Device and method for mechanical and electrical contacting of glow wires of heat-resistant metallic thermal radiation sources for semiconductor and microsystem technology

A device with perforated glow wires and stud bumps forms stable connections for refractory metals, addressing embrittlement and material migration issues, enhancing service life and integration into microelectronic systems.

JP7554912B2Active Publication Date: 2024-09-20INFRASOLID GMBH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023510366
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-11
Filing Date
2021-07-30
Publication Date
2024-09-20
Estimated Expiration
2041-07-30

AI Technical Summary

Technical Problem

Existing technologies face challenges in creating reliable and long-term stable mechanical and electrical contact connections for glow wires made of refractory metals, which are prone to embrittlement and material migration at high temperatures, and are difficult to integrate into microelectronic systems using conventional methods.

Method used

A device and method involving a glow wire with perforations and/or cutouts on its connection surface, combined with wire-bonded stud bumps, forms a flange-like connection that mechanically and electrically attaches to a contact surface, using materials like gold or copper, ensuring stable connections at high temperatures.

Benefits of technology

The solution provides stable, long-term connections without embrittlement or material migration, extending the service life of thermal radiation sources and enabling easy integration into microelectronic systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554912000008
    Figure 0007554912000008
  • Figure 0007554912000005
    Figure 0007554912000005
  • Figure 0007554912000001
    Figure 0007554912000001
Patent Text Reader

Abstract

The present invention discloses an apparatus for mechanical and electrical contacting of a glow-wire of a thermal radiation source, the apparatus comprising a glow-wire made of a heat-resistant metal with at least one flat contacting surface to be contacted, the contacting surface on which the glow-wire is contacted, and a contacting means for connecting the glow-wire to the contacting surface. The present invention also discloses a method for forming the contacting according to the present invention. The object of the present invention is to provide a reliable and long-term stable mechanical and electrical contacting of a glow-wire made of a heat-resistant metal, in which the flat contacting surface of the glow-wire has at least two perforations and / or at least two notches formed in the circumferential edge of the contacting surface of the glow-wire, the contacting means being connected in a material-tight manner to the contacting surface at the perforations and / or the notches, and the flange-shaped design of the contacting means above the contacting surface of the glow-wire allows both an electrical and a mechanical connection to be made at the perforations and / or the notches.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to a device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to the preamble of claim 1, which device comprises a glow-wire made of a heat-resistant metal with at least one flat connection surface to be contacted, a contacting surface on which the glow-wire is contacted and contacting means for connecting the glow-wire to the contacting surface.

[0002] The invention likewise relates to a method for producing the contact connection according to the invention.

[0003] The radiation power of a thermal radiation source is proportional to the fourth power of its absolute temperature and is described by the Stefan-Boltzmann law. Therefore, for high radiation power, the glow-wire of the thermal radiation source must have as high a temperature as possible. This requires materials with a very high melting point. In particular, refractory metals, i.e. base metals with high melting points, such as tungsten, tantalum or molybdenum, are suitable for this.

[0004] The most well-known thermal radiation source is the incandescent lamp, in which a glow wire made of tungsten is heated by an electric current, excited and emits light. The temperature of the glow wire is about 1500 ° C to 3000 ° C depending on the design. In this case, the high temperature and the current flow at the contact connection point can lead to material migration. Here, base material creeps along the glow wire and reacts chemically with it. This leads to embrittlement and the formation of certain destruction points that shorten the service life of the thermal radiation source. Destruction occurs at these embrittled points, especially when switching on or off. Therefore, the correct material selection of the two joining partners, the glow wire and the contact point, should be taken into account. US Patent No. 2,145,186, for example, discloses an incandescent lamp in a sealed bulb, in particular the mechanical fixation of the filament to the internal lead-in.

[0005] Due to passivation, refractory metals are relatively corrosion-resistant at room temperature. However, at high temperatures, refractory metals react very easily with many nonmetals and gases, which places very high demands on the purity and tightness of the housing as well as on the electrical contact connection. A reliable and long-term stable electrical contact connection of the glow wire at very high temperatures is achieved by a welded joint, often by so-called resistance spot welding. In resistance spot welding, the atoms of the two joining parts interact with each other chemically or metallurgically, forming a strong and consistent joint, so that the metals bond. Exemplary welded joints between glow wires and feedthroughs are disclosed in US Pat. No. 1,477,618, DE-A-102004,061,736, DE-A-2200736 and DE-A-735,789. Similarly, U.S. Pat. No. 4,370,589 discloses a welded joint between the filament and lead-in of an electric incandescent lamp in which the inner end of the lead-in is serrated and welded to the end of the filament so that the filament and lead-in are fused to each other at multiple points which provide a strong, reliable electrical connection.

