Positive electrode material for alkali metal ion battery, positive electrode and alkali metal ion battery
By optimizing the X-ray diffraction intensity ratio of potassium phosphate compounds in alkali metal ion batteries, the conductivity and discharge capacity are improved, addressing the conductivity and stability issues of existing potassium-based cathode materials.
Patent Information
- Application Number
- JP2020139624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-20
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-08-20
AI Technical Summary
Existing potassium-containing phosphate cathode materials for alkali metal ion batteries, such as KNiPO4 and KCoPO4, suffer from poor electronic conductivity, which hinders the full realization of their battery characteristics, and are prone to oxygen release during charging and discharging, leading to potential battery failure.
The development of a potassium phosphate compound with specific X-ray characteristics, represented by the general formula KxAyDzPO4, where the intensity ratio I(111)/I(110) is between 0.2 and 0.35, enhances electronic conductivity and suppresses oxygen release, thereby enabling high discharge capacity and stability.
The optimized potassium phosphate compound achieves high discharge capacity, suppresses battery failure, and reduces raw material costs while maintaining energy density, even under overcharging conditions.
Smart Images

Figure 0007559425000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode material for an alkali metal ion battery, a positive electrode, and an alkali metal ion battery. [Background technology]
[0002] As batteries are increasingly installed in xEVs, there is a demand for improved battery energy density. To improve energy density, lithium-containing oxide-based positive electrode materials such as LiNiCoMnO4 and LiNiCoAlO2 are widely used. Although batteries with high energy density can be obtained by using oxide-based positive electrode materials containing lithium such as LiNiCoMnO4 and LiNiCoAlO2, lithium resources are scarce and unevenly distributed, which poses geopolitical risks. In addition, there are problems such as heat generation and oxygen release during charging and discharging, which can cause battery failure when overcharged. As a means for solving the above resource problem, a positive electrode material in which lithium, which is a major resource problem, is replaced with potassium, which is a less resource problem, has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-102247 A Summary of the Invention [Problem to be solved by the invention]
[0004] The potassium-containing positive electrode materials, such as phosphates KNiPO4 and KCoPO4, have strong covalent bonds with oxygen and phosphorus, and are therefore expected to release less oxygen during charging and discharging, and to suppress battery failure even when overcharged. However, KNiPO4 and KCoPO4 have poor electronic conductivity, and it is difficult to fully demonstrate the battery characteristics of the previously reported KNiPO4 and KCoPO4.
[0005] The present invention has been made in view of such circumstances, and an object thereof is to provide an alkali metal ion battery capable of obtaining a high discharge capacity, and a positive electrode material and a positive electrode for an alkali metal ion battery capable of obtaining the battery. [Means for Solving the Problems]
[0006] As a result of intensive studies to solve the above problems, the present inventors have found that even when a potassium phosphate compound such as KNiPO4, KCoPO4 or the like and KCoPO4 having low electronic conductivity is used as a positive electrode material, by having specific X-ray characteristics, electronic conductivity enabling battery operation can be obtained and a high discharge capacity can be exhibited. The present invention has been completed based on such findings.
[0007] That is, the present invention provides the following [1] to [5]. [1] A compound represented by the general formula KxAyDzPO4 is included, The positive electrode material for an alkali metal ion battery in which I(111) / I(110) of the 110-plane peak intensity I(110) appearing at 13.5 to 14.5° and the 111-plane peak intensity I(111) appearing at 21.5 to 22.5° in the X-ray diffraction pattern is 0.2 < I(111) / I(110) < 0.35. However, in the above general formula, A is at least one selected from the group consisting of Co, Mn, and Ni, D is at least one selected from the group consisting of Mn, Fe, Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, and Y, and x, y, z satisfy 0.9 < x < 1.1, 0.65 < y ≤ 1.0, 0 ≤ z < 0.35, and 0.9 < y + z < 1.1. [2] The positive electrode material for an alkali metal ion battery according to [1] above, having a specific surface area of 5 m 2 / g or more and 30 m 2 / g or less. [3] A positive electrode using the positive electrode material for an alkali metal ion battery according to [1] or [2] above. [4] An alkali metal ion battery comprising the positive electrode according to [3] above and an electrolyte containing at least one ion selected from the group consisting of Li ions, Na ions, and K ions. Effect of the Invention
[0008] According to the present invention, it is possible to provide an alkali metal ion battery that can provide a high discharge capacity, and a positive electrode material for an alkali metal ion battery and a positive electrode from which such a battery can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Positive electrode material for alkali metal ion batteries> The positive electrode material for an alkali metal ion battery of this embodiment (sometimes referred to as a potassium-containing positive electrode material) contains a compound represented by the general formula KxAyDzPO4, and has an intensity ratio I(111) / I(110) of the 110 plane peak intensity I(110) appearing at 13.5 to 14.5° in an X-ray diffraction pattern to the 111 plane peak intensity I(111) appearing at 21.5 to 22.5°, of 0.2 <I(111) / I(110)<0.35である。 Even when using potassium phosphate compounds with low electronic conductivity, such as KNiPO4 and KCoPO4, if the specific intensity ratio in the X-ray diffraction pattern is greater than 0.2 and less than 0.35, it is possible to impart electronic conductivity sufficient for battery operation and achieve high discharge capacity. The potassium-containing positive electrode material of the present embodiment has a theoretical chargeable / dischargeable capacity inferior to that of a lithium-containing oxide material, but can be produced at lower raw material costs than a lithium-containing oxide material. In addition, since the potassium-containing positive electrode material has a strong covalent bond with oxygen and phosphorus, it releases less oxygen during charging and discharging, and therefore, even if the battery is overcharged, it can suppress battery failure.
