Composition for forming an electrode for a microbial fuel cell, an electrode for a microbial fuel cell, and a microbial fuel cell

The use of a graphite and carbon material composition with a binder improves electrode conductivity and durability in microbial fuel cells, addressing inefficiencies and cost issues, resulting in better power generation and microbial support.

JP7559490B2Active Publication Date: 2024-10-02TOYO INK MFG CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020172315
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-24
Filing Date
2020-10-13
Publication Date
2024-10-02
Estimated Expiration
2040-10-13

AI Technical Summary

Technical Problem

Existing microbial fuel cells face inefficiencies in electrode reactions, requiring improved conductivity, material diffusivity, and durability, with high costs and metal oxidation issues.

Method used

A composition for forming microbial fuel cell electrodes using a combination of graphite and other carbon materials with specific ratios and aspect ratios, along with a binder, to enhance conductivity and support microorganisms, optimizing surface morphology for improved power generation.

Benefits of technology

The solution provides electrodes with enhanced power generation characteristics and durability at a lower cost, promoting electron transfer and microbial adsorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559490000003
    Figure 0007559490000003
  • Figure 0007559490000001
    Figure 0007559490000001
  • Figure 0007559490000002
    Figure 0007559490000002
Patent Text Reader

Abstract

To provide an electrode formation composition, an electrode, and a microbial fuel cell having excellent power generation characteristics and durability at low cost.SOLUTION: In a microbial fuel cell electrode formation composition including a carbon material (A) and a binder (B), the carbon material (A) contains graphite (A-a) and a carbon material (A-b) other than graphite, and preferably the content of the graphite (A-a) in a total of 100 mass% of the carbon material (A) is 25 to 99 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming an electrode for a microbial fuel cell, an electrode for a microbial fuel cell, and a microbial fuel cell. [Background technology]

[0002] In recent years, the development of biofuel cells, such as biofuel cells using enzymes as biocatalysts and microbial fuel cells using microorganisms, has been progressing. Microbial fuel cells are a power generation method that recovers electrons generated when organic matter is decomposed by microorganisms called power-generating bacteria and uses them as electrical energy. For example, when used to purify domestic wastewater or industrial wastewater, the decomposition process of organic matter in the wastewater and power generation can be performed in parallel, so it is expected to be used as a water treatment method that can reduce energy consumption (Non-Patent Document 1). In addition, since microbial fuel cells can generate power using organic matter contained in water, bottom mud, soil, etc., they can also be expected to be used as a power source in wastewater or soil (Patent Document 1, Non-Patent Document 2).

[0003] In a microbial fuel cell, electrons are generated from an oxidation reaction by electricity-generating bacteria that decompose organic matter at the anode to extract electrons, and the generated electrons are consumed in a reduction reaction at the cathode via an external circuit from the electrode, where they react with oxidants such as oxygen and potassium ferricyanide.

[0004] The cathode and anode materials used in microbial fuel cells need to be conductive in the electrode reaction, and conductive materials are generally used (Patent Documents 1 to 3). Electrodes are made of carbon materials such as carbon paper, carbon felt, carbon cloth, or activated carbon sheets, or metal materials such as aluminum, copper, stainless steel, nickel, or titanium. In the anode, electricity-generating bacteria are used by contacting these materials (Patent Documents 2 and 3). In the cathode, it is also known to use these materials with oxygen reduction catalysts such as platinum supported on them. The efficiency of these electrode reactions is still insufficient, and improving the power generation characteristics is an issue. There are also problems such as deterioration due to metal oxidation and high costs.

[0005] To solve these problems, it is necessary to improve the electrode reaction efficiency, and it is required to improve the electrical conductivity and material diffusivity. Furthermore, it is desirable to increase the amount and activity of microorganisms carried on the anode. For example, Patent Document 4 discloses a laminate in which a non-conductive substrate is coated with a conductive part containing a conductive carbon material and a resin. However, further improvement of power generation efficiency remains an issue, and a technology that can also achieve durability that can maintain stable power generation efficiency is required. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-342412 A [Patent Document 2] JP 2010-102953 A [Patent Document 3] JP 2015-002070 A [Patent Document 4] International Publication No. 2016 / 129678 Brochure [Non-patent literature]

[0007] [Non-Patent Document 1] The cutting edge of wastewater treatment systems using microbial fuel cells, NTS Corporation [Non-Patent Document 2] Environmental Science&Technology,2004,38,4040-4046 Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide an electrode-forming composition, an electrode, and a microbial fuel cell that have excellent power generation characteristics and durability at low cost. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above-mentioned problems and have arrived at the present invention.

[0010] That is, the present invention relates to a composition for forming an electrode for a microbial fuel cell, comprising a carbon material (A) and a binder (B), wherein the carbon material (A) comprises graphite (Aa) and a carbon material other than graphite (Ab).

[0011] The present invention also relates to the composition for forming an electrode for a microbial fuel cell, wherein the content of graphite (Aa) in a total of 100% by mass of the carbon material (A) is 25 to 99% by mass.

[0012] The present invention also relates to the composition for forming an electrode for a microbial fuel cell, wherein the content of the carbon material (A) in 100% by mass of the total solid content of the composition is 80 to 99% by mass.

[0013] The present invention also relates to the composition for forming an electrode for a microbial fuel cell, wherein the aspect ratio of the graphite (Aa) is 1-10.

[0014] The present invention also relates to an electrode for a microbial fuel cell having a coating film of the above-mentioned composition for forming an electrode for a microbial fuel cell on a substrate.

[0015] The present invention also relates to a microbial fuel cell using the above-mentioned electrode for a microbial fuel cell. Effect of the Invention

[0016] According to the present invention, it is possible to provide an electrode-forming composition and an electrode having excellent power generation capacity and durability at low cost, and to provide a microbial battery having excellent power generation characteristics and durability. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a diagram showing the structure of the microbial fuel cell used in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described in detail.

[0019] <Composition for forming microbial fuel cell electrode> The composition for forming a microbial fuel electrode of the present invention (hereinafter, electrode composition) contains at least graphite (Aa), a carbon material other than graphite (Ab), and a binder (B). In the present invention, by using graphite (Aa), a carbon material other than graphite (Ab), and a binder (B) in combination, the conductivity of the electrode can be improved, and the surface morphology can be optimized to improve substance diffusibility. In addition, the adhesion between the carbon materials (A) and with the substrate is strengthened, improving durability. Furthermore, since the carbon material (A) in the electrode has a high affinity with microorganisms, a large number of microorganisms can be supported. Due to these effects, according to the present invention, it is possible to improve the durability as well as the power generation characteristics of the microbial fuel cell.

