Electrode manufacturing method

By preparing a slurry with specific solid content ratios to achieve a pendular or funicular state, the method addresses mold releasability and density variations in electrode manufacturing, ensuring uniform electrode structure and reducing peeling/collapse during the formation of recesses.

JP7552535B2Active Publication Date: 2024-09-18TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021139778
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-09-18
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

Existing methods for forming recesses in active material layers of electrodes face issues with mold releasability and density variations due to low fluidity of solid materials after drying, leading to non-uniform electrode reactions and adhesion to convex shapes, which affects the formation of desired recesses.

Method used

A method involving the preparation of a slurry with specific solid content ratios to achieve a pendular or funicular state in the coating film, allowing for improved mold releasability and reduced density variations by pressing a convex mold onto the film in these states, followed by controlled drying to form an active material layer with recesses.

Benefits of technology

The method ensures effective formation of recesses with reduced adhesion and density variations, enhancing electrode uniformity and reducing the risk of peeling or collapse during the embossing process, resulting in a more consistent electrode structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552535000001
    Figure 0007552535000001
  • Figure 0007552535000007
    Figure 0007552535000007
  • Figure 0007552535000008
    Figure 0007552535000008
Patent Text Reader

Abstract

To provide a method for manufacturing an electrode with a recess.SOLUTION: A slurry is prepared by mixing active material particles, a binder, and a dispersion medium. A first coating film is formed by applying the slurry to the surface of a substrate. A second coating film is formed by drying the first coating film. By pressing a convex mold against the surface of the second coating film, recesses are formed in the surface. After forming the recesses, the second coating film is dried to form an active material layer. In the second coating film, the solid phase, liquid phase, and gas phase form a pendular state or a funicular state.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrode manufacturing method and an electrode manufacturing apparatus. [Background technology]

[0002] Japanese Patent Laid-Open Publication No. 2015-138619 (Patent Document 1) discloses spraying a solvent onto the surface of a negative electrode active material mixture layer before pressing a mold having a concave-convex pattern against the negative electrode active material mixture layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-138619 A Summary of the Invention [Problem to be solved by the invention]

[0004] It has been proposed to form recesses on the surface of the active material layer, which are expected to function as, for example, permeation paths for the electrolyte and paths for discharging gas.

[0005] The active material layer can be formed by coating a slurry. That is, active material particles, a binder, and a dispersion medium are mixed to prepare a slurry. The slurry is coated on the surface of the substrate to form a coating film. The coating film is dried to form the active material layer.

[0006] The recesses can be formed by embossing. That is, a convex mold is pressed against the surface of the active material layer after drying to form the recesses. In the active material layer after drying, the fluidity of the solid material (active material particles, etc.) tends to be low. Therefore, at the bottom of the recesses, the density may increase locally due to compression of the solid material. The occurrence of density variation in the active material layer may cause inconveniences such as non-uniform electrode reactions.

[0007] For example, by re-spraying a liquid (dispersion medium) on the surface of the active material layer after drying, the solid material in the surface layer of the active material layer can be given fluidity. This is expected to reduce density variations due to embossing. However, there is room for improvement in releasability. That is, adhesion may occur due to the solid material becoming wet. There is a possibility that the desired recesses will not be formed due to the solid material adhering to the convex mold. Furthermore, it is thought that the re-sprayed liquid does not penetrate deep into the active material layer. In the deep layer of the active material layer, the fluidity of the solid material is still low, so there is a possibility that density variations will not be eliminated.

[0008] It is an object of the present disclosure to provide a method for manufacturing a recessed electrode.

[0009] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure. [Means for solving the problem]

[0010] 1. A method for producing an electrode includes the following steps (a) to (e): (a) A slurry is prepared by mixing active material particles, a binder, and a dispersion medium. (b) The slurry is applied to the surface of the substrate to form a first coating. (c) The first coating film is dried to form a second coating film. (d) A convex mold is pressed against the surface of the second coating film to form concave portions on the surface. (e) After the recesses are formed, the second coating film is dried to form an active material layer. In the second coating film, the solid, liquid and gas phases form a pendular or funicular state.

[0011] When the slurry (coating) applied to the substrate is dried, the liquid phase (dispersion medium) decreases and the gas phase (bubbles, voids) is generated. The coating finally becomes dry (solid and gas phase).

[0012] FIG. 1 is a conceptual diagram showing the drying process of a coating film. The coating film reaches the "dry state" through the "slurry state," "capillary state," "funicular state," and "pendular state." The classification of dry states is described in detail in "Particle Size Enlargement" by CE CAPES (Elsevier Scientific Publishing Company, 1980). In each state, the relationship between the solid phase (active material particles), liquid phase (dispersion medium), and gas phase (gas) is different.

[0013] The "slurry state" consists of a solid phase (active material particles 1) and a liquid phase (dispersion medium 2). The gas phase (gas 3) is substantially absent. The solid phase (active material particles 1) is suspended in the liquid phase (dispersion medium 2). The solid phase is dispersed in the liquid phase and is not continuous.

[0014] "Capillary state" refers to a state in which the liquid phase has decreased from the slurry state. The capillary state consists of a solid phase, a liquid phase, and a gas phase (gas 3). The solid phase is covered by the liquid phase. The liquid phase is continuous around the solid phase. The gas phase is in contact with the liquid phase. The gas phase is not in contact with the solid phase.

[0015] The "funicular state" is a state in which the liquid phase is further reduced from the capillary state. The funicular state consists of a solid phase, a liquid phase, and a gas phase. The liquid phase is continuous around the solid phase. Part of the solid phase is in contact with the gas phase.