[0010] [X-ray characteristics] In the potassium-containing positive electrode material of this embodiment, the intensity ratio I(111) / I(110) of the 110 plane peak intensity I(110) appearing at 13.5 to 14.5° in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) analysis to the 111 plane peak intensity I(111) appearing at 21.5 to 22.5° is 0.2 <I(111) / I(110)<0.35である。 The ratio I(111) / I(110) is an index showing the degree of exposure of the ab plane of the crystal of the compound. The potassium-containing positive electrode material of this embodiment is a material in which an alkali metal ion desorption / insertion reaction occurs on the ab plane of the crystal during the battery reaction, and the alkali metal ions diffuse in the c-axis direction. Therefore, the more the ab plane is exposed, the more easily the desorption / insertion reaction between the compound crystal and the alkali metal ions occurs, and further, a crystal with a shorter crystal diameter in the c-axis direction is preferable because it shortens the diffusion distance of the alkali metal. If the ratio I(111) / I(110) is 0.2 or less, not only is the ab plane exposed to a small extent, resulting in a small area for the desorption / insertion reaction between the compound crystal and the alkali metal ion, but the crystal thickness in the c-axis direction is large, resulting in a large diffusion distance within the crystal of the alkali metal ion, which is unfavorable to the battery reaction and makes it impossible to increase the energy density. If the ratio I(111) / I(110) is 0.35 or more, the ab plane is exposed to a large extent, resulting in a plate-like crystal shape with a very thin aspect ratio in the c-axis direction, which impairs the crystal packing in the electrode, making it impossible to increase the electrode density and energy density. From the viewpoint of improving the energy density, the ratio I(111) / I(110) is preferably 0.21≦I(111) / I(110)≦0.34, more preferably 0.22≦I(111) / I(110)≦0.32, and further preferably 0.23≦I(111) / I(110)≦0.3. The X-ray diffraction pattern can be measured using an X-ray diffraction device.
[0011] [Compound represented by the general formula KxAyDzPO4] The potassium-containing positive electrode material of this embodiment contains particles of a compound represented by the general formula KxAyDzPO4, and the compound represented by the general formula KxAyDzPO4 functions as a positive electrode active material. In the general formula, A is at least one selected from the group consisting of Co, Mn, and Ni, D is at least one selected from the group consisting of Mn, Fe, Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, and Y, and x, y, and z are each 0.9 <x<1.1、0.65<y≦1.0、0≦z<0.35、0.9<y+z<1.1である。 In the general formula, A and D may each independently be one type or two or more types, for example, KxA 1 y1A 2 y2D 1 z1D 2 z2D 3 z3D 4 In this case, the sum of y1 and y2 should be within the range of y, that is, the range of more than 0.65 and not more than 1.0, and the sum of z1, z2, z3, and z4 should be within the range of z, that is, the range of 0 or more and less than 0.35.
[0012] The compound represented by the general formula KxAyDzPO4 is not particularly limited as long as it has the above structure. In the general formula KxAyDzPO4, A is preferably Co and Ni. D is preferably Mn, Fe, Mg, and Al, and more preferably Al. The phosphate-based compound contains these elements, which can increase the energy density of the battery and provide a positive electrode composite layer that can achieve a high discharge potential and high safety. In addition, since the amount of resources is abundant, these elements are preferable as materials to be selected.
[0013] The particles of the phosphate compound of this embodiment preferably include primary particles and secondary particles which are aggregates of the primary particles. The shape of the primary particles of the olivine-type phosphate compound is not particularly limited, but is preferably spherical, particularly spherical. When the primary particles are spherical, the amount of solvent can be reduced when preparing the paste for forming the positive electrode using the potassium-containing positive electrode material of the present embodiment, and the paste for forming the positive electrode can be easily applied to the current collector. The paste for forming the positive electrode can be prepared, for example, by mixing the potassium-containing positive electrode material of the present embodiment, a binder resin (binder), and a solvent. The primary particles and secondary particles of the phosphate compound are collectively referred to as positive electrode active material particles.
[0014] The potassium phosphate compound represented by the general formula KxAyDzPO4 preferably has a shortened crystal in the C-axis direction. By shortening the crystal in the C-axis direction, the potassium-containing positive electrode material of the present embodiment is likely to have the above-described X-ray characteristics [0.2 < I(111) / I(110) < 0.35]. In the potassium phosphate compound, the shortening of the crystal in the C-axis direction can be confirmed by having the above-described X-ray characteristics [0.2 < I(111) / I(110) < 0.35] and further by the fact that the primary particles have a plate-like particle shape by a scanning electron microscope (SEM).
[0015] 〔Carbonaceous Coating〕 The potassium-containing positive electrode material of the present embodiment is particles (positive electrode active material particles) of a compound represented by the general formula KxAyDzPO4. It may or may not have a carbonaceous coating covering the surface of the particles. When it has a carbonaceous coating, the film thickness of the carbonaceous coating is preferably 0.5 nm or more and 5 nm or less. The positive electrode active material particles having a carbonaceous coating are also referred to as carbon-coated positive electrode active material particles. When the film thickness of the carbonaceous coating is 0.5 nm or more, the total movement resistance of electrons in the carbonaceous coating can be lowered, the internal resistance of the alkali metal ion battery can be suppressed, and the voltage drop at a high charge-discharge rate can be prevented. When the film thickness of the carbonaceous coating is 5 nm or less, the potassium phosphate compound can be imparted with electronic conductivity enabling battery operation. The thickness of the carbonaceous coating is preferably 0.6 nm or more, more preferably 4.5 nm or more, and even more preferably 0.7 nm or more, and is preferably 4 nm or less, more preferably 0.9 nm or less, and even more preferably 3.5 nm or less.
[0016] The carbonaceous coating is a pyrolytic carbonaceous coating obtained by carbonizing an organic substance that is the raw material of the carbonaceous coating. The organic matter is not particularly limited as long as it is a compound capable of forming a carbonaceous coating on the surface of the positive electrode active material particles, and examples thereof include polyvinyl alcohol (PVA), polyvinylpyrrolidone, cellulose, starch, gelatin, carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, hydroxyethylcellulose, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, polyvinyl acetate, phenol, phenolic resin, glucose, fructose, galactose, mannose, maltose, sucrose, lactose, glycogen, pectin, alginic acid, glucomannan, chitin, hyaluronic acid, chondroitin, agarose, polyether, and polyhydric alcohol. Examples of polyhydric alcohol include polyethylene glycol, polypropylene glycol, polyglycerin, and glycerin. These may be used alone or in combination of two or more.
