Wafer back grinding method and electronic device manufacturing method

By forming a protective layer and adhering it to a support via an adhesive layer, the method addresses unevenness on the wafer surface, ensuring stable processing and improved handling, thus enhancing the quality and productivity of electronic devices.

JP7551787B2Active Publication Date: 2024-09-17MITSUI CHEM ICT MATERIA INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022576717
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-21
Filing Date
2022-01-19
Publication Date
2024-09-17
Estimated Expiration
2042-01-19

AI Technical Summary

Technical Problem

Existing wafer back grinding methods struggle to suppress the effects of unevenness on the wafer surface, leading to difficulties in handling and maintaining uniform thickness, which affects the quality and characteristics of electronic devices like power devices.

Method used

A method involving the formation of a protective layer on the wafer surface, followed by flattening the non-contact surface of the protective layer, and adhering it to a support via an adhesive layer to stabilize the wafer during grinding, thereby preventing unevenness transfer to the backside.

Benefits of technology

This method effectively suppresses the influence of unevenness, improves handling properties, and ensures stable processing, reducing damage to circuits and enhancing the quality and productivity of electronic devices by maintaining uniform thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551787000001
    Figure 0007551787000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a rear surface grinding method for a wafer, in which the rear surface of a wafer is ground such that the impact of recesses and protrusions on the front surface of the wafer can be suppressed and in which handling after wafer thinning is improved. The present problem is solved by a rear surface grinding method for a wafer having recesses and protrusions on the front surface thereof, the rear surface grinding method for a wafer being characterized by comprising, prior to rear surface grinding of the wafer, a step (1) for forming a protective layer on the front surface of the wafer, a step (2) for flattening the surface of the protective layer that is not in contact with the wafer, and a step (3) for adhering a support to the surface of the protective layer that is not in contact with the wafer, with an adhesive layer therebetween.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for grinding the backside of a wafer, among methods for thinning a wafer having an uneven surface, and more specifically, to a method for grinding the backside of a wafer in which the surface of the wafer is protected by a protective layer and then the surface of the protective layer that is not in contact with the wafer is flattened, thereby suppressing the effect of the unevenness on the surface of the wafer, and which improves handleability in a wide range of processing processes after the wafer is thinned. [Background technology]

[0002] For the purpose of highly integrated semiconductor devices or for manufacturing high-performance semiconductor devices, back grinding is widely performed in which a wafer on which a circuit is formed is ground thinly and uniformly. However, in the manufacturing process of electronic devices such as semiconductor devices, circuits are formed on the surface of a semiconductor wafer such as silicon or gallium arsenide in the so-called front-end process, or bump electrodes may cause unevenness on the surface of the wafer. Among such electronic devices, power devices used in power converters such as inverters and converters have unevenness on the surface of the wafer due to their characteristics, structure, manufacturing process, and other reasons. If a protective layer such as a protective adhesive tape is created in the so-called back-end process and the back grinding is performed as is, the unevenness on the surface of the wafer is transferred to the back side of the wafer, and the unevenness is reflected in the finished thickness of the wafer, which affects the device characteristics, especially in power devices.

[0003] As a method for grinding the backside of a wafer that suppresses the effect of unevenness on the surface of the wafer, a method is known in which the wafer is supported by an adhesive tape, and then the base material of the tape is flattened by a surface planer to make the finished thickness of the backside of the wafer uniform (Patent Document 1). However, although this method can suppress the variation in the finished thickness of the wafer, it has a problem that the handling properties, such as the transportability, of the wafer after thinning become difficult.

[0004] On the other hand, a method for improving the handleability of thinned wafers is known in which the wafer and the supporting substrate are temporarily fixed with a protective layer to facilitate handling (Patent Document 2). However, with this method, there are cases where the unevenness of the wafer surface, which causes unevenness in the application of the protective layer, etc., makes it difficult to sufficiently suppress the variation in the finished thickness of the wafer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-43931 A [Patent Document 2] JP 2004-64040 A Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above technical background, an object of the present invention is to provide a method for grinding the back surface of a wafer, which can suppress the effects of unevenness on the surface of the wafer and improve the handleability of the wafer after thinning. [Means for solving the problem]

[0007] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by protecting the surface of the wafer with a protective layer prior to grinding the back surface of the wafer, then flattening the surface of the protective layer that is not in contact with the wafer, and adhering the flattened surface of the protective layer that is not in contact with the wafer to a support via an adhesive layer, thereby completing the present invention. That is, the present invention provides: [1] A method for grinding the backside of a wafer having an uneven surface, comprising the steps of: (1) forming a protective layer on the surface of the wafer; (2) planarizing a surface of the protective layer that is not in contact with the wafer; and (3) a step of adhering a surface of the protective layer not in contact with the wafer to a support via an adhesive layer; A method for grinding the back surface of a wafer, comprising: Regarding.

