Organic sulfur material, electrode, lithium ion secondary battery, and manufacturing method

The development of an organic sulfur material for lithium ion secondary batteries addresses cost and performance issues by enhancing charge/discharge capacity and cycle characteristics through modified acrylic resin with sulfur, offering improved capacity retention and cost-effectiveness.

JP7559813B2Active Publication Date: 2024-10-02SUMITOMO RUBBER INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022155306
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-20
Filing Date
2022-09-28
Publication Date
2024-10-02
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face challenges with high production costs due to expensive polyacrylonitrile in positive electrode active materials and poor cycle characteristics from volume changes in negative electrode materials like silicon and tin, as well as limited capacity improvement from carbon materials.

Method used

A novel organic sulfur material is developed by modifying acrylic resin with sulfur, characterized by specific FT-IR and Raman spectra, and produced under a non-oxidizing atmosphere, which is used as a positive or negative electrode active material in lithium ion secondary batteries.

Benefits of technology

The organic sulfur material improves charge/discharge capacity and cycle characteristics, enabling lithium ion secondary batteries with high capacity retention rates and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559813000005
    Figure 0007559813000005
  • Figure 0007559813000006
    Figure 0007559813000006
  • Figure 0007559813000007
    Figure 0007559813000007
Patent Text Reader

Abstract

The present invention provides a novel organic sulfur material capable of improving charge / discharge capacity and cycle characteristics, an electrode comprising the organic sulfur material, i.e., a positive electrode or a negative electrode, and a lithium ion secondary battery comprising the electrode. The organic sulfur material is an acrylic resin modified with sulfur, and the acrylic resin has a characteristic of 756 cm in the FT-IR spectrum. -1 Near 1066cm -1 Near 1150cm -1 Near 1245cm -1 Near 1270cm -1 Near 1453cm -1 Near and 1732 cm -1 The particle diameter of the acrylic resin is 0.1 to 300.0 μm, and the Raman spectrum detected by Raman spectroscopy has a peak in the vicinity of 1450 cm -1 There is a main peak in the vicinity of 200 to 1800 cm -1 Another 485cm in the range -1 Near 1250cm -1 Near 1540cm -1 The peaks around this area are organic sulfur materials.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel organosulfur material, an electrode comprising the organosulfur material, a lithium ion secondary battery comprising the electrode, and methods for producing the same. [Background technology]

[0002] Lithium-ion secondary batteries have a large charge / discharge capacity and are primarily used as batteries for portable electronic devices. They are also increasingly being used as batteries for electric vehicles, and there are high hopes for improved performance.

[0003] Patent Document 1 describes a positive electrode active material for lithium ion secondary batteries obtained by heating raw material powders containing sulfur powder and polyacrylonitrile powder under a non-oxidizing atmosphere. Patent Document 2 aims to provide a low-cost positive electrode active material by using industrial rubber.

[0004] On the other hand, it has been proposed to increase the battery capacity of lithium-ion secondary batteries by using materials capable of absorbing and releasing more lithium ions, such as silicon (Si) and tin (Sn), as the negative electrode active material. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2010 / 044437 [Patent Document 2] JP 2015-92449 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the positive electrode active material of Patent Document 1 has a problem that the raw material polyacrylonitrile is expensive, and in particular polyacrylonitrile with stable quality is even more expensive, making it difficult to provide lithium ion secondary batteries at low cost. The positive electrode active material of Patent Document 2 still has a problem in sufficiently improving cycle characteristics. The above-mentioned material proposed as the negative electrode active material has a problem in that the cycle characteristics when repeatedly charged and discharged are not good because the volume change caused by the absorption and release of lithium ions is large. In addition, carbon materials such as graphite and hard carbon are also used, but the theoretical capacity is already being reached, and a significant improvement in capacity cannot be expected.

[0007] The present invention provides a novel organosulfur material capable of improving the charge / discharge capacity and cycle characteristics of a lithium ion secondary battery, an electrode comprising the organosulfur material, i.e., a positive electrode or a negative electrode, a lithium ion secondary battery comprising the electrode, and methods for producing the same. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that an organic sulfur material exhibiting excellent properties can be obtained by modifying a specific acrylic resin with sulfur, and after further research, have completed the present invention.

[0009] That is, the present invention provides [1] An organic sulfur material made by modifying acrylic resin with sulfur. The acrylic resin has a FT-IR spectrum of 756 cm -1 Near, 1066cm -1 Near, 1150cm -1 Near, 1245cm -1 Near, 1270cm -1 Near, 1453cm -1 Near and 1732 cm -1 Organosulfur materials having a peak near [2] 1150cm -1 Nearby peaks and the above 1732cm -1The organosulfur material according to the above [1], wherein the peak in the vicinity of the first peak is larger than the remaining peaks; [3] The FT-IR spectrum further shows a peak at 846 cm -1 Near, 992cm -1 Near, 1196cm -1 Near, 2955cm -1 Near and 2996 cm -1 The organosulfur material according to [1] or [2] above, having a peak in the vicinity [4] The mass ratios of carbon, hydrogen, nitrogen and sulfur in the total amount of the acrylic resin are, respectively, 60.0 to 70.0%, 7.5 to 9.5%, 0.0% and 0.0 to 1.0%, preferably 60.0 to 69.0%, 7.6 to 9.4%, 0.0% and 0.0 to 0.9%, more preferably 60.0 to 68.0%, 7.7 to 9.3%, 0.0% and 0.0 to 0.8%. %, more preferably 60.0 to 67.0%, 7.7 to 9.2%, 0.0% and 0.0 to 0.7%, still more preferably 60.0 to 67.0%, 7.7 to 9.2%, 0.0% and 0.0 to 0.6%, still more preferably 60.5 to 66.5%, 7.7 to 9.2%, 0.0% and 0.0 to 0.5%; [5] The organic sulfur material according to any one of the above [1] to [4], wherein the modification is carried out by calcination in a non-oxidizing atmosphere. [6] The organic sulfur material according to any one of the above [1] to [5], wherein the particle size of the acrylic resin is 0.1 to 300.0 μm, preferably 1.0 to 270.0 μm, more preferably 1.0 to 200.0 μm, even more preferably 1.0 to 100.0 μm, even more preferably 1.0 to 50.0 μm, even more preferably 1.0 to 20.0 μm, and even more preferably 1.0 to 15.0 μm. [7] The organosulfur material according to any one of the above [1] to [6], wherein the acrylic resin has a porous structure. [8] In the Raman spectrum detected by Raman spectroscopy, the peak at 1450 cm -1 The main peak is in the vicinity of 200 to 1800 cm -1 Another 485cm in the range -1 Near 1250cm-1 Near, 1540cm -1 The organosulfur material according to any one of the above [1] to [7], having a peak in the vicinity [9] In the Raman spectrum, -1 Strength and 1800cm -1 The line connecting the intensity of the -1 The difference between the intensity of the peak near the 1450 ) and 1540 cm -1 The difference between the intensity of the peak near the 1540 ) when calculating I 1450 / I 1540 The organic sulfur material according to the above [8], wherein the value of is in the range of 1 to 4.

