Electrolyte for lithium-sulfur secondary battery and lithium-sulfur secondary battery including the same

The electrolyte solution for lithium-sulfur secondary batteries, comprising specific ether solvents and a compound represented by Chemical Formula 1, addresses electrolyte decomposition issues, enhancing battery life and performance by forming a stable SEI film.

JP7556056B2Active Publication Date: 2024-09-25LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022575452
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2021-10-27
Publication Date
2024-09-25
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

Lithium-sulfur secondary batteries face issues with electrolyte decomposition, leading to reduced life characteristics due to the elution of lithium polysulfide, dendrite growth, and accumulation of byproducts, especially when using ether-based solvents, which also affect performance and longevity, particularly in high-energy density applications.

Method used

An electrolyte solution for lithium-sulfur secondary batteries containing a lithium salt and a non-aqueous solvent comprising an ether solvent and a non-solvent, with specific compositions of linear and cyclic ethers, and a compound represented by Chemical Formula 1, which prevents electrolyte decomposition and improves battery performance.

Benefits of technology

The proposed electrolyte solution effectively prevents electrolyte decomposition, enhances lithium ion mobility, and significantly improves battery life characteristics by forming a stable SEI film, ensuring high stability and long-term operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556056000001
    Figure 0007556056000001
  • Figure 0007556056000002
    Figure 0007556056000002
  • Figure 0007556056000003
    Figure 0007556056000003
Patent Text Reader

Abstract

The present invention relates to an electrolyte for a lithium-sulfur secondary battery and a lithium-sulfur secondary battery including the same. The present invention provides an electrolyte for a lithium-sulfur secondary battery including a lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent includes an ether-based solvent and a non-solvent, the ether-based solvent includes a linear ether and a cyclic ether, and the non-solvent includes a compound having a specific structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2020-0143315, filed October 30, 2020, Korean Patent Application No. 10-2020-0143326, and Korean Patent Application No. 10-2021-0143351, filed October 26, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to an electrolyte for a lithium-sulfur secondary battery and a lithium-sulfur secondary battery including the same. [Background technology]

[0003] As the application area of ​​secondary batteries expands to electric vehicles (EVs) and energy storage systems (ESSs), lithium-ion secondary batteries, which have a relatively low energy storage density relative to weight (~250Wh / kg), have limitations in their application to such products. In contrast, lithium-sulfur secondary batteries are in the spotlight as a next-generation secondary battery technology because they can theoretically realize a high energy storage density relative to weight (~2,600Wh / kg).

[0004] Lithium-sulfur secondary batteries refer to battery systems that use sulfur-based materials with S-S bonds as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur, the main material of the positive electrode active material, is an abundant resource worldwide, and has the advantages of being non-toxic and having a low atomic weight.

[0005] During discharge, lithium, the negative electrode active material, loses electrons and is oxidized while ionizing, while the positive electrode active material, the sulfur-based material, receives electrons and is reduced. Here, the lithium oxidation reaction is the process in which lithium metal loses electrons and is converted into lithium cation form. Meanwhile, the sulfur reduction reaction is the process in which the S-S bond receives two electrons and is converted into sulfur anion form. The lithium cations produced by the lithium oxidation reaction are transferred to the positive electrode via the electrolyte and combine with the sulfur anions produced by the sulfur reduction reaction to form a salt. Specifically, sulfur before discharge has a cyclic S8 structure, which is reduced to lithium polysulfide (LiS x When the lithium polysulfides are completely reduced, lithium sulfide (Li2S) is produced.

[0006] Sulfur, the positive electrode active material, has low electrical conductivity, making it difficult to ensure reactivity with electrons and lithium ions in the solid state. In order to improve the reactivity of sulfur, existing lithium-sulfur secondary batteries use Li2S x In this case, an ether solvent such as dioxolane or dimethoxyethane, which has high solubility in lithium polysulfide, is used as the electrolyte solvent.

[0007] However, when such an ether-based solvent is used, there are problems in that the life characteristics of the lithium-sulfur secondary battery are deteriorated due to various reasons, such as the elution of lithium polysulfide from the positive electrode, the occurrence of shorts due to the growth of dendrites on the lithium negative electrode, and the accumulation of by-products due to the decomposition of the electrolyte.

[0008] In particular, when such an ether-based solvent is used, lithium polysulfide can be dissolved in a large amount, resulting in high reactivity. However, due to the characteristics of lithium polysulfide dissolved in the electrolyte, the reactivity and life characteristics of sulfur are affected by the content of sulfur in the electrolyte.