[0008] Hereinafter, [2] to

[15] are each a preferred aspect or embodiment of the present invention. [2] The method for grinding the backside of a wafer according to [1], wherein the protective layer is a protective adhesive tape. [3] The method for grinding the backside of a wafer according to [2], wherein a base layer of the protective adhesive tape contains at least one resin selected from the group consisting of PET, PEN, PBT, LCP, PI, PA, PEEK and PPS. [4] The method for grinding the backside of a wafer according to any one of [1] to [3], wherein the wafer having an uneven surface is a wafer having unevenness due to at least one of electrodes, circuit patterns, polyimide, defect marks, or bumps formed on the surface. [5] The method for grinding a backside of a wafer according to any one of [1] to [4], wherein the planarizing step is a step of planarizing by cutting, grinding, or polishing. [6] The method for grinding the back surface of a wafer according to [5], wherein the cutting is performed by a cutting tool. [7] The method for grinding a wafer backside according to any one of [1] to [6], wherein the adhesive layer is a liquid adhesive or an adhesive tape. [8] The method for grinding a wafer backside according to any one of [1] to [7], wherein the support is made of glass, silicon, ceramic, metal, resin or a composite material thereof. [9] The method for grinding the backside of a wafer according to any one of [1] to [8], further comprising the step of forming the adhesive layer on a surface of the planarized protective layer not in contact with the wafer, on a surface of the support, or on both, after the step (2) and before the step (3).

[10] The method for grinding a wafer backside according to any one of [1] to [9], further comprising a backside treatment step of the wafer after grinding the backside of the wafer.

[11] The method for grinding the back surface of a wafer according to

[10] , wherein the back surface treatment process of the wafer includes at least one of etching, electrode formation, ion implantation, and annealing.

[12] The method for grinding a wafer backside according to any one of [1] to

[11] , wherein the thickness of the wafer after backside grinding is 200 μm or less.

[13] A method for producing an electronic device, the method including the method for grinding the backside of a wafer according to any one of [1] to

[12] being included in the production process.

[14] The method for producing an electronic device according to

[13] , wherein the electronic device is a device having an electrode also on the back surface side.

[15] The method for producing an electronic device according to

[14] , wherein the electronic device is a power device. Effect of the Invention

[0009] According to the method for grinding the backside of a wafer of the present invention, it is possible to suppress the effect of unevenness on the surface of the wafer when grinding the backside of the wafer, and since the handleability of the wafer after thinning is improved, the wafer can be stably processed in a wide range of processing steps after thinning. This prevents damage to circuits, etc. formed on the wafer, suppresses unintended effects on the characteristics of electronic devices such as semiconductor devices, and makes it possible to carry out multiple and / or wide range of processes on the wafer with high productivity and yield, greatly contributing to improving the productivity of electronic devices such as semiconductor devices. [Brief description of the drawings]

[0010] [Figure 1]1 is a schematic diagram illustrating a process in one embodiment of the present invention. (a) shows a wafer 1 whose back surface 12 is ground in the present invention. (b) shows a wafer 1 in which a protective adhesive tape 3 is attached to the front surface 11 of the wafer 1 in step (1) using the protective adhesive tape 3 as a protective layer. (c) shows a wafer 1 in which a base layer 31 of the protective adhesive tape 3 is flattened in step (2). (d) shows a wafer 1 in which a tacky adhesive layer 4 is formed on the flattened base layer 33 of the protective adhesive tape 3 obtained in step (2). (e) shows a wafer 1 in which a support 5 and the flattened base layer 33 of the protective adhesive tape 3 are bonded to each other via the tacky adhesive layer 4 in step (3). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention relates to A method for grinding the backside of a wafer having an uneven surface, comprising the steps of: (1) forming a protective layer on the surface of the wafer; (2) planarizing a surface of the protective layer that is not in contact with the wafer; and (3) a step of adhering a surface of the protective layer not in contact with the wafer to a support via an adhesive layer; A method for grinding the back surface of a wafer, comprising: It is.

