further suppressed.

[0012] (3) In the holding device of the above embodiment, the difference between the thermal expansion coefficient of the material forming the thermal resistance layer and the thermal expansion coefficient of the ceramic of the ceramic substrate is 20×10 -6 (1 / °C). In this way, the thermal resistance layer follows the thermal expansion that accompanies the rise and fall of temperature due to the operation of the holding device, so that the residual stress in the thermal resistance layer can be suppressed. As a result, the thermal contraction of the thermal resistance layer can be suppressed, and the warping of the first surface of the ceramic substrate can be suppressed.

[0013] (4) In the holding device of the above embodiment, the distortion of the thermal resistance layer may be 10 μm or more. In this way, the thermal resistance layer itself can be easily deformed, so that the stress relaxation property of the thermal resistance layer can be improved and the warping of the first surface of the ceramic substrate can be further suppressed.

[0014] (5) In the holding device of the above embodiment, the thickness of the thermal resistance layer may be 0.1 (mm) or more. In this way, when the temperature rises or falls due to the operation of the holding device, a sudden temperature change in the thermal resistance layer can be suppressed, the thermal contraction rate of the thermal resistance layer can be reduced, and warping of the first surface of the ceramic substrate can be further suppressed.

[0015] (6) In the holding device of the above aspect, the ceramic substrate may have a thickness of 2 mm or more. This makes it difficult for the ceramic substrate itself to deform, and makes it possible to suppress warping of the ceramic substrate.

[0016] (7) In the holding device of the above embodiment, no gap may exist between the ceramic substrate and the thermal resistance layer after the ceramic substrate is heated at 200° C. for 50 hours, which can further suppress peeling between the ceramic substrate and the thermal resistance layer caused by temperature rise and fall due to operation of the holding device.

[0017] The present invention can be realized in various forms, for example, in the form of a semiconductor manufacturing apparatus including a holding device. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is an explanatory diagram illustrating a schematic external configuration of an electrostatic chuck 10 according to an embodiment. [Diagram 2] 1 is an explanatory diagram illustrating a schematic configuration of an XZ cross section of the electrostatic chuck 10. FIG. [Diagram 3] 10A to 10C are diagrams illustrating deformation of a ceramic substrate caused by increasing and decreasing the temperature of an electrostatic chuck 10P of a comparative example. [Figure 4] 2A to 2C are explanatory diagrams of a manufacturing method of the electrostatic chuck 10 according to the embodiment. [Diagram 5] FIG. 13 is an explanatory diagram of a method for measuring distortion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <Embodiment> FIG. 1 is an explanatory diagram that shows a schematic external configuration of an electrostatic chuck 10 according to an embodiment. FIG. 2 is an explanatory diagram that shows a schematic configuration of an XZ cross section of the electrostatic chuck 10. In FIG. 1 and FIG. 2, mutually orthogonal XYZ axes are shown to specify the directions. In FIG. 2, the positive Y-axis direction is the direction toward the back side of the paper. In this specification, for convenience, the positive Z-axis direction is referred to as the upward direction and the negative Z-axis direction is referred to as the downward direction, but the electrostatic chuck 10 may actually be installed in a direction different from these directions. The electrostatic chuck 10 in this embodiment is also referred to as a "holding device."

[0020] The electrostatic chuck 10 is a device that attracts and holds an object (e.g., a wafer W) by electrostatic attraction, and is used, for example, to fix the wafer W in a vacuum chamber of a semiconductor manufacturing device. The electrostatic chuck 10 may be used for a long period of time (e.g., 1000 hours or more) at high temperatures, for example, of 150° C. or higher.

[0021] The electrostatic chuck 10 includes a ceramic substrate 100, a support portion 200, and a joint portion 300 that joins the ceramic substrate 100 and the support portion 200 together, the support portions 200 being arranged in a vertical direction (Z-axis direction).

[0022] The ceramic substrate 100 is a plate-like member having a first surface S1 having a substantially circular planar shape and a second surface S2 which is the back surface of the first surface S1. In this embodiment, the first surface S1 of the ceramic substrate 100 functions as a mounting surface on which a wafer W is mounted. The ceramic substrate 100 is a dense body mainly composed of ceramics (e.g., alumina, aluminum nitride, etc.) known as fine ceramics or new ceramics. The diameter of the first surface S1 of the ceramic substrate 100 is, for example, about 50 mm to 500 mm (usually about 200 mm to 350 mm).

[0023] An adsorption electrode 116 (FIG. 2) made of a conductive material (e.g., tungsten, molybdenum, etc.) is disposed inside the ceramic substrate 100. The shape of the adsorption electrode 116 as viewed in the Z-axis direction is, for example, substantially circular. When a voltage is applied to the adsorption electrode 116 from a power source (not shown), an electrostatic force is generated, and the wafer W is adsorbed and fixed to the first surface S1 of the ceramic substrate 100 by this electrostatic force.

[0024] Furthermore, inside the ceramic substrate 100, a heater 118 (FIG. 2) that is spiral-shaped as viewed in the Z-axis direction is disposed below the attraction electrode 116 (on the negative Z-axis side). In this embodiment, the heater 118 is a metallized layer made of tungsten, molybdenum, or the like. The shape of the heater 118 is not limited to this embodiment, and may be, for example, a disk shape. In other embodiments, the ceramic substrate 100 may not include the heater 118.