[0017] [Specific surface area] The potassium-containing positive electrode material in this embodiment (preferably, carbonaceous-coated positive electrode active material particles) has a specific surface area of 5 m 2 / g or more and 30m 2 It is preferable that the molecular weight is not more than 1 / g. The specific surface area of the potassium-containing positive electrode material is 5m 2 / g or more, the particle size of the primary particles of the olivine-type phosphate compound becomes fine, and the time required for the movement of potassium ions and electrons can be shortened, thereby increasing the capacity during operation at a large current and at a low temperature. The specific surface area of the potassium-containing positive electrode material is 30m 2 / g or less, metal elution can be suppressed. In order to further increase the energy density, the specific surface area of the potassium-containing positive electrode material is set to 7m 2 / g or more and 24m 2 / g or less is more preferable, and 2 / g or more and 20m 2 It is more preferable that the molecular weight is not more than 1 / g. The specific surface area can be measured by the BET method using nitrogen (N2) adsorption, using a specific surface area meter (for example, BELSORP-mini, product name, manufactured by BEL Japan).
[0018] (carbon content) The potassium-containing positive electrode material in this embodiment (preferably, carbonaceous-coated positive electrode active material particles) preferably has a carbon content of 1.0 mass % or more and 4.0 mass % or less. When the carbon content of the potassium-containing positive electrode material is 1.0 mass% or more, the distance between the carbon atoms is reduced and the conductive path is easily formed, which makes it easy to improve the cycle characteristics of the alkali metal ion battery. Also, when the carbon content of the potassium-containing positive electrode material is 4.0 mass% or less, the gap between the primary particles of the olivine-type phosphate compound is not easily narrowed, which makes it possible to increase the electrolyte retention capacity of the potassium-containing positive electrode material and makes it easy to improve the input characteristics. From the viewpoint of increasing the energy density, the carbon content of the potassium-containing positive electrode material is more preferably 1.2 mass % or more and 3.5 mass % or less, and further preferably 1.4 mass % or more and 3.0 mass % or less. The carbon content can be measured using a carbon analyzer (for example, model number EMIA-220V, manufactured by Horiba, Ltd.).
[0019] The tap density of the potassium-containing positive electrode material (preferably, the carbonaceous-coated positive electrode active material particles) in this embodiment is 1.0 to 1.6 g / cm 3 It is preferable that: The tap density of the potassium-containing positive electrode material is 1.0 g / cm 3By setting the tap density of the potassium-containing positive electrode material at 1.6 g / cm or more, the contact area between the positive electrode active material and the electrolyte does not become too large, and the amount of metal eluted from the positive electrode active material can be suppressed. 3 When the positive electrode active material has a capacitance of 100 nm or less, the contact area between the positive electrode active material and the electrolyte is increased, making it easier to insert and remove potassium ions into and from the positive electrode active material, thereby making it possible to increase the capacity. From the above viewpoints, the tap density of the potassium-containing positive electrode material is more preferably 1.1 to 1.5, and further preferably 1.2 to 1.5. The tap density can be measured by a method conforming to JIS R 1628:1997, Method for measuring bulk density of fine ceramic powders.
[0020] The average particle diameter of the primary particles of the positive electrode active material particles coated with a carbonaceous film (carbonaceous coated positive electrode active material particles) is preferably 50 nm or more, more preferably 70 nm or more, and even more preferably 100 nm or more, and is preferably 500 nm or less, more preferably 450 nm or less, and even more preferably 400 nm or less. When the average particle diameter of the primary particles is 50 nm or more, the increase in the carbon amount caused by the increase in the specific surface area of the potassium-containing positive electrode material can be suppressed, and thus the decrease in the charge / discharge capacity of the alkali metal ion battery can be suppressed. On the other hand, when the average particle diameter is 500 nm or less, the migration time of the potassium ions or the migration time of the electrons moving within the potassium-containing positive electrode material can be shortened. This can suppress the deterioration of the output characteristics caused by the increase in the internal resistance of the alkali metal ion battery. Here, the average particle size of the primary particles means the number-average particle size. The average particle size of the primary particles can be determined by averaging the particle sizes of 200 or more particles measured by scanning electron microscope (SEM) observation.
[0021] The average particle diameter of the secondary particles of the carbonaceous-coated positive electrode active material particles is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, and is preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 15 μm or less. When the average particle diameter of the secondary particles is 0.5 μm or more, it is possible to suppress the need for a large amount of conductive assistant and binder when preparing an alkali metal ion battery positive electrode material paste by mixing a potassium-containing positive electrode material, a conductive assistant, a binder resin (binding agent), and a solvent. This makes it possible to increase the battery capacity of the alkali metal ion battery per unit mass in the positive electrode mixture layer of the positive electrode of the alkali metal ion battery. On the other hand, when the average particle diameter is 20 μm or less, it is possible to increase the dispersibility and uniformity of the conductive assistant and binder in the positive electrode mixture layer of the positive electrode of the alkali metal ion battery. As a result, the discharge capacity of the alkali metal ion battery during high-speed charging and discharging is increased. Here, the average particle size of the secondary particles means the volume average particle size. The average particle size of the secondary particles can be measured using a laser diffraction scattering type particle size distribution measuring device or the like.
[0022] The coverage of the positive electrode active material particles with the carbonaceous film is preferably 60% or more, and more preferably 80% or more. When the coverage of the carbonaceous film is 60% or more, the covering effect of the carbonaceous film can be sufficiently obtained. The coverage rate of the carbonaceous coating can be determined by observing particles using a transmission electron microscope (TEM), an energy dispersive X-ray microanalyzer (EDX), or the like, calculating the proportion of the part of the particle surface that is covered, and averaging the calculated values.
[0023] The density of the carbonaceous coating, calculated based on the carbon content constituting the carbonaceous coating, is preferably 0.3 g / cm 3 More preferably, 0.4 g / cm 3 and preferably 2.0 g / cm 3 Less than or equal to 1.8 g / cm 3The density of the carbonaceous coating, which is calculated based on the carbon content constituting the carbonaceous coating, is the mass per unit volume of the carbonaceous coating when it is assumed that the carbonaceous coating is composed only of carbon. The density of the carbonaceous coating is 0.3 g / cm 3 If the carbonaceous coating has a density of 2.0 g / cm or more, the carbonaceous coating can exhibit sufficient electronic conductivity. 3 If the carbonaceous coating contains only a small amount of graphite microcrystals having a layered structure, the graphite microcrystals do not cause steric hindrance when potassium ions diffuse through the carbonaceous coating. This prevents the resistance to potassium ion migration from increasing. As a result, the internal resistance of the alkali metal ion battery does not increase, and the voltage drop during high-speed charge / discharge of the alkali metal ion battery does not occur.