[0012] Wafer with uneven surface The wafer that is back-ground by the method of the present invention has unevenness on its surface. The unevenness on the wafer surface may be due to, for example, electrodes, circuit patterns, thick polyimide (5 to 20 μm) that is a protective film, defective marks (5 to 100 μm) for identifying defective chips, gold bumps (10 to 100 μm) for bump bonding instead of wire bonding, solder bumps (50 to 300 μm), etc., and the height of the unevenness may be 5 to 300 μm.

[0013] The wafer material is a material that is usually used in the manufacture of electronic devices, can form electronic circuits, etc., and is expected to be thinned as a substrate to be ground. Examples include, but are not limited to, silicon wafers, compound semiconductor wafers such as SiC, AlSb, AlAs, AlN, AlP, BN, BP, BAs, GaSb, GaAs, GaN, GaP, InSb, InAs, InN, or InP, quartz wafers, sapphire, or glass. The silicon wafer or compound semiconductor wafer may be doped.

[0014] In particular, wafers having an uneven surface include wafers for power devices used in power converters such as inverters and converters, which are electronic devices.

[0015] Process (1) Step (1) is a step of forming a protective layer on the surface of a wafer.

[0016] protective layer The protective layer is intended to prevent the electronic circuits, etc. on the front surface of the wafer from being damaged or contaminated by grinding debris, grinding water, etc., during grinding of the back surface of the wafer. In order to grind the back surface of the wafer, in-feed grinding is generally adopted, in which the wafer is attracted to and held on a vacuum chuck table, and a grinding tool such as a grinding wheel is pressed against the back surface of the wafer while rotating the chuck table to rotate the wafer, but when grinding the back surface of the wafer in this manner, the front surface of the wafer is covered with a protective layer to prevent the wafer from coming into direct contact with the holding surface of the chuck table and damaging the electronic circuits, etc., on the front surface of the wafer. In one embodiment, the protective layer may be, for example, a protective adhesive tape or a protective resin layer, and preferably, the protective layer is a protective adhesive tape.

[0017] The protective layer in the present invention has a thickness appropriate for protecting the surface of the wafer and at the same time has a thickness that can withstand planarization in the step (2) described below, that is, a thickness that has a margin relative to the required cutting thickness.

[0018] It is preferable to use a protective adhesive tape as the protective layer. When the protective layer is a protective adhesive tape, step (1) is a step of attaching the protective adhesive tape to the surface of the wafer. The protective adhesive tape may be attached to the surface of the wafer by a conventionally known method, but is preferably attached using an automatic attachment device, and it is preferable to appropriately adjust the pressure, temperature, time, etc. according to the material and type of the wafer and the protective adhesive tape.

[0019] Protective Adhesive Tape The protective adhesive tape as a preferred protective layer used in the method of the present invention is not particularly limited as long as it has adhesion sufficient to withstand planarization in step (2) described below, cutting processability, adhesion sufficient to withstand back grinding described below, chemical resistance and heat resistance sufficient to withstand the back treatment step described below, and finally, can be removed from the wafer with reduced contamination of the wafer surface, and can be preferably selected and used from those that are generally used as protective adhesive tapes for back grinding of semiconductor wafers.

[0020] Examples of materials for the base layer of protective adhesive tapes include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), very low density polyethylene (VLDPE), linear low density polyethylene (L-LDPE), random copolymer polypropylene (random PP), block copolymer polypropylene (block PP), homopolypropylene (homo PP), polybutene (PB), polymethylpentene (PMP), ethylene-vinyl acetate copolymer (EVA), ethylene acrylic acid copolymer, ethylene methacrylic acid copolymer and their metal cross-linked bodies (ionomers), etc. Examples of the substrate include polyolefins, polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and liquid crystal polymer (LCP), and further include polyurethane (PU), polycarbonate (PC), polyimide (PI), polyether ether ketone (PEEK), polyetherimide (PEI), polyamide (PA), wholly aromatic polyamide, polyphenyl sulfide (PPS), fluororesin, polyvinyl chloride, polyvinylidene chloride, and cellulose-based resin. The substrate may be a single layer substrate made of the resin alone, or may be a blend of a plurality of the resins or a multi-layer substrate made of different resins. From the viewpoint of heat resistance, a substrate having a melting point or glass transition temperature of 100° C. or higher is preferred, and a substrate having a melting point or glass transition temperature of 150° C. or higher is particularly preferred. In one embodiment, it is particularly preferable that the base layer of the protective adhesive tape contains PET, PEN, PBT, LCP, PI, PA, PEEK, or PPS, taking the following conditions into consideration.