[0009] In recent years, in order to develop lithium-sulfur secondary batteries with high energy density of 500Wh / kg or more required for aircraft and next-generation electric vehicles, it is required that the sulfur loading amount in the electrode is large and the electrolyte content is minimized.

[0010] However, due to the characteristics of the ether-based solvent, the lower the content of the electrolyte, the more rapidly the viscosity increases during charging and discharging, which can cause overvoltage and degradation.

[0011] Therefore, research has been continuously conducted on adding a non-solvent as a solvent for the electrolyte to prevent the electrolyte from decomposing and ensure excellent life characteristics. Nevertheless, the components and composition of the electrolyte that can prevent the electrolyte from decomposing and improve the life characteristics have not been clearly clarified. In particular, the components and composition of the electrolyte suitable for pouch cells and the like that have an extremely small electrolyte content have not been specifically known. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Korean Patent Publication No. 10-2007-0027512 (March 9, 2007), "Electrolyte for Lithium-Sulfur Electrochemical Battery" Summary of the Invention [Problem to be solved by the invention]

[0013] Therefore, in the present invention, in order to prevent decomposition of an electrolyte solution of a lithium-sulfur secondary battery and improve its life characteristics, it has been confirmed that the above problems can be solved and the performance of a lithium-sulfur secondary battery can be improved by providing an electrolyte solution for the lithium-sulfur secondary battery containing a lithium salt and a non-aqueous solvent, and the non-aqueous solvent contains an ether-based solvent and a non-solvent, thereby completing the present invention.

[0014] It is therefore an object of the present invention to provide an electrolyte for a lithium-sulfur secondary battery capable of preventing decomposition of the electrolyte and improving the life characteristics, and to provide a lithium-sulfur secondary battery having improved performance by including the electrolyte. [Means for solving the problem]

[0015] In order to achieve the above object, the present invention provides an electrolyte solution for a lithium-sulfur secondary battery, comprising a lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises an ether-based solvent and a non-solvent, the ether-based solvent comprises a linear ether and a cyclic ether, and the non-solvent comprises a compound represented by the following Chemical Formula 1:

[0016] [ka]

[0017] [In the above Chemical Formula 1, The Rfs may be the same or different, and each independently represents an alkyl group having 1 to 3 carbon atoms substituted with fluorine.] The present invention also relates to a method for producing a lithium salt, the method comprising the steps of: 10 Cl 10The present invention provides an electrolyte solution for a lithium-sulfur secondary battery, which is one or more selected from the group consisting of LiB(Ph)4, LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate, and lithium imide.

[0018] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the linear ether is selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethyl propyl ether, ethyl tert-butyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol tert-butyl ethyl ether, and ethylene glycol ethyl methyl ether.

[0019] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the cyclic ether is selected from the group consisting of dioxolane, methyldioxolane, dimethyldioxolane, vinyldioxolane, methoxydioxolane, ethylmethyldioxolane, oxane, dioxane, trioxane, tetrahydrofuran, methyltetrahydrofuran, dimethyltetrahydrofuran, dimethoxytetrahydrofuran, ethoxytetrahydrofuran, dihydropyran, tetrahydropyran, furan, and 2-methylfuran.

[0020] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the fluoroalkyl group of the formula 1 is a C1 to C3 fluoroalkyl group substituted with 1 to 7 fluorines.

[0021] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the fluoroalkyl group of the formula 1 is a C1-C2 fluoroalkyl group substituted with 1 to 5 fluorines.

[0022] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the fluoroalkyl group of Formula 1 has a difluoromethyl group or a trifluoromethyl group at its terminal.

[0023] The present invention also provides an electrolyte solution for a lithium-sulfur secondary battery, wherein the content of the non-solvent is 5 vol % to 20 vol % based on the total volume of the non-aqueous solvent.

[0024] The present invention also provides an electrolyte solution for a lithium-sulfur secondary battery, wherein the content of the linear ether is 50% by volume to 90% by volume with respect to the total volume of the nonaqueous solvent, and the content of the cyclic ether is 10% by volume to 30% by volume with respect to the total volume of the nonaqueous solvent.

[0025] The present invention also provides an electrolyte solution for a lithium-sulfur secondary battery, in which the volume ratio of the ether solvent to the non-solvent is 95:5 to 80:20.