[0016] The "pendular state" is a state in which the liquid phase is further reduced from the funicular state. The pendular state consists of a solid phase, a liquid phase, and a gas phase. The liquid phase is discontinuous. The liquid phase bridges the solid phases. The gas phase is in contact with both the solid and liquid phases.

[0017] "Dry state" consists of a solid phase and a gas phase. A liquid phase is substantially absent.

[0018] According to the new findings of the present disclosure, when the coating film is in a pendular or funicular state, it is possible to achieve both releasability and flowability during embossing. That is, a coating film in a pendular or funicular state is less likely to adhere to a convex mold and is less likely to have density variations. This is thought to be because a coating film in a pendular or funicular state has a small adhesive force and can flow integrally throughout.

[0019] On the other hand, for example, when the coating film is in a capillary state, the coating film tends to adhere in a convex shape, and for example, when the coating film is in a dry state, the density variation tends to increase.

[0020] 2. The slurry may have a solid content of, for example, 50 to 65% by mass, and the second coating film may have a solid content of, for example, 70 to 99% by mass.

[0021] At a solid content of 50 to 65%, a slurry state tends to form, and at a solid content of 70 to 99%, a pendular state or funicular state tends to form.

[0022] 3. The active material particles may contain, for example, a positive electrode active material. The slurry may have, for example, a solid content rate of 55 to 65% by mass. The second coating film may have, for example, a solid content rate of 80 to 99% by mass.

[0023] When the active material particles are positive electrode active material particles, a slurry state tends to be formed at a solid content rate of 55 to 65%, and a pendular state or funicular state tends to be formed at a solid content rate of 80 to 99%.

[0024] 4. The active material particles may contain, for example, a negative electrode active material. The slurry may have, for example, a solid content rate of 50 to 60% by mass. The second coating film may have, for example, a solid content rate of 70 to 99% by mass.

[0025] When the active material particles are negative electrode active material particles, a slurry state tends to be formed at a solid content rate of 50 to 60%, and a pendular state or funicular state tends to be formed at a solid content rate of 70 to 99%.

[0026] 5. In plan view, the second coating film may have a longitudinal direction and a lateral direction. In the lateral direction, a dripping portion may be formed at an end of the second coating film. The convex mold may be pressed against the second coating film so that at least a part of the dripping portion does not contact the convex mold.

[0027] For example, it is possible to prepare a paint in a pendular or funicular state from the beginning, without going through a slurry state. The paint may be, for example, a wet granule (wet powder or wet granules). Granules are also called granules. Granules can be formed by subjecting powder to a granulation operation.

[0028] The slurry may have high fluidity. In the coating film formed by the slurry, a dripping portion may be formed at the edge of the coating film. In the dripping portion, the coating film is inclined toward the outside.

[0029] Wet powder particles have a lower fluidity than slurries. Coatings formed from wet powder particles tend not to have inclined edges. When embossing is performed on a coating that does not have inclined edges, recesses are formed up to the vicinity of the tip of the coating. The formation of recesses up to the vicinity of the tip may cause the coating to peel off or collapse at the edge.

[0030] In the dripping portion, the thickness of the coating film gradually decreases toward the outside. Therefore, it is possible to perform embossing so that the convex mold is in contact with the coating film in the center of the coating film, but is not in contact with the coating film at the edge (dripping portion) of the coating film. Since no recesses are formed at the edge (dripping portion) of the coating film, it is expected that peeling, collapse, etc. of the coating film at the edge of the coating film will be reduced.

[0031] 6. The method for producing an electrode may further include, for example, the following (f): (f) Compressing the active material layer.

[0032] The dried coating film (active material layer) with recesses may further be subjected to compression processing.

[0033] 7. The electrode manufacturing apparatus includes a conveying device, a coating device, a first drying device, a molding device, and a second drying device. The conveying device is configured to convey the substrate in the order of the coating device, the first drying device, the molding device, and the second drying device. The coating device is configured to form a first coating film by coating a slurry on the surface of the substrate. The slurry includes active material particles, a binder, and a dispersion medium. The first drying device is configured to form a second coating film by drying the first coating film. The molding device is configured to press a convex mold against the surface of the second coating film to form a concave portion on the surface. The second drying device is configured to dry the second coating film to form an active material layer.

[0034] In the molding device, embossing is performed. By arranging the first drying device before the molding device, the coating film can be adjusted to a pendular or funicular state before embossing. In other words, the manufacturing method of the electrode described in "1." above can be performed.

[0035] 8. The second coating film may be formed to have a longitudinal direction and a lateral direction in plan view. The coating device may be configured to form the first coating film, and the first drying device may be configured to dry the first coating film, so that a drip portion is formed at an end of the second coating film in the lateral direction.

[0036] The formation of the dripping portion is expected to reduce peeling and crumbling of the coating film at the edges of the coating film.

[0037] 9. The molding device may include, for example, an embossing roll. A convex shape may be formed on the surface of the embossing roll. The molding device may be configured to press the embossing roll against the second coating film so that at least a part of the dripping portion does not contact the convex shape.

[0038] According to the electrode manufacturing apparatus of "9." above, the electrode manufacturing method of "5." above can be carried out.

[0039] 10. The electrode manufacturing apparatus may further include a compression device. The conveying device may be configured to convey the base material that has passed through the second drying device to the compression device. The compression device may be configured to compress the active material layer.