[0021] The base layer of the protective adhesive tape must be able to withstand flattening, and therefore the thickness before flattening is preferably 10 to 1000 μm, and particularly preferably 25 to 500 μm. If the thickness of the base layer of the protective adhesive tape is thin, the protective layer is thin, and the amount that can be ground during flattening is limited, so the effect of flattening the protective layer tends to be small. Therefore, when the uneven shape on the wafer surface is large, the wafer thickness accuracy after grinding may decrease due to the influence. On the other hand, if the protective layer before flattening is thick, the rigidity of the protective layer is high, the processability in the tape shape decreases, and the cutability when cutting the tape into the wafer shape tends to decrease. In addition, due to the rigidity, the protective adhesive tape is difficult to deform, and the peelability in the protective layer removal step after grinding the back surface of the wafer tends to decrease.

[0022] The base layer of the protective tape has a tensile modulus of elasticity of 1×10 at 23°C according to JIS K7113. 7 The tensile modulus is preferably 5×10 Pa or more. 7 A modulus of tensile elasticity of 1×10 Pa or more is more preferable. When the modulus of tensile elasticity is low, the flattening of the base layer of the protective tape tends to be affected. Specifically, even after flattening, the thickness accuracy of the wafer after back grinding tends to decrease due to the influence of the unevenness of the wafer surface. On the other hand, the modulus of tensile elasticity is set to 1×10 Pa or more from the viewpoints of the workability, cuttability, bendability, etc. of the base layer. 10 Pa or less is preferable, and 6×10 9 Pa or less is more preferable.

[0023] The adhesive layer of the protective adhesive tape can be a commonly used pressure-sensitive adhesive, a curing adhesive, etc. In addition, the adhesive layer may generally be a single layer or multiple layers, and from the viewpoint of conforming to the unevenness of the wafer surface, it may be a multi-layer structure in which a flexible intermediate layer and a low-contamination adhesive layer are laminated.

[0024] Examples of the pressure-sensitive adhesive include adhesives such as acrylic adhesives, rubber adhesives, silicone adhesives, etc. Acrylic adhesives having an acrylic polymer as a base polymer are preferred from the standpoint of adhesiveness to a semiconductor wafer or a base layer, and cleaning and washing properties of the wafer with ultrapure water or an organic solvent such as alcohol after peeling off the protective adhesive tape.

[0025] The curable adhesive may be a photocurable adhesive that is crosslinked and cured by irradiation with light, or a thermosetting adhesive that is crosslinked and cured by heating. The photocurable adhesive may be, for example, a photocurable adhesive that contains a polymerizable polymer as a main component and a photopolymerization initiator. The thermosetting adhesive may be, for example, a thermosetting adhesive that contains a polymerizable polymer as a main component and a thermal polymerization initiator.

[0026] If the adhesive layer of the protective adhesive tape has a small peeling adhesive strength, the adhesive strength to the wafer is insufficient against the shear force when the base layer of the protective adhesive tape is flattened, and the protective adhesive tape peels off from the wafer. On the other hand, if the peeling adhesive strength is large, it may be difficult to peel the protective adhesive tape from the wafer. Therefore, from the viewpoint of the final peeling from the wafer, the thickness is preferably 5 to 500 μm, and more preferably 10 to 100 μm. Except for the case where the adherend is a silicon mirror wafer, the 180° peeling adhesive strength (peeling speed 300 mm / min) according to JIS Z0237 (2009) is preferably 0.3 to 10 N / 25 mm, and more preferably 0.5 to 7 N / 25 mm. It is appropriately adjusted within this range according to the process.

[0027] A protective resin layer can also be used as the protective layer. When the protective layer is a protective resin layer, the protective resin layer is formed by applying a raw material resin dissolved in a solvent or a liquid raw material resin itself (hereinafter referred to as a precursor resin liquid) by a known method such as spin coating, and then curing the applied layer by light irradiation, heating, drying, etc., to function as a solid protective layer. The protective layer may be formed of multiple layers.