[0026] The present invention also provides an electrolyte solution for a lithium-sulfur secondary battery, wherein the volume ratio of the linear ether to the cyclic ether is 9:1 to 5:5.

[0027] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the linear ether is dimethoxyethane.

[0028] The present invention also provides an electrolyte for a lithium-sulfur secondary battery, wherein the cyclic ether is 2-methylfuran.

[0029] In addition, the present invention provides an electrolyte for a lithium-sulfur secondary battery, wherein the compound represented by Chemical Formula 1 is tris(2,2-difluoroethyl)orthoformate or tris(2,2,2-trifluoroethyl)orthoformate.

[0030] The present invention also provides a lithium-sulfur secondary battery comprising the electrolyte, a positive electrode, a negative electrode, and a separator. Effect of the Invention

[0031] The electrolyte for a lithium-sulfur secondary battery according to the present invention includes a lithium salt and a non-aqueous solvent, the non-aqueous solvent includes an ether-based solvent and a non-solvent, the ether-based solvent includes a linear ether and a cyclic ether, and the non-solvent includes a compound having a specific structure, thereby preventing decomposition of the electrolyte during operation of the lithium-sulfur secondary battery and improving the life characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The embodiments provided by the present invention can all be achieved by the following description. It should be understood that the following description describes preferred embodiments of the present invention, and that the present invention is not necessarily limited thereto.

[0033] The present invention provides an electrolyte solution for a lithium-sulfur secondary battery, comprising a lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises an ether-based solvent and a non-solvent, the ether-based solvent comprises a linear ether and a cyclic ether, and the non-solvent comprises a compound represented by the following Chemical Formula 1:

[0034] [ka]

[0035] [In the above Chemical Formula 1, The Rf's may be the same or different, and each independently represents a C1 to C3 fluorinated alkyl group.] The electrolyte for a lithium-sulfur secondary battery of the present invention may include a lithium salt and a non-aqueous solvent. The lithium salt is a material that is easily dissolved in a non-aqueous organic solvent, and may be LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiB(Ph)4, LiC4BO8, LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, LiSO3CH3, LiSO3CF3, LiSCN, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SO2F)2, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate and lithium imide, and preferably LiN(CF3SO2)2.

[0036] The concentration of the lithium salt may be 0.2-2M, specifically 0.5-1.8M, more specifically 0.6-1.7M, depending on various factors such as the exact composition of the electrolyte mixture, the solubility of the salt, the conductivity of the dissolved salt, the charge and discharge conditions of the battery, the operating temperature, and other factors known in the lithium battery art. If less than 0.2M is used, the conductivity of the electrolyte may be reduced, which may reduce the performance of the electrolyte, and if more than 2M is used, the viscosity of the electrolyte may increase, which may reduce the mobility of the lithium ions (Li+).

[0037] The non-aqueous solvent may include ethereal solvents and non-aqueous solvents, and the ethereal solvent may include linear ethers and cyclic ethers.

[0038] The linear ether may be selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethyl propyl ether, ethyl tert-butyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol tert-butyl ethyl ether, and ethylene glycol ethyl methyl ether, and may be preferably dimethoxyethane.

[0039] The cyclic ether may be selected from the group consisting of dioxolane, methyldioxolane, dimethyldioxolane, vinyldioxolane, methoxydioxolane, ethylmethyldioxolane, oxane, dioxane, trioxane, tetrahydrofuran, methyltetrahydrofuran, dimethyltetrahydrofuran, dimethoxytetrahydrofuran, ethoxytetrahydrofuran, dihydropyran, tetrahydropyran, furan and 2-methylfuran, and may be preferably 2-methylfuran.

[0040] The non-solvent may include a compound represented by the following Chemical Formula 1:

[0041] [ka]

[0042] [In the above Chemical Formula 1, The Rf's may be the same or different, and each independently represents a C1 to C3 fluorinated alkyl group.] The compound represented by Chemical Formula 1 does not solvate lithium ions and exhibits a high flash point of 150° C. or more and a low viscosity of 5 cP or less. Specifically, the compound represented by Chemical Formula 1 exhibits the effect of reducing flammability and viscosity. As a result, it is possible to prevent deterioration of the electrolyte, improve the mobility of lithium ions, and ensure high stability even during long-term operation of the battery.

[0043] The fluorinated alkyl group of Chemical Formula 1 may be a C1-C3 fluorinated alkyl group substituted with 1 to 7 fluorines, preferably a C1-C2 fluorinated alkyl group substituted with 1 to 5 fluorines, and more preferably a fluorinated alkyl group containing a difluoromethyl group or a trifluoromethyl group at the terminal of the fluorinated alkyl group.