[0024] (Method of manufacturing positive electrode materials for alkali metal ion batteries) The method for producing the alkali metal ion battery positive electrode material of this embodiment is not particularly limited, but may include, for example, a step (A) of obtaining positive electrode active material particles, a step (B) of adding an organic compound to the positive electrode active material particles obtained in the step (A) to prepare a mixture, and a step (C) of putting the mixture into a firing sheath and firing it.
[0025] [Process (A)] In step (A), the method for producing the positive electrode active material particles is not particularly limited, and for example, a conventional method such as a solid phase method, a liquid phase method, a gas phase method, etc. The particulate KxAyDzPO4 obtained by such a method is hereinafter referred to as "KxAyDzPO4 particles". For example, the KxAyDzPO4 particles can be obtained by hydrothermally synthesizing a slurry mixture obtained by mixing a K source, an A source, a P source, water, and optionally a D source to obtain a precursor, KxAyDzPO4·H2O, and then heat-treating the precursor to obtain the desired KxAyDzPO4 particles. In the hydrothermal synthesis, the KxAyDzPO4·H2O precursor is formed as a precipitate in water. It is preferable to use a pressure-resistant closed vessel for this hydrothermal synthesis.
[0026] As reaction conditions for the hydrothermal synthesis, for example, the heating temperature is preferably 110° C. or more and 230° C. or less, more preferably 115° C. or more and 220° C. or less, and further preferably 120° C. or more and 210° C. or less. By setting the heating temperature within the above range, the specific surface area of the positive electrode active material particles can be set within the above range. The reaction time is preferably from 20 minutes to 169 hours, more preferably from 30 minutes to 24 hours, and even more preferably from 1 hour to 10 hours. The pressure during the reaction is preferably from 0.1 MPa to 22 MPa, and more preferably from 0.1 MPa to 17 MPa. As reaction conditions for the hydrothermal synthesis, for example, the heating temperature is preferably 110° C. or more and 200° C. or less, more preferably 115° C. or more and 195° C. or less, and further preferably 120° C. or more and 190° C. or less. By setting the heating temperature within the above range, it is easy to set the specific surface area of the positive electrode active material particles within the above range. The reaction time is preferably from 20 minutes to 20 hours, more preferably from 30 minutes to 15 hours, even more preferably from 40 minutes to 10 hours, and still more preferably from 50 minutes to 5 hours. Furthermore, the pressure during the reaction is preferably 0.5 MPa or more and 3.5 MPa or less, more preferably 0.7 MPa or more and 3.0 MPa or less, and even more preferably 0.8 MPa or more and 2.5 MPa or less. By setting the heating temperature, reaction time, and pressure during the hydrothermal synthesis within the above ranges, it is easy to produce a potassium phosphate compound represented by the general formula KxAyDzPO4 as a hydrate. In addition, by calcining the obtained potassium phosphate compound hydrate, it is easy to shorten the crystal in the C-axis direction, and it is easy to make the intensity ratio I(111) / I(110) in the XRD pattern greater than 0.2 and less than 0.35.
[0027] The molar ratio of the K source, the A source, the D source and the P source (K:A:D:P) is preferably 2.5-4.0:0.5-1.0:0-1.0:0.9-1.15, and more preferably 2.8-3.5:0.6-1.0:0-1.0:0.95-1.1.
[0028] Here, as the K source, it is preferable to use at least one selected from the group consisting of: hydroxides such as potassium hydroxide (KOH); inorganic acid salts of potassium such as potassium carbonate (K2CO3), potassium chloride (KCl), potassium nitrate (KNO3), potassium phosphate (K3PO4), dipotassium hydrogen phosphate (K2HPO4), and potassium dihydrogen phosphate (KH2PO4); organic acid salts of potassium such as potassium acetate (KCH3COO) and potassium oxalate ((COOK)2); and hydrates thereof. In addition, potassium phosphate (K3PO4) can also be used as a K source and a P source.
[0029] Examples of the A source include chlorides, carboxylates, sulfates, etc., containing at least one selected from the group consisting of Co, Mn, and Ni. For example, when A in KxAyDzPO4 is Ni, examples of the Ni source include nickel chloride (NiCl2), nickel sulfate (NiSO4), and hydrates thereof; when A is Co, examples of the Co source include cobalt chloride (CoCl2), cobalt sulfate (CoSO4), and hydrates thereof.
[0030] Examples of the D source include chlorides, carboxylates, and sulfates containing at least one selected from the group consisting of Mn, Fe, Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, and Y. For example, when D in KxAyDzPO4 is Al, examples of the Al source include aluminum hydroxide (Al(OH)3), aluminum chloride (AlCl3), aluminum sulfate (Al2(SO4)3), aluminum nitrate (Al(NO3)3), aluminum acetate (Al(CH3COO)3), and hydrates thereof.
[0031] Examples of the P source include phosphoric acid compounds such as phosphoric acid (H3PO4), ammonium dihydrogen phosphate (NH4H2PO4), diammonium hydrogen phosphate ((NH4)2HPO4), etc. Among these, it is preferable to use at least one selected from the group consisting of phosphoric acid, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate as the P source.