[0025] Although there are no particular limitations on the thickness of the ceramic substrate 100, it is preferable that the thickness is 2 mm or more. In this way, the thickness of the ceramic substrate 100 can suppress warping of the ceramic substrate 100 itself.

[0026] The support portion 200 is a plate-like member having a substantially circular flat shape with a diameter larger than that of the ceramic substrate 100. The support portion 200 is made of a metal having a high thermal conductivity. For example, aluminum, titanium, molybdenum, alloys containing each of these as a main component, etc. can be used. The diameter of the support portion 200 is, for example, about 220 mm to 550 mm (usually 220 mm to 350 mm). 50 mm), and the thickness of the support portion 200 is, for example, about 20 mm to 40 mm.

[0027] A coolant flow passage 210 (FIG. 2) is formed inside the support part 200. When the wafer W held on the ceramic substrate 100 of the electrostatic chuck 10 is processed using plasma, heat is input from the plasma to the wafer W, and the temperature of the wafer W rises. When a coolant (e.g., a fluorine-based inert liquid or water) flows through the coolant flow passage 210 formed in the support part 200, the support part 200 is cooled. The ceramic substrate 100 is cooled by heat transfer between the support part 200 and the ceramic substrate 100 via the bonding part 300, and the wafer W held on the first surface S1 of the ceramic substrate 100 is cooled. This realizes temperature control of the wafer W. In other embodiments, the support part may not have a coolant flow passage formed therein, and may be cooled from the outside.

[0028] The bonding portion 300 is a substantially circular, flat, plate-like member having a diameter equal to that of the ceramic substrate 100, and is disposed between the ceramic substrate 100 and the supporting portion 200 to bond the ceramic substrate 100 and the supporting portion 200. The bonding portion 300 has a thermal resistance layer 310 bonded to the second surface S2 of the ceramic substrate 100, and a stress relaxation layer 320 having a lower elastic modulus than the thermal resistance layer 310 and bonded to the supporting portion 200. The thermal resistance layer 310 mainly ensures heat resistance, and the stress relaxation layer mainly relaxes stress associated with the difference in thermal expansion coefficient between the ceramic substrate 100 and the supporting portion 200.

[0029] The thermal resistance layer 310 is made of a heat-resistant resin having higher heat resistance than the stress relaxation layer 320, and has a thermal shrinkage rate of 0.5% or less after heating at 350° C. for 2 hours. The heat-resistant resin preferably has a heat weight loss of 5% or less at 300° C. The resin forming the thermal resistance layer 310 is not particularly limited, but examples of the resin that can be used include polyimide, PEEK (Poly Ether Ether Ketone), epoxy, polybenzimidazole, etc.

[0030] FIG. 3 is an explanatory diagram of deformation of the ceramic substrate of the electrostatic chuck 10P of the comparative example with temperature rise and fall. FIG. 3(A) shows the initial state, FIG. 3(B) shows the high temperature state, and FIG. 3(C) shows the state when the temperature returns to room temperature. The electrostatic chuck 10P of the comparative example has a thermal resistance layer 310P different from that of the embodiment, but the other configurations are the same. The thermal resistance layer 310P has a thermal contraction rate of more than 0.5%. As described above, the electrostatic chuck may be used for more than 1000 hours at a high temperature of, for example, 150° C. or more. When used at such a high temperature, each part (ceramic substrate 100, support part 200, and joint part 300P) constituting the electrostatic chuck 10P thermally expands. At this time, the support part 200 has the largest thermal expansion, so the stress relaxation layer 320 of the joint part 300 is stretched (FIG. 3(B)).

[0031] When the electrostatic chuck 10P returns to room temperature after being used at high temperature for a long time, the thermal resistance layer 310P shrinks due to thermal contraction of the thermal resistance layer 310P compared to before the temperature was increased (FIG. 3(A)). As a result, the ceramic substrate 100 is pulled inward as the thermal resistance layer 310P shrinks, causing the ceramic substrate 100 to warp. The stress relaxation layer 320 follows the warping and is distorted. The support portion 200 returns to its original size (FIG. 3(C)).

[0032] In contrast, in the electrostatic chuck 10 of the present embodiment, the thermal shrinkage rate of the thermal resistance layer 310 is 0.5% or less, so that it is possible to suppress the thermal shrinkage of the thermal resistance layer 310 after the temperature is increased or decreased. Therefore, even in the process after the temperature of the electrostatic chuck 10 is increased or decreased, it is possible to suppress the change in the flatness of the first surface S1 of the ceramic substrate 100. As a result, it is possible to make the in-plane temperature distribution of the first surface S1 of the ceramic substrate 100 approximately uniform, which can contribute to improving the yield in semiconductor manufacturing.

[0033] The heat shrinkage rate can be controlled by the following method. (Process Control) Increasing the temperature (heat plate and resin) during thermocompression reduces the thermal shrinkage rate. Increasing the pressure during heat bonding reduces the thermal shrinkage rate. Increasing the thickness of the thermal resistance layer reduces the thermal shrinkage rate. The thermal shrinkage rate will be smaller if slow cooling is performed during thermocompression. (Control from chemical structure) -Having a rigid ring structure like benzene or pyridine. -It has a linear para bond. For example, when polyimide is used as the material for the heat resistance layer, the thermal shrinkage of commonly available polyimides is adjusted by the chemical structure, so the process control is considered to have a large effect.