[10] The organic sulfur material according to any one of the above [1] to [9], wherein the amount of sulfur in the organic sulfur material is 50.0% by mass or more, more preferably 53.0% by mass or more, even more preferably 55.0% by mass or more, and even more preferably 56.0% by mass or more.

[11] An electrode comprising the organosulfur material according to any one of [1] to

[10] above.

[12] A lithium ion secondary battery comprising the electrode according to

[11] above.

[13] A method for producing an organosulfur material, comprising the steps of: (1) preparing an acrylic resin; (2) modifying the acrylic resin with sulfur It includes, and The acrylic resin has a FT-IR spectrum of 756 cm -1 Near, 1066cm -1 Near, 1150cm -1 Near, 1245cm -1 Near, 1270cm -1 Near, 1453cm -1 Near and 1732 cm -1 A manufacturing method having a peak in the vicinity of

[14] The method according to

[13] above, wherein the modification is carried out by firing in a non-oxidizing atmosphere.

[15] The method according to the above

[13] or

[14] , wherein the amount of the sulfur relative to the acrylic resin is 50 to 1000 parts by mass, preferably 100 to 750 parts by mass, more preferably 150 to 500 parts by mass, still more preferably 200 to 500 parts by mass, and still more preferably 250 to 500 parts by mass, relative to 100 parts by mass of the acrylic resin.

[16] The method according to any one of the above

[13] to

[15] , wherein the firing temperature is 250 to 550°C, preferably 300 to 500°C, and more preferably 300 to 450°C.

[17] The method according to any one of the above

[13] to

[16] , wherein the particle size of the acrylic resin is 0.1 to 300.0 μm, preferably 1.0 to 270.0 μm, more preferably 1.0 to 200.0 μm, even more preferably 1.0 to 100.0 μm, even more preferably 1.0 to 50.0 μm, even more preferably 1.0 to 20.0 μm, and even more preferably 1.0 to 15.0 μm.

[18] The method according to any one of the above

[13] to

[17] , wherein the acrylic resin has a porous structure.

[19] A method for producing an electrode, comprising the steps of: After producing an organic sulfur material by the production method according to any one of

[13] to

[18] above, (3) A step of preparing an electrode using the organic sulfur material by a conventional method. A method of manufacturing the

[20] A method for producing a lithium ion secondary battery, comprising the steps of: After the electrode is produced by the production method of

[19] above, (4) A step of producing a lithium ion secondary battery using the electrode by a conventional method. A method of manufacturing comprising the steps of: Regarding. Effect of the Invention

[0010] According to the present invention, it is possible to provide a novel organosulfur material capable of improving charge / discharge capacity and cycle characteristics, an electrode comprising the organosulfur material, i.e., a positive electrode or a negative electrode, and a lithium ion secondary battery comprising the electrode.

[0011] In this specification, the term "cycle characteristic" refers to the characteristic of maintaining the charge / discharge capacity of a secondary battery despite repeated charging and discharging. Therefore, a secondary battery that experiences a large decrease in charge / discharge capacity and a low capacity retention rate with repeated charging and discharging has poor cycle characteristics, whereas a secondary battery that experiences a small decrease in charge / discharge capacity and a high capacity retention rate has excellent cycle characteristics. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a cross-sectional view that illustrates a reaction apparatus used in the production of an organosulfur material in the Examples. [Diagram 2] The FT-IR spectrum profiles of the acrylic resins used in Examples 1 to 4 are shown side by side on the same horizontal axis (wave number (cm-1)) so that their peak positions can be compared. [Diagram 3] The Raman spectrum profiles of the organosulfur materials of Example 1 and Comparative Examples 1 and 2 are shown side by side on the same horizontal axis (Raman shift (cm −1 )) so that their peak positions can be compared. [Figure 4] The I1450 / I1540 values ​​for each Raman spectrum profile in the previous figure are shown on a graph so that they can be understood. Here, I1450 is the difference between the peak intensity near 1450 cm-1 and the corresponding baseline intensity (A in the figure), and I1540 is the difference between the peak intensity near 1540 cm-1 and the corresponding baseline intensity (B in the figure). Note that the baseline is the nearly horizontal line in the figure, which connects the intensity at 1000 cm-1 and the intensity at 1800 cm-1 in each profile. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The configuration of the present disclosure will be described in detail below. The upper and lower limit values ​​of "more than", "less than", and "to" in the description of a numerical range can be arbitrarily combined, and the numerical values ​​in the examples can be the upper and lower limits. In addition, when a numerical range is specified by "to", it means that both ends of the range are included unless otherwise specified.

[0014] One embodiment of the present disclosure is an organic sulfur material obtained by modifying an acrylic resin with sulfur, and the acrylic resin has a sulfur-containing structure having a wavelength of 756 cm in an FT-IR spectrum. -1 Near, 1066cm -1 Near, 1150cm -1 Near, 1245cm -1 Near, 1270cm -1 Near, 1453cm -1 Near and 1732 cm -1 It is an organosulfur material having a peak around

[0015] Another embodiment of the present disclosure is an electrode comprising said organic material.

[0016] Another embodiment of the present disclosure is a lithium ion secondary battery comprising the electrode.

[0017] Another embodiment of the present disclosure is a method for producing an organosulfur material, comprising the steps of: (1) preparing an acrylic resin; (2) modifying the acrylic resin with sulfur The acrylic resin has a refractive index of 756 cm in the FT-IR spectrum. -1 Near, 1066cm -1 Near, 1150cm -1 Near, 1245cm -1 Near, 1270cm -1 Near, 1453cm -1 Near and 1732 cm -1 The manufacturing method has a peak in the vicinity.

[0018] Another embodiment of the present disclosure is a method for producing an electrode, comprising the steps of: producing an organosulfur material by the above-mentioned method; and (3) A step of preparing an electrode using the organic sulfur material by a conventional method. The method of manufacture comprises:

[0019] Another embodiment of the present disclosure is a method for producing a lithium ion secondary battery, comprising the steps of: (4) A step of producing a lithium ion secondary battery using the electrode by a conventional method. The method of manufacture comprises:

[0020] <Acrylic resin> In the present disclosure, the acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066cm -1 Near, 1150cm -1 Near, 1245cm -1 Near, 1270cm -1 Near, 1453cm -1 Near and 1732 cm -1 It has a peak around

[0021] From the viewpoint of the effects of the present disclosure, the acrylic resin is preferably -1 Nearby peaks and the above 1732cm -1 The nearby peak is larger than the remaining peaks.