[0040] According to the electrode manufacturing apparatus of the above "10.", the electrode manufacturing method of the above "6." can be carried out. [Brief description of the drawings]

[0041] [Figure 1] FIG. 1 is a conceptual diagram showing the drying process of a coating film. [Diagram 2] FIG. 2 is a schematic flow chart of the method for producing an electrode in this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the electrodes in this embodiment. [Figure 4] FIG. 4 is a first schematic cross-sectional view showing an electrode in this embodiment. [Diagram 5] FIG. 5 is a plan view showing the electrodes in this embodiment. [Figure 6] FIG. 6 is a second schematic cross-sectional view showing the electrode in this embodiment. [Figure 7] FIG. 7 is a conceptual diagram showing an electrode manufacturing apparatus in this embodiment. [Figure 8] FIG. 8 shows cross-sectional and top surface images of the electrodes in the first to third test examples. [Figure 9] FIG. 9 is a graph showing the relationship between the solid content and the drying time in the first test example. [Figure 10]FIG. 10 is a graph showing the relationship between the solid content and the drying time in the second test example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] <Definitions of terms, etc.> Hereinafter, an embodiment of the present disclosure (which may be abbreviated as "the present embodiment") and an example of the present disclosure (which may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.

[0043] In this specification, the words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The word "consisting of" is closed-ended. However, even in a closed form, additional elements that are normally associated impurities or unrelated to the disclosed technology are not excluded. The word "consisting essentially of..." is semi-closed. In a semi-closed form, the addition of elements that do not substantially affect the basic and novel characteristics of the disclosed technology is permitted.

[0044] In the methods described herein, the order of execution of multiple steps, operations, and the like is not limited to the order described unless otherwise specified. For example, multiple steps may proceed simultaneously. For example, multiple steps may be performed one after the other.

[0045] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only a "single particle" but also an "aggregate of particles (powder, powder, particle group)."

[0046] In this specification, the expressions "may" and "can" are used in the permissive sense of "have the potential to" rather than in the obligatory sense of "must".

[0047] In this specification, unless otherwise specified, a numerical range such as "70 to 99%" includes an upper limit and a lower limit. That is, "70 to 99%" indicates a numerical range of "70% or more and 99% or less". In addition, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part, table, figure, etc. of this specification.

[0048] In this specification, all numerical values ​​are modified by the term "about". The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values ​​are approximations that may vary depending on the application of the disclosed technology. All numerical values ​​are expressed in significant figures. Measurements may be average values ​​of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limits of the measurement device.

[0049] Geometric terms (e.g., "parallel," "perpendicular," "orthogonal," etc.) in this specification should not be interpreted in a strict sense. For example, "parallel" may deviate slightly from the strict meaning of "parallel." Geometric terms in this specification may include, for example, tolerances, errors, etc. in design, work, manufacturing, etc. The dimensional relationships in each figure may not match the actual dimensional relationships. In order to facilitate understanding of the disclosed technology, the dimensional relationships (length, width, thickness, etc.) in each figure may be changed. Furthermore, some configurations may be omitted.

[0050] In this specification, the term "planar view" refers to viewing an object from a line of sight parallel to the thickness direction of the object (e.g., an "electrode"), and the term "cross-sectional view" refers to viewing an object from a line of sight perpendicular to the thickness direction of the object.

[0051] In this specification, for example, "LiCoO 2When a compound is expressed by a stoichiometric formula such as "LiCoO", the stoichiometric formula is merely a representative example. The composition may be non-stoichiometric. For example, lithium cobalt oxide may be expressed as "LiCoO 2 ", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping or substitution with trace elements may also be permitted.

[0052] In this specification, the term "solid content" refers to the mass fraction (percentage) of components other than the liquid in a solid-liquid mixture. The solid content may also be referred to as "NV (Nonvolatile Content)." In slurries and coatings, the dispersion medium is liquid. When a binder is dissolved in the dispersion medium, the binder (solute) is considered to be a component other than the liquid.

[0053] In this specification, "D50" is defined as the particle size at which the cumulative frequency of the smaller particle size reaches 50% in the volume-based particle size distribution. The volume-based particle size distribution can be measured by a laser diffraction particle size distribution measuring device.

[0054] <Electrode manufacturing method> FIG. 2 is a schematic flow chart of the method for producing an electrode in this embodiment. Hereinafter, "the method for manufacturing an electrode in this embodiment" may be abbreviated to "the present manufacturing method". The present manufacturing method includes "(a) preparation of slurry", "(b) coating", "(c) first drying", "(d) embossing", and "(e) second drying". The present manufacturing method may further include, for example, "(f) compression". Each step may be performed in the atmosphere or, for example, in dry air.

[0055] In this manufacturing method, a lithium ion battery can be manufactured. However, the lithium ion battery is merely one example. In this manufacturing method, any battery can be manufactured. In this manufacturing method, a positive electrode or a negative electrode can be manufactured. In this manufacturing method, at least one of a positive electrode and a negative electrode can be manufactured.

[0056] (a) Preparation of Slurry The present manufacturing method includes preparing a slurry by mixing active material particles, a binder, and a dispersion medium. The slurry is a liquid paint. In the present manufacturing method, the slurry can be prepared by any stirring device. For example, a planetary mixer, "High Speed ​​Mixer Series (manufactured by EarthTechnica Corporation)" or the like may be used.

[0057] The active material particles, the binder, and the dispersion medium are put into the stirring tank of the stirring device. For example, optional components (such as a conductive material) may be added. The materials are mixed under predetermined conditions to prepare a slurry.