[0034] The elastic modulus (Young's modulus) of the thermal resistance layer 310 is not particularly limited, but is preferably 10 (GPa) or less. The force pulling the ceramic substrate after the temperature of the electrostatic chuck rises or falls can be calculated by multiplying the elastic modulus of the thermal resistance layer by the strain, and therefore increases in proportion to the elastic modulus and strain. In the electrostatic chuck, the thermal resistance layer is bonded to the ceramic substrate, and since the thermal contraction rate of the ceramic substrate is small, the contraction of the thermal resistance layer is prevented, and the force accompanying the thermal contraction of the thermal resistance layer is directly applied as a force pulling the ceramic substrate inward. If the elastic modulus of the thermal resistance layer 310 is made small, the force pulling the ceramic substrate 100 when the thermal contraction of the thermal resistance layer 310 occurs as the temperature of the electrostatic chuck rises or falls can be suppressed, and the warping of the first surface S1 of the ceramic substrate 100 can be suppressed.

[0035] The thermal expansion coefficient of the material forming the thermal resistance layer 310 is not particularly limited, but the difference between the thermal expansion coefficient of the material forming the ceramic substrate 100 and that of the ceramic is preferably 20×10 -6(1 / °C). If the thermal expansion coefficient of the material forming the thermal resistance layer 310 is significantly different from that of the ceramic of the ceramic substrate 100, residual stress remains in the thermal resistance layer every time the electrostatic chuck is operated. The details are as follows. When the electrostatic chuck is operated (for example, at 150°C), the expansion of the thermal resistance layer is prevented by the ceramic substrate, so the thermal resistance layer receives a force (compressive force) in the direction of contraction from the ceramic substrate, and an internal stress (compressive stress) in the direction of expansion is generated. The thermal resistance layer stores this as residual stress. After the electrostatic chuck is stopped (for example, after long-term use at 150°C), the thermal resistance layer tries to become smaller than before the electrostatic chuck was operated. If the thermal resistance layer stores residual stress, the thermal contraction coefficient becomes larger. However, since the thermal resistance layer is bonded to the ceramic substrate, the thermal resistance layer is prevented from shrinking by the ceramic substrate. Since the thermal resistance layer receives a force (tensile force) in the direction of expansion from the ceramic substrate, an internal stress (tensile stress) in the direction of contraction is generated. At this time, the thermal contraction rate is orders of magnitude larger than the thermal expansion rate, so the contraction force of the thermal resistance layer is very large. In addition, the internal stress is added each time the electrostatic chuck is operated, resulting in a large force. In this way, if the thermal expansion coefficient of the material forming the thermal resistance layer is significantly different from the thermal expansion coefficient of the ceramic of the ceramic substrate, residual stress may accumulate in the thermal resistance layer as the temperature of the electrostatic chuck repeatedly rises and falls, and the warping of the ceramic substrate may become large. In contrast, if the thermal expansion coefficient of the material forming the thermal resistance layer 310 is made close to the thermal expansion coefficient of the ceramic of the ceramic substrate 100, the residual stress in the thermal resistance layer 310 caused by the rise and fall of the temperature due to the operation of the electrostatic chuck 10 can be suppressed. As a result, the thermal contraction of the thermal resistance layer 310 can be suppressed, and the warping of the ceramic substrate 100 can be further suppressed.

[0036] The thermal expansion coefficient of the heat resistance layer can be reduced by adding functional groups such as benzene and pyridine to the resin structure, and can be adjusted by the amount added.

[0037] The distortion of the thermal resistance layer 310 is not particularly limited, but is preferably 10 μm or more. If the distortion is large, the thermal resistance layer 310 itself can easily deform, and therefore the stress relaxation property is improved. can be improved.

[0038] The thickness of the thermal resistance layer 310 is not particularly limited, but is preferably 0.1 (mm) or more. When the thermal resistance layer 310 is made thicker, the temperature rise and fall in the thermal resistance layer 310 proceeds slowly, so that the effect of temperature change can be suppressed and the thermal shrinkage rate can be reduced.

[0039] In the electrostatic chuck 10, it is preferable that no voids exist between the ceramic substrate 100 and the thermal resistance layer 310 after the ceramic substrate 100 is heated at 200° C. for 50 hours. This can further suppress peeling between the ceramic substrate 100 and the thermal resistance layer 310 that occurs when the temperature rises and falls due to the operation of the electrostatic chuck 10. The voids can be measured by ultrasonic flaw detection.

[0040] The thermal resistance layer 310 may be a single layer or may be a multi-layer. When the thermal resistance layer 310 is a multi-layer, the thermal contraction of the entire multi-layer structure is taken into consideration.

[0041] The stress relaxation layer 320 has a lower elastic modulus than the heat resistance layer 310. An adhesive sheet (including not only adhesives but also pressure sensitive adhesives and adhesive tapes) can be used as the stress relaxation layer 320. The material for forming the stress relaxation layer 320 is not particularly limited, but examples of the material that can be used include silicone, acrylic, polyimide, and the like. It is preferable to use silicone as the material, which is highly flexible and heat resistant, because peeling can be suppressed even when the electrostatic chuck 10 is used at high temperatures such as 250°C.