[0022] From the viewpoint of the effects of the present disclosure, it is more preferable that the acrylic resin further has a FT-IR spectrum of 846 cm -1 Near, 992cm -1 Near, 1196cm -1 Near, 2955cm -1 Near and 2996 cm -1 It has a peak around

[0023] In this disclosure, FT-IR spectra were measured using a Fourier transform infrared spectrophotometer (IRAffinity-1) manufactured by Shimadzu Corporation with a resolution of 4 cm. -1 , Accumulation count: 10 times, Measurement range: 400 cm -1 ~4000cm -1 In FIG. 2, the FT-IR spectrum profiles of the acrylic resins used in Examples 1 to 4 are shown on the same horizontal axis (wave number (cm)) so that the peak positions can be compared with each other. -1 The peak positions of the FT-IR spectrum are shown below. -1 , especially ±5cm -1 This means that there is an allowance for error.

[0024] From the viewpoint of the effects of the present disclosure, the mass ratios of carbon, hydrogen, nitrogen and sulfur in the total amount of the acrylic resin are preferably within the ranges of 60.0 to 70.0%, 7.5 to 9.5%, 0.0% and 0.0 to 1.0%, respectively. Here, the mass ratio of the carbon is more preferably 60.0 to 69.0%, more preferably 60.0 to 68.0%, even more preferably 60.0 to 67.0%, and even more preferably 60.5 to 66.5%. The mass ratio of the hydrogen is more preferably 7.6 to 9.4%, more preferably 7.7 to 9.3%, and even more preferably 7.7 to 9.2%. The mass ratio of the nitrogen is 0.0%. The mass ratio of sulfur is more preferably 0.0 to 0.9%, further preferably 0.0 to 0.8%, further preferably 0.0 to 0.7%, further preferably 0.0 to 0.6%, and further preferably 0.0 to 0.5%.

[0025] In the present disclosure, the mass ratio of the elements constituting the acrylic resin can be measured by a method similar to the elemental analysis of the organosulfur material described below.

[0026] Examples of acrylic resins include polymers of (meth)acrylic acid alkyl esters, copolymers of (meth)acrylic acid alkyl esters and alkylene glycol di(meth)acrylates, etc. Here, "(meth)acrylate" refers to either "acrylate" or "methacrylate" (hereinafter the same).

[0027] Non-limiting preferred examples of acrylic resins include homopolymers of methyl (meth)acrylate, homopolymers of butyl (meth)acrylate, copolymers of methyl (meth)acrylate and ethylene glycol di(meth)acrylate, copolymers of butyl (meth)acrylate and ethylene glycol di(meth)acrylate, etc. Among these, methacrylate-type acrylic resins are preferred. More preferred examples include copolymers of butyl methacrylate and ethylene glycol dimethacrylate.

[0028] One or more kinds of acrylic resins can be used.

[0029] (Acrylic resin form) In the present disclosure, the acrylic resin is preferably in the form of fine particles. Here, fine particles refer to particles having a particle diameter of 300.0 μm or less. The particle diameter is preferably 270.0 μm or less, more preferably 200.0 μm or less, even more preferably 100.0 μm or less, even more preferably 50.0 μm or less, even more preferably 20.0 μm or less, even more preferably 15.0 μm or less, even more preferably 13.0 μm or less, even more preferably 10.0 μm or less, even more preferably 6.0 μm or less. On the other hand, the lower limit of the particle diameter is not particularly limited, but is usually, for example, 0.1 μm or more, preferably 1.0 μm or more. The particle diameter is a value measured by a precision particle size distribution measuring device Multisizer 3 manufactured by Beckman Coulter, Inc.

[0030] The acrylic resin may be spherical fine particles or porous fine particles. When the acrylic resin is porous, its oil absorption is preferably 100 ml / 100 g or more, more preferably 110 ml / 100 g or more, even more preferably 120 ml / 100 g or more, even more preferably 130 ml / 100 g or more, and even more preferably 140 ml / 100 g or more. The oil absorption is a value measured according to JIS K 5101-13-2:2004. More specifically, it can be measured by the method of paragraph 0069 of JP2017-88501A.

[0031] (Weight average molecular weight (Mw) of acrylic resin) The Mw of the acrylic resin is not particularly limited as long as it has the above structure. However, the Mw of the acrylic resin is usually within the range of 2,000 to 1,500,000. The Mw is a value measured by gel permeation chromatography (GPC) (calibrated with polystyrene).

[0032] (Acquisition or production of acrylic resin) The acrylic resins are commercially available or can be prepared by conventional methods within the knowledge of one skilled in the art. Commercially available acrylic resins include those manufactured by Sekisui Plastics Co., Ltd. and Sekisui Chemical Co., Ltd.

[0033] <Sulfur> As sulfur, any of various forms such as powdered sulfur, insoluble sulfur, precipitated sulfur, colloidal sulfur can be used, among which precipitated sulfur and colloidal sulfur are preferred. The amount of sulfur is preferably 50 parts by mass or more, more preferably 100 parts by mass or more, more preferably 150 parts by mass or more, more preferably 200 parts by mass or more, and even more preferably 250 parts by mass or more, relative to 100 parts by mass of acrylic resin. By being 100 parts by mass or more, there is a tendency that the charge / discharge capacity and cycle characteristics can be improved. On the other hand, there is no particular upper limit for the amount of sulfur to be blended, but it is usually 1000 parts by mass or less, preferably 750 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and even more preferably 350 parts by mass or less. By being 1000 parts by mass or less, there is a tendency that it is advantageous in terms of cost.

[0034] <Conductive carbon materials> When the acrylic resin is modified with sulfur, a carbon material having electrical conductivity may be added to the acrylic resin in advance. This is because the electrical conductivity of the organic sulfur material can be improved. As such an electrically conductive carbon material, a carbon material having a graphite structure is preferable. As the carbon material, for example, those having a condensed aromatic ring structure such as carbon black, acetylene black, ketjen black, graphite, carbon nanotube (CNT), carbon fiber (CF), graphene, and fullerene can be used. As the electrically conductive carbon material, one or more kinds can be used.

[0035] Among them, acetylene black, carbon black, and ketjen black are preferable because they are inexpensive and have excellent dispersibility. A small amount of CNT or graphene may be used in combination with acetylene black, carbon black, or ketjen black. Such a combination system makes it possible to further improve the cycle characteristics of a lithium ion secondary battery without significantly increasing the cost. The amount of CNT or graphene used in combination is preferably 8% by mass or more and 12% by mass or less of the total amount of the conductive carbon material.

[0036] The amount of the conductive carbon material is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, relative to 100 parts by mass of the acrylic resin. By having an amount of 5 parts by mass or more, it tends to be easier to achieve the purpose of further improving the charge / discharge capacity and cycle characteristics. On the other hand, the amount is preferably 50 parts by mass or less, more preferably 40 parts by mass or less. By having an amount of 50 parts by mass or less, the proportion of the structure containing sulfur in the organic sulfur material does not relatively decrease, and it tends to be easier to achieve the purpose of further improving the charge / discharge capacity and cycle characteristics.

[0037] <Other ingredients> When the acrylic resin is modified with sulfur, other materials commonly used in this field may be added to the acrylic resin in advance, if desired.

[0038] <Production of organic sulfur materials> In the present disclosure, the organic sulfur material can be produced by modifying a certain acrylic resin with sulfur.