[0020] <Carbon material (A)> The carbon material (A) increases the surface area of ​​the electrode and promotes the transfer of electrons in the redox reaction. In addition, when used as an anode, the surface morphology and biocompatibility can increase the adsorption of microorganisms. The carbon material (A) contains graphite (Aa) and a carbon material other than graphite (Ab). Examples of the graphite (Aa) include artificial graphite and natural graphite, and examples of the carbon material other than graphite (Ab) include carbon black, activated carbon, conductive carbon fibers (carbon nanotubes, carbon nanofibers, carbon fibers), graphene, fullerene, carbon catalysts, and the like. These can be used alone or in combination of two or more types. By using the graphite (Aa) in combination with the carbon material other than graphite (Ab), the electron path inside the electrode becomes dense, and the material diffusion is also increased due to the favorable surface morphology, so that high power generation characteristics can be obtained.

[0021] The content of graphite (Aa) in the carbon material (A) ((Aa) / (A)×100) is preferably 25 to 99 mass %, more preferably 50 to 90 mass %, and further preferably 60 to 85 mass %.

[0022] As the graphite (Aa), for example, artificial graphite, natural graphite, etc. can be used. Artificial graphite is obtained by artificially orienting irregularly arranged fine graphite crystals by heat treatment of amorphous carbon, and is generally produced using petroleum coke or coal-based pitch coke as the main raw material. Natural graphite is classified into scaly graphite, semi-scaly graphite, and earthy graphite, and scaly graphite includes scaly graphite and lump graphite. In addition, spherical graphite obtained by scaly graphite being scaly graphite scaly graphite being scaly graphite being chemically treated, expanded graphite (also called expandable graphite), expanded graphite obtained by heat-treating expanded graphite and then micronizing or pressing, etc. can also be used. Among these graphites, natural graphite is preferable from the viewpoint of electrical conductivity, and flaky graphite such as spherical graphite, scaly graphite, and expanded graphite are preferable.

[0023] The aspect ratio of graphite (Aa) is preferably 1 to 10, and more preferably 1 to 5. The aspect ratio is a value expressed by x / y, where x is the longest diameter of the particle and y is the shortest diameter. Particles with a large aspect ratio are generally easy to orient, but when the aspect ratio is smaller than 10, the graphite particles on the electrode surface are difficult to orient, and the surface unevenness increases, so that the surface area of ​​the electrode increases and the reaction points increase. In particular, when used as an anode, the amount of attached microorganisms increases due to the optimal surface morphology. From the viewpoint of aspect ratio, artificial graphite and spherical graphite are preferable as graphite (Aa).

[0024] The aspect ratio can be measured, for example, as follows: Particles are photographed with a scanning electron microscope, and for 10 particles in an arbitrarily selected area, x / y is calculated, where x is the longest diameter of each particle and y is the shortest diameter. The average of the 10 x / y values ​​is taken as the aspect ratio of the sample.

[0025] The average particle size of the graphite (Aa) used is preferably from 0.5 to 500 μm, and particularly preferably from 2 to 100 μm.

[0026] The average particle size is the particle size (D50) at which the volume ratio of particles is 50% when the volume ratio of particles is accumulated from the finest particle size in the volume particle size distribution, and is measured with a general particle size distribution meter, for example, a dynamic light scattering particle size distribution meter ("Microtrac UPA" manufactured by Nikkiso Co., Ltd.).

[0027] Examples of commercially available graphite include scaly graphite such as CMX, UP-5, UP-10, UP-20, UP-35N, CSSP, CSPE, CSP, CP, CB-150, CB-100, ACP, ACP-1000, ACB-50, ACB-100, ACB-150, SP-10, SP-20, J-SP, SP-270, HOP, GR-60, LEP, F#1, F#2, F#3, and FB-150 manufactured by Nippon Graphite Industries Co., Ltd., and CX-3000, FBF, BF, CBR, SSC-3000, and SSC-600 manufactured by Chuetsu Graphite Co., Ltd. , SSC-3, SSC, CX-600, CPF-8, CPF-3, CPB-6S, CPB, 96E, 96L, 96L-3, 90L-3, CPC, S-87, K-3, CF-80, CF-48, CF-32, CP-150, CP-100, CP, HF-80, HF-48, HF-32, SC-120, SC-80, SC-60, SC-32, EC1500, EC1000, EC500, EC300, EC100, EC50 manufactured by Ito Graphite Industries Co., Ltd., 10099M, PB-99 manufactured by Nishimura Graphite Co., Ltd., etc. Examples of spherical graphite include CGC-20, CGC-50, CGB-20, and CGB-50 manufactured by Nippon Graphite Industries Co., Ltd. Examples of amorphous graphite include Blue P, AP, AOP, and P#1 manufactured by Nippon Graphite Industries Co., Ltd., and APR, S-3, AP-6, and 300F manufactured by Chuetsu Graphite Co., Ltd. Examples of artificial graphite include PAG-60, PAG-80, PAG-120, PAG-5, HAG-10W, and HAG-150 manufactured by Nippon Graphite Industries Co., Ltd.; RA-3000, RA-15, RA-44, GX-600, G-6S, G-3, G-150, G-100, G-48, G-30, and G-50 manufactured by Chuetsu Graphite Co., Ltd.; and SGP-100, SGP-50, SGP-25, SGP-15, SGP-5, SGP-1, SGO-100, SGO-50, SGO-25, SGO-15, SGO-5, SGO-1, SGX-100, SGX-50, SGX-25, SGX-15, SGX-5, and SGX-1 manufactured by SEC Carbon Co., Ltd.

[0028] The carbon material (Ab) other than graphite is not particularly limited, but a conductive carbon material is preferable, and it is preferable to use carbon black or conductive carbon fiber from the viewpoints of cost, conductivity, etc. When the electrode is used as a cathode, it is preferable to use a carbon catalyst in order to increase the oxygen reduction catalytic activity.