[0042] In general, in electrostatic chucks, the ceramic substrate is heated to a high temperature and the thermal expansion coefficient difference between the ceramic substrate and the support part is important for the heat resistance and flexibility of the joint. For example, polyimide is preferred as a material for the joint because of its high heat resistance, but it has a low flexibility and a high Young's modulus compared to silicone adhesives, so if polyimide is used alone as a joint, it may warp or peel off. Therefore, we considered using a combination of a highly heat-resistant and highly thermally resistant resin such as polyimide and a highly flexible silicone resin. However, since the electrostatic chuck is used for a long time at a high temperature of 150°C or more, polyimide will remain stretched, and thermal contraction will occur after long-term use. Therefore, we considered making the thermal expansion coefficient of the thermal resistance layer made of polyimide closer to that of the ceramic substrate, but even if the thermal expansion coefficients of the thermal resistance layer and the ceramic substrate were made closer, a shrinking force would be generated in the thermal resistance layer due to thermal contraction, which would result in a loss of flatness of the electrostatic chuck. In contrast, in the electrostatic chuck 10 of this embodiment, the thermal shrinkage rate of the thermal resistance layer 310 after heating at 350° C. for two hours is set to 0.5% or less, thereby making it possible to suppress warping of the ceramic substrate 100.

[0043] FIG. 4 is an explanatory diagram of a manufacturing method of the electrostatic chuck 10 according to the embodiment. First, the thermal resistance layer 310 is formed on the second surface S2, which is the surface opposite to the first surface S1 of the ceramic substrate 100 that serves as the wafer mounting surface. When the uncured thermal resistance layer 310U is in a sheet form, a sheet punched with an electrode pattern is placed. At this time, the thermal resistance layer may be formed as a laminate in which several sheets are stacked as necessary. Also, a layer other than the thermal resistance layer (e.g., metal foil) may be placed on the surface of the thermal resistance layer opposite to the ceramic substrate 100.

[0044] With the uncured thermal resistance layer 310U placed on the ceramic substrate 100, thermocompression bonding is performed in a vacuum state to bond the uncured thermal resistance layer 310U onto the ceramic substrate 100 (FIG. 4(A)). The pressure for thermocompression bonding is preferably 1 MPa to 7 MPa, and more preferably 2 to 5 MPa. The temperature for thermocompression bonding is preferably 100°C to 400°C, and more preferably 300°C to 400°C. The rate of temperature rise and fall during thermocompression bonding is preferably 20°C / min or less. The pressure rise rate is 0. It is preferable that the pressure is 5 MP or less, and when the pressure is reached, it is more preferable that the pressure is continued for 5 minutes or more. After the thermocompression bonding, the thermal resistance layer 310U is hardened in a state where it is integrated with the ceramic substrate 100.

[0045] When the material for forming the thermal resistance layer 310 is in a paste form, an uncured thermal resistance layer is formed on the ceramic substrate 100 by screen printing or the like. With the uncured thermal resistance layer placed on the ceramic substrate 100, thermocompression bonding is performed in a vacuum state to form an uncured thermal resistance layer on the ceramic substrate 100. In the case of a paste form, a resin wall for preventing outflow may be provided. The pressure for thermocompression bonding is preferably 0.1 MPa to 10 MPa, and more preferably 2 to 5 MPa. The temperature for thermocompression bonding is preferably 100°C to 400°C, and more preferably 300°C to 400°C. The rate of temperature rise and fall during thermocompression bonding is preferably 20°C / min or less. The rate of pressure rise is preferably 0.5 MPa / min or less, and when the pressure is reached, it is more preferable to continue applying pressure for 5 minutes or more. After thermocompression bonding, the thermal resistance layer is cured in a state integrated with the ceramic substrate.

[0046] The stress relief layer 320 is formed on the surface of the support part 200. When the uncured stress relief layer 320U is in a sheet shape, it is punched out with an electrode pattern, and then the uncured stress relief layer 320U is placed on the surface of the support part 200 (FIG. 4(B)). When the uncured stress relief layer is in a paste shape, it is formed on the surface of the support part 200 by a method such as screen printing.

[0047] The support part 200 on which the uncured stress relaxation layer 320U is formed and the ceramic substrate 100 on which the thermal resistance layer 310 is formed are bonded together in a vacuum (FIG. 4(C)), and integrated by heat curing to form an electrostatic chuck. Curing may be performed in a vacuum or in the atmosphere, and the temperature is preferably 100°C to 200°C.

[0048] Furthermore, when the thermal resistance layer and the stress relaxation layer are subjected to the same compression bonding temperature, the electrostatic chuck 10 may be fabricated by laminating an uncured thermal resistance layer and an uncured stress relaxation layer and performing a single compression bonding. That is, an uncured stress relaxation layer may be formed on the surface of an uncured thermal resistance layer formed on the ceramic substrate 100. Also, an uncured thermal resistance layer may be formed on the surface of an uncured stress relaxation layer formed on the support portion 200.

[0049] As described above, according to the electrostatic chuck 10 of this embodiment, the bonding portion 300 has the thermal resistance layer 310 made of a heat-resistant resin having higher heat resistance than the stress relaxation layer 320, and the stress relaxation layer 320 having a lower elastic modulus than the thermal resistance layer 310. Therefore, the stress relaxation layer 320 can reduce the difference in thermal expansion coefficient between the ceramic substrate 100 and the supporting portion 200, and the thermal resistance layer 310 can thermally protect the stress relaxation layer 320.