[0039] (Preparation of raw materials) In the modification, it is desirable to thoroughly mix the acrylic resin and sulfur in advance. When a conductive carbon material or the like is added to the acrylic resin in advance, these additives are also mixed together. The mixing can be carried out by a conventional method, for example, using a high-speed blender. On the other hand, the acrylic resin, sulfur, and, if desired, the additives can be molded into pellets.

[0040] (Non-oxidizing atmosphere) The modification is preferably carried out in a non-oxidizing atmosphere. The non-oxidizing atmosphere refers to an atmosphere that is substantially free of oxygen, and is adopted to suppress oxidative deterioration and excessive thermal decomposition of the components. Specifically, it refers to an inert gas atmosphere such as nitrogen or argon, a sulfur gas atmosphere, etc. Therefore, the modification is carried out, for example, in a quartz tube under an inert gas atmosphere.

[0041] (Method of denaturation) The modification of the acrylic resin with sulfur can be carried out by a conventional method, for example, by baking the acrylic resin and sulfur. The baking can be carried out by a conventional method. For example, the baking can be carried out by heating the baking raw material (containing the acrylic resin and sulfur, and optionally an additive) at a predetermined temperature increase rate until it reaches a predetermined temperature, maintaining the temperature at the predetermined temperature for a predetermined time, and then naturally cooling.

[0042] [Heating rate] The temperature rise rate is preferably within a range of, for example, 50 to 500° C. / h. The temperature rise rate is more preferably 100° C. / h or more. On the other hand, the temperature rise rate is more preferably 400° C. / h or less, further preferably 300° C. / h or less, and further preferably 200° C. / h or less. When the temperature rise rate is within such a range, it tends to be easier to achieve the purpose of improving the charge / discharge capacity and cycle characteristics.

[0043] [Firing temperature and time] The calcination temperature is the temperature after the temperature rise of the calcination raw material is completed, and refers to the temperature maintained for a certain period of time for calcination of the calcination raw material. The temperature is preferably in the range of 250 to 550 ° C. By being 250 ° C or higher, the sulfurization reaction is avoided from becoming insufficient, and the charge-discharge capacity of the target product tends to be prevented from decreasing. On the other hand, by setting the temperature to 550 ° C or lower, the decomposition of the calcination raw material is prevented, and the decrease in yield and the decrease in charge-discharge capacity tend to be prevented. The temperature is more preferably 300 ° C or higher, and even more preferably 350 ° C or higher, while more preferably 500 ° C or lower, and more preferably 450 ° C or lower. The time to maintain the calcination temperature may be appropriately set according to the type of calcination raw material, the calcination temperature, etc., but is preferably, for example, 1 to 6 hours. By being 1 hour or more, the calcination tends to be able to proceed sufficiently, and by being 6 hours or less, the excessive thermal decomposition of the constituent components tends to be prevented.

[0044] [Device] The calcination can be carried out by the apparatus shown in Fig. 1, or can be carried out by using a continuous apparatus such as a twin-screw extruder. When a continuous apparatus is used, there is an advantage that the organic sulfur material can be produced continuously by a series of operations, for example, calcination is carried out while kneading, pulverizing and mixing the calcination raw materials in the apparatus.

[0045] (Residue removal process) In the treated product obtained after calcination, unreacted sulfur remains, which is the sulfur that sublimed during calcination and then cooled and precipitated. Since these residues are a factor in reducing cycle characteristics, it is desirable to remove them as much as possible. The removal of the residues can be carried out according to a conventional method, such as reduced pressure heating drying, hot air drying, and solvent washing.

[0046] (Crushing, classification) The obtained organic sulfur material can be pulverized to a predetermined particle size and classified to obtain particles of a size suitable for the manufacture of electrodes. The preferred particle size distribution of the particles is about 5 to 40 μm in median diameter. In the firing method using the twin-screw extruder described above, the organic sulfur material can be pulverized at the same time as the organic sulfur material is produced by shearing during kneading.

[0047] <Organic sulfur materials> The organic sulfur material thus obtained is mainly composed of carbon and sulfur, and the higher the sulfur content, the better the charge / discharge capacity and cycle characteristics. Therefore, the higher the sulfur content, the better. In general, the preferred range of the sulfur content in the organic sulfur material is 50.0% by mass or more, more preferably 53.0% by mass or more, even more preferably 55.0% by mass or more, and even more preferably 56.0% by mass or more. However, when a conductive carbon material is blended, even if the sulfur content is somewhat lower due to the influence of the carbon constituting the conductive carbon material, the effect of improving the charge / discharge capacity and cycle characteristics may be expected. In such a case, the sulfur content may be about 5.0% by mass lower than the above-mentioned sulfur content. The total of the carbon content and the sulfur content in the organic sulfur material is preferably 90% by mass or more, more preferably 92% by mass or more, and even more preferably 94% by mass or more.

[0048] In addition, hydrogen (H) in the acrylic resin reacts with sulfur by baking to become hydrogen sulfide, and is reduced from the sulfide. Therefore, the hydrogen content of the organic sulfur material is preferably 1.8% by mass or less, and more preferably 1.6% by mass or less. When it is 1.8% by mass or less, there is a tendency that the baking (sulfurization reaction) is sufficient, and when it is 1.6% by mass or less, there is a tendency that the baking (sulfurization reaction) is more sufficient. Therefore, in this case, the charge / discharge capacity tends to be improved. The hydrogen content is more preferably 1.0% by mass or less, and even more preferably 0.6% by mass or less. In this specification, the content of an element is measured by elemental analysis according to a conventional method.

[0049] The organic sulfur materials were detected by Raman spectroscopy, with a peak at 1450 cm -1 The main peak is in the vicinity of 200 to 1800 cm -1 Another 485cm in the range -1 Near 1250cm -1 Near, 1540cm -1 In this regard, the Raman spectra of Example 1 and Comparative Examples 1 and 2 are shown in FIG. 3. Note that the term "near" in the peak position of the Raman spectrum means that the peak position is within ±50 cm. -1 , especially ±30cm -1 This means that there is an allowance for error.

[0050] In addition, the organic sulfur material has a Raman spectrum of 1000 cm -1 Strength and 1800cm -1 The line connecting the intensity of the -1 The difference between the intensity of the peak near the 1450 ) and 1540 cm -1 The difference between the intensity of the peak near the 1540 ) when calculating I 1450 / I 1540It is preferable that the value of is in the range of 1 to 4. In this regard, the I 1450 / I 1540 Figure 4 shows the value of I on a graph. The value of A / B in Figure 4 is I 1450 / I 1540 The value is

[0051] Regarding Example 1 and Comparative Examples 1 and 2, 1450 / I 1540 The calculated values ​​are as shown in Table 1 below.

[0052] [Table 1]

[0053] I 1450 / I 1540 From the viewpoint of the effects of the present disclosure, the value is preferably 1.20 or more, more preferably 1.40 or more, even more preferably 1.50 or more, and even more preferably 2.00 or more. On the other hand, the value is preferably 3.80 or less, more preferably 3.60 or less, even more preferably 3.50 or less, and even more preferably 3.20 or less.