[0058] <Active material particles> The active material particles are the dispersoid of the slurry. The active material particles may have any shape. The active material particles may be, for example, spherical, clumpy, flaky, columnar, etc. The active material particles may have any size. The active material particles may have, for example, a D50 of 1 to 30 μm, or a D50 of 5 to 20 μm.

[0059] The active material particles include a positive electrode active material or a negative electrode active material. When the active material particles include a positive electrode active material, a positive electrode can be manufactured. When the active material particles include a negative electrode active material, a negative electrode can be manufactured.

[0060] The positive electrode active material can absorb and release lithium ions at a higher potential than the negative electrode active material. The positive electrode active material can include any component. The positive electrode active material can be, for example, LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , Li(NiCoMn)O 2 , Li(NiCoAl)O 2 , and LiFePO 4 For example, "Li(NiCoMn)O 2"(NiCoMn)" in "Li(NiCoMn)O" indicates that the sum of the composition ratios in the parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. 2 For example, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O 2 , Li(Ni 0.5 Co 0.2 Mn 0.3 )O 2 , Li(Ni 0.8 Co 0.1 Mn 0.1 )O 2 etc. may be included.

[0061] The negative electrode active material can absorb and release lithium ions at a lower potential than the positive electrode active material. The negative electrode active material can include any component. Examples of the negative electrode active material include graphite, soft carbon, hard carbon, silicon, silicon oxide, silicon-based alloys, tin, tin oxide, tin-based alloys, and Li 4 Ti 5 O 12 may contain at least one selected from the group consisting of:

[0062] <Binder> The binder can bind the solid materials together. The binder may be soluble or insoluble in the dispersion medium. The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material particles. The binder may contain any component. The binder may contain at least one selected from the group consisting of, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyimide (PI), polyamideimide (PAI), and polyacrylic acid (PAA).

[0063] <Conductive material> A conductive material may be mixed into the slurry. The conductive material may form an electronic conduction path in the active material layer. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the active material particles. The conductive material may contain any component. The conductive material may contain, for example, at least one selected from the group consisting of carbon black, vapor-grown carbon fiber, carbon nanotubes, and graphene flakes. The carbon black may contain, for example, at least one selected from the group consisting of acetylene black, furnace black, channel black, and thermal black.

[0064] <Dispersion medium> The dispersion medium is a liquid. The dispersion medium may be a solvent for the binder. The dispersion medium may be selected depending on, for example, the type of active material particles, the type of binder, etc. The dispersion medium may contain, for example, water, N-methyl-2-pyrrolidone (NMP), etc.

[0065] The amount of the dispersion medium is adjusted according to the solid content of the slurry. The slurry may have a solid content of, for example, 50 to 65%. When the active material particles contain a positive electrode active material, the slurry may have a solid content of, for example, 55 to 65%. When the active material particles contain a negative electrode active material, the slurry may have a solid content of, for example, 50 to 60%. Within these solid content ranges, aggregation and sedimentation of the active material particles are unlikely to occur, and the slurry state tends to be easily maintained.

[0066] (b) Coating The present manufacturing method includes forming a first coating film by applying a slurry to a surface of a substrate. In the present manufacturing method, the slurry can be applied by any coating device. For example, a die coater, a roll coater, or the like may be used.

[0067] The slurry has high fluidity. Therefore, a dripping portion may be formed in the first coating film. The dripping portion may be formed at an end portion in the short side direction in a plan view. The short side direction is perpendicular to the long side direction. The long side direction may be the same direction as the direction in which the workpiece is transported in the coating device.

[0068] <Base material> The substrate is a support for the active material layer. The substrate may be, for example, sheet-shaped. The substrate may be, for example, strip-shaped. The substrate may be conductive. The substrate may function as a current collector. The substrate may include, for example, a metal foil. The substrate may include, for example, at least one selected from the group consisting of aluminum (Al) foil, Al alloy foil, copper (Cu) foil, Cu alloy foil, nickel (Ni) foil, Ni alloy foil, titanium (Ti) foil, and Ti alloy foil. When the electrode is a positive electrode, the substrate may include, for example, an Al foil. When the electrode is a negative electrode, the substrate may include, for example, a Cu foil. The substrate may have a thickness of, for example, 5 to 50 μm, or 5 to 20 μm.

[0069] 《(c) First drying》 The present manufacturing method includes forming a second coating film by drying the first coating film. The first drying can be, for example, another way of saying "pre-drying". In the first drying, any drying device can be used. For example, a hot air drying device, an infrared drying device, or the like may be used.

[0070] In this manufacturing method, the drying conditions are adjusted so that the solid phase, liquid phase, and gas phase form a pendular state or a funicular state in the second coating film. The drying conditions may include, for example, the drying temperature, drying time, etc. The drying state of the second coating film is confirmed by the following method.

[0071] How to check the dryness In plan view, the second coating film has a longitudinal direction and a lateral direction. The longitudinal direction may be the same direction as the direction in which the workpiece is transported in the drying device. The lateral direction may be rephrased as the "width direction." The second coating film is divided into five equal parts in the lateral direction, thereby dividing the film into five regions. For example, a cutter or the like is used to cut out a sample (second coating film) together with the substrate from near the center of each region. In other words, five samples are prepared.

[0072] A cryo-SEM (cryo scanning electron microscopy) is prepared. The sample is rapidly frozen in the atmosphere using liquid nitrogen. The time from the first drying to the rapid freezing is preferably within 10 minutes. After freezing, the sample is introduced into a cryo chamber. In the cryo chamber, the sample is subjected to cross-section processing. After cross-section processing, the sample is introduced into a cooling stage. In the cooling stage, the sample is observed by SEM. The observation magnification can be 1000 to 5000 times.