[0006] However, not all materials can be joined together equally well by resistance spot welding due to their physical properties and interactions with the electrode material. Ideal material properties for resistance spot welding are: -Same or close melting points -Low electrical conductivity -Low thermal conductivity -High deformability (thermal deformation)

[0007] Such situations are rarely encountered in practical welding tasks. Moreover, hard and brittle materials such as refractory metals tend to form fractures during the welding and cooling processes, which affects the quality and reliability of the electrical contact connection.

[0008] Moreover, welding is not a standard process in microelectronics and microsystems technology - common methods here are, for example, wire bonding and flip-chip bonding.

[0009] In wire bonding, a terminal of one component 5 is connected to an electrical terminal 4 of another component or housing by means of a thin wire (bonding wire) (see FIGS. 1 and 2). Gold, aluminum or copper are often used as the bonding material. A very frequently applied wire bonding method is the so-called ball wedge bonding. Here, the end of the bonding wire 2 protruding downwards from the capillary 1 of the wire bonding device is slightly melted, as a result of which a sphere (ball) 3 is formed by surface tension. This sphere 3 is bonded onto the contact connection surface 4 by means of pressure, heat and ultrasound, resulting in a so-called ball bond 6. In the case of ball wedge bonding, the bonding wire 2 is pulled and bonded to the other contact connection surface 4 (see FIG. 2). However, this is omitted in the case of the so-called ball bond, which is a special form of ball wedge bonding shown in FIG. 1. Here, after the first ball bond 6, the wire clamp in the capillary 1 is closed and the bonding wire 2 is cut off in the immediate vicinity of the bonded sphere when the capillary 1 rises. This results in spherical protuberances, so-called bumps, on the contact surface 4. These are also called stud bumps 7. This method is used, among others, in flip-chip mounting. DE 1 949 869 A1 describes a method for joining a filament to a metallic lead-in wire, in which the metal bead is heated to a plastic or semiplastic state and is pressed against the lead-in wire and the filament that lies above it. The intermetallic or metallurgical bond is produced here by diffusion at the interface between the metal bead and the lead-in wire.

[0010] Aluminum is not suitable for contacting a glow wire made of a heat-resistant metal, since it is a very noble metal and, moreover, has a very low melting point.

[0011] The noble metal gold is frequently used in microelectronics and microsystems technology as conductor tracks, especially as bonding wires, and for contacting surfaces, because gold has excellent electrical and thermal properties, is very easy to process, has high corrosion resistance, and can be easily soldered. However, the high electrical and thermal conductivity of gold limits its weldability. Reliable, long-term stable welded connections with heat-resistant metals are not possible.

[0012] In recent years, bonding with copper wires has gradually begun to be implemented, among other things due to the enormous cost advantages. However, copper wires also offer further advantages over gold wires: the direct current resistance and thermal conductivity are better than in the case of gold wires. Furthermore, copper has a relatively high mechanical stability at high temperatures and a better reliability of the contact connection. However, a disadvantage is the rapid surface oxidation of copper, which begins already at room temperature. If the copper oxide layer is too thick, bonding is no longer possible, since the material is too hard. Furthermore, in this case, the bonding wire ends can no longer be formed into spheres (balls) by slight melting, which is necessary for the formation of stud bumps. It is therefore important to protect the copper wires from oxidation. This requires corresponding oxygen-free storage and processing of the copper bonding wires. As with gold, reliable and long-term stable welded connections with heat-resistant metals are not possible with copper either.

[0013] Even with the described known contact connection forms of wire bonding for microelectronic components, hard and brittle materials such as heat-resistant metals cannot be directly contacted with gold, copper or aluminum wires in a reliable and long-term stable manner.

[0014] The object of the present invention is therefore to provide a reliable and long-term stable mechanical and electrical contacting of a glow wire made of a heat-resistant metal, which can also be produced by the usual methods of microelectronics and microsystems technology, and which allows for easy integration, for example, into microelectronic, optoelectronic or micro-optoelectronic mechanical systems (MOEMS) and makes it possible to achieve a high degree of automation.