[0054] In this disclosure, Raman spectra were measured using a Raman microscope (RMP-320, excitation wavelength λ = 532 nm, grating: 1800 gr / mm, resolution: 3 cm) manufactured by JASCO Corporation. -1 ) can be measured.

[0055] <Lithium-ion secondary battery> The organic sulfur material of the present disclosure can be used as an electrode active material for a lithium ion secondary battery, that is, as a positive electrode active material or a negative electrode active material. That is, an electrode for a lithium secondary battery can be produced in the same manner as in the production of a general electrode for a lithium ion secondary battery, except that the organic sulfur material is used, and a lithium ion secondary battery can be produced in the same manner as in the production of a general lithium ion secondary battery, except that the electrode for a lithium ion secondary battery is used. The lithium ion secondary battery produced in this manner has a large charge / discharge capacity and excellent cycle characteristics.

[0056] 1. When using organic sulfur materials as positive electrode active materials The lithium ion secondary battery of the present disclosure can be produced in accordance with a conventional method by using a positive electrode containing the above-mentioned organic sulfur material (positive electrode active material), a negative electrode, an electrolyte, and, if desired, components such as a separator.

[0057] (positive electrode) The positive electrode for lithium ion secondary batteries can be prepared in the same manner as the positive electrode for general lithium ion secondary batteries, except that the above organic sulfur material is used as the positive electrode active material. For example, the positive electrode can be prepared by mixing a particulate organic sulfur material with a conductive assistant, a binder, and a solvent to prepare a paste-like positive electrode material, applying the positive electrode material to a current collector, and then drying the same. In addition, as another method, the positive electrode can also be prepared by kneading the organic sulfur material with a conductive assistant, a binder, and a small amount of solvent using a mortar or the like, forming it into a film, and then pressing it onto a current collector using a press or the like.

[0058] [Conductive additive] Examples of the conductive assistant include vapor grown carbon fiber (VGCF), carbon powder, carbon black (CB), acetylene black (AB), ketjen black (KB), graphite, or fine powder of a metal such as aluminum or titanium that is stable at a positive electrode potential. These conductive assistants can be used alone or in combination.

[0059] [Binder] Examples of binders include polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), polyimide (PI), polyamide-imide (PAI), carboxymethyl cellulose (CMC), polyvinyl chloride (PVC), acrylic resin, methacrylic resin (PMA), polyacrylonitrile (PAN), modified polyphenylene oxide (PPO), polyethylene oxide (PEO), polyethylene (PE), polypropylene (PP), etc. These binders can be used alone or in combination of two or more.

[0060] [solvent] Examples of the solvent include N-methyl-2-pyrrolidone, N,N-dimethylformaldehyde, alcohol, hexane, water, etc. These solvents can be used alone or in combination of two or more.

[0061] [Amount] The amounts of the materials constituting the positive electrode are not particularly limited, but it is preferable to mix, for example, 2 to 100 parts by mass of the conductive assistant, 2 to 50 parts by mass of the binder, and an appropriate amount of solvent with respect to 100 parts by mass of the organic sulfur material.

[0062] [Current collector] As the current collector, one generally used for the positive electrode of a lithium ion secondary battery may be used. For example, the current collector may be made of aluminum foil, aluminum mesh, punched aluminum sheet, aluminum expand sheet, stainless steel foil, stainless steel mesh, punched stainless steel sheet, stainless steel expand sheet, foamed nickel, nickel nonwoven fabric, copper foil, copper mesh, punched copper sheet, copper expand sheet, titanium foil, titanium mesh, carbon nonwoven fabric, carbon woven fabric, etc. Among these, a current collector made of carbon nonwoven fabric or carbon woven fabric made of carbon with a high degree of graphitization does not contain hydrogen and has low reactivity with sulfur, and is therefore suitable as a current collector when the organic sulfur material of the present disclosure is used as a positive electrode active material. As a raw material for carbon fiber with a high degree of graphitization, various pitches (i.e., by-products of petroleum, coal, coal tar, etc.) and polyacrylonitrile fiber (PAN), etc., which are materials for carbon fibers, may be used. In addition to using one type of current collector, two or more types may be used in combination.

[0063] (Negative electrode) As the negative electrode material, known metallic lithium, carbon-based materials such as graphite, silicon-based materials such as silicon thin film, and alloy-based materials such as copper-tin and cobalt-tin can be used. When a material that does not contain lithium is used as the negative electrode material, for example, a carbon-based material, a silicon-based material, an alloy-based material, etc. among the above-mentioned negative electrode materials, it is advantageous in that a short circuit between the positive and negative electrodes due to the generation of dendrites is unlikely to occur. However, when these lithium-free negative electrode materials are used in combination with the positive electrode of the present disclosure, neither the positive electrode nor the negative electrode contains lithium. For this reason, a lithium pre-doping process is required in which lithium is inserted in advance into either or both of the negative electrode and the positive electrode. The pre-doping method of lithium may be according to a known method. For example, when doping lithium into the negative electrode, a method of inserting lithium by an electrolytic doping method in which a half cell is assembled using metallic lithium as the counter electrode and lithium is electrochemically doped, or a method of inserting lithium by a pasting pre-doping method in which a metallic lithium foil is pasted on the electrode and then left in an electrolyte solution to dope the lithium by utilizing the diffusion of lithium into the electrode, can be mentioned. In addition, the above-mentioned electrolytic doping method can be used when pre-doping the positive electrode with lithium. As the negative electrode material that does not contain lithium, silicon-based materials, which are high-capacity negative electrode materials, are particularly preferred, and among them, thin-film silicon, which has a thin electrode thickness and is advantageous in terms of capacity per volume, is more preferred.

[0064] (electrolyte) The electrolyte used in the lithium ion secondary battery may be an organic solvent in which an electrolyte alkali metal salt is dissolved. As the organic solvent, it is preferable to use at least one selected from non-aqueous solvents such as ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl ether, γ-butyrolactone, and acetonitrile. As the electrolyte, LiPF6, LiBF4, LiAsF6, LiCF3SO3, LiI, LiClO4, etc. may be used. The concentration of the electrolyte may be about 0.5 mol / L to 1.7 mol / L. The electrolyte is not limited to a liquid state. For example, when the lithium ion secondary battery is a lithium polymer secondary battery, the electrolyte is in a solid state (for example, a polymer gel state).

[0065] (Separator) The lithium ion secondary battery may include a separator and other components in addition to the above-mentioned negative electrode, positive electrode, and electrolyte. The separator is interposed between the positive electrode and the negative electrode, and allows the movement of ions between the positive electrode and the negative electrode, and prevents internal short-circuiting between the positive electrode and the negative electrode. If the lithium ion secondary battery is a sealed type, the separator is also required to have a function of retaining the electrolyte. As the separator, it is preferable to use a thin, microporous or nonwoven membrane made of polyethylene, polypropylene, polyacrylonitrile, aramid, polyimide, cellulose, glass, or the like.