[0050] Furthermore, the thermal resistance layer 310 of this embodiment has a thermal shrinkage rate of 0.5% or less after heating at 350° C. for two hours, which can suppress thermal shrinkage of the thermal resistance layer 310 after the electrostatic chuck 10 is used at high temperatures (e.g., 150° C. or higher) for a long period of time (e.g., 1000 hours or more). Therefore, even in processes after the temperature of the electrostatic chuck 10 is increased or decreased, the change in flatness of the first surface S1 of the ceramic substrate 100 can be suppressed. As a result, the in-plane temperature distribution of the first surface S1 of the ceramic substrate 100 can be made substantially uniform, which can contribute to improving the yield in semiconductor manufacturing. EXAMPLES

[0051] The present invention will be explained more specifically with reference to examples. The electrostatic chuck 10 of the above embodiment was used in Examples 1 to 7 and Comparative Examples 1 to 6 to evaluate the warpage of the ceramic substrate. In Table 1, the amount of warpage of the ceramic substrate is indicated as ⊚ when it is less than 30 μm, ◯ when it is 30 μm or more and less than 68 μm, △ when it is 68 μm or more and less than 100 μm, and × when it is 100 μm or more. Even if the amount of warpage of the ceramic substrate is 100 μm or more, it is possible to hold the substrate. Although it is possible, anything over 100 μm is rated as ×, taking into account temperature distribution, etc.

[0052] Table 1 shows the conformity and evaluation results of the requirements (described later) for Examples 1 to 7 and Comparative Examples 1 to 6, and Table 2 shows the specifications and the amount of warping of the ceramic substrate. In Table 1, items that satisfy the requirements are marked with a circle, and items that do not satisfy the requirements are marked with an x.

[0053] [Table 1]

[0054] [Table 2]

[0055] 1. Manufacturing of the holding device The holding devices of the examples and comparative examples were manufactured by the following method.

[0056] Example 1 First, a ceramic green sheet mainly composed of alumina is prepared by a known method. A heater, an electrode for adsorption, vias, and air holes are prepared on the ceramic green sheet. After stacking and thermocompression bonding multiple ceramic green sheets, the sheets are fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. A polyimide film with a thickness of 25 to 30 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 2 MPa and 300°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 20°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was maintained for 10 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. An acrylic adhesive sheet was laminated in a vacuum on the support as a stress relaxation layer. The support with the stress relaxation layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and temporarily cured at a temperature of 100°C or less in a vacuum, and then completely cured at 150°C in air. This resulted in a holding device in which the ceramic substrate and support were bonded by the thermal resistance layer and the stress relaxation layer.

[0057] Example 2 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. A polyimide film with a thickness of 25 to 30 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 2 MPa and 300°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 20°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was maintained for 10 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. An acrylic / epoxy copolymer adhesive sheet was laminated in a vacuum to serve as a stress relief layer on the support section. The support section with the stress relief layer attached was then attached to the ceramic substrate with the heat resistance layer attached in a vacuum, and the resulting mixture was temporarily cured in a vacuum at a temperature of 100°C or less, after which it was completely cured in air at 150°C.

[0058] Example 3 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. A polyimide film with a thickness of 25 to 30 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 4 MPa and 340°C to obtain a bonded ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 20°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was held for 10 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0059] Example 4 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. An epoxy paste was printed on a ceramic substrate. The printing thickness was adjusted to the final target thickness. The composite, which was the ceramic substrate on which the epoxy paste was printed, was thermocompressed at 2 MPa and 150°C to obtain a bonded body of the ceramic substrate and the thermal resistance layer (epoxy film). The heating and cooling rates were 20°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was held for 10 minutes once it had been reached. The physical properties of the cured epoxy film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0060] Example 5 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 4 MPa and 340°C to obtain a bonded body of a ceramic substrate and a thermal resistance layer (polyimide film laminate). The heating and cooling rates were 10°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was maintained for 20 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0061] Example 6 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 4 MPa and 340°C to obtain a bonded body of a ceramic substrate and a thermal resistance layer (polyimide film laminate). The heating and cooling rates were 10°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was maintained for 20 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0062] Example 7 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 6.0 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 5 MPa and 360°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 10°C / min, and the pressure rise rate was 0.5 MPa / min. The pressure was held for 20 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0063] Comparative Example 1 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 0.5 MPa and 270°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 25°C / min, and the pressure rise rate was 1 MPa / min. The pressure was held for 5 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. An acrylic adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing in a vacuum at a temperature of 100°C or less, it was completely cured at 150°C in air.

[0064] Comparative Example 2 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. An epoxy paste was printed on a ceramic substrate. The printing thickness was adjusted to the final target thickness. The composite, which was the ceramic substrate on which the epoxy paste was printed, was thermocompressed at 0.5 MPa and 80°C to obtain a bonded body of the ceramic substrate and the thermal resistance layer (epoxy film). The heating and cooling rates were 25°C / min, and the pressure rise rate was 1 MPa / min. The pressure was maintained for 5 minutes once it had been reached. The physical properties of the cured epoxy film are shown in Table 2. An acrylic / epoxy copolymer adhesive sheet was laminated in a vacuum to serve as a stress relief layer on the support section. The support section with the stress relief layer attached was then attached to the ceramic substrate with the heat resistance layer attached in a vacuum, and the resulting mixture was temporarily cured at a temperature of 100°C or less in a vacuum, after which it was completely cured at 150°C in air.