[0032] [Process (B)] In the step (B), an organic compound is added to the positive electrode active material particles (KxAyDzPO4 particles) obtained in the step (A) to prepare a mixture. First, an organic compound is added to the positive electrode active material particles, and then a solvent is added. From the viewpoint of achieving a carbonaceous coating thickness of 0.5 nm or more and 5 nm or less, the amount of the organic compound blended with respect to the positive electrode active material particles is preferably 0.15 parts by mass or more and 3 parts by mass or less, and more preferably 0.3 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the positive electrode active material particles, when the total mass of the organic compound is converted into carbon element. Furthermore, when the amount of the organic compound blended relative to the positive electrode active material particles is 0.15 parts by mass or more, the coverage of the positive electrode active material particle surface with the carbonaceous coating formed by heat treating the organic compound can be 80% or more. This can improve the high input characteristics and cycle characteristics of the alkali metal ion battery. On the other hand, when the amount of the organic compound blended relative to the positive electrode active material particles is 3 parts by mass or less, the bulk density of the positive electrode active material particles can be reduced, the decrease in electrode density can be suppressed, and the decrease in capacity of the alkali metal ion battery per unit volume can be suppressed.
[0033] When the solvent is added to the positive electrode active material particles, the solid content is adjusted to be preferably 10 to 60 mass%, more preferably 15 to 55 mass%, and further preferably 25 to 50 mass%. By adjusting the solid content within the above range, the tap density of the obtained potassium-containing positive electrode material can be adjusted to be within the above range.
[0034] Examples of the solvent include water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol: IPA), butanol, pentanol, hexanol, octanol, and diacetone alcohol; esters such as ethyl acetate, butyl acetate, ethyl lactate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and γ-butyrolactone; ethers such as diethyl ether, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; ketones such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetylacetone, and cyclohexanone; amides such as dimethylformamide, N,N-dimethylacetoacetamide, and N-methylpyrrolidone; and glycols such as ethylene glycol, diethylene glycol, and propylene glycol. These solvents may be used alone or in combination of two or more. Of these solvents, water is preferred. If necessary, a dispersant may be added.
[0035] The method for dispersing the positive electrode active material particles and the organic compound in the solvent is not particularly limited as long as the positive electrode active material particles are uniformly dispersed and the organic compound is dissolved or dispersed. Examples of the device used for such dispersion include a medium stirring type dispersing device that stirs medium particles at high speed, such as a planetary ball mill, a vibration ball mill, a bead mill, a paint shaker, and an attritor.
[0036] The mixture may be sprayed into a high-temperature atmosphere, for example, air at 110° C. or higher and 200° C. or lower, using a spray pyrolysis method, and dried to produce granules of the mixture. In this spray pyrolysis method, in order to rapidly dry and produce roughly spherical granules, the particle size of the droplets during spraying is preferably 0.01 μm or more and 100 μm or less.
[0037] [Process (C)] In step (C), the mixture obtained in step (B) is placed in a firing sheath and fired. As the sintered sheath, for example, a sintered sheath made of a material having excellent thermal conductivity, such as carbon, is preferably used. The firing temperature is preferably 630°C or higher and 790°C or lower, and more preferably 680°C or higher and 770°C or lower. When the firing temperature is 630°C or higher, the decomposition and reaction of the organic compound proceeds sufficiently, and the organic compound can be sufficiently carbonized. As a result, a low-resistance carbonaceous coating can be formed on the obtained potassium-containing positive electrode material. On the other hand, when the firing temperature is 790°C or lower, the grain growth of the potassium-containing positive electrode material does not proceed, and a sufficiently high specific surface area can be maintained. As a result, when an alkali metal ion battery is formed, the discharge capacity at a high-speed charge / discharge rate is large, and sufficient charge / discharge rate performance can be achieved.
[0038] The calcination time is not particularly limited as long as the organic compound is sufficiently carbonized, and is, for example, from 0.1 hours to 100 hours. The firing atmosphere is preferably an inert atmosphere consisting of an inert gas such as nitrogen (N2) and argon (Ar) or a reducing atmosphere containing a reducing gas such as hydrogen (H2). When it is desired to further suppress oxidation of the mixture, it is more preferable that the firing atmosphere is a reducing atmosphere.
[0039] By the firing in step (C), the organic compound is decomposed and reacted to generate carbon. This carbon then adheres to the surface of the positive electrode active material particles to form a carbonaceous coating. As a result, the surface of the positive electrode active material particles is covered with the carbonaceous coating.
[0040] <Alkaline metal ion battery> The alkali metal ion battery of this embodiment has a positive electrode using the positive electrode material for alkali metal ion batteries of this embodiment, and an electrolyte containing at least one ion selected from the group consisting of Li ions, Na ions, and K ions.
[0041] [Positive electrode] To prepare a positive electrode, the above-mentioned potassium-containing positive electrode material, a binder made of a binder resin, and a solvent are mixed to prepare a paint for forming a positive electrode or a paste for forming a positive electrode. At this time, a conductive assistant such as carbon black, acetylene black, graphite, ketjen black, natural graphite, or artificial graphite may be added as necessary. As the binding agent, that is, the binder resin, for example, polytetrafluoroethylene (PTFE) resin, polyvinylidene fluoride (PVdF) resin, fluororubber, etc. are suitably used. The compounding ratio of the potassium-containing positive electrode material and the binder resin is not particularly limited, but for example, the binder resin is 1 to 30 parts by mass, preferably 3 to 20 parts by mass, per 100 parts by mass of the potassium-containing positive electrode material.
[0042] The solvent used in the paint or paste for forming the positive electrode may be appropriately selected depending on the properties of the binder resin. Examples of the solvent include water, methanol, ethanol, 1-propanol, 2-propanol (isopropyl alcohol: IPA), butanol, pentanol, hexanol, octanol, diacetone alcohol, and other alcohols; ethyl acetate, butyl acetate, ethyl lactate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, γ-butyrolactone, and other esters; diethyl ether, ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (ethyl cellosolve), ethylene glycol monobutyl ether (butyl cellosolve), diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and other ethers; acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), acetylacetone, cyclohexanone, and other ketones; dimethylformamide, N,N-dimethylacetoacetamide, N-methylpyrrolidone, and other amides; ethylene glycol, diethylene glycol, propylene glycol, and other glycols. These may be used alone or in combination of two or more.
[0043] Next, the paint or paste for forming a positive electrode is applied to one side of an aluminum foil, and then dried to obtain an aluminum foil having a coating film made of a mixture of the potassium-containing positive electrode material and the binder resin formed on one side thereof. Next, the coating film is pressed and dried to produce a current collector (positive electrode) having a positive electrode mixture layer on one surface of the aluminum foil. In this manner, a positive electrode capable of producing an alkali metal ion battery having excellent high input characteristics and cycle characteristics can be produced.