[0028] Protective resin layer The protective resin layer that can be used as the protective layer is not particularly limited as long as it has adhesiveness and cutting processability that can withstand planarization in the step (2) described later, adhesiveness that can withstand back grinding described later, chemical resistance and heat resistance that can withstand the back surface treatment step described later, and can finally be removed from the wafer in a state where contamination of the wafer surface is reduced, and can be preferably selected from known materials that temporarily fix device wafers to supports and can be used. Examples of the precursor resin liquid include a rubber-based resin liquid in which rubber, elastomer, etc. are dissolved in a solvent, a one-liquid thermosetting resin liquid based on epoxy, urethane, etc., a two-liquid mixed reaction type resin liquid based on epoxy, urethane, acrylic, etc., a hot melt adhesive, an ultraviolet (UV) or electron beam curable resin liquid based on acrylic, epoxy, etc., and a water-dispersed resin liquid. A UV-curable resin liquid in which a photopolymerization initiator and, in some cases, an additive are added to an oligomer having a polymerizable vinyl group such as urethane acrylate, epoxy acrylate, or polyester acrylate, and / or an acrylic or methacrylic monomer is preferably used. The additives include a thickener, a plasticizer, a dispersant, a filler, a flame retardant, and a heat aging inhibitor, etc. The protective resin layer may be formed of a plurality of layers.

[0029] Process (2) The step (2) is a step of planarizing the surface of the protective layer that is not in contact with the wafer.

[0030] For example, when the protective layer is a protective adhesive tape, this is a step of planarizing the base layer of the protective adhesive tape. In step (1), when the protective adhesive tape is applied to the surface of the wafer, the unevenness of the surface of the wafer is transferred to the base layer of the protective adhesive tape, and if back grinding is performed as is, the force of the back grinder is not applied uniformly, and the unevenness of the base layer of the protective adhesive tape is reflected, and the unevenness is also transferred to the back surface of the wafer. Even when the protective layer is formed from a protective resin layer, there are cases where sufficient planarization cannot be achieved by simple spin coating, and unevenness still occurs on the surface of the protective layer, which may be transferred to the back surface of the wafer. By flattening the base layer of the protective adhesive tape to which the irregularities have been transferred in this manner prior to backgrinding, the force of the back grinder can be applied evenly, preventing the irregularities from being transferred to the back surface of the wafer.

[0031] The planarization is not particularly limited as long as it can prevent the transfer of irregularities to the rear surface of the wafer. For example, it is preferable that the following conditions are satisfied. The difference between the concave and convex portions of the surface of the protective layer not in contact with the wafer is preferably 5 μm or less, more preferably 3 μm or less, and particularly preferably 1 μm or less, over the entire cut surface. In one embodiment, the planarization is performed by cutting, grinding, or polishing.

[0032] In one embodiment, the cutting is performed by cutting with a cutting tool. By cutting with a cutting tool, problems such as clogging of the grinding wheel during polishing can be eliminated, and flattening can be easily performed, compared to the case where flattening is performed by polishing with a polishing machine. Cutting with a cutting tool may be performed by a surface planer.

[0033] Process (3) Step (3) is a step of bonding the surface of the protective layer not in contact with the wafer to a support via an adhesive layer to form a laminate.

[0034] adhesive layer The adhesive layer is used to bond the surface of the protective layer not in contact with the wafer to the support. The adhesive layer may be a known temporary fixing material that can temporarily fix the wafer to the support and easily separate the support after processing is completed, for example, by IR laser method, UV irradiation method, laser lift-off method, solvent peeling method, heat-UV foaming method, mechanical peeling method, etc., and may be a liquid adhesive (adhesive dissolved in a solvent, etc.) applied by spin coating or the like to form a tacky adhesive tape. The adhesive layer may be formed on the support, the protective layer, or both. The thickness variation of the adhesive layer is preferably 5 μm or less, more preferably 3 μm or less, and particularly preferably 1 μm or less.

[0035] The adhesive layer is at least one selected from acrylic, silicone, polyimide, and rubber. When the adhesive layer is an adhesive tape, the adhesive tape may be a single layer or a laminate of multiple layers, or may be a double-sided tape containing a base film in the layers.

[0036] support The support preferably has sufficient strength and rigidity, and is excellent in heat resistance, chemical resistance, and thickness accuracy. By using such a support, even if the wafer is thinned after grinding, the wafer can be stably handled and can be subjected to multiple and / or diverse processes without bending or the like.

[0037] The support may be a known support, but preferred materials include silicon, sapphire, quartz, metals (e.g., aluminum, copper, steel, stainless steel), various glasses and ceramics, and resins (e.g., polyimide, polyamide, epoxy, phenol, polyphenylene ether, polyether ether ketone, polyetherimide, wholly aromatic polyamide, polyphenyl sulfide resin). The support may be made of a single material, or may be made of multiple materials, or may contain other materials deposited on a substrate. For example, a silicon wafer may have a vapor deposition layer of silicon nitride or the like. Particularly preferably, the support is made of glass, silicon, ceramic, metal, resin, or a composite material thereof.