[0066] (shape) The shape of the lithium ion secondary battery is not particularly limited, and it can be in various shapes such as a cylindrical type, a laminated type, a coin type, a button type, and the like.

[0067] 2. When using organic sulfur materials as negative electrode active materials The lithium ion secondary battery of the present disclosure can be produced in accordance with a conventional method by using a negative electrode containing the above-mentioned organic sulfur material (negative electrode active material), a positive electrode, an electrolyte, and, if desired, components such as a separator.

[0068] (Negative electrode) The negative electrode for lithium ion secondary batteries can be prepared in the same manner as the negative electrode for general lithium ion secondary batteries, except that the above organic sulfur material is used as the negative electrode active material. For example, the negative electrode can be prepared by mixing a particulate organic sulfur material with a conductive assistant, a binder, and a solvent to prepare a paste-like negative electrode material, applying the negative electrode material to a current collector, and then drying the paste. In addition, as another method, the negative electrode can also be prepared by kneading the organic sulfur material with a conductive assistant, a binder, and a small amount of solvent using a mortar or the like, forming it into a film, and then pressing the film onto a current collector using a press or the like.

[0069] The conductive assistant, binder and solvent can be the same as those used in the above case where an organic sulfur material is used as the positive electrode active material, and the current collector can also be the same as those used in the above case where an organic sulfur material is used as the positive electrode active material.

[0070] (positive electrode) The positive electrode material is not particularly limited as long as it is, for example, a transition metal oxide or solid solution oxide containing lithium, or a substance capable of electrochemically absorbing and releasing lithium ions. Examples of the transition metal oxide containing lithium include Li·Co-based composite oxides such as LiCoO2, LiNi x Co y Mn z Examples of the solid solution oxide include Li·Ni·Co·Mn-based composite oxides such as LiO2, Li·Ni-based composite oxides such as LiNiO2, and Li·Mn-based composite oxides such as LiMn2O4. a Mn x Co y Ni z O2 (1.150≦a≦1.430, 0.450≦x≦0.600, 0.100≦y≦0.150, 0.200≦z≦0.280), LiMn x Co y Ni z O2 (0.300≦x≦0.850, 0.100≦y≦0.300, 0.100≦z≦0.300), LiMn 1.5 Ni 0.5O4, etc. These compounds may be used alone or in combination of two or more kinds.

[0071] The electrolyte, separator, and shape of the lithium ion secondary battery can be the same as those in the above-mentioned case where an organic sulfur material is used as the positive electrode active material. EXAMPLES

[0072] The present disclosure will be described based on examples, but the present disclosure is not limited to only the examples.

[0073] The various chemicals used in the Examples and Comparative Examples are listed below. The various chemicals were purified according to conventional methods as necessary.

[0074] <Materials used in the test> Acrylic resin 1: spherical acrylic resin (Advancell HB-2051 manufactured by Sekisui Chemical Co., Ltd., particle size: 20 μm) Acrylic resin 2: spherical acrylic resin made of polymethyl methacrylate (Techpolymer MB-8 (spherical acrylic resin made of homopolymer of methyl methacrylate) manufactured by Sekisui Chemical Co., Ltd., particle size: 8 μm) Acrylic resin 3: spherical acrylic resin made of cross-linked polymethyl methacrylate (Techpolymer MB30X-5 (spherical acrylic resin made of methyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 5 μm) Acrylic resin 4: spherical acrylic resin made of cross-linked polybutyl methacrylate (Techpolymer BM30X-8 (spherical acrylic resin made of butyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 8 μm) Acrylic resin 5: spherical acrylic resin made of cross-linked polymethyl methacrylate (Techpolymer MB30X-8 (spherical acrylic resin made of methyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 8 μm) Acrylic resin 6: spherical acrylic resin made of cross-linked polymethyl methacrylate (Techpolymer MB30X-20 (spherical acrylic resin made of methyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 20 μm) Acrylic resin 7: Porous acrylic resin made of cross-linked polymethyl methacrylate (Techpolymer MBP-8 (porous acrylic resin made of methyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 8 μm) Acrylic resin 8: spherical acrylic resin made of polymethyl methacrylate (Parapet GF-P (spherical acrylic resin made of homopolymer of methyl methacrylate) manufactured by Kuraray Co., Ltd., particle size: 270 μm) Acrylic resin 9: spherical acrylic resin made of cross-linked polybutyl methacrylate (Techpolymer BM30X-5 (spherical acrylic resin made of butyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 5 μm) Acrylic resin 10: spherical acrylic resin made of cross-linked polybutyl methacrylate (Techpolymer BM30X-12 (spherical acrylic resin made of butyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by Sekisui Chemical Co., Ltd., particle size: 12 μm) Acrylic resin 11: spherical acrylic resin made of cross-linked polybutyl methacrylate (Ganzpearl GB-15S (spherical acrylic resin made of butyl methacrylate and ethylene glycol dimethacrylate copolymer) manufactured by AICA Kogyo Co., Ltd., particle size: 15 μm) High cis BR: High cis butadiene rubber (BR150L manufactured by Ube Industries, Ltd., cis 1,4 bond content = 98% by mass) PAN: Polyacrylonitrile (Sigma-Aldrich, particle size: 8 μm) Sulfur: Precipitated sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.

[0075] Example 1 <Preparation of raw materials> According to the formulation in Table 3, the materials were mixed in a blender to obtain a raw material for firing (baking raw material).

[0076] (Reaction Apparatus) The raw material to be fired was fired using a reaction apparatus 1 shown in Fig. 1. The reaction apparatus 1 includes a cylindrical reaction vessel 3 made of quartz glass with a bottom, an outer diameter of 60 mm, an inner diameter of 50 mm, and a height of 300 mm, for storing and firing the raw material 2, a silicone lid 4 for closing the upper opening of the reaction vessel 3, an alumina protective tube 5 ("Alumina SSA-S" manufactured by Nikkato Corporation, outer diameter 4 mm, inner diameter 2 mm, length 250 mm) that penetrates the lid 4, two gas inlet tubes 6 and a gas exhaust tube 7 (both manufactured by Nikkato Corporation, "Alumina SSA-S" manufactured by Nikkato Corporation, outer diameter 6 mm, inner diameter 4 mm, length 150 mm), and an electric furnace 8 (crucible furnace, opening width φ80 mm, heating height 100 mm) for heating the reaction vessel 3 from the bottom side.

[0077] The alumina protective tube 5 is formed to a length that extends downward from the lid 4 to the raw material 2 contained at the bottom of the reaction vessel 3, and a thermocouple 9 is inserted inside. The alumina protective tube 5 is used as a protective tube for the thermocouple 9. The tip of the thermocouple 9 is inserted into the raw material 2 while being protected by the closed tip of the alumina protective tube 5, and functions to measure the temperature of the raw material 2. The output of the thermocouple 9 is input to a temperature controller 10 of the electric furnace 8, as shown by the solid arrow in the figure, and the temperature controller 10 functions to control the heating temperature of the electric furnace 8 based on the input from this thermocouple 9.