[0044] The compound represented by Chemical Formula 1 may be a trialkyl orthoformate-based compound substituted with fluorine, and the three alkyl groups in the trialkyl orthoformate-based compound may each independently be an alkyl group having 1 to 3 carbon atoms, preferably an alkyl group having 1 to 2 carbon atoms. The alkyl groups may each independently be a fluorinated alkyl group substituted with 1 to 7 fluorines, preferably a fluorinated alkyl group substituted with 1 to 5 fluorines, and more preferably an alkyl group substituted with a difluoromethyl group or a trifluoromethyl group at the terminal. Specifically, the compound represented by Chemical Formula 1 may be tris(2,2-difluoroethyl)orthoformate or tris(2,2,2-trifluoroethyl)orthoformate.

[0045] In addition, the electrolyte for lithium-sulfur secondary batteries of the present invention contains an ether-based solvent and a non-solvent as a non-aqueous solvent, thereby preventing decomposition of the electrolyte for lithium-sulfur secondary batteries and improving life characteristics. In particular, the electrolyte contains a linear ether and a cyclic ether as the ether-based solvent and a compound represented by Chemical Formula 1 as the non-solvent, thereby significantly improving the life characteristics of the battery.

[0046] In this case, the content of the non-solvent may be 5% by volume to 20% by volume, and preferably 5% by volume to 10% by volume, based on the total volume of the non-aqueous solvent, and the volume ratio of the ether solvent to the non-solvent may be 99:1 to 50:50, and preferably 95:5 to 70:30, and more preferably 95:5 to 80:20.

[0047] If the content of the non-solvent and the volume ratio of the ether-based solvent to the non-solvent are less than the above range, the effect of improving the life characteristics will be insufficient, and if the content of the non-solvent and the volume ratio of the ether-based solvent to the non-solvent exceed the above range, a problem may occur in which discharge is impossible at a high current density. Therefore, it is preferable that the content of the non-solvent and the volume ratio of the ether-based solvent to the non-solvent satisfy the above range.

[0048] The content of the linear ether may be 50% by volume to 90% by volume, preferably 60% by volume to 80% by volume, and more preferably 60% by volume to 75% by volume, based on the total volume of the non-aqueous solvent. The content of the cyclic ether may be 10% by volume to 30% by volume, and preferably 15% by volume to 25% by volume, based on the total volume of the non-aqueous solvent.

[0049] The volume ratio of the linear ether to the cyclic ether may be 9:1 to 1:9, preferably 8:2 to 2:8, and more preferably 7:3 to 3:7.

[0050] The volume ratio of the linear ether to the non-solvent may be 20:1 to 1:1, preferably 15:1 to 5:1, and more preferably 15:1 to 3:1. The volume ratio of the cyclic ether to the non-solvent may be 1:10 to 10:1, preferably 1:5 to 5:1, and more preferably 1:4 to 1:1.

[0051] If the content of linear ether, the content of cyclic ether, the volume ratio of linear ether to cyclic ether, the volume ratio of linear ether to non-solvent, and the volume ratio of cyclic ether to non-solvent are outside the above ranges, the effect of improving the battery life characteristics will be insufficient and the desired effect will not be obtained, so it is preferable that the content of linear ether, the content of cyclic ether, the volume ratio of linear ether to cyclic ether, the volume ratio of linear ether to non-solvent, and the volume ratio of cyclic ether to non-solvent satisfy the above ranges.

[0052] The electrolyte for lithium-sulfur secondary batteries of the present invention may further include a nitric acid or nitrite-based compound as an additive. The nitric acid or nitrite-based compound forms a stable coating on the lithium electrode, and has the effect of improving charge / discharge efficiency. The nitric acid or nitrite-based compound is not particularly limited in the present invention, but may be inorganic nitric acid or nitrite compounds such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), and ammonium nitrite (NH4NO2); methyl nitrate, dialkylimidazolium nitrate, guanidine nitrate, etc. The nitrate may be one selected from the group consisting of organic nitric acid or nitrite compounds such as nitrite, imidazolium nitrate, pyridinium nitrate, ethyl nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, and octyl nitrite; organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, and dinitrotoluene; and combinations thereof, and preferably lithium nitrate (LiNO3).