[0065] Comparative Example 3 A ceramic green sheet mainly composed of alumina is prepared in the same manner as in Example 1. A heater, an electrode for adsorption, a via hole, and a vent hole are formed on the ceramic green sheet, and multiple cells are formed. The laminated green sheets were laminated and thermocompression bonded, and then fired at 1400° C. to 1600° C. in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 0.5 MPa and 270°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 25°C / min, and the pressure rise rate was 1 MPa / min. The pressure was held for 3 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0066] Comparative Example 4 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. A polyimide film with a thickness of 50 to 60 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 0.5 MPa and 250°C to obtain a bonded body of the ceramic substrate and thermal resistance layer (polyimide film laminate). The heating and cooling rates were 25°C / min, and the pressure rise rate was 1 MPa / min. The pressure was held for 3 minutes after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0067] Comparative Example 5 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 4.0 mm. A polyimide film with a thickness of 25 to 30 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 0.5 MPa and 200°C to obtain a bonded body of a ceramic substrate and a thermal resistance layer (polyimide film laminate). The heating and cooling rates were 30°C / min, and the pressure rise rate was 1 MPa / min. The pressure was held for 1 minute after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0068] Comparative Example 6 A ceramic green sheet containing alumina as a main component was prepared in the same manner as in Example 1. A heater, an electrode for adsorption, vias, and air holes were prepared on the ceramic green sheet, and a plurality of ceramic green sheets were laminated and thermocompression bonded, and then fired at 1400°C to 1600°C in a reducing atmosphere to obtain a ceramic substrate with a thickness of 1.8 mm. A polyimide film with a thickness of 25 to 30 μm was laminated onto a ceramic substrate. The thickness and number of films were adjusted to achieve the final target thickness. The polyimide film laminate was thermocompression bonded to the ceramic substrate at 0.5 MPa and 200°C to obtain a bonded body of the ceramic substrate and thermal resistance layer. The heating and cooling rates were 30°C / min, and the pressure rise rate was 1 MPa / min. The pressure was held for 1 minute after it was reached. The physical properties of the cured polyimide film are shown in Table 2. A silicone adhesive sheet was laminated in a vacuum on the support as a stress relief layer. The support with the stress relief layer attached and the ceramic substrate with the thermal resistance layer attached were attached in a vacuum, and after provisional curing at a temperature of 100°C or less in a vacuum, they were completely cured at 150°C in air.

[0069] 2. Measurement and evaluation methods for each physical property The physical properties of the ceramic substrate and the thermal resistance layer in the holding devices of the examples and comparative examples were measured, and the holding devices were evaluated, by the methods described below.

[0070] Heat shrinkage rate The thermal shrinkage of the thermal resistance layer was measured in accordance with JIS K 7133. The thermal resistance layer was formed on a Teflon (registered trademark) film so as to have a thickness suitable for mounting on a holding device, and was cured by thermocompression bonding under the same conditions as in each embodiment. The obtained thermal resistance layer was pretreated and cut out, and then heat-treated at 350°C for 2 hours. The thermal shrinkage was calculated from the sample length L0 before heat treatment and the sample length L after heat treatment by the formula L-L0 / L0×100. Here, a negative value indicates a thermal shrinkage.

[0071] Thermal expansion coefficient The thermal expansion coefficients of the ceramic substrate and the thermal resistance layer were measured by thermomechanical analysis (Rigaku TMA8311). The thermal resistance layer was cut from a sample prepared for thermal contraction measurement. The ceramic substrate was cut from the holding device.

[0072] · Elastic modulus (Young's modulus) The Young's modulus of the thermal resistance layer was calculated from the slope of the stress-strain curve in the elastic region by performing a tensile test on the sample using a known method. In the examples, an autograph AGS-5kNX made by Shimadzu Corporation was used. The sample was cut out and used to measure the thermal shrinkage rate.

[0073] Thickness The thicknesses of the thermal resistance layer and the ceramic substrate were obtained by cutting the holding device vertically and measuring the cross section with an optical microscope.

[0074] ·distortion FIG. 5 is an explanatory diagram of a method for measuring distortion. A thermal resistance layer 310T was formed on the surface of an aluminum plate J to a thickness suitable for mounting on a holding device, sandwiched between aluminum plates J of the same size, and hardened by thermocompression bonding under the same conditions as in each of the examples and comparative examples. Both ends of the aluminum plate J were pulled and the strain was measured. The strain was measured by a tensile test using a known tensile tester (Shimadzu Corporation Autograph AGS-5kNX). In the tensile test, the strain was measured when the shear stress reached its maximum.

[0075] ·Void The voids in the support device can be measured by ultrasonic testing. The support device was subjected to ultrasonic testing before and after heat treatment to check for the occurrence of voids. In this example, the UVS- 101 was used for the measurement.

[0076] Warpage (evaluation) Electricity was applied to the heater electrodes so that the ceramic substrate surface reached 200°C, and 30°C cooling water was run through the support section to cool it, and the substrate was held in this state for 5 hours. The current was turned off, the substrate was returned to room temperature, and the warpage of the ceramic substrate surface was measured. A laser-type 3D measuring device (NEXIV) was used to measure the warpage by measuring 900 points at 1cm intervals on the ceramic substrate surface. The difference between the maximum and minimum values ​​at all measurement points was taken as the warpage.