[0029] Carbon black can be produced by continuously pyrolyzing a gaseous or liquid raw material in a reactor, in particular Ketjen black made from ethylene heavy oil, channel black made by burning a raw material gas and applying the flame to the bottom surface of a channel steel to rapidly cool and precipitate, thermal black made from a gas raw material by periodically repeating combustion and pyrolysis, in particular acetylene black made from acetylene gas, and other various types can be used alone or in combination. In addition, carbon black that has been subjected to a commonly performed oxidation treatment, hollow carbon, etc. can also be used. The oxidation treatment of carbon black is a treatment in which oxygen-containing polar functional groups such as phenol groups, quinone groups, carboxyl groups, and carbonyl groups are directly introduced (covalently bonded) to the carbon black surface by treating carbon black at a high temperature in air or secondary treatment with nitric acid, nitrogen dioxide, ozone, etc., and is generally performed to improve the dispersibility of carbon black. However, it is generally the case that the conductivity of carbon black decreases as the amount of functional groups introduced increases, so it is preferable to use carbon black that has not been subjected to an oxidation treatment.

[0030] The larger the specific surface area of ​​the carbon black used, the more contact points there are between the carbon material particles, which is advantageous for lowering the internal resistance of the electrode, but the dispersibility of the carbon black decreases. Therefore, the preferred range of the specific surface area is specifically 10 to 3000 m in terms of the specific surface area (BET) calculated from the amount of nitrogen adsorption. 2 / g, more preferably 20 to 1500m 2 The specific surface area can be measured by the BET method (JIS Z 8803:2013) using nitrogen gas as the adsorbate.

[0031] The particle size of the carbon black used is preferably 0.005 to 1 μm, particularly preferably 0.01 to 0.2 μm, in terms of primary particle size, where the primary particle size is the average particle size measured with an electron microscope or the like.

[0032] Examples of commercially available carbon black include Tokai Carbon's Tokablack #4300, #4400, #4500, and #5500; Degussa's Printex L; and Colombian's Raven7000, 5750, 5250, 5000ULTRAIII, and 500. 0ULTRA, Conductex SC ULTRA, Conductex 975 ULTRA, PUER Examples of the black include furnace blacks such as BLACK100, 115, and 205; #2350, #2400B, #2600B, #3050B, #3030B, #3230B, #3350B, #3400B, and #5400B manufactured by Mitsubishi Chemical Corporation; MONARCH1400, 1300, and 900, VulcanXC-72R, and BlackPearls2000 manufactured by Cabot Corporation; Ensaco250G, Ensaco260G, Ensaco350G, and SuperP-Li manufactured by TIMCAL Corporation; ketjen blacks such as EC-200L, EC-300J, and EC-600JD manufactured by Lion Specialty Chemicals; and acetylene blacks such as Denka Black, Denka Black HS-100, and FX-35 manufactured by Denka Co., Ltd., but are not limited to these. Two or more of the blacks may be used in combination.

[0033] Specific examples of activated carbon include activated phenol-based, coconut shell-based, rayon-based, acrylic-based, coal-petroleum pitch coke, mesocarbon microbeads (MCMB), and the like. Activated carbon with a large specific surface area is preferred, since it is possible to form a larger interface with the same mass. Specifically, activated carbon with a specific surface area of ​​30 m 2 / g or more is preferable, More preferably, 500 to 5,000 m 2 / g, more preferably 1000 to 3000m 2 / g.

[0034] Conductive carbon fibers are preferably obtained by firing petroleum-derived raw materials, but those obtained by firing plant-derived raw materials can also be used. Carbon nanotubes include single-walled carbon nanotubes, which form tubes with a diameter in the nanometer range with one graphene sheet, and multi-walled carbon nanotubes, which form tubes with multiple graphene sheets. Therefore, the diameter of multi-walled carbon nanotubes is large, at 30 nm, compared to 0.7 to 2.0 nm for typical single-walled carbon nanotubes.

[0035] Examples of commercially available conductive carbon fibers and carbon nanotubes include vapor grown carbon fibers such as VGCF manufactured by Showa Denko K.K.; single-walled carbon nanotubes such as EC1.0, EC1.5, EC2.0, and EC1.5-P manufactured by Meijo Nano Carbon K.K.; FloTube9000, FloTube9100, FloTube9110, and FloTube9200 manufactured by CNano; NC7000 manufactured by Nanocyl Corporation; and 100T manufactured by Knano Corporation.

[0036] The carbon catalyst is a carbon catalyst produced by mixing one or more kinds of carbon materials with a compound containing a nitrogen element and a base metal element and subjecting the mixture to a heat treatment, and a conventionally known carbon catalyst can be used. The carbon material used for the carbon catalyst is not particularly limited as long as it is a carbon particle derived from an inorganic material and / or a carbon particle obtained by subjecting an organic material to a heat treatment. In general, examples of the active site of a carbon catalyst include a base metal element contained in a base metal-N4 structure (a structure in which four nitrogen elements are arranged on a plane with a base metal element at the center) on the surface of a carbon particle, and a carbon element in the vicinity of a nitrogen element introduced to an edge portion of the carbon particle surface. Therefore, it is important for the carbon catalyst to contain the nitrogen element and base metal element that constitute the active site in order to have oxygen reduction activity. Furthermore, the carbon catalyst should have a BET specific surface area of ​​20 to 2000 m. 2 / g is preferable, and 40 to 1000m 2 / g is more preferable, and 60 to 600m 2 / g is more preferred.

[0037] The average specific surface area of ​​the carbon material (A) is 5 to 300 m2 / g is preferable, and 5 to 100m 2 / g is even more preferable. Here, the average specific surface area of ​​the carbon material (A) refers to the arithmetic mean of the specific surface areas of two or more types of carbon materials (A) contained in the electrode composition. As an example, the case where C1 and C2 are used as the carbon materials (A) will be shown. When the specific surface area of ​​C1 is A1 m 2 / g, the amount of C1 added to the composition is B1 g, and the specific surface area of ​​C2 is A2 m 2 / g and the amount of B added is 2 g, the average specific surface area of ​​the carbon material (A) is expressed by the following formula 1. (A1×B1+A2×B2) / (B1+B2) …Formula 1

[0038] The average specific surface area of ​​the carbon material (A) is 5 m 2 When the average specific surface area of ​​the carbon material (A) is 300 m / g or more, the surface area of ​​the electrode is increased, and the redox reaction is promoted. 2 When the content is 100m / g or less, the strength of the electrode is improved. 2 When the surface morphology of the electrode is less than 1 / g, the surface morphology of the electrode becomes rough, and the adsorption of microorganisms is improved.