[0038] In one embodiment, the adhesive layer may be formed on the base layer of the protective adhesive tape flattened in step (2), or may be formed on the surface of the support, or may be formed on both sides. Examples of methods for forming the adhesive layer include, but are not limited to, a method in which the adhesive layer is formed by spin coating when the adhesive layer is a liquid adhesive (such as an adhesive dissolved in a solvent), and a method in which the adhesive layer is formed by laminating tapes when the adhesive layer is a tape.

[0039] Back grinding process The back grinding process is typically a process of grinding and polishing the wafer, but is not limited to this and may also include singulation and the like. When grinding or polishing a wafer having electrodes formed on its front surface, the surface on which no electrodes are formed (back surface) is ground or polished. The thickness of the wafer after grinding or polishing the back surface varies depending on the electronic device in which the semiconductor device is used, but is preferably set to 200 μm or less, more preferably 50 μm or less. This allows the semiconductor device to be thinned, and the electronic device using the semiconductor device to be miniaturized.

[0040] When grinding or polishing the wafer, in step (3), the wafer is laminated with a rigid support via the adhesive layer to form a laminate with high thickness accuracy, whereby the wafer can be ground, etc. with better processing accuracy, and after the grinding, etc., the wafer can be subjected to the back surface treatment step described below or easily separated from the support and the adhesive layer without damaging the wafer.

[0041] In one embodiment, the method for grinding the backside of a wafer of the present invention may further include at least one of a wafer backside treatment step, a support removal step, a tacky adhesive layer removal step, or a protective adhesive tape removal step after grinding the backside of the wafer.

[0042] Back surface processing The method for grinding the backside of a wafer of the present invention may further include a step of subjecting the wafer to processing and / or chemical treatment as a backside treatment step after grinding the backside of the wafer.

[0043] Examples of the processing include, but are not limited to, annealing, back electrode formation (sputtering), deposition, etching, chemical vapor deposition (CVD), physical vapor deposition (PVD), resist coating / patterning, reflow, and dopant ion implantation.

[0044] The above-mentioned chemical treatment is typically a treatment using an acid, an alkali, or an organic solvent, and examples thereof include plating treatments such as electrolytic plating and electroless plating, wet etching treatments using hydrofluoric acid, an aqueous solution of tetramethylammonium hydroxide (TMAH), or the like, resist stripping processes using N-methyl-2-pyrrolidone, monoethanolamine, DMSO, or the like, and cleaning processes using concentrated sulfuric acid, aqueous ammonia, aqueous hydrogen peroxide, or the like, but are not limited to these.

[0045] In one embodiment, the back surface treatment includes at least one of etching, electrode formation, ion implantation, and annealing.

[0046] Support removal process The support removing step is a step of removing the support from the laminate, and examples of the support removing method include, but are not limited to, an IR laser method, a UV irradiation method, a laser lift-off method, a solvent stripping method, a heat / UV foaming method, and a mechanical stripping method.

[0047] Protective layer and adhesive layer removal process The protective layer and adhesive layer removing step is a step of removing the protective layer and the like from the thinned wafer, and the protective layer and the adhesive layer may be removed simultaneously or sequentially. Examples of the removal method include peeling, washing, and the like.

[0048] In one aspect, a method for manufacturing an electronic device is provided, which includes the method for grinding the backside of a wafer of the present invention in the manufacturing process. That is, the wafer ground by the method for grinding the backside of a wafer of the present invention can be subjected to the subsequent process to manufacture a final product. When a circuit or the like is formed on the wafer, the process that is usually used in the manufacture of a semiconductor device or an electronic device, such as dicing, bonding, packaging, and sealing, can be carried out to manufacture a semiconductor device or an electronic device as a product.

[0049] In one embodiment, the electronic device is a power device. As described above, power devices are used in power converters such as inverters and converters, and have unevenness on the surface of the wafer due to their characteristics, structure, manufacturing process, etc. The present invention makes it possible to suppress the influence of the unevenness on the device characteristics. Furthermore, since the effect of unevenness can be suppressed and handling can be improved not only in wafer back grinding but also in a wide range of processing processes, it can also be used for grinding electrodes (TSVs) that vertically penetrate silicon substrates and bump wafers with large unevenness.

[0050] Hereinafter, the method for grinding the back surface of a wafer according to one embodiment of the present invention will be further described with reference to the drawings, but the present invention is not limited to these embodiments.