[0053] In addition, the electrolyte may further contain other additives for the purpose of improving charge / discharge characteristics, flame retardancy, etc. Examples of the additives include pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propene sultone (PRS), vinylene carbonate (VC), etc.

[0054] The method for producing the electrolyte solution for lithium-sulfur secondary batteries of the present invention is not particularly limited in the present invention, and the electrolyte solution can be produced by a conventional method known in the art.

[0055] The present invention also provides a lithium-sulfur secondary battery including an electrolyte for a lithium-sulfur secondary battery.

[0056] The lithium-sulfur secondary battery may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the electrolyte may include the electrolyte for a lithium-sulfur secondary battery according to the present invention.

[0057] The positive electrode may include a positive electrode current collector and a positive electrode active material coated on one or both sides of the positive electrode current collector.

[0058] The positive electrode current collector is not particularly limited as long as it supports the positive electrode active material, does not induce chemical changes in the battery, and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.

[0059] The positive electrode current collector may have fine irregularities on its surface to strengthen the bonding force with the positive electrode active material, and may be in various forms such as a film, a sheet, a foil, a mesh, a net, a porous body, a foam, or a nonwoven fabric.

[0060] The positive electrode active material may include a positive electrode active material, and optionally a conductive material and a binder.

[0061] The positive electrode active material is elemental sulfur (S8); Li2S n (n≧1), organic sulfur compounds or carbon-sulfur polymers (C2S x ) n: x = 2.5 to 50, n ≥ 2) may be one or more selected from the group consisting of. Preferably, inorganic sulfur (S8) can be used.

[0062] In addition to the positive electrode active material, the positive electrode may further include one or more additives selected from a transition metal element, a Group IIIA element, a Group IVA element, sulfur compounds of these elements, and alloys of these elements with sulfur.

[0063] The transition metal elements may include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Os, Ir, Pt, Au, or Hg, and the IIIA group elements may include Al, Ga, In, or Ti, and the IVA group elements may include Ge, Sn, or Pb.

[0064] The conductive material is for improving electrical conductivity and is not particularly limited as long as it is an electronically conductive material that does not undergo chemical changes in the lithium secondary battery, and generally carbon black, graphite, carbon fiber, carbon nanotubes, metal powder, conductive metal oxide, organic conductive material, etc. can be used, and currently commercially available conductive materials include acetylene black (Chevron Chemical Company or Gulf Oil Company products, etc.), Ketjen Black EC (Armak Company product), Vulcan XC-72 (Cabot Company product), and Super P (MMM product), etc. Examples include acetylene black, carbon black, graphite, etc.

[0065] In addition, the positive electrode active material may further include a binder having a function of supporting the positive electrode active material on the positive electrode current collector and binding between the active materials. As the binder, various types of binders can be used, such as polyvinylidene fluoride-hexafluoropropylene (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, styrene butadiene rubber (SBR), and carboxyl methyl cellulose (CMC).

[0066] The positive electrode may be a positive electrode having a high sulfur loading. 2 or more, preferably 4.0 mAh / cm 2 More preferably, it is 5.0 mAh / cm 2 It may be more than that.

[0067] The negative electrode may include a negative current collector and a negative active material disposed on the negative current collector, or the negative electrode may be a lithium metal plate.

[0068] The negative electrode current collector is for supporting the negative electrode active material, and is not particularly limited as long as it has excellent conductivity and is electrochemically stable in the voltage region of the lithium secondary battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, silver, or the like, aluminum-cadmium alloy, or the like can be used.

[0069] The negative electrode current collector may have fine irregularities on its surface to strengthen the bonding force with the negative electrode active material, and may be in various forms such as a film, a sheet, a foil, a mesh, a net, a porous body, a foam, a nonwoven fabric, etc.

[0070] The negative electrode active material is lithium (Li + The lithium ion (Li) may be reversibly intercalated or deintercalated, a material capable of reacting with lithium ions to reversibly form a lithium-containing compound, lithium metal, or a lithium alloy. + The material capable of reversibly absorbing and releasing lithium ions (Li) may be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. + The material capable of reacting with lithium-containing compound to reversibly form a lithium-containing compound may be, for example, tin oxide, titanium nitrate, or silicon. The lithium alloy may be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), and tin (Sn). Preferably, the negative electrode active material may be lithium metal, and may be in the form of a lithium metal thin film or lithium metal powder.