[0039] <Binder (B)> The type of binder (B) is not particularly limited as long as it can impart dispersibility of the carbon material (A), stability of the electrode composition, adhesion to the substrate, and flexibility to the electrode, and examples of the binder include binder resins.

[0040] The binder resin may include one or more selected from the group consisting of polyurethane resin, polyamide resin, acrylonitrile resin, acrylic resin, butadiene resin, polyvinyl resin, polyvinyl butyral resin, polyolefin resin, polyester resin, polystyrene resin, EVA resin, polyvinylidene fluoride resin, polytetrafluoroethylene resin, silicone resin, polyether resin, cellulose resin such as carboxymethyl cellulose, etc. However, it is not limited to these resins. The binder resin may be used alone or in combination of two or more. As the binder resin, a non-fluoride resin is preferable from the viewpoint of cost and adhesion.

[0041] The binder resin may be a curable resin that undergoes a curing (crosslinking) reaction after the binder resin is applied to the substrate. The binder resin may be a soluble resin that dissolves in an aqueous or non-aqueous solvent or a dispersion-type resin fine particle. Dispersion-type resin fine particles are resin fine particles that do not dissolve in an aqueous or non-aqueous dispersion medium and exist in the form of fine particles, and the dispersion is generally called an emulsion. These may be used alone or in combination of two or more.

[0042] The particle structure of the dispersion type resin fine particles can be a multi-layer structure, so-called core-shell particles. For example, by localizing a resin obtained by mainly polymerizing a monomer having a functional group in the core or shell, or by providing a difference in Tg or composition between the core and the shell, it is possible to improve the curability, drying property, film-forming property, and mechanical strength of the binder. From the viewpoint of binding property and particle stability, the average particle diameter of the resin fine particles is preferably 10 to 1000 nm, and more preferably 10 to 300 nm. In addition, since the stability of the particles is impaired when a large amount of coarse particles exceeding 1 μm are contained, it is preferable that the amount of coarse particles exceeding 1 μm is at most 5% or less. The average particle diameter can be measured as follows. Depending on the solid content of the resin fine particles, the resin fine particles are diluted 200 to 1000 times with the same dispersion liquid as the dispersion medium. About 5 ml of the diluted dispersion liquid is poured into the cell of a measuring device (Nanotrack manufactured by Nikkiso Co., Ltd.), and the dispersion medium and the refractive index conditions of the resin according to the sample are input, and then the measurement is performed. The particle size can be measured based on the peak of the volume particle size distribution data (histogram) obtained at this time.

[0043] The dispersed resin particles preferably contain crosslinked resin particles. The crosslinked resin particles refer to resin particles having an internal crosslinked structure (three-dimensional crosslinked structure), and it is important that the particles are crosslinked inside. In addition, the crosslinked resin particles contain specific functional groups, which can contribute to adhesion with other electrode constituent materials and substrates. Furthermore, by adjusting the amount of the crosslinked structure and functional groups, excellent durability of the battery can be obtained.

[0044] From the viewpoint of wettability and permeability to the electrolyte, it is preferable to use, as the binder (B), a water-soluble resin (Ba) that can be dissolved in an aqueous solvent, or aqueous resin fine particles (Bb) that do not dissolve in an aqueous dispersion medium and exist in the form of fine particles. Also, from the viewpoint of the slurry stability and coatability of the electrode composition, and the water resistance and flexibility of the electrode, it is more preferable to use the water-soluble resin (Ba) and the aqueous resin fine particles (Bb) in combination.

[0045] (Water-soluble resin (Ba)) Water-soluble resin (Ba) is a resin that can be completely dissolved in water without separation or precipitation after 1 g of resin is added to 99 g of water at 25°C, stirred, and left at 25°C for 24 hours.

[0046] The water-soluble resin (Ba) has the effect of increasing the dispersibility of the carbon material (A), so a stable composition can be obtained with a small amount of resin, and the conductivity of the electrode is improved. In addition, when an electrode containing the water-soluble resin (Ba) is immersed in water, the high affinity of the water-soluble resin for water improves the wettability of the electrode to the electrolyte, and a flow path is formed due to the swelling and elution of the water-soluble resin, so that an electrode with excellent diffusion of protons required for power generation in a microbial fuel cell can be provided. In addition, the high affinity of the water-soluble resin (Ba) for microorganisms promotes the attachment and growth of microorganisms to the anode, so that many microorganisms can be supported, and the binding between the microorganisms and the carbon material (A) and the substrate is also strengthened.

[0047] The water-soluble resin (Ba) is roughly classified into anionic resin, cationic resin, amphoteric resin having both anionic and cationic properties, and other nonionic resin, and further, the resin may be composed of a plurality of monomers. Moreover, the water-soluble resin (Ba) may be used alone or in combination of two or more kinds.

[0048] Examples of anionic resins include resins containing a carboxyl group, a sulfo group, a phosphoric acid group, and a skeleton in which these groups are partially or completely neutralized. Examples of such resins include homopolymers of polymerizable monomers such as (meth)acrylic acid, itaconic acid, fumaric acid, maleic acid, 2-sulfoethyl methacrylate, and 2-methacryloyloxyethyl acid phosphate, copolymers with other polymerizable monomers, carboxymethyl cellulose, and alkali-neutralized products thereof.

[0049] Examples of cationic resins include resins containing cyclic amino groups, skeletons in which amino groups are partially or completely neutralized, and quaternary ammonium salts. Examples include homopolymers of polymerizable monomers such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethyl (meth)acrylate, and vinylpyridine, copolymers with other polymerizable monomers, and acid-neutralized products thereof.

[0050] The amphoteric resin may be a resin containing both the anionic skeleton and the cationic skeleton, such as a copolymer of styrene, maleic acid, and N,N-dimethylaminoethyl (meth)acrylate.

[0051] The nonionic resin is a resin other than the anionic, cationic and amphoteric resins. Examples of the nonionic resin include polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl butyral, polyacrylamide, poly-N-vinylacetamide, polyalkylene glycol, etc.

[0052] The molecular weight of the water-soluble resin (Ba) is not particularly limited, but the mass average molecular weight is preferably 5,000 to 2,500,000. The mass average molecular weight (Mw) refers to the molecular weight calculated as polyethylene oxide by gel permeation chromatography (GPC).