[0051] (Embodiment 1) Reference numeral 1 in Fig. 1(a) denotes a semiconductor wafer (hereinafter referred to as wafer) to be thinned by back grinding. This wafer 1 is a silicon wafer or the like, and its thickness before processing is uniform, for example, 700 µm to 800 µm. A surface 11 of the wafer 1 is partitioned into a plurality of rectangular devices by grid-like division lines. Electrodes and the like are formed on the devices, which cause unevenness on the surface 11 of the wafer 1.

[0052] 1(a) to 1(e), the method for grinding the backside of a wafer according to this embodiment involves applying a protective adhesive tape 3 to the front side 11 of a wafer 1, flattening the base layer 31 of the protective adhesive tape 3 by grinding with a tool, adhering the base layer 33 of the flattened protective adhesive tape 3 to a support 5 via an adhesive layer 4, and grinding the back side 12 of the wafer 1 to thin it to a desired thickness (for example, 200 μm or less). The process will be described in detail below.

[0053] As described above, in this embodiment, first, the protective adhesive tape 3 is applied to the surface 11 of the wafer 1. The application is performed by reducing the pressure to 100 Pa or less and heating to 100° C. or less using an automatic application device. As shown in FIG. 1(b), the unevenness on the surface 11 of the wafer 1 is transferred to the base layer 31 of the applied protective adhesive tape 3.

[0054] After the wafer 1 has the protective adhesive tape 3 attached to its front surface 11, the base layer 31 of the protective adhesive tape 3 is then cut flat. A surface planer is used for this cutting. With this surface planer, the back surface 12 of the wafer 1 is held by suction on the suction surface of a vacuum chuck table, and the base layer 31 of the protective adhesive tape 3 is cut flat by the bit of a rotating cutting tool of a cutting unit.

[0055] Next, the adhesive layer 4 is formed on the flattened base layer 33 of the protective adhesive tape. To form this adhesive layer 4, a spin coating method is preferably adopted in which the wafer 1 is placed and held on a rotating table so that the base layer 33 of the flattened protective adhesive tape is exposed and the center of the wafer 1 coincides with the rotation axis of the table, the table is rotated, and a liquid adhesive is dropped on the center of the rotating wafer 1, and the adhesive is spread and applied over the entire surface of the base layer 33 of the flattened protective adhesive tape by centrifugal force. In this way, the adhesive layer 4 is formed on the flattened base layer 33 of the protective adhesive tape as shown in FIG. 1(d).

[0056] Next, the support 5 is bonded to the adhesive layer 4 to obtain the laminate shown in Fig. 1(e). Since the laminate thus obtained has no irregularities in the base layer 33 of the protective adhesive tape 3, the irregularities on the front surface 11 of the wafer 1 are not transferred when the back surface 12 of the wafer 1 is ground, and since the support 5 is present, even if the wafer 1 is thinned by back surface grinding, handling properties such as transportability are not lost in the subsequent processing process.

[0057] Next, the back surface 12 of the wafer 1 is ground to thin the wafer 1 to a target thickness. A grinding device that performs in-feed grinding is suitably used for grinding the back surface of the wafer 1. With this grinding device, the support 5 is adsorbed to the adsorption surface of a vacuum chuck table to hold the laminate, and rough grinding and finish grinding are sequentially performed on the back surface 12 of the wafer 1 by two grinding units (one for rough grinding and one for finish grinding).

[0058] In this case, to remove the thinned wafer 1, the support 5 is removed and then the protective adhesive tape 3 is removed. The support 5 is removed by a mechanical peeling method in which a remover is inserted into the interface between the support 5 and the adhesive layer 4 and the support 5 is pulled up. The protective adhesive tape 3 is removed by peeling it off from the wafer 1. By using the protective adhesive tape 3, the wafer cleaning process after peeling is unnecessary or can be minimized, which provides excellent workability and allows the manufacturing costs of semiconductor devices and electronic devices to be reduced.

[0059] (Embodiment 2) Instead of the protective adhesive tape 3 of the first embodiment, a protective resin layer can be used to protect the surface 11 of the wafer 1. In this case, the wafer 1 is placed and held on a rotating table so that the surface 11 of the wafer 1 is exposed and the center of the wafer 1 coincides with the rotation axis of the table, the table is rotated, and a precursor resin liquid is dropped onto the center of the rotating wafer 1, and the precursor resin liquid is spread over the entire surface of the surface 11 of the wafer 1 by centrifugal force to apply the precursor resin liquid. The coating film after spin coating is placed on a hot plate and dried, and the solvent in the film is completely removed to form a protective layer. The other steps are the same as those of the first embodiment.