[0073] In the SEM image, "active material particles whose surface is partially covered with the dispersion medium" are considered to be in a pendular or funicular state. In other words, active material particles other than those in (i) and (ii) below are considered to be in a pendular or funicular state.

[0074] (i) "Active material particles whose entire surface is covered with a dispersion medium" (ii) "Active material particles whose entire surface is covered with a gas phase (voids)"

[0075] In the SEM image of each sample, the state of 20 or more active material particles is confirmed. In other words, the state of 100 or more active material particles is confirmed in total. It is considered that the more the number of confirmed particles, the more reliable the measurement results are. When 50% or more of the active material particles are in the pendular or funicular state in terms of number ratio, the solid phase, liquid phase, and gas phase in the second coating film are considered to form a pendular or funicular state.

[0076] For example, 70% or more of the active material particles in terms of number ratio may be in the pendular or funicular state.For example, 80% or more of the active material particles in terms of number ratio may be in the pendular or funicular state.

[0077] <Solid content> The solid content of the second coating film may be confirmed. For example, a sample (second coating film) is cut out together with the substrate. The area of ​​the sample is, for example, 10 to 50 cm. 2The mass of the sample in a wet state and the mass of the sample in a dry state are measured. The mass of the dispersion medium is calculated from the difference between the mass in the wet state and the mass in the dry state. The solid content is further calculated from the mass of the dispersion medium.

[0078] The second coating film may have a solid content of, for example, 70 to 99%. At a solid content of 70 to 99%, pendular or funicular states tend to form easily.

[0079] When the active material particles contain a positive electrode active material, the second coating film may have a solid content of, for example, 80 to 99%. When the active material particles contain a positive electrode active material, a pendular state or a funicular state tends to be formed at a solid content of 80 to 99%. When the active material particles contain a positive electrode active material, the second coating film may have a solid content of, for example, 81 to 97%.

[0080] When the active material particles contain a negative electrode active material, the second coating film may have a solid content of, for example, 70 to 99%. When the active material particles contain a negative electrode active material, a pendular state or a funicular state tends to be formed at a solid content of 70 to 99%. When the active material particles contain a negative electrode active material, the second coating film may have a solid content of, for example, 72 to 96%.

[0081] (d) Embossing The method includes forming recesses in the surface of the second coating by pressing a convex mold against the surface.

[0082] In the embossing process, for example, an embossing roll or the like may be used. In this manufacturing method, the second coating film (processing target) is in a pendular state or a funicular state. Therefore, the releasability of the second coating film can be good. In other words, the second coating film (material) is unlikely to adhere to the convex mold. Furthermore, since the contact portion with the convex mold and its surroundings can flow as one unit, the occurrence of density variation can be reduced. In addition, there is also an advantage that molding can be performed with a smaller load than in a dry state.

[0083] In this manufacturing method, one or more recesses are formed. A plurality of recesses may be formed. By forming a plurality of recesses, a concave-convex structure can be formed on the surface of the second coating film. Each recess may be, for example, linear, curved, wavy, or dot-shaped. The planar pattern of the recesses may be, for example, a line pattern or a lattice pattern.

[0084] (e) Second Drying The present production method includes forming an active material layer by drying the second coating film after the formation of the recesses.

[0085] The second drying may be referred to as "main drying", for example. In the second drying, the second coating film is dried until it is in a dry state (see FIG. 1). This forms an active material layer (a coating film in a dry state). In the second drying, any drying device may be used. For example, a hot air drying device, an infrared drying device, or the like may be used.

[0086] (f) Compression The present manufacturing method may include compressing the active material layer. The thickness and density of the active material layer can be adjusted by compression. For example, the active material layer may be compressed by a roll press device.

[0087] The electrode (raw sheet) can be manufactured as described above. The raw sheet can be cut into a predetermined shape according to the battery specifications.

[0088] <Electrode> FIG. 3 is a schematic diagram showing the electrodes in this embodiment. The electrode 100 includes a substrate 110 and an active material layer 120. Details of the substrate 110 are as described above. The active material layer 120 is formed on the surface of the substrate 110. The active material layer 120 may be formed on only one surface of the substrate 110. The active material layer 120 may be formed on both the front and back surfaces of the substrate 110. The active material layer 120 may have a thickness of, for example, 10 to 1000 μm, 50 to 500 μm, or 100 to 200 μm.

[0089] The active material layer 120 includes active material particles and a binder. The active material layer 120 may further include, for example, a conductive material. Details of each material are as described above. A recess 121 (groove) is formed on the surface of the active material layer 120. One recess 121 may be formed, or a plurality of recesses 121 (groove group) may be formed.

[0090] FIG. 4 is a first schematic cross-sectional view showing an electrode in this embodiment. The cross-sectional shape of the recess 121 is arbitrary. In the cross-sectional view, the bottom of the recess 121 may be, for example, flat, curved, or inclined. In the cross-sectional view, the recess 121 may be, for example, V-shaped or U-shaped.

[0091] The pitch 121p of the recesses 121 indicates the distance between the deepest parts of adjacent recesses 121. If the bottom of the recess 121 is flat, the center of the bottom is considered to be the deepest part. The pitch 121p may be, for example, 0.1 to 10 mm, 0.5 to 5 mm, or 1 to 3 mm.

[0092] Depth 121d of recess 121 indicates the depth from the surface of active material layer 120 (the apex of protrusion 122) to the deepest part of recess 121. Depth 121d may be, for example, 10 to 150 μm, or 50 to 100 μm. The ratio of depth 121d of recess 121 to thickness 120t of active material layer 120 may be, for example, 0.1 to 0.9, 0.2 to 0.8, or 0.3 to 0.7.