[0044] [Negative electrode] Examples of the negative electrode include metallic Li, natural graphite, carbon materials such as hard carbon, Li alloys, and Li4Ti5O 12 , Si(Li 4.4 Examples include those containing a negative electrode material such as silicon.
[0045] [Electrolyte] The electrolyte contains at least one selected from the group consisting of Li ions, Na ions, and K ions. The electrolyte is preferably a non-aqueous electrolyte, and for example, ethylene carbonate and diethyl carbonate are mixed in a mass ratio of 1:1, and metal hexafluorophosphate (MPF6) is added to the resulting mixed solvent at a concentration of, for example, 1 mol / dm 3 Here, in MPF6, M represents Li ion, Na ion, or K ion. Only one type of MPF6 may be used, or two or more types may be mixed and used.
[0046] [Separator] The positive electrode and the negative electrode of the present embodiment can be opposed to each other via a separator, which can be made of, for example, porous propylene. Moreover, a solid electrolyte may be used in place of the nonaqueous electrolyte and the separator.
[0047] The alkali metal ion battery of the present embodiment has a positive electrode composite layer made of the alkali metal ion battery positive electrode material of the present embodiment, and therefore has excellent Li ion migration around all of the battery constituent members, and has excellent high input characteristics and cycle characteristics. Therefore, the battery is suitably used as a battery for driving an electric vehicle, a battery for driving a hybrid vehicle, etc. EXAMPLES
[0048] The present invention will be specifically described below with reference to examples and comparative examples. Note that the present invention is not limited to the embodiments described in the examples.
[0049] [Production of positive electrode material for alkali metal ion batteries] (1) Positive electrode material whose active material is KNiPO4 Example 1 1. Preparation of raw material slurry A1 A KNiPO4 compound with a shortened crystal along the C-axis was prepared as follows. K3PO4 was used as the K source and P source, and an aqueous NiSO4 solution was used as the Ni source. These were mixed in a molar ratio of K:Ni:P=3:1:1 to prepare 2.0 L of raw material slurry A1.
[0050] 2. Hydrothermal synthesis Next, the raw material slurry A1 was placed in a pressure vessel. Thereafter, the raw material slurry A1 was subjected to a heating reaction at 190° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 1.1 MPa.
[0051] 3. Preparation of KNiPO4·H2O particles After the reaction, the atmosphere in the heat-resistant container was cooled to room temperature, and a cake-like precipitate of the reaction product was obtained. This precipitate was thoroughly washed multiple times with distilled water, and the moisture content was kept at 40% to prevent drying, to give a cake-like substance. This cake-like material was vacuum dried at 70℃ for 2 hours to obtain KNiPO4·H2O particles.
[0052] 4. Firing The obtained KNiPO4·H2O particles were heated at 680℃ for 1 hour to obtain KNiPO4 particles with shortened crystals along the C-axis.
[0053] Example 2 KNiPO4 particles were produced in the same manner as in Example 1, except that "2. Hydrothermal synthesis" in Example 1 was changed as follows.
[0054] The raw material slurry A1 was placed in a pressure vessel. Thereafter, the raw material slurry A1 was subjected to a heating reaction at 170° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.9 MPa.
[0055] Example 3 KNiPO4 particles were produced in the same manner as in Example 1, except that "2. Hydrothermal synthesis" in Example 1 was changed as follows.
[0056] The raw material slurry A1 was placed in a pressure vessel. Thereafter, the raw material slurry A1 was subjected to a heating reaction at 210° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 1.9 MPa.
[0057] Example 4 KNiPO4 particles were produced in the same manner as in Example 1, except that "4. Calcination" in Example 1 was changed as follows.
[0058] Raw material slurry B1, which was made by dispersing 4% by mass of polyvinyl alcohol (preliminarily adjusted to 20% by mass) in an aqueous solvent with 96% by mass of KNiPO4·H2O particles, was dried and granulated. It was then heated at 680°C for 1 hour, shortening the crystals in the C-axis direction and obtaining KNiPO4 particles whose surfaces were covered with a carbonaceous film.
[0059] Comparative Example 1 KNiPO4 particles in which the crystals were significantly shortened in the C-axis direction were produced in the same manner as in Example 1, except that "2. Hydrothermal synthesis" in Example 1 was changed as follows.
[0060] The raw material slurry A1 was placed in a pressure vessel. Thereafter, the raw material slurry A1 was subjected to a heating reaction at 140° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.4 MPa.
[0061] Comparative Example 2 KNiPO4 particles in which the crystals were not shortened in the C-axis direction were produced in the same manner as in Example 1, except that "2. Hydrothermal synthesis" in Example 1 was changed as follows.
[0062] The raw material slurry A1 was placed in a pressure vessel. Thereafter, the raw material slurry A1 was subjected to a heating reaction at 250° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 4.0 MPa.
[0063] (2) Positive electrode material whose active material is KCoPO4 Example 5 1. Preparation of raw material slurry A2 A KCoPO4 compound with a shortened crystal along the C-axis was prepared as follows. K3PO4 was used as the K source and P source, and a CoSO4 aqueous solution was used as the Co source. These were mixed in a molar ratio of K:Co:P=3:1:1 to prepare 2.0 L of raw material slurry A2.
[0064] 2. Hydrothermal synthesis Next, the raw material slurry A2 was placed in a pressure vessel. Thereafter, the raw material slurry A2 was subjected to a heating reaction at 180° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 1.0 MPa.
[0065] 3. Preparation of KCoPO4·H2O particles After the reaction, the atmosphere in the heat-resistant container was cooled to room temperature, and a cake-like precipitate of the reaction product was obtained. This precipitate was thoroughly washed multiple times with distilled water, and the moisture content was kept at 40% to prevent drying, to give a cake-like substance. This cake-like material was vacuum dried at 70℃ for 2 hours to obtain KCoPO4·H2O particles.
[0066] 4. Firing The obtained KCoPO4·H2O particles were heated at 680℃ for 1 hour to obtain KCoPO4 particles with shortened crystals along the C-axis.