[0071] The method for forming the negative electrode active material is not particularly limited, and a method for forming a layer or film commonly used in the art can be used, such as compression bonding, coating, deposition, etc. In addition, the negative electrode of the present invention also includes a case where a thin metallic lithium film is formed on a metal plate by initial charging after assembling a battery without a thin lithium film on a current collector.

[0072] The separator is for physically separating the positive electrode and the negative electrode in the lithium-sulfur secondary battery of the present invention. Any separator that is generally used as a separator in a lithium-sulfur secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to the ion migration of the electrolyte and excellent humidification ability for the electrolyte is preferable.

[0073] The separator may be made of a porous substrate. The porous substrate may be any porous substrate typically used in electrochemical devices, such as, but not limited to, a polyolefin-based porous membrane or nonwoven fabric.

[0074] Examples of the polyolefin-based porous membrane include membranes formed from polyolefin-based polymers such as polyethylene (e.g., high density polyethylene, linear low density polyethylene, low density polyethylene, ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination.

[0075] Examples of the nonwoven fabric include, in addition to polyolefin-based nonwoven fabric, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate, each of which is used alone or in combination. The structure of the nonwoven fabric may be a spunbonded or meltblown nonwoven fabric made of long fibers.

[0076] The thickness of the porous substrate is not particularly limited, but may be 1 to 100 μm, preferably 5 to 50 μm.

[0077] The size of the pores present in the porous substrate and the pores are not particularly limited, but may be 0.001 to 50 μm and 10 to 95%, respectively.

[0078] The electrolyte contains lithium ions and serves to cause an electrochemical oxidation or reduction reaction between the positive and negative electrodes using the lithium ions as a medium, as described above.

[0079] The electrolyte may be injected at an appropriate stage in the manufacturing process of the electrochemical device depending on the manufacturing process and required properties of the final product, i.e., before assembly of the electrochemical device or at the final stage of assembly of the electrochemical device.

[0080] The lithium-sulfur secondary battery according to the present invention can be manufactured by laminating (stack) and folding processes of the separator and the electrodes in addition to the general winding process.

[0081] The shape of the lithium-sulfur secondary battery is not particularly limited, and may be various shapes such as a cylindrical type, a laminated type, a coin type, or the like.

[0082] In the following, preferred examples are presented to aid in understanding the present invention. However, the following examples are provided only to facilitate understanding of the present invention, and the present invention is not limited thereto.

[0083] [Example] Manufacturing of electrolyte for lithium-sulfur secondary batteries Example 1-1 75M (mol / L) lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and 5% by weight lithium nitrate (LiNO3) were dissolved in a mixed solvent of 75% by volume of dimethoxyethane (DME), 20% by volume of 2-methylfuran (2-MeF), and 5% by volume of tris(2,2,2-trifluoroethyl)orthoformate (TFEO) based on the total volume of the non-aqueous solvent to prepare an electrolyte for a lithium-sulfur secondary battery.

[0084] Example 1-2 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 70 volume % and tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used at 10 volume %.

[0085] Examples 1-3 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 60 volume % and tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used at 20 volume %.

[0086] Example 2-1 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that tris(2,2,2-difluoroethyl)orthoformate (TDOF) was used instead of tris(2,2,2-trifluoroethyl)orthoformate (TFEO).

[0087] Example 2-2 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 70 vol% and tris(2,2-difluoroethyl)orthoformate (TDOF) was used at 10 vol%.

[0088] Example 2-3 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 60 vol% and tris(2,2-difluoroethyl)orthoformate (TDOF) was used at 20 vol%.

[0089] Comparative Example 1-1 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 77 vol% and tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used at 3 vol%.

[0090] Comparative Example 1-2 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 58 volume % and tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used at 22 volume %.

[0091] Comparative Example 1-3 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 80 volume % and tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was not used.

[0092] Comparative Example 1-4 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that dimethoxyethane (DME) was used at 90 volume %, tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used at 10 volume %, and 2-methylfuran (2-MeF) was not used.

[0093] Comparative Examples 1-5 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 1-1, except that 90% by volume of 2-methylfuran (2-MeF) was used, 10% by volume of tris(2,2,2-trifluoroethyl)orthoformate (TFEO) was used, and dimethoxyethane (DME) was not used.

[0094] Comparative Example 2-1 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 77 vol% and tris(2,2-difluoroethyl)orthoformate (TDOF) was used at 3 vol%.

[0095] Comparative Example 2-2 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 58 vol% and tris(2,2-difluoroethyl)orthoformate (TDOF) was used at 22 vol%.