[0053] (Aqueous resin fine particles (Bb)) The aqueous resin particles are dispersion-type resin particles in which the resin does not dissolve in water but exists in the form of fine particles, and are also called water-dispersed resin particles. The aqueous dispersion is generally called an aqueous emulsion.

[0054] Examples of the aqueous resin particles (Bb) include (meth)acrylic emulsions, nitrile emulsions, urethane emulsions, polyolefin emulsions, fluorine emulsions (polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE)), diene emulsions (styrene-butadiene rubber (SBR)), etc. Here, (meth)acrylic means methacrylic or acrylic.

[0055] When a coating film is formed, the electrode composition containing the aqueous resin fine particles (Bb) has excellent adhesion between particles and with the substrate, and can provide an electrode with high strength. In addition, since the binding between the aqueous resin fine particles (Bb) and the carbon material (A) is by point contact, it is difficult to inhibit the reaction in which the interface is the reaction field. In addition, it is possible to form a surface morphology to which microorganisms can easily adhere. Furthermore, since the aqueous resin fine particles (Bb) have excellent adhesion, only a small amount of the aqueous resin fine particles (Bb) is required, and as a result, the conductivity of the electrode is improved. Furthermore, the aqueous resin fine particles can be produced inexpensively depending on the monomer that constitutes them, so the manufacturing cost of the electrode can be reduced. In order to obtain the above-mentioned effects, the aqueous resin fine particles (Bb) are preferably (meth)acrylic emulsions or urethane emulsions, which have excellent binding between particles and flexibility (flexibility of the film).

[0056] The (meth)acrylic emulsion is an emulsion polymer containing 10 parts by mass or more of a monomer having a (meth)acryloyl group, preferably 20 parts by mass or more, more preferably 30 parts by mass or more. The monomer having an acryloyl group has excellent reactivity, so that resin microparticles can be relatively easily produced. Therefore, the (meth)acrylic emulsion is particularly preferable as the aqueous resin microparticle (Bb).

[0057] <Solvent (dispersion medium)> When the conductive carbon material (A) and the binder (B) are mixed uniformly, a solvent can be appropriately used. Such a solvent is not particularly limited as long as it can dissolve the resin or stably disperse the resin fine particle emulsion, and examples of the solvent include water and organic solvents.

[0058] The organic solvent can be appropriately selected from among alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol methyl ether, and diethylene glycol methyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether; hydrocarbons such as hexane, heptane, and octane; aromatics such as benzene, toluene, xylene, and cumene; and esters such as ethyl acetate and butyl acetate, depending on the composition of the conductive composition. The solvent may be water and an organic solvent, or two or more organic solvents may be used.

[0059] When the water-soluble resin (Ba) or the aqueous resin particles (Bb) are used, it is preferable to use water as a solvent from the viewpoint of solubility and dispersibility, and a liquid medium compatible with water may be added as necessary. As the liquid medium compatible with water, an alcohol-based solvent having a carbon number of 4 or less is preferable.

[0060] In addition, various additives such as ultraviolet absorbers, ultraviolet stabilizers, radical scavengers, fillers, thixotropy-imparting agents, antiaging agents, antioxidants, antistatic agents, flame retardants, thermal conductivity improvers, plasticizers, anti-sagging agents, antifouling agents, preservatives, bactericides, defoamers, leveling agents, antiblocking agents, curing agents, thickeners, dispersants, and silane coupling agents may be added to the electrode composition of the present invention, if necessary, within a range that does not impair the effects of the present invention.

[0061] <Composition of electrode composition> The content of the carbon material (A) is preferably 50% by mass or more, more preferably 80 to 99% by mass, and particularly preferably 85 to 99% by mass, based on 100% by mass of the total solid content of the electrode composition, in terms of electrical conductivity and adhesion to the substrate. When the content of the carbon material (A) is 50% by mass or more, the electron path inside the electrode is developed, and sufficient electrical conductivity is obtained. When the content of the carbon material (A) is 80% by mass or more, the carbon material (A) is exposed on the surface, increasing the electron path between the carbon material (A) and the microorganism, and promoting the anode reaction, thereby improving the power generation characteristics of the battery. From the viewpoint of electrical conductivity, the content of graphite (Aa) is preferably 25 to 99 mass%, more preferably 50 to 90 mass%, and particularly preferably 60 to 85 mass% relative to 100 mass% of the total carbon material (A). By using graphite (Aa) in combination with a carbon material other than graphite (Ab) within a suitable range, packing inside the electrode is improved, improving electrical conductivity. Furthermore, a suitable surface morphology is formed, which enhances substance diffusibility and microbial adsorption, improving reactivity, and obtaining high power generation characteristics. The content of the binder (B) is preferably 0.1 to 50 mass%, more preferably 0.5 to 20 mass%, and particularly preferably 1 to 15 mass%, relative to 100 mass% of the total solid content of the electrode composition, in terms of electrical conductivity, adhesion to the substrate, etc.

[0062] When the water-soluble resin (Ba) is contained, its content is preferably 0.1 to 30 mass%, more preferably 0.5 to 20 mass%, and particularly preferably 1 to 15 mass%, based on 100 mass% of the total solid content of the electrode composition. When the content of the water-soluble resin is 0.1 mass% or more, as described above, a larger amount of microorganisms can be supported, and an anode with good proton diffusivity can be obtained. When the content of the water-soluble resin is 30 mass% or less, an anode with good durability in the electrolyte can be obtained. When the aqueous resin fine particles (Bb) are contained, the content thereof is preferably 0.5 to 40 mass%, more preferably 1 to 30 mass%, and particularly preferably 2 to 25 mass%, based on 100 mass% of the total solid content of the electrode composition. When the content of the aqueous resin fine particles is 0.5 mass% or more, the strength of the anode is improved. When the content of the aqueous resin fine particles is 40 mass% or less, good electrical conductivity is obtained. Furthermore, when the content of the aqueous resin fine particles is 30 mass% or less, a surface morphology suitable for adsorption of microorganisms is formed by point-bonding between the aqueous resin fine particles and the carbon material (A). Furthermore, when the content of the aqueous resin fine particles is 25 mass% or less, a larger amount of the carbon material (A) is exposed on the coating surface, and thus the oxidation-reduction reaction is promoted. In addition, when both the water-soluble resin (Ba) and the aqueous resin fine particles (Bb) are contained, it is preferable to contain more aqueous resin fine particles (Bb) than the water-soluble resin (Ba) since this improves the substance diffusibility.