[0077] 3. Evaluation results As shown in Tables 1 and 2, in Examples 1 to 7, the amount of warping of the ceramic substrate was suppressed compared to Comparative Examples 1 to 6, and the amount of warping was 100 μm or less.

[0078] Table 1 shows the suitability of the examples and comparative examples for the following requirements 1 to 7. In the examples and comparative examples, the heat resistance layer is made of a heat-resistant resin that has higher heat resistance than the stress relaxation layer. [1] The thermal resistance layer has a thermal shrinkage rate of 0.5% or less after heating at 350°C for 2 hours. [2] The elastic modulus of the thermal resistance layer is 10 (GPa) or less. [3] The difference between the thermal expansion coefficient of the material forming the thermal resistance layer and the thermal expansion coefficient of the ceramic of the ceramic substrate is 20 × 10 -6 (1 / ℃). [4] The distortion of the heat resistance layer is 10 μm or more. [5] The thickness of the thermal resistance layer is 0.1 mm or more. [6] The thickness of the ceramic substrate is 2 mm or more. [7] After the ceramic substrate is heated at 200° C. for 50 hours, no gap exists between the ceramic substrate and the thermal resistance layer.

[0079] Example 1 satisfies the above requirements [1] and [7]. Example 2 satisfies the above requirements [1] and [7], as well as requirement [2]. Example 3 satisfies the above requirements [1] to [2] and requirement [7], as well as requirement [3]. Example 4 satisfies the above requirements [1] to [3] and requirement [7], as well as requirement [4]. The fifth embodiment satisfies the above requirements [1] to [4] and requirement [7], as well as requirement [5]. Example 6 satisfies the above requirements [1] to [5] and requirement [7], as well as requirement [6], and therefore satisfies all of the above requirements [1] to [7].

[0080] In contrast, Comparative Examples 1 to 6 do not satisfy the above requirement [1]. Comparative Example 4 also does not satisfy requirement [4], Comparative Example 5 also does not satisfy requirement [5], and Comparative Example 6 also does not satisfy requirement [6]. That is, Comparative Example 6 does not satisfy all the requirements.

[0081] As described above, Examples 1 to 7 satisfy requirement [1], the thermal resistance layer is made of a heat-resistant resin having higher heat resistance than the stress relaxation layer, and the thermal shrinkage rate after heating at 350°C for 2 hours is 0.5% or less. Therefore, when the ceramic substrate of the holding device is heated and held, and then cooled, the force that causes the thermal resistance layer to shrink from its original size can be suppressed, and the change in flatness (warping) of the ceramic substrate can be suppressed compared to Comparative Examples 1 to 6. Comparative Example 1 satisfies all requirements except requirement [1], but the amount of warping of the ceramic substrate is 100 μm or more. From this, it is considered that requirement [1] has the greatest effect on the warping of the ceramic substrate.

[0082] Example 2 further satisfies requirement [2], and the elastic modulus (Young's modulus) of the thermal resistance layer is 10 (GPa) or less, which is smaller than that of Example 1. Since the elastic modulus of the thermal resistance layer of Example 2 is smaller than that of Example 1, it is possible to suppress the force pulling the ceramic substrate 100 due to the thermal contraction of the thermal resistance layer 310 after the temperature of the holding device is increased or decreased, and it is possible to suppress the warping of the ceramic substrate 100 more than in Example 1.

[0083] Example 3 further satisfies requirement [3], and the difference between the thermal expansion coefficient of the material forming the thermal resistance layer and the thermal expansion coefficient of the ceramic of the ceramic substrate 100 is smaller than those of Examples 1 and 2, and is 20×10-6 Therefore, the residual stress in the thermal resistance layer caused by the rise and fall of the temperature of the holding device can be suppressed more than in Examples 1 and 2, and the thermal contraction of the thermal resistance layer can be suppressed, so that the warpage of the ceramic substrate can be suppressed more than in Examples 1 and 2.

[0084] Example 4 further satisfies requirement [4], and the distortion of the thermal resistance layer is 10 (μm) or more, which is larger than that of Examples 1 to 3. Therefore, the thermal resistance layer of Example 4 is more easily deformed than the thermal resistance layers of Examples 1 to 3, and the stress relaxation property of the thermal resistance layer is higher than that of Examples 1 to 3, so that the warping of the ceramic substrate can be suppressed more than that of Examples 1 to 3.

[0085] Example 5 further satisfies requirement [5], and the thickness of the thermal resistance layer 310 is 0.1 (mm) or more, which is thicker than Examples 1 to 4. Since the thickness of the thermal resistance layer is thicker than Examples 1 to 4, the temperature rise and fall in the thermal resistance layer proceeds more slowly than in Examples 1 to 4. Therefore, it is less susceptible to the effect of temperature changes than Examples 1 to 4, the thermal shrinkage rate can be reduced, and the warping of the ceramic substrate can be suppressed more than in Examples 1 to 4.

[0086] Example 6 further satisfies requirement [6], and the thickness of the ceramic substrate is 4.0 mm, which is 2 mm or more, which is thicker than Examples 1 to 5. In this way, the ceramic substrate itself is less likely to warp, and therefore warping of the ceramic substrate can be suppressed more than in Examples 1 to 5.