[0078] The gas inlet pipe 6 and the gas outlet pipe 7 are formed so that their lower ends protrude downward from the lid 4 by 3 mm. Ar (argon) gas is continuously supplied to the gas inlet pipe 6 from a gas supply system (not shown). The gas outlet pipe 7 is connected to a trap tank 12 containing an aqueous sodium hydroxide solution 11. Exhaust air attempting to exit the reaction vessel 3 through the gas outlet pipe 7 passes through the aqueous sodium hydroxide solution 11 in the trap tank 12 before being released to the outside. Therefore, even if the exhaust air contains hydrogen sulfide gas generated by the vulcanization reaction, it is neutralized with the aqueous sodium hydroxide solution and removed from the exhaust air.

[0079] (Firing process) First, with the raw material 2 accommodated at the bottom of the reaction vessel 3, Ar gas was continuously supplied from the gas supply system at a flow rate of 80 ml / min, and 30 minutes after the start of the supply, heating was started in the electric furnace 8. The temperature was increased at a rate of 150°C / h. When the temperature of the raw material reached the firing temperature (400°C) in Table 3, firing was performed for 2 hours while maintaining the firing temperature. Next, the reaction product was naturally cooled to 25°C in an Ar gas atmosphere while adjusting the flow rate of Ar gas, and the product was then removed from the reaction vessel 3.

[0080] (Removal of unreacted sulfur) In order to remove the unreacted sulfur (free elemental sulfur) remaining in the product after the calcination process, the following process was carried out. That is, the product was crushed in a mortar, and 2 g of the crushed material was placed in a glass tube oven and heated at 250°C for 3 hours while suctioning under vacuum to obtain an organic sulfur material from which the unreacted sulfur had been removed (or which contained only a trace amount of unreacted sulfur). The heating rate was 10°C / min.

[0081] (Classification work) In order to remove coarse particles from the fired product, the fired product was classified using a 32 μm mesh stainless steel sieve to obtain an organic sulfur material 1.

[0082] <Production of lithium-ion secondary battery> A lithium ion secondary battery was fabricated as follows.

[0083] (positive electrode) The organic sulfur material 1 was used as the active material, acetylene black as the conductive assistant, and acrylic resin as the binder. These were weighed so that the ratio of active material:conductive assistant:binder was 90:5:5 (mass%), and placed in a container. MilliQ water was used as a dispersant, and the mixture was stirred and mixed using a centrifugal mixer (ARE-250 manufactured by Thinky Corporation) to prepare a uniform slurry. The prepared slurry was applied to an aluminum foil of 20 μm using an applicator with a slit width of 60 μm, and the electrode compressed using a roll press was heated in a dryer at 120 ° C for 3 hours, dried, and punched out to φ11 to obtain an electrode (positive electrode). The weight of the electrode was then measured, and the amount of active material in the electrode was calculated from the above ratio.

[0084] (Negative electrode) The negative electrode used was a metallic lithium foil (disk-shaped, diameter 14 mm, thickness 500 μm, manufactured by Honjo Metals Co., Ltd.).

[0085] (electrolyte) The electrolyte used was a non-aqueous electrolyte in which LiPF6 was dissolved in a mixed solvent of ethylene carbonate and diethyl carbonate. The ethylene carbonate and diethyl carbonate were mixed in a volume ratio of 1:1. The concentration of LiPF6 in the electrolyte was 1.0 mol / l.

[0086] (Lithium-ion secondary battery) A coin battery was produced using the above positive and negative electrodes. In detail, in a dry room, a separator (Celgard2400 manufactured by Celgard, a polypropylene microporous membrane having a thickness of 25 μm) and a glass nonwoven fabric filter (440 μm thick, GA100 manufactured by ADVANTEC) were sandwiched between the positive and negative electrodes to produce an electrode body battery. This electrode body battery was housed in a battery case (a member for CR2032 type coin batteries, manufactured by Hosen Co., Ltd.) made of a stainless steel container. The above electrolyte was injected into the battery case. The battery case was sealed with a crimping machine to obtain the lithium ion secondary battery of Example 1.

[0087] Examples 2 to 16 and Comparative Examples 1 to 2 Except for making appropriate changes according to the compositions and conditions in Tables 3 and 4, the same treatment as in Example 1 was carried out to prepare the respective firing raw materials, the organic sulfur materials, and the lithium ion secondary batteries.

[0088] <Measurement of discharge capacity and capacity retention rate> The coin-type lithium ion secondary batteries produced in each Example and Comparative Example were charged and discharged at a current value equivalent to 50 mA per 1 g of positive electrode active material from the 1st to 9th times under the condition of a test temperature of 30° C. The batteries were charged and discharged at a current value equivalent to 250 mA from the 10th to 30th times. The discharge end voltage was 1.0 V, and the charge end voltage was 3.0 V. The batteries were repeatedly charged and discharged, and the battery discharge capacity (mAh) was observed for the 10th and 30th times.

[0089] The second discharge capacity (mAh / g) was taken as the initial capacity. The larger the initial capacity, the greater the charge / discharge capacity of the lithium-ion secondary battery, and the more favorable it is. 10 (mAh / g) and 30th discharge capacity DC 30 From (mAh / g), the following formula (a): Capacity retention rate (%)=(DC 30 / DC 10 )×100 (a) As explained above, the higher the capacity retention rate, the better the cycle characteristics of the lithium-ion secondary battery.

[0090] <Elemental analysis> (method) The masses of carbon, hydrogen, sulfur and nitrogen are measured using a fully automated elemental analyzer, vario MICRO cube, manufactured by Elementar, and the mass ratios (%) of each are calculated.

[0091] (Acrylic resin) The acrylic resin used in the examples was subjected to elemental analysis. The results are shown in the table below. The mass ratios of C (carbon), H (hydrogen), N (nitrogen) and S (sulfur) are actual measured values. The remainder when these measured values ​​are subtracted from the total amount (100%) is estimated to be approximately the mass ratio of O (oxygen).

[0092] [Table 2]

[0093] (organic sulfur material) The organic sulfur materials produced in the Examples and Comparative Examples were subjected to elemental analysis. The results are shown in Tables 3 and 4.

[0094] <IRスペクトル> The IR spectra were measured by the method described above. The results for acrylic resin 1 (Example 1), acrylic resin 2 (Example 2), acrylic resin 3 (Example 3) and acrylic resin 4 (Example 4) are shown in FIG.

[0095] <Raman spectrum> The Raman spectra were measured by the method described above. The results for the organosulfur materials of Example 1 and Comparative Examples 1 and 2 are shown in FIG.