[0015] The above-mentioned object is achieved by a device for mechanical and electrical contacting of a glow-wire of a thermal radiation source, as described in the independent device claim. According to the invention, the flat connection surface of the glow-wire has at least two perforations and / or at least two recesses are formed on the circumferential edge of the connection surface of the glow-wire, the contact means is connected in a material-tight manner with the contact surface at the perforations and / or the recesses, and by the flange-like formation of the contact means above the connection surface of the glow-wire, both the electrical and mechanical connection with the glow-wire is formed at the perforations and / or the recesses. A flat connection surface means a part of the glow-wire that lies planarly and flat on the contact surface, the extension of the connection surface in the plane being significantly greater than its thickness.

[0016] Particularly advantageously, perforations and / or recesses in the connection surface of the glow-wire are used to clamp and thus fix the glow-wire with a wire-bonded sphere, a so-called stud bump, on the flat contact surface. The connection formed allows the glow-wire made of heat-resistant metal to be reliably contacted, both electrically and mechanically, to the contact surface. By structural modifications of the flat connection surface of the glow-wire in combination with the known ball bonding, heat-resistant metals, which up until now could only be contacted without long-term stability or at great expense, can be contacted reliably, long-term and without great expense using established and highly automated methods of semiconductor technology and microsystem technology.

[0017] Wire-bonded spheres, known in semiconductor technology and microsystem technology as stud bumps, form a material-tight connection with the contact surface by pressure, heat and ultrasound, and the bonding ball is a flattened sphere in cross section. In the device according to the invention, such a flange-like flattening is used for mechanical clamping of the connection surface of the glow-wire to the contact surface, similar to a rivet connection. An electrical connection is also formed by the surface-like contact connection of the connection surface of the glow-wire with the stud bump in the perforations and / or in the recesses at the edge of the connection surface of the glow-wire. During operation of the thermal radiation source with the contact connection according to the invention, a thermal expansion of the glow-wire and the contact means additionally occurs, so that the contact resistance between the connection surface of the glow-wire and the contact surface approaches zero.

[0018] The advantage over the previously known contacting of refractory metals is, in particular, that with the device according to the invention no embrittlement of the contacting points of the refractory metal occurs, no material transfer occurs anymore and thus the service life of components with contacting points made of refractory metal can be significantly extended. Such contacting configurations can be produced very easily by established and highly automated methods of semiconductor and microsystem technology and can therefore be easily integrated into the manufacturing processes of microelectronic, optoelectronic or micro-optoelectronic mechanical systems (MOEMS) to which the refractory metals have to be contacted.

[0019] In one configuration of the device according to the invention, the perforations are circular, triangular (n=3), rectangular (n=4) and / or n-sided, where n is a natural number greater than 2. Depending on the size of the stud bump in relation to the diameter of the bonding wire and the process parameters during wire bonding, the mechanical and electrical contacting can be optimized. Typical bonding wire diameters are in the range of (10...50) μm. This results in stud bumps with diameters typically less than 100 μm. The diameter of the perforations and the notches must be smaller than the diameter of the stud bump in order to be able to perform a reliable clamping.

[0020] In further configurations of the device according to the invention, the recesses are triangular (n=3), rectangular (n=4), trapezoidal (n=4), arcuate and / or n-sided, where n is a natural number greater than 2. Depending on the size of the stud bump in relation to the diameter of the bonding wire and the process parameters during wire bonding, the mechanical and electrical contact can be optimized.

[0021] The connection surface of the glow-wire may have both perforations and recesses or may have perforations and recesses whose shapes can be freely combined.

[0022] In a further embodiment of the contact according to the invention, the contacting surfaces and the contacting means preferably consist of gold and / or copper. Gold and copper have excellent electrical and thermal properties and are very easy to process. Gold in particular is moreover highly corrosion-resistant and can be easily soldered.

[0023] In a further configuration of the contact according to the invention, the heat-resistant metal of the glow-wire is tungsten or tantalum, which are preferably used in thermal radiation sources with high radiation power, since these materials have a very high melting point.