[0060] In this case, the protective layer is removed by a cleaning process instead of peeling off the protective adhesive tape 3 in the above-mentioned embodiment 1. In the cleaning process, the wafer 1 is fixed on a rotating table with the protective layer facing up, a cleaning solvent is sprayed, the cleaning solvent is placed on the wafer and allowed to stand, the cleaning solvent is discarded, and a new cleaning solvent is placed on the wafer in the same manner and allowed to stand. This procedure is repeated twice, and then the wafer 1 is rotated while being sprayed with isopropyl alcohol (IPA) to rinse the wafer. [Industrial Applicability]

[0061] The method for grinding the backside of a wafer of the present invention can suppress the effects of unevenness on the surface of the wafer and improve handleability in a wide range of treatment processes after the wafer is thinned, and therefore contributes greatly to improving the productivity of semiconductor devices, electronic devices, and the like, and has high applicability in various fields of industry, such as the electronic component industry including the semiconductor process industry, the electrical and electronics industry that uses electronic components, the transportation machinery industry, the information and communications industry, and the precision equipment industry. [Explanation of symbols]

[0062] 1. Semiconductor wafer 11 Wafer surface 12 Backside of wafer 3 Protective adhesive tape 31 Base layer of protective adhesive tape 32 Adhesive layer of protective adhesive tape 33 Flattened base layer of protective adhesive tape 4 Adhesive layer 5 Support

Claims

1. A method for grinding the backside of a wafer having an uneven surface, comprising the steps of: A step (1) of forming a protective layer on the surface of the wafer; (2) planarizing a surface of the protective layer that is not in contact with the wafer; and a step (3) of adhering a surface of the protective layer not in contact with the wafer to a support via an adhesive layer; A method for grinding the back surface of a wafer, comprising: However, the protective layer is a protective adhesive tape.

2. 2. The method for grinding a wafer backside according to claim 1, wherein the base layer of the protective adhesive tape contains at least one resin selected from the group consisting of PET, PEN, PBT, LCP, PI, PA, PEEK, and PPS.

3. 3. The method for grinding the back surface of a wafer according to claim 1, wherein the wafer having an uneven surface is a wafer having unevenness due to at least one of electrodes, circuit patterns, polyimide, defect marks, and bumps formed on the surface.

4. 4. The method for grinding a back surface of a wafer according to claim 1, wherein the planarizing step is a step of planarizing by cutting, grinding, or polishing.

5. 5. The method for grinding the back surface of a wafer according to claim 4, wherein the cutting is performed by a cutting tool.

6. The method for grinding a wafer backside according to any one of claims 1 to 5, wherein the adhesive layer is a liquid adhesive or an adhesive tape.

7. 7. The method for grinding a wafer backside according to claim 1, wherein the support is made of glass, silicon, ceramic, metal, resin or a composite material thereof.

8. The method for grinding the backside of a wafer according to any one of claims 1 to 7, further comprising the step of forming the adhesive layer on a surface of the planarized protective layer not in contact with the wafer, on a surface of the support, or on both of the surface and the support, after the step (2) and before the step (3).

9. The method for grinding the backside of a wafer according to any one of claims 1 to 8, further comprising a backside treatment step for the wafer after grinding the backside of the wafer.

10. 10. The method for grinding the back surface of a wafer according to claim 9, wherein the back surface processing step of the wafer includes at least one of etching, electrode formation, ion implantation, and annealing.

11. The method for grinding the backside of a wafer according to any one of claims 1 to 10, wherein the thickness of the wafer after backside grinding is 200 μm or less.

12. A method for manufacturing an electronic device, comprising the method for grinding the backside of a wafer according to any one of claims 1 to 11 in the manufacturing process.

13. The method for producing an electronic device according to claim 12 , wherein the electronic device is a device having an electrode also on the back side.

14. The method for producing an electronic device according to claim 13 , wherein the electronic device is a power device.

Citation Information

Patent Citations

  • Laminate including substrate to be ground, method of manufacturing the same, method of manufacturing ultrathin substrate using the laminate, and apparatus therefor

    JP2004064040A

  • Rear-surface grinding method for wafer

    JP2009043931A

  • Processing method

    JP2013026380A

  • Wafer processing method

    JP2013118324A