[0096] [Table 3]

[0097] [Table 4]

[0098] From Tables 3 and 4, it can be seen that the Examples show higher initial capacity (mAh / g) and also maintain a higher capacity retention rate (%) than Comparative Example 1. Comparative Example 2 shows high initial capacity and capacity retention rate, but is difficult to provide at low cost because it uses expensive polyacrylonitrile as a raw material. According to the organosulfur material of the present disclosure, a lithium ion secondary battery having a high initial capacity and a good capacity retention rate can be provided at low cost. [Explanation of symbols]

[0099] 1. Reactor 2 Raw materials 3 Reaction vessel 4 Silicone lid 5 Alumina protection tube 6 Gas inlet pipe 7 Gas exhaust pipe 8. Electric Furnace 9 Thermocouples 10 Temperature Controller 11 Sodium hydroxide solution 12 Trap tank A 1450cm -1 Difference between nearby peak intensities and the corresponding baseline intensity B 1540cm -1 Difference between nearby peak intensities and the corresponding baseline intensity

Claims

1. It is an organic sulfur material made by modifying acrylic resin with sulfur. The acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066 cm -1 Near, 1150 cm -1 Near, 1245 cm -1 Near, 1270 cm -1 Near, 1453 cm -1 Near and 1732 cm -1 It has a peak near The particle size of the acrylic resin is 0.1 to 300.0 μm, In the Raman spectrum detected by Raman spectroscopy, -1 The main peak is present in the vicinity of 200 to 1800 cm -1 Another 485 cm in the range -1 Near, 1250 cm -1 Near, 1540 cm -1 There is a peak near the nucleus, which indicates an organosulfur material.

2. It is an organic sulfur material made by modifying acrylic resin with sulfur. The acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066 cm -1 Near, 1150 cm -1 Near, 1245 cm -1 Near, 1270 cm -1 Near, 1453 cm -1 Near and 1732 cm -1 It has a peak near The acrylic resin has a porous structure, In the Raman spectrum detected by Raman spectroscopy, -1 The main peak is present in the vicinity of 200 to 1800 cm -1 Another 485 cm in the range -1 Near, 1250 cm -1 Near, 1540 cm -1 There is a peak near the nucleus, which indicates an organosulfur material.

3. 3. The organic sulfur material according to claim 2, wherein the acrylic resin having a porous structure has an oil absorption of 100 ml / 100 g or more.

4. It is an organic sulfur material made by modifying acrylic resin with sulfur. The acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066 cm -1 Near, 1150 cm -1 Near, 1245 cm -1 Near, 1270 cm -1 Near, 1453 cm -1 Near and 1732 cm -1 It has a peak near The median diameter of the organic sulfur material is 5 to 40 μm; In the Raman spectrum detected by Raman spectroscopy, -1 The main peak is present in the vicinity of 200 to 1800 cm -1 Another 485 cm in the range -1 Near, 1250 cm -1 Near, 1540 cm -1 There is a peak near the nucleus, which indicates an organosulfur material.

5. In the FT-IR spectrum of the acrylic resin, -1 Nearby peaks and the 1732 cm -1 5. The organosulfur material of claim 1, wherein the neighboring peaks are greater than the remaining peaks.

6. The FT-IR spectrum further shows -1 Near, 992 cm -1 Near, 1196 cm -1 Near, 2955 cm -1 Near and 2996 cm -1 The organosulfur material according to any one of claims 1 to 5, having a peak around

7. The mass ratios of carbon, hydrogen, nitrogen and sulfur in the total amount of the acrylic resin are 60.0 to 70.0%, 7.5 to 9.5%, 0.0% and 0.0 to 1.0%, respectively. The organic sulfur material according to any one of claims 1 to 6.

8. The organic sulfur material according to any one of claims 1 to 7, wherein the modification is carried out by calcination in a non-oxidizing atmosphere.

9. The organic sulfur material according to any one of claims 1 to 8, wherein the amount of sulfur in the organic sulfur material is 50.0 mass% or more.

10. The organic sulfur material according to any one of claims 1 to 9, wherein the hydrogen content in the organic sulfur material is 1.8 mass% or less.

11. The organic sulfur material according to any one of claims 1 to 3 and 5 to 10, wherein the median diameter of the organic sulfur material is 5 to 40 μm.

12. An electrode comprising the organosulfur material according to any one of claims 1 to 11.

13. A lithium ion secondary battery comprising the electrode of claim 12.

14. 1. A method for producing an organosulfur material, comprising: (1) preparing an acrylic resin; (2) modifying the acrylic resin with sulfur It includes, and The acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066 cm -1 Near, 1150 cm -1 Near, 1245 cm -1 Near, 1270 cm -1 Near, 1453 cm -1 Near and 1732 cm -1 having a peak near The particle size of the acrylic resin is 0.1 to 300.0 μm, In the Raman spectrum detected by Raman spectroscopy of the organic sulfur material, -1 The main peak is present in the vicinity of 200 to 1800 cm -1 Another 485 cm in the range -1 Near, 1250 cm -1 Near, 1540 cm -1 A manufacturing method in which a peak is present near

15. 1. A method for producing an organosulfur material, comprising: (1) preparing an acrylic resin; (2) modifying the acrylic resin with sulfur It includes, and The acrylic resin has a peak at 756 cm in the FT-IR spectrum. -1 Near, 1066 cm -1 Near, 1150 cm -1 Near, 1245 cm -1 Near, 1270 cm -1 Near, 1453 cm -1 Near and 1732 cm -1 having a peak near The acrylic resin has a porous structure, In the Raman spectrum detected by Raman spectroscopy of the organic sulfur material, -1 The main peak is present in the vicinity of 200 to 1800 cm -1 Another 485 cm in the range -1 Near, 1250 cm -1 Near, 1540 cm -1 A manufacturing method in which a peak is present near

16. The method according to claim 14 or 15, wherein the modification is carried out by calcination in a non-oxidizing atmosphere.

17. The method according to any one of claims 14 to 16, wherein the amount of sulfur relative to the acrylic resin is 50 to 1000 parts by mass of sulfur per 100 parts by mass of acrylic resin.

18. The modification is carried out by calcination in a non-oxidizing atmosphere, The method according to any one of claims 14, 15 and 17, wherein the firing temperature is 250 to 550°C.

19. A method for manufacturing an electrode, comprising the steps of: After producing an organic sulfur material by the production method according to any one of claims 14 to 18, (3) A step of preparing an electrode using the organosulfur material The manufacturing method comprising:

20. A method for producing a lithium ion secondary battery, comprising: After the electrode is produced by the method according to claim 19, (4) A step of producing a lithium ion secondary battery using the electrode. The method of manufacturing the same.

Citation Information

Patent Citations

  • Sulfur / electric conducting polymer composition used as positive electrode of electrochemical power supply and its method

    CN1396202A

  • Sulfur modified polyacrylonitrile sheet, method for manufacturing the same, and application of the same

    JP2010153296A

  • Sulfur-based positive electrode active material, and lithium ion secondary battery

    JP2015092449A

  • Electrode material for lithium ion battery, electrode material for lithium ion capacitor, electrode, battery, capacitor, electric apparatus, manufacturing method for electrode material for lithium ion battery, and manufacturing method for electrode material for lithium ion capacitor

    JP2019032983A

  • JPP7163983B