[0063] The electrode composition may contain any component other than the carbon material (A) and the binder (B). From the viewpoints of electrical conductivity, adhesion, and the like, the total proportion of the carbon material (A) and the binder (B) to the total solid content of the electrode composition is preferably 50 mass % or more, and more preferably 80 mass % or more.

[0064] The appropriate viscosity of the electrode composition depends on the method of coating the composition, but in general it is preferable that it be 10 mPa·s or more and 30,000 mPa·s or less.

[0065] <Method of preparing electrode composition> There is no particular limitation on the method for preparing the electrode composition. (1) Each component may be dispersed simultaneously; (2) After dispersing the carbon material (A) in the solvent, other materials may be added. (3) After dispersing the carbon material (A) and the binder (B) in a solvent, other materials may be added. This can be optimized by using the carbon material (A) and binder (B). When using the water-soluble resin (Ba) or the aqueous resin fine particles (Bb), adding the aqueous resin fine particles (Bb) after dispersing the carbon material (A) and the water-soluble resin (Ba) in an aqueous liquid medium can contribute greatly to cost reduction, for example by shortening the dispersion time.

[0066] <Dispersing machine / mixer> As the apparatus used in obtaining the electrode composition, a dispersing machine or a mixer that is generally used for dispersing pigments or the like can be used.

[0067] For example, mixers such as a Disper, Homomixer, or Planetary Mixer; homogenizers such as M-Technique's "Clearmix" or PRIMIX's "Filmix"; media-type dispersers such as a paint conditioner (Red Devil), ball mill, sand mill (Shinmaru Enterprises' "Dynomill", etc.), attritor, pearl mill (Eirich's "DCP Mill", etc.), or Coball mill; media-less dispersers such as wet jet mills (Zenus' "Zenus PY", Sugino Machine's "Starburst", Nanomizer's "Nanomizer", etc.), M-Technique's "Clear SS-5", or Nara Machine's "MICROS"; or other roll mills, but are not limited to these.

[0068] For example, when using a media-type disperser, it is preferable to use a method in which a disperser with an agitator and a vessel made of ceramic or resin is used, or a disperser in which the surface of a metal agitator and a vessel is treated with tungsten carbide spraying or resin coating is used. As the media, it is preferable to use ceramic beads such as glass beads, zirconia beads, or alumina beads. Also, when using a roll mill, it is preferable to use a ceramic roll. Only one type of dispersing device may be used, or multiple types of devices may be used in combination. Also, when the particles are easily broken or crushed by strong impact, a media-less dispersing device such as a roll mill or a homogenizer is preferable to a media-type dispersing device.

[0069] <Electrode manufacturing method> Next, a method for producing an electrode from the electrode composition will be described. The electrode can be produced using a conventionally known method, and is not particularly limited. For example, (1) An electrode prepared by applying an electrode composition to a substrate, (2) An electrode obtained by forming the electrode composition into a pellet shape, (3) An electrode prepared by wrapping a pellet-shaped electrode composition in a conductive substrate; (4) An electrode prepared by encapsulating a pellet-shaped electrode composition in a conductive substrate having a frame or basket shape; etc. In particular, for anodes involving microorganisms, for example, the anode may be prepared after mixing the microorganisms into the electrode composition, or the electrode may be prepared in advance as described above, and then the microorganisms may be added or inoculated. Also, the electrode may be placed in soil and then function as an anode by adsorption of the microorganisms in the soil.

[0070] <Base material> The substrate used in the electrode may be a conductive substrate or a non-conductive substrate.

[0071] The conductive substrate functions as a current collector. The conductive substrate is preferably one that has excellent corrosion resistance and electrical conductivity, a large surface area, and excellent diffusion of reactants and products, and the material and shape are not particularly limited. For example, carbon materials such as graphite paper (carbon paper), graphite cloth (carbon cloth), and graphite felt (carbon felt) can be used, as well as metal materials such as stainless steel mesh, copper mesh, and platinum mesh, but this is not limited thereto. The conductive substrate used for the electrode may be water-repellent in advance. For example, the cathode is impregnated with a dispersion of PTFE, and the water-repellency is expressed by heating at about 400°C after drying. A conductive material may also be dispersed in the PTFE dispersion. The water-repellent treatment is not limited to these.

[0072] Alternatively, a composition capable of forming a conductive coating or a conductive polymer such as polyaniline, polyacetylene, polypyrrole, or polythiophene may be applied to a non-conductive support such as paper, cloth, or resin film and then dried, or a combination of these may be used.

[0073] As the non-conductive substrate, the same materials as the non-conductive supports described above can be used.

[0074] As the substrate, a conductive substrate having a non-conductive support and a non-conductive substrate are preferred from the viewpoints of cost and corrosion resistance.

[0075] <Coating method> The method of applying (coating) the electrode composition of the present invention to a substrate is not particularly limited, and any known method can be used. Examples include gravure coating, spray coating, screen printing, dip coating, die coating, roll coating, doctor coating, knife coating, screen printing, and electrostatic painting, and drying methods include, but are not limited to, standing drying, air blowing dryer, hot air dryer, infrared heater, and far-infrared heater.

[0076] The volume resistivity of the electrode for the microbial fuel cell of the present invention is 5×10 1 It is preferably less than 5×10 Ω cm, and more preferably less than 5×10 0 Less than Ω cm, preferably less than 1×10 -1 The better the conductivity of the electrode, the more effectively it is possible to extract electricity.

[0077] <Microbial fuel cell> As shown in FIG. 1, the microbial fuel cell of the present invention uses an anode, a cathode, an electrolyte, an external resistor, and the like. The anode contains a microorganism, and the cathode contains a reduction catalyst. The anode and the cathode are in contact with each other via an electrolyte, and the cathode is disposed in a position where it can come into contact with an oxidizing agent. As the oxidizing agent, oxygen present in the atmosphere is preferably used. In addition, the anode and the cathode are electrically connected via an external resistor. Here, the external resistor refers to the electrical resistance in an electric circuit.