[0096] Comparative Example 2-3 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 80 volume % and tris(2,2-difluoroethyl)orthoformate (TDOF) was not used.

[0097] Comparative Example 2-4 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that dimethoxyethane (DME) was used at 90 volume %, tris(2,2-difluoroethyl)orthoformate (TDOF) was used at 10 volume %, and 2-methylfuran (2-MeF) was not used.

[0098] Comparative Example 2-5 An electrolyte for a lithium-sulfur secondary battery was prepared in the same manner as in Example 2-1, except that 90% by volume of 2-methylfuran (2-MeF) was used, 10% by volume of tris(2,2-difluoroethyl)orthoformate (TDOF) was used, and dimethoxyethane (DME) was not used.

[0099] In the lithium-sulfur secondary battery electrolyte solutions of Examples 1-1 to 1-3, 2-1 to 2-3, Comparative Examples 1-1 to 1-5, and 2-1 to 2-5, the contents of the linear ether and the compound represented by Chemical Formula 1 are as shown in Table 1 below.

[0100] [Table 1]

[0101] [Experimental Example] Evaluation of life characteristics of lithium-sulfur secondary batteries Sulfur was mixed with a conductive material and a binder in acetonitrile using a ball mill to prepare a positive active material slurry. Carbon black was used as the conductive material, and a binder in the form of a mixture of SBR and CMC was used as the binder, with the mixture ratio of sulfur:conductive material:binder being 72:24:4 by weight. The positive active material slurry was loaded onto an aluminum current collector at a loading amount of 5.0 mAh / cm. 2 After coating, the mixture was dried to produce a positive electrode with a porosity of 68%. Lithium metal with a thickness of 45 μm was used as the negative electrode.

[0102] The positive and negative electrodes prepared as described above were positioned to face each other, and a polyethylene separator having a thickness of 20 μm and a porosity of 45% was interposed between the positive and negative electrodes.

[0103] Thereafter, the electrolyte solutions according to Examples 1-1 to 1-3, Examples 2-1 to 2-3, Comparative Examples 1-1 to 1-5, and Comparative Examples 2-1 to 2-5 were injected into the case to prepare lithium-sulfur secondary batteries.

[0104] The lithium-sulfur secondary battery manufactured by the above method was charged and discharged 2.5 times at a current density of 0.1 C, then charged and discharged 3 times at a current density of 0.2 C, and then cycled for 300 times at a current density of 0.5 C. The life cycle at which the capacity retention rate of the lithium-sulfur secondary battery reached 80% was measured to confirm the life characteristics of the battery. The results are shown in Table 2.

[0105] [Table 2]

[0106] However, the electrolyte solutions of Comparative Examples 1-5 and 2-5, which do not contain linear ethers, are unable to sufficiently dissolve lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lithium nitrate (LiNO3), making it difficult to operate the battery and making it impossible to measure the life characteristics.

[0107] As shown in Table 2, the lithium-sulfur secondary batteries using the electrolyte solutions according to Examples 1-1 to 1-3 and 2-1 to 1-3 were found to have superior battery life characteristics compared to the lithium-sulfur secondary batteries using the electrolyte solutions according to Comparative Examples 1-1 to 1-2 and 2-1 to 2-2.

[0108] Specifically, the lithium-sulfur secondary battery according to the present invention uses the electrolyte for lithium-sulfur secondary batteries according to Examples 1-1 to 1-3 and Examples 2-1 to 2-3, in which the content of the compound represented by Chemical Formula 1 (Tris(2,2,2-trifluoroethyl)orthoformate) or the trialkyl orthoformate compound (Tris(2,2-difluoroethyl)orthoformate)) in the non-aqueous solvent is 5% by volume to 20% by volume, thereby forming a stable SEI (Solid-Electrolyte Interphase) film on the lithium negative electrode, suppressing the reaction between lithium and polysulfide and decomposition of the electrolyte, and improving the life characteristics of the battery.

[0109] In addition, it was confirmed that the lithium-sulfur secondary batteries using the electrolyte solutions according to Examples 1-1 to 1-3 and Examples 2-1 to 2-3 had superior battery life characteristics compared to the lithium-sulfur secondary batteries using the electrolyte solutions according to Comparative Examples 1-3 to 1-5 and Comparative Examples 2-3 to 2-5.