[0093] The protrusions 122 are formed between the recesses 121. In this embodiment, it is expected that there is a small density variation (difference in density) between the recesses 121 and the protrusions 122. The ratio of the density of the active material particles in the protrusions 122 to the density of the active material particles in the recesses 121 may be, for example, 0.7 to 1.0, 0.8 to 1.0, or 0.9 to 1.0. For example, in a cross-sectional SEM image of the active material layer 120, the ratio of the area of ​​the active material particles included in the recesses 121 to the area of ​​the recesses 121 may be regarded as the density of the recesses 121. For example, the ratio of the area of ​​the active material particles included in the recesses 122 to the area of ​​the recesses 122 may be regarded as the density of the recesses 122.

[0094] FIG. 5 is a plan view showing the electrodes in this embodiment. In plan view (XY plane), active material layer 120 has a longitudinal direction (Y-axis direction) and a lateral direction (X-axis direction). The longitudinal direction may be alternatively referred to as the "length direction". The lateral direction may be alternatively referred to as the "width direction". Recesses 121 and protrusions 122 extend along the lateral direction. However, recesses 121 and protrusions 122 may extend along, for example, the longitudinal direction.

[0095] In the short-side direction (X-axis direction), the active material layer 120 includes a central portion 123 and an end portion 124. The end portion 124 is connected to the central portion 123. The end portion 124 may be formed on both sides of the central portion 123, or may be formed on only one side. The width of the end portion 124 (one side) may be, for example, 0.001 to 10 mm, 0.01 to 5 mm, or 0.1 to 3 mm. The central portion 123 may have any width. The ratio of the width of the end portion 124 (one side) to the width of the central portion 123 may be, for example, 0.001 to 0.05.

[0096] FIG. 6 is a second schematic cross-sectional view showing the electrode in this embodiment. End 124 may include, for example, dripping portion 125. Dripping portion 125 may be referred to as, for example, an "inclined portion." In dripping portion 125, active material layer 120 is inclined. That is, in dripping portion 125, the thickness of active material layer 120 gradually decreases toward the outside. Dripping portion 125 has inclination angle 125θ of, for example, 1 to 60 degrees, or 1 to 30 degrees. Dripping portion 125 has width 125w of, for example, 0.1 to 3 mm, or 0.5 to 2 mm.

[0097] For example, the convex shape does not reach dripping portion 125, and therefore recess 121 may not be formed in at least a part of dripping portion 125. This is expected to reduce, for example, peeling and collapse of active material layer 120 at end 124. The distance between the tip of dripping portion 125 and the tip of recess 121 in the short direction may be, for example, 0.1 to 3 mm, or 0.5 to 2 mm.

[0098] <Electrode manufacturing equipment> FIG. 7 is a conceptual diagram showing an electrode manufacturing apparatus in this embodiment. The present manufacturing method can be carried out in the electrode manufacturing apparatus 200. In the electrode manufacturing apparatus 200, electrodes can be manufactured by a roll-to-roll method. The electrode manufacturing apparatus 200 includes a conveying apparatus 210, a coating apparatus 220, a first drying apparatus 230, a molding apparatus 240, and a second drying apparatus 250. The electrode manufacturing apparatus 200 may further include, for example, a compression apparatus 260, etc.

[0099] The electrode manufacturing apparatus 200 may further include, for example, a mixer (not shown) and the like. The mixer may prepare, for example, a slurry. The electrode manufacturing apparatus 200 may further include, for example, a cutting device (not shown) and the like. The cutting device may cut, for example, the compressed electrode into a predetermined shape. The electrode manufacturing apparatus 200 may further include, for example, a control device (not shown) and the like. The control device may control, for example, the operation and cooperation of each device.

[0100] <<Transportation device>> The conveying device 210 conveys the substrate 110. The conveying device 210 may include, for example, a feed roll 211 and a take-up roll 212. For example, the feed roll 211 feeds out the substrate 110. The take-up roll 212 takes up the substrate 110 (electrode 100). The substrate 110 may pass through each of the devices in the order of the coating device 220, the first drying device 230, the molding device 240, the second drying device 250, and the compression device 260.

[0101] <<Coating Equipment>> The coating device 220 coats the surface of the substrate 110 with the slurry. This can form a first coating film. The coating device 220 can coat the slurry by any method. The coating device 220 can include, for example, a die coater, a roll coater, or the like. The first coating film can be formed so that the second coating film has a dripping portion. For example, the slope and width of the dripping portion can be adjusted depending on the basis weight, viscosity, and the like of the slurry.

[0102] 《First drying device》 The first drying device 230 dries the first coating film to form a second coating film. The first drying device 230 can dry the first coating film so that the second coating film has a dripping portion. For example, the inclination and width of the dripping portion can be adjusted by the drying conditions (drying temperature, drying time, etc.). The first drying device 230 can dry the first coating film by any method. The first drying device 230 may include, for example, a hot air drying device, an infrared drying device, etc. The drying conditions are adjusted so that the solid phase, liquid phase, and gas phase form a pendular state or a funicular state in the second coating film.