[0078] At the anode, organic matter is oxidized and decomposed by the metabolism of microorganisms, and electrons and protons are generated at the same time. The generated electrons are taken up by the anode and move to the cathode via an external resistor. The generated protons pass through the electrolyte and move to the cathode. At the cathode, the electrons and protons transferred from the anode side react with an oxidant near the cathode due to the action of a reduction catalyst. As the above reaction is repeated, an electromotive force is generated between the cathode and the anode.

[0079] The electrolyte used in the microbial fuel cell contains a substrate that has proton conductivity and is oxidatively decomposed by microorganisms. The substrate is not particularly limited as long as it is a substance that can be metabolized by the microorganism that donates electrons. For example, organic substances such as sugars, proteins, and lipids, as well as inorganic substances such as ammonia, may be included, and one or more of these may be included. Therefore, the electrolyte may be domestic wastewater, industrial wastewater, environmental wastewater (ponds, lakes, rivers, seas), soil, sludge, etc. that satisfy the above conditions. In addition, a mediator that is responsible for electron transfer between the microorganisms and the anode may be introduced, and examples of such mediators include methylene blue and neutral red.

[0080] The microorganisms that donate electrons at the anode may be of a single species or a plurality of species, so long as they cause an anode reaction that oxidizes and decomposes the substrate to generate electrons. The microorganisms are retained in the electrolytic cell by floating in the electrolytic cell or by being immobilized on the anode. The microbial species is not particularly limited, but examples include those belonging to the genera Shewanella and Geobacter.

[0081] The catalyst that can be used in the cathode is not particularly limited as long as it functions as a microbial fuel cell, but an oxygen reduction catalyst will be described as an example. Examples of oxygen reduction catalysts include precious metal catalysts, base metal oxide catalysts, carbon catalysts, activated carbon, and reducing enzymes. These may be used alone or in combination of two or more types.

[0082] The microbial fuel cell may be configured as a single tank type in which an anode holding an electron donor microorganism and a cathode containing a catalyst material are inserted into an electrolytic cell containing organic wastewater or the like as an electrolyte without a partition, or as a two tank type in which an anode tank and a cathode tank are separated by a solid polymer membrane, as in a solid polymer fuel cell. Furthermore, it may be an environment that is not enclosed, such as a rice field, a lake, a river, or the sea, as well as an electrolytic cell surrounded by a surface. For example, a cathode may be installed on the liquid surface, side, or bottom surface that separates the inside of the electrolytic cell holding the electrolyte from the outside of the electrolytic cell, such as the atmosphere containing oxygen, or a cassette-type electrode that can take in outside air may be immersed in the liquid. At this time, the catalyst layer of the cathode is installed so that it is in contact with the electrolyte, and the back surface is in contact with the atmosphere containing oxygen. As a result, the atmosphere containing oxygen flows directly into the cathode from the outside of the electrolytic cell, and a reaction occurs on the catalyst in the cathode in contact with the electrolyte. EXAMPLES

[0083] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the present invention in any way.

[0084] <Carbon materials for electrodes> [Manufacturing Example A1] (Preparation of carbon material (1)) Graphene nanoplatelet xGnP-C-750 (manufactured by XGscience Co., Ltd.) and iron phthalocyanine P-26 (manufactured by Sanyo Pigment Co., Ltd.) were mixed in a mass ratio of 1 / 0.5 (graphene nanoplatelet The mixture was then filled into an alumina crucible and heat-treated in an electric furnace under a nitrogen atmosphere at 800°C for 2 hours to obtain a carbon material (1). The specific surface area of ​​the carbon material (1) was 220 m 2 / g.

[0085] <Preparation of electrode composition> [Example 1] 12% by mass of spherical graphite CGB-50 (manufactured by Nippon Graphite Co., Ltd.) as graphite (Aa), 3% by mass of acetylene black HS-100 (manufactured by Denka Co., Ltd.) as carbon material other than graphite (Ab), 5% by mass of KF polymer #9200 (manufactured by Kureha Co., Ltd.) which is polyvinylidene fluoride as binder (B), and 80% by mass of N-methylpyrrolidone as solvent were mixed in a mixer to obtain an electrode composition (1) with a solid content of 20% by mass.

[0086] [Examples 2 to 27, Comparative Examples 1 and 2] Using graphite (Aa), a carbon material other than graphite (Ab), a binder (B), and a solvent shown in Table 1, electrode compositions (2) to (29) were prepared in the same manner as electrode composition (1).

[0087] [Table 1]

[0088] <Preparation of electrodes for microbial fuel cells>

[0089] [Examples 28 to 45, 48 to 54, Comparative Examples 3 and 4] The electrode compositions (1) to (18), (21) to (29) of Examples 1 to 18, 21 to 27 and Comparative Examples 1 and 2 were applied in a coating amount of 2 mg / cm on a 100 μm-thick PET film (size 10 cm × 10 cm) as a non-conductive substrate. 2After adding the components so as to obtain the above, the mixture was dried by heating at 110° C. for 10 minutes to prepare electrodes for microbial fuel cells (1) to (18) and (21) to (29).

[0090] [Examples 46 and 47] The electrode compositions (19) and (20) of Examples 19 and 20 were applied in a coating amount of 2 mg / cm on a conductive carbon paper substrate (size 10 cm x 10 cm, manufactured by Toray Industries, Inc.). 2 After adding the components so that the total amount of the electrolyte was 100%, the mixture was dried by heating at 110°C for 10 minutes to prepare electrodes for microbial fuel cells (19) and (20).

[0091] The coating of the microbial fuel cell electrode (28) peeled off, so further evaluation was not performed.

[0092] [Manufacturing example B1] 12% by mass of carbon material (1), 40% by mass of Nafion (registered trademark) (20% by mass solution), 24% by mass of water, and 24% by mass of 1-propyl alcohol were mixed in a mixer to obtain a cathode composition (1). The cathode composition (1) was added onto carbon felt LFP-210 (size 10 cm × 10 cm, manufactured by Osaka Gas Chemicals Co., Ltd.), and then heated and dried at 110°C for 10 minutes to obtain a cathode (1) for a microbial fuel cell (basis weight 10 mg / cm 2 ) was prepared.