[0110] Specifically, it was confirmed that the lithium-sulfur secondary battery according to the present invention, which uses the electrolyte solutions for lithium-sulfur secondary batteries according to Examples 1-1 to 1-3 and 2-1 to 2-3 containing any of a linear ether, a cyclic ether, and a compound represented by Chemical Formula 1 as a non-aqueous solvent, has superior battery life characteristics compared to Comparative Examples 1-3 and 2-3 which do not contain a compound represented by Chemical Formula 1, Comparative Examples 1-4 and 2-4 which do not contain a cyclic ether, and Comparative Examples 1-5 and 2-5 which do not contain a linear ether.

[0111] Any simple variations or modifications of the present invention belong to the scope of the present invention, and the specific protection scope of the present invention will be made clear by the appended claims.

Claims

1. An electrolyte for a lithium-sulfur secondary battery comprising a lithium salt and a non-aqueous solvent, The non-aqueous solvent includes an ether solvent and a non-solvent, The ether solvent includes linear ethers and cyclic ethers, The non-solvent is a compound represented by the following formula 1: The content of the non-solvent is 5% by volume to 20% by volume based on the total volume of the non-aqueous solvent; The volume ratio of the ether solvent to the non-solvent is 95:5 to 80:

20. [Formula 1] [In the above Chemical Formula 1, The Rf's may be the same or different, and each independently represents a C1 to C3 fluorinated alkyl group.

2. The lithium salt is LiCl, LiBr, LiI, LiClO 4 , LiBF 4 , LiB 10 C 10 , LiB(Ph) 4 , LiC 4 B.O. 8 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , LiSO 3 CH 3 , LiSO 3 CF 3 , LiSCN, LiC(CF 3 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN (C 2 F 5 SO 2 ) 2 , LiN(SO 2 F) 22. The electrolyte for a lithium-sulfur secondary battery according to claim 1, wherein the lithium borane is at least one selected from the group consisting of lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate, and lithium imide.

3. The linear ether is selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethyl propyl ether, ethyl tert-butyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol butyl methyl ether, diethylene glycol tert-butyl ethyl ether, and ethylene glycol ethyl methyl ether. The electrolyte for a lithium-sulfur secondary battery according to claim 1 or 2.

4. The cyclic ether is selected from the group consisting of dioxolane, methyldioxolane, dimethyldioxolane, vinyldioxolane, methoxydioxolane, ethylmethyldioxolane, oxane, dioxane, trioxane, tetrahydrofuran, methyltetrahydrofuran, dimethyltetrahydrofuran, dimethoxytetrahydrofuran, ethoxytetrahydrofuran, dihydropyran, tetrahydropyran, furan and 2-methylfuran. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 3.

5. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 4, wherein the fluoroalkyl group of the formula (1) is a C1 to C3 fluoroalkyl group substituted with 1 to 7 fluorines.

6. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 5, wherein the fluoroalkyl group of the formula (1) is a C1 to C2 fluoroalkyl group substituted with 1 to 5 fluorines.

7. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 6, wherein the fluoroalkyl group of the formula (1) has a difluoromethyl group or a trifluoromethyl group at its terminal.

8. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 7, wherein the content of the non-solvent is 5% by volume to 10% by volume based on the total volume of the non-aqueous solvent.

9. The content of the linear ether is 50% by volume to 90% by volume based on the total volume of the non-aqueous solvent, and the content of the cyclic ether is 10% by volume to 30% by volume based on the total volume of the non-aqueous solvent. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 8.

10. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 9, wherein the volume ratio of the linear ether to the cyclic ether is 9:1 to 5:

5.

11. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 10, wherein the linear ether is dimethoxyethane.

12. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 11, wherein the cyclic ether is 2-methylfuran.

13. The electrolyte for a lithium-sulfur secondary battery according to any one of claims 1 to 12, wherein the compound represented by Chemical Formula 1 is tris(2,2-difluoroethyl)orthoformate or tris(2,2,2-trifluoroethyl)orthoformate.

14. The electrolyte solution according to any one of claims 1 to 13; Positive electrode; A negative electrode; and A lithium-sulfur secondary battery including a separator.

Citation Information

Patent Citations

  • Pyridine sulfur trioxide complexes as electrolyte components for high voltage batteries.

    JP2020504434A

  • Electrolyte solution for lithium-sulfur battery and lithium-sulfur battery containing the same

    JP2021508148A

  • Electrolytes for lithium-sulfur electrochemical cells

    KR1020070027512A

  • Electrolyte for stable cycling of rechargeable alkali metal and alkali ion batteries