[0067] Example 6 KCoPO4 particles were produced in the same manner as in Example 5, except that "2. Hydrothermal synthesis" in Example 5 was changed as follows.
[0068] The raw material slurry A2 was placed in a pressure vessel. Thereafter, the raw material slurry A2 was subjected to a heating reaction at 160° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.8 MPa.
[0069] Example 7 KCoPO4 particles were produced in the same manner as in Example 5, except that "2. Hydrothermal synthesis" in Example 5 was changed as follows.
[0070] The raw material slurry A2 was placed in a pressure vessel. Thereafter, the raw material slurry A2 was subjected to a heating reaction at 210° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 1.9 MPa.
[0071] Example 8 KCoPO4 particles were produced in the same manner as in Example 5, except that "4. Calcination" in Example 5 was changed as follows.
[0072] Raw material slurry B2, which was made by dispersing 4% by mass of polyvinyl alcohol (preliminarily adjusted to 20% by mass) in an aqueous solvent with 96% by mass of KCoPO4·H2O particles, was dried and granulated. It was then heated at 680℃ for 1 hour, shortening the crystals in the C-axis direction and obtaining KCoPO4 particles whose surfaces were covered with a carbonaceous film.
[0073] Comparative Example 3 KCoPO4 particles in which the crystals were significantly shortened in the C-axis direction were produced in the same manner as in Example 5, except that "2. Hydrothermal synthesis" in Example 5 was changed as follows.
[0074] The raw material slurry A2 was placed in a pressure vessel. Thereafter, the raw material slurry A2 was subjected to a heating reaction at 140° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.4 MPa.
[0075] Comparative Example 4 KCoPO4 particles in which the crystals were not shortened in the C-axis direction were produced in the same manner as in Example 5, except that "2. Hydrothermal synthesis" in Example 5 was changed as follows.
[0076] The raw material slurry A2 was placed in a pressure vessel. Thereafter, the raw material slurry A2 was subjected to a heating reaction at 250° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 4.0 MPa.
[0077] (3) The active material is KNi 0.9 Co 0.05 Al 0.05 Positive electrode material is PO4 Example 9 1. Preparation of Raw Slurry A3 The crystals of KNi were shortened along the C-axis as follows: 0.9 Co 0.05 Al 0.05 PO4 compound was produced. K3PO4 was used as the K source and P source, a NiSO4 aqueous solution as the Ni source, a CoSO4 aqueous solution as the Co source, and an Al2(SO4)3 aqueous solution as the Al source. These were mixed in a molar ratio of K:Ni:P = 3:0.9:0.05:0.05:1 to prepare 2.0 L of raw material slurry A3.
[0078] 2. Hydrothermal synthesis Next, the raw material slurry A3 was placed in a pressure vessel. Thereafter, the raw material slurry A3 was subjected to a heating reaction at 190° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 1.1 MPa.
[0079] 3. KNi 0.9 Co 0.05 Al 0.05 Production of PO4·H2O particles After the reaction, the atmosphere in the heat-resistant container was cooled to room temperature, and a cake-like precipitate of the reaction product was obtained. This precipitate was thoroughly washed multiple times with distilled water, and the moisture content was kept at 40% to prevent drying, to give a cake-like substance. The cake-like substance was vacuum dried at 70°C for 2 hours to obtain KNi 0.9 Co 0.05 Al 0.05 PO4·H2O particles were obtained.
[0080] 4. Firing The obtained KNi0.9 Co 0.05 Al 0.05 By heating PO4·H2O particles at 680℃ for 1 hour, the crystals of KNi were shortened along the C-axis. 0.9 Co 0.05 Al 0.05 PO4 particles were obtained.
[0081] Example 10 The procedure of Example 9 was repeated except for the following changes in "2. Hydrothermal synthesis" in Example 9 to produce KNi 0.9 Co 0.05 Al 0.05 PO4 particles were produced.
[0082] The raw material slurry A3 was placed in a pressure vessel. Thereafter, the raw material slurry A3 was subjected to a heating reaction at 170° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.9 MPa.
[0083] Example 11 The procedure of Example 9 was repeated except for the following changes in "2. Hydrothermal synthesis" in Example 9 to produce KNi 0.9 Co 0.05 Al 0.05 PO4 particles were produced.
[0084] The raw material slurry A3 was placed in a pressure vessel. Thereafter, the raw material slurry B was subjected to a heating reaction at 210° C. for 1 hour to carry out hydrothermal synthesis. The pressure inside the pressure vessel at this time was 1.9 MPa.
[0085] Example 12 The same procedure as in Example 9 was repeated except that "4. Firing" in Example 9 was changed as follows. 0.9 Co 0.05 Al 0.05 PO4 particles were produced.
[0086] KNi 0.9 Co 0.05 Al 0.05The raw material slurry B3, which was made by dispersing 4% by mass of polyvinyl alcohol (preliminarily adjusted to 20% by mass) in an aqueous solvent with 96% by mass of PO4·H2O particles, was dried and granulated. It was then heated at 680°C for 1 hour, resulting in a KNi powder with the crystals shortened in the C-axis direction and the surface covered with a carbonaceous film. 0.9 Co 0.05 Al 0.05 PO4 particles were obtained.
[0087] Comparative Example 5 The procedure of "2. Hydrothermal synthesis" in Example 9 was repeated except for the following changes to the KNi alloy with significantly shortened crystals in the C-axis direction. 0.9 Co 0.05 Al 0.05 PO4 particles were produced.
[0088] The raw material slurry A3 was placed in a pressure vessel. Thereafter, the raw material slurry A3 was subjected to a heating reaction at 140° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 0.4 MPa.
[0089] Comparative Example 6 The procedure of "2. Hydrothermal synthesis" in Example 9 was changed as follows, but the same procedure as in Example 9 was repeated to obtain KNi with no shortening of the crystal in the C-axis direction. 0.9 Co 0.05 Al 0.05 PO4 particles were produced.
[0090] The raw material slurry A3 was placed in a pressure vessel. Thereafter, the raw material slurry A3 was subjected to a heating reaction at 250° C. for 1 hour to carry out hydrothermal synthesis. At this time, the pressure inside the pressure-resistant vessel was 4.0 MPa.