[0103] 《Forming equipment》 The molding device 240 presses a convex mold against the surface of the second coating film to form a concave portion on the surface. The molding device 240 may include, for example, an embossing roll 241. One or more convex molds are formed on the surface of the embossing roll 241. Convex molds can be formed according to the pattern of the convex molds. For example, a ceramic layer may be formed on the surface of the embossing roll 241. The convex molds may be formed on the ceramic layer. By the contact portion with the active material layer being a ceramic layer, for example, the inclusion of metallic foreign matter in the active material layer can be reduced. The ceramic layer may include, for example, alumina, titania, etc. For example, the convex molds can be formed on the ceramic layer by laser engraving. For example, the depth of the concave portion can be adjusted by the height of the convex mold, etc. The convex mold may have a height of, for example, 50 to 200 μm. The core of the embossing roll 241 may be formed of, for example, stainless steel material, etc.

[0104] 《Second drying device》 The second drying device 250 dries the second coating film to form an active material layer. The second drying device 250 can dry the second coating film by any method. The second drying device 250 may include, for example, a hot air drying device, an infrared drying device, or the like. The drying conditions are adjusted so that the active material layer is in a dry state.

[0105] Compression Device The compression device 260 compresses the active material layer. The compression device 260 may compress the active material layer by any method. The compression device 260 may include, for example, a roll press device or the like. EXAMPLES

[0106] This embodiment will be described below.

[0107] <First test example> In the first test example, a positive electrode was produced.

[0108] (a) Preparation of Slurry The following materials were prepared: Active material particles: Li(Ni)1 / 3 Co 1 / 3 Mn 1 / 3 )O 2 Conductive material: Acetylene black Binder: PVDF Dispersion medium: NMP

[0109] A planetary mixer was prepared as a stirring device. 90 parts by mass of active material particles, 2 parts by mass of binder, and 8 parts by mass of conductive material were put into the stirring tank of the stirring device. Furthermore, a dispersion medium was put into the stirring tank so that the solid content rate of the slurry became 62.5%. The materials were mixed in the stirring tank to prepare a slurry.

[0110] (b) Coating An aluminum foil was prepared as a substrate. A die coater was prepared as a coating device. The slurry was applied to the surface of the substrate to form a first coating film.

[0111] 《(c) First drying》 The second coating film was formed by drying the first coating film (initial solid content: 62.5%). The solid content of the second coating film was 80%. The dry state of the second coating film was confirmed by the above-mentioned method. In the second coating film, the solid phase, liquid phase, and gas phase formed a pendular or funicular state. The target thickness of the second coating film was 150 μm.

[0112] (d) Embossing The embossing roll formed depressions on the surface of the second coating film. The height of the protrusions was 100 μm. The depressions were formed in a line pattern. That is, in plan view, a concave-convex structure was formed by a plurality of parallel lines. Each depression extended along the short side direction (width direction) of the second coating film. The depression pitch was 1 mm. The line pressure was 40 N / cm.

[0113] (e) Second Drying After the recesses were formed, the second coating film was dried to form an active material layer.

[0114] (f) Compression The active material layer was compressed by a roll press device. The linear pressure was 4 t / cm. In this manner, an electrode (positive electrode) was produced.

[0115] <Second test example> In a second test example, a negative electrode was produced.

[0116] (a) Preparation of Slurry The following materials were prepared: Active material particles: graphite Binder: CMC, SBR Dispersion medium: water

[0117] A planetary mixer was prepared as the stirring device. 98 parts by mass of active material particles and 2 parts by mass of binder (1 part by mass of CMC and 1 part by mass of SBR) were put into the stirring tank of the stirring device. Furthermore, a dispersion medium was put into the stirring tank so that the solid content rate of the slurry was 60%. The materials were mixed in the stirring tank to prepare a slurry.

[0118] (b) Coating A Cu foil was prepared as a substrate. A die coater was prepared as a coating device. A first coating film was formed by coating the surface of the substrate with the slurry.

[0119] 《(c) First drying》 The second coating film was formed by drying the first coating film (initial solid content: 60%). The solid content of the second coating film was 72%. The drying state of the second coating film was confirmed by the above-mentioned method. In the second coating film, the solid phase, liquid phase, and gas phase formed a pendular state or a funicular state.

[0120] (d) Embossing The embossing roll formed depressions on the surface of the second coating film. The depressions were formed in a line pattern. Each depression extended along the short side direction (width direction) of the second coating film. The depression pitch was 1 mm. The line pressure was 40 N / cm.

[0121] (e) Second Drying After the recesses were formed, the second coating film was dried to form an active material layer.

[0122] (f) Compression The active material layer was compressed by a roll press device. The linear pressure was 1 t / cm. In this manner, an electrode (negative electrode) was produced.

[0123] Third Test Example In the third test example, a positive electrode was produced. In the third test example, a coating was formed using wet powder instead of a slurry. The materials used were the same as those in the first test example.

[0124] A high-speed mixer (manufactured by EarthTechnica) was prepared as a stirring device. 90 parts by mass of active material particles, 2 parts by mass of binder, and 8 parts by mass of conductive material were charged into the stirring tank of the stirring device. In the stirring tank, the solid materials were mixed for 15 seconds. The rotation speed of the mixing blade was 4500 rpm. After mixing, liquid (NMP) was added so that the solid content rate was 90%. After the addition of the liquid, the materials were mixed in the stirring tank for 30 seconds. The rotation speed of the mixing blade was 300 rpm. The materials were mixed for an additional 2 seconds to finely disperse the materials. The rotation speed of the mixing blade was 4500 rpm.

[0125] A roll coater was prepared as a coating device. In the roll gap, the wet powder was compressed to form a sheet-like molded body. The molded body was transferred to the surface of the substrate to form a coating film. The edge of the coating film was shaped using a spatula-shaped scraping tool. Thereafter, embossing, drying, and compression were performed in the same manner as in the first test example to produce an electrode (positive electrode).