[0093] <Microbial fuel cell> [Example 55] The evaluation was carried out using the microbial fuel cell shown in Figure 1. 400 g of soil (Flower and Vegetable Soil: Akagi Farm Co., Ltd.), a cathode, and an anode were placed in a 500 mL container, and 250 g of tap water as an electrolyte was added to the soil to create a microbial fuel cell. The anode used was a microbial fuel cell electrode (1), and the cathode used was a microbial fuel cell cathode (1). Next, wiring was attached to the cathode and anode and connected to an external resistor (1 kΩ), and the microbial fuel cell was operated continuously.

[0094] [Examples 56 to 72, 75 to 81, Comparative Example 5] As shown in Table 2, the microbial fuel cell was operated continuously in the same manner as in Example 55, except that microbial fuel cell electrodes (2) to (18), (21) to (27), and (29) were used as the anode instead of microbial fuel cell electrode (1).

[0095] [Examples 73 and 74] As shown in Table 2, the microbial fuel cell was operated continuously in the same manner as in Example 55, except that microbial fuel cell electrodes (19) and (20) were used instead of the microbial fuel cell cathode (1) as the cathode.

[0096] [Table 2]

[0097] (Power generation characteristics evaluation) After 3 weeks, the voltage and current of the microbial fuel cell were measured with a tester and the output was calculated. The criteria for evaluation are shown below, and the results are shown in Table 2. ◎: Power generation characteristics 30μW or more (very good) 〇: Power generation characteristics: 20μW or more and less than 30μW (good) 〇△: Power generation characteristics: 10μW or more, less than 20μW (no practical problems) △: Power generation characteristics: 5μW or more and less than 10μW (bad) ×: Power generation characteristics: less than 5 μW (extremely poor)

[0098] (Durability evaluation) The power generation characteristics at the time of the power generation characteristic evaluation were set to 100%, and the power generation characteristics were measured after another 3 weeks to calculate and evaluate the maintenance rate of the power generation characteristics. The evaluation criteria are shown below, and the results are shown in Table 2. ◎: Power generation characteristic retention rate 80% or more (very good) 〇: Power generation characteristic maintenance rate: 70% or more but less than 80% (good) 〇△: Power generation characteristic retention rate is 60% or more and less than 70% (no problem in practical use) △: Power generation characteristic retention rate is 40% or more but less than 60% (poor) ×: Power generation characteristic retention rate is less than 40% (extremely poor)

[0099] As shown in Table 2, by using the electrode composition of the present invention, good power generation characteristics and durability were obtained in the microbial fuel cell. It is believed that the reaction rate was high due to the high conductivity of the electrode and the high diffusivity of the substance. In addition, it is believed that the surface morphology of the anode was optimized, which improved the adsorption of microorganisms. Comparing Examples 8 to 10, Example 8, which used a combination of the water-soluble resin (Ba) and the water-based resin particles (Bb), had excellent power generation characteristics and durability. Compared to Example 27 in which the content of the water-soluble resin (Ba) in the total solid content of the composition (100 mass%) was 20%, Examples 15 and 25 in which the content was 1 to 15% had excellent power generation characteristics and durability. Compared to Example 12, which used flake graphite, Examples 3 and 11, which used spherical graphite or artificial graphite with an aspect ratio of 1 to 10, had excellent power generation characteristics and durability. Compared with Example 15 and Example 18, in which the content of carbon material (A) in the total solid content of the composition (100 mass%) is 75%, Examples 25 and 26, in which the content of carbon material (A) is 80 to 99 mass%, had excellent power generation characteristics and durability. Also, compared with Example 24, in which the content of carbon material (A) is 80%, Examples 4, 5, and 23, in which the content of carbon material (A) is 85 to 99%, had excellent power generation characteristics. Example 15, which uses Ketjen black with a smaller specific surface area, had better durability than Example 16, which uses activated carbon with a larger specific surface area. Also, Example 6 and Example 26, which use acetylene black with an even smaller specific surface area, had better power generation characteristics and durability than Example 14, which uses furnace black, and Example 25, which uses Ketjen black. Example 26, in which the content of graphite (Aa) in the carbon material (A) is 80%, had better power generation characteristics than Example 17, in which the content of graphite (Aa) in the carbon material (A) is 60%. Also, Example 23, in which the content of graphite (Aa) is 80%, had better power generation characteristics than Example 22, in which the content of graphite (Aa) is 40%. The average specific surface area of ​​the carbon material (A) is 300m2 / g, the average specific surface area of ​​the carbon material (A) is about 150 m 2 / g, the power generation characteristics and durability were excellent. 2 / g of Example 25, the average specific surface area of ​​the carbon material (A) is about 8 m 2 / g, the power generation characteristics were excellent. [Explanation of symbols]

[0100] 1 container 2 Cathode 3 Anode 4 Electrolyte 5 External Resistance

Claims

1. A composition for forming an electrode for a microbial fuel cell comprising a carbon material (A) and a binder (B), wherein the carbon material (A) comprises graphite (A-a) and a carbon material other than graphite (A-b); the binder (B) contains a water-soluble resin (Ba) and aqueous resin fine particles (B-b); A composition for forming an electrode for a microbial fuel cell, wherein the content of graphite (A-a) in a total of 100% by mass of the carbon material (A) is 20.0% by mass or more, and the content of the carbon material (A) in a total of 100% by mass of the solid content of the composition is 50% by mass or more.

2. The composition for forming a microbial fuel cell electrode according to claim 1, wherein the content of graphite (Aa) in a total of 100% by mass of the carbon material (A) is 25 to 99% by mass.

3. A composition for forming an electrode for a microbial fuel cell according to claim 1 or 2, wherein the content of the carbon material (A) in the total solid content of the composition (100% by mass) is 80 to 99% by mass.

4. A composition for forming a microbial fuel cell electrode according to any one of claims 1 to 3, wherein the aspect ratio of the graphite (Aa) is 1 to 10.

5. An electrode for a microbial fuel cell having a coating film of the composition for forming a microbial fuel cell electrode according to any one of claims 1 to 4 on a substrate.

6. A microbial fuel cell using the electrode for a microbial fuel cell according to claim 5.

Citation Information

Patent Citations

  • Air cathode and microbial fuel cell

    CN105161730A

  • Power generation method and device using organic substance

    JP2004342412A

  • Microbiological power generation device and positive electrode for microbiological power generation device

    JP2009295488A

  • Power generation method

    JP2010102870A

  • Microbiological power generation device and positive electrode for the microbiological power generation device

    JP2010102953A