[0091] [Evaluation of positive electrode materials] The properties of the positive electrode materials obtained in the examples and comparative examples and the components contained in the positive electrode materials were evaluated. The evaluation methods are as follows. The results are shown in Table 1.
[0092] (1) Carbon content The carbon amount in the positive electrode material was measured using a carbon analyzer (manufactured by Horiba, Ltd., model number: EMIA-220V).
[0093] (2) X-ray properties [I(111) / I(110)] Using a benchtop powder X-ray diffractometer (Spectris Corporation, trade name "Aeris"), the XRD pattern was measured with CuKα radiation, the intensity I(110) of the 110 plane peak appearing at 13.5 to 14.5° and the intensity I(111) of the 111 plane peak appearing at 21.5 to 22.5° were measured, and the intensity ratio I(111) / I(110) was calculated.
[0094] (3) Specific surface area The specific surface area of the positive electrode material was measured by the BET method using nitrogen (N2) adsorption using a specific surface area meter (manufactured by BEL JAPAN, product name: BELSORP-mini).
[0095] [Preparation and evaluation of potassium ion secondary batteries] (1) Fabrication of laminated potassium ion secondary battery 90% by mass of the positive electrode materials for alkali metal secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2, 5% by mass of acetylene black, and 5% by mass of polyvinylidene fluoride (PVdF) were added to N-methyl-2-pyrrolidone (NMP) and mixed to prepare a slurry. This slurry was applied to a current collector made of aluminum foil with a thickness of 15 μm, dried, and then pressed to prepare a positive electrode.
[0096] 90% by mass of natural graphite powder, 5% by mass of acetylene black, and 5% by mass of polyvinylidene fluoride (PVdF) were added to N-methyl-2-pyrrolidone (NMP) and mixed to prepare a slurry. This slurry was applied to a current collector made of copper foil having a thickness of 15 μm, dried, and then pressed to prepare a negative electrode.
[0097] The obtained positive electrode was cut into a size of 2.8 cm × 2.6 cm; the negative electrode was cut into a size of 3.0 cm × 2.8 cm; and the porous polypropylene film with a thickness of 25 μm as the separator was cut into a size of 3.2 cm × 3.2 cm. Then, the separator was placed between the coated surfaces of the positive and negative electrodes, and these electrodes and the separator were sandwiched between two aluminum laminate films. Three sides except for one side of the long side were heat-sealed with a width of 8 mm. After injecting the electrolyte, the remaining side was heat-sealed to fabricate a laminated potassium-ion secondary battery. As the electrolyte, a mixture of ethylene carbonate and diethyl carbonate at a ratio of 1:1 (mass ratio) was further added with 0.7 M KPF6 solution and dissolved was used.
[0098] (2) Evaluation of Potassium-Ion Secondary Battery At an ambient temperature of 25 °C, constant current charging was performed at a current value of 0.1 CA until the voltage of the positive electrode reached 5.6 V with respect to the natural graphite negative electrode voltage. After reaching the target voltage, constant voltage charging was performed until the current value reached 0.01 CA. After that, after a 1-minute rest, at an ambient temperature of 25 °C, constant current discharge at 0.1 CA was performed until the voltage of the positive electrode reached 2.0 V with respect to the natural graphite negative electrode voltage, and the 0.1C discharge capacity was evaluated according to the following criteria. ◎: The 0.1C discharge capacity is 60 mAh / g or more, and it is particularly excellent in potassium-ion electrical discharge characteristics. ○: The 0.1C discharge capacity is 40 mAh / g or more and less than 60 mAh / g, and it is excellent in potassium-ion electrical discharge characteristics. ×: The 0.1C discharge capacity is less than 40 mAh / g, and it is not excellent in potassium-ion electrical discharge characteristics. The results are shown in Table 1.
[0099]
Table 1
[0100] (Summary of Results) As can be seen from Table 1, by setting the intensity ratio I(111) / I(110) in the range of 0.2 < I(111) / I(110) < 0.35, high discharge characteristics can be obtained as a potassium-ion battery, and a high energy density can be obtained. [Industrial Applicability]
[0101] The positive electrode material for an alkali metal ion battery of the present invention is useful as a positive electrode for various alkali metal ion secondary batteries such as lithium ion, sodium ion, and potassium ion batteries.
Claims
1. General formula: KxAyDzPO 4 The compound represented by the formula: A positive electrode material for an alkali metal ion battery, in which the intensity ratio I(111) / I(110) of the 110 plane peak intensity I(110) appearing at 13.5 to 14.5° in an X-ray diffraction pattern to the 111 plane peak intensity I(111) appearing at 21.5 to 22.5° satisfies 0.2<I(111) / I(110)<0.
35. In the above general formula, A is at least one selected from the group consisting of Co, Mn, and Ni, D is at least one selected from the group consisting of Fe, Mg, Ca, Sr, Ba, Ti, Zn, B, Al, Ga, In, Si, Ge, Sc, and Y, and x, y, and z are within the range of 0.9<x<1.1, 0.65<y≦1.0, 0≦z<0.35, and 0.9<y+z<1.
1.
2. Specific surface area is 5m 2 / g or more and 30m 2 2. The positive electrode material for an alkali metal ion battery according to claim 1, wherein the molecular weight of the positive electrode material is 1 / g or less.
3. A positive electrode using the positive electrode material for an alkali metal ion battery according to claim 1 or 2.
4. The positive electrode according to claim 3 , An electrolyte containing at least one selected from the group consisting of Li ions, Na ions, and K ions; An alkali metal ion battery having
Citation Information
Patent Citations
Application of iron phosphate and iron phosphate composite material as negative electrodes in potassium ion battery
CN108063237A
Potassium ion secondary battery cathode active material and secondary battery
JP2019102247A
Aqueous electrolyte solution and aqueous potassium ion battery
JP2019220294A
Positive electrode active material for potassium secondary battery and potassium secondary battery including the same
JP2019523540A
Negative electrode for potassium ion secondary batteries, negative electrode for potassium ion capacitors, potassium ion secondary battery, potassium ion capacitor, and binder for negative electrodes of potassium ion secondary batteries or negative electrodes of potassium ion capacitors
WO2016059907A1