[0087] In Example 7, the ceramic substrate had an even greater thickness of 6.0 mm. Therefore, the ceramic substrate itself was even less susceptible to warping, and warping of the ceramic substrate was more suppressed than in Example 6.

[0088] Moreover, all of Examples 1 to 7 satisfied the requirement [7], and therefore it was possible to suppress peeling between the ceramic substrate and the thermal resistance layer caused by the rise and fall of the temperature of the holding device.

[0089] In contrast, Comparative Examples 1 to 6 did not satisfy the above requirement [1], and the amount of warping of the ceramic substrate was 100 μm or more.

[0090] In the examples, polyimide or epoxy is used as the heat resistance layer, but when PEEK (Poly Ether Ether Ketone), polybenzimidazole, etc. are used, the same effect against the warping of the ceramic substrate can be obtained by making the physical properties (thermal shrinkage rate, etc.) the same as those in the above examples. This is because the physical properties such as the thermal shrinkage rate and Young's modulus have a dominant effect on the warping of the ceramic substrate, rather than the type of resin.

[0091] <Modifications of this embodiment> The present invention is not limited to the above-described embodiment, and can be embodied in various forms without departing from the spirit and scope of the invention. For example, the following modifications are also possible.

[0092] In the above embodiment, an example is shown in which an object is held on the first surface S1 of the ceramic substrate 100. However, a configuration may also be used in which another ceramic substrate is bonded on top of the ceramic substrate 100 and the object is held on top of that.

[0093] In the above embodiment, an electrostatic chuck is used as the holding device, but the holding device is not limited to the electrostatic chuck. For example, CVD, PVD, PLD (Pulsed Laser The present invention can be configured as a heater device, susceptor, or mounting table for a vacuum device such as a vacuum deposition device.

[0094] In the above embodiment, the holding device is provided with a stack of plate-like members having a substantially circular planar shape, but the planar shape is not limited to that in the above embodiment. For example, the holding device may be rectangular, polygonal, or the like.

[0095] The bonding layer may further include another layer, such as a metal layer, between the thermal resistance layer and the stress relaxation layer. Copper (Cu) foil, aluminum (Al) foil, stainless steel foil, etc. may be disposed between the thermal resistance layer and the stress relaxation layer. When the thermal resistance layer and the stress relaxation layer do not fit well together, the bonding between the thermal resistance layer and the stress relaxation layer can be improved by using the above-mentioned metal foil as a bonding auxiliary layer.

[0096] The present invention has been described above based on the embodiments and modifications, but the above-mentioned embodiments are intended to facilitate understanding of the present invention and do not limit the present invention. The present invention may be modified or improved without departing from the spirit and scope of the claims, and the present invention includes equivalents thereof. Furthermore, if a technical feature is not described as essential in this specification, it may be deleted as appropriate. [Explanation of symbols]

[0097] 10, 10P...Electrostatic chuck 100...Ceramics substrate 116...Adsorption electrode 118…Heater 200...Support part 210... Coolant flow path 300, 300P…Joint part 310, 310P, 310T, 310U...thermal resistance layer 320, 320U...Stress relief layer J…Aluminum plate S1...Side 1 S2…Second side W…wafer

Claims

1. A holding device for holding an object, a ceramic substrate containing alumina as a main component and having a first surface and a second surface opposite to the first surface; a support portion disposed on the ceramic substrate so as to face the second surface, the support portion being mainly composed of a material having a thermal expansion coefficient different from that of the ceramic of the ceramic substrate; a joining portion disposed between the ceramic substrate and the support portion and joining the ceramic substrate and the support portion; Equipped with The joint is a thermal resistance layer bonded to the second surface of the ceramic substrate; a stress relaxation layer having a modulus of elasticity lower than that of the thermal resistance layer and joined to the support portion; The thermal resistance layer is The stress relaxation layer is made of a heat-resistant resin having a higher heat resistance than the stress relaxation layer, and has a thermal shrinkage rate of 0.41% or less after heating at 350°C for 2 hours. holding device.

2. 2. The holding device according to claim 1, The thermal resistance layer has an elastic modulus of 10 GPa or less. holding device.

3. A holding device according to claim 1 or 2, The difference between the thermal expansion coefficient of the material forming the thermal resistance layer and the thermal expansion coefficient of the ceramic of the ceramic substrate is 20×10 -6 1 / °C or less, holding device.

4. A holding device according to any one of claims 1 to 3, The distortion of the thermal resistance layer is 10 μm or more. holding device.

5. A holding device according to any one of claims 1 to 4, The thickness of the thermal resistance layer is 0.1 mm or more. holding device.

6. A holding device according to any one of claims 1 to 5, The ceramic substrate has a thickness of 2 mm or more. holding device.

7. A holding device according to any one of claims 1 to 6, After the ceramic substrate is heated at 200° C. for 50 hours, no gap exists between the ceramic substrate and the thermal resistance layer. holding device.

Citation Information

Patent Citations

  • Construction of paddy footpath

    JP1984048513A

  • Wafer-supporting member, method for producing the same, and electrostatic chuck using the same

    WO2009107701A1

  • Wafer holding stage and method for producing same

    WO2016035878A1

  • Wafer holding stage

    WO2019176544A1