[0024] In one configuration of the contact connection according to the invention, the glow-wire can be heated to temperatures above 700 ° C without chemical reactions between the glow-wire and the contact connection points. The contact connection points represent the points at which the contact connection means is connected in a material-connecting manner with the contact connection surface and where a mechanical and electrical connection is made between the connection surface of the glow-wire and the contact connection surface by means of the perforations and / or cutouts. This is only possible by a combination of a modified connection surface of the glow-wire and the bonding of the contact connection means at the perforations and / or cutouts with the underlying contact connection surface. Since the glow-wire made of a heat-resistant metal is not chemically bonded to the contact connection surface, at very high temperatures above 700 ° C, no material flow or material transfer occurs anymore between the heat-resistant metal and the material of the contact connection means. Creep of base materials along the glow-wire and chemical reactions with the glow-wire are thus prevented. Embrittlement and the formation of certain fracture points, which shorten the service life of the thermal radiation source, no longer occur.

[0025] The above-mentioned object is also achieved by a method for producing a device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to one of claims 1 to 6, in which the contacting means is applied to the contacting surface at the location of the perforation and / or cut-out by means of wire bonding and the contacting means is detached at the location of the perforation and / or cut-out directly above an upper flange-like protrusion of the connecting surface of the glow-wire.

[0026] The device and device fabrication according to the present invention are intended for, suitable for and adapted for use in semiconductor and microsystems technology.

[0027] Hereinafter, the present invention will be described in more detail based on examples. [Brief description of the drawings]

[0028] [Figure 1] 1 shows a ball bonding method known from flip-chip mounting for producing spherical bumps, so-called stud bumps, on a flat contact-connection surface; [Diagram 2] 1 shows a contact topology for wire bonding in microelectronic components as known from the prior art; [Diagram 3] 1A-1D show embodiments of the connection surface of a glow-wire with perforations according to the present invention, where (a) a circular perforation, (b) a triangular perforation, (c) a square perforation, and (d) an n-gonal perforation. [Figure 4] 1A-1D show embodiments of the connection surface of a glow-wire with notches according to the present invention, here (a) triangular notches, (b) square notches, (c) trapezoidal notches, and (d) a combination of different notches. [Diagram 5] 1A-1C show embodiments of a glow-wire connection surface made of a heat-resistant metal with perforations and notches according to the present invention, where (a) is a circular perforation and a trapezoidal notch, and (b) is a circular perforation and a triangular notch. [Figure 6] FIG. 2 shows an embodiment according to the invention of a contact connection of a glow wire made of heat-resistant metal by means of a stud bump. [Figure 7] FIG. 2 shows a cross section of a contact according to the invention of a glow-wire on a contact surface at one perforation and two cutouts.

[0029] 3 shows an embodiment of the connection surface 10 according to the invention of a glow-wire with different shapes of perforations. Depending on the size of the stud bump 7, i.e. the size of the contacting means, which is related to the diameter of the bonding wire and the process parameters during wire bonding, the mechanical and electrical contacting can be optimized.

[0030] 4 shows further embodiments of the connection surface 10 of the glow-wire according to the invention with differently shaped cutouts. Depending on the size of the stud bump 7 in relation to the diameter of the bonding wire and the process parameters during wire bonding, the mechanical and electrical contacting can be optimized.

[0031] FIG. 5 shows preferred embodiments of the connection surface 10 of the glow-wire according to the invention with different shapes of perforations 11 and recesses 17. Since the diameter of the bonding wire cannot be made arbitrarily small, the combination of perforations 11 and recesses 17 is advantageous especially when the area of ​​the contact connection points is very small, because in this way it becomes possible to make more contact connection points. By providing the first stud bump 7 in the perforation 11, the glow-wire is fixed and prevented from shifting. Here, the further stud bump 7 in the recess 17 provides the required mechanical stability and a good electrical contact connection.

[0032] 6 shows a preferred embodiment of the contact connection according to the invention between a structured connection surface 10 of a glow-wire made of heat-resistant metal and a bonded stud bump 7. Particularly advantageously, perforations 11 and / or recesses 17 in the connection surface 10 of the glow-wire are used to clamp and thus fix the glow-wire with the wire-bonded sphere, i.e. the stud bump 7, on the flat contact connection surface 4. Due to the connection formed, the glow-wire made of heat-resistant metal is contact-connected reliably, both electrically and mechanically, to the contact connection surface 4. Such a connection can be formed reliably, reliably and without great costs in the long term.