[0126] <Result> FIG. 8 shows cross-sectional and top surface images of the electrodes in the first to third test examples. In the first and second test examples, an active material layer was formed by coating a slurry. As shown in the cross-sectional images, a dripping portion (inclined portion) was formed at the end in the short side direction (X-axis direction). The dripping portion was formed over an area of ​​about 1 mm.

[0127] In the third test example, an active material layer was formed from wet powder particles. Furthermore, the coating film was scraped off at the end in the short direction (X-axis direction). As shown in the cross-sectional image, there were almost no dripping areas in the third test example. In the third test example, the deviation between the upper and lower surfaces of the active material layer was about 20 μm.

[0128] As shown in the top view images, in the first and second test examples, the recesses do not extend to the ends in the short direction (X-axis direction). This is thought to be because in the first and second test examples, dripping portions are formed at the ends in the short direction. No peeling or collapse of the active material layer (coating film) is observed at the ends in the short direction.

[0129] As shown in the top view image, in the third test example, the recesses extend to the ends in the short direction. This is thought to be because no dripping portion is formed. In the third test example, peeling and collapse of the active material layer occurred at the ends in the short direction.

[0130] FIG. 9 is a graph showing the relationship between the solid content and the drying time in the first test example. The horizontal axis of FIG. 9 indicates the drying time in "(c) First Drying". The vertical axis of FIG. 9 indicates the solid content immediately after "(c) First Drying". In the first test example (positive electrode), the formation of a pendular state or a funicular state was confirmed at a solid content of 80 to 99%. At a solid content of 80 to 99%, recesses of the desired shape were formed. The depth of the recesses was 60 to 80 μm. At a solid content of less than 80%, the material adhered to the convex shape, making it difficult to form recesses of the desired shape.

[0131] FIG. 10 is a graph showing the relationship between the solid content and the drying time in the second test example. The horizontal axis of FIG. 10 indicates the drying time in "(c) First Drying". The vertical axis of FIG. 10 indicates the solid content immediately after "(c) First Drying". In the second test example (negative electrode), the formation of a pendular state or a funicular state was confirmed at a solid content of 70 to 99%. At a solid content of 70 to 99%, recesses of the desired shape were formed. The depth of the recesses was 70 to 80 μm. At a solid content of less than 70%, the material adhered to the convex shape, making it difficult to form recesses of the desired shape.

[0132] <Additional Notes> The present embodiment and the present example also disclose the following "electrode." A substrate and an active material layer are included, the active material layer is formed on a surface of the substrate, the active material layer includes active material particles and a binder, a concave portion and a convex portion are formed on a surface of the active material layer, a ratio of a density of the active material particles in the protrusions to a density of the active material particles in the recesses is 0.7 to 1.0; In a plan view, the active material layer has a longitudinal direction and a lateral direction, In the short direction, an inclined portion (a dripping portion) is formed at an end portion of the active material layer. electrode.

[0133] The recess extends along the short side direction, The recess does not extend to the tip of the inclined portion (dripping portion). electrode.

[0134] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]

[0135] 1 active material particle, 2 dispersion medium, 3 gas, 100 electrode, 110 substrate, 120 active material layer, 120t thickness, 121 recess, 121d depth, 121p pitch, 122 protrusion, 123 center, 124 end, 125θ inclination angle, 125 liquid dripping portion, 200 electrode manufacturing device, 210 conveying device, 211 roll, 212 take-up roll, 220 coating device, 230 first drying device, 240 molding device, 241 embossing roll, 250 second drying device, 260 compression device.

Claims

1. (a) preparing a slurry by mixing active material particles, a binder, and a dispersion medium; (b) applying the slurry to a surface of a substrate to form a first coating; (c) drying the first coating film to form a second coating film; (d) forming recesses in the surface of the second coating film by pressing a convex mold against the surface; and (e) after forming the recesses, drying the second coating film to form an active material layer; Including, In the second coating film, the solid phase, the liquid phase and the gas phase form a pendular state or a funicular state. A method for manufacturing an electrode.

2. The slurry has a solids content of 50 to 65% by mass, The second coating film has a solid content of 70 to 99% by mass. A method for producing the electrode according to claim 1 .

3. The active material particles include a positive electrode active material, The slurry has a solids content of 55 to 65% by mass, The second coating film has a solid content of 80 to 99% by mass. A method for producing the electrode according to claim 1 or 2.

4. The active material particles include a negative electrode active material, The slurry has a solids content of 50 to 60% by mass, The second coating film has a solid content of 70 to 99% by mass. A method for producing the electrode according to claim 1 or 2.

5. In a plan view, the second coating film has a longitudinal direction and a lateral direction, A dripping portion is formed at an end of the second coating film in the short side direction, The convex mold is pressed against the second coating film so that at least a part of the dripping portion does not come into contact with the convex mold. A method for producing the electrode according to any one of claims 1 to 4.

6. (f) compressing the active material layer; Further comprising: A method for producing the electrode according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Secondary cell using nonaqueous electrolyte

    JP2003187875A

  • Electrode for lithium secondary battery, manufacturing method therefor, and the lithium secondary battery

    JP2008010253A

  • Lithium ion secondary battery manufacturing method

    JP2013229315A

  • Method for manufacturing negative electrode of nonaqueous electrolyte secondary battery, and device for manufacturing negative electrode of nonaqueous electrolyte secondary battery

    JP2015138619A

  • Method for manufacturing electrode material for lithium ion battery, and device for manufacturing electrode material for lithium ion battery