[0033] The stud bump 7, which is made of, for example, gold or copper, forms a material-tight connection with the contacting surface 4, which is also made of, for example, gold or copper, and the bonded bonding ball 3, seen in cross section, is a flattened sphere 18 with a cut-off bonding wire end 19 (FIG. 7). Such a flange-like flattening 18 is used for mechanical clamping of the connection surface 10 of the glow-wire to the contacting surface 4, similar to a rivet connection. An electrical connection is also formed by the surface-like contact connection of the connection surface 10 of the glow-wire with the stud bump 7 in the perforations 11 and / or in the recesses 17 at the edge of the connection surface 10 of the glow-wire. During operation of the thermal radiation source with the contacting according to the invention, a thermal expansion of the glow-wire and the contacting means (for example a gold wire) additionally occurs, so that the contact resistance between the connection surface 10 of the glow-wire and the contacting surface 4 approaches zero.

[0034] The advantage over previously known contacts made of refractory metals is, in particular, that with the device according to the invention embrittlement of the contacts does not occur, material transfer no longer occurs and thus the service life of components with contacts made of refractory metals can be significantly extended. Extensive passivation of contacts etc. is dispensed with. [Explanation of symbols]

[0035] 1. Capillary of wire bonding equipment 2 Bonding Wire 3. Ball 4 Contact surface, electrical terminal 5. Components 6 Ball bonding 7 Stud Bump 8 Substrate 9. Wedge Bonding 10 Glow Wire Connection Surface / Contact Surface 11 Circular perforation 12 Triangular perforation 13 Square perforated section 14 n-gonal perforation 15 Triangular notch 16 Square notch 17 Trapezoidal notch 18 Flattened sphere 19 Separated bonding wire

Claims

1. 1. A device for mechanical and electrical contacting of a glow-wire of a thermal radiation source, comprising: A device comprising a glow-wire made of heat-resistant metal with at least one flat connection surface (10) to be contacted, a contact surface (4) on which the glow-wire is contacted, and contacting means (7) for connecting the glow-wire to the contact surface (4), the flat connection surface (10) of the glow-wire has at least two perforations (11, 12, 13, 14) and / or at least two notches (15, 16, 17) are formed in the circumferential edge of the connection surface (10) of the glow-wire, the contact-connection means (7) is connected in a material-tight manner with the contact-connection surface (4) at the location of the perforations (11, 12, 13, 14) and / or the recesses (15, 16, 17) and, by means of a flange-shaped formation (18) of the contact-connection means (7) above the connection surface (10) of the glow-wire, both an electrical and a mechanical connection with the glow-wire is formed at the location of the perforations (11, 12, 13, 14) and / or the recesses (15, 16, 17), 13. An apparatus for mechanical and electrical contacting of a glow-wire of a thermal radiation source, comprising:

2. 2. The device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, wherein the perforations are formed in the shape of a circle (11), a triangle (12), a square (13) and / or an n-gon (14).

3. 2. The device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, wherein the recess is formed in the shape of a triangle (15), a square (16), a trapezoid (17), a circular arc and / or an n-gon.

4. 2. The device for the mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, wherein the contacting surface (4) and the contacting means (7) preferably consist of gold and / or copper.

5. 2. An apparatus for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, wherein the refractory metal of the glow-wire is tungsten or tantalum.

6. 2. The device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, characterized in that the glow-wire can be heated to temperatures of more than 700° C. without chemical reactions occurring between the glow-wire and the contacting surface (4).

7. 7. A method for manufacturing a device for mechanical and electrical contacting of a glow-wire of a thermal radiation source according to claim 1, comprising the steps of: applying the contact-connecting means (7) to the contact-connecting surface (4) at the location of the perforations (11, 12, 13, 14) and / or the notches (15, 16, 17) by means of wire bonding and detaching the contact-connecting means (7) at the location of the perforations and / or the notches directly above the upper flange-like projection of the connection surface (10) of the glow-wire.

13. A method for manufacturing a device for mechanical and electrical contacting of a glow-wire of a thermal radiation source, comprising the steps of:

Citation Information

Patent Citations

  • Electron gun

    JP1982036750A

  • Manufacture of semiconductor device

    JP1983091649A

  • An intake air heating device

    JP1984188966U

  • Semiconductor device and its manufacture

    JP1991044050A

  • Lead frame and method of connecting lead frame with semiconductor device

    JP1992026149A